Reducing defects in semiconductor layers and semiconductor devices by annealing and related methods

By annealing the semiconductor layer, the problem of defects between the GaN layer and the silicon substrate is solved, the signal conduction and current conduction efficiency is improved, the performance and reliability of the semiconductor device are improved, and the growth process is accelerated.

CN111211053BActive Publication Date: 2024-10-01SEMICON COMPONENTS IND LLC
0 Cites 0 Cited by

Patent Information

Application Number
CN201911040783.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-04-18
Filing Date
2019-10-30
Publication Date
2024-10-01
Estimated Expiration
2039-10-30

AI Technical Summary

Technical Problem

In semiconductor devices, the difference in material properties between the GaN layer and the silicon substrate leads to the generation of defects, affecting the efficiency of signal conduction and current conduction. There is also a mismatch in thermal expansion coefficients during the growth process, leading to the accumulation of defects.

Method used

Defects are reduced by using focused energy to anneal the semiconductor layer after it is isolated from the substrate. During the annealing process, focused energy such as laser can be used. The support structure supports the semiconductor layer to avoid deformation, and further growth is performed after annealing. Improves layer homogeneity and growth rate.

Benefits of technology

It significantly reduces the number of defects in the semiconductor layer, improves signal and current conduction capabilities, increases breakdown voltage, improves device performance and reliability, and accelerates the growth rate of the semiconductor layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111211053B_ABST
    Figure CN111211053B_ABST
Patent Text Reader

Abstract

The present invention is entitled "Reducing Defects in Semiconductor Layers and Semiconductor Devices by Annealing and Related Methods". The present invention relates to systems and methods. The systems and methods of the disclosed embodiments include reducing defects in a semiconductor layer. Defects can be reduced by forming a semiconductor layer on a substrate, removing at least a portion of the substrate from an underside of the semiconductor layer, and annealing the semiconductor layer to reduce defects in the layer. Annealing includes focusing energy at the layer.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] Semiconductor devices typically use several types of materials to create transistor switches in the circuits of the device. One common material is silicon, and techniques for purifying silicon for wafers used in semiconductor devices have been improved. Another material that can be used in semiconductor devices is gallium nitride (GaN). GaN is most typically formed by epitaxially growing a GaN layer on a substrate. For example, the substrate can be a silicon layer. However, growing GaN can result in defects in the GaN due to different material properties between the GaN and the substrate (e.g., a silicon substrate layer). BRIEF DESCRIPTION OF THE DRAWINGS

[0002] Figure 1 is a cross-sectional schematic side view of an embodiment of a semiconductor wafer having a GaN layer;

[0003] Figure 2 is a cross-sectional schematic side view of an embodiment of a semiconductor wafer illustrating an annealing process for reducing defects in a GaN layer;

[0004] Figure 3 is a cross-sectional schematic side view of an embodiment of a semiconductor wafer showing reduced defects in a GaN layer;

[0005] Figure 4 is a cross-sectional schematic side view of an embodiment of a semiconductor wafer showing filler below GaN;

[0006] Figure 5 is a cross-sectional schematic side view of an embodiment of a semiconductor wafer showing isolation of discrete semiconductor devices;

[0007] Figure 6 is a cross-sectional schematic side view of an embodiment of a semiconductor device showing an annealed GaN layer supported by a backing metal;

[0008] Figure 7 is a cross-sectional schematic side view of an embodiment of a semiconductor device showing an annealed GaN layer supported by a backing metal and a filler substrate;

[0009] Figure 8 is a cross-sectional schematic side view of an embodiment of a semiconductor device showing an annealed GaN layer and a backside source electrode supported by a backing metal;

[0010] Fig. 9 is a cross-sectional schematic side view of an embodiment of a semiconductor device showing an annealed GaN layer supported by a backing metal with a backside source and a filled substrate; and

[0011] Fig.10is a cross-sectional schematic side view of an embodiment of a semiconductor device showing an annealed GaN layer and a backside gate electrode supported by a backing metal. DETAILED DESCRIPTION

[0012] Solutions proposed to reduce defects in semiconductor layers include annealing the semiconductor layer with focused energy after it has been isolated from the substrate. This method is particularly beneficial in increasing the breakdown voltage of the semiconductor layer by increasing its ability to propagate electrical signals and conduct current.

[0013] Turning now to the accompanying drawings, Figure 1 1 is a cross-sectional schematic side view of an embodiment of a wafer 100. Wafer 100 includes a substrate layer 102 and an epitaxial semiconductor layer 104, such as gallium nitride (GaN). Wafer 100 may be of any size and configuration, such as 6 and 8 inch diameter wafers used in semiconductor manufacturing. The ratio of the thickness to the diameter of the wafer is not necessarily Figure 1 For example, the substrate 102 may include a silicon layer 1 to 100 microns thick. The substrate 102 is formed by any known method, such as purifying a silicon ingot and slicing to produce wafers that form the substrate layer 102.

[0014] After providing the substrate layer 102, the semiconductor layer 104 can be epitaxially grown on the substrate 102. For example, the material can grow to a total thickness of between 0.1 microns and 20 microns at a rate of 1 micron per hour. Alternatively, the semiconductor layer 104 can be added to the substrate 102 by other methods. The thickness of the semiconductor layer 104 enables the breakdown voltage to be from a few volts for a thin layer to several thousand volts for a thicker layer. In some embodiments, the material of the semiconductor layer 104 can include GaN, but can also include aluminum gallium nitride, silicon carbide, gallium arsenide, diamond, gallium oxide, and similar compositions on a silicon substrate, or can include these or other compositions on a germanium substrate or other substrate materials. The semiconductor layer 104 may include additional layers made of different materials, such as aluminum nitride (AlN), silicon nitride, silicon oxide, or any combination thereof.

[0015] When the semiconductor layer 104 is grown and / or formed on the face 108 of the substrate 102, the difference in the crystal properties between the semiconductor layer 104 and the substrate 102 may produce defects 106. For example, in an embodiment where the substrate 102 is silicon and the semiconductor layer 104 is GaN, the difference in the lattice structure may cause defects 106. That is, the larger lattice structure of silicon causes the face 108 to have small variations that do not match the lattice structure of GaN. Therefore, in order to grow GaN on the face 108 of silicon, the atoms of GaN are forced to form a configuration that does not match the natural lattice structure of pure GaN. In addition, the difference in the thermal expansion coefficient may also cause defects 106 to be produced. GaN is usually grown on silicon at an elevated temperature relative to typical atmospheric temperatures and then processed at a lower temperature. When the layers 102, 104 expand and contract, the substrate 102 may expand or contract more than the semiconductor layer 104. This can compress the semiconductor layer 104, which further exacerbates the generation of defects 106.

[0016] The defects 106 in the semiconductor layer 104 are relatively small, but may be numerous throughout the semiconductor layer 104. Individually, the defects 106 do not prevent signals from flowing through the semiconductor layer 104, but cumulatively, the defects 106 may cause power loss or other problems in circuits that use the semiconductor layer 104 in semiconductor devices. As described below, reducing the number and / or significance of the defects 106 may facilitate better signal and current flow through the semiconductor layer 104, and in certain embodiments, may facilitate increasing the growth rate of the semiconductor layer 104 in subsequent growth operations.

[0017] Figure 2 2 is a schematic cross-sectional side view of an embodiment of a wafer 200 having a semiconductor layer 204 and having a substrate layer 202, the semiconductor layer 204 having a defect 206 formed as described above, a portion of the substrate layer 202 being removed from below the semiconductor layer 204, leaving only a support ring 210. Alternatively, the substrate layer 202 may be completely removed, or a pattern may be left. The support ring 210 may surround the entire circumference of the wafer 200 to strengthen the wafer 200 during transportation and handling of the wafer 200. The substrate layer 202 may be removed by a combination of mechanical and chemical techniques. For example, a Taiko process may be used to grind away at least a portion of the substrate layer 202. Any remaining portion of the substrate layer 202 may be removed using a chemical wash. Specifically, a fluid chemical such as an acid etchant stops etching when it contacts the GaN / semiconductor layer 204, leaving the GaN substantially intact or unetched.

[0018] Once all or part of the substrate layer 202 is removed from beneath the semiconductor layer 204, the wafer 200 is subjected to focused energy 212 from the top of the semiconductor layer 204, or focused energy 214 from the bottom of the semiconductor layer 204, or any combination thereof. The focused energy 212, 214 is used to anneal the semiconductor layer 204 and reduce the defects 206. The reduction of the defects 206 can be the result of the heating of the semiconductor layer 204, which softens the semiconductor layer 204 and fuses (e.g., eliminates) the defects 206. This allows the defects 206 to be reduced due to the absence of the causes of the defects 206 during the annealing step (e.g., lattice mismatch and thermal differences). The semiconductor layer 204 can be supported by a support structure during the annealing process, particularly in embodiments where a large portion of the semiconductor layer 204 is annealed at once. That is, the semiconductor layer 204 can be sufficiently softened during the annealing procedure so that the support structure is necessary to prevent sagging or other deformation of the semiconductor layer 204.

[0019] The focused energy of the annealing process may include lasers of a wide wavelength / frequency range. For example, annealing may be accomplished using a short wavelength laser. Lasers of other wavelengths may also be used. The laser may be focused on selected areas of the semiconductor layer 204 and / or masked 216 from other areas to increase the effectiveness of the annealing in the selected area or to achieve other purposes.

[0020] Figure 3 3 is a cross-sectional schematic side view of an embodiment of a semiconductor wafer 300 showing reduced defects 306 in a semiconductor layer 304 and a support ring 310. The semiconductor layer 304 may include some defects 306, but Figure 2 After the annealing process shown, the defects 306 are significantly reduced. For example, the semiconductor layer 304 made of any combination of GaN or Si can have 10 9 The treatment disclosed in the embodiments herein can reduce dislocations and / or defects to as low as 10 per square centimeter. 7Due to the reduction in resistance and the improvement in homogeneity in the semiconductor layer 304, this reduction significantly improves device performance, reliability and cost. Compared with the same semiconductor layer 204 with defects 206 before the annealing process, the reduction of defects 306 enables the semiconductor layer 304 to handle signals from 25 percent higher voltage to signals with hundreds of percent higher voltage without power loss. For example, the breakdown voltage of a semiconductor using the annealed semiconductor layer 304 can be doubled, or alternatively, the semiconductor layer 304 may require half the thickness to achieve the breakdown voltage. The quality of the crystal is improved, which can improve electrical performance (lower resistance, reduced dynamic effects, higher system efficiency), reliability and wafer yield. In addition, because the defects 306 have been reduced, the semiconductor layer 304 can undergo further growth at an increased rate. That is, the top surface 322 of the semiconductor layer 304 is more susceptible to epitaxial growth. Therefore, after the annealing process is completed, the growth rate may be 50% to 1000% faster. Further growth may also be formed at the bottom of the semiconductor, preferably by placing the growth surface facing the incoming growth element.

[0021] like Figure 4 As shown, one or more embodiments of semiconductor wafer 400 may include a replacement substrate layer 420 within support ring 410. Because semiconductor layer 404 has been subjected to annealing, defects 406 have been reduced, and any differences that exist at face 408 of semiconductor layer 404 do not result in further defects 406. In addition, because defects 406 have been reduced, semiconductor layer 404 can undergo further growth at an increased rate. That is, top surface 422 of semiconductor layer 404 is more receptive to epitaxial growth. Therefore, the growth rate may be ten times faster after the annealing process is complete.

[0022] Alternatively, another embodiment utilizing a support element can be used prior to annealing. The support element is selected so that it does not cause the same lattice and thermal mismatch as the Si substrate. An example is a silicon oxide layer bonded to an engineered substrate or a top Si substrate. Silicon oxide is an amorphous material that does not form the same lattice stress as caused by a crystalline Si substrate. The support element may comprise an alloy of materials such as polysilicon, AlN, aluminum oxide, SiC, etc. Depending on the type of support element, it will be retained for further device fabrication and assembly, or removed in the desired step of the fabrication process.

[0023] Figure 5is a cross-sectional schematic side view of an embodiment of a semiconductor wafer 500 showing the isolation of discrete semiconductor devices 530. The isolation of semiconductor devices 530 on semiconductor layer 504 supported by support ring 510 is possible after semiconductor layer 504 has been separated from any substrate. The isolation of semiconductor devices 530 is electrical isolation, such as by nitrogen implantation, wherein semiconductor layer 504 is periodically converted into insulating strips 532.

[0024] Figure 6 6 is a cross-sectional schematic side view of an embodiment of a semiconductor device 630 that can be located on the above-mentioned semiconductor layer 104, 204, 304, 404, 504. The device 630 includes a backing metal 634, a drain 636 connected to a drain electrode 637, a gate 638 connected to a gate electrode 639, and a source 640 connected to a source electrode 641. The semiconductor layer 604 is annealed as described above, so that it can better pass signals and current between the drain 636 and the source 640. The backing metal 634 can be directly on the back side of the semiconductor layer 604. Figure 7 In the various embodiments shown, the semiconductor device 730 includes a substrate layer 720 between signal components (i.e., drain 736, gate 738, and source 740) and a backing metal 734 and also includes a semiconductor layer 704. As shown, the signal components 636 / 736, 638 / 738, 640 / 740 can be positioned with the source 640 / 740 located in a central position flanked by gates 638 / 738 and drains 636 / 736, or alternatively, the gates and drains can be positioned in different configurations. For example, the semiconductor device 730 can be a vertical trench configuration, or alternatively a lateral configuration.

[0025] Figure 8 830, showing a semiconductor layer 804 having a source electrode 841 connected to a backing metal 834 instead of an electrode on the front side of the semiconductor device 830. The drain 836, gate 838, and source 840 can be located in other conventional locations, but the source electrode 841 positioned through the semiconductor layer 804 allows the circuit in the semiconductor device 830 to be made more compact. Fig. 9 As shown, the source electrode 941 of the semiconductor device 930 may also pass through the substrate layer 920 that has been fabricated between the semiconductor layer 904 and the backing metal 934. The source electrode passing through the semiconductor is preferably formed by a metallized through hole that is electrically isolated by an insulating material at its sidewalls. The semiconductor device 930 may have a drain 936, a gate 938, and a source 940 positioned as shown. Alternatively, the semiconductor device 930 may include other configurations of the drain 936, the gate 938, and the source 940. Fig.10is a cross-sectional schematic side view of an embodiment of a semiconductor device 1030 showing a semiconductor layer 1004 having a gate electrode 1046 connected to a backing metal 1034. The semiconductor device 1030 can have a drain 1036, a gate 1038, and a source 1040 positioned as shown. Alternatively, the semiconductor device 1030 can include other configurations of the drain 1036, the gate 1038, and the source 1040, such as the drain being sandwiched and insulated at the bottom of the device.

[0026] Embodiment 1. As another embodiment, the present disclosure includes a method for reducing defects in a semiconductor layer, the method comprising: forming a semiconductor layer on a substrate; removing at least a portion of the substrate from a lower portion of the semiconductor layer; and annealing the semiconductor layer to reduce defects in the layer, wherein the annealing includes focusing energy at the layer.

[0027] Embodiment 2. The method of embodiment 1, wherein the semiconductor layer comprises gallium nitride (GaN), aluminum GaN, silicon carbide, gallium arsenide, diamond, gallium oxide, or any combination thereof.

[0028] Embodiment 3. The method of embodiment 2, wherein the semiconductor layer includes an additional layer comprising aluminum nitride (AlN), silicon nitride, silicon oxide, or any combination thereof.

[0029] Embodiment 4. The method of embodiment 1, wherein the semiconductor layer comprises an aluminum gallium nitride (AlGaN) layer, and wherein aluminum accounts for 5% to 50% of the AlGaN layer.

[0030] Embodiment 5. The method of embodiment 5, wherein the aluminum content in the AlGaN layer is greater than 27.5%.

[0031] Embodiment 6. The method of embodiment 1, wherein annealing the semiconductor layer comprises annealing with a laser.

[0032] Embodiment 7. The method of embodiment 6, wherein the laser comprises a short wavelength laser.

[0033] Embodiment 8. The method of Embodiment 6, wherein the laser annealing comprises focusing the laser on selected areas of the semiconductor layer and masking the laser from unselected areas of the semiconductor layer.

[0034] Embodiment 9. The method of embodiment 1, wherein separating the Si substrate comprises a Taiko process.

[0035] Embodiment 10. The method of Embodiment 1, wherein removing the Si substrate comprises removing a central portion of the Si substrate and not removing an outer support ring of the Si substrate.

[0036] Embodiment 11. The method of embodiment 1, comprising filling a substrate on the back side of the semiconductor layer.

[0037] Embodiment 12. The method of Embodiment 1, comprising growing additional gallium nitride (GaN) on the semiconductor layer after the semiconductor layer has been annealed.

[0038] Embodiment 13. The method of embodiment 1, comprising supporting the semiconductor layer with a support structure during annealing.

[0039] Embodiment 14. The method of embodiment 1, wherein growing the semiconductor layer comprises epitaxially growing a GaN layer.

[0040] Embodiment 15. As another embodiment, the present disclosure includes a method for manufacturing a semiconductor device, the method comprising growing a gallium nitride (GaN) layer on a silicon (Si) layer; removing a pattern of the Si layer from the GaN layer; annealing the GaN layer after the Si layer has been removed to reduce defects in the GaN layer; and adding a gate, a source, and a drain to the GaN layer.

[0041] Embodiment 16. The method of embodiment 15, comprising growing additional GaN after annealing and before adding the gate, source, and drain.

[0042] Although the subject matter of the present invention has been described above in conjunction with specific preferred embodiments and exemplary embodiments, the aforementioned drawings and descriptions thereof are only used to describe typical embodiments of the subject matter of the present invention and therefore should not be considered as limiting the scope of the subject matter of the present invention. Obviously, many alternatives and variations will be apparent to those skilled in the art.

[0043] As reflected in the claims below, aspects of the present invention may have fewer than all of the features of a single embodiment disclosed herein. Therefore, the claims expressed below are hereby expressly incorporated into the detailed description, and each claim itself represents an independent embodiment of the present invention. In addition, although some embodiments described herein include some features included in other embodiments, but do not include other features included therein, it should be understood by those skilled in the art that the combination of features of different embodiments is intended to fall within the scope of the present invention and is intended to form different embodiments.

Claims

1. A semiconductor device, comprising: a semiconductor layer comprising a gallium nitride (GaN) layer or an aluminum (GaN) layer, wherein structural defects within the semiconductor layer caused by growing the semiconductor layer on the substrate are reduced throughout the thickness of the semiconductor layer as a result of annealing the semiconductor layer by focused energy with at least some of the substrate removed from beneath the semiconductor layer; A backing metal directly contacts and supports the semiconductor layer; a drain electrode coupled to the first surface of the semiconductor layer and connected to the first electrode; as well as a source electrode coupled to the semiconductor layer and connected to a second electrode on a second surface of the semiconductor layer opposite to the first surface; a gate coupled to the first surface of the semiconductor layer; and The drain, source and gate are isolated from each other and provide a transistor device structure.

2. The semiconductor device according to claim 1, wherein the semiconductor layer has a thickness of 0.1 µm to 20 µm to allow a breakdown voltage from several volts to several kilovolts. 3 . The semiconductor device of claim 1 , wherein the semiconductor layer comprises aluminum GaN, and an aluminum percentage is between 5% and 50%. The semiconductor device according to claim 1 , wherein the semiconductor layer comprises annealed GaN. 5 . The semiconductor device of claim 1 , wherein the semiconductor layer further comprises a top surface that is more susceptible to epitaxial growth as a result of annealing by focused energy. 6 . The semiconductor device of claim 1 , wherein the semiconductor layer further comprises additional GaN or aluminum GaN grown on the semiconductor layer after annealing by focusing energy. 7 . The semiconductor device according to claim 6 , wherein the semiconductor layer includes unannealed GaN in addition to the annealed GaN.

8. The semiconductor device according to claim 1, wherein: reducing the structural defects caused by growing the semiconductor layer on the substrate throughout the thickness of the semiconductor layer as a result of annealing by focused energy with all of the substrate removed; as well as The backing metal directly contacts and supports the entire semiconductor layer.