A self-sensing FRP rib embedded with a piezoelectric ceramic sensor and a method of using the same

By embedding piezoelectric ceramic sensors on FRP bars and combining impedance method and wave method monitoring, the problem of monitoring FRP bar wear and interface damage is solved, real-time safety assessment of reinforced concrete structures is achieved, and structural accidents are prevented.

CN110702515BActive Publication Date: 2024-10-11DONGGUAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910991009.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-10-18
Publication Date
2024-10-11
Estimated Expiration
2039-10-18

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively monitor the wear of FRP bars and the damage to the interface between FRP bars and concrete in real time, resulting in a decrease in the ultimate bearing capacity of the reinforced concrete structure and a shortening of the normal service life, and there is a risk of structural accidents.

Method used

A self-sensing FRP bar embedded with a piezoelectric ceramic sensor was designed. By opening a notch on the surface of the FRP bar and embedding the piezoelectric ceramic sensor, the wear and interface damage of the FRP bar was monitored by combining the impedance method and the wave method, and the wavelet energy ratio was used. Index evaluates structural safety performance.

Benefits of technology

It realizes real-time online monitoring of FRP bars, accurately evaluates the safety performance of reinforced concrete structures, and can take remedial measures before structural accidents occur to prevent catastrophic structural accidents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110702515B_ABST
    Figure CN110702515B_ABST
Patent Text Reader

Abstract

The present invention discloses a self-sensing FRP rib embedded with a piezoelectric ceramic sensor and a method for using the same. The self-sensing FRP rib includes an FRP rib and a sensor assembly. The sensor assembly includes a piezoelectric ceramic sensor and a BNC connector. The piezoelectric ceramic sensor includes a piezoelectric ceramic sheet and a copper shell. The piezoelectric ceramic sensor is embedded in the notch of the FRP rib and fixed by a packaging material layer. The self-sensing FRP rib structure is novel in design and can effectively achieve real-time, online monitoring. The method for using the same includes the following steps: a. preparing a piezoelectric ceramic sensor; b. connecting the piezoelectric ceramic sensor to the BNC connector; c. selecting the type of FRP rib and opening a notch; d. packaging material ratio test and ratio selection; e. embedding the piezoelectric ceramic sensor and filling the packaging material; f. monitoring step. The method for using the same can solve the problems of FRP rib wear and monitoring the interface between the FRP rib and concrete, and can accurately evaluate the safety performance of the enhanced concrete structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of civil engineering, and in particular to a self-sensing FRP rib embedded with a piezoelectric ceramic sensor and a use method thereof. Background Art

[0002] FRP bars are widely used in the field of civil engineering, especially in reinforced concrete structures. It should be pointed out that FRP bar reinforced concrete structures are prone to wear of FRP bars and degradation of the interface performance between FRP bars and concrete under the long-term action of natural environment, which leads to a decrease in the ultimate bearing capacity of the reinforced concrete structure and a shortened normal service life.

[0003] In view of the above situation, it is of great significance to effectively monitor the wear of FRP bars and the damage of the interface between FRP bars and concrete in real time to evaluate the safety performance of reinforced concrete structures and avoid the occurrence of structural accidents.

[0004] It should be pointed out that it is difficult for traditional sensors to monitor the wear of FRP bars and the interface damage between FRP bars and concrete. Summary of the invention

[0005] The purpose of the present invention is to provide a self-sensing FRP rib embedded with a piezoelectric ceramic sensor to address the deficiencies of the prior art. The self-sensing FRP rib embedded with a piezoelectric ceramic sensor has a novel structural design and can effectively achieve real-time, online monitoring.

[0006] Another object of the present invention is to provide a method for using self-sensing FRP bars embedded with piezoelectric ceramic sensors, which can effectively solve the problems of FRP bar wear and FRP bar-concrete interface monitoring, and can accurately evaluate the safety performance of reinforced concrete structures, so as to take corresponding remedial measures before the occurrence of structural accidents, thereby preventing catastrophic structural accidents.

[0007] To achieve the above object, the present invention is implemented through the following technical solutions.

[0008] A self-sensing FRP rib embedded with a piezoelectric ceramic sensor, comprising an FRP rib and a sensor assembly, wherein the sensor assembly comprises a piezoelectric ceramic sensor and a BNC connector, wherein the piezoelectric ceramic sensor comprises a piezoelectric ceramic sheet and a copper shell wrapped around the periphery of the piezoelectric ceramic sheet, wherein the positive electrode terminal of the piezoelectric ceramic sheet is connected to a positive electrode wire, and the negative electrode terminal of the piezoelectric ceramic sheet is connected to a negative electrode wire, wherein the positive electrode wire and the negative electrode wire respectively pass through the copper shell and are respectively led out from the upper surface of the copper shell, and the positive electrode wire and the negative electrode wire are respectively wrapped by an insulating outer layer; the positive electrode terminal of the BNC connector is connected to the lead-out end of the positive electrode wire, and the negative electrode terminal of the BNC connector is connected to the lead-out end of the negative electrode wire;

[0009] The surface of the FRP bar is provided with a groove formed by cutting with a high-speed laser cutting machine, and the piezoelectric ceramic sensor of the sensor assembly is completely embedded in the groove of the FRP bar. The groove of the FRP bar is filled with a packaging material layer that fixes the piezoelectric ceramic sensor. The packaging material layer uses a mixture of resin and curing agent, and the resin material used for the packaging material is the same as the base resin material of the FRP bar.

[0010] Wherein, the FRP bars are glass fiber reinforced bars or basalt fiber reinforced bars.

[0011] Wherein, the notch depth of the FRP bar is less than one third of the diameter of the FRP bar.

[0012] The surface of the FRP bar is provided with slots arranged in sequence along the length direction of the FRP bar, and the distance between two adjacent slots is greater than 30 cm.

[0013] Wherein, the surface of the packaging material layer is flush with the surface of the FRP rib.

[0014] Wherein, the thickness of the piezoelectric ceramic sheet is less than 1.2 mm, and the thickness of the copper shell is less than 0.02 mm.

[0015] A method for using a self-sensing FRP rib embedded with a piezoelectric ceramic sensor includes the following steps, specifically:

[0016] a. Prepare a piezoelectric ceramic sensor: select a piezoelectric ceramic sheet and a copper shell of appropriate size, and wrap the copper shell around the outer periphery of the piezoelectric ceramic sheet, the positive terminal of the piezoelectric ceramic sheet is connected to a positive wire, and the negative terminal of the piezoelectric ceramic sheet is connected to a negative wire, the positive wire and the negative wire pass through the copper shell respectively and are led out from the upper surface of the copper shell respectively, and the positive wire and the negative wire are wrapped by an insulating outer layer respectively;

[0017] b. Connect the piezoelectric ceramic sensor to the BNC connector: connect the lead-out end of the positive wire of the piezoelectric ceramic sensor to the positive terminal of the BNC connector, and connect the lead-out end of the negative wire of the piezoelectric ceramic sensor to the negative terminal of the BNC connector;

[0018] c. Select the type of FRP reinforcement and cut notches on the surface of the selected FRP reinforcement using a high-precision laser cutting machine;

[0019] d. Select the same resin as the matrix resin material of the selected FRP bar as the resin material of the encapsulation material, mix and stir the resin material for the encapsulation material and the curing agent according to seven groups, the ratio of the resin material for the encapsulation material to the curing agent in the first group is 4:1, the ratio of the resin material for the encapsulation material to the curing agent in the second group is 3:1, the ratio of the resin material for the encapsulation material to the curing agent in the third group is 2:1, the ratio of the resin material for the encapsulation material to the curing agent in the fourth group is 1:1, the ratio of the resin material for the encapsulation material to the curing agent in the fifth group is 1:2, the ratio of the resin material for the encapsulation material to the curing agent in the sixth group is 1:3, and the ratio of the resin material for the encapsulation material to the curing agent in the seventh group is 1:4, and the encapsulation materials of each group after mixing and stirring the resin material and the curing agent are placed in an environment with a temperature of 22°C for curing, and the curing time of each group of encapsulation materials is measured; after the curing time of each group of encapsulation materials is determined, select the encapsulation material with a curing time of 4h-8h as the backup encapsulation material;

[0020] e. The piezoelectric ceramic sensor is completely embedded in the notch of the FRP rib, and then the selected spare packaging material is filled into the notch of the FRP rib. After the packaging material layer in the notch is solidified, a packaging material layer is formed. The piezoelectric ceramic sensor is fixed in the notch of the FRP rib by the packaging material layer. The surface of the packaging material layer is flush with the surface of the FRP rib, and the positive and negative wires of the piezoelectric ceramic sensor are respectively extended to the outside of the packaging material layer. The preparation of the self-sensing FRP rib is completed;

[0021] f. Use impedance method to monitor the wear of self-sensing FRP tendons: connect the BNC connector of the piezoelectric ceramic sensor to the impedance tester, obtain the resistance-frequency spectrum at different times, observe the resistance-frequency spectrum and analyze the wear degree of the FRP tendons at different times according to the number, size and offset of the resonance peaks;

[0022] Alternatively, the wave method is used to monitor the wear of the self-sensing FRP reinforcement: the self-sensing FRP reinforcement is provided with two notches, each of which is embedded with a piezoelectric ceramic sensor fixed by a packaging material layer, the BNC connector of one of the piezoelectric ceramic sensors is connected to the transmitting end of the NIUSB-6366 data acquisition card, the BNC connector of the other piezoelectric ceramic sensor is connected to the receiving end of the NIUSB-6366 data acquisition card, and the NIUSB-6366 data acquisition card is connected to a computer; after the BNC connector, the NIUSB-6366 data acquisition card, and the computer are connected, After the connection is completed, the same signal excitation is selected to act on the piezoelectric ceramic sensor connected to the transmitting end of the NIUSB-6366 data acquisition card. At this time, the piezoelectric ceramic sensor connected to the transmitting end of the NIUSB-6366 data acquisition card vibrates and generates stress waves. The stress waves propagate along the FRP tendons and are received by the piezoelectric ceramic sensor connected to the receiving end of the NIUSB-6366 data acquisition card. The NIUSB-6366 data acquisition card sends the received data to the computer, and the computer judges the wear degree of the FRP tendons according to the difference in signals received at different times.

[0023] Alternatively, the wave method is used to monitor the interface damage between FRP bars and self-compacting concrete: a bond-slip specimen is prepared using self-sensing FRP bars and self-compacting concrete, and before preparing the bond-slip specimen, an intelligent aggregate sensor is buried in the center of the specimen near the FRP bar, and the piezoelectric ceramic sensor embedded in the groove of the FRP bar is located on the outside of the self-compacting concrete specimen, wherein the positive terminal of the intelligent aggregate sensor is connected to the positive terminal of the BNC connector through a wire, and the negative terminal of the intelligent aggregate sensor is connected to the negative terminal of the BNC connector through a wire; after the preparation of the bond-slip specimen is completed, the BNC connector of the piezoelectric ceramic sensor on the FRP bar is connected to the transmitting end of the NIUSB-6366 data acquisition card, and the BNC connector of the intelligent aggregate sensor is connected to the transmitting end of the NIUSB-6366 data acquisition card. Connect to the receiving end of the NIUSB-6366 data acquisition card, and the NIUSB-6366 data acquisition card is connected to the computer; after the BNC connector, the NIUSB-6366 data acquisition card, and the computer are connected, the bond-slip specimen is installed on the tensile testing machine and a pull-out test is performed on the tensile testing machine. During the pull-out test on the tensile testing machine, the same signal excitation is selected to act on the piezoelectric ceramic sensor on the FRP bar. At this time, the piezoelectric ceramic sensor vibrates and generates stress waves. The stress waves propagate in the FRP bar, the interface between the FRP bar and the self-compacting concrete, and the self-compacting concrete. The intelligent aggregate sensor receives the stress wave and judges the degree of damage to the interface between the FRP bar and the self-compacting concrete based on the signal amplitude and frequency shift differences received at different times.

[0024] In the process of using the wave method to monitor the wear of self-sensing FRP bars, in order to quantify the degree of damage to the interface between FRP bars and self-compacting concrete, a wavelet energy ratio index was proposed and symbolized by K. i express;

[0025] Each time the received signal S is decomposed into n+1 frequency bands by n-level wavelet, the signal X in each frequency band j Expressed as: X j =[X j,1 ,X j,2 ,……,X j,m ]; where j represents the frequency band (j=1, 2, ..., n+1), and m represents the amount of sampled data;

[0026] The energy of each frequency band is expressed as: Where i represents the time index;

[0027] According to the energy of each frequency band, the total energy of the signal received for the i-th time can be expressed as:

[0028]

[0029] In order to accurately reflect the damage degree of the interface between FRP bars and self-compacting concrete in the pull-out test, the wavelet energy ratio index is defined as: K i =E i / E0; where E i represents the total wavelet energy at different time indices, and E0 represents the total wavelet energy in the healthy state with a load of 0 kN;

[0030] The wavelet energy ratio at different time indices is calculated as a quantitative index, and the bond-slip curve of FRP bars and self-compacting concrete and the wavelet energy ratio index-slip curve are drawn in the same figure; when the bond stress reaches the peak value, the wavelet energy ratio index begins to degenerate rapidly, which indicates the failure of the interfacial bond between FRP bars and self-compacting concrete; the wavelet energy ratio index can quantify the damage condition of the interface between FRP bars and self-compacting concrete, lock the moment of bond degradation, and fully grasp the internal interface condition of the structure, thereby providing a basis for the macroscopic mechanical analysis of the structure.

[0031] The beneficial effects of the present invention are as follows: the self-sensing FRP rib embedded with a piezoelectric ceramic sensor of the present invention comprises an FRP rib and a sensor assembly, the sensor assembly comprises a piezoelectric ceramic sensor and a BNC connector, the piezoelectric ceramic sensor comprises a piezoelectric ceramic sheet and a copper shell wrapped around the outer periphery of the piezoelectric ceramic sheet, the positive electrode terminal of the piezoelectric ceramic sheet is connected to a positive electrode wire, the negative electrode terminal of the piezoelectric ceramic sheet is connected to a negative electrode wire, the positive electrode wire and the negative electrode wire respectively pass through the copper shell and are respectively led out from the upper surface of the copper shell, and the positive electrode wire and the negative electrode wire are respectively connected through an insulating outer The cladding is wrapped; the positive terminal of the BNC connector is connected to the lead-out end of the positive wire, and the negative terminal of the BNC connector is connected to the lead-out end of the negative wire; the surface of the FRP bar is provided with a notch formed by cutting by a high-speed laser cutting machine, and the piezoelectric ceramic sensor of the sensor assembly is completely embedded in the notch of the FRP bar, and the notch of the FRP bar is filled with a packaging material layer that fixes the piezoelectric ceramic sensor; the packaging material used in the packaging material layer is a mixture of resin and curing agent, and the resin material used in the packaging material is the same as the base resin material of the FRP bar. Through the above structural design, the present invention has the advantages of novel structural design and can effectively realize real-time and online monitoring.

[0032] Another beneficial effect of the present invention is: the method for using a self-sensing FRP rib embedded with a piezoelectric ceramic sensor described in the present invention includes the following steps, specifically: a. preparing a piezoelectric ceramic sensor: selecting a piezoelectric ceramic sheet and a copper shell of suitable size, and wrapping the copper shell around the periphery of the piezoelectric ceramic sheet, the positive terminal of the piezoelectric ceramic sheet is connected to a positive wire, and the negative terminal of the piezoelectric ceramic sheet is connected to a negative wire, the positive wire and the negative wire pass through the copper shell respectively and are led out from the upper surface of the copper shell respectively, and the positive wire and the negative wire are respectively wrapped by an insulating outer layer; b. connecting the piezoelectric ceramic sensor to a BNC connector: connecting the lead-out end of the positive wire of the piezoelectric ceramic sensor to the BN The method comprises the following steps: connecting the positive terminal of the C connector to the positive terminal of the C connector, and connecting the lead end of the negative wire of the piezoelectric ceramic sensor to the negative terminal of the BNC connector; c. selecting the type of FRP rib, and opening a notch on the surface of the selected FRP rib by a high-precision laser cutting machine; d. selecting a resin material that is the same as the base resin material of the selected FRP rib (1) as the resin material of the packaging material, and mixing the resin material and the curing agent for the packaging material according to seven groups, wherein the ratio of the resin material for the packaging material to the curing agent in the first group is 4:1, the ratio of the resin material for the packaging material to the curing agent in the second group is 3:1, the ratio of the resin material for the packaging material to the curing agent in the third group is 2:1, and the ratio of the resin material for the packaging material to the curing agent in the fourth group is 4:1. The ratio of the resin material to the curing agent for the packaging material is 1:1, the ratio of the resin material to the curing agent for the packaging material in the fifth group is 1:2, the ratio of the resin material to the curing agent for the packaging material in the sixth group is 1:3, and the ratio of the resin material to the curing agent for the packaging material in the seventh group is 1:4. The packaging materials of each group after mixing the resin material and the curing agent are placed in an environment with a temperature of 22°C for curing, and the curing time of each group of packaging materials is measured; after the curing time of each group of packaging materials is determined, the packaging material with a curing time of 4h-8h is selected as the backup packaging material; e. The piezoelectric ceramic sensor is completely embedded in the notch of the FRP rib, and then the selected backup Fill the notch of the FRP rib with packaging material, and after the packaging material layer in the notch is solidified, a packaging material layer is formed. The piezoelectric ceramic sensor is fixed in the notch of the FRP rib by the packaging material layer. The surface of the packaging material layer is flush with the surface of the FRP rib, and the positive and negative wires of the piezoelectric ceramic sensor are respectively extended to the outside of the packaging material layer, and the self-sensing FRP rib is prepared; f. Use the impedance method to monitor the wear of the self-sensing FRP rib: connect the BNC connector of the piezoelectric ceramic sensor to the impedance tester, obtain the resistance-frequency spectrum at different times, observe the resistance-frequency spectrum, and analyze the wear degree of the FRP rib at different times according to the number, size and offset of the resonance peaks;Alternatively, a wave method is used to monitor the wear of the self-sensing FRP reinforcement: the self-sensing FRP reinforcement is provided with two notches, each of which is embedded with a piezoelectric ceramic sensor fixed by a packaging material layer, the BNC connector of one of the piezoelectric ceramic sensors is connected to the transmitting end of the NIUSB-6366 data acquisition card, the BNC connector of the other piezoelectric ceramic sensor is connected to the receiving end of the NIUSB-6366 data acquisition card, and the NIUSB-6366 data acquisition card is connected to a computer; after the BNC connector, the NIUSB-6366 data acquisition card, and the computer are connected, the same signal excitation is selected to act on the piezoelectric ceramic sensor connected to the transmitting end of the NIUSB-6366 data acquisition card, at which time the piezoelectric ceramic sensor connected to the transmitting end of the NIUSB-6366 data acquisition card vibrates and generates stress waves, the stress waves propagate along the FRP reinforcement and are received by the piezoelectric ceramic sensor connected to the receiving end of the NIUSB-6366 data acquisition card, and the NIUSB-6366 data acquisition card receives the received signal. The receiving end sends the received data to the computer, and the wear degree of the FRP bar is judged by the computer according to the difference of the signals received at different times; or, the interface damage of the FRP bar and the self-compacting concrete is monitored by the wave method: the bonding slip specimen is prepared by using the self-sensing FRP bar and the self-compacting concrete, and before preparing the bonding slip specimen, the intelligent aggregate sensor is buried in the center of the specimen near the FRP bar, and the piezoelectric ceramic sensor embedded in the notch of the FRP bar is located on the outside of the self-compacting concrete specimen, wherein the positive terminal of the intelligent aggregate sensor is connected to the positive terminal of the BNC connector through a wire, and the negative terminal of the intelligent aggregate sensor is connected to the negative terminal of the BNC connector through a wire; after the preparation of the bonding slip specimen is completed, the BNC connector of the piezoelectric ceramic sensor on the FRP bar is connected to the transmitting end of the NIUSB-6366 data acquisition card, and the BNC connector of the intelligent aggregate sensor is connected to the receiving end of the NIUSB-6366 data acquisition card, and the NIUSB-6366 data acquisition card is connected to the computer;After the BNC connector, NIUSB-6366 data acquisition card, and computer are connected, the bond slip specimen is installed on the tensile testing machine and a pull-out test is performed on the tensile testing machine. During the pull-out test on the tensile testing machine, the same signal is selected to excite the piezoelectric ceramic sensor on the FRP bar. At this time, the piezoelectric ceramic sensor vibrates and generates stress waves. The stress waves propagate in the FRP bar, the interface between the FRP bar and the self-compacting concrete, and the self-compacting concrete. The intelligent aggregate sensor receives the stress wave and judges the degree of damage to the interface between the FRP bar and the self-compacting concrete based on the amplitude and frequency shift differences of the received signals at different times. Through the above-mentioned design steps, the method for using the self-sensing FRP bar embedded with the piezoelectric ceramic sensor can effectively solve the problems of FRP bar wear and the monitoring of the interface between the FRP bar and the concrete, and can accurately evaluate the safety performance of the reinforced concrete structure, so as to take corresponding remedial measures before the occurrence of structural accidents, thereby preventing catastrophic structural accidents. ; BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The present invention is further described below with the aid of the accompanying drawings. However, the embodiments in the accompanying drawings do not constitute any limitation to the present invention.

[0034] Figure 1 It is a schematic diagram of the structure of the self-sensing FRP reinforcement of the present invention.

[0035] Figure 2 It is a schematic diagram of the structure of the sensor assembly of the present invention.

[0036] Figure 3 Schematic diagram of the impedance method for monitoring the wear of self-sensing FRP tendons.

[0037] Figure 4 Schematic diagram of the wear condition of self-sensing FRP bars monitored using the wave method.

[0038] Figure 5 Schematic diagram of using the wave method to monitor the interface damage between FRP bars and self-compacting concrete.

[0039] Figure 6 This is the time domain signal diagram when the wave method is used to monitor the interface damage between FRP bars and self-compacting concrete.

[0040] Figure 7 This is the frequency domain signal diagram when the wave method is used to monitor the interface damage between FRP bars and self-compacting concrete.

[0041] Figure 8 Schematic diagram of the bond-slip curve and wavelet energy ratio index-slip curve when the wave method is used to monitor the interface damage between FRP bars and self-compacting concrete.

[0042] exist Figures 1 to 8 Included are:

[0043] 1——FRP rib 11——notch

[0044] 2——Piezoelectric ceramic sensor 21——Piezoelectric ceramic sheet

[0045] 22——Copper shell 3——BNC connector

[0046] 4——Packaging material layer 5——Impedance tester

[0047] 6——NIUSB-6366 data acquisition card 7——Computer

[0048] 8——Intelligent aggregate sensor. DETAILED DESCRIPTION

[0049] The present invention is described below in conjunction with specific implementation methods.

[0050] like Figure 1 and Figure 3 As shown, a self-sensing FRP rib embedded with a piezoelectric ceramic sensor includes an FRP rib 1, a sensor assembly, the sensor assembly includes a piezoelectric ceramic sensor 2, and a BNC connector 3. The piezoelectric ceramic sensor 2 includes a piezoelectric ceramic sheet 21 and a copper shell 22 wrapped around the outer periphery of the piezoelectric ceramic sheet 21. The positive terminal of the piezoelectric ceramic sheet 21 is connected to a positive wire, and the negative terminal of the piezoelectric ceramic sheet 21 is connected to a negative wire. The positive wire and the negative wire pass through the copper shell 22 and are respectively led out from the upper surface of the copper shell 22, and the positive wire and the negative wire are respectively wrapped by an insulating outer layer; the positive terminal of the BNC connector 3 is connected to the lead-out end of the positive wire, and the negative terminal of the BNC connector 3 is connected to the lead-out end of the negative wire. It should be explained that, for the piezoelectric ceramic sensor 2 of the present invention, its piezoelectric ceramic sheet 21 is wrapped by a copper shell 22, and the copper shell 22 has the function of shielding noise. When the self-sensing FRP reinforcement 1 of the present invention is used to monitor the wear condition or the interface damage condition between the FRP reinforcement 1 and the self-compacting concrete, the copper shell 22 can shield external noise and improve the accuracy of monitoring.

[0051] Furthermore, the surface of the FRP bar 1 is provided with a notch 11 formed by cutting with a high-speed laser cutting machine, and the piezoelectric ceramic sensor 2 of the sensor assembly is completely embedded in the notch 11 of the FRP bar 1, and the notch 11 of the FRP bar 1 is filled with a packaging material layer 4 for fixing the piezoelectric ceramic sensor 2; the packaging material used in the packaging material layer 4 is a mixture of resin and curing agent, and the resin material used in the packaging material is the same as the base resin material of the FRP bar 1. Among them, the surface of the packaging material layer 4 is flush with the surface of the FRP bar 1, and the thickness of the piezoelectric ceramic sheet 21 is less than 1.2mm, and the thickness of the copper shell 22 is less than 0.02mm.

[0052] Preferably, the FRP bar 1 is a glass fiber reinforced bar or a basalt fiber reinforced bar.

[0053] It should be explained that the depth of the notch 11 of the FRP bar 1 is less than one third of the diameter of the FRP bar 1 .

[0054] In addition, the FRP bar 1 of the present invention may be provided with a plurality of notches 11. Specifically, the surface of the FRP bar 1 is provided with notches 11 arranged in sequence along the length direction of the FRP bar 1, and the distance between two adjacent notches 11 is greater than 30 cm.

[0055] In addition, the self-sensing FRP tendon 1 of the present invention can use the following method to monitor the wear of the FRP tendon 1. Specifically, a method for using a self-sensing FRP tendon embedded with a piezoelectric ceramic sensor includes the following steps, specifically:

[0056] a. Preparation of piezoelectric ceramic sensor 2: A Φ12×1mm PZT-5 type piezoelectric ceramic sheet 21 is selected as the piezoelectric ceramic sheet 21 of the present invention. The size of the copper shell 22 is slightly larger than the size of the selected piezoelectric ceramic sheet 21. The copper shell 22 is wrapped around the outer periphery of the piezoelectric ceramic sheet 21. The positive electrode terminal of the piezoelectric ceramic sheet 21 is connected to a positive electrode wire, and the negative electrode terminal of the piezoelectric ceramic sheet 21 is connected to a negative electrode wire. The positive electrode wire and the negative electrode wire pass through the copper shell 22 and are respectively led out from the upper surface of the copper shell 22, and the positive electrode wire and the negative electrode wire are respectively wrapped by an insulating outer layer;

[0057] b. Connect the piezoelectric ceramic sensor 2 to the BNC connector 3: connect the lead-out end of the positive wire of the piezoelectric ceramic sensor 2 to the positive terminal of the BNC connector 3, and connect the lead-out end of the negative wire of the piezoelectric ceramic sensor 2 to the negative terminal of the BNC connector 3;

[0058] c. Select an FRP bar 1 with a diameter of 16 mm, a base material of vinyl resin, and a reinforcing fiber of glass fiber, and open a notch 11 on the surface of the selected FRP bar 1 by a high-precision laser cutting machine; the bottom surface size of the notch 11 is 11.314×11.314 mm, and the depth is 2.343 mm;

[0059] d. Packaging material ratio test and ratio selection: Vinyl resin is selected as the resin material of the packaging material and hexahydrophthalic anhydride is selected as the curing agent of the packaging material. The vinyl resin and hexahydrophthalic anhydride are mixed and stirred according to seven groups. The ratio of vinyl resin to hexahydrophthalic anhydride in the first group is 4:1, the ratio of vinyl resin to hexahydrophthalic anhydride in the second group is 3:1, the ratio of vinyl resin to hexahydrophthalic anhydride in the third group is 2:1, and the ratio of vinyl resin to hexahydrophthalic anhydride in the fourth group is 1:1 , the ratio of vinyl resin to hexahydrophthalic anhydride in the fifth group is 1:2, the ratio of vinyl resin to hexahydrophthalic anhydride in the sixth group is 1:3, and the ratio of vinyl resin to hexahydrophthalic anhydride in the seventh group is 1:4, and the packaging materials of each group after mixing and stirring the vinyl resin and hexahydrophthalic anhydride are placed in an environment at a temperature of 22°C for curing, and the curing time of each group of packaging materials is measured; after the curing time of each group of packaging materials is determined, the packaging material with a curing time of 4h-8h is selected as the backup packaging material;

[0060] e. The piezoelectric ceramic sensor 2 is completely embedded in the notch 11 of the FRP tendon 1, and then the selected spare packaging material is filled into the notch 11 of the FRP tendon 1. After the packaging material layer 4 in the notch 11 is solidified, a packaging material layer 4 is formed. The piezoelectric ceramic sensor 2 is fixed in the notch 11 of the FRP tendon 1 by the packaging material layer 4. The surface of the packaging material layer 4 is flush with the surface of the FRP tendon 1, and the positive and negative wires of the piezoelectric ceramic sensor 2 are respectively extended to the outside of the packaging material layer 4. The self-sensing FRP tendon 1 is prepared;

[0061] f. Use impedance method to monitor the wear of self-sensing FRP tendon 1: Connect the BNC connector 3 of the piezoelectric ceramic sensor 2 to the impedance tester 5, obtain the resistance-frequency spectrum at different times, observe the resistance-frequency spectrum and analyze the wear degree of the FRP tendon 1 at different times according to the number, size and offset of the resonance peaks (see Appendix Figure 3 shown);

[0062] Alternatively, a wave method is used to monitor the wear of the self-sensing FRP rib 1: the self-sensing FRP rib 1 is provided with two notches 11, each notch 11 is respectively embedded with a piezoelectric ceramic sensor 2 fixed by a packaging material layer 4, a BNC connector 3 of one of the piezoelectric ceramic sensors 2 is connected to the transmitting end of the NIUSB-6366 data acquisition card 6, a BNC connector 3 of another piezoelectric ceramic sensor 2 is connected to the receiving end of the NIUSB-6366 data acquisition card 6, and the NIUSB-6366 data acquisition card 6 is connected to the computer 7; after the BNC connector 3, the NIUSB-6366 data acquisition card 6, After the computer 7 is connected, the same signal excitation is selected to act on the piezoelectric ceramic sensor 2 connected to the transmitting end of the NIUSB-6366 data acquisition card 6. At this time, the piezoelectric ceramic sensor 2 connected to the transmitting end of the NIUSB-6366 data acquisition card 6 vibrates and generates stress waves. The stress waves propagate along the FRP rib 1 and are received by the piezoelectric ceramic sensor 2 connected to the receiving end of the NIUSB-6366 data acquisition card 6. The NIUSB-6366 data acquisition card 6 sends the received data to the computer 7 at the receiving end. The computer 7 judges the wear degree of the FRP rib 1 according to the difference in signals received at different times (such as Figure 4 shown).

[0063] It should be further pointed out that the self-sensing FRP bar 1 of the present invention can use the following method to monitor the interface damage between the FRP bar 1 and the self-compacting concrete. Specifically, a method for using a self-sensing FRP bar embedded with a piezoelectric ceramic sensor includes the following steps, specifically:

[0064] a. Preparation of piezoelectric ceramic sensor 2: A Φ8×0.8mm PZT-5 type piezoelectric ceramic sheet 21 is selected as the piezoelectric ceramic sheet 21 of the present invention. The size of the copper shell 22 is slightly larger than the size of the selected piezoelectric ceramic sheet 21. The copper shell 22 is wrapped around the outer periphery of the piezoelectric ceramic sheet 21. The positive electrode terminal of the piezoelectric ceramic sheet 21 is connected with a positive electrode wire, and the negative electrode terminal of the piezoelectric ceramic sheet 21 is connected with a negative electrode wire. The positive electrode wire and the negative electrode wire pass through the copper shell 22 and are respectively led out from the upper surface of the copper shell 22, and the positive electrode wire and the negative electrode wire are respectively wrapped by an insulating outer layer;

[0065] b. Connect the piezoelectric ceramic sensor 2 to the BNC connector 3: connect the lead-out end of the positive wire of the piezoelectric ceramic sensor 2 to the positive terminal of the BNC connector 3, and connect the lead-out end of the negative wire of the piezoelectric ceramic sensor 2 to the negative terminal of the BNC connector 3;

[0066] c. Select an FRP bar 1 with a diameter of 12 mm, a matrix material of epoxy resin, and a reinforcing fiber of glass fiber, and open a notch 11 on the surface of the selected FRP bar 1 using a high-precision laser cutting machine; the bottom surface size of the notch 11 is 8.485×8.485 mm, and the depth is 1.757 mm;

[0067] d. Packaging material ratio test and proportion selection: Epoxy resin was selected as the resin material of the packaging material and 651 low molecular weight polyamide was selected as the curing agent of the packaging material. The epoxy resin and 651 low molecular weight polyamide were mixed and stirred according to seven groups. The ratio of epoxy resin to 651 low molecular weight polyamide in the first group was 4:1, the ratio of epoxy resin to 651 low molecular weight polyamide in the second group was 3:1, the ratio of epoxy resin to 651 low molecular weight polyamide in the third group was 2:1, and the ratio of epoxy resin to 651 low molecular weight polyamide in the fourth group was 1:1 The ratio of epoxy resin to 651 low molecular weight polyamide in the fifth group is 1:2, the ratio of epoxy resin to 651 low molecular weight polyamide in the sixth group is 1:3, and the ratio of epoxy resin to 651 low molecular weight polyamide in the seventh group is 1:4. The packaging materials of each group after mixing epoxy resin and 651 low molecular weight polyamide are placed in an environment with a temperature of 22°C for curing, and the curing time of each group of packaging materials is measured; after the curing time of each group of packaging materials is determined, the packaging materials with a curing time of 4h-8h are selected as the backup packaging materials;

[0068] e. The piezoelectric ceramic sensor 2 is completely embedded in the notch 11 of the FRP tendon 1, and then the selected spare packaging material is filled into the notch 11 of the FRP tendon 1. After the packaging material layer 4 in the notch 11 is solidified, a packaging material layer 4 is formed. The piezoelectric ceramic sensor 2 is fixed in the notch 11 of the FRP tendon 1 by the packaging material layer 4. The surface of the packaging material layer 4 is flush with the surface of the FRP tendon 1, and the positive and negative wires of the piezoelectric ceramic sensor 2 are respectively extended to the outside of the packaging material layer 4. The self-sensing FRP tendon 1 is prepared;

[0069] f. Use the wave method to monitor the interface damage between FRP bar 1 and self-compacting concrete: Use the self-sensing FRP bar 1 and self-compacting concrete to prepare a bonding slip specimen. Before preparing the bonding slip specimen, the intelligent aggregate sensor 8 is buried in the center of the specimen near the FRP bar 1. The piezoelectric ceramic sensor 2 embedded in the notch 11 of the FRP bar 1 is located on the outside of the self-compacting concrete specimen, wherein the positive terminal of the intelligent aggregate sensor 8 is connected to the positive terminal of the BNC connector 3 through a wire, and the negative terminal of the intelligent aggregate sensor 8 is connected to the negative terminal of the BNC connector 3 through a wire; after the bonding slip specimen is prepared, the BNC connector 3 of the piezoelectric ceramic sensor 2 on the FRP bar 1 is connected to the transmitting end of the NIUSB-6366 data acquisition card 6, and the BNC connector of the intelligent aggregate sensor 8 is connected to the transmitting end of the NIUSB-6366 data acquisition card 6. The head 3 is connected to the receiving end of the NIUSB-6366 data acquisition card 6, and the NIUSB-6366 data acquisition card 6 is connected to the computer 7; after the BNC connector 3, the NIUSB-6366 data acquisition card 6, and the computer 7 are connected, the bond slip specimen is installed on the tensile testing machine and a pull-out test is performed through the tensile testing machine. During the pull-out test through the tensile testing machine, the same signal excitation is selected to act on the piezoelectric ceramic sensor 2 on the FRP tendon 1. At this time, the piezoelectric ceramic sensor 2 vibrates and generates stress waves. The stress waves propagate in the FRP tendon 1, the interface between the FRP tendon 1 and the self-compacting concrete, and the self-compacting concrete. The intelligent aggregate sensor 8 receives the stress waves and judges the degree of damage to the interface between the FRP tendon 1 and the self-compacting concrete according to the signal amplitude and frequency shift differences received at different times. Figure 5 As shown; among them, the time domain signal diagram received at different times is as follows Figure 6 As shown in the frequency domain signal diagram Figure 7 As shown;

[0070] It should be explained that in the process of using the wave method to monitor the wear of the self-sensing FRP bar 1, in order to quantify the degree of damage to the interface between the FRP bar 1 and the self-compacting concrete, the wavelet energy ratio index was proposed and the symbol K was used. i express;

[0071] Each time the received signal S is decomposed into n+1 frequency bands by n-level wavelet, the signal X in each frequency band j Expressed as: X j =[X j,1 ,X j,2 ,……,X j,m ]; where j represents the frequency band j=1,2,…,n+1, and m represents the amount of sampled data;

[0072] The energy of each frequency band is expressed as: Where i represents the time index;

[0073] According to the energy of each frequency band, the total energy of the signal received for the i-th time can be expressed as:

[0074] In order to accurately reflect the damage degree of the interface between FRP bar 1 and self-compacting concrete in the pull-out test, the wavelet energy ratio index is defined as: K i =E i / E0; where E i represents the total wavelet energy at different time indices, and E0 represents the total wavelet energy in the healthy state with a load of 0 kN;

[0075] The wavelet energy ratio at different time indices is calculated as a quantitative index, and the bond-slip curve between FRP bar 1 and self-compacting concrete and the wavelet energy ratio index-slip curve are plotted in the same figure (e.g. Figure 8 When the bonding stress reaches its peak value, the wavelet energy ratio index begins to degenerate rapidly, which indicates the failure of the bonding at the interface between FRP tendon 1 and self-compacting concrete. The wavelet energy ratio index can be used to quantify the damage status of the interface between FRP tendon 1 and self-compacting concrete, lock the moment of bonding degradation, and fully understand the internal interface status of the structure, thereby providing a basis for the macroscopic mechanical analysis of the structure.

[0076] Based on the above, it can be seen that the self-sensing FRP bar embedded with piezoelectric ceramic sensors described in the present invention has the advantages of novel structural design and can effectively realize real-time and online monitoring. In addition, the method of using the self-sensing FRP bar embedded with piezoelectric ceramic sensors described in the present invention can effectively solve the problems of FRP bar 1 wear and FRP bar 1 and concrete interface monitoring, and can accurately evaluate the safety performance of the reinforced concrete structure, so as to take corresponding remedial measures before the occurrence of structural accidents, thereby preventing catastrophic structural accidents.

[0077] The above contents are only preferred embodiments of the present invention. For ordinary technicians in this field, according to the concept of the present invention, there will be changes in the specific implementation methods and application scopes. The content of this specification should not be understood as limiting the present invention.

Claims

1. A method for using a self-sensing FRP rib embedded with a piezoelectric ceramic sensor, characterized in that: The self-sensing FRP rib embedded with a piezoelectric ceramic sensor comprises an FRP rib (1), a sensor assembly, the sensor assembly comprises a piezoelectric ceramic sensor (2), and a BNC connector (3), the piezoelectric ceramic sensor (2) comprises a piezoelectric ceramic sheet (21) and a copper shell (22) wrapped around the outer periphery of the piezoelectric ceramic sheet (21), the positive electrode terminal of the piezoelectric ceramic sheet (21) is connected to a positive electrode wire, the negative electrode terminal of the piezoelectric ceramic sheet (21) is connected to a negative electrode wire, the positive electrode wire and the negative electrode wire respectively pass through the copper shell (22) and are respectively led out from the upper surface of the copper shell (22), and the positive electrode wire and the negative electrode wire are respectively wrapped by an insulating outer layer; the positive electrode terminal of the BNC connector (3) is connected to the lead-out end of the positive electrode wire, and the negative electrode terminal of the BNC connector (3) is connected to the lead-out end of the negative electrode wire; The surface of the FRP rib (1) is provided with a notch (11) formed by cutting with a high-speed laser cutting machine, the piezoelectric ceramic sensor (2) of the sensor assembly is completely embedded in the notch (11) of the FRP rib (1), and the notch (11) of the FRP rib (1) is filled with a packaging material layer (4) for fixing the piezoelectric ceramic sensor (2); the packaging material used in the packaging material layer (4) is a mixture of resin and curing agent, and the resin material used in the packaging material is the same as the base resin material of the FRP rib (1); The method for using the self-sensing FRP rib embedded with a piezoelectric ceramic sensor includes the following steps, specifically: a. Prepare a piezoelectric ceramic sensor (2): select a piezoelectric ceramic sheet (21) and a copper shell (22) of suitable size, and wrap the copper shell (22) around the outer periphery of the piezoelectric ceramic sheet (21); the positive electrode terminal of the piezoelectric ceramic sheet (21) is connected to a positive electrode wire, and the negative electrode terminal of the piezoelectric ceramic sheet (21) is connected to a negative electrode wire, the positive electrode wire and the negative electrode wire respectively pass through the copper shell (22) and are respectively led out from the upper surface of the copper shell (22), and the positive electrode wire and the negative electrode wire are respectively wrapped by an insulating outer layer; b. Connecting the piezoelectric ceramic sensor (2) to the BNC connector (3): connecting the lead end of the positive wire of the piezoelectric ceramic sensor (2) to the positive terminal of the BNC connector (3), and connecting the lead end of the negative wire of the piezoelectric ceramic sensor (2) to the negative terminal of the BNC connector (3); c. Select the type of FRP reinforcement (1), and open a notch (11) on the surface of the selected FRP reinforcement (1) using a high-precision laser cutting machine; d. Ratio test of encapsulating material and selection of ratio: a resin material identical to the base resin material of the selected FRP bar (1) is selected as the resin material of the encapsulating material, and the resin material for the encapsulating material and the curing agent are mixed and stirred in seven groups, wherein the ratio of the resin material for the encapsulating material to the curing agent in the first group is 4:1, the ratio of the resin material for the encapsulating material to the curing agent in the second group is 3:1, the ratio of the resin material for the encapsulating material to the curing agent in the third group is 2:1, the ratio of the resin material for the encapsulating material to the curing agent in the fourth group is 1:1, the ratio of the resin material for the encapsulating material to the curing agent in the fifth group is 1:2, the ratio of the resin material for the encapsulating material to the curing agent in the sixth group is 1:3, and the ratio of the resin material for the encapsulating material to the curing agent in the seventh group is 1:

4. The encapsulating materials of each group after mixing the resin material and the curing agent are placed in an environment at a temperature of 22°C for curing, and the curing time of each group of encapsulating materials is measured; After the curing time of each group of packaging materials is determined, the packaging material with a curing time of 4h-8h is selected as the backup packaging material; e. The piezoelectric ceramic sensor (2) is completely embedded in the notch (11) of the FRP rib (1), and then the selected spare packaging material is filled into the notch (11) of the FRP rib (1). After the packaging material layer (4) in the notch (11) is solidified, a packaging material layer (4) is formed. The piezoelectric ceramic sensor (2) is fixed in the notch (11) of the FRP rib (1) by the packaging material layer (4). The surface of the packaging material layer (4) is flush with the surface of the FRP rib (1), and the positive and negative wires of the piezoelectric ceramic sensor (2) are respectively extended to the outside of the packaging material layer (4). The self-sensing FRP rib (1) is prepared; f. Using the impedance method to monitor the wear of the self-sensing FRP tendon (1): connect the BNC connector (3) of the piezoelectric ceramic sensor (2) to the impedance tester (5), obtain the resistance-frequency spectra at different times, observe the resistance-frequency spectra, and analyze the wear degree of the FRP tendon (1) at different times based on the number, size and offset of the resonance peaks; Alternatively, a wave method is used to monitor the wear of a self-sensing FRP rib (1): the self-sensing FRP rib (1) is provided with two notches (11), each notch (11) is respectively embedded with a piezoelectric ceramic sensor (2) fixed by a packaging material layer (4), a BNC connector (3) of one piezoelectric ceramic sensor (2) is connected to the transmitting end of a NIUSB-6366 data acquisition card (6), and a BNC connector (3) of another piezoelectric ceramic sensor (2) is connected to the receiving end of the NIUSB-6366 data acquisition card (6), and the NIUSB-6366 data acquisition card (6) is connected to a computer (7); after the BNC connector (3) and the NIUSB-6366 data acquisition card (6) are connected, After the card (6) and the computer (7) are connected, the same signal excitation is selected to act on the piezoelectric ceramic sensor (2) connected to the transmitting end of the NIUSB-6366 data acquisition card (6). At this time, the piezoelectric ceramic sensor (2) connected to the transmitting end of the NIUSB-6366 data acquisition card (6) vibrates and generates a stress wave. The stress wave propagates along the FRP tendon (1) and is received by the piezoelectric ceramic sensor (2) connected to the receiving end of the NIUSB-6366 data acquisition card (6). The NIUSB-6366 data acquisition card (6) sends the received data to the computer (7) at the receiving end. The computer (7) determines the degree of wear of the FRP tendon (1) based on the difference in signals received at different times. Alternatively, a wave method is used to monitor the interface damage between the FRP bar (1) and the self-compacting concrete: a bond slip specimen is prepared by using the self-sensing FRP bar (1) and the self-compacting concrete. Before preparing the bond slip specimen, an intelligent aggregate sensor (8) is embedded in the center of the specimen near the FRP bar (1). The piezoelectric ceramic sensor (2) embedded in the notch (11) of the FRP bar (1) is located outside the self-compacting concrete specimen, wherein the positive terminal of the intelligent aggregate sensor (8) is connected to the positive terminal of the BNC connector (3) through a wire, and the negative terminal of the intelligent aggregate sensor (8) is connected to the negative terminal of the BNC connector (3) through a wire. After the preparation of the bond slip specimen is completed, the BNC connector (3) of the piezoelectric ceramic sensor (2) on the FRP bar (1) is connected to the transmitting end of the NIUSB-6366 data acquisition card (6), and the B The NC connector (3) is connected to the receiving end of the NIUSB-6366 data acquisition card (6), and the NIUSB-6366 data acquisition card (6) is connected to the computer (7); after the BNC connector (3), the NIUSB-6366 data acquisition card (6), and the computer (7) are connected, the bond slip specimen is installed on a tensile testing machine and a pull-out test is performed on the tensile testing machine. During the pull-out test on the tensile testing machine, the same signal is selected to excite the piezoelectric ceramic sensor (2) on the FRP bar (1). At this time, the piezoelectric ceramic sensor (2) vibrates and generates stress waves. The stress waves propagate in the FRP bar (1), the interface between the FRP bar (1) and the self-compacting concrete, and the self-compacting concrete. The intelligent aggregate sensor (8) receives the stress waves and judges the degree of damage to the interface between the FRP bar (1) and the self-compacting concrete according to the difference in signal amplitude and frequency shift received at different times.

2. The method for using a self-sensing FRP rib embedded with a piezoelectric ceramic sensor according to claim 1, characterized in that: The FRP bars (1) are glass fiber reinforced bars or basalt fiber reinforced bars.

3. The method for using a self-sensing FRP rib embedded with a piezoelectric ceramic sensor according to claim 1, characterized in that: The depth of the notch (11) of the FRP bar (1) is less than one third of the diameter of the FRP bar (1).

4. The method for using a self-sensing FRP rib embedded with a piezoelectric ceramic sensor according to claim 1, characterized in that: The surface of the FRP bar (1) is provided with slots (11) arranged in sequence and at intervals along the length direction of the FRP bar (1), and the distance between two adjacent slots (11) is greater than 30 cm.

5. The method for using the self-sensing FRP rib embedded with a piezoelectric ceramic sensor according to claim 1, characterized in that: The surface of the packaging material layer (4) is flush with the surface of the FRP rib (1).

6. The method for using the self-sensing FRP rib embedded with a piezoelectric ceramic sensor according to claim 1, characterized in that: The thickness of the piezoelectric ceramic sheet (21) is less than 1.2 mm, and the thickness of the copper shell (22) is less than 0.02 mm.

7. The method for using the self-sensing FRP rib embedded with a piezoelectric ceramic sensor according to claim 1, characterized in that: In the process of using the wave method to monitor the wear of the self-sensing FRP bar (1), in order to quantify the degree of damage at the interface between the FRP bar (1) and the self-compacting concrete, a wavelet energy ratio index is proposed and symbolized by K. i express; Each time the received signal S is decomposed into n+1 frequency bands by n-level wavelet, the signal X in each frequency band j Expressed as: X j =[X j,1 ,X j,2 ,……,X j,m ]; where j represents the frequency band, j=1,2,…,n+1, and m represents the amount of sampled data; The energy of each frequency band is expressed as: Where i represents the time index; According to the energy of each frequency band, the total energy of the signal received for the i-th time can be expressed as: In order to accurately reflect the damage degree of the interface between FRP bars (1) and self-compacting concrete in the pull-out test, the wavelet energy ratio index is defined as: K i =E i / E0; where E i represents the total wavelet energy at different time indices, and E0 represents the total wavelet energy in the healthy state with a load of 0 kN; The wavelet energy ratio at different time indices is calculated as a quantitative index, and the bond-slip curve of the FRP bar (1) and the self-compacting concrete and the wavelet energy ratio index-slip curve are plotted in the same figure; when the bond stress reaches the peak value, the wavelet energy ratio index begins to degenerate rapidly, which indicates the failure of the interface bond between the FRP bar (1) and the self-compacting concrete; the wavelet energy ratio index can be used to quantify the damage condition of the interface between the FRP bar (1) and the self-compacting concrete, lock the moment of bond degradation, and fully understand the internal interface condition of the structure, thereby providing a basis for the macroscopic mechanical analysis of the structure.