MEMS device and method for manufacturing the same
By using ultraviolet light to remove the protective film in the MEMS device manufacturing method, the problem of packaging quality degradation caused by the SAM film during the MEMS sensor packaging process is solved, the packaging quality and production efficiency are improved, and the defects of the mask process are avoided.
Patent Information
- Application Number
- CN201811611783.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-12-27
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2038-12-27
AI Technical Summary
During the wafer-level packaging process of MEMS sensors, the deposited SAM film material will lead to a decrease in packaging quality and problems such as voids and air leakage.
In the MEMS device manufacturing method, in the step of removing the protective film, a low-pressure quartz mercury lamp is used to generate ultraviolet rays, the protective film is removed at a preset angle and time, and the protective film located on the side wall of the groove and blocked by the mass block is retained, and the bonding is cleared Protective film in the area to avoid direct impact on the wafer surface.
It improves the packaging quality of MEMS devices, saves costs, improves production efficiency, avoids alignment and template size accuracy problems in the mask process, and protects the structure under the suspended mass block.
Smart Images

Figure CN109650326B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor devices, and more particularly to a MEMS device and a manufacturing method thereof. Background Art
[0002] The preparation of single or multi-molecular-layer ultra-thin films on the surface of micro-electro-mechanical system (MEMS) materials can significantly reduce the friction coefficient of the surface of MEMS materials without reducing their load-bearing capacity, and even produce a super-slip state. This is an effective means to solve the lubrication problem of MEMS systems.
[0003] The molecular films used for MEMS surface lubrication mainly include Langmuir-Blodgett (LB) films and self-assembled monolayer (SAM) films. By using LB film technology, a molecular ordered system can be formed on the surface of the material through single molecule assembly. It has the advantages of stable performance, low friction coefficient, and controllable thickness. It has been used for the lubrication problem of magnetic recording systems. However, due to the complex preparation method of LB film and the combination with the substrate by van der Waals force, the thermal stability and dynamic stability of the film are reduced, which limits its application to a certain extent. SAM film is a new type of organic ultra-thin film developed in recent years. SAM film has a stable structure and is tightly stacked. It has the functions of anti-corrosion, friction reduction, and wear reduction. It has great development potential in solving the lubrication problem of MEMS systems.
[0004] However, some MEMS sensors require wafer-level packaging processes. Depositing SAM film materials on the wafer surface will seriously affect the wafer-level packaging, resulting in a significant decrease in packaging quality, voids, air leaks, and other phenomena. Summary of the invention
[0005] In view of this, the present invention provides a MEMS device and a method for manufacturing the same, wherein in the step of removing the protective film, the protective film on the first bonding area is removed, thereby achieving the purpose of improving the packaging quality.
[0006] According to one aspect of the present invention, a method for manufacturing a MEMS device is provided, comprising: forming a sacrificial layer on a first substrate; forming a mass block on the sacrificial layer; removing part of the mass block to form a first groove; removing part of the sacrificial layer through the first groove to form a cavity reaching the surface of the first substrate; forming a first bonding area on the mass block; forming a protective film, the protective film covering the first bonding area, the surface of the mass block and the first substrate, and the sidewall of the first groove; and removing part of the protective film, wherein, in the step of removing the protective film, the protective film located on the sidewall of the first groove, the protective film located on the surface of the mass block opposite to the first substrate, and the protective film located on the surface of the first substrate are retained because they are blocked by the mass block.
[0007] Preferably, the protective film also covers the side wall of the sacrificial layer. In the step of removing the protective film, the protective film located on the side wall of the sacrificial layer is retained because it is blocked by the mass block.
[0008] Preferably, the step of removing the protective film comprises: generating ultraviolet rays using a low-pressure quartz mercury lamp; and irradiating the protective film with the ultraviolet rays for a predetermined time, wherein the ultraviolet rays are at a preset angle to the MEMS device.
[0009] Preferably, the method of removing the protective film comprises ultraviolet-ozone cleaning.
[0010] Preferably, the preset angle ranges from 5° to 60°.
[0011] Preferably, the preset angle is between 40° and 50°.
[0012] Preferably, the predetermined time ranges from 10 to 60 minutes.
[0013] Preferably, the wavelength of the ultraviolet light is selected from at least one of 254 nm and 185 nm.
[0014] Preferably, the ratio of the depth to the width of the first groove is not less than 5.
[0015] Preferably, the ratio of the depth to the width of the first groove ranges from 5 to 30.
[0016] Preferably, the material of the protective film is selected from at least one of an organic film of an organosilane type and an organic film of an organosiloxane type.
[0017] Preferably, the material of the protective film is selected from FOTS (CF3 (CF2) 5 (CH2) 2SiCl3), OTS (CH3 (CH2) 17SiCl3), DDMS(Cl2Si(CH3)2), MTOS(CH3Si(OCH3)3), FOTES(CF3(CF2)5(CH2)2Si(OC2H5)3), FOMDS(CF3(CF2)5(CH2)2Si(CH3)Cl2), FOMMS(CF3(CF2)5(CH2)2Si(CH3)2Cl), PFDA(C 10 HF 19 At least one of O2), DMS (SiO (CH3) 2) and FDTS (CF3 (CF2) 7 (CH2) 2SiCl3).
[0018] Preferably, the thickness range of the protective film includes to
[0019] Preferably, the method further includes: forming a MEMS sensor, the MEMS sensor including a second bonding area; and bonding the first bonding area to the second bonding area.
[0020] Preferably, the step of forming the MEMS sensor includes forming a second groove on the second substrate, wherein the second groove corresponds to the position of the first groove.
[0021] Preferably, the first groove is communicated with the second groove and the cavity.
[0022] Preferably, a bonding method of the first bonding area and the second bonding area is selected from at least one of eutectic bonding, glass powder bonding, and anodic bonding.
[0023] Preferably, the material of the first bonding region includes Al, and the material of the second bonding region includes Ge.
[0024] Preferably, the bonding method of the first bonding region and the second bonding region includes Al / Ge eutectic bonding.
[0025] According to another aspect of the present invention, there is provided a MEMS device, comprising: a first substrate; a sacrificial layer located on the first substrate; a mass block located on the sacrificial layer; a first groove located in the mass block; a cavity exposing the surface of the first substrate via the first groove; a first bonding area located on the mass block; and a protective film covering the side walls of the first groove, the surface of the mass block opposite to the first substrate, and the surface of the first substrate.
[0026] Preferably, the protection film also covers the sidewalls of the sacrificial layer.
[0027] Preferably, the ratio of the depth to the width of the first groove is not less than 5.
[0028] Preferably, the ratio of the depth to the width of the first groove ranges from 5 to 30.
[0029] Preferably, the material of the protective film is selected from at least one of an organic film of an organosilane type and an organic film of an organosiloxane type.
[0030] Preferably, the thickness range of the protective film includes to
[0031] Preferably, a MEMS sensor is further included, wherein the MEMS sensor includes a second bonding area, and the first bonding area is bonded to the second bonding area.
[0032] Preferably, the MEMS sensor further comprises a second groove located on the second substrate, and the second groove corresponds to the position of the first groove.
[0033] Preferably, the first groove is in communication with the cavity and the second groove.
[0034] Preferably, the material of the first bonding region includes Al, and the material of the second bonding region includes Ge.
[0035] According to the manufacturing method of the MEMS device provided by the present invention, in the step of removing the protective film, the protective film located on the side wall of the first groove, the protective film located on the surface of the mass block opposite to the first substrate, and the protective film located on the surface of the first substrate are retained because they are blocked by the mass block, while the protective film located on the first bonding area is removed, so that the first bonding area of the MEMS device can be better bonded with other structures, thereby achieving the purpose of improving the quality of wafer-level packaging.
[0036] In addition, in the manufacturing method of the MEMS device provided by the present invention, in the step of removing the protective film, the mass block can block the retained protective film, thereby selectively removing the protective film in the bonding area, and there is no need to add a mask in this step, which saves costs and improves production efficiency.
[0037] The present invention replaces the mask of the existing solution by presetting the angle, which can remove the protective film on the surface of the bonding area, facilitating the subsequent process steps, and does not damage the protection of the bottom of the groove and the suspended mass block, thereby achieving the purpose of protection.
[0038] The existing process using a mask has problems such as alignment and low template size accuracy. At the same time, the mask process will damage the MEMS device with a movable structure, affecting the product yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings of the embodiments will be briefly introduced below. Obviously, the drawings in the following description only relate to some embodiments of the present disclosure, rather than limiting the present disclosure.
[0040] Figure 1a A schematic diagram of a method for manufacturing a MEMS device according to an embodiment of the present invention is shown.
[0041] Figure 1b A schematic diagram of a method for manufacturing a MEMS structure of a MEMS device according to an embodiment of the present invention is shown.
[0042] Figures 2 to 8 The cross-sectional schematic diagram shows a part of the stages in the method for manufacturing a MEMS device according to an embodiment of the present invention. DETAILED DESCRIPTION
[0043] The invention will be described in more detail below with reference to the accompanying drawings. In each of the accompanying drawings, the same elements are represented by similar reference numerals. For the sake of clarity, the various parts in the accompanying drawings are not drawn to scale. In addition, some well-known parts may not be shown in the drawings.
[0044] Many specific details of the invention are described below, such as component structures, materials, dimensions, processing techniques, and technologies, in order to more clearly understand the invention. However, as those skilled in the art will appreciate, the invention may be implemented without following these specific details.
[0045] It should be understood that when describing the structure of a component, when a layer or a region is referred to as being "on" or "over" another layer or another region, it may mean that it is directly on the other layer or another region, or that other layers or regions are included between it and the other layer or another region. Moreover, if the component is turned over, the layer or a region will be "below" or "beneath" another layer or another region.
[0046] Figure 1a FIG. 1 is a schematic diagram showing a method for manufacturing a MEMS device according to an embodiment of the present invention. Figures 2 to 8 The manufacturing method of the MEMS device according to the embodiment of the present invention is described in detail.
[0047] In step S01, a MEMS structure is formed. Figure 1b As shown, a MEMS structure can be formed through the following steps S011 to S015.
[0048] In step S011, a sacrificial layer 102 is formed on the first substrate 101, wherein the material of the sacrificial layer 102 includes SiO2, such as Figure 2 shown.
[0049] In step S012, a mass block 103 is formed on the sacrificial layer 102, wherein the material of the mass block 103 includes polysilicon, such as Figure 2 shown.
[0050] In step S013, a first bonding region 104 is formed on the mass block 103, wherein the material of the first bonding region 104 includes Al, such as Figure 2 shown.
[0051] In this embodiment, the first bonding regions 104 are respectively located on both sides of the mass block 103 , however, the embodiments of the present invention are not limited thereto, and those skilled in the art may make other arrangements for the number and position of the first bonding regions 104 as required.
[0052] In step S014, a portion of the mass block 103 is etched to form a first groove 10, and a portion of the sacrificial layer 102 is exposed through the first groove 10. Figure 3 shown.
[0053] In this embodiment, the number of the first grooves 10 includes two. The ratio of the depth H to the width L of the first groove 10 is not less than 5. Preferably, the ratio of the depth H to the width L of the first groove 10 is 5 to 30. More preferably, the depth-to-width ratio is selected in the range of 8 to 12, which can better achieve the selective removal of the protective film on the surface of the mass block and the first bonding area, and avoid the protective film located on the side wall of the first groove 10, the protective film located on the surface opposite to the mass block 103 and the first substrate 101, and the protective film located on the surface of the first substrate 101. The embodiment of the present invention is not limited to this, and those skilled in the art can set the number and depth-to-width ratio of the first grooves 10 as needed.
[0054] In step S015, a portion of the sacrificial layer 102 is removed through the first groove 10 by etching to form a cavity 20, wherein a portion of the first substrate 101 is exposed through the cavity 20 and the first groove 10. At least a portion of the sacrificial layer 102 between the two sides of the mass block 103 and the first substrate 101 is retained, such as Figure 4 shown.
[0055] In this embodiment, for example, hydrofluoric acid (HF) gas phase fumigation is used to corrode the sacrificial layer 102 between the middle of the proof mass 103 and the first substrate 101, so that the middle proof mass pattern is released and the corresponding portion of the first substrate 101 is exposed.
[0056] In step S02, a protective film is formed. Specifically, Figure 5 As shown, the protection film 105 covers the first bonding area 104 , the mass block 103 , the surface of the first substrate 101 , and the sidewalls of the first groove 10 and the sacrificial layer 102 .
[0057] The method for forming the protective film 105 includes a molecular vapor deposition method (MVD). The protective film 105 is a SAM film, and its thickness range includes to The material of the protective film 105 is selected from at least one of an organic film of an organic silane type and an organic film of an organic siloxane type. Further, the material of the protective film 105 is selected from FOTS (CF3 (CF2) 5 (CH2) 2SiCl3), OTS (CH3 (CH2) 17 SiCl3), DDMS(Cl2Si(CH3)2), MTOS(CH3Si(OCH3)3), FOTES(CF3(CF2)5(CH2)2Si(OC2H5)3), FOMDS(CF3(CF2)5(CH2)2Si(CH3)Cl2), FOMMS(CF3(CF2)5(CH2)2Si(CH3)2Cl), PFDA(C 10 HF 19 O2) and DMS (SiO (CH3) 2). In some preferred embodiments, the material of the protective film 105 is FDTS (CF3 (CF2) 7 (CH2) 2SiCl3).
[0058] In step S03, a portion of the protective film is removed. Specifically, Figure 6 As shown, the wafer surface is cleaned by gas cleaning to remove part of the protective film 105. For example, the wafer surface is cleaned by UV-Ozone cleaning, the low-pressure quartz mercury lamp 110 generating ultraviolet rays is set at a predetermined angle to the MEMS, and the protective film 105 is irradiated for a predetermined time, wherein the preset angle ranges from 5° to 60°, preferably from 40° to 50°, and more preferably from 45°, within which the effect of removing the protective film is better; the range of the predetermined time ranges from 10 to 60 minutes, preferably 30 minutes; the wavelength of the ultraviolet rays generated by the low-pressure quartz mercury lamp 110 is selected from at least one of 254nm and 185nm, O2 in the air generates O atoms under the action of ultraviolet rays with a wavelength of 185nm, and O atoms and O2 molecules produce O3; O3 dissociates into O atoms under the action of ultraviolet rays with a wavelength of 254nm, and O atoms react with the protective film 105 to generate products such as CO2 and H2O that will be emitted. The protective film on the side wall of the first groove 10, the protective film on the surface of the mass block 103 opposite to the first substrate 101, the protective film on the side wall of the sacrificial layer 102, and the protective film on the surface of the first substrate 101 are retained because they are blocked by the mass block 103. The protective film on the surface of the wafer, especially the protective film on the surface of the bonding area 104, has been completely removed. Figure 7 shown.
[0059] In step S04, a MEMS sensor is formed. Specifically, a second groove 30 is formed in the second substrate 202, and a second bonding area 201 is formed on the second substrate 202, wherein the position of the second groove 30 corresponds to the first groove 10, and the number and position of the second bonding area 201 correspond to the first bonding area 104, wherein the material of the second bonding area 201 includes Ge, such as Figure 8 shown.
[0060] In step S05, the MEMS structure and the MEMS sensor are bonded to form the MEMS device of this embodiment, wherein the second groove 30, the first groove 10 and the cavity 20 are connected, such as Figure 8 shown.
[0061] In this embodiment, the method of bonding the first bonding area 104 and the second bonding area 201 is selected from at least one of eutectic bonding, glass powder bonding, and anodic bonding. In some preferred embodiments, the method of bonding the first bonding area 103 and the second bonding area 201 is Al / Ge eutectic bonding.
[0062] The embodiment of the present invention also provides Figure 8 The MEMS device shown includes a MEMS structure and a MEMS sensor. The MEMS structure includes: a first substrate 101 , a sacrificial layer 102 , a mass block 103 , a first bonding area 104 , a protective film 105 , a first groove 10 and a cavity 20 .
[0063] The sacrificial layer 102 is located on the first substrate 101. The cavity 20 is formed by removing part of the sacrificial layer 102, and the first substrate 101 is exposed through the first groove 10. The mass block 103 is located on the sacrificial layer 102. The first groove 10 is located in the mass block 103 and is connected to the cavity 20. The first bonding area 104 is located on the mass block 103. The protective film 105 covers the sidewalls of the first groove 10, the surface of the mass block 103 opposite to the first substrate 101, the sidewalls of the sacrificial layer 102 and the surface of the first substrate 101. Among them, the ratio of the depth to the width of the first groove 20 is not less than 5, preferably, the ratio of the depth to the width of the first groove 10 is 5 to 30, and more preferably, the aspect ratio is selected in the range of 8 to 12. The thickness range of the protective film 105 includes to The material of the protective film 105 is selected from at least one of an organic film of an organosilane type and an organic film of an organosiloxane type.
[0064] The MEMS sensor includes: a second bonding area 201, a second substrate 202, and a second groove 30. The second groove 30 corresponds to the position of the first groove 10, and the second groove 30 is connected to the first groove 10 and the cavity 20. The material of the first bonding area 104 includes Al, and the material of the second bonding area 201 includes Ge. The first bonding area 104 and the second bonding area 201 are bonded by Al / Ge eutectic bonding.
[0065] According to the manufacturing method of the MEMS device provided by the present invention, in the step of removing the protective film, the protective film located on the side wall of the mass block, the protective film located on the surface of the mass block opposite to the first substrate, and the protective film located on the surface of the first substrate are retained because they are blocked by the mass block, while the protective film located on the first bonding area is removed, so that the first bonding area of the MEMS device can be better bonded with other structures, thereby achieving the purpose of improving the quality of wafer-level packaging.
[0066] In addition, in the manufacturing method of the MEMS device provided by the present invention, in the step of removing the protective film, the mass block can block the retained protective film, thereby selectively removing the protective film in the bonding area, and there is no need to add a mask in this step, which saves costs and improves production efficiency.
[0067] The present invention replaces the mask of the existing solution by presetting the angle, which can remove the protective film on the surface of the bonding area, facilitating the subsequent process steps, and does not damage the protection of the bottom of the groove and the suspended mass block, thereby achieving the purpose of protection.
[0068] The existing process using a mask has problems such as alignment and low template size accuracy. At the same time, the mask process will damage the MEMS device with a movable structure, affecting the product yield.
[0069] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "comprise", "include" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0070] According to the embodiments of the invention, these embodiments do not describe all the details in detail, nor do they limit the invention to specific embodiments. Obviously, many modifications and changes can be made based on the above description. This specification selects and describes these embodiments in detail in order to better explain the principles and practical applications of the invention, so that those skilled in the art can make good use of the invention and modify and use it based on the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for manufacturing a MEMS device, include: forming a sacrificial layer on the first substrate; forming a mass block on the sacrificial layer; Etching the mass block to form a first groove; removing a portion of the sacrificial layer through the first groove to form a cavity; forming a first bonding region on the mass block; forming a protective film, the protective film covering the first bonding area, the surfaces of the mass block and the first substrate, and the sidewall of the first groove; and Remove part of the protective film, Among them, in the step of removing the protective film, the protective film located on the side wall of the first groove, the protective film located on the surface of the mass block opposite to the first substrate, and the protective film located on the surface of the first substrate are retained because they are blocked by the mass block.
2. The manufacturing method according to claim 1, in, The protective film also covers the side wall of the sacrificial layer. In the step of removing the protective film, the protective film located on the side wall of the sacrificial layer is retained because it is blocked by the mass block.
3. The manufacturing method according to claim 1, in, The step of removing the protective film comprises: Use low-pressure quartz mercury lamps to generate UV light; and The protective film is irradiated with the ultraviolet rays for a predetermined time. Wherein, the ultraviolet rays and the MEMS device are at a preset angle.
4. The manufacturing method according to claim 3, in, The method of removing the protective film includes ultraviolet-ozone cleaning.
5. The manufacturing method according to claim 3, in, The preset angle ranges from 5° to 60°.
6. The manufacturing method according to claim 3, in, The preset angle includes 40° to 50°.
7. The manufacturing method according to claim 3, in, The predetermined time ranges from 10 to 60 minutes.
8. The manufacturing method according to claim 3, in, The wavelength of the ultraviolet rays is selected from at least one of 254 nm and 185 nm.
9. The manufacturing method according to claim 1, in, The ratio of the depth to the width of the first groove is not less than 5.
10. The manufacturing method according to claim 9, in, The ratio of the depth to the width of the first groove ranges from 5 to 30.
11. The manufacturing method according to claim 1, in, The material of the protective film is selected from at least one of an organic film of an organosilane type and an organic film of an organosiloxane type.
12. The manufacturing method according to claim 1, in, The material of the protective film is selected from FOTS (CF 3 (CF 2 ) 5 (CH 2 ) 2 SiCl 3 )、OTS(CH 3 (CH 2 ) 17 SiCl 3 )、DDMS(Cl 2 Si(CH 3 ) 2 )、MTOS(CH 3 Si(OCH 3 ) 3 )、FOTES(CF 3 (CF 2 ) 5 (CH 2 ) 2 Si(OC 2 H 5 ) 3 )、FOMDS(CF 3 (CF 2 ) 5 (CH 2 ) 2 Si(CH 3 )Cl 2 )、FOMMS(CF 3 (CF 2 ) 5 (CH 2 ) 2 Si(CH 3 )2Cl)、PFDA(C 10 HF 19 O 2 )、DMS(SiO(CH 3 ) 2 ) and FDTS(CF 3 (CF 2 ) 7 (CH 2 ) 2 SiCl 3 ) at least one of.
13. The manufacturing method according to claim 1, in, The thickness of the protective film ranges from 10Å to 30Å.
14. The manufacturing method according to any one of claims 1 to 13, further comprising: include: forming a MEMS sensor, the MEMS sensor comprising a second bonding region; as well as The first bonding region is bonded to the second bonding region.
15. The manufacturing method according to claim 14, in, The step of forming the MEMS sensor includes forming a second groove on a second substrate, wherein the second groove corresponds to the first groove in position.
16. The manufacturing method according to claim 15, in, The first groove is communicated with the second groove and the cavity.
17. The manufacturing method according to claim 14, in, The bonding method of the first bonding area and the second bonding area is selected from at least one of eutectic bonding, glass frit bonding, and anodic bonding.
18. The manufacturing method according to claim 14, in, The material of the first bonding area includes Al, The material of the second bonding region includes Ge.
19. The manufacturing method according to claim 18, in, The bonding method of the first bonding region and the second bonding region includes Al / Ge eutectic bonding.