Quantum dots, method for manufacturing the same, electroluminescent device and display device

The cadmium-free quantum dots with a core-shell structure composed of zinc, tellurium, and selenium solve the problem that it is difficult to achieve improved photoluminescence properties in electroluminescent devices using cadmium-free quantum dots in existing technologies. This results in blue light emission, reduced FWHM, and improved external quantum efficiency, making them suitable for display devices, biolabeling, bioimaging, photodetectors, and solar cells.

CN110246987BActive Publication Date: 2024-11-01SAMSUNG ELECTRONICS CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN201910180460.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-03-09
Filing Date
2019-03-11
Publication Date
2024-11-01
Estimated Expiration
2039-03-11

AI Technical Summary

Technical Problem

Existing technologies struggle to develop cadmium-free quantum dots with improved photoluminescence properties, particularly those capable of emitting blue light, and it is difficult to achieve reduced FWHM, improved external quantum efficiency, and increased brightness in electroluminescent devices.

Method used

Cadmium-free quantum dots with a core-shell structure composed of zinc, tellurium, and selenium are formed by reacting them in an organic solvent at high temperature to create a semiconductor nanocrystal shell. This ensures that the quantum dots have a specific morphology and composition, including a shell composed of at least four protrusions and a gradient, and ensures that the size of the quantum dots is greater than or equal to 10 nanometers. This allows for their application in electroluminescent devices.

Benefits of technology

A cadmium-free quantum dot was used to emit blue light in an electroluminescent device with improved electroluminescence properties, having a half-width of less than or equal to about 40 nm, an external quantum efficiency greater than or equal to about 4%, and exhibiting improved quantum efficiency and brightness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110246987B_ABST
    Figure CN110246987B_ABST
Patent Text Reader

Abstract

The present invention relates to quantum dots, methods for making the same, electroluminescent devices and display devices. The quantum dots include: a core including a first semiconductor nanocrystalline material including zinc, tellurium and selenium; and a semiconductor nanocrystalline shell disposed on the core (e.g., directly disposed on the core) and including zinc, selenium and sulfur, wherein the quantum dots do not include cadmium, wherein the size of the quantum dots is greater than or equal to about 10 nanometers (nm) and the quantum dots include at least four protrusions. Methods for making the same and electronic devices including the same are also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2018-0028319 filed in the Korean Intellectual Property Office on March 9, 2018, and all rights arising therefrom, the entire contents of which are incorporated herein by reference. Technical Field

[0003] Quantum dots are disclosed. Background Art

[0004] Unlike bulk (body) materials, the physical properties (e.g., band gap and melting point) of nanoparticles can be controlled by changing the nanoparticle size. For example, semiconductor nanocrystal particles (also referred to as quantum dots) are crystalline materials with a size of several nanometers. Semiconductor nanocrystal particles have a relatively small size and a relatively large surface area per unit volume and present a quantum confinement (confinement) effect, and therefore can have properties different from bulk materials with the same composition. Quantum dots can absorb light from an excitation source to be excited, and can emit energy corresponding to the band gap of the quantum dots.

[0005] Quantum dots can be synthesized using vapor deposition methods such as metal organic chemical vapor deposition (MOCVD), molecular beam epitaxy (MBE), etc., wet chemical methods including adding precursor materials to organic solvents to grow crystals, etc. In the wet chemical methods, organic compounds such as ligands / coordinating solvents can be coordinated to (e.g., bonded to) the surface of nanocrystals to control crystal growth during crystal production.

[0006] To improve the photoluminescent properties of quantum dots, core-shell structures can be used, but core-shell quantum dots with improved properties may include cadmium-based materials. Therefore, there remains a need to develop cadmium-free semiconductor nanocrystal particles with desirable photoluminescent properties. Summary of the invention

[0007] Embodiments provide cadmium-free quantum dots capable of emitting blue light with improved electroluminescent properties.

[0008] Embodiments provide methods of manufacturing the quantum dots.

[0009] An embodiment provides an electronic device including the quantum dots.

[0010] In an embodiment, a quantum dot comprises: a core comprising a first semiconductor nanocrystalline material comprising zinc, tellurium, and selenium; and a semiconductor nanocrystalline shell disposed on the core (e.g., directly disposed on the core) and comprising zinc, selenium, and sulfur, wherein the quantum dot does not include cadmium, wherein the quantum dot has a size greater than or equal to approximately 10 nanometers (nm) and the quantum dot (e.g., the semiconductor nanocrystalline shell) has at least four protrusions.

[0011] In the quantum dots, a molar ratio of tellurium to selenium may be greater than or equal to about 0.001:1.

[0012] In the quantum dots, a molar ratio of tellurium to selenium may be less than or equal to about 0.05:1.

[0013] The quantum dots may have a maximum photoluminescence peak wavelength greater than or equal to about 450 nanometers (nm).

[0014] The maximum photoluminescence peak wavelength of the quantum dots may be less than or equal to about 470 nm.

[0015] The photoluminescence peak of the quantum dot may have a half width of less than or equal to about 50 nm, less than or equal to about 45 nm, less than or equal to about 40 nm, or less than or equal to about 36 nm.

[0016] The core may include ZnTe x Se 1-x , where x is greater than 0 and less than or equal to approximately 0.05.

[0017] The core may have a size greater than or equal to about 2 nm.

[0018] The semiconductor nanocrystal shell may have a gradient composition varying in a radial direction from the core toward the outermost surface of the quantum dot. In the semiconductor nanocrystal shell, the amount of sulfur may increase in a radial direction from the core toward the outermost surface of the quantum dot.

[0019] The semiconductor nanocrystal shell may include a first layer disposed directly on the core and an outer layer disposed on the first layer. The first layer may include a second semiconductor nanocrystal. The outer layer may include a third semiconductor nanocrystal having a composition different from that of the second semiconductor nanocrystal.

[0020] The second semiconductor nanocrystal may include zinc and selenium and optionally sulfur. The outer layer may include zinc and sulfur. The outermost layer of the semiconductor nanocrystal shell may not include selenium.

[0021] At least one of the protrusions of the quantum dot may have a length greater than or equal to about 1 nm, for example, greater than or equal to about 2 nm, or greater than or equal to about 3 nm.

[0022] In a two-dimensional image obtained from electron microscopy analysis, the area ratio of the quantum dot to the circumscribed circle may be greater than or equal to about 0.4: 1. The circumscribed circle may be the smallest circle that completely surrounds the quantum dot and the outermost point of the quantum dot may be on the circumference of the circumscribed circle.

[0023] In a two-dimensional image obtained from electron microscopy analysis, at least one of the protrusions of the quantum dot may have an edge point angle of less than about 70 degrees. The edge point angle may be the angle between two surfaces of the quantum dot that defines the at least one of the pods in the two-dimensional image.

[0024] The quantum dots may have a quantum efficiency of greater than or equal to about 70%.

[0025] The full width at half maximum (FWHM) of the photoluminescence peak of the quantum dots may be less than about 35 nm.

[0026] The quantum dots may have a size greater than or equal to about 11 nm.

[0027] In an embodiment, a method for manufacturing the aforementioned quantum dots comprises:

[0028] preparing a core comprising a first semiconductor nanocrystal comprising zinc, selenium, and tellurium; and

[0029] A selenium precursor, a sulfur precursor, or a combination thereof is reacted with a zinc precursor in an organic solvent in the presence of the core and an organic ligand in multiple steps at a temperature of about 300° C. or greater to form a semiconductor nanocrystal shell comprising zinc, selenium, and sulfur and having at least four protrusions.

[0030] In the core including the first semiconductor nanocrystal, a ratio of tellurium to selenium may be less than about 0.05:1.

[0031] The forming of the semiconductor nanocrystal shell may include reacting the zinc precursor with the selenium precursor and then reacting the zinc precursor with the sulfur precursor.

[0032] In an embodiment, the electroluminescent device may include: a first electrode and a second electrode facing each other and a light-emitting layer (ie, a quantum dot emission layer) disposed between the first electrode and the second electrode and including a plurality of quantum dots, and the plurality of quantum dots may include the aforementioned quantum dots.

[0033] The electroluminescent device may further include a charge auxiliary layer between the first electrode and the light emitting layer, between the second electrode and the light emitting layer, or between the first electrode and the light emitting layer and between the second electrode and the light emitting layer.

[0034] The charge assisting layer may include a charge injection layer, a charge transport layer, or a combination thereof.

[0035] The electroluminescent device may have a peak external quantum efficiency (EQE) greater than or equal to about 4%.

[0036] The electroluminescent device may be configured to emit light having a maximum emission peak wavelength between about 450 nm and about 460 nm and a half width less than or equal to about 25 nm.

[0037] In an embodiment, a display apparatus includes the aforementioned electroluminescent device.

[0038] Cadmium-free quantum dots capable of emitting blue light can be provided. The quantum dots can be applied to a variety of display devices, biomarkers (biosensors, bioimaging), light (electric) detectors, solar cells, hybrid composites, etc. When the quantum dots of the embodiments are applied to electroluminescent devices, they can present improved EQE and increased maximum (Max) brightness. The quantum dots of the embodiments can show reduced FWHM and increased quantum efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] The above and other advantages and features of the present disclosure will become more apparent by further describing exemplary embodiments thereof in detail with reference to the accompanying drawings, in which:

[0040] Figure 1 is a schematic diagram of a two-dimensional image (eg, obtained from electron microscopy analysis) of quantum dots according to an embodiment.

[0041] Figure 2 is a schematic cross-sectional view of a quantum dot (QD) LED device according to an embodiment.

[0042] Figure 3 is a schematic cross-sectional view of a QD LED device according to an embodiment.

[0043] Figure 4 is a schematic cross-sectional view of a QD LED device according to an embodiment.

[0044] Figure 5 is a transmission electron microscopy image of the quantum dots (QD2) synthesized in Example 1.

[0045] Figure 6 is a transmission electron microscopy image of the quantum dots (QD3) synthesized in Example 2.

[0046] Figure 7 is a transmission electron microscopy image of the quantum dots (QD1) synthesized in Comparative Example 1.

[0047] Figure 8Shown are diagrams illustrating transmission electron microscopy images of each of the quantum dots synthesized in Examples and their circumscribed circles.

[0048] Fig. 9 Shown are diagrams illustrating transmission electron microscopy images of each of the quantum dots synthesized in Examples and their edge dot angles.

[0049] Fig.10 A diagram illustrating a transmission electron microscopy image of each of quantum dots synthesized in Comparative Example and its edge dot angle is shown.

[0050] Fig.11 is the ratio of EQE (percentage (%)) to luminance (candela / square meter (Cd / m 2 )) shows the electroluminescent properties of the devices of Example 3, Example 4 and Comparative Example 2.

[0051] Fig.12 is the current density (mA / cm 2 ) versus voltage (V), which illustrates the electroluminescent properties of the devices of Example 3, Example 4 and Comparative Example 2. DETAILED DESCRIPTION

[0052] With reference to the following example embodiments together with the figures attached hereto, the advantages and characteristics of the present disclosure, and the methods for realizing them will become clear. However, the embodiments should not be interpreted as being limited to the embodiments set forth herein. Unless otherwise defined, all terms (including technical and scientific terms) used in the specification can be used with the meanings commonly understood by those skilled in the art of ordinary knowledge. The terms defined in the common dictionary cannot be interpreted ideally or exaggeratedly, unless clearly defined. In addition, unless explicitly described to the contrary, the word "including (comprising)" will be understood to mean including the elements described, but does not exclude any other elements.

[0053] Furthermore, the singular includes the plural unless otherwise mentioned.

[0054] In the drawings, the thickness of layers, films, panels, regions, etc., are exaggerated for clarity. The same reference numerals denote the same elements throughout the specification.

[0055] It will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, it can be directly on the other element or intervening elements may also be present. Conversely, when an element is referred to as being "directly on" another element, there are no intervening elements.

[0056] It will be understood that although the terms "first", "second", "third", etc. may be used herein to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings herein, the "first element", "component", "region", "layer" or "part" discussed below may be referred to as a second element, component, region, layer or part.

[0057] As used herein, "about" includes the stated value and means within an acceptable range of deviation for a particular value as determined by one of ordinary skill in the art taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean within one or more standard deviations of the stated value, or within ±10% or 5% of the stated value.

[0058] Exemplary embodiments are described herein with reference to cross-sectional views, which are schematic diagrams of idealized embodiments. Thus, deviations from the illustrated shapes as a result of, for example, manufacturing techniques and / or tolerances are expected. Therefore, the embodiments described herein should not be construed as being limited to the specific shapes of the regions as illustrated herein, but rather include deviations in shape caused by, for example, manufacturing. For example, a region illustrated or described as flat may typically have rough and / or nonlinear features. Moreover, the illustrated sharp corners may be rounded. Therefore, the regions illustrated in the figures are schematic in nature, and their shapes are not intended to illustrate the precise shapes of the regions and are not intended to limit the scope of the claims.

[0059] As used herein, when no definition is otherwise provided, "substituted" refers to a compound or moiety in which at least one of its hydrogen atoms is replaced by a substituent, wherein the substituent may be a C1-C30 alkyl, a C2-C30 alkenyl, a C2-C30 alkynyl, a C6-C30 aryl, a C7-C30 alkaryl, a C1-C30 alkoxyl, a C1-C30 heteroalkyl, a C3-C30 heteroalkaryl, a C3-C30 cycloalkyl, a C3-C15 cycloalkenyl, a C6-C30 cycloalkynyl, a C2-C30 heterocycloalkyl, a halogen (-F, -Cl, -Br or -I), a hydroxyl (-OH), a nitro (-NO 2 ), cyano (-CN), amino (-NRR', wherein R and R' are independently hydrogen or C1-C6 alkyl), azido (-N 3 ), amidino (-C(=NH)NH 2 ), hydrazino (-NHNH 2 ), hydrazine (=N(NH 2)), aldehyde group (-C(=O)H), carbamoyl group (-C(O)NH 2 ), thiol group (-SH), ester group (-C(=O)OR, wherein R is C1-C6 alkyl or C6-C12 aryl), carboxyl group (-COOH) or its salt (-C(=O)OM, wherein M is an organic or inorganic cation), sulfonic acid group (-SO 3 H) or its salt (-SO 3 M, where M is an organic or inorganic cation), a phosphate group (-PO 3 H 2 ) or its salt (-PO 3 MH or -PO 3 M 2 , wherein M is an organic or inorganic cation), or a combination thereof.

[0060] As used herein, a hydrocarbyl group refers to a group comprising carbon and hydrogen (e.g., an alkyl, alkenyl, alkynyl, or aryl group). The hydrocarbyl group may be a group having a monovalent or polyvalent valence formed by removing one or more hydrogen atoms from an alkane, an alkene, an alkyne, or an aromatic hydrocarbon. In the hydrocarbyl group, at least one methylene group may be replaced by an oxygen moiety, a carbonyl moiety, an ester moiety, -NH-, or a combination thereof.

[0061] As used herein, "alkyl" refers to a linear or branched saturated monovalent hydrocarbon group (methyl, ethyl, hexyl, etc.).

[0062] As used herein, "alkenyl" refers to a linear or branched monovalent hydrocarbon group having one or more carbon-carbon double bonds.

[0063] As used herein, "alkynyl" refers to a linear or branched monovalent hydrocarbon group having one or more carbon-carbon triple bonds.

[0064] As used herein, "aryl" refers to a group formed by removing at least one hydrogen from an aromatic hydrocarbon (eg, phenyl or naphthyl).

[0065] As used herein, "hetero" means that it includes one or more (eg, 1 to 3) heteroatoms of N, O, S, Si, P, or a combination thereof.

[0066] As used herein, "Group" refers to a Group of the Periodic Table.

[0067] Semiconductor nanocrystal particles (hereinafter, also referred to as quantum dots) can absorb light from an excitation source and can emit light corresponding to its energy band gap. The energy band gap of a quantum dot can vary depending on its size and composition. For example, as the size of the quantum dot increases, the quantum dot can have a narrower energy band gap and can display an increased luminescent wavelength. Semiconductor nanocrystals can be used as luminescent materials in a variety of fields such as display devices, energy devices, or bioluminescent devices.

[0068] Quantum dots having photoluminescent properties may include cadmium (Cd). Cadmium may cause environmental and / or health issues and is a restricted element in many countries under the Restriction of Hazardous Substances Directive (RoHS). Therefore, there remains a need to develop cadmium-free quantum dots with improved photoluminescent properties. For example, it may be advantageous to develop cadmium-free quantum dots that can emit blue light. In addition, there is a need to develop cadmium-free quantum dots that can display reduced FWHM, improved external quantum efficiency, and increased brightness in electroluminescent devices.

[0069] The quantum dot according to the embodiment has a structure and composition to be described below, and thus can emit light with a desired wavelength (eg, blue light) and improved properties in an electroluminescent device.

[0070] The quantum dots (e.g., quantum dots or multiple quantum dots) of the embodiments do not include cadmium. The quantum dots or cores of the embodiments may not include manganese, copper, or a combination thereof. The quantum dots of the embodiments include: a core including a first semiconductor nanocrystal including zinc, tellurium, and selenium; and a semiconductor nanocrystal shell disposed on at least a portion of the core and including zinc, selenium, and sulfur. The quantum dots (or multiple quantum dots) have a particle size (e.g., an average particle size) greater than or equal to about 10 nm and the semiconductor nanocrystal shell (on average) has at least four pods. In embodiments, the pods (or protrusions) may be protrusions that are separated from each other in a two-dimensional image of the quantum dots analyzed by electron microscopy (see Figure 1 ). As used herein, the word "pod" and the word "protrusion" are used interchangeably.

[0071] In the quantum dots of the embodiment, the molar ratio of tellurium to selenium may be greater than or equal to about 0.001:1. The molar ratio of tellurium to selenium may be less than or equal to about 0.05:1. The quantum dots of the embodiment may emit blue light. The blue light has a maximum luminescence peak in a wavelength range of greater than or equal to about 450 nm and less than or equal to about 470 nm. The maximum luminescence peak of the quantum dot may have a half width of less than or equal to about 41 nm, for example, about 40 nm.

[0072] In the core, the first semiconductor nanocrystal may include a limited amount of tellurium. The core may include ZnTe x Se 1-x , where x is greater than 0 and less than or equal to approximately 0.05.

[0073] For example, in the core or quantum dot of the embodiment, the amount of tellurium per 1 mole of selenium may be greater than or equal to about 0.001 mole, greater than or equal to about 0.005 mole, greater than or equal to about 0.006 mole, greater than or equal to about 0.007 mole, greater than or equal to about 0.008 mole, greater than or equal to about 0.009 mole, greater than or equal to about 0.01 mole, greater than or equal to about 0.02 mole, or greater than or equal to about 0.025 mole. In the core or in the quantum dot, the amount of tellurium relative to 1 mole of selenium may be less than or equal to about 0.053 mole, for example, less than or equal to about 0.05 mole, less than or equal to about 0.049 mole, less than or equal to about 0.048 mole, less than or equal to about 0.047 mole, less than or equal to about 0.046 mole, less than or equal to about 0.045 mole, less than or equal to about 0.044 mole, less than or equal to about 0.043 mole, less than or equal to about 0.042 mole, less than or equal to about 0.041 mole, less than or equal to about 0.04 mole, less than or equal to about 0.035 mole, less than or equal to about 0.03 mole, less than or equal to about 0.025 mole, or less than or equal to about 0.02 mole.

[0074] The core may have a size (average size) (e.g., diameter or average diameter) greater than or equal to about 2 nm, greater than or equal to about 3 nm, or greater than or equal to about 3.5 nm. The (average) size of the core may be less than or equal to about 5 nm, or less than or equal to about 4 nm.

[0075] The quantum dots of the embodiment have a semiconductor nanocrystal shell including zinc (Zn), selenium (Se) and sulfur (S) disposed on the core, wherein the quantum dots have a morphology (e.g., also referred to as a multi-pod structure) having (on average) at least four pods (e.g., greater than or equal to about 5 pods, or greater than or equal to about 6 pods) in a two-dimensional image such as obtained by electron microscopy analysis thereof. The (average) number of the pods may be less than or equal to about 15, such as less than or equal to about 10, less than or equal to about 9, less than or equal to about 8, less than or equal to about 7, or less than or equal to about 6.

[0076] Reference Figure 1, the quantum dots of the embodiment have 6 pods, but the embodiments are not limited thereto. The quantum dots of the embodiment may have valleys, i.e., spaces between adjacent pods. In the quantum dots of the embodiment, the number of valleys (or the lowest points of the valleys) may be greater than or equal to about 2, greater than or equal to about 3, greater than or equal to about 4. In the quantum dots of the embodiment, the number of valleys (or the lowest points of the valleys) may be less than or equal to about 10, less than or equal to about 9, less than or equal to about 8, less than or equal to about 7, less than or equal to about 6, or less than or equal to about 5.

[0077] The lowest point of the valley may be the point where two opposite sides of the cross section of two adjacent pods (or their extensions) meet in the two-dimensional image obtained from electron microscopy analysis. The lowest point of the valley may be located closer to the center of the quantum dot than the straight line connecting the vertices of the two adjacent pods. (See Figure 1 Line)

[0078] In a two-dimensional image obtained from electron microscopy analysis, at least one pod of the quantum dot may have an edge point angle a of less than about 70 degrees, such as 69 degrees, less than or equal to about 68 degrees, less than or equal to about 67 degrees, less than or equal to about 66 degrees, less than or equal to about 65 degrees, less than or equal to about 64 degrees, less than or equal to about 63 degrees, less than or equal to about 62 degrees, less than or equal to about 61 degrees, or less than or equal to about 60 degrees. The angle may be from about 44 degrees to about 68 degrees. The edge point angle of the quantum dot may be the angle formed by two opposite sides of the cross-section of two adjacent pods (or their extensions). The edge point angle may be the angle between the two surfaces of the quantum dot that define the pod in the two-dimensional image. (See Figure 1 , angle a)

[0079] At least one of the pods of the quantum dots may have a (e.g., protruding) length (e.g., as determined by a two-dimensional image analyzed by electron microscopy) greater than or equal to about 0.5 nm, such as greater than or equal to 1 nm, greater than or equal to about 2 nm, or greater than or equal to about 3 nm, greater than or equal to about 4 nm, or greater than or equal to about 5 nm. The length of at least one of the pods may be less than or equal to about 20 nm, less than or equal to about 20 nm, less than or equal to about 15 nm, less than or equal to about 10 nm, or less than or equal to about 6 nm. The length of the pod may be determined by electron microscopy analysis. For example, the length of the pod (protrusion) may be measured as the vertical distance (e.g., height) from an edge point to a straight line connecting the two lowest points of a valley adjacent to the edge point.

[0080] In the two-dimensional image of the quantum dot obtained from electron microscopy analysis, the area ratio of the quantum dot relative to the circumscribed circle may be greater than or equal to about 0.4:1, for example, greater than or equal to about 0.5:1, greater than or equal to about 0.51:1, greater than or equal to about 0.52:1, or greater than or equal to about 0.53:1. The circumscribed circle may be a circle whose diameter is the maximum length of a straight line connecting (e.g., two opposite) vertices of the pod, for example, a circle that includes all points of the two-dimensional image of the quantum dot obtained from its electron microscopy analysis and has the smallest diameter. The circumscribed circle may be the smallest circle that completely surrounds the quantum dot, wherein the outermost point of the quantum dot is on the circumference of the circumscribed circle. (See Figure 1 and Figure 8 )

[0081] When applied to electroluminescent devices, quantum dots of embodiments having the aforementioned features of morphology, size, etc. may exhibit improved properties compared to quantum dots not having the aforementioned features such as size and morphology (e.g., quantum dots having substantially round shapes or having no protrusions or valleys).

[0082] In an embodiment, the semiconductor nanocrystal shell may have a gradient composition that varies in a radial direction (eg, from the core).In the semiconductor nanocrystal shell, the amount of sulfur may increase toward the surface of the quantum dot.

[0083] In an embodiment, the semiconductor nanocrystal shell may include at least two layers, wherein adjacent layers may have different compositions. In an embodiment, the semiconductor nanocrystal shell may include a first layer directly disposed on the core and at least one outer layer (e.g., a second layer or a third layer) disposed on or above the first layer. The first layer may include a second semiconductor nanocrystal. The outer layer (e.g., the second layer or the third layer above the second layer) may include a third semiconductor nanocrystal having a composition different from that of the second semiconductor nanocrystal.

[0084] The second semiconductor nanocrystals may include zinc, selenium and optionally sulfur. The semiconductor nanocrystals of the outer layer may include zinc and sulfur and optionally selenium. The outermost layer of the quantum dot may include semiconductor nanocrystals composed of zinc and sulfur.

[0085] The outer layer of the semiconductor nanocrystal shell may include a second layer and a third layer, the second layer including a third semiconductor nanocrystal including zinc and selenium and optionally sulfur, and the third layer including a fourth semiconductor nanocrystal including zinc and sulfur. The third layer may be the outermost layer.

[0086] The fourth semiconductor nanocrystal may have a band gap greater than the second semiconductor nanocrystal and the third semiconductor nanocrystal. In an embodiment, the second semiconductor nanocrystal may include ZnSe, ZnSeS, or a combination thereof. The third semiconductor nanocrystal may include ZnSeS, ZnS, or a combination thereof. The fourth semiconductor nanocrystal may include ZnS (or be composed of ZnS).

[0087] In the quantum dots of the embodiment, the molar ratio of tellurium to selenium may be less than or equal to about 0.1:1, less than or equal to about 0.05:1, less than or equal to about 0.049:1, less than or equal to about 0.048:1, less than or equal to about 0.047:1, less than or equal to about 0.046:1, less than or equal to about 0.045:1, less than or equal to about 0.044:1, less than or equal to about 0.043:1, less than or equal to about 0.042:1, less than or equal to about 0.041:1, less than or equal to about 0.04:1, less than or equal to about 0.035:1, or less than or equal to about 0.03:1. In the quantum dots of the embodiment, the molar ratio of tellurium to selenium may be greater than or equal to about 0.0001:1, greater than or equal to about 0.005:1, or greater than or equal to about 0.01:1. In the quantum dots, the amounts of each component can be measured and confirmed via a suitable analytical tool such as inductively coupled plasma atomic emission spectrometry (ICP-AES) and the like.

[0088] In an embodiment, the quantum dots may have a predetermined molar ratio of tellurium to zinc. In an embodiment, the quantum dots may have a predetermined molar ratio of sulfur to selenium. The quantum dots of an embodiment may have a predetermined molar ratio of the sum of sulfur and selenium to zinc. In an embodiment, the quantum dots may have a predetermined molar ratio of sulfur to zinc. In an embodiment, the quantum dots may have a predetermined molar ratio of selenium to zinc.

[0089] In the quantum dots of the embodiment, the molar ratio of tellurium to zinc may be less than 0.01: 1, for example, less than or equal to about 0.009: 1, less than or equal to about 0.008: 1, or less than or equal to about 0.007: 1. The molar ratio of tellurium to zinc may be greater than or equal to about 0.001: 1, for example, greater than or equal to about 0.002: 1, greater than or equal to about 0.003: 1, or greater than or equal to about 0.004: 1.

[0090] In the quantum dots of the embodiment, the molar ratio of selenium to sulfur may be greater than or equal to about 0.3: 1, for example, greater than or equal to about 0.4: 1, or greater than or equal to about 0.5: 1. In the quantum dots of the embodiment, the molar ratio of selenium to sulfur may be less than or equal to about 1: 1, for example, less than or equal to about 0.9: 1, or less than or equal to about 0.8: 1.

[0091] In the quantum dots of the embodiment, the molar ratio of sulfur to Zn may be greater than or equal to about 0.3: 1, greater than or equal to about 0.4: 1, greater than or equal to about 0.49: 1, or greater than or equal to about 0.5: 1. In the quantum dots of the embodiment, the molar ratio of sulfur to Zn may be less than or equal to about 0.9: 1.

[0092] In the quantum dots of the embodiment, the molar ratio of selenium to Zn may be greater than or equal to about 0.1: 1. In the quantum dots of the embodiment, the molar ratio of selenium to Zn may be less than or equal to about 0.47: 1, for example, less than or equal to about 0.45: 1, less than or equal to about 0.4: 1, or less than or equal to about 0.39: 1.

[0093] The quantum dots of the embodiments may have a size (e.g., average size) greater than or equal to about 10 nm, for example, greater than or equal to about 11 nm, or greater than or equal to about 15 nm. The (average) size of the quantum dots may be less than or equal to about 50 nm, for example, less than or equal to about 45 nm, less than or equal to about 40 nm, less than or equal to about 35 nm, less than or equal to about 30 nm, less than or equal to about 29 nm, less than or equal to about 28 nm, less than or equal to about 27 nm, or less than or equal to about 26 nm. The size (or average size) of the quantum dots may be determined by a two-dimensional image obtained by electron microscopy analysis (e.g., TEM analysis). In an embodiment, the size (or average size) of the quantum dots may be the diameter of a circumscribed circle.

[0094] The quantum dots of the embodiments may emit blue light having a maximum photoluminescence peak at a wavelength of about 450 nm or more, for example, about 451 nm or more, about 455 nm or more and about 470 nm or less (for example, about 470 nm or less, about 465 nm or less, or about 460 nm or less). The blue light may have a maximum emission peak wavelength of about 450 nm to about 460 nm.

[0095] The maximum (photoluminescence) peak may have a half width (FWHM) of less than or equal to about 40 nm, less than or equal to about 39 nm, less than or equal to about 38 nm, less than or equal to about 37 nm, less than or equal to about 36 nm, less than or equal to about 35 nm, less than or equal to about 34 nm, less than or equal to about 33 nm, less than or equal to about 32 nm, less than or equal to about 31 nm, less than or equal to about 30 nm, less than or equal to about 29 nm, less than or equal to about 28 nm, or less than or equal to about 27 nm.

[0096] The quantum dots of the embodiments can emit blue light with an improved quantum efficiency (also referred to herein as quantum yield (QY)) of about 70% or more, such as about 71% or more, about 72% or more, about 73% or more, about 74% or more, about 75% or more, about 76% or more, about 77% or more, about 78% or more, or about 79% or more. The quantum dots can have a quantum efficiency of about 80% or more, about 90% or more, about 95% or more, about 99% or more, or 100%.

[0097] In an embodiment, the method of manufacturing the quantum dot includes: preparing a core including a first semiconductor nanocrystal including zinc, selenium, and tellurium (hereinafter, also referred to as a core); and

[0098] A zinc precursor is reacted with a non-metallic precursor selected from at least one of a selenium precursor and a sulfur precursor in an organic solvent in multiple steps in the presence of the core comprising the first semiconductor nanocrystal and an organic ligand at a temperature greater than or equal to about 300° C. to form a semiconductor nanocrystal shell comprising zinc, selenium and sulfur and having the aforementioned morphology on the surface of the core.

[0099] The forming of the semiconductor nanocrystal shell may include reacting a zinc precursor and a selenium precursor, and then reacting the zinc precursor and a sulfur precursor.

[0100] In an embodiment, the core may be obtained by preparing a zinc precursor solution including a zinc precursor and an organic ligand; preparing a selenium precursor and a tellurium precursor; heating the zinc precursor solution to a first reaction temperature and adding the selenium precursor and the tellurium precursor thereto, optionally together with the organic ligand, to react therebetween.

[0101] The zinc precursor may include Zn powder, ZnO, alkylated Zn compounds (e.g., C2-C30 dialkyl zinc such as diethyl zinc), zinc alcohol (e.g., zinc ethoxide), zinc carboxylate (e.g., zinc acetate), zinc nitrate, zinc perchlorate, zinc sulfate, zinc acetylacetonate, zinc halide (e.g., zinc chloride), zinc cyanide, zinc hydroxide, zinc carbonate, zinc peroxide, or a combination thereof. Examples of the zinc precursor may include dimethyl zinc, diethyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oxide, zinc peroxide, zinc perchlorate, zinc sulfate, or a combination thereof.

[0102] The selenium precursor may include selenium-trioctylphosphine (Se-TOP), selenium-tributylphosphine (Se-TBP), selenium-triphenylphosphine (Se-TPP), selenium-diphenylphosphine (Se-DPP), or a combination thereof, but is not limited thereto.

[0103] The tellurium precursor may include tellurium-trioctylphosphine (Te-TOP), tellurium-tributylphosphine (Te-TBP), tellurium-triphenylphosphine (Te-TPP), or a combination thereof, but is not limited thereto.

[0104] The sulfur precursor may include hexanethiol, octylthiol, decanethiol, dodecanethiol, hexadecanethiol, mercaptopropylsilane, sulfur-trioctylphosphine (S-TOP), sulfur-tributylphosphine (S-TBP), sulfur-triphenylphosphine (S-TPP), sulfur-trioctylamine (S-TOA), bistrimethylsilylsulfide, ammonium sulfide, sodium sulfide, or a combination thereof.

[0105] The organic solvent may be a C6-C22 primary amine such as hexadecylamine, a C6-C22 secondary amine such as dioctylamine, a C6-C40 tertiary amine such as trioctylamine, a nitrogen-containing heterocyclic compound such as pyridine, a C6-C40 olefin such as octadecene, a C6-C40 aliphatic hydrocarbon such as hexadecane, octadecane or squalane, an aromatic hydrocarbon substituted with a C6-C30 alkyl group such as phenyldodecane, phenyltetradecane, or phenylhexadecane, a primary, secondary or tertiary phosphine substituted with at least one (e.g., 1, 2 or 3) C6-C22 alkyl group (e.g., trioctylphosphine), a primary, secondary or tertiary phosphine oxide substituted with (e.g., 1, 2 or 3) C6-C22 alkyl group (e.g., trioctylphosphine oxide), a C12-C22 aromatic ether such as phenyl ether or benzyl ether, or a combination thereof.

[0106] The organic ligands can coordinate to (e.g., bond to) the surface of the produced nanocrystals and can have an effect on luminescence and electrical properties and can effectively disperse the nanocrystals in the solution phase. The quantum dots of the embodiments can be dispersed in organic solvents because they include organic ligands bonded to their surfaces. The organic ligands can include RCOOH, RNH 2 , R 2 NH, R 3 N, RSH, RH 2 PO, R 2 HPO, R 3 PO, RH 2 P.R 2 HP, R 3 P, ROH, RCOOR, RPO(OH) 2 , R 2 POOH, or a combination thereof, wherein R is the same or different and independently comprises hydrogen, a substituted or unsubstituted C1-C24 aliphatic hydrocarbon group, a substituted or unsubstituted C6-C20 aromatic hydrocarbon group, or a combination thereof, provided that at least one of R is not hydrogen. One or more ligands may be used.

[0107] Examples of organic ligand compounds may include: methyl mercaptan, ethyl mercaptan, propanethiol, butanethiol, pentanethiol, hexanethiol, octanethiol, dodecanethiol, hexanethiol, octadecanethiol, benzyl mercaptan; methylamine, ethylamine, propylamine, butylamine, pentaneamine, hexaneamine, octadecaneamine, dodecaneamine, hexadecaneamine, oleylamine, octadecaneamine, dimethylamine, diethylamine, dipropylamine; formic acid, acetic acid, propionic acid, butyric acid, pentane acid, hexadecane acid, heptane acid, octane acid, dodecane acid, hexadecane acid, octadecane acid, oleic acid, benzoic acid, palmitic acid, stearic acid; phosphine such as methyl phosphine, ethyl phosphine, propyl phosphine, butyl phosphine, pentane phosphine, tributyl phosphine or trioctyl phosphine; phosphine oxide compounds such as methyl phosphine oxide, ethyl phosphine oxide, propyl phosphine oxide, butyl phosphine oxide or trioctyl phosphine oxide; diphenyl phosphine or triphenyl phosphine compounds, or oxide compounds thereof; phosphonic acid, etc., but are not limited thereto. One or more organic ligand compounds may be used. In an embodiment, the organic ligand compound may be RCOOH and an amine (eg, RNH 2 , R 2 NH and / or R 3 N).

[0108] In the core including the first semiconductor nanocrystal, the molar ratio of tellurium to selenium may be less than or equal to about 0.05: 1. To form the core, the amount of the selenium precursor used to form the core may be greater than or equal to about 20 moles, such as greater than or equal to about 25 moles, greater than or equal to about 26 moles, greater than or equal to about 27 moles, greater than or equal to about 28 moles, greater than or equal to about 29 moles, greater than or equal to about 30 moles, greater than or equal to about 31 moles, greater than or equal to about 32 moles, greater than or equal to about 33 moles, greater than or equal to about 34 moles, greater than or equal to about 35 moles, greater than or equal to about 36 moles, greater than or equal to about 37 moles, greater than or equal to about 38 moles, greater than or equal to about 39 moles, or greater than or equal to about 40 moles, based on 1 mole of the tellurium precursor. The amount of the selenium precursor may be less than or equal to about 60 mol, less than or equal to about 59 mol, less than or equal to about 58 mol, less than or equal to about 57 mol, less than or equal to about 56 mol, or less than or equal to about 55 mol, based on 1 mol of the tellurium precursor. Within the aforementioned amount range, the core having the aforementioned composition may be formed.

[0109] The first reaction temperature may be greater than or equal to about 280°C, for example, greater than or equal to about 290°C. The reaction time for forming the core is not particularly limited and may be appropriately selected. For example, the reaction time may be greater than or equal to about 5 minutes, greater than or equal to about 10 minutes, greater than or equal to about 15 minutes, greater than or equal to about 20 minutes, greater than or equal to about 25 minutes, greater than or equal to about 30 minutes, greater than or equal to about 35 minutes, greater than or equal to about 40 minutes, greater than or equal to about 45 minutes, or greater than or equal to about 50 minutes, but is not limited thereto. For example, the reaction time may be less than or equal to about 2 hours, but is not limited thereto. By controlling the reaction time, the size of the core can be controlled.

[0110] The reaction conditions for forming the shell may be appropriately selected according to the desired composition of the shell. In an embodiment, the solvent and optionally the organic ligand may be heated (or treated under vacuum) at a predetermined temperature (e.g., at a temperature of about 100° C. or more), and the atmosphere may be changed to an inert gas, and then heated at a predetermined temperature (e.g., at a temperature of about 100° C. or more). Then, the core may be injected, and the shell precursor may be injected sequentially or simultaneously and the resulting mixture may be heated to a predetermined reaction temperature to react.

[0111] The shell precursors may be added sequentially, for example as mixtures of varying ratios, for a reaction time to achieve the desired composition and / or morphology of the quantum dots or to form a gradient or multilayer shell on the core. In an embodiment, a first layer may be formed by reacting a zinc precursor and a selenium precursor, and then an outer layer may be formed, for example by reacting a zinc precursor and a sulfur precursor. The reaction temperature for forming the shell may be greater than or equal to about 300° C., or greater than or equal to about 310° C. and less than or equal to about 330° C., or less than or equal to about 325° C.

[0112] In the reaction system, the amount and concentration of the precursor may be selected in consideration of the composition of the core and the shell and the reactivity between the precursors.

[0113] After the reaction is completed, a non-solvent is added to the reaction product, and the nano-crystal particles coordinated with the ligand compound (for example, bonded to the ligand compound) can be separated. The non-solvent can be a polar solvent that can be miscible with the solvent used in the core formation and / or shell formation reaction and can not make the produced nano-crystals dispersed therein. The non-solvent can be selected depending on the solvent used in the reaction, and can be, for example, acetone, ethanol, butanol, isopropanol, water, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), diethyl ether, formaldehyde, acetaldehyde, ethylene glycol, a solvent with a solubility parameter similar to the aforementioned non-solvent, or a combination thereof. The separation of the nano-crystal particles can include centrifugation, sedimentation, chromatography or distillation. If necessary, the separated nano-crystal particles can be added to a washing solvent and washed. The type of the washing solvent is not particularly limited, and a solvent with a solubility parameter similar to the solubility parameter of the ligand can be used, and its example can include hexane, heptane, octane, chloroform, toluene, benzene, etc.

[0114] The quantum dots of the embodiments may not be dispersible in water, any of the non-solvents listed above, or mixtures thereof. The quantum dots of the embodiments may be insoluble in water. The quantum dots of the embodiments may be dispersible in the above-mentioned organic solvents. In some embodiments, the quantum dots may be dispersible in C6-C40 aliphatic hydrocarbons, C6-C40 aromatic hydrocarbons, or mixtures thereof.

[0115] In an embodiment, an electronic device includes the semiconductor nanocrystal particles. The device may include a display device, a light emitting diode (LED), an organic light emitting diode (OLED), a quantum dot LED, a sensor, a solar cell, an image sensor, or a liquid crystal display (LCD), but is not limited thereto.

[0116] In an embodiment, the electronic device may be a photoluminescent element (eg, a lighting device such as a quantum dot sheet or quantum dot track or a liquid crystal display (LCD)) or an electroluminescent device (eg, a QD LED).

[0117] In embodiments, the electronic device may include a quantum dot sheet and the quantum dots may be included in the quantum dot sheet (eg, in the form of a semiconductor nanocrystal-polymer composite).

[0118] In an embodiment, the electronic device may be an electroluminescent device. The electronic device may include an anode 1 and a cathode 5 facing each other and a quantum dot emission layer 3 disposed between the anode and the cathode and including a plurality of quantum dots, and the plurality of quantum dots may include blue light emitting semiconductor nanocrystal particles (see Figure 2 ).

[0119] The cathode may include an electron injection conductor (e.g., having a relatively low work function). The anode may include a hole injection conductor (e.g., having a relatively high work function). The electron / hole injection conductor may include a metal (e.g., aluminum, magnesium, tungsten, nickel, cobalt, platinum, palladium, or calcium), a metal compound (e.g., LiF), an alloy, or a combination thereof; a metal oxide such as indium gallium oxide or indium tin oxide; or a conductive polymer such as polyethylenedioxythiophene (e.g., having a relatively high work function), but is not limited thereto.

[0120] At least one of the cathode and the anode may be a light-transmitting electrode or a transparent electrode. In an embodiment, both the anode and the cathode may be light-transmitting electrodes. The electrode may be patterned.

[0121] The light-transmitting electrode may be made of, for example, a transparent conductor such as indium tin oxide (ITO) or indium zinc oxide (IZO), gallium indium tin oxide, zinc indium tin oxide, titanium nitride, polyaniline or LiF / Mg:Ag, or a thin single-layer or multi-layer metal film, but is not limited thereto. When one of the cathode and the anode is a non-light-transmitting electrode, the non-light-transmitting cathode or anode may be made of, for example, an opaque conductor such as aluminum (Al), lithium aluminum (Li:Al) alloy, magnesium-silver alloy (Mg:Ag), or lithium fluoride-aluminum (LiF:Al).

[0122] The light-transmitting electrode may be disposed on a transparent substrate (eg, an insulating transparent substrate). The substrate may be rigid or flexible. The substrate may be plastic, glass, or metal.

[0123] The thickness of the anode and the cathode is not particularly limited and can be selected in consideration of device efficiency. For example, the thickness of the anode (or the cathode) may be greater than or equal to about 5 nm, such as greater than or equal to about 50 nm, but is not limited thereto. For example, the thickness of the anode (or the cathode) may be less than or equal to about 100 micrometers (μm), such as less than or equal to about 10 um, less than or equal to about 1 μm, less than or equal to about 900 nm, less than or equal to about 500 nm, or less than or equal to about 100 nm, but is not limited thereto.

[0124] The quantum dot emission layer may include a plurality of quantum dots. The plurality of quantum dots may include blue light emitting semiconductor nanocrystal particles according to an embodiment. The quantum dot emission layer may include a single layer of blue light emitting semiconductor nanocrystal particles.

[0125] The emission layer can be formed by preparing a dispersion comprising the quantum dots dispersed in a solvent, applying the dispersion via spin coating, inkjet coating or spray coating, and drying it. The emission layer can have a thickness of greater than or equal to about 5 nm, for example, greater than or equal to about 10 nm, greater than or equal to about 15 nm, greater than or equal to about 20 nm, or greater than or equal to about 25 nm and less than or equal to about 100 nm, for example, less than or equal to about 90 nm, less than or equal to about 80 nm, less than or equal to about 70 nm, less than or equal to about 60 nm, less than or equal to about 50 nm, less than or equal to about 40 nm, or less than or equal to about 30 nm.

[0126] The electronic device may include a charge (hole or electron) auxiliary layer between the anode and the cathode. For example, the electronic device may include a hole auxiliary layer 2 between the anode and the quantum dot emission layer and / or an electron auxiliary layer 4 between the cathode and the quantum dot emission layer (see Figure 2 ).

[0127] In the drawing, the electron / hole auxiliary layer is formed as a single layer, but the electron / hole auxiliary layer is not limited thereto and may include a plurality of layers including at least two stacked layers.

[0128] The hole auxiliary layer may include, for example, a hole injection layer (HIL) for promoting hole injection, a hole transport layer (HTL) for promoting hole transport, an electron blocking layer (EBL) for inhibiting electron transport, or a combination thereof. For example, the hole injection layer may be disposed between the hole transport layer and the anode. For example, the electron blocking layer may be disposed between the emission layer and the hole transport (injection) layer, but is not limited thereto. The thickness of each layer may be appropriately selected. For example, the thickness of each layer may be greater than or equal to about 1 nm, greater than or equal to about 5 nm, greater than or equal to about 10 nm, greater than or equal to about 15 nm, greater than or equal to about 20 nm, or greater than or equal to about 25 nm and less than or equal to about 500 nm, less than or equal to about 400 nm, less than or equal to about 300 nm, less than or equal to about 200 nm, less than or equal to about 100 nm, less than or equal to about 90 nm, less than or equal to about 80 nm, less than or equal to about 70 nm, less than or equal to about 60 nm, or less than or equal to about 50 nm, but is not limited thereto. The hole injection layer may be an organic layer formed by a solution process (e.g., spin coating, etc.). The hole transport layer may be an organic layer formed by a solution process (e.g., spin coating, etc.).

[0129] The electron auxiliary layer may include, for example, an electron injection layer (EIL) for promoting electron injection, an electron transport layer (ETL) for promoting electron transport, a hole blocking layer (HBL) for inhibiting hole transport, or a combination thereof. For example, the electron injection layer may be disposed between the electron transport layer and the cathode. For example, the hole blocking layer may be disposed between the emission layer and the electron transport (injection) layer, but is not limited thereto. The thickness of each layer may be appropriately selected. For example, the thickness of each layer may be greater than or equal to about 1 nm, greater than or equal to about 5 nm, greater than or equal to about 10 nm, greater than or equal to about 15 nm, greater than or equal to about 20 nm, or greater than or equal to about 25 nm and less than or equal to about 500 nm, less than or equal to about 400 nm, less than or equal to about 300 nm, less than or equal to about 200 nm, less than or equal to about 100 nm, less than or equal to about 90 nm, less than or equal to about 80 nm, less than or equal to about 70 nm, less than or equal to about 60 nm, or less than or equal to about 50 nm, but is not limited thereto. The electron injection layer may be an organic layer formed by deposition. The electron transport layer may include an inorganic oxide or nanoparticles thereof or may include an organic layer formed by deposition.

[0130] The quantum dot emission layer may be disposed in a hole injection (or transport) layer or an electron injection (or transport) layer. The quantum dot emission layer may be disposed as a separate layer between the hole auxiliary layer and the electron auxiliary layer.

[0131] The charge auxiliary layer, the electron blocking layer and the hole blocking layer may include, for example, an organic material, an inorganic material or an organic / inorganic material. The organic material may be a compound having hole or electron related properties. The inorganic material may be, for example, a metal oxide such as molybdenum oxide, tungsten oxide, zinc oxide or nickel oxide, but is not limited thereto.

[0132] The hole transport layer (HTL) and / or the hole injection layer may include, for example, poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) (PEDOT:PSS), poly(9,9-dioctyl-fluorene-co-N-(4-butylphenyl)-diphenylamine) (TFB), polyarylamine (polyarylamine), poly(N-vinylcarbazole) (PVK), polyaniline, polypyrrole, N,N,N',N'-tetrakis(4-methoxyphenyl)- benzidine (TPD), 4,4'-bis[N-(1-naphthyl)-N-phenyl-amino]biphenyl (α-NPD), m-MTDATA (4,4',4"-tri[phenyl(m-tolyl)amino]triphenylamine), 4,4',4"-tri(N-carbazolyl)-triphenylamine (TCTA), 1,1-bis[(di-4-tolylamino)phenyl]cyclohexane (TAPC), p-type metal oxides (e.g., NiO, WO 3 、MoO3 etc.), carbonaceous materials such as graphene oxide, or a combination thereof, but not limited thereto.

[0133] The electron blocking layer (EBL) may include, for example, poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) (PEDOT:PSS), poly(9,9-dioctyl-fluorene-co-N-(4-butylphenyl)-diphenylamine) (TFB), polyarylamine (polyarylamine), poly(N-vinylcarbazole), polyaniline, polypyrrole, N,N,N',N'-tetrakis(4-methoxyphenyl)-benzidine (TPD), 4,4'-bis[N-(1-naphthyl)-N-phenyl-amino]biphenyl (α-NPD), m-MTDATA, 4,4',4"-tris(N-carbazolyl)-triphenylamine (TCTA), or a combination thereof, but is not limited thereto.

[0134] The electron transport layer (ETL) and / or the electron injection layer may include, for example, 1,4,5,8-naphthalene-tetracarboxylic dianhydride (NTCDA), bathocuproine (BCP), tris[3-(3-pyridyl)- yl]borane (3TPYMB), LiF, Alq 3 , Gaq 3 、Inq 3 、Znq 2 、Zn(BTZ) 2 、BeBq 2 , ET204 (8-(4-(4,6-di(naphthalene-2-yl)-1,3,5-triazine-2-yl)phenyl)quinolone), 8-hydroxyquinoline lithium (Liq), n-type metal oxides (e.g., zinc oxide (ZnO), HfO 2 , etc.), or a combination thereof, but not limited thereto. In the foregoing, "q" is 8-hydroxyquinoline, "BTZ" is 2-(2-hydroxyphenyl)benzothiazole, and "Bq" is 10-hydroxybenzo[h]quinoline.

[0135] The hole blocking layer (HBL) may include, for example, 1,4,5,8-naphthalene-tetracarboxylic dianhydride (NTCDA), bathocuproin (BCP), tris[3-(3-pyridyl)- yl]borane (3TPYMB), LiF, Alq 3 , Gaq 3 、Inq 3 、Znq 2 、Zn(BTZ) 2 、BeBq 2 , or a combination thereof, but not limited thereto.

[0136] In the device according to the embodiment, the anode 10 disposed on the transparent substrate 100 may include a metal oxide transparent electrode (e.g., an ITO electrode), and the cathode 50 facing the anode may include a metal (Mg, Al, etc.) with a predetermined (e.g., relatively low) work function. For example, TFB and / or PVK as the hole transport layer 20 and PEDOT:PSS and / or p-type metal oxide as the hole injection layer 20 may be disposed between the transparent electrode 10 and the emission layer 30. The electron auxiliary layer (e.g., electron transport layer) 40 may be disposed between the quantum dot emission layer 30 and the cathode 50. (See Figure 3 )

[0137] The device according to the embodiment has an inverted structure. Here, the cathode 50 disposed on the transparent substrate 100 may include a metal oxide transparent electrode (e.g., ITO), and the anode 10 facing the cathode may include a metal with a predetermined (e.g., relatively high) work function (e.g., Au, Ag, etc.). For example, an n-type metal oxide (ZnO) may be disposed between the transparent electrode 50 and the emission layer 30 as an electron auxiliary layer (e.g., electron transport layer) 40. The hole auxiliary layer 20 (e.g., a hole transport layer including TFB and / or PVK and / or a hole transport layer including MoO 3 or another hole injection layer of a p-type metal oxide) may be disposed between the metal anode 10 and the quantum dot emission layer 30. (See Figure 4 )

[0138] Hereinafter, specific embodiments are described. However, these embodiments are exemplary, and the present disclosure is not limited thereto.

[0139] Example

[0140] Analytical methods

[0141] 1. Photoluminescence Analysis

[0142] The photoluminescence (PL) spectra of the produced nanocrystals were obtained using a Hitachi F-7000 spectrometer at an illumination wavelength of 372 nanometers (nm).

[0143] 2. Ultraviolet (UV) spectroscopy analysis

[0144] UV spectroscopy analysis was performed using a Hitachi U-3310 spectrometer to obtain UV-visible absorption spectra.

[0145] 3. Transmission Electron Microscopy (TEM) Analysis

[0146] Transmission electron micrographs of the nanocrystals were obtained using a UT F30 Tecnai electron microscope and the imaging program Image J.

[0147] 4. Inductively coupled plasma (ICP) analysis

[0148] Inductively coupled plasma-atomic emission spectrometry (ICP-AES) analysis was performed using Shimadzu ICPS-8100.

[0149] 5. Electroluminescence Analysis

[0150] When a voltage was applied, a current depending on the voltage was measured by using a current-voltage (IV) tester 2635B manufactured by Keithley Co., Ltd., and electroluminescence brightness was measured using CS-2000A of Konica Minolta Co., Ltd.

[0151] Unless otherwise mentioned, the synthesis was performed under an inert gas atmosphere (nitrogen flowing condition).In the following Examples and the like, the (amount) ratio between precursors refers to a molar ratio unless otherwise defined.

[0152] Synthesis of quantum dots

[0153] Embodiment 1:

[0154] Selenium, sulfur and tellurium were dispersed in trioctylphosphine (TOP) to obtain 2 molar (M) Se / TOP stock solution, 2M S / TOP stock solution and 0.1M Te / TOP stock solution.

[0155] 1. In a 300 milliliter (mL) reaction flask, zinc acetate was dissolved in trioctylamine along with palmitic acid and heated under vacuum at 120° C. Within 1 hour, the atmosphere in the reactor was switched to nitrogen.

[0156] After heating at 300°C, the prepared Se / TOP stock solution and Te / TOP stock solution were quickly added at a predetermined ratio. After 60 minutes, the reaction solution was quickly cooled to room temperature and acetone was added thereto to obtain a precipitate, which was separated via centrifugation. The obtained ZnTeSe cores were dispersed in toluene.

[0157] The molar ratio between the Zn precursor used and the Se precursor used (Zn:Se) was 2:1, and the molar ratio of Te to Se was 0.05:1 (Te:Se).

[0158] 2. In a 300 mL reaction flask, trioctylamine was placed, and zinc acetate and oleic acid were added thereto at a molar ratio of 2:1 and treated at 120°C under vacuum. 2) replaced the atmosphere in the flask. When the temperature of the reaction flask was raised to 300° C., the toluene dispersion of the prepared ZnTeSe core was rapidly injected, and then Se / TOP stock solution was added thereto and the reaction was carried out for 120 minutes to form a ZnSe layer on the core. Then, S / TOP was added together with zinc oleate and the reaction was carried out for 60 minutes to form a ZnS layer on the ZnSe layer. The molar ratio between the amounts of the Zn precursor, the Se precursor and the S precursor was about 1:0.3:1.1.

[0159] 3. Analysis

[0160] (1) For the prepared quantum dots, photoluminescence analysis was performed and the results are summarized in Table 1.

[0161] (2) For the prepared quantum dots, inductively coupled plasma atomic emission spectrometry analysis was performed and the results are summarized in Table 2.

[0162] (3) The prepared quantum dots were analyzed by transmission electron microscopy and the results are shown in Figure 5 In. From Figure 5 As a result, the prepared quantum dots had an average size of about 11 nm and had at least four pods.

[0163] Embodiment 2:

[0164] 1. Core-shell quantum dots were prepared in the same manner as in Example 1, except that the reaction temperature was increased to 320° C. during shell formation.

[0165] 2. Analysis

[0166] (1) For the prepared quantum dots, photoluminescence analysis was performed and the results are summarized in Table 1.

[0167] (2) For the prepared quantum dots, inductively coupled plasma atomic emission spectrometry analysis was performed and the results are summarized in Table 2.

[0168] (3) The prepared quantum dots were analyzed by transmission electron microscopy and the results are shown in Figure 6 In. From Figure 6 As a result, the prepared quantum dots had an average size of about 15.1 nm and had at least four pods.

[0169] Comparative Example 1:

[0170] 1. Core-shell quantum dots were prepared in the same manner as in Example 1, except that Se was not used in the shell formation and a molar ratio of Zn:S=1:0.6 was used.

[0171] 2. Analysis

[0172] (1) For the prepared quantum dots, photoluminescence analysis was performed and the results are summarized in Table 1.

[0173] (2) For the prepared quantum dots, inductively coupled plasma atomic emission spectrometry analysis was performed and the results are summarized in Table 2.

[0174] (3) The prepared quantum dots were analyzed by transmission electron microscopy and the results are shown in Figure 7 In. From Figure 7 As a result, the prepared quantum dots had an average size of about 8.3 nm and the average number of their pods was less than four.

[0175] Comparative Example 1-1:

[0176] 1. Core-shell quantum dots were prepared in the same manner as in Example 1, except that tellurium was not used during the preparation of the core.

[0177] 2. Analysis

[0178] (1) For the prepared quantum dots, photoluminescence analysis was performed and the results are summarized in Table 1.

[0179] (2) For the prepared quantum dots, inductively coupled plasma atomic emission spectrometry analysis was performed and the results are summarized in Table 2.

[0180] Table 1

[0181]

[0182] Table 2

[0183]

[0184] Morphological analysis of quantum dots

[0185] 1. Area ratio of quantum dots to circumscribed circle

[0186] The area ratio of the quantum dots to the circumscribed circle was measured for the quantum dots prepared in the examples, and the results are shown in Figure 8 middle. Figure 8 The results show that in the case of the quantum dots prepared in the examples, on average, the area ratio relative to the circumscribed circle is greater than or equal to about 0.4:1.

[0187] 2. Pod edge point angle

[0188] (1) The edge point angle of the pod relative to the circumscribed circle was measured for the quantum dots prepared in the examples, and the results are shown in Fig. 9 middle. Fig. 9 The results show that in the case of the quantum dots prepared in the example, the edge dot angle of the pod is less than about 70 degrees.

[0189] (2) The edge point angle of the quantum dots prepared in Comparative Example 1 relative to the circumscribed circle was measured, and the results are shown in Fig.10 middle. Fig.10 The results show that in the case of the quantum dots prepared in Comparative Example 1, on average, the edge dot angle of the pod is greater than or equal to about 70 degrees.

[0190] Example 3

[0191] A light-emitting device was manufactured by using the quantum dots of Example 1 in the following manner. On a glass substrate with a deposited indium tin oxide (ITO) electrode (anode), a poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) (PEDOT:PSS) layer and a PVK layer were formed as a hole injection layer and a hole transport layer via spin coating, respectively. On top of the poly(N-vinylcarbazole) (PVK) layer thus formed, an octane dispersion of quantum dots was spin-coated to form a quantum dot emission layer, and on top of the quantum dot emission layer, a 8-(4-(4,6-di(naphthalene-2-yl)-1,3,5-triazine-2-yl)phenyl)quinolone):8-hydroxyquinoline lithium (ET204:Liq) layer was formed as an electron auxiliary layer, and an aluminum electrode was vapor-deposited on top of it.

[0192] For the prepared devices, the electroluminescent properties were evaluated and the results are summarized in Fig.11 , Fig.12 and Table 3.

[0193] Embodiment 4:

[0194] An electroluminescent device was prepared in the same manner as described in Example 3, except that the quantum dots of Example 2 were used as quantum dots.

[0195] For the prepared devices, the electroluminescent properties were evaluated and the results are summarized in Fig.11 , Fig.12 and Table 3.

[0196] Comparative Example 2:

[0197] An electroluminescent device was prepared in the same manner as described in Example 3, except that the quantum dots of Comparative Example 1 were used as quantum dots.

[0198] For the prepared devices, the electroluminescent properties were evaluated and the results are summarized in Fig.11 , Fig.12 and Table 3.

[0199] Table 3

[0200]

[0201] 1 Nite = candela / square meter

[0202] 2 λmax = peak emission wavelength

[0203] Fig.11 , Fig.12 The results of Table 3 and Table 3 confirm that, compared with Comparative Example 1, the device including the quantum dots of the Examples can exhibit improved electroluminescent properties.

[0204] While the present disclosure has been described with respect to what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but on the contrary is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.

Claims

1. Quantum dots, include: including a core of a first semiconductor nanocrystalline material comprising zinc, tellurium, and selenium; as well as a semiconductor nanocrystalline shell disposed on the core and comprising zinc, selenium, and sulfur, wherein the quantum dots do not include cadmium, The size of the quantum dots is greater than or equal to 10 nanometers, and wherein the quantum dot comprises at least four protrusions, wherein at least one of the protrusions of the quantum dot has a length greater than or equal to 1 nanometer, wherein in the quantum dots, the molar ratio of tellurium to selenium is greater than or equal to 0.001:1 and less than or equal to 0.1:1, The maximum photoluminescence peak wavelength of the quantum dots is greater than or equal to 450 nanometers and less than or equal to 470 nanometers, The quantum dots have a quantum efficiency greater than or equal to 70%, and The maximum photoluminescence peak of the quantum dots has a half-width less than or equal to 50 nanometers. 2 . The quantum dot of claim 1 , wherein in the quantum dot, a molar ratio of tellurium to selenium is greater than or equal to 0.001:1 and less than or equal to 0.05:

1.

3. The quantum dot according to claim 1, wherein The maximum photoluminescence peak of the quantum dots has a half-width less than or equal to 45 nanometers.

4. The quantum dot of claim 1, wherein the core comprises ZnTe x Se 1-x , where x is greater than 0 and less than or equal to 0.

05.

5. The quantum dot of claim 1, wherein the semiconductor nanocrystal shell comprises a gradient composition that varies in a radial direction from the core toward an outermost surface of the quantum dot.

6. The quantum dot of claim 1, wherein in the semiconductor nanocrystal shell, the amount of sulfur increases in a radial direction from the core toward the outermost surface of the quantum dot.

7. The quantum dot according to claim 1, wherein The semiconductor nanocrystal shell includes a first layer disposed directly on the core, and an outer layer disposed on the first layer, and The first layer includes second semiconductor nanocrystals, and The outer layer includes semiconductor nanocrystals having a composition different from a composition of the second semiconductor nanocrystals.

8. The quantum dot of claim 7, wherein the second semiconductor nanocrystal comprises zinc and selenium and the outer layer comprises zinc and sulfur. 9 . The quantum dot according to claim 1 , wherein the maximum photoluminescence peak wavelength of the quantum dot is 460 nm to 470 nm.

10. The quantum dot of claim 1, wherein in a two-dimensional image obtained from electron microscopy analysis, an area ratio of the quantum dot relative to a circumscribed circle is greater than or equal to 0.4:

1.

11. The quantum dot of claim 1, wherein in a two-dimensional image obtained from electron microscopy analysis, at least one of the protrusions of the quantum dot has an edge point angle of less than 70 degrees.

12. The quantum dot of claim 1, wherein the half width of the maximum photoluminescence peak of the quantum dot is less than 35 nanometers.

13. The quantum dot of claim 1, wherein the quantum dot has a size greater than or equal to 11 nanometers.

14. A method for producing a quantum dot as claimed in any one of claims 1 to 13, wherein include: preparing a core comprising a first semiconductor nanocrystal comprising zinc, selenium, and tellurium; as well as A selenium precursor, a sulfur precursor, or a combination thereof is reacted with a zinc precursor in multiple steps in an organic solvent in the presence of the core and an organic ligand at a temperature greater than or equal to 300° C. to form a semiconductor nanocrystal shell comprising zinc, selenium, and sulfur and having at least four protrusions.

15. The method of claim 14, wherein in the core comprising the first semiconductor nanocrystal, the ratio of tellurium to selenium is less than 0.05:

1.

16. The method of claim 14, wherein the formation of the semiconductor nanocrystal shell include: The zinc precursor is reacted with the selenium precursor, and then the zinc precursor is reacted with the sulfur precursor.

17. Electroluminescent devices, include: a first electrode and a second electrode facing each other, and a light-emitting layer disposed between the first electrode and the second electrode, The light-emitting layer comprises a plurality of quantum dots, and the plurality of quantum dots comprise the quantum dots as described in any one of claims 1 to 13.

18. The electroluminescent device of claim 17, further comprising a charge assist layer between the first electrode and the light emitting layer, between the second electrode and the light emitting layer, or between the first electrode and the light emitting layer and between the second electrode and the light emitting layer.

19. The electroluminescent device of claim 18, wherein the charge assisting layer comprises a charge injection layer, a charge transport layer, or a combination thereof.

20. The electroluminescent device of claim 17, wherein the electroluminescent device has a peak external quantum efficiency greater than or equal to 4%.

21. The electroluminescent device of claim 17, wherein the electroluminescent device is configured to emit light having a maximum emission peak wavelength between 450 nanometers and 460 nanometers and a half-width less than or equal to 25 nanometers.

22. A display device comprising the electroluminescent device according to any one of claims 17 to 21.

Citation Information

Patent Citations

  • Collecting apparatus of dust in exhaust gas using water

    KR1020180028319A

  • Quantum dot, manufacturing method, quantum dot-polymer composite comprising same and electronic device

    CN107663452A

  • Semiconductor nano crystal particle, manufacturing method thereof and device including the same

    CN108865109A

  • A semiconductor nanocrystal, and a method of preparing the same

    KR1020140056500A

  • Preparation of stable, bright luminescent nanoparticles having compositionally engineered properties

    US20050214536A1