Plasma Etching Method
By introducing a cyclic process, including etching and desorption steps, the microgrooving problem is solved by introducing a cyclic process during plasma etching, including etching and desorption steps, and the microgrooving problem is solved, improving the etching performance and maintaining the cleanliness of the etching chamber.
Patent Information
- Application Number
- CN201910550373.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-06-25
- Filing Date
- 2019-06-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-06-24
AI Technical Summary
In existing plasma etching methods, microgrooving phenomenon causes uneven etching depth, which may lead to defects in semiconductor devices. Existing prevention methods such as adjusting self-biasing or using polymer gas do not always effectively prevent microgrooving and may affect Etching chamber cleanliness.
A cycle process is employed, including an etching step and a desorption step, during which an etching agent gas is supplied for etching, and during which the desorption step is only supplied inert gas to allow the reactive substance to desorption from the substrate surface, reducing the occurrence of microgrooving.
Effectively reduce or eliminate microgrooving, improve etching performance, and avoid the adverse effects of the use of polymer gas on the cleanliness of the etching chamber.
Smart Images

Figure CN110634738B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a plasma etching method, in particular to a method for plasma etching a silicon-based compound semiconductor substrate. Background Art
[0002] Microgrooving is a term used to refer to localized etching at the base of the sidewalls of a plasma etched feature, which can result in large differences in etch depth across the bottom of the feature. Microgrooving can be caused when etching ions reach the sidewalls at a grazing angle. These ions reflect from the sidewalls and accumulate at the corners of the trench, resulting in locally higher etch rates. Figure 4 A typical microgrooved structure during plasma etching of silicon carbide (SiC) using sulfur hexafluoride (SF6) / oxygen (O2) / helium (He) process gas is shown. Microgrooving is undesirable because it may lead to defective semiconductor devices, especially if the microgrooves pass through to the underlying electrode.
[0003] Typical methods for preventing microgrooving rely on adjusting the direct current (DC) self-bias to reduce ion energy, or using polymerizing gases (e.g., silicon tetrafluoride (SiF4), octafluorocyclobutane (C4F8), trifluoromethane (CHF3)). However, these methods do not always guarantee the prevention of microgrooving, and may result in less than ideal etching performance (e.g., low etching rate or low selectivity) depending on the etching requirements. The use of polymer forming gases may also adversely affect the cleanliness of the etching chamber, requiring frequent mechanical cleaning of the etching chamber.
[0004] US 2007 / 0281462 discloses a method for overcoming the problem of microgrooving, wherein a first plasma etching step is followed by a second plasma etching step to remove any microgrooves created during the first plasma etching step.
[0005] It is an object of the present invention to prevent or at least reduce microgrooving during plasma etching. Summary of the invention
[0006] According to one aspect of the present invention, there is provided a method for plasma etching a silicon-based compound semiconductor substrate, the method comprising:
[0007] (a) providing a substrate in an etching chamber;
[0008] (b) performing a cyclic process on the substrate, each cycle of the cyclic process comprising:
[0009] i. supplying an etchant gas into an etching chamber, exciting the etchant gas into a plasma and performing an etching step on a substrate using the plasma; and
[0010] ii. performing a desorption step, wherein during the desorption step, the only gas supplied into the etching chamber is an inert gas, thereby allowing the reactive species adsorbed to the substrate surface during the etching step to be desorbed from the substrate surface.
[0011] The inventors have discovered that microgrooving can be greatly reduced or completely eliminated by providing a desorption step that stops the flow of any reactive species into the etch chamber and only supplies an inert gas into the etch chamber for a predetermined amount of time before continuing to the next step or cycle. Presumably, the desorption step provides time for any reactive species to desorb from the substrate surface, thereby reducing the amount of reactive species to below a threshold level required to form microgrooves.
[0012] In this manner, microgrooving may be reduced or eliminated without requiring a polymerizing gas to form a passivation layer which, as discussed above, may adversely affect etch chamber cleanliness.
[0013] The term "compound semiconductor" refers to a semiconductor made of two or more elements. The term "silicon-based compound semiconductor" refers to a compound semiconductor in which one element is silicon.
[0014] During the etching step, the etchant gas may include a fluorine-containing gas. For example, the etchant gas may include sulfur hexafluoride (SF6). Alternatively or additionally, the etchant gas may include carbon tetrafluoride (CF4) or octafluorocyclobutane (C4F8). The fluorine-containing gas provides a source of fluorine radicals in the plasma, which react on the substrate surface to etch.
[0015] During the etching step, the flow rate of the fluorine-containing gas may be about 10 sccm (standard cubic centimeters per minute) to 50 sccm (standard cubic centimeters per minute).
[0016] The duration of the etching step in each cycle may be about 0.5 seconds to 5 seconds.
[0017] The etchant gas may also include an inert gas, such as helium, argon, krypton, or xenon. During the etching step, the flow rate of the inert gas may be about 15 sccm to 40 sccm.
[0018] In some embodiments, the etchant gas consists of a fluorine-containing gas (eg, SF6) and an inert gas (eg, He, Ar, Kr, or Xe), i.e., the only gases supplied to the etching chamber during the etching step are the fluorine-containing gas and the inert gas.
[0019] In some embodiments, the etchant gas may also include an oxygen-containing gas (e.g., O2 or O3). The flow rate of the oxygen-containing gas may be less than the flow rate of the fluorine-containing gas. The oxygen-containing gas may flow during the etching step for only a portion of the total time of the etching step, and / or only a subset of the total number of cycles.
[0020] During the desorption step, the inert gas supplied to the etching chamber may be, for example, helium, argon, krypton or xenon, or a mixture of inert gases. The flow rate of the inert gas during the desorption step may be about 15 sccm to 40 sccm.
[0021] The duration of the desorption step in each cycle can be at least 0.5 seconds. In some embodiments, the duration of the desorption step can be at least 1 second. In some embodiments, the duration of the desorption step can be at least 1.5 seconds. In some embodiments, the duration of the desorption step can be at least 2 seconds. The maximum duration will be driven by productivity considerations, but may be, for example, about 5 seconds. The duration of the desorption step can be, for example, about 0.5 seconds to 5 seconds. Shorter desorption steps will result in faster cycles, but if the desorption step is too short, microgrooving may recur or the degree of microgrooving may be unacceptable.
[0022] Before performing the cyclic process, a mask layer, for example, a SiO2 mask layer, may be provided on the substrate to protect the substrate area that is not etched during the etching step. In this case, each cycle of the cyclic process may further include:
[0023] iii. performing a mask strengthening step to strengthen the mask layer, wherein during the mask strengthening step, only an oxygen-containing gas and optionally an inert gas are supplied into the etching chamber;
[0024] Therein, the etching step, the desorption step and the mask strengthening step may be performed in any order during each cycle.
[0025] The mask strengthening step is not necessary to reduce microgrooving and generally does not affect the extent of microgrooving. However, by providing a mask strengthening step, degradation of the mask layer during each cycle can be mitigated, thereby allowing greater etch depths.
[0026] These steps need not be performed in any particular order. For example, in one embodiment, the etching step may be performed first, followed by the desorption step, followed by the mask strengthening step. In another embodiment, the etching step may be performed first, followed by the mask strengthening step, followed by the desorption step. In another embodiment, the desorption step may be performed first, followed by the etching step, followed by the mask strengthening step.
[0027] During the mask strengthening step, the oxygen-containing gas may be O2 or O3.
[0028] In an embodiment, the gas supplied to the etching chamber during the mask strengthening step is composed of an oxygen-containing gas (e.g., O2 or O3) and optionally an inert gas (e.g., helium, argon, krypton, or xenon). If the inert gas is supplied during the mask strengthening step, the flow rate of the inert gas during the mask strengthening step may be about 15 sccm to 40 sccm.
[0029] The flow rate of the oxygen-containing gas during the mask strengthening step may be less than or equal to 30 sccm. In some embodiments, the flow rate of the oxygen-containing gas during the mask strengthening step may be less than or equal to 25 sccm. In some embodiments, the flow rate of the oxygen-containing gas during the mask strengthening step may be less than or equal to 20 sccm. In some embodiments, the flow rate of the oxygen-containing gas during the mask strengthening step may be less than or equal to 15 sccm. In some embodiments, the flow rate of the oxygen-containing gas during the mask strengthening step may be about 3 sccm to 12 sccm.
[0030] The duration of the mask strengthening step in each cycle may be about 0.5 seconds to 5 seconds.
[0031] The method of the present invention may be a method of plasma etching a silicon-based compound semiconductor substrate, wherein the substrate is made of SiC. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The present invention will now be described, by way of example only, with reference to the accompanying drawings, in which:
[0033] Figure 1 A schematic diagram of a substrate on which the method of the present invention may be performed is shown.
[0034] Figure 2 A schematic diagram of a cycle process according to the present invention is shown.
[0035] Figure 3 A cross section of a plasma etched trench using the method according to the invention is shown.
[0036] Figure 4 A cross section of a plasma etched trench is shown where microgrooving has occurred. DETAILED DESCRIPTION
[0037] Figure 1 A substrate 110 to be etched using the method of the present invention is shown. The substrate 110 in this example is made of silicon carbide (SiC). On top of the substrate 110 is a mask 120 made of silicon dioxide (SiO2). During the etching process, due to the difference in materials, the etching rate of the mask 120 will be lower than the etching rate of the substrate 110. Therefore, the mask 120 acts as a barrier above the substrate 110 to protect the portion of the substrate 110 that is not etched. The top of the portion to be etched of the substrate 110 is exposed.
[0038] The substrate 110 is etched in a typical plasma etching apparatus (not shown) including an etching chamber in which the substrate 110 is supported on a platen. An exemplary high density plasma etching tool that can etch silicon carbide substrates may be a SPTS Synapse TM The etching chamber includes a gas inlet through which gas can be introduced into the etching chamber and a gas outlet through which gas can leave the etching chamber.
[0039] Figure 2 A flow chart of an exemplary cyclic process according to the present invention is shown. In the described embodiment, the etching step 210 is performed first, followed by the mask strengthening step 220, followed by the desorption step 230. However, these steps need not be performed in this order and can be rearranged in any order. In addition, in order to reduce or prevent micro-grooving, the mask strengthening step 220 is optional. The mask strengthening step 220 advantageously allows a greater etching depth to be achieved.
[0040] Typical parameters for each step are shown in Table 1. Typical operating pressure is 1mTorr to 50mTorr (about 0.13Pa to 6.67Pa), and typical RF bias power is 250W to 1000W.
[0041] Table 1
[0042] Step 210 (etching) Step 220 (Mask Strengthening) Step 230 (Desorption) Time (seconds) 0.5-5 0.5-5 0.5-5 Coil power (W) 500-1500 500-1500 500-1500 <![CDATA[SF6(sccm)]]> 10-50 0 0 <![CDATA[O2(sccm)]]> 0 3-12 0 He(sccm) 15-40 15-40 15-40
[0043] During the etching step 210, an etchant gas mixture of SF6 and He is supplied to the etching chamber. The etchant gas mixture is then excited into a plasma and is used to etch a portion of the substrate 110 to begin forming a groove. Although there is no O2 flow during the etching step 210 in this example, in some embodiments, the etchant gas mixture may also include O2. Adding O2 during the etching step can increase F* radicals, thereby advantageously increasing the etching rate. However, the increase in F* radicals can also make microgrooving more likely to occur. If O2 is to be incorporated into the etchant gas mixture, the flow rate of O2 may generally be less than the flow rate of SF6. In some embodiments, O2 may be added only during a portion of the total time of the etching step 210 and / or only during a subset of the total number of cycles. The flow rate of O2 during the etching step 210 and the duration of the O2 flow may be optimized to increase the etching rate without microgrooving.
[0044] During the mask strengthening step 220, the supply of SF6 to the etching chamber is stopped and a gas mixture of O2 and He is supplied to the etching chamber instead. The O2 gas promotes the formation of compounds to strengthen the mask layer 120 so that the trenches can be etched to a greater depth. This step has no significant effect on microgrooving and is optional.
[0045] The only gas supplied to the etching chamber is He during the desorption step 230. Supplying only inert gas during this step allows any reactive etching species adsorbed to the etched surface of the substrate 110 time to desorb from the surface, which reduces microgrooving.
[0046] For the desorption step, increasing the flow rate of He had no major effect on reducing microgrooving. The step time of the desorption step was a more important factor in reducing microgrooving. Increasing the step time of the desorption step resulted in reduced or no microgrooving; however, this was at the expense of increasing the total time to perform each cycle. Desorption step times exceeding 2 seconds generally resulted in etching without microgrooving.
[0047] Steps 210, 220 and 230 form a cycle that can be repeated until the desired etching depth is reached. For example, using the process parameters shown in Table 1, the process can be repeated for 20 cycles to produce a groove with a depth of about 1 micron. Using the present invention, greater etching depths can be achieved while reducing or preventing microgrooving.
[0048] Figure 3 A cross section of a trench that was plasma etched using the process parameters of Table 1 and using a 3-step cycle process according to the present invention is shown. The trench shown shows no microgrooving.
Claims
1. A method for plasma etching a silicon-based compound semiconductor substrate, the method comprising: (a) providing a substrate in an etching chamber; (b) performing a cyclic process on the substrate, each cycle of the cyclic process comprising: i. supplying an etchant gas into the etching chamber, exciting the etchant gas into plasma and performing an etching step on the substrate using the plasma of the etchant gas to etch a portion of the substrate; and ii. performing a desorption step, wherein during the desorption step, the only gas supplied into the etching chamber is an inert gas, thereby allowing the reactive species adsorbed to the surface of the substrate during the etching step to be desorbed from the surface of the substrate.
2. The method according to claim 1, wherein: The etchant gas includes a fluorine-containing gas.
3. The method according to claim 2, wherein: The flow rate of the fluorine-containing gas during the etching step is 10 sccm to 50 sccm.
4. The method according to claim 2 or 3, wherein: The fluorine-containing gas is SF6.
5. The method according to any one of claims 1 to 3, wherein: The etchant gas also includes an inert gas.
6. The method according to claim 5, wherein: The flow rate of the inert gas during the etching step is 15 sccm to 40 sccm.
7. The method according to claim 5, wherein: The inert gas in the etchant gas is He.
8. The method according to any one of claims 1 to 3, wherein: The etchant gas consists of SF6 and inert gas.
9. The method according to any one of claims 1 to 3, wherein: The duration of the etching step in each cycle is 0.5 seconds to 5 seconds.
10. The method according to any one of claims 1 to 3, wherein: The inert gas supplied in the desorption step is He.
11. The method according to any one of claims 1 to 3, wherein: The flow rate of the inert gas during the desorption step is 15 sccm to 40 sccm.
12. The method according to any one of claims 1 to 3, wherein: The duration of the desorption step in each cycle is between 0.5 seconds and 5 seconds.
13. The method according to any one of claims 1 to 3, wherein: The duration of the desorption step in each cycle is at least 2 seconds.
14. The method according to any one of claims 1 to 3, wherein: Before performing the cyclic process, a SiO2 mask layer is provided on the substrate, wherein the SiO2 mask layer is used to protect the non-etched area of the substrate during the etching step; and wherein each cycle in the cyclic process further comprises: iii. performing a mask strengthening step to strengthen the mask layer, wherein during the mask strengthening step, only an oxygen-containing gas and optionally an inert gas are supplied into the etching chamber; The etching step, the desorption step and the mask strengthening step may be performed in any order during each cycle.
15. The method according to claim 14, wherein: The oxygen-containing gas supplied in the mask strengthening step is O2 or O3.
16. The method according to claim 14, wherein: During the mask strengthening step, the gas supplied to the etching chamber consists of O2 and optionally an inert gas.
17. The method according to claim 14, wherein: The flow rate of the oxygen-containing gas during the mask strengthening step is less than or equal to 30 sccm.
18. The method according to claim 14, wherein: The flow rate of the oxygen-containing gas during the mask strengthening step is 3 sccm to 12 sccm.
19. The method according to claim 14, wherein: The duration of the mask strengthening step in each cycle is 0.5 seconds to 5 seconds.
20. The method according to claim 14, wherein: The substrate is made of SiC.