Internal pressure test apparatus and test method for measuring the hoop tensile properties of fiber reinforced composite pipes for structural engineering
By designing an internal pressure test device for composite pipes, the edge effect, bending and friction problems in the measurement of the circumferential tensile performance of composite pipes are solved, and the circumferential elastic modulus and Poisson are realized. The accuracy of the ratio is suitable for composite tubes of different sizes and fiber winding angles, simplifying the test process and improving the reliability of the measurement.
Patent Information
- Application Number
- CN202010362447.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-04-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-04-30
AI Technical Summary
The existing test methods for measuring the mechanical properties of composite materials have problems such as edge effects, bending, friction and other problems when measuring the circumferential tensile elastic modulus and Poisson's ratio of composite pipes, resulting in large measurement errors and complex traditional hydraulic pressure test devices. Moreover, the adaptability to the dimensional deviation of composite pipes is poor, and accurate circumferential tensile performance parameters of composite pipes cannot be obtained.
An internal pressure test device with simple structure and easy to operate is designed, including upper and lower end plates, pulling screws, sealing rings and strain gauges. By pasting the strain gauge on the composite tube sample, the internal pressure is applied to make it expand evenly. The axial stress is obtained by straining the tension screw, and the circumferential elastic modulus and Poisson's ratio of the composite tube are calculated. It is suitable for composite tubes of different sizes and fiber winding angles.
The precise measurement of the annular tensile properties of composite pipes is achieved, the test process is simplified, the test process is widely applicable, it can adapt to the discrete geometric dimensions of composite pipes, and the test results are reliable, avoiding error problems in traditional methods.
Smart Images

Figure CN111398045B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a structural material performance detection technology in civil engineering, and in particular to an internal pressure test device and a test method for measuring the circumferential tensile performance of a fiber reinforced composite material pipe used in structural engineering. Background Art
[0002] Fiber reinforced composite materials have been widely used as a structural material in the field of civil engineering in recent years due to their high specific strength and excellent corrosion resistance. The most typical application is composite tube confined concrete. Under the action of axial pressure, the lateral expansion of concrete can be effectively constrained by the fibers arranged in a near circumferential direction, thereby greatly improving the strength and ductility of the component. For composite tube confined concrete, the circumferential tensile properties of the composite tube (including circumferential ultimate tensile strain, circumferential elastic modulus and Poisson's ratio), especially the circumferential elastic modulus, have a crucial influence on its mechanical properties. Among the test methods for measuring the tensile properties of composite materials, in addition to the traditional straight strip sheet tensile test and split disk test, scholars from all over the world have also proposed various test methods, but these existing methods have certain limitations in practical applications, especially in the problem of measuring the circumferential elastic modulus of composite tubes, there is still no accurate and convenient solution.
[0003] The straight sheet tensile test method for measuring the tensile properties of fiber-reinforced composites is clearly described in the test specifications of many countries and regions, such as "Standard Test Method for Tensile Properties of Polymer Matrix Composites" [ASTMD3039 / D3039M-14(2014)], "Standard Test Method for Tensile Properties of Fiber-Reinforced Composites for Civil Engineering Reinforcement" [ASTM D7565 / D7565 M-10(2017)], "Test Method for Tensile Properties of Directed Fiber-Reinforced Polymer Matrix Composites" [GB / T 3354(2014), "Test Method for Elastic Constants of Fiber-Reinforced Composites" [GB / T 32376(2015)], etc. However, the straight sheet tensile test method is mainly applicable to continuous unidirectional fiber-reinforced composite flat plates. For composite tubes used in structural engineering, in order to ensure that they have a certain axial stiffness, the winding or laying direction of the fiber often has a certain angle with the horizontal direction. For non-continuous eccentric materials, especially when the eccentricity is relatively large, the fiber material will be cut off at the edge of the specimen to form an edge effect, which will underestimate the elastic modulus of the material measured by the test; on the other hand, for composite pultruded or wound tubes, only arc-shaped specimens can be cut out along the circumferential direction, and the straight sheet tensile test method cannot be applied; for composite tubes made by manual wet laying, although straight sheet specimens with the same material and the same layup as the tube can be made and tensile tests can be carried out, due to the difference in curvature between the two and the different production methods, the results of the straight sheet tensile test method are difficult to accurately calibrate the actual performance of the composite tube.
[0004] Compared with the straight sheet test method, the split disk test method uses an annular specimen, which relatively completely maintains the original shape of the pipe and is widely used to measure the circumferential properties of composite pipes, such as the Standard Test Method for Apparent Circumferential Tensile Strength of Plastic or Reinforced Plastic Pipes [ASTM D2290-16 (2016)] and Plastic Piping Systems - Test Method for Apparent Initial Circumferential Tensile Strength of Glass Fiber Reinforced Thermosetting Plastic Pipes [ISO 8521 (2009)]. However, in the split disk test method, in order to reduce the adverse effect of the friction between the specimen and the split disk on the test results, the test section of the annular specimen should be as close as possible to the gap between the two semicircular split disks. However, as the test progresses, the two split disks gradually separate under the action of tension, and an unavoidable bend will occur on the test section of the specimen, resulting in the inability to obtain an accurate circumferential elastic modulus of the composite pipe in the end. In response to this problem, people have proposed many measures to improve the split disk test, such as keeping the test section of the specimen away from the gap of the split disk to eliminate the influence of the specimen bending on the test results. However, this treatment brings another problem: the friction between the specimen and the split disk causes a tensile stress gradient in the circumferential direction on the specimen, resulting in the inability to obtain the accurate tensile stress of the test section, and thus the inability to obtain accurate circumferential material properties of the composite tube. In addition, whether it is an industrially produced composite winding tube or a composite tube made by manual wet laying, its tube diameter and wall thickness have a certain degree of discreteness, and the split disk of fixed size has poor adaptability to the discreteness of the composite tube diameter. When the difference between the split disk and the composite tube diameter is greater, the measurement error caused by the bending of the test section will be more serious.
[0005] If you want to eliminate the influence of adverse factors such as boundary effect, bending, friction and so on on the determination of the circumferential performance of composite pipes, the internal pressure test of composite pipes is the best choice. On the one hand, the internal pressure test ensures the integrity of the sample. On the other hand, under the action of internal pressure, the composite pipe expands evenly, and its stress state is very similar to that of the composite pipe confined concrete. Therefore, the measured circumferential elastic modulus of the composite pipe is very reliable. The basic principle of the internal pressure test of composite pipes is consistent with the "Test Method for Short-term Water Pressure Failure of Fiber Reinforced Thermosetting Plastic Pipes" [GB / T 5351-2005]. However, if this national standard test method is used to determine the circumferential elastic modulus and Poisson's ratio of composite pipes, there are two problems: First, in order to allow the water pressure to be normally applied to the inner wall of the pipe and ensure that the test device does not leak during the pressurization process, the sealing device at its end is crucial. Especially for composite pipes with small diameters or thick walls, it is necessary to apply a very high internal pressure to obtain accurate circumferential material performance data, so the end sealing device is usually designed to be very complicated. The discreteness of the diameter and wall thickness of the composite tube often leads to the failure of the standardized size sealing device. Second, the sealing of the end during the test will inevitably cause axial stress in the specimen. If the influence of this part is not accurately considered, it will be impossible to obtain accurate circumferential tensile performance parameters of the composite tube.
[0006] In summary, based on the analysis of the existing technology, it can be known that the traditional test method for measuring the mechanical properties of composite materials has the following four main defects, which make it unsuitable for measuring the hoop tensile elastic modulus and Poisson's ratio of composite pipes for structural engineering:
[0007] Defect 1: The straight sheet tensile test method is only applicable to the determination of the relevant properties of the composite flat plate, and cannot solve the problem that the composite tube has an arc along the circumferential direction;
[0008] Defect 2: The unavoidable bending or friction problems of the split disk test method lead to large errors in the measured circumferential elastic modulus of the composite pipe, and the fixed-size separation disk has poor adaptability to the diameter deviation of the composite pipe;
[0009] Defect 3: The test device of the traditional water pressure test method is complicated and cumbersome, and has poor adaptability to the deviation of the composite pipe size (pipe diameter and wall thickness), making it difficult to promote and apply in actual projects;
[0010] Defect 4: The traditional water pressure test method does not take into account the axial stress on the composite pipe during the test, and cannot obtain accurate circumferential tensile performance parameters of the composite pipe.
[0011] In order to solve the limitations of the existing test methods, based on the existing technical conditions, a test method for measuring the hoop elastic modulus and Poisson's ratio of composite pipes for structural engineering is proposed, which is simple, feasible, reliable and widely applicable. Summary of the invention
[0012] In view of the technical problems existing in the prior art, the purpose of the present invention is to provide an internal pressure test device and a test method for measuring the circumferential tensile properties of fiber reinforced composite pipes for structural engineering, which have a simple structure, are easy to operate and have reliable results.
[0013] In order to achieve the above object, the present invention adopts the following technical solution:
[0014] The internal pressure test device for measuring the circumferential tensile properties of fiber reinforced composite pipes for structural engineering is characterized by: comprising an upper end plate, a lower end plate, a tension screw, a nut, a water inlet, an exhaust valve, a sealing ring, and a strain gauge; the lower end of the upper end plate and the upper end of the lower end plate are both provided with a groove, and screw holes are evenly arranged along the periphery of the groove; the sample is tubular, the upper end of the sample with the sealing ring is located in the groove of the upper end plate, and the lower end of the sample with the sealing ring is located in the groove of the lower end plate; the tension screw passes through the upper end plate and the lower end plate, and the two ends are locked by nuts; the upper end plate is provided with a water inlet and an exhaust valve; the strain gauge is attached to the outer wall of the sample and the middle of the tension screw.
[0015] As a preferred embodiment, the internal pressure testing device for measuring the circumferential tensile properties of fiber reinforced composite pipes for structural engineering further includes a reinforcement section; the reinforcement section is provided on the outer side of the upper end and the outer side of the lower end of the sample.
[0016] As a preference, the number of strain gauges is multiple groups, and at a position half the height of the specimen, the multiple groups of strain gauges are evenly distributed along the circumference; each group of strain gauges includes an axial strain gauge and a circumferential strain gauge.
[0017] As a preferred embodiment, there are multiple tension screws, which are evenly distributed around the circumference of the sample; and strain gauges are adhered to the middle of the tension screws along the longitudinal direction.
[0018] The internal pressure test method for measuring the circumferential tensile properties of fiber reinforced composite pipes for structural engineering uses an internal pressure test device for measuring the circumferential tensile properties of fiber reinforced composite pipes for structural engineering, and comprises the following steps:
[0019] a. Sample preparation: Cut the sample from the fiber reinforced composite material tube;
[0020] b. Sample installation: Paste strain gauges on the sample and the tension screw, set sealing rings on the upper and lower ends of the sample respectively, insert the upper end of the sample into the groove of the upper end plate, and insert the lower end of the sample into the groove of the lower end plate. Align the screw holes of the upper and lower end plates, put on the tension screw, and lock the upper and lower end plates by tightening the nuts at both ends of the tension screw, so as to seal the ends of the sample;
[0021] c. Pressurization: After the specimen is filled with water and exhausted, it is pressurized to the specified hoop strain through an external pressurizing device connected to the water inlet;
[0022] d. Data selection and calculation: Select the test data within the specified hoop strain range during the test process, and calculate the hoop elastic modulus and hoop Poisson's ratio of the fiber reinforced composite material tube.
[0023] As a preferred embodiment, in step a, the samples are taken from the same batch of fiber reinforced composite tubes as the fiber reinforced composite tube-constrained concrete components, and the total number of samples is not less than 5; the sample height H=2l+d, where l is the length of the reinforcement section, which is 10-30mm, and d is the inner diameter of the sample; the elastic modulus of the reinforcement section material corresponds to the elastic modulus of the sample.
[0024] As a preferred embodiment, in step b, the nuts at both ends of the tension screw are tightened symmetrically one by one; in the process of tightening the nuts, pay attention to the reading of the axial strain gauge on the specimen, and adjust the tightness of each nut to make the specimen evenly compressed axially, and ensure that the axial strain of the specimen does not exceed 0.03% when the ends of the specimen are sealed.
[0025] As a preferred embodiment, in step c, the sample is uniformly pressurized at a speed that ensures that the hoop strain of the sample increases by 0.001% per second.
[0026] As a preferred embodiment, in step d, the arithmetic mean, standard deviation and dispersion coefficient of the hoop elastic modulus are calculated, and the arithmetic mean, standard deviation and dispersion coefficient of the hoop Poisson's ratio are calculated.
[0027] As a preferred embodiment, in step b, the diameter and number of the tension screws are selected according to the following principles: when the maximum test internal pressure is reached, the stress of the tension screws should be less than or equal to 70% of the yield strength of the tension screws; 1 to 2 strain gauges are longitudinally pasted on the tension screws to monitor the strain level of the tension screws during the test.
[0028] The present invention is proposed after analyzing the existing composite material performance test methods:
[0029] For defect 1, the method adopted is to directly cut a composite tube sample along the circumference of the composite tube (fiber reinforced composite tube) to measure its circumferential elastic modulus and Poisson's ratio.
[0030] For defect 2, the method adopted is to directly apply internal pressure to the composite tube sample to make it expand evenly, thereby achieving uniform circumferential tensioning of the sample. The stress and strain difference within the specified circumferential strain range during the test is selected to calculate the circumferential elastic modulus and Poisson's ratio of the composite tube. There is no bending or friction problem in the split disk test.
[0031] For defect 3, the method adopted is to put sealing rings on both ends of the composite tube and insert them into the grooves of the end plates. Finally, the internal pressure test device is sealed by tightening the tension screws of the upper and lower end plates. The sealing rings at the ends have a certain elasticity, and the grooves of the end plates have a certain redundancy, which can adapt to fluctuations in the diameter and thickness of the specimen within a certain range.
[0032] For defect 4, the approach adopted is to consider that the composite pipe sample is in a bidirectional stress state during the internal pressure test, and obtain its tensile force by measuring the strain of the tension screw, and finally obtain the axial stress value of the composite pipe sample through axial force balance calculation.
[0033] The present invention has the following advantages:
[0034] 1. The present invention is a new type of simple test method, which can accurately measure the hoop tensile properties of fiber reinforced composite pipes for structural engineering (hereinafter referred to as: composite pipes), including hoop elastic modulus and Poisson's ratio.
[0035] 2. The end of the composite pipe can be sealed by a simple test device, which has a simple structure and is easy to operate.
[0036] 3. The wide applicability is mainly reflected in the following three aspects: (1) In addition to typical composite pultrusion and winding tubes, all composite tubes handmade by wet laying can be applied to this method; (2) There is a high degree of acceptance for the discrete level of the measured geometric dimensions (diameter and thickness) of the composite tubes; (3) It is applicable to composite tubes with any fiber winding or laying angle.
[0037] 4. The composite pipe can be pressurized evenly. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is a schematic diagram of the structure of the sample.
[0039] Figure 2 This is the arrangement diagram of strain gauges on the specimen.
[0040] Figure 3 It is a schematic diagram of the structure of the test device.
[0041] Figure 4 It is a three-dimensional diagram of the test device.
[0042] Figure 5 It is a three-dimensional diagram of the sealing ring.
[0043] Figure 6a is a top view of the lower end plate.
[0044] Figure 6b is a side view of the lower end plate.
[0045] Figure 7It is a three-dimensional view of the lower end plate.
[0046] Figure 8 It is the test hoop stress-strain curve.
[0047] Fig. 9 It is the axial tension-axial strain curve of the axial tensile test of the tension screw.
[0048] Among them, 1 is the upper end plate, 2 is the lower end plate, 3 is the tension screw, 4 is the nut, 5 is the water inlet, 6 is the exhaust valve, 7 is the sealing ring, 8 is the groove, 9 is the screw hole, 10 is the specimen, 11 is the reinforcement section, 12 is the axial strain gauge, and 13 is the annular strain gauge. DETAILED DESCRIPTION
[0049] An internal pressure test device for measuring the circumferential tensile properties of fiber reinforced composite pipes for structural engineering comprises an upper end plate, a lower end plate, a tension screw, a nut, a water inlet, an exhaust valve, a sealing ring, and a strain gauge; a groove is provided at the lower end of the upper end plate and the upper end of the lower end plate; the specimen is tubular, the upper end of the specimen with the sealing ring is located in the groove of the upper end plate, and the lower end of the specimen with the sealing ring is located in the groove of the lower end plate; the tension screw passes through the upper end plate and the lower end plate, and both ends are locked by nuts; a water inlet and an exhaust valve are provided on the upper end plate; the strain gauge is attached to the outer side wall of the specimen and the polished outer surface of the tension screw.
[0050] The following is a detailed description:
[0051] 1 sample
[0052] 1.1 Sample type
[0053] The specimens shall be taken from the same batch of composite tubes as the composite tube-confined concrete components, and the total number of specimens shall not be less than 5. The ends of the specimens may be reinforced. For specimen types, see Figure 1 D is the outer diameter of the specimen; d is the inner diameter of the specimen; t0 is the thickness of the reinforcement layer; l is the length of the reinforcement section; L is the distance between the two reinforcement sections; H is the height of the specimen; t is the thickness of the specimen. If the specimen does not leak at the end within the pressure range required by this test method, the end may be unreinforced.
[0054] 1.2 Sample size
[0055] The specimen height H = 2 × the length of the reinforcement section l + the inner diameter d of the specimen.
[0056] 1.3 Materials and manufacturing methods of specimen reinforcement section
[0057] In order to ensure the sealing effect of the sample end during the internal pressure test, the sample end is reinforced to increase the contact area between the sample end and the sealing ring.
[0058] 1.3.1 Length of the specimen reinforcement section
[0059] The length of the reinforcement section l is (10-30 mm), and the thickness of the reinforcement layer t0 should not be too thick while ensuring that the end face is watertight. It is recommended to be (0.5-1.0) times the wall thickness of the specimen.
[0060] 1.3.2 Material of the specimen reinforcement section
[0061] The elastic modulus of the material of the specimen reinforcement section should be as close as possible to the elastic modulus of the specimen.
[0062] 1.3.3 Reinforcement segment production method
[0063] 1.3.3.1 Cut the test specimen into appropriate length.
[0064] 1.3.3.2 The surface of the reinforced part of the specimen needs to be polished, and any lumps or other protrusions should be smoothed.
[0065] 1.3.3.3 Clean the surface of the reinforced part of the specimen with a solvent (such as acetone).
[0066] 1.3.3.4 Use wet winding with sufficient tension or vacuum resin infusion or other appropriate methods.
[0067] 1.3.3.5 After the resin is cured, the end face of the specimen is processed to meet the requirements of the end face of the specimen.
[0068] 1.4 Requirements for the end face of the specimen
[0069] In order to ensure the close fit between the end face of the sample and the sealing ring, the end face of the sample should be flat, without delamination, tearing, etc., and the rest of the surface should be free of damage. The two end faces of the sample are required to be parallel and perpendicular to the axis of the sample, and the parallelism should not be greater than 0.1mm.
[0070] 1.5 Pasting of the sample strain gauge
[0071] like Figure 2 As shown, 4-8 groups of strain gauges should be evenly pasted along the outer surface of the cross section at half the height of the specimen. If the diameter of the specimen is large, the number of strain gauges can be appropriately increased. Each group of strain gauges includes two unidirectional strain gauges, one arranged along the axial direction of the specimen and the other arranged along the circumferential direction. Strain gauges with a gauge length of 5mm to 20mm are preferably used.
[0072] 1.6 Number of samples
[0073] Each group of mechanical properties specimens shall not be less than 5, and there shall be 5 valid specimens in the same batch. The physical properties specimens shall comply with the requirements of the relevant standards.
[0074] 2 Test conditions
[0075] 2.1 Test environment conditions
[0076] 2.2.1 Laboratory standard environmental conditions
[0077] Temperature: (23±2)℃; Relative humidity: (50±10)%.
[0078] 2.2.2 Non-standard laboratory environmental conditions
[0079] If the laboratory standard environmental conditions are not available, select laboratory environmental conditions that are close to the laboratory standard environmental conditions.
[0080] 2.2 Test status adjustment
[0081] If conditions permit, place the device in an environment with a temperature of (23±2)℃ for at least 4 hours and conduct the test in the same environment. If conditions do not permit, conduct the test at the laboratory ambient temperature.
[0082] 3. Devices and Equipment
[0083] 3.1 Test apparatus
[0084] The test device of this internal pressure test method consists of upper and lower end plates and tension screws, such as Figure 3 and Figure 4 In the figure, B is the width of the end plate; t1 is the effective thickness of the end plate; h is the depth of the end plate groove; and D0 is the diameter of the end plate groove.
[0085] 3.1.1 Sealing system
[0086] The end sealing ring can be made of nitrile rubber UPH type or other sealing rings that can achieve the sealing effect, such as Figure 5 As shown, the sealing ring should be able to withstand the maximum test internal pressure and should avoid sealing failure caused by unreasonable selection and installation.
[0087] 3.1.2 End plate
[0088] 3.1.2.1 The upper and lower steel end plates of the test device should be flat and smooth. Figure 6a , Figure 6b and Figure 7 shown.
[0089] 3.1.2.3 Effective t1 of end plate: when diameter d is less than or equal to 200mm, t1≥25mm; when diameter d is greater than 200mm and less than or equal to 400mm, t1≥30mm; when diameter d is greater than 400mm and less than or equal to 600mm, t1≥35mm; when diameter d is greater than 600mm and less than or equal to 600mm, t1≥40mm.
[0090] 3.1.2.4 The diameter D0 of the end plate groove should be such that the end of the specimen after the sealing ring is put on can be tightly inserted into the end plate groove.
[0091] 3.1.2.5 The end plate groove depth h should be greater than or equal to the sealing ring height.
[0092] 3.1.3 Tension screw
[0093] The principle for selecting the diameter and number of the tension screw is: the stress of the tension screw should be less than or equal to 70% of the screw yield strength when the maximum test internal pressure is reached. The middle of the tension screw should be ground flat, and 1-2 strain gauges should be attached to it longitudinally to monitor the strain level of the screw during the test.
[0094] 3.1.4 Installation of test equipment
[0095] 3.1.4.1 Put the sealing rings on both ends of the sample and take care not to damage the sample during installation.
[0096] 3.1.4.2 Insert the two ends of the sealing ring on the specimen into the grooves of the upper and lower end plates respectively.
[0097] 3.1.4.3 Adjust the upper and lower end plates so that they are perpendicular to the specimen and ensure that the screw holes of the upper and lower end plates are aligned.
[0098] 3.1.4.4Install the tension screws and nuts.
[0099] 3.1.4.5 Tighten the nuts on the tension screws symmetrically one by one. During the process of tightening the nuts, pay attention to the reading of the axial strain gauge on the specimen, adjust the tightness of each nut to make the specimen evenly compressed in the axial direction, and ensure that the axial strain of the specimen does not exceed 0.03% under the action of the tension screws.
[0100] 3.2 Test equipment
[0101] The test pressurizing equipment can be a manual or electric pressure pump or a pressure supply system equipped with a pressure regulator and a hydraulic reservoir. The test equipment should meet the following requirements:
[0102] 3.2.1 The pressurized water should be kept clean and the water temperature should be within the range of (23±2)℃. If there are special requirements, the pressurized liquid medium or medium temperature can be specified separately.
[0103] 3.2.2 The pressure supply system should be selected so that the maximum internal pressure required for the test falls within the range of 10% to 90% of the full load (as far as possible on the full load side).
[0104] 3.2.3 The pressure supply system should be able to pressurize the sample evenly and continuously.
[0105] 3.2.4 The pressure supply system needs to be connected to a pressure sensor, the relative error of which should not be greater than 1% of the full scale, and the maximum internal pressure applied in the test should be around 60% of the full scale.
[0106] 3.2.5 Necessary safety protection measures should be taken during the test and the pressure system should be subject to safety checks.
[0107] 3.2.6 Test equipment should be calibrated regularly by a qualified metrology department.
[0108] 3.2.5 The test equipment for physical properties should comply with the requirements of relevant standards.
[0109] 3.3 Pressurization speed
[0110] The pressing speed is that the hoop strain of the specimen increases by 0.001% per second.
[0111] 4 Test steps
[0112] 4.1 The specimens shall be prepared in accordance with the provisions of 1.3, 1.4 and 1.5.
[0113] 4.2 The specimens shall be inspected visually. Any specimens with defects or not meeting the size and preparation requirements shall be discarded.
[0114] 4.3 Number the qualified samples and measure the sample dimensions. Before the samples are reinforced, measure the inner diameter, outer diameter and thickness of the samples respectively, with the measurement accuracy of 0.01mm. On the two end faces of the sample, measure the outer diameter in two directions perpendicular to each other, and take the average value as the average outer diameter. Measure the wall thickness at eight equally spaced points on any end face of the sample, discard the maximum and minimum values, and take the average value of the remaining points as the average wall thickness. The wall thickness of the sample is the average of the average wall thickness of the two end faces.
[0115] 4.4 The specimen state shall be adjusted in accordance with the provisions of 2.2.
[0116] 4.5 The installation of the specimen shall be in accordance with the provisions of 3.1.4.
[0117] 4.6 Connect the pressurizing system to the water inlet of the test device, open the exhaust valve, fill the sample with water, exhaust the air, and close the exhaust valve.
[0118] 4.7 All test data are reset to zero.
[0119] 4.8 The loading speed shall be in accordance with the provisions of 3.3, and the pressure shall be applied uniformly and continuously until the readings of all annular strain gauges on the specimen exceed 0.4%.
[0120] 4.9 During the test, the data that needs to be collected and stored include: internal pressure, strain of the specimen and the tension screw, and pressurization time.
[0121] 4.10 If the test device leaks before the maximum internal pressure required for the test is applied, or if the sample has obvious defects, it should be discarded. If there are less than 5 valid samples in the same batch, the test should be repeated.
[0122] 4.11 Complete the tensile test of the tension screw and measure the axial tension-axial strain curve of the tension screw, such as Fig. 9 shown.
[0123] 5. Calculation
[0124] 5.1 Figure 8 The figure shows the full process hoop stress-strain curve of the hoop tensile performance internal pressure test of a typical fiber reinforced composite pipe for structural engineering. θ is the hoop stress, ε ave is the average strain, ε θ,ave and ε x,ave They are the average values of the annular and axial strain gauge readings on the specimen, respectively. Fig. 9 The figure shows a typical axial tension-axial strain diagram of a tension screw. s and ε s is the axial tension and axial strain. In the above, tension is defined as positive and pressure is defined as negative.
[0125] 5.2 Calculate the hoop stress of the specimen according to formula (1):
[0126]
[0127] Where:
[0128] σ θ —— Hoop stress of the specimen (MPa);
[0129] P——internal pressure (MPa);
[0130] d——average inner diameter of the sample (mm);
[0131] t——average thickness of the specimen (mm).
[0132] 5.3 Calculate the axial stress of the specimen according to formula (2):
[0133]
[0134] Where:
[0135] σ x ——Axial stress of the specimen (MPa);
[0136] n——the number of tension screws;
[0137] F si——Tension force of the ith tension screw (MPa), according to the strain gauge reading ε on the tension screw si The axial tension-axial strain curve of the tension screw is obtained, such as Fig. 9 As shown;
[0138] A in ——Area enclosed by the inner wall of the specimen (mm 2 ), which is equal to πd 2 / 4;
[0139] A frp ——Cross-sectional area of the specimen (mm 2 ), which is equal to π[(d+2t) 2 -d 2 ] / 4.
[0140] 5.4 Calculate the hoop elastic modulus of the specimen according to formula (3):
[0141]
[0142] Where:
[0143] E θ ——The hoop elastic modulus of the specimen (MPa);
[0144] Δε θ,ave ——Calculate the average hoop strain increment corresponding to the selected straight line segment of the hoop stress-hoop strain curve, such as Figure 8 As shown, it should be at least 0.2%, and it is recommended to select the average hoop strain range of 0.1%-0.3%.
[0145] Δσ θ ——is the increment of the average hoop strain Δε θ,ave The corresponding hoop stress increment (MPa);
[0146] Δσ x ——is the increment of the average hoop strain Δε θ,ave The corresponding axial stress increment (MPa);
[0147] Δε x,ave ——is the increment of the average hoop strain Δε θ,ave The corresponding average axial strain increment;
[0148] E x ——It is the axial compressive elastic modulus of the composite pipe (MPa), which is measured by the axial compression test of the same batch of composite pipes. For the specific method, please refer to the "Test Method for Axial Compression Performance of Fiber Reinforced Thermosetting Plastic Pipe (GB5350-2005)".
[0149] 5.5 Calculate the circumferential Poisson’s ratio of the specimen according to formula (4):
[0150]
[0151] Where:
[0152] v θx ——is the annular Poisson’s ratio of the sample.
[0153] 6 Test results
[0154] The arithmetic mean, standard deviation, coefficient of dispersion, etc. of the test results such as the initial hoop elastic modulus and the initial hoop Poisson's ratio should be calculated. For large coefficients of dispersion, the specific reasons should be analyzed. If it is due to sample quality problems, a new batch of samples should be made and tested again.
[0155] 6.1 Performance value of each specimen: X1, X2, X3, ..., Xn. If necessary, the damage of each specimen should be stated.
[0156] 6.2 Calculate the arithmetic mean according to formula (5) to three significant figures:
[0157]
[0158] Where:
[0159] ——arithmetic mean;
[0160] X i ——Performance value of each sample;
[0161] n——number of samples.
[0162] 6.3 Calculate the standard deviation S according to formula (6) to two significant figures:
[0163]
[0164] Where:
[0165] S——standard deviation.
[0166] 6.4 Calculate the dispersion coefficient C according to formula (7) v , calculated to two significant figures:
[0167]
[0168] Where:
[0169] C v ——Dispersion coefficient.
[0170] 6.5 Confidence interval for the mean.
[0171] Calculated according to ISO 2602:1980.
[0172] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. An internal pressure test device for measuring the hoop tensile properties of fiber reinforced composite pipes for structural engineering, characterized in that: It includes an upper end plate, a lower end plate, a tension screw, a nut, a water inlet, an exhaust valve, a sealing ring, and a strain gauge; a groove is provided at the lower end of the upper end plate and the upper end of the lower end plate, and screw holes are evenly arranged along the periphery of the groove; the sample is tubular, the upper end of the sample with the sealing ring is located in the groove of the upper end plate, and the lower end of the sample with the sealing ring is located in the groove of the lower end plate; the tension screw passes through the upper end plate and the lower end plate, and the two ends are locked by nuts; the upper end plate is provided with a water inlet and an exhaust valve; the strain gauge is attached to the outer wall of the sample and the middle of the tension screw.
2. The internal pressure test device for measuring the hoop tensile properties of fiber reinforced composite pipes for structural engineering according to claim 1, characterized in that: It also includes a reinforcement section; the outer side of the upper end and the outer side of the lower end of the specimen are both provided with reinforcement sections.
3. The internal pressure test device for measuring the hoop tensile properties of fiber reinforced composite pipes for structural engineering according to claim 1, characterized in that: The number of strain gauges is multiple groups, and at the position of half the height of the specimen, the multiple groups of strain gauges are evenly distributed along the circumference; each group of strain gauges includes an axial strain gauge and a circumferential strain gauge.
4. The internal pressure test device for measuring the hoop tensile properties of fiber reinforced composite pipes for structural engineering according to claim 1, characterized in that: There are multiple tension screws, which are evenly distributed around the circumference of the specimen; strain gauges are adhered to the middle of the tension screws along the longitudinal direction.
5. An internal pressure test method for measuring the hoop tensile properties of a fiber reinforced composite material pipe for structural engineering, using the internal pressure test device for measuring the hoop tensile properties of a fiber reinforced composite material pipe for structural engineering as claimed in any one of claims 1 to 4, characterized in that: The steps include: a. Sample preparation: Cut the sample from the fiber reinforced composite material tube; b. Sample installation: Paste strain gauges on the sample and the tension screw, set sealing rings on the upper and lower ends of the sample respectively, insert the upper end of the sample into the groove of the upper end plate, and insert the lower end of the sample into the groove of the lower end plate. Align the screw holes of the upper and lower end plates, put on the tension screw, and lock the upper and lower end plates by tightening the nuts at both ends of the tension screw, so as to seal the ends of the sample; c. Pressurization: After the specimen is filled with water and exhausted, it is pressurized to the specified hoop strain through an external pressurizing device connected to the water inlet; d. Data selection and calculation: Select the test data within the specified hoop strain range during the test process, and calculate the hoop elastic modulus and hoop Poisson's ratio of the fiber reinforced composite material tube.
6. The internal pressure test method for measuring the hoop tensile properties of fiber reinforced composite pipes for structural engineering according to claim 5, characterized in that: In step b, tighten the nuts at both ends of the tension screw symmetrically one by one; pay attention to the reading of the axial strain gauge on the specimen during the tightening of the nuts, adjust the tightness of each nut to make the specimen evenly compressed in the axial direction, and ensure that the axial strain of the specimen does not exceed 0.03% when the ends of the specimen are sealed.
7. The internal pressure test method for measuring the hoop tensile properties of fiber reinforced composite pipes for structural engineering according to claim 5, characterized in that: In step c, the sample is uniformly pressurized at a speed that ensures that the hoop strain of the sample increases by 0.001% per second.
8. The internal pressure test method for measuring the hoop tensile properties of fiber reinforced composite pipes for structural engineering according to claim 5, characterized in that: In step d, the arithmetic mean, standard deviation and coefficient of dispersion of the hoop elastic modulus are calculated, and the arithmetic mean, standard deviation and coefficient of dispersion of the hoop Poisson's ratio are calculated.
9. The internal pressure test method for measuring the hoop tensile properties of fiber reinforced composite pipes for structural engineering according to claim 5, characterized in that: In step b, the principle for selecting the diameter and number of the tension screws is: when the maximum test internal pressure is reached, the stress of the tension screws should be less than or equal to 70% of the yield strength of the tension screws; 1 to 2 strain gauges are longitudinally attached to the tension screws to monitor the strain level of the tension screws during the test.
10. An internal pressure test method for measuring the hoop tensile properties of fiber reinforced composite pipes for structural engineering, characterized in that: An internal pressure test device for measuring the circumferential tensile properties of fiber reinforced composite pipes for structural engineering is used. The internal pressure test device includes an upper end plate, a lower end plate, a tension screw, a nut, a water inlet, an exhaust valve, a sealing ring, and a strain gauge; a groove is provided at the lower end of the upper end plate and an upper end of the lower end plate, and screw holes are evenly arranged along the periphery of the groove; the sample is tubular, the upper end of the sample with a sealing ring is located in the groove of the upper end plate, and the lower end of the sample with a sealing ring is located in the groove of the lower end plate; the tension screw passes through the upper end plate and the lower end plate, and the two ends are locked by nuts; a water inlet and an exhaust valve are provided on the upper end plate; the strain gauge is attached to the outer wall of the sample and the middle of the tension screw; The internal pressure test device also includes a reinforcement section; the outer side of the upper end and the outer side of the lower end of the specimen are both provided with reinforcement sections; Internal pressure test method The following steps are involved: a. Sample preparation: Cut the sample from the fiber reinforced composite material tube; b. Sample installation: Paste strain gauges on the sample and the tension screw, set sealing rings on the upper and lower ends of the sample respectively, insert the upper end of the sample into the groove of the upper end plate, and insert the lower end of the sample into the groove of the lower end plate. Align the screw holes of the upper and lower end plates, put on the tension screw, and lock the upper and lower end plates by tightening the nuts at both ends of the tension screw, so as to seal the ends of the sample; c. Pressurization: After the specimen is filled with water and exhausted, it is pressurized to the specified hoop strain through an external pressurizing device connected to the water inlet; d. Data selection and calculation: select the test data of the specified hoop strain range during the test process, and calculate the hoop elastic modulus and hoop Poisson's ratio of the fiber reinforced composite material tube; In step a, the samples are taken from the same batch of fiber reinforced composite tubes as the fiber reinforced composite tube-constrained concrete components, and the total number of samples is not less than 5; the sample height H=2l+d, where l is the length of the reinforcement section, which is 10-30mm, and d is the inner diameter of the sample; the elastic modulus of the reinforcement section material corresponds to the elastic modulus of the sample.
Citation Information
Patent Citations
Permeameter for contact surface of soil and works at high stress, high hydraulic gradient, and large shear deformation
CN102323159A
Piping test device of seepage corrosion stress coupling
CN102411042A
Bentonite two-way swelling force measuring instrument
CN105928643A
Method for evaluating binding strength of mechanical composite pipe
WO2013071673A1