Cathode of solid-state lithium-sulfur battery and method for manufacturing the same

By using porous sulfur composite layer and conductive polymer in the cathode of lithium sulfur batteries, combined with freeze-drying technology, the conductivity and polysulfide migration of the sulfur cathode are solved, and the discharge capacity and cycling performance of the battery are improved.

CN111162242BActive Publication Date: 2024-11-22CORNING INC +1
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN201811325286.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-11-08
Publication Date
2024-11-22
Estimated Expiration
2038-11-08

AI Technical Summary

Technical Problem

The electronic and ionic insulation of elemental sulfur in lithium sulfur batteries leads to excessive use of cathode conductive additives, reducing actual capacity and applicability. At the same time, the long-chain polysulfide produced by conventional organic electrolytes during discharge migrates to the lithium anode, resulting in Coulomb efficiency Reduce and loss of active cathode material.

Method used

Using a sulfur-based composite layer with a porosity of 60% to 99%, and a conductive polymer is provided on the top and pores of the composite layer to form a porous structure by freeze-drying, increasing the porosity and introducing carbon materials and metal carbides. Adsorb polysulfides to improve sulfur utilization.

Benefits of technology

The high discharge capacity retention rate and energy density of lithium-sulfur batteries are achieved, which reduces the loss of active materials, improves the ionic conductivity and cyclic stability of the electrodes, and reduces the total impedance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111162242B_ABST
    Figure CN111162242B_ABST
Patent Text Reader

Abstract

A cathode of a lithium-sulfur battery comprises a sulfur-based composite layer having a porosity in the range of 60% to 99%; and a conductive polymer disposed on top of the composite layer and within the pores of the composite layer. In addition, a method of forming a cathode of a lithium-sulfur battery comprises: providing a substrate; disposing a sulfur-based slurry layer on the substrate; freeze drying the slurry layer to form a sulfur-based composite layer having a porosity in the range of 60% to 99%; and disposing a conductive polymer on top of the composite layer and within the pores of the composite layer.
Need to check novelty before this filing date? Find Prior Art

Description

background 1. Technical field

[0002] The present disclosure relates to cathodes for solid-state lithium-sulfur (Li-S) batteries and methods for making the same. 2. Background technology

[0004] Lithium-sulfur (Li-S) batteries are attractive candidates to replace conventional lithium-ion batteries because they are cheaper, lighter, and can store nearly twice as much energy for the same mass. For example, Li-S battery chemistry has a high energy density (e.g., 2600 W·h·kg -1 ) and theoretical specific capacity (e.g. 1675 mA·h·g -1 ), high natural abundance and environmentally friendly.

[0005] One difficulty with conventional Li-S technology is the electronic and ionic insulating properties of elemental sulfur (used as a component of the cathode), which requires a large portion of conductive additives in the cathode, significantly reducing practical capacity and applicability. Another drawback is the solubility of long-chain polysulfides generated during battery discharge in conventional organic electrolytes. As polysulfides migrate from the cathode to the lithium (Li) anode, undesirable side reactions are triggered, while polysulfide shuttling leads to reduced Coulombic efficiency and a continuous loss of active cathode material.

[0006] The present application discloses improved cathodes and methods of forming the same for solid-state lithium-sulfur (Li-S) battery applications. Summary of the invention

[0007] In some embodiments, a cathode of a lithium-sulfur battery includes: a sulfur-based composite layer having a porosity ranging from 60% to 99%; and a conductive polymer disposed on top of the composite layer and within pores of the composite layer.

[0008] In one aspect that may be combined with any other aspect or embodiment, the composite layer has a porosity in a range of 60% to 80%.

[0009] In one aspect that may be combined with any other aspect or embodiment, the pores of the composite layer have a size in the range of 1 μm to 50 μm.

[0010] In one aspect that may be combined with any other aspect or embodiment, the pores have a size in the range of 2 μm to 10 μm.

[0011] In one aspect that may be combined with any other aspect or embodiment, the composite layer comprises carbon material in the form of at least one of nanoparticles, nanowires, nanofibers, nanorods, nanotubes, nanospheres, graphene, or a combination thereof.

[0012] In one aspect that may be combined with any other aspect or embodiment, the carbon material is present in an amount ranging from 5 wt% to 40 wt%.

[0013] In one aspect that may be combined with any other aspect or embodiment, the composite layer comprises metal carbide in a range of 1 wt % to 20 wt %.

[0014] In one aspect that may be combined with any other aspect or embodiment, the conductive polymer comprises at least one of carbon polysulfides (CS), polyethylene oxide (PEO), polyaniline (PANI), polypyrrole (PPY), poly(3,4-ethylenedioxythiophene) (PEDOT), polystyrene sulfonic acid (PSS), polyacrylonitrile (PAN), polyacrylic acid (PAA), polyallylamine hydrochloride (PAH), poly(vinylidene fluoride-co-hexafluoropropylene) (P(VdF-co-HFP)), poly(methyl methacrylate) (PMMA), polyvinylidene fluoride (PVDF), poly(diallyldimethylammonium)bis(trifluoromethanesulfonyl)imide (TFSI) (PDDATFSI), or a combination thereof, and comprises at least one of bis(trifluoromethane)sulfonyl imide lithium salt (LiTFSI), lithium perchlorate, lithium bis(oxalate)borate (LiBOB), lithium bis(fluorosulfonyl)imide (LiFSI), or a combination thereof.

[0015] In some embodiments, a lithium-sulfur (Li-S) battery comprises: a lithium anode; a solid-state electrolyte; and a cathode disclosed herein.

[0016] In one aspect that may be combined with any other aspect or embodiment, the Li—S battery is configured to have a discharge capacity retention rate of at least 90%.

[0017] In one aspect that may be combined with any other aspect or embodiment, the solid electrolyte comprises at least one of: Li 6.4 LqCy 1.4 Ta 0.6 O 12 (LLZTO), Li 10 GeP2S 12 , Li 1.5 Al 0.5 Ge 1.5 (PO4)3、Li 1.4 Al 0.4 Ti 1.6 (PO4)3、Li 0.55 La 0.35TiO3, interpenetrating polymer network (ipn-PEA) electrolyte of poly(ethyl acrylate), three-dimensional ceramic / polymer network, in situ plasticized polymer, composite polymer with well-aligned ceramic nanowires, PEO-based solid polymer, flexible polymer, polymeric ionic liquid, in situ formed Li3PS4 or a combination thereof.

[0018] In some embodiments, a method of forming a cathode for a lithium-sulfur battery includes: providing a substrate; disposing a sulfur-based slurry layer on the substrate; freeze-drying the slurry layer to form a sulfur-based composite layer having a porosity in a range of 60% to 99%; and disposing a conductive polymer on top of the composite layer and within the pores of the composite layer.

[0019] In one aspect that may be combined with any other aspect or embodiment, the substrate is a current collector.

[0020] In one aspect that may be combined with any other aspect or embodiment, the method further comprises: mixing the metal carbide, the carbon material, and the sulfur material in a solvent to form a sulfur precursor; and dry-milling the dried sulfur precursor to form the sulfur composite.

[0021] In one aspect that may be combined with any other aspect or embodiment, the method further comprises: stirring the sulfur complex with the binder to form a sulfur-based slurry.

[0022] In one aspect that may be combined with any other aspect or embodiment, the carbon material is at least one of: nanoparticles, nanowires, nanofibers, nanorods, nanotubes, nanospheres, graphene, or a combination thereof, and the binder comprises at least one of: styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid (PAA), sodium alginate, or a combination thereof.

[0023] In one aspect that may be combined with any other aspect or embodiment, the composite layer has a porosity in a range of 60% to 80%.

[0024] In one aspect that may be combined with any other aspect or embodiment, the pores of the composite layer have a size in the range of 1 μm to 50 μm.

[0025] In one aspect that may be combined with any other aspect or embodiment, the pores have a size in the range of 2 μm to 10 μm.

[0026] In one aspect that may be combined with any other aspect or embodiment, the freeze-drying step comprises: freezing the slurry layer at a temperature in the range of -50°C to 0°C for a time in the range of 1 hour to 12 hours; and drying the frozen slurry layer in a freeze dryer for a time in the range of 1 hour to 24 hours.

[0027] In one aspect that may be combined with any other aspect or embodiment, the step of providing the conductive polymer is performed by at least one of spin coating, dip coating, layer-by-layer deposition, sol-gel deposition, inkjet printing, or a combination thereof.

[0028] In some embodiments, a method of forming a lithium-sulfur (Li-S) battery includes: providing a substrate; providing a cathode, wherein the cathode is formed by: disposing a sulfur-based slurry layer on the substrate, freeze drying the slurry layer to form a sulfur-based composite layer having a porosity in a range of 60% to 99%, and disposing a conductive polymer on top of the composite layer and within the pores of the composite layer; providing a solid electrolyte; and providing a lithium anode.

[0029] In one aspect that may be combined with any other aspect or embodiment, the solid electrolyte comprises at least one of: Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 (LLZTO), Li 10 GeP2S 12 , Li 1.5 Al 0.5 Ge 1.5 (PO4)3、Li 1.4 Al 0.4 Ti 1.6 (PO4)3、Li 0.55 La 0.35 TiO3, interpenetrating polymer network (ipn-PEA) electrolyte of poly(ethyl acrylate), three-dimensional ceramic / polymer network, in situ plasticized polymer, composite polymer with well-aligned ceramic nanowires, PEO-based solid polymer, flexible polymer, polymeric ionic liquid, in situ formed Li3PS4 or a combination thereof. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The present disclosure can be more fully understood through the following specific embodiments in conjunction with the accompanying drawings, in which:

[0031] Figure 1 The structure of a solid-state lithium-sulfur (Li-S) battery according to some embodiments is illustrated.

[0032] Figure 2 Schemes for drying the Li—S sulfur cathode by (a) thermal drying; and (b) freeze drying are illustrated.

[0033] Figure 3 (a) A surface scanning electron microscope (SEM) image and (b) a cross-sectional scanning electron microscope (SEM) image of the cathode electrode in Comparative Example 1 are illustrated.

[0034] Figure 4 A cross-sectional SEM image of the cathode sample (coated with PEO) in Comparative Example 1 and a corresponding energy dispersive spectroscopy (EDS) profile are illustrated.

[0035] Figure 5 Illustrated are (a) a surface SEM image and (b) a cross-sectional SEM image of the cathode electrode in Example 1; and (c) a surface SEM image and (d) a cross-sectional SEM image of a cathode sample coated with a PEO-based electrolyte layer.

[0036] Figure 6 A cross-sectional SEM image and the corresponding EDS profile of a cathode sample (coated with PEO) as in Example 1 are illustrated.

[0037] Figure 7 Impedance plots of Li-S cells where the cathode was prepared by (I) freeze drying or (II) thermal drying are illustrated.

[0038] Figure 8 The cycling performance of Li-S cells whose cathodes were prepared by (I) freeze drying or (II) thermal drying is illustrated.

[0039] Fig. 9 The sulfur cathode is prepared by (a) thermal drying; and (b) freeze drying. The Li-S battery is shown in Figure 2 at 60 °C with a current density of 0.1 mA cm -2 The charge-discharge curves at .

[0040] Fig.10 The cycling performance of a Li-S cell in which the cathode in Example 2 is prepared by freeze drying and has a Li-Au anode is illustrated. DETAILED DESCRIPTION

[0041] The exemplary embodiments shown in the accompanying drawings will now be described in detail. Whenever possible, the same reference numerals are used in the accompanying drawings to represent the same or similar parts. The components in the accompanying drawings are not necessarily drawn to scale, but the focus is on illustrating the principles of the exemplary embodiments. It should be understood that the application is not limited to the details or methodology set forth in the specification or illustrated in the accompanying drawings. It should also be understood that the terms are for descriptive purposes only and should not be considered restrictive.

[0042] In addition, any examples listed in this specification are illustrative rather than limiting, and only list some of the many possible embodiments of the claimed invention. Other appropriate modifications and adjustments to various conditions and parameters are common in the art and are obvious to those skilled in the art, and are within the spirit and scope of the present disclosure.

[0043] The present disclosure relates to solid-state lithium-sulfur batteries, and more particularly, to sulfur cathodes and methods for producing the same, wherein a porous sulfur cathode coated with a lithium ion conductive polymer layer, such as polyethylene oxide (PEO), is used in solid-state lithium-sulfur batteries.

[0044] Figure 1 An example of a solid-state lithium-sulfur (Li-S) battery structure according to some embodiments is illustrated. Those skilled in the art will appreciate that the methods described herein may be applicable to other configurations of solid-state lithium-sulfur (Li-S) battery structures.

[0045] In some embodiments, the battery 100 may include a substrate 102 (e.g., a current collector), a sulfur electrode (e.g., a cathode) 104 disposed on the substrate, a first intermediate layer 106 disposed on the cathode, a solid electrolyte 108 disposed on the first intermediate layer, a second intermediate layer 110 disposed on the electrolyte, and a lithium electrode (e.g., an anode) 112 disposed on the second intermediate layer. These may be placed horizontally or vertically relative to each other.

[0046] In some examples, the substrate 102 may be a current collector comprising at least one of three-dimensional nickel (Ni) foam, carbon fiber, foil (e.g., aluminum foil, stainless steel foil, copper foil, platinum foil, nickel foil, etc.), or a combination thereof. In some examples, the intermediate layers 106 and 110 may be independently selected from at least one of carbon-based intermediate layers (e.g., interconnected independent, containing micropores / mesoporous, functionalized, derived from biomass), polymer-based intermediate layers (e.g., PEO, polypyrrole (PPY), polyvinylidene fluoride, etc.), metal-based (e.g., Ni foam, etc.), or a combination thereof.

[0047] In some examples, a solid electrolyte 108 can be used to solve common safety issues common in Li-S batteries using liquid electrolytes, such as leakage, poor chemical stability, and flammability. In addition, the solid electrolyte can also inhibit the shuttling of polysulfides from the cathode to the anode, thereby improving cathode utilization and obtaining high discharge capacity and energy density. In some examples, the solid electrolyte may include at least one of the following: Li 6.4 LqCy 1.4 Ta 0.6 O 12 (LLZTO), Li 10 GeP2S 12 , Li 1.5 Al 0.5 Ge 1.5 (PO4)3、Li 1.4 Al 0.4 Ti 1.6 (PO4)3、Li 0.55 La 0.35TiO3, interpenetrating polymer network (ipn-PEA) electrolyte of poly(ethyl acrylate), three-dimensional ceramic / polymer network, in situ plasticized polymer, composite polymer with well-aligned ceramic nanowires, PEO-based solid polymer, flexible polymer, polymeric ionic liquid, in situ formed Li3PS4 or a combination thereof.

[0048] In some examples, the anode 112 may include lithium (Li) metal. In some examples, the battery may include at least one anode protectant, such as an electrolyte additive (such as LiNO3, lanthanum nitrate, copper acetate, P2S5, etc.); an artificial interface layer (such as Li3N, (CH3)3SiCl, Al2O3, LiAl, etc.), a composite metal [such as Li7B6, Li-rGO (reduced graphene oxide), layered Li-rGO, etc.] or a combination thereof.

[0049] A description of the sulfur cathode 104 and methods of formation are described below.

[0050] Figure 2 A scheme 200 for drying a Li-S sulfur cathode by (a) thermal drying; and (b) freeze drying is illustrated. In the first step of the cathode formation scheme, a current collector substrate 206 is coated with a sulfur-based slurry layer comprising a binder 202 and a sulfur composite 204. The slurry layer can be formed as follows. First, a metal carbide, a carbon material, and a sulfur material are mixed in a solvent to form a sulfur precursor. The metal carbide can be a carbide comprising at least one of tungsten (W), iron (Fe), chromium (Cr), manganese (Mn), cobalt (Co), nickel (Ni), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), molybdenum (Mo), sodium (Na), calcium (Ca), or a combination thereof. The carbon material can be at least one of nanoparticles, nanowires, nanofibers, nanorods, nanotubes, nanospheres, graphene, or a combination thereof. The sulfur material is elemental sulfur. The solvent can be any known compatible solvent, such as at least one of the following: water, hexane, octane, acetone, tetrahydrofuran, 2-butanone, toluene, xylene, ethanol, methanol, isopropanol, benzene or a combination thereof. In some examples, the mixing can be performed by at least one of ball milling, ultrasonic treatment, magnetic mixing, vortex mixing, etc.

[0051] Subsequently, the sulfur precursor can be ground (e.g., dry grinding, etc.) to form a sulfur complex, and then the sulfur complex is mixed and stirred with a binder to form a sulfur-based slurry. In some examples, the binder includes at least one of the following: styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid (PAA), sodium alginate, or a combination thereof. In some examples, the binder includes styrene-butadiene rubber and carboxymethyl cellulose. In some examples, the binder includes water. Then, the slurry with the sulfur complex 204 and the binder 202 is placed on the substrate 206 by at least one of spin coating, dip coating, layer-by-layer deposition, sol-gel deposition, inkjet printing, or a combination thereof.

[0052] Conventionally, the slurry layer is thermally dried, e.g. Figure 2 As the solvent is removed during the thermal drying process, thermal drying generally results in a dense filling structure 208. As shown and explained in the examples below, the dense filling structure 208 results in a lower available internal volume space within the composite layer for containing the subsequently formed conductive polymer (i.e., lower porosity, fewer irregular pores).

[0053] According to the present disclosure, Figure 2 In route (b), after the sulfur-based slurry layer has been placed on the substrate, the slurry layer is freeze-dried to form a sulfur-based composite layer 210 having a porosity in the range of 60% to 99%. The structure of the sulfur cathode can be maintained by freezing the solvent in the slurry layer at low temperatures before drying. As the frozen solvent sublimates during drying, pores are formed in the composite layer (i.e., the pores remain where the solvent was originally located). In other words, during the freeze-drying process, the internal volume space of the composite layer occupied by the solvent can be retained, thereby avoiding shrinkage of the composite layer due to solvent volatilization during the drying process. Compared to traditional thermal drying, freeze drying can increase the porosity of the composite layer by 3-5 times.

[0054] In some examples, the porosity of the composite layer is in the range of 60% to 80% (this is in contrast to the porosity of the heat-dried slurry layer, which is in the range of 30% to 50%). In some examples, the size of the pores of the composite layer is in the range of 1 μm to 50 μm. In some examples, the pores may have a range of 2 μm to 10 μm. In some examples, freezing is performed at the following temperatures: in the range of -50°C to 0°C, or in the range of -35°C to -10°C, or in the range of -25°C to -15°C. In some examples, freezing is performed at a temperature of -20°C. In some examples, the freezing time is in the range of 1 hour to 12 hours, or in the range of 2 hours to 9 hours, or in the range of 4 hours to 7 hours. In some examples, freezing is performed for 6 hours. In some examples, freezing is performed for 6 hours at a temperature of -20°C. In some examples, the drying is performed in a freeze dryer for 1 to 24 hours, or 6 to 18 hours, or 9 to 15 hours. In some examples, the drying is performed for 12 hours.

[0055] In some examples, the composite layer comprises carbon material in the range of 5 wt % to 40 wt %, or in the range of 10 wt % to 30 wt %, or in the range of 15 wt % to 25 wt %. In some examples, the composite layer comprises metal carbides in the range of 1 wt % to 20 wt %, or in the range of 3 wt % to 17 wt %, or in the range of 5 wt % to 15 wt %. Carbon material and metal carbides are conductive moieties uniformly dispersed in the final sulfur cathode, which help adsorb polysulfide (i.e., minimize polysulfide migration) to improve sulfur utilization (i.e., minimize the loss of active cathode material).

[0056] After the freeze drying step, a conductive polymer 212 is placed on top of the composite layer 210 and within the pores of the composite layer 210 by at least one of spin coating, dip coating, layer-by-layer deposition, sol-gel deposition, inkjet printing, or a combination thereof to achieve the final cathode structure 214. In some examples, the conductive polymer includes at least one of carbon polysulfide (CS), polyethylene oxide (PEO), polyaniline (PANI), polypyrrole (PPY), poly(3,4-ethylenedioxythiophene) (PEDOT), polystyrene sulfonic acid (PSS), polyacrylonitrile (PAN), polyacrylic acid (PAA), polyallylamine hydrochloride (PAH), poly(vinylidene fluoride-co-hexafluoropropylene) (P(VdF-co-HFP)), poly(methyl methacrylate) (PMMA), polyvinylidene fluoride (PVDF), poly(diallyldimethylammonium)bis(trifluoromethanesulfonyl)imide (TFSI) (PDDATFSI), or a combination thereof, and includes at least one of bis(trifluoromethane)sulfonyl imide lithium salt (LiTFSI), lithium perchlorate, lithium bis(oxalate)borate (LiBOB), lithium bis(fluorosulfonyl)imide (LiFSI), or a combination thereof.

[0057] In some examples, the conductive polymer is polyethylene oxide. Since freeze drying forms pores and passages in the interior of the composite layer, after the conductive polymer slurry (e.g., PEO electrolyte) is coated on the surface of the composite layer, it can penetrate into the composite layer through the porous structure of the composite layer. This surface coating and internal penetration improves the interfacial compatibility of the resulting sulfur electrode and enhances ionic conductivity.

[0058] Example

[0059] Example 1

[0060] Sulfur, tungsten carbide (WC) and vapor-grown carbon fiber (VGCF) are ball-milled in ethanol at a weight ratio of 6:2:2. After ball-milling for 4 hours, the mixed powder is filtered and dried. After additional dry grinding (e.g., dry grinding) for 24 hours, the mixture is sieved to form a sulfur composite. A slurry is prepared by ball-milling or stirring a mixture of a previously prepared sulfur composite, tungsten carbide (WC), vapor-grown carbon fiber (VGCF), styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC) in a weight ratio of 80:5:5:5:5. Subsequently, the slurry is coated on an aluminum foil having a thickness of 100 μm.

[0061] The aluminum foil coated with the slurry was then frozen at -20°C for about 6 hours and then placed in a freeze dryer for about 12 hours to remove the water content in the slurry. After freeze drying, the electrode was cut into 12 mm diameter discs. The sulfur content of the cathode was measured to be about 1.78 mg / cm 2 .

[0062] Polyethylene oxide (PEO) powder and bis(trifluoromethane)sulfonyl imide lithium salt (LiN(CF3SO2)2 or LiTFSI) were used to react PEO with Li + The molar ratio of about 18: 1 is dissolved in acetonitrile. The solid content of the slurry is about 10%. The slurry is cast on the freeze-dried cathode surface, and the cathode is then vacuum dried at about 60°C, where the solvent evaporates to form a sulfur cathode. In order to ensure that there is a sufficient ionic and electronic conductive network in the cathode, the cathode is designed to have a thickness of less than 200 μm. The final sulfur cathode is then assembled into a battery together with other components (such as an intermediate layer, an electrolyte, and a Li anode).

[0063] Comparative Example 1

[0064] The sample formed as Comparative Example 1 was prepared as provided above in Example 1, except for the freeze drying step. Instead, after coating the slurry onto aluminum foil, the structure was thermally dried in an oven at a temperature of about 60° C. to remove the water content in the slurry. Subsequently, the electrode was cut into 12 mm diameter disks.

[0065] Characterization of Example 1 and Comparative Example 1

[0066] Figure 3 (a) Surface SEM image (plan view) and (b) cross-sectional SEM image of the cathode electrode as in Comparative Example 1 are illustrated. The morphological analysis described herein was performed by a scanning electron microscope (SEM, Hitachi JSM 6700), and the element distribution map was characterized by an energy dispersive spectrometer (EDS) belonging to HITACHI SEM. Figure 3 As can be seen from (a) and 3(b), the heat drying of the furnace resulted in considerable particle agglomeration, and the agglomerated particles were separated from the conductive network. For example, the initial coating thickness of the slurry on the aluminum foil was set to 100 μm. After heat treatment at 60°C, the thickness of the initial slurry film dropped significantly by about 70%, as the thickness after heat drying was measured to be about 30 μm. More importantly, since the sulfur-based composite layer shrinks as the contained water evaporates, the composite layer retains a lower porosity and the cathode finally formed has a non-uniform thickness. In other words, the heat treatment corresponds to a lower available internal volume space in the composite layer for containing the conductive polymer.

[0067] Figure 4The cross-sectional SEM image and corresponding energy dispersive spectrum (EDS) distribution diagram of the cathode sample coated with PEO conductive polymer (i.e., PEO electrolyte) as in Comparative Example 1 are illustrated. As shown in the cross-sectional SEM image (upper left figure), after application, although the surface of the sulfur electrode is completely covered by the PEO electrolyte, there is a distribution gradient of oxygen in the electrode (as seen in the EDS distribution diagram, lower right figure). In other words, oxygen is concentrated toward the top surface of the electrode and cannot fully penetrate the electrode body. This is observed in the EDS image. The position where most of the oxygen is located has bright luminescence (i.e., on the top surface of the electrode deposited with the PEO electrolyte), and then, as the depth from the top surface to the electrode increases, the luminescence drops sharply). The insufficient penetration of the PEO polymer layer indicates that less irregular holes are formed in the electrode by the thermal drying process. As seen in the upper right figure and the lower left figure, the content of sulfur and carbon is unevenly distributed throughout the electrode, because a small scattered area with a high degree of luminescence is observed; This confirms that in the thermal drying process, the particles agglomerate.

[0068] Figure 5 (a) Surface SEM image and (b) cross-sectional SEM image of the cathode electrode as in Example 1; and (c) Surface SEM image and (d) cross-sectional SEM image of the cathode sample coated with a PEO-based electrolyte layer. Figure 3 The results obtained from the thermal drying process in (a) and 3(b) show that the particle agglomeration is reduced ( Figure 5 (a) and 5(b)), because the resulting cathode is relatively uniform and has a smooth, uniform surface and a highly conductive network (i.e., the particles are connected to the carbon nanofibers). Figure 3 Comparison of the cross sections between (b) and 5(b) shows that the sample prepared by freeze drying has a significantly less rough top surface, as well as a greater overall thickness (30 μm for thermal drying vs. 80 μm for freeze drying), suggesting a less stacked morphology with a greater amount of open space (i.e., pore volume) in the bulk of the cathode. These results are consistent with Figure 2 The structures 208 (heat dried) and 210 (freeze dried) are consistent. Since the cathode below has a more consistent surface morphology and a larger internal pore volume, when covered with PEO electrolyte, a smooth PEO layer (about 20 μm) is formed on the top of the cathode and PEO is uniformly infiltrated into the bulk of the electrode ( Figure 5 (c) and 5(d)).

[0069] Figure 6 A cross-sectional SEM image and a corresponding EDS profile of a cathode sample coated with a PEO electrolyte as in Example 1 are illustrated. As indicated by the cross-sectional image (upper left), the surface of the sulfur electrode is completely covered by the PEO electrolyte. Figure 4The image of the thermal drying process, the uniform distribution of sulfur (upper right) and carbon (lower left) in the electrode proves that the electrode prepared by freeze drying does not show particle agglomeration. In addition, although there is a slightly larger oxygen content toward the top surface of the electrode, oxygen more completely penetrates axially through the pores of the electrode and provides a relatively more uniform lateral distribution of oxygen (lower right figure). In other words, the distribution of oxygen elements in the electrode shows that, compared to the electrode prepared by thermal drying, the PEO slurry can be more completely infiltrated into the interior of the electrode prepared by freeze drying (defined by the rich pore structure), thereby improving the ionic conductivity of the electrode.

[0070] PEO penetration plays an important role as an ion-conducting medium in the electrolyte (e.g., PEO interlayer, solid electrolyte, etc.) and cathode active material. In conventional thermal drying processes, PEO is added through a simple casting process and subsequent thermal drying. Therefore, the PEO slurry is not able to fully penetrate into the pores and other pathways of the sulfur electrode (e.g., Figure 2 The structure 20) does not form an effective ion conduction path, resulting in poor utilization of the active material. The cathode prepared by thermal drying without sufficient pore-forming PEO permeability still suffers from polysulfide dissolution and migration through the PEO electrolyte (i.e., the shuttle effect) at high temperatures.

[0071] Figure 7 and 8 The impedance diagram and cycle performance of the Li-S battery prepared by freeze drying and heat drying are illustrated respectively. Electrochemical impedance spectroscopy (EIS) is carried out on the Autolab electrochemical workstation (ECO CHEMIE BV company of the Netherlands) with a frequency response analyzer. Due to the pore volume formed in the cathode prepared by freeze drying, and comprising a conductive polymer (such as PEO), the ion conductor based on PEO can better contact the active material, so that the solid-state lithium-sulfur battery has a lower total impedance (60Ω, 80Ω of the contrast heat drying cathode). Due to PEO contacting with the cathode active material, the charge transfer resistance is effectively reduced by having a lower total impedance. The lower porosity of the cathode prepared by heat drying is unfavorable for PEO electrolyte penetration, which can cause high charge transfer resistance.

[0072] Figure 8The cycling performance of Li-S batteries whose cathodes are prepared by freeze drying and heat drying processes is illustrated. The cathode prepared by heat drying shows a higher initial discharge capacity and poorer cycling performance than the cathode prepared by freeze drying. The higher initial discharge capacity of the heat dried cathode is due to the short charge transfer path, which causes PEO to penetrate and contact the active material during rest. Since the reaction products dissolve in the PEO layer, the capacity of the heat dried cathode battery decreases with cycling. Since polysulfide dissolves and diffuses slowly from the thick electrode to the PEO layer, the freeze dried cathode shows a relatively stable capacity with cycling. Since a large amount of PEO electrolyte penetrates into the cathode prepared by freeze drying, the discharge product dissolves into the PEO that is still in contact with the conductive network of the electrode, and the discharge product can therefore be reused.

[0073] Fig. 9 The charge-discharge curves of Li-S cells with sulfur cathodes prepared by (a) thermal drying and (b) freeze drying are shown. -2 The electrochemical performance of solid-state lithium-sulfur batteries was measured with a LANDCT2001A battery test system at a current density of 3 V to 1.5 V. The samples were kept at 70 °C for about 12 hours before testing. The Li-S battery containing a thermally dried cathode showed more than 1200 mAh g in the first cycle. -1 S; however, the specific capacity decreases rapidly with additional cycles as it drops to about 800 mAhg at the tenth cycle. -1 Li-S batteries containing freeze-dried cathodes showed over 1000 mAh g in the first cycle -1 In other words, the Li-S battery with freeze-dried cathode provided about 1000 mAhg in the first ten cycles. -1 S, and because the curves of different cycles overlap each other, this suggests that the battery has the benefit of enhanced cycling stability.

[0074] Example 2

[0075] The slurry was prepared as described in Example 1, and then coated on an aluminum foil having a thickness of 150 μm.

[0076] The aluminum foil coated with the slurry was then frozen at -20°C for about 6 hours and then placed in a freeze dryer for about 12 hours to remove the water content in the slurry. After freeze drying, the electrode was cut into 2 cm x 2 cm sections. The sulfur content of the cathode was measured to be about 2.9 mg / cm 2 .

[0077] PEO powder and LiTFSI were mixed to form PEO and Li + The molar ratio of sulfur to sulfur is about 8:1 and dissolved in acetonitrile. The solid content of the slurry is about 5%. The slurry is poured on the freeze-dried cathode surface, and the cathode is then vacuum dried at about 60°C, where the solvent evaporates to form a sulfur cathode. As in Example 1, the cathode is designed to have a thickness of less than 200 μm.

[0078] Intermediate layer preparation

[0079] PEO powder and LiTFSI were mixed to form PEO and Li + The molar ratio of about 18:1 is dissolved in acetonitrile. The ionic liquid and 10 wt % SiO2 particles (less than 1000 nm) are added and mixed thoroughly. In some examples, the concentration of silica particles in PEO ranges from 1 wt % to 15 wt %, which is determined by the silica particle size. The SiO2 particles help reduce the crystallinity of PEO and increase the Li + Electrical conductivity: The interlayer electrolyte was obtained by pouring the obtained interlayer slurry mixture into a polytetrafluoroethylene (PTFE) mold and vacuum drying it.

[0080] The intermediate layer between the cathode and the electrolyte reduces the interfacial impedance. In order not to significantly reduce the mass energy density and volume energy density of the solid-state battery, the thickness of the intermediate layer is as thin as possible. In some examples, the thickness of the intermediate layer can be in the range of 5 μm to 50 μm.

[0081] Solid electrolyte preparation

[0082] The cubic phase Li is synthesized from the stoichiometric starting powders LiOH·H2O(AR), La2O3 (purity 99.99%), ZrO2(AR), and Ta2O5 (purity 99.99%). 6.4 Ln3Z 1.4 Ta 0.6 O 12(LLZTO). 2 wt% excess LiOH·H2O was added to compensate for lithium loss during sintering. Trace amounts of moisture and adsorbed CO2 were removed from La2O3 by heat treatment at 900°C for about 12 hours. The raw materials were mixed by a wet grinding process, in which yttrium-stabilized zirconium oxide (YSZ) balls and isopropyl alcohol (IPA) were used as grinding media. After the second mixing step, the mixture was dried and calcined at 950°C for about 6 hours in an alumina crucible, and then calcined again at 950°C for about 6 hours to obtain pure cubic garnet phase powder. After the second calcination process, the powder was pressed into green pellets of ~16 mm diameter and sintered in a platinum crucible at 1250°C for about 10 hours, which were covered with 10 wt% Li excess LLZTO powder. The sintered pellets were polished to a thickness of about 0.8 mm.

[0083] In some examples (e.g., Example 2), a thin layer of gold (Au) is sputter-coated on one side of the LLZTO ceramic for 10 minutes. The sample is then transferred to a glove box filled with argon. A portion of the Li foil is melted by heating to at least 250°C. The molten lithium is then poured onto the surface of the LLZTO pellet containing the sputter-coated gold layer. The final sulfur cathode (such as the sulfur cathode in Example 2) is then assembled into a battery together with the intermediate layer and the LLZTO-Au-Li solid electrolyte.

[0084] Battery Assembly

[0085] The Li-S battery obtained by the process described herein comprises a freeze-dried sulfur cathode coated with PEO, and a PEO-based interlayer coated on the sulfur cathode; an LLZTO ceramic solid electrolyte; and a lithium metal anode. The solid-state lithium-sulfur battery was assembled in a glove box filled with an inert gas (Ar), and the structure is shown in Figure 1 (Sulfur cathode / interlayer 1 / LLZTO / interlayer 2 / lithium anode).

[0086] Fig.10 A Li-S cell with a cathode prepared by freeze drying and a Li-Au anode (ie, Example 2) was shown to have a current density of 0.1 mA·cm at 60°C. -2 The solid-state Li-S battery shows a cycling performance of 980 mAh g -1 The initial discharge capacity and excellent cycle performance. After 30 cycles, the Li-S battery maintained 888 mAh g -1 of discharge capacity, which provides a capacity retention rate of 90%.

[0087] Therefore, as described herein, the present disclosure relates to solid-state lithium-sulfur batteries, and more specifically, to sulfur cathodes and methods for producing the same, wherein a porous sulfur cathode coated with a lithium ion conductive polymer layer is used in a solid-state lithium-sulfur battery. The sulfur electrode formed by the freeze-drying process disclosed herein is more porous and uniform than the cathode prepared by conventional thermal drying. In addition, this porous electrode structure helps the PEO electrolyte to penetrate into the cathode, thereby providing excellent contact between the cathode active material, the conductive carbon and the ion conductive network, and increasing the utilization of the sulfur active material. The PEO electrolyte coating can also improve interfacial stress and reduce interfacial resistance. Therefore, the Li-S battery manufactured using the S cathode formed by the method described herein has a higher reversible specific capacity, lower overall impedance and more stable cycle performance than the Li-S battery formed using the cathode prepared by thermal drying.

[0088] As used herein, the terms "approximately," "about," "substantially," and similar terms are intended to have a broad meaning consistent with the common and acceptable usage by those of ordinary skill in the art to which the subject matter of the present disclosure relates. Those skilled in the art who review the present disclosure should understand that these terms are intended to allow for a description of certain features described and claimed without limiting the scope of those features to the precise numerical ranges provided. Accordingly, these terms should be interpreted as indicating that insubstantial or minor modifications or alterations of the subject matter described and claimed are considered to be within the scope of the present invention as described in the appended claims.

[0089] As used herein, "optional" or "optionally" etc. are intended to indicate that the subsequently described event or circumstance may or may not occur, and that the description includes instances where the event or circumstance occurs and instances where it does not occur. Unless otherwise specified, the indefinite article "a" or "an" and the corresponding definite article "the" used herein mean at least one, or one or more.

[0090] The element positions mentioned herein (e.g., "top", "bottom", "above", "below", etc.) are only used to describe the orientation of the various elements in the drawings. It should be noted that the orientation of the various elements may be different according to other exemplary embodiments, and such changes are intended to be included within the scope of the present disclosure.

[0091] For substantially any plural and / or singular terms used herein, those skilled in the art may appropriately convert from the plural to the singular and / or from the singular to the plural as appropriate as applicable to the context and / or application. For clarity, various singular / plural arrangements may be explicitly described herein.

[0092] It will be apparent to those skilled in the art that various modifications and variations may be made without departing from the spirit or scope of the subject matter claimed. Therefore, the subject matter claimed is not limited by any content other than the attached claims and their equivalents.

Claims

1. A method for preparing a cathode of a lithium-sulfur battery, the method comprising: mixing a metal carbide, a carbon material, and a sulfur material in a solvent to form a sulfur precursor; dry milling the dried sulfur precursor to form a sulfur composite; The sulfur composite is mixed with a carbon material and a binder by stirring using water as a solvent to form a sulfur-based slurry; providing a substrate; disposing a sulfur-based slurry layer on a substrate; freeze drying the slurry layer to form a sulfur-based composite layer having a porosity ranging from 60% to 99%; as well as disposing a conductive polymer on top of the composite layer and within the pores of the composite layer, Wherein, the freeze-drying step comprises: Freezing the slurry layer at a temperature in the range of -50°C to 0°C for a period in the range of 1 hour to 12 hours; and The frozen slurry layer is dried in a freeze dryer for a period ranging from 1 hour to 24 hours.

2. The method of claim 1, wherein: The substrate is a current collector.

3. The method of claim 1, wherein: The carbon material is at least one of the following: nanoparticles, nanowires, nanofibers, nanorods, nanotubes, nanospheres, graphene, or a combination thereof, and The binder includes at least one of styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid (PAA), sodium alginate, or a combination thereof.

4. The method of claim 1, wherein: The porosity of the composite layer is in the range of 60% to 80%.

5. The method of claim 1, wherein: The size of the pores of the composite layer is in the range of 1 μm to 50 μm.

6. The method of claim 5, wherein: The size of the pores is in the range of 2 μm to 10 μm.

7. The method of claim 1, wherein: The step of disposing the conductive polymer is performed by at least one of spin coating, dip coating, layer-by-layer deposition, sol-gel deposition, inkjet printing, or a combination thereof.

8. A cathode of a lithium-sulfur battery, manufactured by the method according to any one of claims 1 to 7, wherein the cathode of the lithium-sulfur battery comprises: a sulfur-based composite layer having a porosity ranging from 60% to 99%; and A conductive polymer is disposed on top of the composite layer and within the pores of the composite layer.

9. The cathode according to claim 8, wherein The porosity of the composite layer is in the range of 60% to 80%.

10. The cathode according to claim 8, wherein The size of the pores of the composite layer is in the range of 1 μm to 50 μm.

11. The cathode according to claim 10, wherein The size of the pores is in the range of 2 μm to 10 μm.

12. The cathode of claim 8, wherein The composite layer includes a carbon material, and the carbon material exists as at least one of nanoparticles, nanowires, nanofibers, nanorods, nanotubes, nanospheres, graphene, or a combination thereof.

13. The cathode of claim 12, wherein The carbon material is present in an amount ranging from 5 wt % to 40 wt %.

14. The cathode of claim 8, wherein The composite layer contains metal carbide in the range of 1 wt % to 20 wt %.

15. The cathode of claim 8, wherein The conductive polymer comprises at least one of carbon polysulfide (CS), polyethylene oxide (PEO), polyaniline (PANI), polypyrrole (PPY), poly(3,4-ethylenedioxythiophene) (PEDOT), polystyrene sulfonic acid (PSS), polyacrylonitrile (PAN), polyacrylic acid (PAA), polyallylamine hydrochloride (PAH), poly(vinylidene fluoride-co-hexafluoropropylene) (P(VdF-co-HFP)), poly(methyl methacrylate) (PMMA), polyvinylidene fluoride (PVDF), poly(diallyldimethylammonium)bis(trifluoromethanesulfonyl)imide (TFSI) (PDDATFSI) or a combination thereof, and comprises at least one of bis(trifluoromethane)sulfonyl imide lithium salt (LiTFSI), lithium perchlorate, lithium bis(oxalate)borate (LiBOB), lithium bis(fluorosulfonyl)imide (LiFSI) or a combination thereof.

16. A lithium-sulfur battery comprising: Lithium anode; Solid electrolytes; and The cathode as claimed in claim 8.

17. The lithium-sulfur battery of claim 16, which is configured to have a discharge capacity retention rate of at least 90%.

18. The lithium-sulfur battery according to claim 17, wherein: The solid electrolyte comprises at least one of the following: Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 , Li 10 GeP2S 12 , Li 1.5 Al 0.5 Ge 1.5 (PO4)3、Li 1.4 Al 0.4 Ti 1.6 (PO4)3、Li 0.55 La 0.35 TiO3, interpenetrating polymer network electrolytes of poly(ethyl acrylate), three-dimensional ceramic / polymer networks, in situ plasticized polymers, composite polymers with well-aligned ceramic nanowires, PEO-based solid polymers, flexible polymers, polymeric ionic liquids, in situ formed Li3PS4, or combinations thereof.

19. A method of forming a lithium-sulfur battery, the method comprising: providing a substrate; A cathode is provided, the cathode being formed by: mixing a metal carbide, a carbon material, and a sulfur material in a solvent to form a sulfur precursor; dry milling the dried sulfur precursor to form a sulfur composite; The sulfur composite is mixed with a carbon material and a binder by stirring using water as a solvent to form a sulfur-based slurry; disposing a sulfur-based slurry layer on a substrate; freeze drying the slurry layer to form a sulfur-based composite layer having a porosity ranging from 60% to 99%; as well as disposing a conductive polymer on top of the composite layer and within the pores of the composite layer; Providing solid electrolytes; and Providing a lithium anode, Wherein, the freeze-drying step comprises: Freezing the slurry layer at a temperature in the range of -50°C to 0°C for a period in the range of 1 hour to 12 hours; and The frozen slurry layer is dried in a freeze dryer for a period ranging from 1 hour to 24 hours.

20. The method of claim 19, wherein: The solid electrolyte comprises at least one of the following: Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 , Li 10 GeP2S 12 , Li 1.5 Al 0.5 Ge 1.5 (PO4)3、Li 1.4 Al 0.4 Ti 1.6 (PO4)3、Li 0.55 La 0.35 TiO3, interpenetrating polymer network electrolytes of poly(ethyl acrylate), three-dimensional ceramic / polymer networks, in situ plasticized polymers, composite polymers with well-aligned ceramic nanowires, PEO-based solid polymers, flexible polymers, polymeric ionic liquids, in situ formed Li3PS4, or combinations thereof.

Citation Information

Patent Citations

  • Solid electrolytic capacitor containing a pre-coat layer

    CN104157461A

  • Graded porous composite lithium-sulfur battery cathode and preparation method thereof

    CN106410116A

  • Rechargeable lithium batteries having ultra-high volumetric energy density and required production process

    CN108140850A

  • Anode comprising multiple protective layers, and lithium secondary battery comprising same

    CN108713267A

  • Manufacture of electrode for fuel cell