Method for manufacturing semiconductor device and structure thereof

Through self-aligned dual patterning technology and etching operations, the problem that existing photolithography technology is difficult to achieve small pitches is solved, and closer spacing and performance improvement of semiconductor device components are achieved.

CN109817527BActive Publication Date: 2024-10-18TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN201811367420.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-11-16
Publication Date
2024-10-18
Estimated Expiration
2039-11-12

AI Technical Summary

Technical Problem

Existing photolithography technology is difficult to achieve a sufficiently small pitch between semiconductor device components, which limits the further reduction and performance improvement of semiconductor devices.

Method used

Using self-aligned double patterning (SADP) technology, by forming a spacer layer on the mandrel layer and performing an etching operation using sacrificial materials and protective layers, the width of the line-end cutting pattern is reduced, thereby achieving tighter patterning and Smaller spacing.

Benefits of technology

Successfully achieved pitch accommodation of less than 30nm, surpassing the limitations of existing lithography equipment and improving the density and performance of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109817527B_ABST
    Figure CN109817527B_ABST
Patent Text Reader

Abstract

Embodiments of the present invention relate to methods and structures for manufacturing semiconductor devices. Embodiments of the present invention relate to a method for manufacturing a semiconductor device, comprising: forming a first mandrel and a second mandrel on a mask layer; depositing a spacer layer on the first mandrel and the second mandrel; forming a line end cut pattern on the spacer layer between the first mandrel and the second mandrel; depositing a protective layer on the line end cut pattern; etching the protective layer on the line end cut pattern; reducing the width of the line end cut pattern; etching a first horizontal portion of the spacer layer by using the reduced line end cut pattern as an etching mask; removing the first mandrel and the second mandrel; and patterning the mask layer using the etched spacer layer and the etched line end cut pattern as etching masks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present invention relate to a method for manufacturing a semiconductor device and a structure thereof. Background Art

[0002] With the current trend of scaling down of advanced semiconductor devices, process techniques (e.g., photolithography) are adapted to allow device components with smaller sizes and improved accuracy. However, continued improvements in process performance (e.g., photolithography resolution) may be prevented from being achieved due to limitations in available manufacturing techniques and equipment. Efforts have been made to extend the lifecycle of purchased manufacturing equipment to facilitate development processes and reduce expenses. As semiconductor devices are manufactured to smaller and smaller sizes, the component spacing (i.e., pitch) of the device may be reduced to a point that may not be achievable using existing photolithography equipment and processes. Summary of the invention

[0003] An embodiment of the present invention relates to a method for manufacturing a semiconductor device, which includes: forming a first spindle and a second spindle on a mask layer; depositing a spacer layer on the first spindle and the second spindle; forming a line end cut pattern on the spacer layer between the first spindle and the second spindle; depositing a protective layer on the line end cut pattern; etching the protective layer; reducing the width of the line end cut pattern; etching a first horizontal portion of the spacer layer using the reduced line end cut pattern as an etching mask; removing the first spindle and the second spindle; and patterning the mask layer using the etched spacer layer and the etched line end cut pattern as etching masks.

[0004] An embodiment of the present invention relates to a method for manufacturing a semiconductor device, which includes: a first opening in a patterned core shaft layer; depositing a spacer layer on and along the sidewalls of the first opening; forming a first patterned mask on the spacer layer, wherein the first patterned mask includes a second opening, which exposes a portion of the spacer layer on a bottom portion of the first opening; depositing a sacrificial material in the second opening; removing the first patterned mask; forming a line end cutting pattern by etching the sacrificial material; depositing a protective layer covering the line end cutting pattern; trimming the line end cutting pattern and the protective layer; patterning the spacer layer so that a portion of the spacer layer remains on the sidewalls of the core shaft layer; and forming a second patterned mask by removing the core shaft layer while retaining the etched line end cutting pattern and the patterned spacer layer.

[0005] An embodiment of the present invention relates to a method, which includes: patterning multiple spindles on a mask layer; depositing a spacer layer on and along the sidewalls of the multiple spindles; forming a patterned mask on the spacer layer, the patterned mask including an opening that exposes a portion of the spacer layer between adjacent ones of the multiple spindles; depositing a sacrificial material in the opening over the patterned mask; removing the patterned mask to thereby form a line end cut pattern on the spacer layer; depositing a protective layer that covers the sacrificial material and the spacer layer; trimming the protective layer while retaining the spacer layer covered by the protective layer; reducing the width of the line end cut pattern; patterning the spacer layer to expose the multiple spindles; removing the multiple spindles; and patterning the mask layer using the sidewall portion of the spacer layer and the reduced line end cut pattern as an etching mask. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] Aspects of the present disclosure are best understood from the following detailed description when read in conjunction with the accompanying drawings. It should be noted that, in accordance with standard practice in the industry, various components are not drawn to scale. In particular, the sizes of various components may be arbitrarily increased or reduced for clarity of discussion.

[0007] According to some embodiments, Figures 1 to 5 , 6A, 6B, 7A, 7B, 8A, 8B, 9A, 9B, 10A, 10B, 11A, 11B, 12A, 12B, 13A, 13B, 14A, 14B, 15A, 15B and 16 are schematic cross-sectional views of intermediate stages in the manufacture of semiconductor devices.

[0008] According to some other embodiments, Fig.17A , 17B , 18A, 18B, 19A, 19B and 20 are schematic cross-sectional views of intermediate stages in the manufacture of a semiconductor device. DETAILED DESCRIPTION

[0009] The following disclosure provides many different embodiments or examples of different components for implementing the subject matter provided. The following describes the specific examples of components and arrangements to simplify the disclosure. Of course, these components and arrangements are only examples and are not intended to be restrictive. For example, in the following description, the formation of a first component above or on a second component may include an embodiment in which the first component and the second component are directly contacted, and may also include an embodiment in which an additional component may be formed between the first component and the second component so that the first component and the second component may not be directly contacted. In addition, the disclosure may repeat the reference numerals and / or letters in various examples. This repetition is for the purpose of simplification and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.

[0010] Further, spatially relative terms, such as "below," "below," "lower," "above," "top," and the like, may be used herein to describe the relationship of one element or component relative to other elements or components illustrated in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein interpreted accordingly.

[0011] The advanced lithography processes, methods, and materials described in the current disclosure can be used in many applications, including fin-type field effect transistors (FinFETs). For example, heat sinks can be patterned to create relatively tight spacing between components, and the above disclosure is well suited for such situations. In addition, spacers used to form heat sinks for FinFETs can be processed according to the above disclosure.

[0012] The present disclosure is directed to patterning operations for semiconductor devices. Specifically, a self-aligned double patterning (SADP) operation is introduced in which a central mandrel is patterned and then spacers are formed along the sidewalls of the mandrel. The mandrel is removed, while the spacers are retained and used to define a pattern at approximately half the pitch of the mandrel. The above-described patterning operation can be performed on patterned lines in a semiconductor device. Lines patterned in this manner can achieve pitches that are difficult to achieve using existing lithography equipment alone.

[0013] In the present disclosure, exemplary conductive lines are defined between adjacent sidewalls of spacers, and a patterned sacrificial material (sometimes referred to as an inverse material) is formed in the patterned lines. After forming the sacrificial material, the spacers and sacrificial material are used to pattern an underlying mask layer, which in turn is used to pattern a target layer below the mask layer. The sacrificial material patterned in the continuous line pattern is used to define blocking portions that intersect the continuous lines. The target layer patterned by the mask layer can thereby accommodate adjacent line segments with a spacing (pitch) of less than about 30 nm. In addition, using the principles discussed in the present disclosure, the disclosed patterning operations can be extended to other advanced lithography techniques, such as self-aligned quadruple patterning (SAQP) or the like.

[0014] According to some exemplary embodiments, Figures 1 to 5, 6A, 6B, 7A, 7B, 8A, 8B, 9A, 9B, 10A, 10B, 11A, 11B, 12A, 12B, 13A, 13B, 14A, 14B, 15A, 15B, and 16 are schematic cross-sectional views of intermediate stages of patterning a target layer 102 in a semiconductor device 100. In some embodiments, the semiconductor device 100 is processed on a larger wafer. Various components (e.g., active components, passive components, interconnect structures, and the like) may be formed on the semiconductor device 100. A die singulation operation may be applied to the saw line regions of the wafer to separate the wafer into individual semiconductor dies or chips, at least one of which includes the semiconductor device 100.

[0015] On display at Figure 1 Among the layers of the semiconductor device 100 in FIG. 1 , the target layer 102 is a layer that should remain in the finished product of the semiconductor device 100. As discussed in subsequent paragraphs, the target layer 102 may be processed by patterns to be formed and transferred thereto through other layers.

[0016] See also Figure 1 , obtaining or providing a substrate 104. The substrate 104 may be formed of a semiconductor material such as silicon, doped or undoped, or an active layer of a semiconductor-on-insulator (SOI) substrate. The substrate 104 may include: other semiconductor materials, such as germanium; compound semiconductors, including silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, and / or indium antimonide; alloy semiconductors, including SiGe, GaAsP, AlInAs, AlGaAs, GaInAs, GaInP, and / or GaInAsP; or combinations thereof. Other substrates may also be used, such as multilayer substrates or gradient substrates. In some embodiments where the target layer 102 is a semiconductor substrate for FinFETs, the substrate 104 may be omitted.

[0017] The film stack is formed over a substrate 104. In the depicted embodiment, the film stack includes a target layer 102, an anti-reflective coating (ARC) 106, a mask layer 108, a dielectric layer 110, and a mandrel layer 112.

[0018] The target layer 102 is formed on the substrate layer 104. In some embodiments, the target layer 102 is an inter-metal dielectric (IMD) layer. The IMD layer 102 may contain interconnecting wires and vias to provide electrical connections for components in the semiconductor device 100. The target layer 102 may include a dielectric material that electrically insulates the wires and vias. The dielectric material may be a low-k value material, for example, having a dielectric constant (k value) of less than 3.8, less than about 3.0, or less than about 2.5. In alternative embodiments, the dielectric material may be a high-k dielectric material having a dielectric constant greater than 3.8. The wires or vias may be formed in patterned openings of the dielectric material.

[0019] In some embodiments, the target layer 102 is formed of a conductive layer such as metal or polysilicon. Conductive components of FinFETs, such as conductive vias or gates, can be formed in the target layer 102 via the proposed patterning operation. The pitch of conductive vias or gates can be reduced, while the gate density can be increased.

[0020] In some embodiments, the target layer 102 is a semiconductor substrate. The semiconductor substrate may be formed of a semiconductor material such as silicon, silicon germanium, or the like. In some embodiments, the semiconductor substrate is a crystalline semiconductor substrate. Various components of the semiconductor device 100, such as isolation structures, source / drain regions, fin structures, dielectric layers, or contacts, may be formed via patterning operations discussed in the present disclosure.

[0021] In some embodiments, an intervening layer (not shown separately) is placed between the target layer 102 and the substrate 104. Exemplary intervening layers include an interlayer dielectric (ILD) layer comprising a low-k dielectric having contact plugs, an adhesion layer, and an etch stop layer formed therein. In some embodiments, an additional IMD layer is formed as another intervening layer.

[0022] ARC 106 is formed over target layer 102. ARC 106 aids in exposure and focusing performance of a patterning operation when the overlying photoresist layer is subjected to exposure radiation. In some embodiments, ARC 106 is formed from a dielectric material such as SiON, silicon carbide, or the like. In some embodiments, ARC 106 is substantially free of nitrogen and is formed from an oxide. ARC 106 may be formed using chemical vapor deposition (CVD), physical vapor deposition (PVD), or the like.

[0023] The mask layer 108 is formed on the ARC 106. In some embodiments, the mask layer 108 is a hard mask. The mask layer 108 may be formed of a metal material such as titanium nitride, titanium, tantalum nitride, or tantalum. The mask layer 108 may be formed of a metal doped carbide (e.g., tungsten carbide) or a metalloid (e.g., silicon nitride, boron nitride, or silicon carbide). The mask layer 108 may be formed using CVD, PVD, atomic layer deposition (ALD), or the like. In some embodiments, the mask layer 108 is initially patterned, and then the target layer 102 is etched through the mask layer 108 as an etch mask. Thus, the pattern of the mask layer 108 is transferred to the target layer 102.

[0024] A dielectric layer 110 is formed over the mask layer 108. The dielectric layer 110 may be formed of a dielectric material, such as silicon oxide (e.g., borophosphosilicate tetraethylorthosilicate (BPTEOS) or undoped tetraethylorthosilicate (TEOS) oxide). The dielectric layer 110 may be formed using CVD, ALD, spin-on coating, or the like. In some embodiments, the dielectric layer 110 serves as an etch stop layer for a mandrel or spacer layer subsequently formed over the dielectric layer 110.

[0025] A mandrel layer 112 is formed over the dielectric layer 110. The first mandrel layer 112 may be formed of a semiconductor material such as amorphous silicon, polycrystalline silicon, silicon nitride, silicon oxide, or the like. In one embodiment, the underlying layer, e.g., the dielectric layer 110, is selected to obtain a high etch selectivity between the mandrel layer 112 and the dielectric layer 110. In some embodiments, the etch selectivity between the mandrel layer 112 and its underlying layer is between about 2.0 and about 10.0.

[0026] A photoresist stack 120 is formed on the mandrel layer 112. The photoresist stack 120 includes a bottom layer 114, an intermediate layer 116, and a top layer 118. The bottom layer 114 and the top layer 118 may be formed of a photosensitive material, such as an organic material, and the intermediate layer 116 may include an inorganic material, such as a nitride, an oxynitride, an oxide, or the like. In some embodiments, the intermediate layer 116 has a high etching selectivity relative to the top layer 118 and the bottom layer 114. In some embodiments, the bottom layer 114 is a bottom anti-reflective coating (BARC) layer. The layers of the photoresist stack 120 may be sequentially deposited in a blanket form using a spin-on coating method, CVD, or other similar processes. In some embodiments, the photoresist stack 120 is a single-layer or double-layer structure, in which at least one layer (such as the intermediate layer 116) is omitted from the photoresist stack 120. The single-layer or double-layer configuration may be used in extreme ultraviolet (EUV) lithography operations.

[0027] Still viewing Figure 1 , for the patterning operation of the mandrel 124 (see Figure 4 ) starts with a patterning operation on the top layer 118. The top layer 118 is patterned as a first stage etching mask. Thus, openings 122 are formed. In some embodiments, the patterned top layer 118 includes extended parallel openings 122 extending perpendicular to the paper surface. The pitch P1 of the openings 122 may be the minimum pitch that can be achieved alone using existing photolithography processes. In some embodiments, the pitch P1 of the openings 122 is greater than about 80 nm. The openings 122 can be formed using an etching operation such as wet etching, dry etching, or a combination thereof. In an embodiment of the present invention, dry etching is used to perform anisotropic etching in a direction orthogonal to the surface of the top layer 118.

[0028] Subsequent reference Figure 2 , the middle layer 116 is patterned via an etching operation using the top layer 118 as an etching mask. The middle layer 116 is then used as a second stage etching mask for patterning the bottom layer 114. Similarly, as Figure 3 As shown in , the bottom layer 114 is patterned and acts as a third stage etch mask for patterning the mandrel layer 112 .

[0029] like Figure 4 As shown in FIG. 1 , the mandrel layer 112 is patterned via an etching operation with the bottom layer 114 as an etching mask. Thus, the mandrels 124 are formed above the dielectric layer 110. In some embodiments, each of the mandrels 124 has a stripe shape when viewed from above. It has been observed that the three-stage etching process using the photoresist stack 120 can help etch the mandrel layer 112 with desired pattern transfer properties. Figures 1 to 4, the pitch P1 of the openings 122 in the top layer 118 can be successfully transferred toward the mandrel layer 112 through the middle layer 116 and the bottom layer 114. The openings 122 extending downward until the upper surface of the mandrel layer 112 are exposed, and the pitch of the mandrels 124 is substantially maintained at P1.

[0030] In some embodiments, the top layer 118 (see Figure 2 and 3 ) is completely or partially consumed during patterning of the bottom layer 114. In some embodiments, the intermediate layer 116 or the bottom layer 114 (see Figure 3 and 4 ) is completely or partially consumed during patterning of the mandrel layer 112. In some embodiments, after the mandrels 124 have been formed, the residue of the photoresist stack 120 (including the bottom layer 114, the middle layer 116, and the top layer 118) is removed or stripped, such as using an ashing process.

[0031] exist Figure 5 , a spacer layer 126 is formed over the mandrel 124 and the dielectric layer 110. The spacer layer 126 may cover the sidewalls of the mandrel 124. The material of the spacer layer 126 is selected to have a high etching selectivity between the dielectric layer 110 and the mandrel 124. For example, the etching selectivity between the mandrel 124 and the dielectric layer 110 is between about 2.0 and about 8.0. The spacer layer 126 may include AlO, AlN, AlON, TaN, TiN, TiO, Si, SiO, SiN, a metal, a metal alloy, or the like. The spacer layer 126 may be formed using a deposition operation such as ALD, CVD, or the like. In some embodiments, the spacer layer 126 is conformally formed so that the spacer layer 126 has a substantially equal thickness throughout the sidewalls and the top surface of the mandrel 124 and the bottom surface of the opening 122. In some embodiments, the area of ​​the opening 122 between the sidewalls of the spacer layer 126 defines the pattern of the subsequently formed conductive line.

[0032] The following description discusses forming a line end cut pattern 148 in the opening 122 over selected portions of the spacer layer 126 (see Fig. 12A and 12B ). Initially, sacrificial material 138 is deposited in selected areas of the line pattern. Sacrificial material 138 is then patterned to define line end cut portions in target layer 102. For example, line end cut patterns 148 are formed to define areas between line segments where no conductive material is formed. In other words, a continuous line is cut into separated segments by the line end cut portions therebetween.

[0033] Throughout Fig. 6A , 6B, 7A, 7B, 8A, 8B, 9A, 9B, 10A, 10B, 11A, 11B, 12A, 12B, 13A, 13B, 14A, 14B, 15A and 15B, and the figures ending with the symbol "A" and Figures 1 to 5 The same cross-sectional view, but the figure ending with the label "B" illustrates a cross-sectional view taken along the line BB of the respective figure having the label "A". For example, Figure 6B Description Fig. 6A A cross-sectional view taken along line BB.

[0034] refer to Fig. 6A and 6B , a photoresist stack 134 is formed on the spacer layer 126. The photoresist stack 134 includes a bottom layer 128, an intermediate layer 130, and a top layer 132. In some embodiments, the materials and configurations of the component layers in the photoresist 134 are similar to those of the photoresist 120. The bottom layer 128 and the top layer 132 may be formed of a photosensitive material such as an organic material. The bottom layer 128 may be deposited between the mandrels 124, such as for spacing of a line pattern between the sidewalls of the spacer layer 126. In some embodiments, the bottom layer 128 is a BARC. The intermediate layer 130 may include an inorganic material such as a nitride, an oxynitride, an oxide, or the like. The intermediate layer 130 has a higher etching selectivity relative to the top layer 132 and the bottom layer 128. The layers of the photoresist stack 134 may be deposited in series in a blanket form using a spin-on coating method, CVD, or other similar processes.

[0035] Still refer to Fig. 6A and 6B , the patterning operation for the line end cutting pattern 148 starts with the patterning operation on the top layer 132. The top layer 132 is patterned as a first stage etching mask. Openings 136 (e.g., 136A, 136B, and 136C) are formed and substantially aligned with the corresponding openings 122 between the sidewalls of the spacer layer 126. In some embodiments, the width of the opening 136 is less than the width of the opening 122 between the sidewalls of the spacer layer 126. The opening 136 can be formed using an etching operation such as wet etching, dry etching, or a combination thereof. In an embodiment of the present invention, dry etching is used to perform anisotropic etching in a direction orthogonal to the surface of the top layer 132. Shown in Fig. 6A The openings 136A and 136B in the Figure 5 The different parallel openings 122 are formed and shown in Figure 6B The openings 136A and 136C in FIG. 1 are formed corresponding to the same opening 122. Fig. 6A and 6B , the opening 136 may have an annular shape or a polygonal shape, such as a quadrilateral shape.

[0036] Subsequent reference Fig. 7A and 7B , the middle layer 130 is patterned via an etching operation using the top layer 132 as an etching mask. The middle layer 130 is then used as a second stage etching mask for patterning the bottom layer 128. Fig. 7A and 7B , the opening 136 extends through the middle layer 116 and the bottom layer 114 and exposes a portion of the spacer layer 126. In some embodiments, the top layer 132 is completely or partially consumed during patterning of the middle layer 130 and the bottom layer 128.

[0037] exist Fig. 8A and 8B 1, a sacrificial material 138 is deposited over the middle layer 130. The sacrificial material 138 may fill the opening 136. In some embodiments (not illustrated), the middle layer 130 is removed before depositing the sacrificial material 138. The middle layer 130 may be removed using dry etching, wet etching, or a combination thereof. In that case, the sacrificial material 138 is formed directly on the upper surface of the bottom layer 128.

[0038] In some embodiments, the sacrificial material 138 includes an inorganic material. For example, the sacrificial material 138 is an inorganic oxide, such as titanium trioxide, tantalum oxide, silicon oxide, or the like. In some embodiments, the inorganic material is a low temperature oxide (LTO). As used throughout the present disclosure, the term "LTO" refers to an oxide deposited at a relatively low processing temperature (e.g., 200° C. or below). The selection of a low temperature deposition operation can help protect the bottom layer 128 from damage. Under the same etchant, the sacrificial material 138 can have sufficient etching selectivity relative to the spacer layer 126. For example, the ratio of the etching rate of the sacrificial material 138 to the etching rate of the spacer layer 126 relative to the same etchant is greater than about 2. Therefore, the patterning performance of the sacrificial material 138 can be better managed through the appropriate selection of its material.

[0039] The sacrificial material 138 may be formed using a suitable operation, such as a spin-on coating process, CVD, PVD, ALD, or the like. The deposition operation may be a conformal operation, in which the sacrificial material 138 lines the sidewalls and bottom surface of the opening 136. In some embodiments using a film deposition operation, portions of the sacrificial material 138 on opposing sidewalls in the opening 136 may be incorporated as the deposition thickness increases, thereby filling the opening 136. In some embodiments, the top surface of the sacrificial material 138 is not planar. For example, there is a notch 139 in the top surface of the sacrificial material 138. Compared to a spin-on process, a film deposition operation (e.g., CVD, PVD, or ALD) allows the sacrificial material 138 to be filled in the opening 136 with improved gap filling performance. Fewer defects (e.g., bubbles) may be introduced through the film deposition operation.

[0040] Later, in Fig.9A and 9B During the planarization operation, a planarization operation (e.g., chemical mechanical polish (CMP), grinding, dry etching, or a combination thereof) is performed to remove excess portions of the sacrificial material 138 above the intermediate layer 130. Thus, a line end cut pattern 148 (including guide pillars 148A, 148B, and 148C) is formed in the bottom layer 128. In some embodiments, the intermediate layer 130 is also removed during the planarization operation. In some embodiments, the thickness of the bottom layer 128 is also removed during the planarization operation. After the planarization operation, the bottom layer 128 is exposed, and the upper surface of the line end cut pattern 148 may be parallel to the upper surface of the bottom layer 128.

[0041] exist Fig. 10A and 10B In some embodiments, the bottom layer 128 is removed using an ashing process. By removing the bottom layer 128, the opening 122 is exposed again. In some portions of some openings 122, the guide posts 148A, 148B, and 148C of the line end cut pattern 148 remain and fill portions of the openings 122. The guide posts 148A, 148B, and 148C also shield selected portions of the spacer layer 126. In some embodiments, the guide posts of the line end cut pattern 148 span from a first sidewall portion of the spacer layer 126 on a first mandrel 124 to an adjacent sidewall portion of the spacer layer 126 on a second mandrel 124 that is adjacent to the first mandrel. In some embodiments, see Fig. 10B , the width W1 of the guide pillar 148A or 148B of the line end cutting pattern 148 is about 40 nm.

[0042] Then, if Fig.11A and 11BAs described in FIG. 1 , the protection layer 152 is deposited on the bottom layer 128 and the line end cutting pattern 148. The protection layer 152 may be deposited on the top surface and sidewalls of the line end cutting pattern 148. In some embodiments, the protection layer 152 covers the upper surface of the spacer layer 126. Fig. 7A and 7B , the formed opening 136 may have a tapered sidewall from the upper surface to the bottom surface. Therefore, each of the openings 136 may have a higher width at the top than at the bottom. Therefore, the patterned line end cutting pattern 148 follows the width dimension of the opening 136. In some embodiments, a deposited protective layer 152 is used to shape the guide post profile of the line end cutting pattern 148, wherein the protective layer 152 has a higher thickness around the bottom portion of the guide post of the line end cutting pattern 148 than around the top surface of the line end cutting pattern 148. Plasma assisted deposition, such as PVD, CVD, or other suitable operations can be used to perform uneven thickness deposition. Thus, the bottom portion of the guide post can be better protected under subsequent etching operations. In some embodiments, the protective layer 152 has a thickness of less than about 30nm. In some embodiments, the protective layer 152 has a thickness in a range between about 5nm and about 30nm.

[0043] In some embodiments, the protective layer 152 includes a dielectric material, such as a nitride (e.g., silicon nitride) or an oxide (e.g., silicon oxide). In some embodiments, the protective layer 152 includes a carbon-based material, such as silicon carbonitride, silicon oxycarbonitride, silicon boron carbonitride, or a polymer material, such as epoxy resin, polyimide (PI), benzocyclobutene (BCB), polybenzoxazole (PBO). In some embodiments, the polymer material includes CF xClass molecules, where the subscript x is a natural number. In some embodiments, the protective layer 152 is formed in a conformal manner using CVD, ALD or other suitable operations, the operations using suitable reaction precursors, such as SiCH4-based gases, NF3-based gases, SiCl4-based gases or CH4-based gases. In some embodiments, the CVD operation of the protective layer 152 has a higher deposition rate in the vertical direction than in the horizontal direction. Therefore, the protective layer 152 has a higher thickness in the area above the top of the line end cutting pattern 148 and in the area above the spacer layer 126 than in the sidewall area of ​​the line end cutting pattern 148. In one embodiment, a plasma-enhanced chemical vapor deposition (PECVD) operation is used to form the uneven sidewalls of the protective layer 152. Due to plasma bombardment, the sidewall deposition using plasma is performed together with the sidewall etching. In one embodiment, since the top receives more plasma bombardment than the bottom portion, the net deposition rate of the protective layer 152 at the top portion of the sidewall is less than the net deposition rate of the sidewall at the bottom portion. Thus, an uneven sidewall of the protective layer 152 is formed such that the bottom portion is thicker than the top portion. In one embodiment, the protective layer 152 has an uneven sidewall thickness that tapers from the bottom portion to the top portion. Thus, because the guide posts of the wire end cutting pattern 148 have a higher width at the bottom than at the top, the modified wire end cutting pattern 148 covered by the protective layer 152 has a more uniform width.

[0044] exist Fig. 12A and 12BIn the present disclosure, the line end cut pattern 148 is trimmed to achieve a reduced width of less than about 30 nm, for example, 10 nm. As previously discussed, the guide pillar width W1 obtained using existing photolithography techniques and equipment can reach a limit of greater than about 40 nm and can no longer be thinner (for example, less than 30 nm). In the present disclosure, it is proposed to produce a reduced guide pillar width of the line end cut pattern 148 by applying a trimming operation. In addition, the protective layer 152 can act as a sacrificial layer in the guide pillars of the line end cut pattern 148 so that the bottom portion of the guide pillar can be protected from damage during the trimming. As previously discussed, because the protective layer 152 helps shape the sidewalls of the line end cut pattern 148 so that the constituent guide pillars of the line end cut pattern 148 / 152 have a more uniform width, the line end cut pattern 148 can be protected from damage around the bottom portion during the etching operation. In some embodiments, the spacer layer 126 is inevitably affected during the trimming of the line end cut pattern 148. In that case, the protective layer 152 on the spacer layer 126 may play another function of protecting the spacer layer 126 from etching. In some embodiments, the protective layer 152 on the upper surface and the sidewall of the guide pillar of the line end cutting pattern 148 is completely removed during the trimming of the line end cutting pattern 148. In some embodiments, an etchant is used in which the etching selectivity between the protective layer 152 and the spacer layer 126 is greater than about 3. In some embodiments, an etchant is used in which the etching selectivity between the protective layer 152 and the spacer layer 126 is between about 3 and about 10. In some embodiments, the sacrificial material 138 has an etching selectivity similar to that of the protective layer 152 relative to the spacer layer 126 under the same etchant. In some embodiments, an etchant is used in which the etching selectivity between the sacrificial material 138 and the spacer layer 126 is between about 3 and about 10. In embodiments where the spacer layer 126 is formed of TiO, fluorine-based etching gases, such as CF4, CH2F2, or CH3F, provide sufficient etching selectivity (eg, greater than about 5) when trimming the protection layer 152 and the line end cut pattern 148 while keeping the spacer layer 126 intact.

[0045] In some embodiments, the trimming operation removes the height of the guide posts of the line end cutting pattern 148 to below the topmost surface of the spacer layer 126 (see Fig. 12A ). In some embodiments, the trimmed wire end cut pattern 148 has a top surface that is lower than the top surface of the mandrel 124. The wire end cut pattern 148 has a reduced height H2. In some embodiments, the sidewall portion of the spacer layer 126 above the reduced wire end cut pattern 148 is exposed by the trimming operation. In some embodiments, the trimming operation removes the width of the guide post of the wire end cut pattern 148 to below the topmost surface of the spacer layer 126 (see Fig. 12B). In some embodiments, each guide pillar of the trimmed line end cut pattern 148 has a tapered sidewall. The guide pillar of the line end cut pattern 148 has a reduced width W2. In some embodiments, throughout the trimming operation, the horizontal portion of the spacer layer 126 is still covered by the protection layer 152.

[0046] exist Fig.13A and 13B In the embodiment of the present invention, in the case where the protective layer 152 is not completely removed along with the trimming of the line end cut pattern 148, the remnants of the protective layer 152 on the horizontal portion above the spacer layer 126 are removed using an etching operation after the trimming operation of the line end cut pattern 148. The horizontal portion of the spacer layer 126 is thus exposed. In some embodiments, the etching operation includes dry etching, wet etching, or a combination thereof. In some embodiments, the comprehensive removal of the protective layer 152 is performed in the same operation of etching the line end cut pattern 148, wherein different etching factors (e.g., plasma bombardment angle, duty cycle of the pulsed plasma source, and duty cycle of the pulsed RF source) are utilized throughout the operation.

[0047] See also Fig.13A , the wire end cut pattern 148 has a reduced height H3 that is less than the height H2. In some embodiments, the completed wire end cut pattern 148 is reduced by more than about 10% compared to its original height H1. In some embodiments, the wire end cut pattern 148 is reduced by about 10% to about 30% of its original height H1. In some embodiments, the resulting wire end cut pattern 148 has a reduced height H3 that is less than about 100nm. In some embodiments, the height H3 is between about 30nm and about 100nm. In some embodiments, the height H3 is between about 30nm and about 50nm.

[0048] In some embodiments, the trimming operation continuously removes the width of each guide post of the line end cutting pattern 148, for example, from the original width W1 ( Fig. 10B ) to a reduced width W2 ( Fig. 12B ), and then to the final width W3 ( Fig. 13B ). In some embodiments, width W2 is substantially equal to width W3, such that Fig. 13BThe trimming operation in the embodiment is mainly focused on removing the protective layer 152 on the spacer layer 126. In some embodiments, the final width W3 of each guide post of the line end cutting pattern 148 is reduced from its original width W1 by about 10% to about 30%. In some embodiments, the final width W3 of each guide post of the line end cutting pattern 148 is reduced from its original width W1 by more than about 30%. In some embodiments, the final width W3 of each guide post of the line end cutting pattern 148 is reduced from its original width W1 by about 30% to about 50%. In some embodiments, the resulting width W3 of the line end cutting pattern 148 is less than about 30nm. In some embodiments, the width W3 is less than about 10nm. In some embodiments, the width W3 is between about 10nm and about 30nm. In some embodiments, the width W3 is between about 15nm and about 30nm.

[0049] Return to reference Fig. 12A and 12B In an embodiment of the present invention, the trimming operation of the protective layer 152 and the line end cutting pattern 148 may include dry etching. In some embodiments using dry etching, a fluorine-based etchant (e.g., CF4) is used. In some embodiments, other etchants, such as oxygen (O2), nitrogen (N2), argon (Ar) or the like, are used in a mixed etchant formulation. For example, using plasma assisted etching, isotropic etching can be achieved through an etching operation. Isotropic etching is performed using a high-voltage and low-bias plasma source to increase the amount of neutral particles or radicals in the plasma, rather than the amount of ionic particles. The increased neutral particles help provide side etching on the sidewalls of the line end cutting pattern 148. In this state, the etching rates in the vertical and horizontal directions may be similar. In some embodiments, the pressurization of the etching operation is, for example, in a range between about 40 and about 60 mTorr, and the bias voltage is less than about 40 volts.

[0050] In some embodiments, the etching ratio between the lateral direction (i.e., the direction opposite to the sidewalls of the guide pillar 148A) and the vertical direction (i.e., the direction opposite to the planar surface of the spacer layer 126) is greater than about 2. In some embodiments, the etching operation can be implemented in an anisotropic manner. In one embodiment, the etching recipe is adjusted to provide a higher etching rate on the sidewalls of the guide pillar 148 compared to its top portion. In one embodiment, by controlling the composition of the reactive gas, a thin film (e.g., a polymer) is simultaneously formed as a byproduct during the etching process. The film covers the upper surface of the etched guide pillar 148 to prevent the plasma from further etching the guide pillar 148 from above, resulting in a lower etching rate in the vertical direction. In some embodiments, a pulsed RF source can be used, wherein a reduced duty cycle of the RF source reduces the etching rate in the vertical direction. In some embodiments, a pulsed plasma source can be used, wherein a lower amount of ion particles reduces the etching rate in the vertical direction. Reference Fig. 12A and12B , the ring and arrow Fh indicate the direction of horizontal etching, where the ring Fh surrounding the dot means pointing to the horizontal direction of the paper, and the ring Fh surrounding the cross means pointing to the horizontal direction of the reader. Further, Fig. 12A , 12B , 13A and 13B indicate the direction of vertical etching.

[0051] In some embodiments, an isotropic etching operation is used based on the recipe of isotropic etching as described above. The concentration of the diluted fluorine-based gas provided is further reduced, so that the concentration difference at different positions in the processing chamber is more obvious. The difference in gas concentration causes the etching rate of the protective layer 152 on the sidewall and top part of the guide post of the line end cutting pattern 148 to be greater than the etching rate of the protective layer 152 on the spacer layer 126. Therefore, part of the protective layer 152 is retained on the upper surface of the horizontal part of the spacer layer 126. The etching operation can be performed at a first etching rate for the etching sidewall of the protective layer 152, and the etching rate is greater than the second etching rate on the horizontal part of the protective layer 152. In one embodiment, the etching operation provides an etching ratio in the range of about 1 and about 2 between the lateral direction and the vertical direction. The higher etching performance in the lateral direction compared to the vertical direction contributes to the width reduction of the guide post 148A and the protective spacer layer 126.

[0052] Then, refer to Fig.14A and 14B , an etching operation is performed to remove some horizontal portions of the spacer layer 126. Thinned vertical portions of the spacer layer 126 (labeled as spacer layer 127) may remain after the etching operation. In some embodiments, some horizontal portions of the spacer layer 126 shielded by the line end cut pattern 148 remain after the etching operation. A portion of the dielectric layer 110 is exposed after the etching operation. In some embodiments, the etching operation is performed using a dry etch, which is performed using an etchant such as CH4, Cl2, combinations thereof, and the like. During the dry etching operation, other gases, such as nitrogen (N2), may be used in conjunction with the etchant. The dry etching operation may include anisotropic etching that does not significantly remove vertical portions of the spacer layer 127 or the line end cut pattern 148.

[0053] exist Fig.15A and 15B In the embodiment of the present invention, an etching operation is used to remove the mandrel 124. Since the mandrel 124 and the line end cut pattern 148 of the spacer layer 126 are different in terms of the etching selectivity relative to the same etching operation, the mandrel 124 is removed without significantly removing the line end cut pattern 148 of the etched spacer layer 127. The underlying dielectric layer 110 acts as an etch stop layer during etching of the mandrel 124.

[0054] After removing the mandrel 124, the wire end cut pattern 148 has a width W3. In some embodiments employing a SADP process as described above, the width W3 is below the critical dimension achievable by a photolithography process alone. The combination of the spacer layer 127 and the wire end cut pattern 148 defines a conductive line pattern for the mask layer 108. Fig.16 A plan view illustrating a pattern defined by the spacer layer 127 and the line end cut pattern 148 . Fig.15A Description Fig.16 The cross-sectional view is taken along the section line AA, and Fig. 15B Description Fig.16 In some embodiments, the space other than the area defined by the spacer layer 127 and the wire end cutting pattern 148 corresponds to the pattern of the conductive line to be formed subsequently. Fig.16 As illustrated, the line end cut pattern 148, which includes guide pillars 148A, 148B, and 148C, cuts between adjacent segments of the line pattern in the spacer layer 127. When the conductive lines are subsequently formed, a desired line pitch W3 of the conductive line segments is obtained.

[0055] Fig.17A , 17B , 18A, 18B, 19A, 19B and 20 Fig.15A and 15B 1 is a cross-sectional view of a method of post-processing a target layer 102 for an operation in FIG. In an embodiment, the target layer 102 is a dielectric layer, and the patterned conductive member is formed in such a dielectric layer. Fig.17A and 17B , the dielectric layer 110 and the mask layer 108 are sequentially etched using the spacer layer 127 and the line end cut pattern 148 as an etching mask. Therefore, the mask layer 108 receives a pattern that is the same as the pattern composed of the spacer layer 127 and the line end cut pattern 148 in a plan view. In some embodiments, the etching operation includes an anisotropic dry etching or wet etching operation. After the mask layer 108 is patterned, a wet wash may be performed to remove any remaining portions of the spacer layer 127, the line end cut pattern 148, and the dielectric layer 110.

[0056] Later, in Fig.18A and 18B In the embodiment, mask layer 108 is used as an etch mask to pattern openings 140 in target layer 102. An etching operation is used, which sequentially etches through ARC 106 and target layer 102. The remaining portion of target layer 102 may have a Fig.16 The pattern formed by the spacers 127 and the line end cut pattern 148 of the target layer 102 may be the same. The etching operation for patterning the target layer 102 may include dry etching, wet etching, or a combination thereof. After the opening 140 is patterned, a wet cleaning operation may be performed to remove the remaining portion of the ARC 106 of the mask layer 108.

[0057] After the opening 140 is patterned in the target layer 102, a conductive member is formed in the opening 140 of the target layer 102. In some embodiments, the target layer 102 is formed of a low-k material, and patterning the target layer 102 provides IMD for forming an interconnect structure. Fig.19A and 19B As illustrated, a conductive line or conductive via 146 is formed in the target layer 102. The conductive line includes a conductive material 144 formed of, for example, copper, tungsten, titanium, or the like. In some embodiments, the conductive line 146 includes one or more layers, such as a liner 142 along the sidewalls and bottom surface of the opening 140. The liner 142 includes TiO, TiN, TaO, TaN, or the like, and provides a diffusion barrier, adhesion layer, and / or seed layer for the conductive material 144. The liner 142 and the conductive material 144 are deposited using any suitable process, such as PVD, CVD, ALD, and the like.

[0058] In some embodiments, a planarization process is performed to remove excess portions of the conductive material 144 over the target layer 102. Thus, a conductive feature is formed in the target layer 102. Fig. 20 A top view of the conductor 146 is illustrated. Fig.19A Description Fig. 20 The cross-sectional view is taken along the section line AA, and Fig.19B Description Fig. 20 The cross-sectional view is taken along the section line BB. Fig. 20 The exemplary wire end cutting portion 150 in Fig.16 The line end cutting pattern 148 in the pattern. As shown by Fig. 20 As illustrated, the line end cutting portion 150 cuts the conductive line into adjacent line segments, thereby maintaining the line spacing of about 30 nm or less defined by the line end cutting pattern 150.

[0059] According to an embodiment of the present invention, a method for manufacturing a semiconductor device includes: forming a first spindle and a second spindle on a mask layer; depositing a spacer layer on the first spindle and the second spindle; depositing a spacer layer on the first spindle and the second spindle; forming a line end cutting pattern on the spacer layer between the first spindle and the second spindle; depositing a protective layer on the line end cutting pattern; etching the protective layer on the line end cutting pattern; reducing the width of the line end cutting pattern; reducing the width of the line end cutting pattern; etching a first horizontal portion of the spacer layer using the reduced line end cutting pattern as an etching mask; removing the first spindle and the second spindle; and patterning the mask layer using the etched spacer layer and the etched line end cutting pattern as etching masks.

[0060] According to an embodiment of the present invention, a method for manufacturing a semiconductor device includes: patterning a first opening in a core shaft layer; depositing a spacer layer on and along the sidewalls of the first opening; forming a first patterned mask on the spacer layer, wherein the first patterned mask includes a second opening that exposes a portion of the spacer layer on a bottom portion of the first opening; depositing a sacrificial material in the second opening; removing the first patterned mask; forming a line end cutting pattern by etching the sacrificial material; depositing a protective layer covering the line end cutting pattern; trimming the line end cutting pattern and the protective layer; patterning the spacer layer so that a portion of the spacer layer remains on the sidewalls of the core shaft layer; and forming a second patterned mask by removing the core shaft layer while retaining the etched line end cutting pattern and the patterned spacer layer.

[0061] According to an embodiment of the present invention, a method for manufacturing a semiconductor device includes: patterning a plurality of spindles on a mask layer; depositing a spacer layer on and along the sidewalls of the plurality of spindles; forming a patterned mask on the spacer layer, the patterned mask including an opening exposing a portion of the spacer layer between adjacent ones of the plurality of spindles; depositing a sacrificial material in the opening on the patterned mask; removing the patterned mask to thereby form a line end cut pattern on the spacer layer; depositing a protective layer covering the sacrificial material and the spacer layer; trimming the protective layer while retaining the spacer layer covered by the protective layer; trimming the protective layer while retaining the spacer layer covered by the protective layer; patterning the spacer layer to expose the plurality of spindles; removing the plurality of spindles; and patterning the mask layer using the sidewall portion of the spacer layer and the reduced line end cut pattern as an etching mask.

[0062] The foregoing summarizes the components of several embodiments so that those skilled in the art can better understand the aspects of the present disclosure. Those skilled in the art will appreciate that they can readily use the present disclosure as a basis for designing or modifying other processes and structures for achieving the same purposes and / or achieving the same advantages of the embodiments introduced herein. Those skilled in the art will also recognize that such equivalent constructions do not depart from the spirit and scope of the present disclosure, and that various changes, substitutions, and modifications may be made herein without departing from the spirit and scope of the present disclosure.

[0063] Explanation of symbols

[0064] 100 Semiconductor devices

[0065] 102 Target layer

[0066] 104 Substrate

[0067] 106 Anti-reflective coating

[0068] 108 mask layer

[0069] 110 Dielectric layer

[0070] 112 Mandrel Layer

[0071] 114 bottom layer

[0072] 116 Middle Layer

[0073] 118 top layer

[0074] 120 Photoresist stack

[0075] 122 Opening

[0076] 124 Spindle

[0077] 126 Spacer layer

[0078] 127 Spacer layer

[0079] 128 bottom layer

[0080] 130 Middle Layer

[0081] 132 Top Layer

[0082] 134 Photoresist stack

[0083] 136 Opening

[0084] 136A Opening

[0085] 136B Open

[0086] 136C Open

[0087] 138 Sacrificial Materials

[0088] 139 Gap

[0089] 140 Opening

[0090] 142 Lining

[0091] 144 Conductive materials

[0092] 146 Conductive wires / conductive vias

[0093] 148 Wire end cutting pattern

[0094] 148A Wire End Cutting Pattern

[0095] 148B Wire End Cutting Pattern

[0096] 148C Wire End Cutting Pattern

[0097] 150 Wire end cutting part

[0098] 152 protective layer

[0099] Fh Ring

[0100] Fv Arrow

[0101] H1 Height

[0102] H2 Height

[0103] H3 Height

[0104] W1 Width

[0105] W2 Width

[0106] W3 Width

Claims

1. A method for manufacturing a semiconductor device, comprising: forming a first mandrel and a second mandrel on the mask layer; depositing a spacer layer over the first mandrel and the second mandrel; forming a line end cutting pattern between the first mandrel and the second mandrel and on the spacer layer; depositing a protective layer on the line end cutting pattern; etching the protective layer; reducing the width of the line end cutting pattern; etching a first horizontal portion of the spacer layer using the reduced line end cut pattern as an etching mask; removing the first mandrel and the second mandrel; and The mask layer is patterned using the etched spacer layer and the reduced line end cut pattern as an etch mask.

2. The method according to claim 1, wherein forming the wire end cutting pattern comprises: forming a patterned mask over the spacer layer, the patterned mask comprising openings exposing portions of the spacer layer between the first mandrel and the second mandrel; depositing a sacrificial material in the opening; and An additional portion of the sacrificial material is removed over the opening using a planarization operation. 3 . The method according to claim 1 , wherein the etching of the protection layer is performed by the same operation as reducing the width of the line end cut pattern. The method of claim 1 , wherein reducing the width of the wire end cutting pattern also reduces the height of the wire end cutting pattern. 5 . The method of claim 1 , wherein depositing a protection layer over the line end cutting pattern comprises depositing the protection layer to cover an upper surface and sidewalls of the spacer layer. 6 . The method of claim 1 , wherein etching the protection layer on the line end cut pattern comprises etching a sidewall of the protection layer at a first etching rate greater than a second etching rate on a horizontal portion of the protection layer.

7. The method of claim 1, wherein the protective layer comprises at least one of: a nitride, an oxide, and a carbon-based material. 8 . The method of claim 1 , wherein the wire end cutting pattern comprises titanium oxide, tantalum oxide, silicon oxide, silicon nitride, silicon carbide, or a combination thereof.

9. The method of claim 1, wherein the line end cutting pattern comprises at least one guide pillar, the method further comprising patterning a target layer using the patterned mask layer and forming conductive line segments in the target layer, wherein a width of the guide pillar corresponds to a pitch of the segments. 10 . The method of claim 1 , wherein the line end cutting pattern masks a second horizontal portion of the spacer layer while removing the first horizontal portion of the spacer layer.

11. A method for manufacturing a semiconductor device, comprising: patterning a first opening in the mandrel layer; depositing a spacer layer over and along sidewalls of the first opening; forming a first patterned mask over the spacer layer, wherein the first patterned mask includes a second opening exposing a portion of the spacer layer on a bottom portion of the first opening; depositing a sacrificial material in the second opening; removing the first patterned mask; forming a line end cutting pattern by etching the sacrificial material; depositing a protective layer so as to cover the wire end cutting pattern; Modifying the wire end cutting pattern and the protective layer; patterning the spacer layer so that portions of the spacer layer remain on sidewalls of the mandrel layer; and A second patterned mask is formed by removing the mandrel layer while leaving behind the modified line end cut pattern and the patterned spacer layer. 12 . The method of claim 11 , wherein the sacrificial material differs from the spacer layer by an etch selectivity ratio of between 3 and 10. 13 . The method of claim 11 , wherein the protection layer differs from the spacer layer by an etch selectivity ratio between 3 and 10. The method of claim 11 , wherein the sacrificial material is an inorganic material. 15 . The method of claim 11 , wherein the line end cut pattern shields a bottom portion of the spacer layer in the first opening from being etched while the spacer layer is patterned.

16. The method of claim 11, wherein forming a first patterned mask over the spacer layer comprises: depositing a photoresist stack over the spacer layer; and The second opening is formed through the photoresist stack.

17. The method of claim 16, wherein depositing a photoresist stack over the spacer layer comprises: depositing a bottom layer over the spacer layer; depositing an intermediate layer over the base layer; depositing an upper layer over the intermediate layer; and Prior to depositing the sacrificial material in the second opening, the upper layer is removed.

18. A method for manufacturing a semiconductor device, comprising: patterning a plurality of mandrels over the mask layer; depositing a spacer layer over and along sidewalls of the plurality of mandrels; forming a patterned mask over the spacer layer, the patterned mask comprising openings exposing portions of the spacer layer between adjacent ones of the plurality of mandrels; depositing a sacrificial material in the opening over the patterned mask; removing the patterned mask, thereby forming a line end cut pattern on the spacer layer; depositing a protective layer to cover the sacrificial material and the spacer layer; modifying the protective layer while leaving the spacer layer covered by the protective layer; reducing the width of the line end cutting pattern; patterning the spacer layer to expose the plurality of mandrels; removing the plurality of mandrels; and The mask layer is patterned using sidewall portions of the spacer layer and the reduced line end cut pattern as an etch mask.

19. The method of claim 18, further comprising removing the protective layer before patterning the spacer layer.

20. The method of claim 18, wherein depositing the sacrificial material comprises depositing the sacrificial material at a temperature of 200°C or less.

21. A method for manufacturing a semiconductor device, comprising: forming a first mandrel and a second mandrel on the mask layer; depositing a spacer layer over the first mandrel and the second mandrel; forming a line end cutting pattern between the first mandrel and the second mandrel and on the spacer layer; depositing a protective layer on the line end cutting pattern; etching the protective layer and exposing an upper portion of the line end cutting pattern; reducing the width of the line end cutting pattern; etching the spacer layer to expose the first mandrel and the second mandrel; and The mask layer is patterned using the etched spacer layer and the reduced line end cut pattern as an etching mask.

22. The method of claim 21, wherein forming the wire end cutting pattern comprises: forming a patterned mask over the spacer layer, the patterned mask comprising openings exposing portions of the spacer layer between the first mandrel and the second mandrel; depositing a sacrificial material in the opening; and An additional portion of the sacrificial material is removed over the opening using a planarization operation. 23 . The method of claim 21 , wherein the etching of the protection layer is performed by the same operation as reducing the width of the line end cutting pattern.

24. The method of claim 21, wherein said reducing the width of the wire end cut pattern also reduces the height of the wire end cut pattern. 25 . The method of claim 21 , wherein depositing a protection layer over the line end cutting pattern comprises depositing the protection layer to cover an upper surface and sidewalls of the spacer layer. 26 . The method of claim 21 , wherein etching the protection layer comprises etching a sidewall of the protection layer at a first etch rate, and etching a horizontal portion of the protection layer at a second etch rate that is less than the first etch rate.

27. The method of claim 21, wherein the protective layer comprises at least one of: a nitride, an oxide, and a carbon-based material.

28. The method of claim 21, wherein the wire end cutting pattern comprises titanium oxide, tantalum oxide, silicon oxide, silicon nitride, silicon carbide, or a combination thereof.

29. The method of claim 21, wherein the line end cutting pattern comprises at least one guide pillar, the method further comprising patterning a target layer using the patterned mask layer and forming segments of a conductive line in the target layer, wherein a width of the guide pillar corresponds to a pitch of the segments.

30. The method of claim 21, wherein the line end cut pattern shields a second horizontal portion of the spacer layer from being etched while the spacer layer is etched.

31. A method of manufacturing a semiconductor device, comprising: providing a mandrel layer having a first opening; depositing a spacer layer over and along sidewalls of the first opening; forming a first patterned mask over the spacer layer, wherein the first patterned mask includes a second opening exposing a first portion of the spacer layer; filling the second opening with a sacrificial material; planarizing the sacrificial material and the first patterned mask; removing the planarized first patterned mask while leaving the sacrificial material in the second opening to form a line end cut pattern; depositing a protective layer to cover the line end cutting pattern; etching a lateral portion of the protection layer to expose a sidewall of the spacer layer and remove a certain thickness of the line end cutting pattern; completely removing the protective layer; patterning the spacer layer so that a second portion of the spacer layer remains on a sidewall of the mandrel layer; and A second patterned mask is formed by removing the mandrel layer while leaving the line end cut pattern and the patterned spacer layer.

32. The method of claim 31 , wherein the sacrificial material differs from the spacer layer by an etch selectivity ratio of between 3 and 10.

33. The method of claim 31, wherein the protection layer differs from the spacer layer by an etch selectivity ratio between 3 and 10.

34. The method of claim 31 , wherein the sacrificial material is an inorganic material.

35. The method of claim 31, wherein the line end cut pattern shields a bottom portion of the spacer layer in the first opening from being etched while the spacer layer is patterned.

36. The method of claim 31 , wherein forming a first patterned mask over the spacer layer comprises: depositing a photoresist stack over the spacer layer; and The second opening is formed through the photoresist stack.

37. The method of claim 36, wherein depositing a photoresist stack over the spacer layer comprises: depositing a bottom layer over the spacer layer; depositing an intermediate layer over the base layer; depositing an upper layer over the intermediate layer; and Prior to depositing the sacrificial material in the second opening, the upper layer is removed.

38. A method of manufacturing a semiconductor device, comprising: patterning a plurality of mandrels over the mask layer; depositing a spacer layer over and along sidewalls of the plurality of mandrels; forming a patterned mask over the spacer layer, the patterned mask comprising openings exposing portions of the spacer layer between two adjacent mandrels; depositing a sacrificial material in the opening over the patterned mask; removing the patterned mask, thereby forming a line end cut pattern on the spacer layer; depositing a protective layer to cover the sacrificial material and the spacer layer; performing isotropic etching on the protection layer to expose the line end cutting pattern; etching the sidewalls of the line end cutting pattern; patterning the spacer layer to expose the plurality of mandrels; removing the plurality of mandrels; and The mask layer is patterned using sidewall portions of the spacer layer and the etched line end cut patterns as an etching mask.

39. The method of claim 38, further comprising removing the protective layer before patterning the spacer layer.

40. The method of claim 38, wherein depositing the sacrificial material comprises depositing the sacrificial material at or below 200°C.

Citation Information

Patent Citations

  • Mask patterns with spacers for pitch multiplication and methods of forming the same

    CN101297391A

  • Semiconductor circuit structure and process of making the same

    CN103367258A