Implantable Devices
By controlling the particle size and average content in the metal matrix of the vascular stent and optimizing the microstructure, the problem of insufficient plastic deformation ability of the vascular stent is solved, the risk of fracture is reduced, and the stability and safety of the device are improved.
Patent Information
- Application Number
- CN201811425843.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-11-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2038-11-27
AI Technical Summary
After implantation, existing vascular stents are insufficient in plastic deformation due to frequent vascular movements and contraction and diastolicity, and are prone to breaking due to fatigue, resulting in local mechanical vascular stimulation, inflammation and blood flow block, increasing clinical risks.
By controlling the size and average content of particulate matter in the metal matrix, the microstructure is optimized and the plastic deformation ability is improved. Specific methods include reasonably controlling the size of particles (greater than or equal to 1 μm, and the average content is within a specific range) in the metal matrix and reducing the content of particles and improving the continuity of materials through process processing such as electroslag remelting and vacuum arc smelting. .
It effectively improves the plastic deformation ability of implantable devices, reduces the risk of abnormal fracture, enhances the stability and safety of the devices, and reduces the occurrence of local blood flow block and inflammation.
Smart Images

Figure CN111297527B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of interventional medical devices, and in particular to an implantable device. Background Art
[0002] Vascular stents are a kind of implantable medical device in the form of a mesh tube, which can be used to treat various vascular diseases. Vascular stents are implanted into the diseased segment to support the stenotic and occluded segment of the blood vessel, reduce the elastic retraction and reshaping of the blood vessel, and maintain smooth blood flow in the lumen.
[0003] Vascular stents are generally formed of metal materials or polymer materials. Vascular stents are generally cut or woven into shape and then pressed onto a delivery balloon or retracted into a delivery sheath to be fixed on the delivery system. During this process, the outer diameter of the stent may be reduced by more than 50%, and undergo a large deformation. After the vascular stent is delivered to the lesion site, the vascular stent is released and expanded, and the outer diameter of the vascular stent is expanded by more than 200%, and undergoes a greater deformation. The vascular stent undergoes repeated large deformations during the pressing and expansion process. In addition, after implantation in the body, the stent will bend, stretch, or even twist in the blood vessel as the blood vessel moves and contracts and relaxes. The stent is subjected to periodic loads (such as radial pulsating extrusion, axial stretching, and bending) in the blood vessel, which places high demands on the plastic deformation capacity of the stent. However, the current stents have insufficient plastic deformation capacity, which makes the stent easily break due to fatigue after implantation, and even breaks during the expansion process. This will have adverse consequences: on the one hand, broken stent rods will cause local mechanical vascular stimulation, resulting in inflammation and neointimal hyperplasia; on the other hand, broken stent rods will cause damage to the local stent structure, leading to thrombosis and blood flow blockage, thereby affecting the blood supply to the organ. This will not only cause the local area of the stent to lose its radial support performance and make it difficult to play the role of radial support, but may also bring great clinical risks to patients.
[0004] The plastic deformation capacity of vascular stents is mainly related to their structural design and stent materials. When the structural design of the stent is certain, the plastic deformation capacity of the material itself will play a greater role. The plastic deformation capacity of metal-based materials depends on their microstructure, which includes grain size and orientation, metallographic structure, second phase particles and dislocation structure, etc. Different microstructures correspond to very different plastic deformation capacities. The plastic deformation capacity of the material can be optimized by optimizing the microstructure. Summary of the invention
[0005] Based on this, it is necessary to provide an implantable device with better plastic deformation ability.
[0006] An implantable device comprises a metal matrix, wherein the metal matrix contains particles, the size of the particles is greater than 1 μm, wherein:
[0007] When the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the average content of the particles is less than or equal to 40 ppm;
[0008] When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the average content of the particles is less than or equal to 100 ppm;
[0009] When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the average content of the particle is less than or equal to 220 ppm.
[0010] In one embodiment, when the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 10 μm, and the average content of the particles is less than or equal to 40 ppm;
[0011] When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 15 μm, and the average content of the particles is less than or equal to 100 ppm;
[0012] When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 20 μm, and the average content of the particle is less than or equal to 220 ppm.
[0013] In one embodiment, when the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the maximum size of the particles is less than or equal to 10 μm, and the average content of the particles is less than or equal to 20 ppm;
[0014] When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 15 μm, and the average content of the particles is less than or equal to 50 ppm;
[0015] When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 20 μm, and the average content of the particle is less than or equal to 110 ppm.
[0016] In one embodiment, when the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 20 ppm;
[0017] When the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 40 ppm;
[0018] When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 50 ppm;
[0019] When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 100 ppm;
[0020] When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 110 ppm;
[0021] When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 220 ppm.
[0022] In one embodiment, when the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 10 ppm;
[0023] When the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 20 ppm;
[0024] When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 25 ppm;
[0025] When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 50 ppm;
[0026] When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 55 ppm;
[0027] When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 110 ppm.
[0028] In one embodiment, when the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 10 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 10 ppm;
[0029] When the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 10 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 20 ppm;
[0030] When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 25 ppm;
[0031] When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 50 ppm;
[0032] When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 55 ppm;
[0033] When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 110 ppm.
[0034] In one embodiment, the material of the metal matrix is selected from one of nitrided iron, pure iron, cobalt-chromium alloy and magnesium alloy.
[0035] In one embodiment, the implantable device is a vascular stent, a biliary stent, an esophageal stent or a urethral stent.
[0036] In one embodiment, the vascular stent is a coronary vascular stent or a peripheral vascular stent.
[0037] In one embodiment, the material of the metal matrix is prepared by first performing electroslag remelting and then performing vacuum arc melting.
[0038] Experiments have shown that reasonably controlling the size and average content of particles according to the wall thickness of the metal matrix of the implantable device can optimize the microstructure of the metal matrix, which is beneficial to improving the plastic deformation capacity of the implantable device and reducing the risk of abnormal fracture of the implantable device. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 A schematic structural diagram of a metal substrate of an implantable device according to an embodiment;
[0040] Figure 2 for Figure 1 A schematic diagram of an axial expansion of a metal matrix of an implantable device shown;
[0041] Figure 3 is a scanning electron microscope (SEM) image of the fracture of the coronary stent of Example 2;
[0042] Figure 4 is a scanning electron microscope (SEM) image of the fracture of the coronary stent of Comparative Example 1;
[0043] Figure 5 This is a scanning electron microscope (SEM) image of the fracture of the coronary vascular stent of Comparative Example 2. DETAILED DESCRIPTION
[0044] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Preferred embodiments of the present invention are provided in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0046] The size of a particle referred to herein is the maximum distance between two points on the edge of the particle in the same plane.
[0047] An implantable device according to one embodiment is a vascular stent, a biliary stent, an esophageal stent or a urethral stent. In one embodiment, the vascular stent is a coronary stent or a peripheral vascular stent.
[0048] like Figure 1 As shown, the implantable device includes a metal substrate 100, and the metal substrate 100 is a hollow tubular structure.
[0049] Please also read Figure 2 The metal substrate 100 includes a plurality of corrugated rings 110 arranged along the axial direction Y and a connecting member 120 connecting two adjacent corrugated rings 110. The corrugated ring 110 includes a plurality of corrugated structures 112 arranged along the circumferential direction Z.
[0050] The material of the metal matrix 100 is a metal material. In one embodiment, the material of the metal matrix 100 is one of nitrided iron, pure iron, cobalt-chromium alloy and magnesium alloy. It is understood that in other embodiments, the material of the metal matrix 100 can be other metals or alloys other than the metals and alloys listed above, and any metal or alloy that can meet the requirements of implantable devices and has good biocompatibility with the organism can be used.
[0051] The material forming the metal matrix 100 contains a plurality of particles, resulting in the formation of a plurality of particles in the metal matrix 100, and the size of the particles is greater than or equal to 1 μm. The particles include externally introduced inclusions, as well as endogenous inclusions or second phases. The particles may originate from foreign matter introduced during the smelting process of the metal material. For example, during the smelting process of steel materials, oxides and silicates are formed due to the addition of deoxidizers, and sulfides and nitrides are formed during the solidification process of steel due to the decrease in the solubility of certain elements (such as sulfur and nitrogen). These particles do not have time to be discharged and remain in the steel. It is difficult to completely avoid the generation of particles, and the distribution of these particles is random, and it is difficult to accurately control their distribution.
[0052] The size and content of the particulate matter will have an adverse effect on the microstructure of the metal matrix 100, thereby causing a certain degree of deterioration in the plastic deformation ability of the metal matrix 100. The degree of deterioration is mainly related to the distribution of the particulate matter and the size of the particulate matter. Particulate matter distributed in the severely deformed area of the metal matrix 100 is more likely to cause abnormal fracture of the implantable device. The larger the size of the particulate matter, the more serious the damage to the continuity of the material, and the more likely it is to cause abnormal fracture of the implantable device. Therefore, controlling the particulate matter can reduce the risk of fracture of the implantable device. Therefore, it is necessary to reduce the content of the particulate matter, because the less the content of the particulate matter, the lower the probability of its distribution in the deformed part of the implantable device, and the less harm it will cause.
[0053] As for the size of the particles, the smaller the size of the particles, the less damage to the continuity of the material and the less harm. In addition, the smaller the size of the implantable device, the smaller the size of the particles is required. Especially in the field of vascular stents, thin-wall design is currently preferred. The thinner the wall thickness, the more it is necessary to control the size of the particles. Studies have found that for particles in metal-based materials, when the size of the particles is less than 1 μm, these submicron or nano-scale particles have basically no effect on the plastic deformation ability of the material, and can even play a strengthening effect and improve the strength of the material. However, when the size of the particles is above 1 μm, the particles will destroy the continuity of the material, which may cause the plasticity, toughness and fatigue properties of the material to decrease. If these particles appear at the deformation position of the metal matrix 100, it is very easy to cause abnormal fracture of the metal matrix 100 at these positions (such as fracture during expansion). Therefore, it is necessary to control the size and content of particles with a size of more than 1 μm.
[0054] In one embodiment, when the wall thickness of the metal substrate 100 is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the average content of the particles is less than or equal to 40 ppm.
[0055] When the wall thickness of the metal substrate 100 is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the average content of the particles is less than or equal to 100 ppm.
[0056] When the wall thickness of the metal substrate 100 is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the average content of the particles is less than or equal to 220 ppm.
[0057] In one embodiment, when the wall thickness of the metal substrate 100 is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 10 μm, and the average content of the particles is less than or equal to 40 ppm.
[0058] When the wall thickness of the metal substrate 100 is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 15 μm, and the average content of the particles is less than or equal to 100 ppm.
[0059] When the wall thickness of the metal substrate 100 is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 20 μm, and the average content of the particles is less than or equal to 220 ppm.
[0060] In one embodiment, when the wall thickness of the metal substrate 100 is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 10 μm, and the average content of the particles is less than or equal to 20 ppm.
[0061] When the wall thickness of the metal substrate 100 is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 15 μm, and the average content of the particles is less than or equal to 50 ppm.
[0062] When the wall thickness of the metal substrate 100 is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 20 μm, and the average content of the particles is less than or equal to 110 ppm.
[0063] In one embodiment, when the wall thickness of the metal substrate 100 is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal substrate 100 is 25-45%, the average particle content is less than or equal to 20 ppm.
[0064] When the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix 100 is greater than 45%, the average particle content is less than or equal to 40 ppm.
[0065] When the wall thickness of the metal matrix 100 is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix 100 is 25-45%, the average particle content is less than or equal to 50 ppm.
[0066] When the wall thickness of the metal matrix 100 is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix 100 is greater than 45%, the average particle content is less than or equal to 100 ppm.
[0067] When the wall thickness of the metal matrix 100 is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the theoretical overexpansion capacity of the metal matrix 100 is 25-45%, the average particle content is less than or equal to 110 ppm.
[0068] When the wall thickness of the metal matrix 100 is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the theoretical overexpansion capacity of the metal matrix 100 is greater than 45%, the average particle content is less than or equal to 220 ppm.
[0069] In one embodiment, when the wall thickness of the metal substrate 100 is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal substrate 100 is 25-45%, the average particle content is less than or equal to 10 ppm.
[0070] When the wall thickness of the metal matrix 100 is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix 100 is greater than 45%, the average content of the particles is less than or equal to 20 ppm.
[0071] When the wall thickness of the metal matrix 100 is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix 100 is 25-45%, the average particle content is less than or equal to 25 ppm.
[0072] When the wall thickness of the metal matrix 100 is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix 100 is greater than 45%, the average particle content is less than or equal to 50 ppm.
[0073] When the wall thickness of the metal matrix 100 is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the theoretical overexpansion capacity of the metal matrix 100 is 25-45%, the average particle content is less than or equal to 55 ppm.
[0074] When the wall thickness of the metal matrix 100 is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the theoretical overexpansion capacity of the metal matrix 100 is greater than 45%, the average particle content is less than or equal to 110 ppm.
[0075] In one embodiment, when the wall thickness of the metal matrix 100 is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 10 μm, and the theoretical overexpansion capacity of the metal matrix 100 is 25-45%, the average particle content is less than or equal to 10 ppm.
[0076] When the wall thickness of the metal matrix 100 is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 10 μm, and the theoretical overexpansion capacity of the metal matrix 100 is greater than 45%, the average particle content is less than or equal to 20 ppm.
[0077] When the wall thickness of the metal matrix 100 is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix 100 is 25-45%, the average particle content is less than or equal to 25 ppm.
[0078] When the wall thickness of the metal matrix 100 is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix 100 is greater than 45%, the average particle content is less than or equal to 50 ppm.
[0079] When the wall thickness of the metal matrix 100 is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix 100 is 25-45%, the average particle content is less than or equal to 55 ppm.
[0080] When the wall thickness of the metal matrix 100 is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix 100 is greater than 45%, the average particle content is less than or equal to 110 ppm.
[0081] Wherein, N is defined as the theoretical over-expansion capacity of the metal substrate 100, L is defined as the length of a wave coil 110 of the metal substrate 100 after being completely straightened, and D is defined as the nominal outer diameter of the metal substrate 100.
[0082] The nominal outer diameter refers to the nominal diameter of the metal matrix 100 plus twice the wall thickness. The nominal diameter refers to the inner diameter of the metal matrix 100 after expansion (the inner diameter of the metal matrix 100 after implantation in a blood vessel and expansion). The nominal diameter is expressed in the stent specifications. For example, the nominal diameter of a 30008 specification stent after expansion is 3 mm and the nominal length is 8 mm; the nominal diameter of a 27538 specification stent after expansion is 2.75 mm and the nominal length is 38 mm; the nominal diameter of a 35015 specification stent after expansion is 3.5 mm and the nominal length is 15 mm.
[0083] The average content of particles in the metal matrix 100 is the area occupied by particles in the metal matrix 100 per unit area of the metal matrix 100. That is, the average content of particles in the metal matrix 100 = the area occupied by particles in the detection area / the area of the detection area. Among them, the area of the detection area is the total area of the detection area, and the area occupied by particles in the detection area refers to the area of 10mm randomly detected under a scanning electron microscope at a magnification of 500 times. 2 The area occupied by the particles in the above detection area. There are at least two detection areas, which are distributed on two mutually perpendicular planes of the metal substrate 100, and the detection area of each detection area is 5mm 2 The above means that the average content of particulate matter = the total area occupied by the particulate matter in the multiple detection areas / the total area of the multiple detection areas.
[0084] The larger the size of the particles, the more the number of particles, and the larger the area of the particles per unit area of the metal substrate 100. When the average content of the particles is constant, if the size of the particles is large, the number of particles is small, so the probability of the particles appearing at the key deformation position is small, and the deterioration of the plastic deformation of the implantable device is small. However, when the average content of the particles is constant, if the number of particles is large, the size of the particles is small, and even if they appear at the key deformation position, the deterioration of the plastic deformation of the implantable device is small. Therefore, reasonable control of the size of the particles and the content of the particles is conducive to avoiding the adverse effects of the particles on the plastic deformation ability of the implantable device.
[0085] In one embodiment, the material of the metal matrix 100 is prepared by at least one of electroslag remelting and vacuum arc melting. The particles in the metal matrix 100 mainly come from its raw materials, and the level of the particles (size and average content) is basically not affected during the preparation process of the metal matrix 100. Therefore, it is necessary to control the level of particles in the raw materials. Electroslag remelting and vacuum arc melting can improve the purity of the metal material, reduce the level of particles in the metal material, and optimize the microstructure of the metal material, thereby optimizing the plastic deformation ability of the metal material.
[0086] Electroslag remelting uses the resistance heat generated by electric current passing through molten slag as a heat source to melt the electrode. The molten metal gathers into droplets and passes through the slag layer into the molten metal pool. In the process of passing through the slag layer, non-metallic inclusions are absorbed by the slag, and harmful elements (phosphorus, sulfur, lead, antimony, bismuth and tin, etc.) are effectively removed through steel-slag reaction and high-temperature vaporization, so that the steel ingot is purified and finally solidified into a casting in a water-cooled crystallizer.
[0087] Vacuum arc melting refers to a smelting method in which the molten material is used as one electrode and a water-cooled copper crucible is used as the other electrode under vacuum. An arc is struck between the two electrodes, and the molten material is melted by the high temperature of the arc and drips into the crucible, gradually melting and condensing into an ingot. Melting in a vacuum can significantly remove hydrogen and some volatile impurities, and can significantly reduce the content of particulate matter through the flotation effect.
[0088] In one embodiment, the material of the metal matrix 100 is prepared by first performing electroslag remelting and then performing vacuum arc melting. Performing electroslag remelting first and then further purifying by vacuum arc melting is conducive to reducing the content of particulate matter.
[0089] The size of the particles and the average content of the particles are reasonably controlled according to the wall thickness of the metal matrix 100 of the implantable device. Experiments have shown that this can effectively prevent the particles in the material from having an adverse effect on the microstructure of the metal matrix 100, which is beneficial to improving the plastic deformation capacity of the implantable device and reducing the risk of abnormal fracture of the implantable device.
[0090] Furthermore, by rationally controlling the particle size and average content according to the wall thickness of the metal matrix 100 and the theoretical overexpansion capacity of the metal matrix 100 , the microstructure of the metal matrix 100 can be further optimized, thereby improving the plastic deformation capacity of the implantable device.
[0091] The following is a specific embodiment section (the following embodiments take coronary artery stents and peripheral vascular stents as examples to further illustrate the above-mentioned implantable devices in detail, but the scope of protection of the present invention is not limited to this).
[0092] The particles referred to in the following examples are particles with a size of 1 μm or more. The samples in the following examples were prepared by grinding and polishing the materials on an ECOMet250 semi-automatic grinding and polishing machine produced by BRUKER to obtain a mirror-bright cross-section, and then observing it under a scanning electron microscope; or by placing the samples in liquid nitrogen for brittle fracture to obtain a cross-section, and then observing it under a scanning electron microscope with a magnification of 500 times.
[0093] The effect of particulate matter on the plastic deformation ability of the stent is evaluated through expansion test. Some raw materials are randomly selected to be made into 3 tubes or 3 wires to prepare vascular stents. The length of the tubes or wires made of the selected raw materials is not less than 1.0 meter. When the process conditions permit, these tubes or wires are made into stents for expansion test as much as possible. The stent is expanded until it breaks, and then the fracture is observed under a SEM scanning electron microscope produced by Japan Co., Ltd. If no particulate matter is found at the fracture, it means that the stent fracture is not caused by the influence of the particulate matter, and the particulate matter in the material has not caused serious deterioration in the plastic deformation ability of the stent.
[0094] Example 1
[0095] The raw material is nitrided iron, and the nitrided iron is prepared by electroslag remelting and then vacuum arc melting. A portion of the raw material is randomly cut and ground and polished to obtain a bright section, with an observation area of 15mm 2 The results are as follows: the maximum particle size is 5 μm, and the average particle content is 5 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare coronary stents with a wall thickness of 0.040 mm, and the theoretical over-expansion capacity was 60%.
[0096] The prepared coronary stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0097] Example 2
[0098] The raw material is nitrided iron, which is prepared by electroslag remelting. Randomly cut part of the material for grinding and polishing to obtain the bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 10 μm, and the average particle content is 10 ppm. Three 1.2-meter-long tubes were randomly selected from some raw materials to prepare coronary stents with a wall thickness of 0.053 mm, and the theoretical over-expansion capacity was 51%.
[0099] The prepared coronary stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0100] Example 3
[0101] The raw material is pure iron, which is prepared by vacuum arc melting. The raw material is placed in liquid nitrogen for brittle fracture, and the cross section is obtained. The observation area is 12mm2. The results are: the size of the largest particle is 10μm, and the average content of particles is 40ppm. Some of the raw materials are randomly selected to make three 1.5-meter-long pipes to prepare coronary stents with a wall thickness of 0.070mm, and its theoretical over-expansion capacity is 65%.
[0102] The prepared coronary stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0103] Example 4
[0104] The raw material is cobalt-chromium alloy, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, and the observation area is 10mm 2 The results are as follows: the maximum particle size is 15 μm, and the average particle content is 20 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare coronary stents with a wall thickness of 0.080 mm, and the theoretical overexpansion capacity was 45%.
[0105] The prepared coronary stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0106] Example 5
[0107] The raw material is nitrided iron, and the nitrided iron is prepared by electroslag remelting and then vacuum arc melting. A portion of the raw material is randomly cut and ground and polished to obtain a bright section, with an observation area of 15mm 2 The results are as follows: the maximum particle size is 5 μm, and the average particle content is 10 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare coronary stents with a wall thickness of 0.090 mm, and the theoretical overexpansion capacity was 36%.
[0108] The prepared coronary stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0109] Example 6
[0110] The raw material is nitrided iron, which is prepared by vacuum arc melting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 5 μm, and the average particle content is 10 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare coronary stents with a wall thickness of 0.100 mm, and the theoretical over-expansion capacity was 25%.
[0111] The prepared coronary stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0112] Example 7
[0113] The raw material is magnesium alloy, which is prepared by vacuum arc melting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, and the observation area is 10mm 2 The results are as follows: the maximum particle size is 10 μm, and the average particle content is 20 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare coronary stents with a wall thickness of 0.120 mm, and the theoretical over-expansion capacity was 60%.
[0114] The prepared coronary stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0115] Example 8
[0116] The raw material is nitrided iron, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 10 μm, and the average particle content is 25 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.150 mm, and the theoretical overexpansion capacity is 40%.
[0117] The prepared peripheral vascular stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0118] Example 9
[0119] The raw material is nitrided iron material, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, and the observation area is 10mm 2 The results are as follows: the maximum particle size is 15 μm, and the average particle content is 50 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.180 mm, and the theoretical overexpansion capacity was 50%.
[0120] The prepared peripheral vascular stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0121] Example 10
[0122] The raw material is cobalt-chromium alloy material, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, and the observation area is 10mm 2The results are as follows: the maximum particle size is 15 μm, and the average particle content is 60 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.190 mm, and the theoretical overexpansion capacity was 45%.
[0123] The prepared peripheral vascular stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0124] Embodiment 11
[0125] The raw material is nitrided iron, which is prepared by electroslag remelting. Prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain a bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 20 μm, and the average particle content is 100 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.200 mm, and the theoretical overexpansion capacity was 65%.
[0126] The prepared peripheral vascular stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0127] Example 12
[0128] The raw material is nitrided iron, which is prepared by electroslag remelting. Prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain a bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 10 μm, and the average particle content is 30 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.200 mm, and the theoretical overexpansion capacity was 35%.
[0129] The prepared peripheral vascular stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0130] Example 13
[0131] The raw material is pure iron, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, and the observation area is 10mm 2 The results are as follows: the maximum particle size is 15 μm, and the average particle content is 80 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.200 mm, and the theoretical overexpansion capacity was 65%.
[0132] The prepared peripheral vascular stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0133] Embodiment 14
[0134] The raw material is nitrided iron, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 20 μm, and the average particle content is 55 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.230 mm, and the theoretical overexpansion capacity was 60%.
[0135] The prepared peripheral vascular stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0136] Embodiment 15
[0137] The raw material is nitrided iron, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 15 μm, and the average particle content is 110 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.280 mm, and the theoretical over-expansion capacity was 50%.
[0138] The prepared peripheral vascular stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0139] Example 16
[0140] The raw material is nitrided iron, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 18 μm, and the average particle content is 40 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.290 mm, and the theoretical overexpansion capacity was 45%.
[0141] The prepared peripheral vascular stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0142] Embodiment 17
[0143] The raw material is nitrided iron, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 10 μm, and the average particle content is 20 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.300 mm, and the theoretical overexpansion capacity was 25%.
[0144] The prepared peripheral vascular stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0145] Embodiment 18
[0146] The raw material is nitrided iron, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 15 μm, and the average particle content is 60 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.300 mm, and the theoretical overexpansion capacity was 35%.
[0147] The prepared peripheral vascular stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0148] Embodiment 19
[0149] The raw material is nitrided iron, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 25 μm, and the average particle content is 220 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.300 mm, and the theoretical overexpansion capacity was 65%.
[0150] The prepared peripheral vascular stent was subjected to an expansion experiment, and no particles were found at the fracture.
[0151] Comparative Example 1
[0152] The raw material is nitrided iron, and the difference from Example 2 is that the average particle content is 50 ppm. Part of the raw materials are randomly selected to make three 1.2-meter-long pipes to prepare the same coronary stent as in Example 2.
[0153] The prepared coronary stent was subjected to an expansion experiment, and particles were found at the eight fractures of the coronary stent, such as Figure 3 As shown, Figure 3 There are particles in the circle.
[0154] Comparative Example 2
[0155] The raw material is nitrided iron, and the difference from Example 2 is that the maximum particle size is 20 μm. Part of the raw materials are randomly selected to make three 1.2-meter-long pipes to prepare the same coronary stent as in Example 2.
[0156] The prepared coronary stent was subjected to an expansion experiment, and particles were found at five fractures of the coronary stent, such as Figure 4 As shown, Figure 4 There are particles in the circle.
[0157] Comparative Example 3
[0158] The raw material is nitrided iron, and the nitrided iron is prepared by electroslag remelting and then vacuum arc melting. A portion of the raw material is randomly cut and ground and polished to obtain a bright section, with an observation area of 15mm 2 The results are as follows: the maximum particle size is 5 μm, and the average particle content is 25 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare coronary stents with a wall thickness of 0.090 mm, and the theoretical overexpansion capacity was 36%.
[0159] The prepared coronary stent was subjected to an expansion experiment, and particles were found at six fractures of the coronary stent.
[0160] Comparative Example 4
[0161] The raw material is nitrided iron, and the nitrided iron is prepared by electroslag remelting and then vacuum arc melting. A portion of the raw material is randomly cut and ground and polished to obtain a bright section, with an observation area of 15mm 2 The results are as follows: the maximum particle size is 20 μm, and the average particle content is 10 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare coronary stents with a wall thickness of 0.090 mm, and the theoretical overexpansion capacity was 36%.
[0162] The prepared coronary stent was subjected to an expansion experiment, and particles were found at four fractures of the coronary stent.
[0163] Comparative Example 5
[0164] The raw material is nitrided iron material, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, and the observation area is 10mm 2 The results are as follows: the maximum particle size is 15 μm, and the average particle content is 110 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.180 mm, and the theoretical overexpansion capacity was 50%.
[0165] The prepared peripheral vascular stent was subjected to an expansion experiment, and particles were found at eight fractures of the peripheral vascular stent.
[0166] Comparative Example 6
[0167] The raw material is nitrided iron material, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, and the observation area is 10mm 2 The results are as follows: the maximum particle size is 25 μm, and the average particle content is 50 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.180 mm, and the theoretical overexpansion capacity is 50%.
[0168] The prepared peripheral vascular stent was subjected to an expansion experiment, and particles were found at eight fractures of the peripheral vascular stent.
[0169] Comparative Example 7
[0170] The raw material is nitrided iron, which is prepared by electroslag remelting. Prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain a bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 10 μm, and the average particle content is 55 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.200 mm, and the theoretical overexpansion capacity was 35%.
[0171] The prepared peripheral vascular stent was subjected to an expansion experiment, and particles were found at seven fractures of the peripheral vascular stent.
[0172] Comparative Example 8
[0173] The raw material is nitrided iron, which is prepared by electroslag remelting. Prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain a bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 25 μm, and the average particle content is 30 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.200 mm, and the theoretical overexpansion capacity is 35%.
[0174] The prepared peripheral vascular stent was subjected to an expansion experiment, and particles were found at five fractures of the peripheral vascular stent.
[0175] Comparative Example 9
[0176] The raw material is nitrided iron, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, the observation area is 10mm 2The results are as follows: the maximum particle size is 15 μm, and the average particle content is 120 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.300 mm, and the theoretical overexpansion capacity was 35%.
[0177] The prepared peripheral vascular stent was subjected to an expansion experiment, and particles were found at 10 fractures of the peripheral vascular stent.
[0178] Comparative Example 10
[0179] The raw material is nitrided iron, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 30 μm, and the average particle content is 60 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.300 mm, and the theoretical overexpansion capacity was 35%.
[0180] The prepared peripheral vascular stent was subjected to an expansion experiment, and particles were found at eight fractures of the peripheral vascular stent.
[0181] Comparative Example 11
[0182] The raw material is nitrided iron, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 15 μm, and the average particle content is 230 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.280 mm, and the theoretical overexpansion capacity was 50%.
[0183] The prepared peripheral vascular stent was subjected to an expansion experiment, and particles were found at eight fractures of the peripheral vascular stent.
[0184] Comparative Example 12
[0185] The raw material is nitrided iron, which is prepared by electroslag remelting. Randomly cut part of the raw material for grinding and polishing to obtain the bright section, the observation area is 10mm 2 The results are as follows: the maximum particle size is 30 μm, and the average particle content is 110 ppm. Three 1.0-meter-long tubes were randomly selected from some raw materials to prepare peripheral vascular stents with a wall thickness of 0.280 mm, and the theoretical overexpansion capacity was 50%.
[0186] The prepared peripheral vascular stent was subjected to an expansion experiment, and particles were found at eight fractures of the peripheral vascular stent.
[0187] It can be seen from the above embodiments and comparative examples that by controlling the level of particulate matter in the material for vascular stents with different wall thicknesses, the adverse effects of the particulate matter on the plastic deformation ability of the stent can be avoided or reduced.
[0188] Among them, compared with Comparative Example 1, the average content of particles in Example 2 is lower, the probability of appearing in key deformation positions is small, and the adverse effect on the plastic deformation ability of the stent is small; compared with Comparative Example 2, the size of the largest particles in Example 2 is smaller, and the deterioration of the plastic deformation ability of the stent is smaller.
[0189] Compared with Comparative Example 3, the average content of particles in Example 5 is lower, the probability of appearing in key deformation positions is small, and the adverse effect on the plastic deformation ability of the stent is small; compared with Comparative Example 4, the size of the largest particles in Example 5 is smaller, and the deterioration of the plastic deformation ability of the stent is smaller.
[0190] Compared with Comparative Example 5, the average content of particles in Example 9 is lower, the probability of appearing in key deformation positions is small, and the adverse effect on the plastic deformation ability of the stent is small; compared with Comparative Example 6, the size of the largest particles in Example 9 is smaller, and the deterioration of the plastic deformation ability of the stent is smaller.
[0191] Compared with Comparative Example 7, the average content of particles in Example 12 is lower, the probability of appearing in key deformation positions is small, and the adverse effect on the plastic deformation ability of the stent is small; compared with Comparative Example 8, the size of the largest particles in Example 12 is smaller, and the deterioration of the plastic deformation ability of the stent is smaller.
[0192] Compared with Comparative Example 9, the average content of particles in Example 18 is lower, the probability of appearing in key deformation positions is small, and the adverse effect on the plastic deformation ability of the stent is small; compared with Comparative Example 10, the size of the largest particles in Example 18 is smaller, and the deterioration of the plastic deformation ability of the stent is smaller.
[0193] Compared with Comparative Example 11, the average content of particles in Example 15 is lower, the probability of appearing in key deformation positions is small, and the adverse effect on the plastic deformation ability of the stent is small; compared with Comparative Example 12, the size of the largest particles in Example 15 is smaller, and the deterioration of the plastic deformation ability of the stent is smaller.
[0194] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0195] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An implantable device comprising a metal substrate, characterized in that: The material of the metal matrix is selected from one of nitrided iron, pure iron, cobalt-chromium alloy and magnesium alloy, and the metal matrix contains externally introduced inclusions, endogenous inclusions or second phase particles, and the size of the particles is above 1 μm, wherein: When the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 20 ppm; When the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 40 ppm; When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 50 ppm; When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 100 ppm; When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 110 ppm; When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 220 ppm; The theoretical overexpansion capacity of the metal matrix is: Wherein, N is the theoretical over-expansion capacity of the metal matrix, L is the length of a wave coil of the metal matrix after being completely straightened, and D is the nominal outer diameter of the metal matrix; The nominal outer diameter of the metal substrate refers to the nominal diameter of the metal substrate plus twice the wall thickness; The nominal diameter of the metal matrix refers to the inner diameter of the metal matrix after expansion.
2. The implantable device according to claim 1, characterized in that When the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 10 ppm; When the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 20 ppm; When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 25 ppm; When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 50 ppm; When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 55 ppm; When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 25 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 110 ppm.
3. The implantable device according to claim 1, characterized in that When the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 10 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 10 ppm; When the wall thickness of the metal matrix is greater than or equal to 0.04 mm and less than or equal to 0.12 mm, the size of the largest particle is less than or equal to 10 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 20 ppm; When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 25 ppm; When the wall thickness of the metal matrix is greater than 0.12 mm and less than or equal to 0.2 mm, the size of the largest particle is less than or equal to 15 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 50 ppm; When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix is 25-45%, the average content of the particles is less than or equal to 55 ppm; When the wall thickness of the metal matrix is greater than 0.2 mm and less than or equal to 0.3 mm, the size of the largest particle is less than or equal to 20 μm, and the theoretical overexpansion capacity of the metal matrix is greater than 45%, the average content of the particles is less than or equal to 110 ppm.
4. The implantable device according to claim 1, characterized in that The implantable device is a vascular stent, a biliary stent, an esophageal stent or a urethral stent.
5. The implantable device according to claim 4, characterized in that The vascular stent is a coronary vascular stent or a peripheral vascular stent.
6. The implantable device according to claim 1, characterized in that The material of the metal matrix is prepared by first performing an electroslag remelting treatment and then performing a vacuum arc melting treatment.
7. The implantable device according to claim 1, characterized in that The metal matrix includes a plurality of corrugations arranged along an axial direction Y and a connecting piece connecting two adjacent corrugations.