Composite glass and its preparation method and application
By alternately setting multiple refractive layers with different refractive indexes on the glass substrate, high reflection of ultraviolet light and low reflection of visible light are achieved, which solves the problem of high reflectivity of existing ultraviolet-proof glasses to visible light and is neutral. color meets the needs of neutral color glass.
Patent Information
- Application Number
- CN201911087975.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-11-08
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2039-11-08
AI Technical Summary
While reflecting ultraviolet light, existing ultraviolet glasses also have a high reflective effect on visible light, affecting transmission, and most ultraviolet glasses are non-neutral, which cannot meet the needs of neutral glasses.
The composite glass with a multi-layer refractive layer structure is controlled by alternately setting the first refractive layer with a refractive index of 2.0 to 2.5 and the second refractive layer with a refractive index of 1.47 to 1.53 on the glass substrate to control the thickness of each layer so that the composite glass is It has a high reflectivity to ultraviolet light, a low reflectivity to visible light, and is neutral.
The reflectivity reaches more than 65% in the wavelength range of 300 to 380nm, and the reflectivity to visible light is 8%±0.1%. The appearance shows a natural neutral color close to the original sheet of float glass, meeting the needs of neutral glass, and Improves the weather resistance and production efficiency of the product.
Smart Images

Figure CN110746121B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, and in particular to a composite glass and a preparation method and application thereof. Background Art
[0002] In the energy radiation of the sun, most of the energy is distributed in the visible light band, ultraviolet light band and infrared light band. Among them, the ultraviolet band has the shortest wavelength, the highest energy and the strongest radiation damage. Ultraviolet radiation will cause the skin to produce a large number of free radicals, leading to peroxidation of the cell membrane and causing melanocytes to produce more melanin. Long-term ultraviolet radiation can cause sunburn, microvascular dilation, dermatitis, and even carcinogenicity. Therefore, the development of anti-ultraviolet glass is of great significance. However, although the existing anti-ultraviolet glass has a certain performance of shielding ultraviolet light, it also has a high reflective effect on visible light, which affects the transmission of visible light, and most anti-ultraviolet glass is non-neutral in color and cannot meet the demand for neutral color glass. Summary of the invention
[0003] Based on this, it is necessary to provide a composite glass that can reflect ultraviolet rays, has a low reflectivity to visible light and is roughly neutral in color, as well as a preparation method and application thereof.
[0004] A composite glass comprises: a glass substrate, a plurality of first refractive layers and a plurality of second refractive layers, wherein the first refractive layers and the second refractive layers are alternately stacked on the glass substrate, the number of refractive layers is greater than or equal to 3, the refractive index of the first refractive layer is 2.0-2.5, the thickness of the first refractive layer is 20nm-70nm, and the thickness of each first refractive layer is different, the refractive index of each second refractive layer is 1.47-1.53, the thickness of the second refractive layer is 20nm-120nm, and the thickness of each second refractive layer is different.
[0005] In the composite glass, by alternately arranging a first refractive layer with a refractive index of 2.0 to 2.5 and a second refractive layer with a refractive index of 1.47 to 1.53 on a glass substrate, and controlling the thickness of the first refractive layer and the second refractive layer, the composite glass has a high reflectivity to ultraviolet light, a low reflectivity to visible light, and is roughly neutral in color. According to experimental verification, the composite glass has a reflectivity of more than 65% in the wavelength range of 300 to 380 nm, a reflectivity of 8% ± 0.1% to visible light, which is equivalent to the reflectivity of the original glass sheet, and the a value in the LAB value of the composite glass is -0.8 to -0.1, and the appearance presents a natural neutral color close to that of the original float glass sheet.
[0006] In one embodiment, the material of the first refractive layer is Si3N4, Nb2O5 or TiO2;
[0007] And / or, the material of the second refractive layer is SiO2.
[0008] In one embodiment, the first refractive layer and the second refractive layer are alternately stacked to form a stacked body, and the first refractive layer and the second refractive layer are respectively provided at two ends of the stacked body in a stacking direction of the stacked body.
[0009] In one embodiment, the first refractive layer located at one end of the stacked body is directly disposed on the glass substrate.
[0010] In one embodiment, the thickness of the second refractive layer farthest from the glass substrate is greater than the thickness of the remaining second refractive layers.
[0011] In one embodiment, the thickness of the second refractive layer farthest from the glass substrate is 90 nm to 120 nm, and the thickness of the remaining second refractive layers is 20 nm to 70 nm;
[0012] Alternatively, the thickness of the second refractive layer farthest from the glass substrate is 70 nm to 110 nm, and the thickness of the remaining second refractive layers is 20 nm to 60 nm.
[0013] In one of the embodiments, in a direction in which the stacked body is away from the glass substrate, the thickness of the multiple layers of the first refractive layers gradually increases.
[0014] In one embodiment, the first refractive layer has 2 to 5 layers, and the second refractive layer has 2 to 5 layers.
[0015] In one embodiment, the first refractive layer has two layers, the second refractive layer has two layers, in the direction of the stack away from the glass substrate, the thicknesses of the two first refractive layers are 20nm-50nm and 30nm-60nm respectively, the thicknesses of the two second refractive layers are 30nm-60nm and 90nm-120nm respectively, the material of each first refractive layer is Nb2O5, and the material of each second refractive layer is SiO2.
[0016] In one embodiment, the first refractive layer has three layers, the second refractive layer has three layers, in the direction of the stack away from the glass substrate, the thicknesses of the three first refractive layers are 20nm-50nm, 30nm-60nm and 20nm-60nm, respectively, the thicknesses of the three second refractive layers are 40nm-70nm, 20nm-50nm and 90nm-120nm, respectively, the material of each first refractive layer is Si3N4, and the material of each second refractive layer is SiO2.
[0017] In one embodiment, the first refractive layer has three layers, the second refractive layer has three layers, in the direction of the stack away from the glass substrate, the thicknesses of the three first refractive layers are 20nm-50nm, 30nm-60nm and 20nm-60nm, respectively, the thicknesses of the three second refractive layers are 35nm-60nm, 20nm-50nm and 90nm-120nm, respectively, the material of each first refractive layer is Nb2O5, and the material of each second refractive layer is SiO2.
[0018] In one embodiment, the first refractive layer has four layers, and the second refractive layer has four layers. In the direction of the stack away from the glass substrate, the thicknesses of the four first refractive layers are 20nm-60nm, 30nm-60nm, 20nm-60nm and 40nm-80nm, respectively, and the thicknesses of the four second refractive layers are 30nm-60nm, 20nm-60nm, 20nm-50nm and 70nm-110nm, respectively. The material of each first refractive layer is Si3N4 or Nb2O5, and the material of each second refractive layer is SiO2.
[0019] In one embodiment, the first refractive layer and the second refractive layer are alternately stacked to form a stacked body, and the composite glass further includes a protective layer, and the protective layer covers the stacked body.
[0020] In one embodiment, the material of the protective layer is ZrO2, Si3N4 or SiC;
[0021] And / or, the thickness of the protective layer is 5 nm to 10 nm.
[0022] A method for preparing composite glass comprises the following steps:
[0023] A first refractive layer and a second refractive layer are alternately stacked on a glass substrate, the number of the refractive layers is greater than or equal to 3, the refractive index of the first refractive layer is 2.0-2.5, the thickness of the first refractive layer is 20nm-80nm, and the thickness of each first refractive layer is different, the refractive index of the second refractive layer is 1.47-1.53, the thickness of the second refractive layer is 20nm-120nm, and the thickness of each second refractive layer is different.
[0024] In one embodiment, the first refractive layer and the second refractive layer that are alternately stacked are formed on the glass substrate by magnetron sputtering.
[0025] In one embodiment, the laminated body formed by alternately stacking the first refractive layer and the second refractive layer further comprises the following step after the step of forming the first refractive layer and the second refractive layer alternately stacked on the glass substrate: forming a protective layer on a side of the laminated body away from the glass substrate, wherein the protective layer covers the laminated body.
[0026] A glass product comprises the composite glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is a schematic cross-sectional view of a composite glass according to an embodiment;
[0028] Figure 2 is a schematic cross-sectional view of a composite glass according to another embodiment;
[0029] Figure 3 is a schematic cross-sectional view of a composite glass according to another embodiment;
[0030] Figure 4 is a schematic cross-sectional view of a composite glass according to another embodiment;
[0031] Figure 5 is a schematic cross-sectional view of a composite glass according to another embodiment;
[0032] Figure 6 is a schematic cross-sectional view of a composite glass according to another embodiment;
[0033] Figure 7 is a reflection spectrum diagram of the composite glass of Example 1 in the range of 300nm to 1200nm;
[0034] Figure 8 is a reflection spectrum diagram of the composite glass of Example 2 in the range of 300nm to 1200nm;
[0035] Fig. 9 is a reflection spectrum diagram of the composite glass of Example 3 in the range of 300nm to 1200nm;
[0036] Fig.10 is a reflection spectrum diagram of the composite glass of Example 4 in the range of 300nm to 1200nm;
[0037] Fig.11 This is a reflection spectrum diagram of the composite glass of Example 5 in the range of 300nm to 1200nm. DETAILED DESCRIPTION
[0038] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Preferred embodiments of the present invention are provided in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0040] like Figure 1 As shown, the composite glass 100 of one embodiment can reflect ultraviolet rays, has a low reflectivity to visible light and is approximately neutral in color, and can be applied to glass products such as building curtain wall glass, decorative glass, and functional glass that need to reflect ultraviolet rays or cut off ultraviolet transmission. Furthermore, the composite glass 100 can be used as a single piece, or can be used to make hollow or laminated glass products.
[0041] The composite glass 100 includes a glass substrate 110, a plurality of first refractive layers 121, and a plurality of second refractive layers 123. The first refractive layers 121 and the second refractive layers 123 are alternately stacked on the glass substrate 110. The number of refractive layers is greater than or equal to 3. The refractive index of the first refractive layer 121 is 2.0 to 2.5. The thickness of the first refractive layer 121 is 20 nm to 80 nm. The thickness of each first refractive layer 121 is different. The refractive index of the second refractive layer 123 is 1.47 to 1.53. The thickness of the second refractive layer 123 is 20 nm to 120 nm. The thickness of each second refractive layer 123 is different.
[0042] In the composite glass 100, by alternately arranging the first refractive layer 121 with a refractive index of 2.0 to 2.5 and the second refractive layer 123 with a refractive index of 1.47 to 1.53 on the glass substrate 110, and controlling the thickness of the first refractive layer 121 and the second refractive layer 123, the composite glass 100 has a higher reflectivity to ultraviolet light, a lower reflectivity to visible light, and is approximately neutral in color.
[0043] The glass substrate 110 is used to support the first refractive layer 121 and the second refractive layer 123 .
[0044] In one embodiment, the thickness of the glass substrate 110 is 2 mm to 19 mm. In some embodiments, the thickness of the glass substrate 110 is 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 8 mm, 10 mm, 12 mm, 15 mm or 19 mm. It should be noted that the thickness of the glass substrate 110 is not limited to the above range and can be set as needed.
[0045] In one embodiment, the maximum width of the glass substrate 110 is 3300 mm, and the maximum length of the glass substrate 110 is 6000 mm. This configuration enables the composite glass 100 to be cut into other small sizes and can be safely used in subsequent cutting, edge grinding, tempering and other processes to achieve mass production.
[0046] In one embodiment, the material of the first refractive layer 121 is Si3N4, Nb2O5 or TiO2, and the material of the second refractive layer 123 is SiO2. This arrangement is conducive to improving the reflectivity of the composite glass 100 to ultraviolet light and the transmittance of visible light, and makes the composite glass 100 roughly neutral in color, so that the composite glass 100 has excellent weather resistance, so that the composite glass 100 can be used in different environments, and the materials of the first refractive layer 121 and the second refractive layer 123 are both environmentally friendly materials, which is conducive to the large-scale preparation of the composite glass 100. Some studies use HfO2 and MgF2 to make the composite glass 100, but these materials pollute the environment, are not suitable for large-area coating, and are difficult to mass produce.
[0047] See also Figure 1 The first refractive layer 121 and the second refractive layer 123 are alternately stacked to form a stacked body 120. The two ends of the stacked body 120 in the stacking direction of the stacked body 120 are the first refractive layer 121 and the second refractive layer 123 respectively. This arrangement is conducive to improving the reflectivity of the composite glass 100 to ultraviolet light and the transmittance of visible light.
[0048] It should be noted that the two ends of the stacked body 120 in the stacking direction of the stacked body 120 are not limited to being the first refractive layer 121 and the second refractive layer 123. The two ends of the stacked body 120 in the stacking direction of the stacked body 120 may also be the first refractive layer 121 (e.g. Figure 2 As shown), both ends of the stacked body 120 in the stacking direction of the stacked body 120 may also be the second refractive layer 123 (as shown Figure 3 shown).
[0049] See also Figures 1-2Furthermore, the first refractive layer 121 at one end of the laminate 120 is directly disposed on the glass substrate 110. This arrangement is conducive to improving the reflectivity of ultraviolet light and the transmittance of visible light of the composite glass 100. It should be noted that the first refractive layer 121 at one end of the laminate 120 is not limited to being directly disposed on the glass substrate 110, and the second refractive layer 123 at one end of the laminate 120 may also be directly disposed on the glass substrate 110 (e.g. Figure 3 shown).
[0050] The thickness of the second refractive layer 123 farthest from the glass substrate 110 is greater than the thickness of the remaining second refractive layers 123. This arrangement is beneficial to improving the reflectivity of the composite glass 100 to ultraviolet light.
[0051] In one embodiment, the thickness of the second refractive layer 123 farthest from the glass substrate 110 is 90nm-120nm, and the thickness of the remaining second refractive layers 123 is 20nm-70nm. This configuration is beneficial to improving the reflectivity of the composite glass 100 to ultraviolet light and the transmittance of visible light.
[0052] In one embodiment, the thickness of the second refractive layer 123 farthest from the glass substrate 110 is 70nm-110nm, and the thickness of the remaining second refractive layers 123 is 20nm-60nm. This configuration is beneficial to improving the reflectivity of the composite glass 100 to ultraviolet light and the transmittance of visible light.
[0053] The thickness of the multiple first refractive layers 121 gradually increases in the direction of the laminate 120 away from the glass substrate 110. This arrangement is beneficial to improving the reflectivity of the composite glass 100 to ultraviolet light and the transmittance of visible light.
[0054] In one embodiment, the first refractive layer 121 has 2 to 5 layers, and the second refractive layer 123 has 2 to 5 layers. This arrangement is beneficial to improving the reflectivity of the composite glass 100 to ultraviolet light.
[0055] See also Figure 1 In one embodiment, the first refractive layer 121 has two layers, and the second refractive layer 123 has two layers. In the direction of the laminate 120 away from the glass substrate 110, the thickness of the two first refractive layers 121 is 20nm-50nm and 30nm-60nm respectively, and the thickness of the two second refractive layers 123 is 30nm-60nm and 90nm-120nm respectively. The material of each first refractive layer 121 is Nb2O5, and the material of each second refractive layer 123 is SiO2. This arrangement is conducive to improving the reflectivity of the composite glass 100 to ultraviolet light and making the composite glass 100 substantially neutral in color.
[0056] See also Figure 4 In one embodiment, the first refractive layer 121 has three layers, and the second refractive layer 123 has three layers. In the direction of the laminate 120 away from the glass substrate 110, the thicknesses of the three first refractive layers 121 are 20nm-50nm, 30nm-60nm and 20nm-60nm, respectively, and the thicknesses of the three second refractive layers 123 are 40nm-70nm, 20nm-50nm and 90nm-120nm, respectively. The material of each first refractive layer 121 is Si3N4, and the material of each second refractive layer 123 is SiO2. This arrangement is conducive to improving the reflectivity of the composite glass 100 to ultraviolet light and making the composite glass 100 substantially neutral in color.
[0057] See also Figure 4 In one embodiment, the first refractive layer 121 has three layers, and the second refractive layer 123 has three layers. In the direction of the laminate 120 away from the glass substrate 110, the thicknesses of the three first refractive layers 121 are 20nm-50nm, 30nm-60nm and 20nm-60nm, respectively, and the thicknesses of the three second refractive layers 123 are 35nm-60nm, 20nm-50nm and 90nm-120nm, respectively. The material of each first refractive layer 121 is Nb2O5, and the material of each second refractive layer 123 is SiO2. This arrangement is conducive to improving the reflectivity of the composite glass 100 to ultraviolet light, so that the composite glass 100 is approximately neutral in color.
[0058] See also Figure 5 In one embodiment, the first refractive layer 121 has four layers, and the second refractive layer 123 has four layers. In the direction of the laminate 120 away from the glass substrate 110, the thicknesses of the four first refractive layers 121 are 20nm-60nm, 30nm-60nm, 20nm-60nm and 40nm-80nm, respectively, and the thicknesses of the four second refractive layers 123 are 30nm-60nm, 20nm-60nm, 20nm-50nm and 70nm-110nm, respectively. The material of each first refractive layer 121 is Si3N4 or Nb2O5, and the material of each second refractive layer 123 is SiO2. This arrangement is conducive to improving the reflectivity of the composite glass 100 to ultraviolet light, so that the composite glass 100 is approximately neutral in color.
[0059] See also Figure 6The composite glass 100 further includes a protective layer 130. The protective layer 130 covers the laminate 120. By providing the protective layer 130, the laminate 120 can be protected and the laminate 120 can be prevented from being scratched or chemically corroded, so as to ensure the integrity of the glass during transportation, installation and use, and enable the composite glass 100 to be used in an outdoor environment. In the illustrated embodiment, the protective layer 130 covers the second refractive layer 123 farthest from the glass substrate 110. It can be understood that the protective layer 130 can be omitted.
[0060] In one embodiment, the material of the protective layer 130 is ZrO2, Si3N4 or SiC. The protective layer 130 configured in this way has the properties of scratch resistance, abrasion resistance and corrosion resistance, and can better protect the layer 130 stack 120.
[0061] In one embodiment, the thickness of the protective layer 130 is 5 nm to 10 nm. This configuration can better protect the layer 130 stack 120 to ensure the integrity and service life of the composite glass 100.
[0062] In the composite glass 100, the first refractive layer 121 with a refractive index of 2.0 to 2.5 and the second refractive layer 123 with a refractive index of 1.47 to 1.53 are alternately arranged on the glass substrate 110, and the thickness of the first refractive layer 121 and the second refractive layer 123 are controlled, so that the composite glass 100 has a high reflectivity to ultraviolet light, a low reflectivity to visible light, and is approximately neutral in color. According to experimental verification, the reflectivity of the composite glass 100 in the wavelength range of 300 to 380 nm is above 65%, and the reflectivity to visible light is 8%±0.1%, which is equivalent to the reflectivity of the original glass sheet, and the a value in the LAB value of the composite glass 100 is -0.8 to -0.1, and the appearance presents a natural neutral color close to the original float glass sheet.
[0063] Some studies use tantalum oxide as a high refractive layer and a low refractive layer to make a composite glass 100. However, such composite glasses 100 are all non-neutral in color and cannot achieve an optical effect similar to that of the original float glass in the visible light range. Moreover, such composite glasses 100 require 10 to 20 layers of tantalum oxide and 10 to 20 layers of low refractive layers to meet the reflection of ultraviolet light. From the perspective of production technology, the larger the number of film layers, the narrower the production process window and the greater the difficulty of large-scale production. However, this study selects appropriate materials and the thickness of each film layer to make the composite glass 100 have a higher reflectivity for ultraviolet light and a lower reflectivity for visible light, and is roughly neutral in color. In addition, the first refractive layer 121 in the composite glass 100 of this study has 2 to 5 layers, and the second refractive layer 123 has 2 to 5 layers, which is conducive to large-scale and mass production of composite glass 100.
[0064] The total thickness of the film layer of the traditional composite glass 100 is relatively thick, the production efficiency is relatively low, the film layer material is limited, it is difficult to produce large-area and large-size products, the film layer is easily damaged during the subsequent processing, the product processability is not strong, and the product does not have the optical properties of the original glass sheet in the visible light range. In the composite glass 100 of the above embodiment, the physical principle of optical interference is applied to make the reflectivity of the coated glass in the wavelength range of 300 to 380nm above 65%, and in the visible light wavelength range, it has a reflectivity value of 8% ± 0.1% equivalent to the reflectivity of the float glass original sheet, and at the same time, it presents a natural neutral color close to the float glass original sheet in appearance. The thickness of the laminated body 120 of the composite glass 100 of the above embodiment is nanometer-level, and the laminated body 120 does not contain precious metals such as Ag and Au, which greatly reduces the production cost.
[0065] The method for preparing the composite glass 100 of the above embodiment includes the following steps: forming first refractive layers 121 and second refractive layers 123 alternately stacked on a glass substrate 110 , wherein the number of the refractive layers is greater than or equal to 3.
[0066] Among them, the refractive index of the first refractive layer 121 is 2.0-2.5, the thickness of the first refractive layer 121 is 20nm-80nm, and the thickness of each first refractive layer 121 is different. The refractive index of the second refractive layer 123 is 1.47-1.53, the thickness of the second refractive layer 123 is 20nm-120nm, and the thickness of each second refractive layer 123 is different.
[0067] The structure of the composite glass 100 has been described above and will not be described again here.
[0068] In one embodiment, the first refractive layer 121 and the second refractive layer 123 are formed alternately on the glass substrate 110 by magnetron sputtering. Further, the first refractive layer 121 and the second refractive layer 123 are formed alternately on the glass substrate 110 by medium frequency vacuum magnetron sputtering. Furthermore, the background vacuum degree is 10 -6 mbar~10 -7 mbar. The sputtering vacuum is 3×10 -3 mbar~8×10 -3 The deposition rate of each first refractive layer 121 is 2.8 nm (m / min) / KW to 4.5 nm (m / min) / KW. The deposition rate of each second refractive layer 123 is 2.8 nm (m / min) / KW to 4.5 nm (m / min) / KW.
[0069] In a specific example, the step of forming the first refractive layer 121 and the second refractive layer 123 alternately stacked on the glass substrate 110 includes: placing the glass substrate 110 in a magnetron sputtering coating area of a magnetron sputtering coating arrangement, and coating the first refractive layer 121 and the second refractive layer 123 alternately stacked on the glass substrate 110 using a medium frequency AC power supply and a rotating cathode.
[0070] In one embodiment, after the step of forming the first refractive layer 121 and the second refractive layer 123 alternately stacked on the glass substrate 110, the stacked body 120 further includes the following step: forming a protective layer 130 on the side of the stacked body 120 away from the glass substrate 110, wherein the protective layer 130 covers the stacked body 120. Further, the protective layer 130 is formed by magnetron sputtering. Furthermore, the background vacuum degree is 10 - 6 mbar~10 -7 mbar. The sputtering vacuum is 3×10 -3 mbar~8×10 -3 The deposition rate of the protective layer 130 is 2.8 nm (m / min) / KW to 4.5 nm (m / min) / KW.
[0071] In one embodiment, before the step of forming the first refractive layer 121 and the second refractive layer 123 alternately stacked on the glass substrate 110, the following step is further included: cleaning the glass substrate 110. The dirt on the surface of the glass substrate 110 is removed by cleaning to facilitate the deposition of the first refractive layer 121 and the second refractive layer 123. Furthermore, before the step of forming the first refractive layer 121 and the second refractive layer 123 alternately stacked on the glass substrate 110, after the step of cleaning the glass substrate 110, the step of polishing the cleaned glass substrate 110 is further included.
[0072] It should be noted that if the glass substrate 110 can meet actual requirements, the steps of cleaning and polishing the glass substrate 110 can be omitted.
[0073] In one embodiment, an automated production line is used to produce the composite glass 100. Specifically, the process flow of the automated production line for producing the composite glass 100 is as follows: a glass substrate 110 is placed on an automatic loading table; an automatic cleaning machine cleans and polishes the glass substrate 110; the glass substrate 110 is dried; a magnetron sputtering coating device is used to coat the dried glass substrate 110 with a first reflective layer, a second reflective layer and a protective layer 130 to obtain the composite glass 100; an automatic unloading table is used to unload and package the glass; and other various sizes of cutting and subsequent processing (cutting, grinding, tempering, etc.) are performed.
[0074] In the preparation method of the above-mentioned composite glass 100, a composite glass 100 with a specific structure is prepared. The obtained composite glass 100 can have a reflectivity of more than 65% at a wavelength of 300nm to 380nm, and a reflectivity of 8%±0.1% in the visible light wavelength range. The appearance color of the composite glass 100 presents a natural neutral color similar to that of the original float glass.
[0075] The composite glass 100 obtained by the method for preparing the composite glass 100 has excellent weather resistance, and different materials of the first refractive layer 121 can be selected to obtain the composite glass 100 that can be stably used in different environments for a long time. The method for preparing the composite glass 100 has a simple process and a short production cycle, which reduces costs and greatly improves production efficiency.
[0076] In the preparation method of the composite glass 100, environmentally friendly solid pure inorganic materials are used to avoid the pollution and damage to the environment and human body caused by organic chemical production raw materials. The obtained composite glass 100 can be used as a single piece or made into hollow or laminated glass products.
[0077] In the preparation method of the above-mentioned composite glass 100, the magnetron sputtering offline coating process can be used to prepare composite glass 100 with a maximum width of 3300 mm and a maximum length of 6000 mm, which has the characteristics of large-area and large-size production, high production efficiency and high yield.
[0078] The following is a specific embodiment:
[0079] If not specifically stated, in the following embodiments, the glass substrate is a white glass sheet with a width of 3300 mm, a length of 6000 mm, and a thickness of 6 mm. The material of the second refractive layer is SiO2.
[0080] Example 1
[0081] The structure of the composite glass of this embodiment is as follows: glass substrate (6mm) / first refractive layer (31.8nm) / second refractive layer (47.2nm) / first refractive layer (46.7nm) / second refractive layer (105nm) / protective layer (5nm) (the “ / ” in the above structure represents stacking), the material of the first refractive layer is Nb2O5, and the material of the protective layer is ZrO2.
[0082] The preparation method of the composite glass of this embodiment is as follows:
[0083] The glass substrate was cleaned and polished, and then dried. A magnetron sputtering process was used to form a first refractive layer of 31.8 nm, a second refractive layer of 47.2 nm, a first refractive layer of 46.7 nm, a second refractive layer of 105 nm, and a protective layer of 5 nm, which were stacked in sequence, on the dried glass substrate to obtain a composite glass. The sputtering vacuum degree was 3×10 -3 mbar~8×10 -3 The deposition rates of the first refractive layers, the second refractive layers and the protective layer are all 2.8 nm (m / min) / KW to 4.5 nm (m / min) / KW.
[0084] test:
[0085] The reflectance spectrum of the composite glass in the range of 300nm to 1200nm was measured by a PerkinElmer Lambda 950 UV-visible spectrophotometer, and the chromaticity coordinate parameters of the composite glass in the visible light wavelength range were measured by a Datacolor 650 colorimeter. The measurement results are shown in Tables 1 and Figure 7 Table 1 shows the chromaticity coordinate parameters of the composite glass of Example 1 in the visible light wavelength range and the reflectivity at 300nm to 380nm. Figure 7 It shows the reflection spectrum of the composite glass of Example 1 in the range of 300nm to 1200nm, wherein "R%" represents the reflectivity and "Wavelength" represents the wavelength.
[0086] Table 1
[0087]
[0088] From Table 1 and Figure 7 It can be seen that the composite glass of Example 1 has a reflectivity of 66.8% at 300nm-380nm, has a high reflectivity for ultraviolet light, a reflectivity of 8.05% for visible light, a transmittance of 90.8% for visible light, and is neutral in appearance color.
[0089] Example 2
[0090] The structure of the composite glass of this embodiment is as follows: glass substrate (6mm) / first refractive layer (34.8nm) / second refractive layer (45.2nm) / first refractive layer (38.1nm) / second refractive layer (30.6nm) / first refractive layer (42.6nm) / second refractive layer (108.2nm) / protective layer (5nm) (in the above structure, “ / ” represents stacking), the material of the first refractive layer is Nb2O5, and the material of the protective layer is ZrO2.
[0091] The preparation method of the composite glass of this embodiment is as follows:
[0092] The glass substrate was cleaned and polished, and then dried. A first refractive layer of 34.8 nm, a second refractive layer of 45.2 nm, a first refractive layer of 38.1 nm, a second refractive layer of 30.6 nm, a first refractive layer of 42.6 nm, a second refractive layer of 108.2 nm, and a protective layer of 5 nm were stacked in sequence on the dried glass substrate by magnetron sputtering to obtain a composite glass. The sputtering vacuum degree was 3×10 -3 mbar~8×10 -3 The deposition rates of the first refractive layers, the second refractive layers and the protective layer are all 2.8 nm (m / min) / KW to 4.5 nm (m / min) / KW.
[0093] test:
[0094] The reflectance spectrum of the composite glass in the range of 300nm to 1200nm was measured by a PerkinElmer Lambda 950 UV-visible spectrophotometer, and the chromaticity coordinate parameters of the composite glass in the visible light wavelength range were measured by a Datacolor 650 colorimeter. The measurement results are detailed in Table 2 and Figure 8 Table 2 shows the chromaticity coordinate parameters of the composite glass of Example 2 in the visible light wavelength range and the reflectivity at 300nm to 380nm. Figure 8 It shows the reflection spectrum of the composite glass of Example 2 in the range of 300nm to 1200nm, wherein "R%" represents the reflectivity and "Wavelength" represents the wavelength.
[0095] Table 2
[0096]
[0097] From Table 2 and Figure 8 It can be seen that the composite glass of Example 2 has a reflectivity of 85.2% at 300nm-380nm, has a high reflectivity for ultraviolet light, a reflectivity of 7.96% for visible light, a transmittance of 91.1% for visible light, and is neutral in appearance color.
[0098] Example 3
[0099] The structure of the composite glass of this embodiment is as follows: glass substrate (6mm) / first refractive layer (36.2nm) / second refractive layer (57nm) / first refractive layer (40.4nm) / second refractive layer (33.4nm) / first refractive layer (50.3nm) / second refractive layer (116.5nm) / protective layer (5nm) (in the above structure, “ / ” represents stacking), the material of the first refractive layer is Si3N4, and the material of the protective layer is ZrO2.
[0100] The preparation method of the composite glass of this embodiment is as follows:
[0101] The glass substrate was cleaned and polished, and then dried. A first refractive layer of 36.2 nm, a second refractive layer of 57 nm, a first refractive layer of 40.4 nm, a second refractive layer of 33.4 nm, a first refractive layer of 50.3 nm, a second refractive layer of 116.5 nm, and a protective layer of 5 nm were stacked in sequence on the dried glass substrate by magnetron sputtering to obtain a composite glass. The sputtering vacuum degree was 3×10 -3 mbar~8×10 -3 The deposition rates of the first refractive layers, the second refractive layers and the protective layer are all 2.8 nm (m / min) / KW to 4.5 nm (m / min) / KW.
[0102] test:
[0103] The reflectance spectrum of the composite glass in the range of 300nm to 1200nm was measured by a PerkinElmer Lambda 950 UV-visible spectrophotometer, and the chromaticity coordinate parameters of the composite glass in the visible light wavelength range were measured by a Datacolor 650 colorimeter. The measurement results are shown in Table 3 and Fig. 9 Table 3 shows the chromaticity coordinate parameters of the composite glass of Example 3 in the visible light wavelength range and the reflectivity at 300nm to 380nm. Fig. 9 It shows the reflection spectrum of the composite glass of Example 3 in the range of 300nm to 1200nm, wherein "R%" represents the reflectivity and "Wavelength" represents the wavelength.
[0104] Table 3
[0105]
[0106] From Table 3 and Fig. 9 It can be seen that the composite glass of Example 3 has a reflectivity of 71.8% at 300nm-380nm, has a high reflectivity for ultraviolet light, a reflectivity of 7.96% for visible light, a transmittance of 89.9% for visible light, and is neutral in appearance color.
[0107] Example 4
[0108] The structure of the composite glass of this embodiment is as follows: glass substrate (6mm) / first refractive layer (31.5nm) / second refractive layer (42.2nm) / first refractive layer (40.7nm) / second refractive layer (48.2nm) / first refractive layer (34.6nm) / second refractive layer (30.5nm) / first refractive layer (65.8nm) / second refractive layer (80.8nm) / protective layer (5nm) (in the above structure, “ / ” represents stacking), the material of the first refractive layer is Nb2O5, and the material of the protective layer is ZrO2.
[0109] The preparation method of the composite glass of this embodiment is as follows:
[0110] The glass substrate was cleaned and polished, and then dried. A first refractive layer of 31.5 nm, a second refractive layer of 42.2 nm, a first refractive layer of 40.7 nm, a second refractive layer of 48.2 nm, a first refractive layer of 34.6 nm, a second refractive layer of 30.5 nm, a first refractive layer of 65.8 nm, a second refractive layer of 80.8 nm, and a protective layer of 5 nm were sequentially stacked on the dried glass substrate by magnetron sputtering to obtain a composite glass. The sputtering vacuum degree was 3×10 -3 mbar~8×10 -3 The deposition rates of the first refractive layers, the second refractive layers and the protective layer are all 2.8 nm (m / min) / KW to 4.5 nm (m / min) / KW.
[0111] test:
[0112] The reflectance spectrum of the composite glass in the range of 300nm to 1200nm was measured by a PerkinElmer Lambda 950 UV-visible spectrophotometer, and the chromaticity coordinate parameters of the composite glass in the visible light wavelength range were measured by a Datacolor 650 colorimeter. The measurement results are shown in Table 4 and Fig.10 Table 4 shows the chromaticity coordinate parameters of the composite glass of Example 4 in the visible light wavelength range and the reflectivity at 300nm to 380nm. Fig.10 It shows the reflection spectrum of the composite glass of Example 4 in the range of 300nm to 1200nm, wherein "R%" represents the reflectivity and "Wavelength" represents the wavelength.
[0113] Table 4
[0114]
[0115] From Table 4 and Fig.10It can be seen that the composite glass of Example 4 has a reflectivity of 92.3% at 300nm-380nm, has a high reflectivity for ultraviolet light, a reflectivity of 8.01% for visible light, a transmittance of 91.3% for visible light, and is neutral in appearance color.
[0116] Example 5
[0117] The structure of the composite glass of this embodiment is as follows: glass substrate (6 mm) / first refractive layer (36.5 nm) / second refractive layer (34.7 nm) / first refractive layer (35.6 nm) / second refractive layer (109.5 nm) (the “ / ” in the above structure represents stacking), and the material of the first refractive layer is TiO2.
[0118] The preparation method of the composite glass of this embodiment is as follows:
[0119] The glass substrate was cleaned and dried, and a first refractive layer of 36.5 nm, a second refractive layer of 34.7 nm, a first refractive layer of 35.6 nm, and a second refractive layer of 109.5 nm were stacked in sequence on the dried glass substrate by magnetron sputtering to obtain a composite glass. The sputtering vacuum degree was 3×10 -3 mbar~8×10 -3 The deposition rates of the first refractive layers, the second refractive layers and the protective layer are all 2.8 nm (m / min) / KW to 4.5 nm (m / min) / KW.
[0120] test:
[0121] The reflectance spectrum of the composite glass in the range of 300nm to 1200nm was measured by a PerkinElmer Lambda 950 UV-visible spectrophotometer, and the chromaticity coordinate parameters of the composite glass in the visible light wavelength range were measured by a Datacolor 650 colorimeter. The measurement results are shown in Table 5 and Fig.11 Table 5 shows the chromaticity coordinate parameters of the composite glass of Example 5 in the visible light wavelength range and the reflectivity at 300nm to 380nm. Fig.11 It shows the reflection spectrum of the composite glass of Example 5 in the range of 300nm to 1200nm, wherein "R%" represents the reflectivity and "Wavelength" represents the wavelength.
[0122] Table 5
[0123]
[0124] From Table 5 and Fig.11It can be seen that the composite glass of Example 5 has a reflectivity of 67.4% at 300nm-380nm, has a high reflectivity for ultraviolet light, a reflectivity for visible light of 8.03%, a transmittance for visible light of 91.3%, and is neutral in appearance color.
[0125] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0126] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A composite glass, characterized in that: include: A glass substrate, a plurality of first refractive layers and a plurality of second refractive layers, wherein the first refractive layers and the second refractive layers are alternately stacked on the glass substrate, the number of refractive layers is greater than or equal to 3, the refractive index of the first refractive layer is 2.0 to 2.5, the thickness of the first refractive layer is 20 nm to 80 nm, and the thickness of each first refractive layer is different, the refractive index of the second refractive layer is 1.47 to 1.53, the thickness of the second refractive layer is 20 nm to 120 nm, and the thickness of each second refractive layer is different; The material of the first refractive layer is Si3N4, Nb2O5 or TiO2; The first refractive layer has 3 to 5 layers, and the second refractive layer has 3 to 5 layers; The reflectivity of the composite glass in the wavelength range of 300-380nm is above 71.8%.
2. The composite glass according to claim 1, characterized in that: The material of the second refractive layer is SiO2.
3. The composite glass according to claim 1, characterized in that: The first refractive layers and the second refractive layers are alternately stacked to form a stacked body, and the first refractive layers and the second refractive layers are respectively provided at two ends of the stacked body in a stacking direction of the stacked body.
4. The composite glass according to claim 3, characterized in that: The first refractive layer located at one end of the stacked body is directly disposed on the glass substrate.
5. The composite glass according to claim 3, characterized in that: The thickness of the second refractive layer farthest from the glass substrate is greater than the thickness of the remaining second refractive layers.
6. The composite glass according to claim 5, characterized in that: The thickness of the second refractive layer farthest from the glass substrate is 90nm to 120nm, and the thickness of the remaining second refractive layers is 20nm to 70nm; Alternatively, the thickness of the second refractive layer farthest from the glass substrate is 70 nm to 110 nm, and the thickness of the remaining second refractive layers is 20 nm to 60 nm.
7. The composite glass according to claim 3, characterized in that: In a direction in which the stacked body is away from the glass substrate, the thicknesses of the plurality of first refractive layers gradually increase.
8. The composite glass according to any one of claims 3 to 7, characterized in that: The first refractive layer has three layers, and the second refractive layer has three layers. In the direction of the stacked body away from the glass substrate, the thicknesses of the three first refractive layers are 20nm-50nm, 30nm-60nm and 20nm-60nm, respectively, and the thicknesses of the three second refractive layers are 40nm-70nm, 20nm-50nm and 90nm-120nm, respectively. The material of each first refractive layer is Si3N4, and the material of each second refractive layer is SiO2.
9. The composite glass according to any one of claims 3 to 7, characterized in that: The first refractive layer has four layers, and the second refractive layer has four layers. In the direction of the stacked body away from the glass substrate, the thicknesses of the four first refractive layers are 20nm-60nm, 30nm-60nm, 20nm-60nm and 40nm-80nm, respectively, and the thicknesses of the four second refractive layers are 30nm-60nm, 20nm-60nm, 20nm-50nm and 70nm-110nm, respectively. The material of each first refractive layer is Si3N4, and the material of each second refractive layer is SiO2.
10. The composite glass according to claim 1, characterized in that: The first refractive layers and the second refractive layers are alternately stacked to form a stacked body. The composite glass further includes a protective layer, and the protective layer covers the stacked body.
11. The composite glass according to claim 10, characterized in that: The material of the protective layer is ZrO2, Si3N4 or SiC; And / or, the thickness of the protective layer is 5 nm to 10 nm.
12. A method for preparing the composite glass according to any one of claims 1 to 11, characterized in that: The steps include: A first refractive layer and a second refractive layer are alternately stacked on a glass substrate, the number of the refractive layers is greater than or equal to 3, the refractive index of the first refractive layer is 2.0-2.5, the thickness of the first refractive layer is 20nm-80nm, and the thickness of each first refractive layer is different, the refractive index of the second refractive layer is 1.47-1.53, the thickness of the second refractive layer is 20nm-120nm, and the thickness of each second refractive layer is different.
13. The method for preparing composite glass according to claim 12, characterized in that: The first refractive layer and the second refractive layer are formed alternately stacked on the glass substrate by magnetron sputtering.
14. The method for preparing composite glass according to claim 12, characterized in that: The laminated body formed by alternately stacking the first refractive layer and the second refractive layer further comprises the following step after the step of forming the first refractive layer and the second refractive layer alternately stacked on the glass substrate: forming a protective layer on a side of the laminated body away from the glass substrate, wherein the protective layer covers the laminated body.
15. A glass product, characterized in that: The composite glass comprises the composite glass according to any one of claims 1 to 11.
Citation Information
Patent Citations
Anti-reflective films
CA2294127A1
Method for preparing anti-reflection glass and anti-reflection glass
CN110357452A
Improvements in or related to coated glass
GB9707135D0
Solar control coatings and coated articles
WO2000027771A1
Low-reflection coating glass
WO2018147666A1