Glass substrate heterojunction solar cell and preparation method thereof
By using a heterojunction structure with a combination of glass substrate and specific materials in a heterojunction solar cell, the problem of unreasonable combination of conductive oxide and hole selection layer materials is solved, and the light utilization rate and cell efficiency of solar cells are improved , especially by using molybdenum-doped indium oxide materials, the cost-effective improvement is achieved.
Patent Information
- Application Number
- CN201910331284.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-04-23
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2039-04-23
Smart Images

Figure CN109980020B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and more particularly to a glass substrate heterojunction solar cell and a preparation method thereof. Background Art
[0002] With the emergence of the fossil energy crisis, humans began to seek new energy sources to replace traditional fossil energy sources. In the field of new energy, the solar energy field currently has the greatest advantages. Solar energy is clean, safe to use, and easy to convert and utilize. The development and utilization of solar energy has accelerated the development of solar cell technology. Currently, mature solar cell technologies on the market include single-crystal silicon and polycrystalline silicon solar cell technologies. Due to the pollution caused by the casting process of silicon, the large-scale application of solar cells in the future will limit the development of crystalline silicon cells to a certain extent. Amorphous silicon thin film batteries have begun to appear. Amorphous silicon thin film has the advantages of less consumables, relatively low manufacturing costs, and relatively little environmental pollution. It has become a research hotspot for scientific research institutes and photovoltaic companies around the world.
[0003] Existing heterojunction solar cells form a stacked structure by using a conductive oxide and a hole selection layer to reduce the reflection of incident light, thereby improving the cell efficiency and short-circuit current. However, the material combination of the conductive oxide and the hole selection layer is unreasonable, and the optical band gap difference is relatively large, resulting in a relatively weak response in the short-wave band of visible light, poor lateral transport capacity of carriers, low light utilization, and the cell efficiency and short-circuit current need to be improved.
[0004] Therefore, how to solve the above technical problems is of great practical significance to those skilled in the art. Summary of the invention
[0005] The purpose of the present invention is to solve the technical problems that the material combination of the conductive oxide and the hole selection layer in the existing heterojunction solar cell is unreasonable, the optical band gap is relatively large, resulting in a relatively weak response in the short-wave band of visible light, poor lateral transport capacity of carriers, and low light utilization. The present invention provides a glass substrate heterojunction solar cell and a preparation method thereof.
[0006] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:
[0007] A glass substrate heterojunction solar cell comprises a glass substrate, a transparent conductive oxide layer, a hole selection layer, an intrinsic amorphous silicon layer and an n-type doped amorphous silicon layer which are sequentially connected from bottom to top, the hole selection layer is a molybdenum oxide film, and the transparent conductive oxide layer comprises any one of molybdenum-doped indium oxide, titanium-doped indium oxide and tungsten-doped indium oxide.
[0008] Furthermore, a metal gate line anode layer is disposed on the top surface of the transparent conductive oxide layer, and the thickness of the metal gate line anode layer is 240nm. A metal gate line cathode layer is disposed on the top surface of the n-type doped amorphous silicon layer, and the thickness of the metal gate line cathode layer is 50nm.
[0009] Furthermore, the material of the metal gate line positive electrode layer and the metal gate line negative electrode layer are any one of Cu, Cu alloy, Ag, and Ag alloy, and the Cu alloy is an alloy formed by Cu and any one of Mo, W, Ti, Ni, Al, Mg, Ta, Sn, and Ag.
[0010] Furthermore, the thickness of the transparent conductive oxide layer is 50-120 nm.
[0011] Furthermore, the thickness of the hole selection layer is 80-150 nm.
[0012] Furthermore, the thickness of the intrinsic amorphous silicon layer is 5-10 nm.
[0013] Furthermore, the thickness of the n-type doped amorphous silicon layer is 30-100 nm.
[0014] Furthermore, the light transmittance of the glass substrate is 90%-95%, and the thickness of the glass substrate is 3mm-5mm.
[0015] A method for preparing a glass substrate heterojunction solar cell comprises the following steps:
[0016] S1: Select a glass substrate with a light transmittance of 90%-95%, clean the surface of the glass substrate with ethanol, and blow dry with nitrogen;
[0017] S2: on the upper surface of the glass substrate, a transparent conductive oxide layer is prepared using a magnetron sputtering coater;
[0018] S3: On the upper surface of the transparent conductive oxide layer, a mask is used to leave a space for preparing the metal grid line positive electrode layer, and then a magnetron sputtering coating machine is used to prepare a hole selection layer on the upper surface of the transparent conductive oxide layer. The gas for magnetron sputtering is oxygen, and the purity specification of oxygen is 99.9%;
[0019] S4: using a mask plate to cover the hole selection layer, and preparing an intrinsic amorphous silicon layer on the upper surface of the hole selection layer by plasma enhanced chemical vapor deposition, using silane as the gas;
[0020] S5: a mask is placed on the intrinsic amorphous silicon layer to cover the layer, and an n-type doped amorphous silicon layer is prepared on the upper surface of the intrinsic amorphous silicon layer by plasma enhanced chemical vapor deposition, using phosphine and silane as the gases;
[0021] S6: Use a mask plate to cover the n-type doped amorphous silicon layer, use a vacuum coating machine to prepare a metal gate line negative electrode layer on the upper surface of the n-type doped amorphous silicon layer, and finally use a vacuum coating machine to prepare a metal gate line positive electrode layer in the empty position on the upper surface of the transparent conductive oxide layer.
[0022] The beneficial effects of the present invention are as follows:
[0023] 1. The hole selection layer is a molybdenum oxide film with an optical band gap of 3.6-3.9ev. The transparent conductive oxide layer includes any one of molybdenum-doped indium oxide, titanium-doped indium oxide, and tungsten-doped indium oxide. The optical band gaps of molybdenum-doped indium oxide, titanium-doped indium oxide, and tungsten-doped indium oxide are all 3.8-3.9. The hole selection layer and the transparent conductive oxide layer form a stacked combination with a similar optical band gap. After superposition, the luminous flux of the incident light is increased, the response to the short-wave band of visible light is relatively strong, the photogenerated current density is increased, the lateral transport capacity of carriers is enhanced, and the utilization rate of light is improved, thereby improving the battery efficiency and short-circuit current. Among them, the preparation cost of molybdenum-doped indium oxide is relatively cheap, and the effect is better than the other two materials, which is suitable for promotion.
[0024] 2. The thickness of the transparent conductive oxide layer is 50-120nm, and the thickness of the hole selection layer is 80-150nm. The stacking combination has a better effect. If it is too thick, the gain is not large and it also wastes costs. The thickness of the intrinsic amorphous silicon layer is 5-10nm. The function of the intrinsic amorphous silicon layer is to passivate the defects of the subsequent n-type doped amorphous silicon layer. If the glass substrate is too thick, it is not conducive to the assembly of the battery cell. If the glass substrate is too thin, it will lead to an increase in the fragmentation rate. Therefore, the thickness of the glass substrate is 3mm-5mm to meet the use conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a structural schematic diagram of a glass substrate heterojunction solar cell of the present invention.
[0026] Figure numerals: 1-glass substrate, 2-transparent conductive oxide layer, 3-hole selection layer, 4-intrinsic amorphous silicon layer, 5-n-type doped amorphous silicon layer, 6-metal gate line cathode layer, 7-metal gate line anode layer. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention described and shown in the drawings herein can be arranged and designed in various different configurations.
[0028] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.
[0029] It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0030] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0031] Example 1
[0032] like Figure 1 As shown, this embodiment provides a glass substrate heterojunction solar cell, comprising a glass substrate 1, a transparent conductive oxide layer 2, a hole selection layer 3, an intrinsic amorphous silicon layer 4 and an n-type doped amorphous silicon layer 5 connected in sequence from bottom to top, the hole selection layer 3 is a molybdenum oxide thin film, and the transparent conductive oxide layer 2 includes any one of molybdenum-doped indium oxide, titanium-doped indium oxide, and tungsten-doped indium oxide.
[0033] In this embodiment, the hole selection layer is a molybdenum oxide film with an optical band gap of 3.6-3.9 eV. The transparent conductive oxide layer includes any one of molybdenum-doped indium oxide, titanium-doped indium oxide, and tungsten-doped indium oxide. The optical band gaps of molybdenum-doped indium oxide, titanium-doped indium oxide, and tungsten-doped indium oxide are all 3.8-3.9. The hole selection layer and the transparent conductive oxide layer form a stacked combination with a similar optical band gap. After being superimposed on each other, the luminous flux of the incident light is increased, the response to the short-wave band of visible light is relatively strong, the photogenerated current density is increased, the lateral transport capacity of carriers is enhanced, and the utilization rate of light is improved, thereby improving the battery efficiency and short-circuit current. Among them, the preparation cost of molybdenum-doped indium oxide is relatively cheap, and the effect is better than the other two materials, which is suitable for promotion.
[0034] Example 2
[0035] like Figure 1As shown, this embodiment is further optimized on the basis of Embodiment 1. Specifically, a metal gate line positive electrode layer 7 is further provided on the top surface of the transparent conductive oxide layer 2. The thickness of the metal gate line positive electrode layer 7 is 240 nm. A metal gate line negative electrode layer 6 is provided on the top surface of the n-type doped amorphous silicon layer 5. The thickness of the metal gate line negative electrode layer 6 is 50 nm. The thickness is reasonably designed to meet the use requirements. The materials of the metal gate line positive electrode layer 7 and the metal gate line negative electrode layer 6 are any one of Cu, Cu alloy, Ag, and Ag alloy. The Cu alloy is an alloy formed by Cu and any one of Mo, W, Ti, Ni, Al, Mg, Ta, Sn, and Ag. There are various materials to choose from.
[0036] Example 3
[0037] like Figure 1 As shown, this embodiment is further optimized on the basis of embodiment 1. Specifically, the thickness of the transparent conductive oxide layer 2 is 50-120nm, the thickness of the hole selection layer 3 is 80-150nm, preferably 80nm, the stacking combination effect is better, too thick gain is not large, and it also wastes cost, the thickness of the intrinsic amorphous silicon layer 4 is 5-10nm, preferably 5nm, the role of the intrinsic amorphous silicon layer 4 is to passivate the defects of the subsequent n-type doped amorphous silicon layer 5, the thickness of the n-type doped amorphous silicon layer 5 is 30-100nm, preferably 30nm, the transmittance of the glass substrate 1 is 90%-95%, the thickness of the glass substrate 1 is 3mm-5mm, the glass substrate 1 is too thick, which is not conducive to the assembly of the battery cell, and the glass substrate 1 is too thin, which will lead to an increase in the fragmentation rate. Therefore, the thickness of the glass substrate 1 is 3mm-5mm to meet the use conditions.
[0038] Example 4
[0039] like Figure 1 As shown, this embodiment provides a method for preparing a glass substrate heterojunction solar cell, comprising the following steps:
[0040] S1: Select a glass substrate 1 with a light transmittance of 90%-95%, clean the surface of the glass substrate 1 with ethanol, and blow dry with nitrogen;
[0041] S2: on the upper surface of the glass substrate 1, a transparent conductive oxide layer 2 is prepared by using a magnetron sputtering coating machine;
[0042] S3: On the upper surface of the transparent conductive oxide layer 2, a mask is used to leave a space for preparing the metal grid line positive electrode layer 7, and then a magnetron sputtering coating machine is used to prepare a hole selection layer 3 on the upper surface of the transparent conductive oxide layer 2. The gas for magnetron sputtering is oxygen, and the purity specification of oxygen is 99.9%;
[0043] S4: using a mask to cover the hole selection layer 3, and preparing an intrinsic amorphous silicon layer 4 on the upper surface of the hole selection layer 3 by plasma enhanced chemical vapor deposition, using silane as the gas;
[0044] S5: Covering the intrinsic amorphous silicon layer 4 with a mask, preparing an n-type doped amorphous silicon layer 5 on the upper surface of the intrinsic amorphous silicon layer 4 by plasma enhanced chemical vapor deposition, using phosphine and silane as the gases;
[0045] S6: Use a mask plate to cover the n-type doped amorphous silicon layer 5, use a vacuum coating machine to prepare a metal gate line negative electrode layer 6 on the upper surface of the n-type doped amorphous silicon layer 5, and finally use a vacuum coating machine to prepare a metal gate line positive electrode layer 7 in the empty position on the upper surface of the transparent conductive oxide layer 2.
[0046] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. The patent protection scope of the present invention shall be based on the claims. All equivalent structural changes made using the contents of the description and drawings of the present invention should also be included in the protection scope of the present invention.
Claims
1. A glass substrate heterojunction solar cell, comprising a glass substrate (1), a transparent conductive oxide layer (2), a hole selection layer (3), an intrinsic amorphous silicon layer (4) and an n-type doped amorphous silicon layer (5) connected in sequence from bottom to top, characterized in that: The hole selection layer (3) is a molybdenum oxide film, and the transparent conductive oxide layer (2) is selected from any one of molybdenum-doped indium oxide, titanium-doped indium oxide, and tungsten-doped indium oxide; the thickness of the transparent conductive oxide layer (2) is 50-120nm, the thickness of the hole selection layer (3) is 80-150nm, the thickness of the intrinsic amorphous silicon layer (4) is 5-10nm, and the thickness of the n-type doped amorphous silicon layer (5) is 30-100nm.
2. A glass substrate heterojunction solar cell according to claim 1, characterized in that: A metal gate line positive electrode layer (7) is also arranged on the top surface of the transparent conductive oxide layer (2), and the thickness of the metal gate line positive electrode layer (7) is 240 nm. A metal gate line negative electrode layer (6) is arranged on the top surface of the n-type doped amorphous silicon layer (5), and the thickness of the metal gate line negative electrode layer (6) is 50 nm.
3. A glass substrate heterojunction solar cell according to claim 2, characterized in that: The material of the metal grid line positive electrode layer (7) and the metal grid line negative electrode layer (6) is any one of Cu, Cu alloy, Ag, and Ag alloy. The Cu alloy is an alloy formed by Cu and any one of Mo, W, Ti, Ni, Al, Mg, Ta, Sn, and Ag.
4. The glass substrate heterojunction solar cell according to claim 1, characterized in that: The light transmittance of the glass substrate (1) is 90%-95%, and the thickness of the glass substrate (1) is 3mm-5mm.
5. The method for preparing a glass substrate heterojunction solar cell according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1: Select a glass substrate (1) with a light transmittance of 90%-95%, clean the surface of the glass substrate (1) with ethanol, and blow dry with nitrogen; S2: on the upper surface of the glass substrate (1), a transparent conductive oxide layer (2) is prepared using a magnetron sputtering coating machine; S3: On the upper surface of the transparent conductive oxide layer (2), a mask is used to leave a space for preparing the metal grid line positive electrode layer (7), and then a magnetron sputtering coating machine is used to prepare a hole selection layer (3) on the upper surface of the transparent conductive oxide layer (2), and the gas used for magnetron sputtering is oxygen, and the purity specification of oxygen is 99.9%; S4: using a mask to cover the hole selection layer (3), and preparing an intrinsic amorphous silicon layer (4) on the upper surface of the hole selection layer (3) by plasma enhanced chemical vapor deposition, using silane as the gas; S5: using a mask plate to cover the intrinsic amorphous silicon layer (4), and using plasma enhanced chemical vapor deposition to prepare an n-type doped amorphous silicon layer (5) on the upper surface of the intrinsic amorphous silicon layer (4), using phosphine and silane as the gases; S6: A mask is used to cover the n-type doped amorphous silicon layer (5), and a metal gate line cathode layer (6) is prepared on the upper surface of the n-type doped amorphous silicon layer (5) using a vacuum coating machine. Finally, a metal gate line cathode layer (7) is prepared on the remaining position on the upper surface of the transparent conductive oxide layer (2) using a vacuum coating machine.