Gold-tin solder laser attachment assembly for ceramic cover plate and attachment method thereof
Through the laser attachment assembly and attachment method of the gold-tin solder of the ceramic cover plate, the positioning groove of the lower module and the laser welding gun of the upper module are used to realize the precise attachment of the gold-tin solder, which solves the problem of the number of patches and positioning accuracy in the prior art. The problem of low increases the efficiency and accuracy of the packaging process.
Patent Information
- Application Number
- CN201911365237.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-12-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2039-12-26
AI Technical Summary
During the packaging of existing optical communication chips, the number of patches of ceramic cover plates and gold-tin solder is operated frequently, resulting in increased costs and low positioning accuracy, and easy to cause air leakage.
A gold-tin solder laser attachment assembly for ceramic covers is designed, including the lower module and the upper module. The gold-tin soldering ring is accurately positioned through the positioning groove of the lower ceramic covers, and spot welding is used for use with a laser welding gun to ensure position accuracy and one-time sticking. The film is completed.
Improve processing efficiency and accuracy, reduce the number of patches, avoid air leakage, and ensure the accuracy and efficiency of welding.
Smart Images

Figure CN110899978B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a gold-tin solder laser attachment component of a ceramic cover plate and an attachment method thereof. Background Art
[0002] In the existing optical communication chip packaging process, the ceramic cover plate, gold-tin solder, etc. need to be sintered and sealed with the tube shell at low temperature. In this process, the ceramic cover plate and gold-tin solder are mounted in batches, which will increase the number of mounting times and increase the cost. Secondly, the positioning accuracy of multiple mountings is low, which makes the position of the cover plate deviate after welding, and it is also easy to cause the solder position to be inaccurate, resulting in air leakage. The prior art urgently needs a gold-tin solder laser attachment component and an attachment method for a ceramic cover plate that can accurately attach gold-tin solder to a ceramic substrate. Summary of the invention
[0003] The purpose of the present invention is to overcome the defects in the prior art and provide a gold-tin solder laser attachment assembly for a ceramic cover plate that can accurately attach gold-tin solder to a ceramic substrate and an attachment method thereof.
[0004] To achieve the above-mentioned purpose, the technical solution of the present invention is to provide a gold-tin solder laser attachment assembly for a ceramic cover plate, comprising a lower module and an upper module used in conjunction with the lower module, wherein a lower ceramic cover plate positioning groove is provided at the center of the lower module, and the ceramic cover plate and the gold-tin solder ring are sequentially placed in the lower ceramic cover plate positioning groove; the outer edge of the ceramic cover plate and / or the outer edge of the gold-tin solder ring are positioned in conjunction with the inner edge of the lower ceramic cover plate positioning groove;
[0005] A welding point is arranged near the edge of the gold-tin soldering ring, and a laser welding gun which moves up and down is arranged above the welding point;
[0006] An upper ceramic cover plate receiving groove for receiving the ceramic cover plate is provided in the middle of the upper module. When the lower module and the upper module are molded together, the outer edge of the upper ceramic cover plate receiving groove contacts with the gold-tin soldering ring.
[0007] By using the components described in the present application, the ceramic cover plate and the gold-tin solder ring can be accurately positioned through the positioning groove of the lower ceramic cover plate before packaging, and attached by laser spot welding to ensure positioning accuracy. In subsequent packaging, only one patch is required, thereby improving processing efficiency and processing accuracy and avoiding adverse phenomena such as air leakage.
[0008] Preferably, the ceramic cover plate includes a central ceramic plate core and a nickel-plated layer and a gold-plated layer formed by vacuum coating; a positioning boss is provided in the middle of the ceramic cover plate, and the periphery of the positioning boss is a cover plate welding ring area; the ring hole in the middle of the gold-tin soldering ring is adapted to be positioned with the positioning boss. With such a design, the gold-tin soldering ring can be positioned first by the positioning boss, further improving the positioning accuracy.
[0009] Preferably, the outer edge of the upper ceramic cover plate receiving groove is a downwardly protruding edge, and the depth of the upper ceramic cover plate receiving groove is greater than the thickness of the positioning boss; when the lower module and the upper module are molded together, the edge pressing presses the gold-tin soldering ring against the cover plate welding ring area; gold-tin paste is provided between the gold-tin soldering ring and the cover plate welding ring area, and the position where the gold-tin paste is attached is adapted to the welding point. With such a design, the gold-tin soldering ring can be pressed against the cover plate welding ring area by edge pressing before welding, so that welding can proceed smoothly and cold soldering can be avoided. By providing gold-tin paste between the gold-tin soldering ring at the bottom of the welding point and the cover plate welding ring area, the two can be better bonded by the gold-tin paste. Even if there is a matching gap between the gold-tin soldering ring and the cover plate welding ring area, the laser heat can still be conducted by the gold-tin paste to achieve electric welding and ensure zero cold soldering.
[0010] Preferably, a pressurizing device is provided on the upper part of the upper module. Such a design is a further optimization of the solution.
[0011] Preferably, the ceramic cover plate and the gold-tin soldering ring are both rectangular, and the soldering points are arranged at the four corners of the gold-tin soldering ring; the positioning groove of the lower ceramic cover plate is also rectangular, and expands outward at the four corners to form an arc-shaped soldering groove. With this design, an operable area is designed around the soldering point to avoid interference with the groove body.
[0012] Preferably, the upper module is in a rectangular block shape, and arc-shaped notches are provided at the four corners of the upper module; when the lower module and the upper module are molded together, the arc-shaped notches cooperate with the welding groove to form a welding operation space area. An operable area is designed around the welding point to avoid interference with the groove body.
[0013] A method for laser attaching a gold-tin solder to a ceramic cover plate, using a gold-tin solder laser attaching assembly of the ceramic cover plate, comprises the following steps:
[0014] The first step is to form a ceramic cover plate: the ceramic cover plate is subjected to vacuum coating to obtain a nickel-plated layer and a gold-plated layer in sequence, wherein the thickness of the nickel-plated layer is 3-8 μm and the thickness of the gold-plated layer is 0.5-1.8 μm;
[0015] The second step is to form a gold-tin solder ring: press the AU80SN20 alloy ingot into a foil strip, and punch the foil strip to obtain a gold-tin solder ring that matches the size of the ceramic cover plate; the thickness of the gold-tin solder ring is 50-200μm;
[0016] The third step is to place the components, fit the ring hole in the middle of the gold-tin soldering ring with the positioning boss; fit the ceramic cover plate with the positioning groove of the lower ceramic cover plate; fit the lower module and the upper module together to close the mold, and press the gold-tin soldering ring tightly against the welding ring area of the cover plate;
[0017] The fourth step is laser spot welding, using a laser welding gun to work at the welding point to weld the four corners of the gold-tin solder ring to the four corners of the ceramic cover plate;
[0018] The fifth step is mold opening inspection.
[0019] Through this method, a ceramic cover plate and a gold-tin solder ring attachment component with high position accuracy can be obtained, which can reduce the number of patch times in subsequent packaging and improve processing efficiency and effects.
[0020] Preferably, when the upper module and the lower module are molded together, the pressure applied by the pressure device on the upper module is 1-100 N. Such a design can ensure that the edge pressing presses the gold-tin soldering ring tightly against the soldering ring area of the cover plate.
[0021] As a preferred embodiment, the operating parameters of laser spot welding are: spot size 5-100 microns, frequency 10-80 Hz, power 10-300 W. Such a design can ensure the smooth progress of laser welding and ensure the welding effect.
[0022] Preferably, the area of the laser spot welding is less than 0.2 mm in diameter. Such a small welding area can ensure the appearance quality of the welding and will not affect the quality of the subsequent reflow welding (large welding spots will cause excessive welding and empty welding).
[0023] Preferably, in step three, before the gold-tin soldering ring is fitted and positioned with the positioning boss, gold-tin paste is attached to the four corners of the upper surface of the cover plate welding ring area. After the gold-tin paste is attached, the ring hole in the middle of the gold-tin soldering ring is fitted and positioned with the positioning boss; the position of the attached gold-tin paste is adapted to the welding point position. By attaching gold-tin paste between the gold-tin soldering ring at the lower part of the welding point and the cover plate welding ring area, after mold closing, the cover plate welding ring area and the gold-tin soldering ring can be bonded at the welding point to ensure the conductivity of laser heat. Even if there is a matching gap between the gold-tin soldering ring and the cover plate welding ring area, the laser heat can still be conducted by the gold-tin paste to achieve electric welding and ensure zero false solder joints.
[0024] Preferably, the weight ratio of Au powder to Sn powder in the gold-tin paste is 80:20, and the percentage of organic solvent is 10-45%; the attachment method of the gold-tin paste is screen printing or dispensing; the attachment amount of the gold-tin paste at each attachment position is 0.05-2 ml. Such a design is an implementation method of the gold-tin paste component.
[0025] The advantages and beneficial effects of the present invention are that by using the components described in the present application, the ceramic cover plate and the gold-tin solder ring can be accurately positioned through the positioning groove of the lower ceramic cover plate before packaging, and attached by laser spot welding, so that the positioning accuracy can be guaranteed, and only one patch is required in the subsequent packaging, thereby improving the processing efficiency and processing accuracy, and avoiding the occurrence of undesirable phenomena such as leakage. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram of the separation state of the lower module and the upper module of the present invention;
[0027] Figure 2 This is a schematic diagram of the lower module structure of the present invention;
[0028] Figure 3 This is a schematic diagram of the upper module structure of the present invention;
[0029] Figure 4 Schematic diagram of the mold closing state of the lower module and the upper module (top view, omitting the laser welding gun and pressurizing device);
[0030] Figure 5 This is a schematic diagram of the welding operation structure of the present invention (side view);
[0031] Figure 6 It is a schematic diagram of the separation structure of the ceramic cover plate and the gold-tin soldering ring of the present invention;
[0032] Figure 7 It is a schematic diagram of the structure of a gap between the ceramic cover plate and the gold-tin soldering ring of the present invention;
[0033] Figure 8 It is a schematic diagram of the structure before mold closing after the gold-tin paste is attached in step 3 when there is a gap between the ceramic cover plate and the gold-tin solder ring of the present invention;
[0034] Fig. 9 This is a schematic diagram of the structure after mold closing after the gold-tin paste is attached in step three when there is a gap between the ceramic cover plate and the gold-tin solder ring of the present invention.
[0035] In the figure: 1. lower module; 2. upper module; 3. positioning groove of lower ceramic cover; 5. ceramic cover; 7. gold-tin soldering ring; 8. welding point; 9. laser welding gun; 10. upper ceramic cover receiving groove; 11. positioning boss; 12. cover welding ring area; 13. edge pressing; 14. pressurizing device; 15. soldering groove; 16. arc-shaped notch; 17. gold-tin slurry; 18. gap. DETAILED DESCRIPTION
[0036] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and embodiments. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.
[0037] like Figures 1 to 9 As shown,
[0038] Example 1
[0039] A gold-tin solder laser attachment assembly for a ceramic cover plate 5, comprising a lower module 1 and an upper module 2 used in conjunction with the lower module 1, wherein a lower ceramic cover plate positioning groove 3 is provided at the center of the lower module 1, wherein the ceramic cover plate 5 and the gold-tin soldering ring 7 are sequentially placed in the lower ceramic cover plate positioning groove 3; the outer edge of the ceramic cover plate 5 and / or the outer edge of the gold-tin soldering ring 7 are matched with the inner edge of the lower ceramic cover plate positioning groove 3 for positioning;
[0040] A welding point 8 is arranged near the edge of the gold-tin soldering ring 7, and a laser welding gun 9 that moves up and down is arranged above the welding point 8;
[0041] An upper ceramic cover plate receiving groove 10 for receiving the ceramic cover plate 5 is formed in the middle of the upper module 2 . When the lower module 1 and the upper module 2 are molded together, the outer edge of the upper ceramic cover plate receiving groove 10 contacts the gold-tin soldering ring 7 .
[0042] The ceramic cover plate 5 includes a central ceramic plate core and a nickel-plated layer and a gold-plated layer formed by vacuum coating; a positioning boss 11 is provided in the middle of the ceramic cover plate 5, and the periphery of the positioning boss 11 is a cover plate welding ring area 12; the ring hole in the middle of the gold-tin soldering ring 7 is adapted to be positioned with the positioning boss 11.
[0043] The outer edge of the upper ceramic cover plate receiving groove 10 is a downwardly protruding pressing edge 13, and the depth of the upper ceramic cover plate receiving groove 10 is greater than the thickness of the positioning boss 11; when the lower module 1 and the upper module 2 are molded together, the pressing edge 13 presses the gold-tin soldering ring 7 tightly against the cover plate welding ring area 12. A gold-tin paste 17 is provided between the gold-tin soldering ring 7 and the cover plate welding ring area 12, and the position where the gold-tin paste 17 is attached is adapted to the welding point 8.
[0044] A pressurizing device 14 is provided on the upper portion of the upper module 2. The pressurizing device 14 is a spring or a cylinder.
[0045] The ceramic cover plate 5 and the gold-tin soldering ring 7 are both rectangular, and the soldering points 8 are arranged at the four corners of the gold-tin soldering ring 7; the lower ceramic cover plate positioning groove 3 is also rectangular, and expands outward at the four corners to form an arc-shaped soldering groove 15.
[0046] The upper module 2 is in a rectangular block shape, and arc-shaped notches 16 are provided at the four corners of the upper module 2; when the lower module 1 and the upper module 2 are molded together, the arc-shaped notches 16 cooperate with the welding grooves 15 to form a welding operation space area.
[0047] Example 2
[0048] A method for laser attaching a gold-tin solder to a ceramic cover plate 5, using the gold-tin solder laser attaching assembly of the ceramic cover plate 5 in Example 1, comprises the following steps:
[0049] The first step is to form a ceramic cover plate 5: the ceramic cover plate 5 is subjected to vacuum coating to obtain a nickel-plated layer and a gold-plated layer in sequence, wherein the thickness of the nickel-plated layer is 3-8 μm, and the thickness of the gold-plated layer is 0.5-1.8 μm;
[0050] Step 2: forming a gold-tin soldering ring 7: pressing the AU80SN20 alloy ingot into a foil strip, and punching the foil strip to obtain a gold-tin soldering ring 7 matching the size of the ceramic cover plate 5; the thickness of the gold-tin soldering ring 7 is 50-200 μm;
[0051] The third step is to place the components, fit the ring hole in the middle of the gold-tin soldering ring 7 with the positioning boss 11; fit the ceramic cover plate 5 with the positioning groove 3 of the lower ceramic cover plate; the lower module 1 and the upper module 2 are molded together, and the pressing edge 13 presses the gold-tin soldering ring 7 tightly against the cover plate welding ring area 12 (this ensures that the gold-tin soldering ring 7 at the four welding points 8 is in close contact with the cover plate welding ring area 12 without any gap);
[0052] The fourth step is laser spot welding. Use a laser welding gun 9 to work at the welding point 8 to weld the four corners of the gold-tin solder ring 7 to the four corners of the ceramic cover plate 5. Preferably, a laser welding machine with a German IPG-QCW150W multi-mode laser, a SCANLAB galvanometer with an incident spot of 20mm, an incident spot of 20mm, and a field lens with a focal length of F160mm is used.
[0053] The fifth step is mold opening inspection.
[0054] When the upper die block 2 and the lower die block 1 are molded together, the pressure applied by the pressure device 14 on the upper die block 2 is 1-100 Newtons.
[0055] The operating parameters for laser spot welding are spot size 5-100 microns, frequency 10-80HZ, and power 10-300 watts.
[0056] The area of the laser spot welding is less than 0.2mm in diameter.
[0057] Example 3
[0058] For further optimization of Example 2, in step three, before the gold-tin solder ring 7 is fitted and positioned with the positioning boss 11, gold-tin paste 17 is attached to the four corners of the upper surface of the cover plate welding ring area 12. After the gold-tin paste 17 is attached, the ring hole in the middle of the gold-tin solder ring 7 is fitted and positioned with the positioning boss 11; the position 17 of the attached gold-tin paste is adapted to the position of the welding point 8.
[0059] The weight ratio of Au powder to Sn powder in the gold-tin paste 17 is 80:20, and the percentage of organic solvent is 10-45%. The gold-tin paste 17 is attached by screen printing or dispensing. The attachment amount of the gold-tin paste 17 at each attachment position is 0.05-2 ml.
[0060] Preferably, the gold-tin paste is prepared by the following method: firstly, gold-tin powder (particle size 10 nm-5 microns) or Au powder and Sn powder are mixed into metal powder in a weight ratio of 80:20;
[0061] Add the powder, plasticizer and organic solvent obtained in the previous step into a mixer, wherein the percentage of the organic solvent is 10-45%; seal and stir the powder, plasticizer and organic solvent at a temperature of 35-50°C, the rotation speed of the mixer is 205-315 rpm, and the mixing time is 24-120h to obtain a slurry with a reasonable viscosity, and then vacuum the slurry to remove bubbles.
[0062] Preferably, the plasticizer includes PVB and ethyl acetate.
[0063] Preferably, the organic solvent comprises butanone, alcohol and acetone.
[0064] Before the gold-tin soldering ring 7 is adapted and positioned with the positioning boss 11, the gold-tin paste 17 is attached to the four corners of the upper surface of the cover plate soldering ring area 12 in a drop shape. After the mold is closed, the gold-tin soldering ring 7 is pressed tightly against the cover plate soldering ring area 12 by the edge pressing 13. The drop-shaped gold-tin paste 17 is squeezed into a thin layer, and the upper and lower surfaces are respectively bonded to the lower surface of the gold-tin soldering ring 7 and the upper surface of the cover plate soldering ring area 12. In the case of local deformation of the gold-tin soldering ring 7, the thermal conductivity of the gold-tin paste 17 and the ceramic cover plate 5 can still be relied on;
[0065] It is found in practice that in the absence of gold-tin paste 17, when the gold-tin solder ring 7 at the bottom of the welding point 8 is locally deformed, a gap 18 will exist between the gold-tin solder ring 7 at the bottom of the welding point 8 and the cover welding ring area 12. In the subsequent laser spot welding, heat cannot be conducted through the gap to the upper surface of the cover welding ring area 12, resulting in a cold weld.
[0066] In the present application, the addition and use of the gold-tin paste 17 effectively solves the above-mentioned risks and can achieve zero cold soldering.
[0067] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for laser attachment of gold-tin solder to a ceramic cover plate. Features: Gold-tin solder laser attachment components for ceramic cover plates include: A lower module and an upper module used in conjunction with the lower module, wherein a lower ceramic cover plate positioning groove is provided at the center of the lower module, and the ceramic cover plate and the gold-tin soldering ring are sequentially placed in the lower ceramic cover plate positioning groove; the outer edge of the ceramic cover plate and / or the outer edge of the gold-tin soldering ring are matched with the inner edge of the lower ceramic cover plate positioning groove for positioning; A welding point is arranged near the edge of the gold-tin soldering ring, and a laser welding gun which moves up and down is arranged above the welding point; The middle of the upper module is provided with an upper ceramic cover plate receiving groove for receiving the ceramic cover plate, and when the lower module and the upper module are molded together, the outer edge of the upper ceramic cover plate receiving groove contacts with the gold-tin soldering ring; The ceramic cover plate comprises a central ceramic plate core and a nickel-plated layer and a gold-plated layer formed by vacuum coating; a positioning boss is arranged in the middle of the ceramic cover plate, and the periphery of the positioning boss is a cover plate welding ring area; the ring hole in the middle of the gold-tin soldering ring is adapted to be positioned with the positioning boss; The outer edge of the upper ceramic cover plate receiving groove is a downwardly protruding pressing edge, and the depth of the upper ceramic cover plate receiving groove is greater than the thickness of the positioning boss; when the lower module and the upper module are molded together, the pressing edge presses the gold-tin soldering ring tightly against the cover plate welding ring area; gold-tin paste is arranged between the gold-tin soldering ring and the cover plate welding ring area, and the position where the gold-tin paste is attached is adapted to the welding point; A pressurizing device is provided on the upper portion of the upper module; The ceramic cover plate and the gold-tin soldering ring are both rectangular, and the soldering points are arranged at the four corners of the gold-tin soldering ring; the positioning groove of the lower ceramic cover plate is also rectangular, and expands outward at the four corners to form an arc-shaped soldering groove; The upper module is in a rectangular block shape, and arc-shaped notches are provided at the four corners of the upper module; when the lower module and the upper module are molded together, the arc-shaped notches cooperate with the welding grooves to form a welding operation space area; The gold-tin solder laser attachment method of the ceramic cover plate uses a gold-tin solder laser attachment component of the ceramic cover plate, and comprises the following steps: The first step is to form a ceramic cover plate: the ceramic cover plate is subjected to vacuum coating to obtain a nickel-plated layer and a gold-plated layer in sequence, wherein the thickness of the nickel-plated layer is 3-8 μm and the thickness of the gold-plated layer is 0.5-1.8 μm; The second step is to form a gold-tin solder ring: press the AU80SN20 alloy ingot into a foil strip, and punch the foil strip to obtain a gold-tin solder ring that matches the size of the ceramic cover plate; the thickness of the gold-tin solder ring is 50-200μm; The third step is to place the components, fit the ring hole in the middle of the gold-tin soldering ring with the positioning boss; fit the ceramic cover plate with the positioning groove of the lower ceramic cover plate; fit the lower module and the upper module together to close the mold, and press the gold-tin soldering ring tightly against the welding ring area of the cover plate; The fourth step is laser spot welding, using a laser welding gun to work at the welding point to weld the four corners of the gold-tin solder ring to the four corners of the ceramic cover plate; The fifth step is mold opening inspection; When the upper and lower modules are molded together, the pressure applied by the pressure device on the upper module is 1-100 Newtons; The operating parameters of laser spot welding are: spot size 5-100 microns, frequency 10-80HZ, power 10-300 watts; the area of laser spot welding is less than 0.2mm in diameter; In step three, before the gold-tin soldering ring is matched and positioned with the positioning boss, gold-tin paste is attached to the four corners of the upper surface of the cover plate soldering ring area, and after the gold-tin paste is attached, the ring hole in the middle of the gold-tin soldering ring is matched and positioned with the positioning boss; the position of the attached gold-tin paste is matched with the position of the soldering point; The weight ratio of Au powder to Sn powder in the gold-tin paste is 80:20, and the percentage of organic solvent is 10-45%. The attachment method of the gold-tin paste is screen printing or dispensing. The attachment amount of the gold-tin paste at each attachment position is 0.05-2 ml.
Citation Information
Patent Citations
Welding method for semiconductor ceramic shell sealing cap
CN103056500A
Presetting gold-tin cover plate and manufacturing method thereof
CN104952808A
Surface-mounted photoelectric detector packaging housing
CN108615773A
Fixture for precise welding
CN203579077U
Special frock clamp of process standard
CN207077138U