Semiconductor device manufacturing method, substrate processing device and recording medium

By arranging multiple substrates vertically in the substrate processing device and adjusting the dilution gas flow rate, the problem of uneven film thickness distribution between substrates is solved and the uniformity of film thickness is achieved.

CN111755355BActive Publication Date: 2024-10-18KOKUSAI DENKI KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202010193528.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-03-18
Publication Date
2024-10-18
Estimated Expiration
2040-03-18

AI Technical Summary

Technical Problem

It is difficult to effectively control the film thickness distribution of thin films formed on multiple substrates with the existing technology, resulting in uneven film thickness.

Method used

By arranging a plurality of substrates and a substrate with a smaller surface area in the vertical direction, and supplying the processing gas in the substrate arrangement area, the film thickness is adjusted by using different flow rates of the diluting gas, specifically in the area including multiple large surface area substrates. A smaller flow rate of diluting gas is provided, while a larger flow rate of diluting gas is supplied in the area including the small surface area substrate.

Benefits of technology

This achieves uniform film thickness distribution of thin films formed on multiple substrates and reduces film thickness variation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111755355B_ABST
    Figure CN111755355B_ABST
Patent Text Reader

Abstract

The present invention is a method for manufacturing a semiconductor device, a substrate processing device, and a recording medium, which can control the inter-substrate film thickness distribution of a thin film formed on a plurality of substrates. The method for manufacturing a semiconductor device of the present invention includes: (a) a process of arranging a plurality of first substrates and a second substrate having a surface area smaller than that of the first substrate in a direction perpendicular to the surface direction and accommodating them in a processing chamber, and (b) a process of supplying a processing gas to a substrate arrangement area where a plurality of first substrates and a second substrate are arranged, thereby forming a thin film on the plurality of first substrates; in (b), while supplying a dilution gas to a first supply area including an area where at least a portion of the plurality of first substrates are arranged and not including an area where the second substrate is arranged, or not supplying a dilution gas, a dilution gas is supplied to a second supply area including an area where the second substrate is arranged, which is an area other than the first supply area, at a flow rate greater than the dilution gas flow rate supplied to the first supply area.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for manufacturing a semiconductor device that processes a substrate, a substrate processing device, and a recording medium. Background Art

[0002] As one of the steps in the process of manufacturing a semiconductor device, a process of supplying a process gas to a plurality of substrates to form a thin film on each substrate is sometimes performed (for example, refer to Patent Document 1).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2016 / 110956 Pamphlet Summary of the invention

[0006] Problems to be solved by the invention

[0007] An object of the present disclosure is to provide a technology capable of controlling the distribution of film thickness among substrates of a thin film formed on a plurality of substrates.

[0008] Solution to the problem

[0009] According to one embodiment of the present disclosure, there are:

[0010] (a) arranging a plurality of first substrates and a second substrate having a smaller surface area than the first substrate in a direction perpendicular to the surface direction and accommodating the plurality of first substrates in a processing chamber, and

[0011] (b) supplying a processing gas to a substrate arrangement region where the plurality of first substrates and the second substrates are arranged, thereby forming a thin film on the plurality of first substrates;

[0012] (b) comprising the following steps:

[0013] The dilution gas is supplied to a first supply region in the substrate arrangement region or the dilution gas is not supplied, wherein the first supply region includes a region where at least a portion of the plurality of first substrates are arranged and does not include a region where the second substrate is arranged, and

[0014] A step of supplying the dilution gas at a flow rate greater than the flow rate of the dilution gas supplied to the first supply region to a second supply region in the substrate arrangement region, which is a region other than the first supply region and includes a region where the second substrate is arranged.

[0015] Effects of the Invention

[0016] According to the technology according to the present disclosure, it is possible to control the distribution of film thickness among substrates of thin films formed on a plurality of substrates. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] [ Figure 1 ] is a schematic diagram of the structure of a vertical processing furnace of a substrate processing device suitable for use in one embodiment of the present disclosure, and is a diagram showing a processing furnace portion in a vertical cross-sectional view.

[0018] [ Figure 2 ] is a schematic diagram of a vertical processing furnace of a substrate processing device suitable for use in one embodiment of the present disclosure, Figure 1 The AA line cross-sectional view is used to show the processing furnace part.

[0019] [ Figure 3 ] is a schematic configuration diagram of a controller of a substrate processing device suitable for use in one embodiment of the present disclosure, and is a diagram showing the control system of the controller in the form of a block diagram.

[0020] [ Figure 4 ] is a diagram showing an example of a film forming process according to an embodiment of the present disclosure.

[0021] [ Figure 5 ] is a diagram showing the arrangement state of wafers according to one embodiment of the present disclosure.

[0022] [ Figure 6 ] is a diagram showing the arrangement state of wafers according to other embodiments of the present disclosure.

[0023] [ Figure 7 ] is a diagram showing the arrangement state of wafers according to another embodiment of the present disclosure.

[0024] [ Figure 8 ] is a diagram showing the arrangement state of wafers according to another embodiment of the present disclosure.

[0025] [ Fig. 9 ] is a schematic diagram of the structure of a nozzle suitable for use in one embodiment of the present disclosure.

[0026] [ Fig.10 ] is a schematic diagram of the structure of a nozzle suitable for use in other embodiments of the present disclosure.

[0027] [ Fig.11 ] is a graph showing the measurement results of the thickness of the oxide film formed on the substrate in the reference example and the embodiment.

[0028] Explanation of symbols

[0029] 200: Wafer (substrate)

[0030] 249a: Nozzle (raw material supply unit)

[0031] 249b: Nozzle (oxidizing agent supply unit, nitriding agent supply unit)

[0032] 249c~249e: Nozzle (inert gas supply part). DETAILED DESCRIPTION

[0033] Hereinafter, for one embodiment (first embodiment) of the present disclosure, Figure 1 to Figure 5 , Fig. 9 etc. for explanation.

[0034] (1) Configuration of substrate processing apparatus

[0035] like Figure 1 As shown, the processing furnace 202 has a heater 207 as a heating mechanism (temperature adjustment unit). The heater 207 is cylindrical and is vertically installed by supporting a holding plate. The heater 207 also functions as an activation mechanism (excitation unit) that activates (excites) the gas by heat.

[0036] A reaction tube 210 is disposed concentrically with the heater 207 inside the heater 207. The reaction tube 210 has a double tube structure including an inner tube 204 as an inner reaction tube and an outer tube 203 as an outer reaction tube concentrically surrounding the inner tube 204. The inner tube 204 and the outer tube 203 are each made of, for example, quartz (SiO 2 ) or heat-resistant materials such as silicon carbide (SiC), and is formed into a cylindrical shape with a closed upper end and an open lower end.

[0037] A processing chamber 201 for processing wafers 200 as substrates is formed in the hollow portion of the inner tube 204. The processing chamber 201 is configured to accommodate the wafers 200 in a state of being arranged from one end side (lower side) to the other end side (upper side) in the processing chamber 201 in a direction perpendicular to the surface direction of the wafers 200. The area in the processing chamber 201 where a plurality of wafers 200 are arranged is also referred to as a substrate arrangement area (wafer arrangement area). In addition, the arrangement direction of the wafers 200 in the processing chamber 201 is also referred to as a substrate arrangement direction (wafer arrangement direction).

[0038] The inner tube 204 and the outer tube 203 are supported from below by a header 209, respectively. The header 209 is made of a metal material such as stainless steel (SUS) and is formed into a cylindrical shape with upper and lower ends opened. An annular flange portion 209a made of a metal material such as SUS and extending radially inwardly of the header 209 is provided at the upper end of the inner wall of the header 209. The lower end of the inner tube 204 abuts against the upper surface of the flange portion 209a. The lower end of the outer tube 203 abuts against the upper end of the header 209. An O-ring 220a as a sealing member is provided between the outer tube 203 and the header 209. The lower end opening of the header 209 constitutes the furnace port of the processing furnace 202, and is airtightly closed by a disc-shaped sealing cap 219 as a cover when the wafer box 217 is raised by the wafer box elevator 115 described later. An O-ring 220 b serving as a sealing member is provided between the header 209 and the sealing cap 219 .

[0039] The top of the inner tube 204 is formed in a flat shape, and the top of the outer tube 203 is formed in a dome shape. If the top of the inner tube 204 is formed in a dome shape, the gas supplied to the processing chamber 201 will not flow between the plurality of wafers 200, but will easily flow into the internal space of the dome portion in the top of the inner tube 204. By making the top of the inner tube 204 flat, the gas supplied to the processing chamber 201 can effectively flow between the plurality of wafers 200. By making the gap (space) between the top of the inner tube 204 and the top plate of the wafer box 217 described later smaller, for example, by making the arrangement intervals (pitch) of the wafers 200 substantially the same, the gas can effectively flow between the wafers 200.

[0040] like Figure 2As shown, a nozzle accommodation chamber 204a for accommodating nozzles 249a, 249b, and 249d and a nozzle accommodation chamber 204b for accommodating nozzles 249c and 249e are formed on the side wall of the inner tube 204. The nozzle accommodation chambers 204a and 204b protrude from the side wall of the inner tube 204 toward the outside in the radial direction of the inner tube 204, respectively, and are formed into a channel shape extending in the vertical direction. The inner walls of the nozzle accommodation chambers 204a and 204b respectively constitute a part of the inner wall of the processing chamber 201. The nozzle accommodation chamber 204a and the nozzle accommodation chamber 204b are respectively arranged at positions separated by a predetermined distance from each other along the inner wall of the inner tube 204, that is, along the outer circumference of the wafer 200 accommodated in the processing chamber 201. Specifically, the nozzle accommodation chambers 204a and 204b are respectively arranged at such positions that the central angle θ (the central angle of the arc with the centers of the nozzle accommodation chambers 204a and 204b as both ends) formed by the straight line L1 connecting the center of the wafer 200 accommodated in the processing chamber 201 and the center of the nozzle accommodation chamber 204a and the straight line L2 connecting the center of the wafer 200 accommodated in the processing chamber 201 and the center of the nozzle accommodation chamber 204b is, for example, in the range of 30 to 150 degrees. The nozzles 249b and 249d accommodated in the nozzle accommodation chamber 204a are arranged to sandwich the nozzle 249a on both sides thereof, that is, to sandwich the nozzle 249a from both sides along the inner wall of the nozzle accommodation chamber 204a (the outer periphery of the wafer 200). In this specification, the nozzles 249a and 249b are also referred to as R1 and R2, respectively, and the nozzles 249c, 249d, and 249e are also referred to as Rt, Rc, and Rb, respectively. The nozzles 249c to 249e are also referred to as Rt to Rb.

[0041] The nozzles 249a to 249e are respectively arranged to extend from the lower part of the nozzle accommodation chambers 204a and 204b to the upper part, that is, to stand upright along the wafer arrangement direction. That is, the nozzles 249a to 249e are respectively arranged to extend along the wafer arrangement area in the area horizontally surrounding the wafer arrangement area on the side of the wafer arrangement area. Fig. 9 As shown, gas ejection ports 250a to 250e as first to fifth gas supply ports are provided on the side surfaces of the nozzles 249a to 249e, respectively. The nozzles 249a to 249e are made of a heat-resistant material such as quartz or SiC.

[0042] like Fig. 9As shown, it is also possible to consider dividing the above-mentioned wafer arrangement area into a plurality of partitions. In this embodiment, the partition on one end side (here, the upper side) in the wafer arrangement direction of the wafer arrangement area is also referred to as the first partition (top partition). In addition, the partition in the central part of the wafer arrangement direction of the wafer arrangement area is also referred to as the second partition (middle partition). In addition, the partition on the other end side (here, the lower side) in the wafer arrangement direction of the wafer arrangement area is also referred to as the third partition (bottom partition).

[0043] A plurality of gas ejection ports 250a and 250b of the nozzles 249a and 249b are provided from the upper part to the lower part so as to correspond to the entire area of ​​the wafer arrangement direction of the wafer arrangement area. The nozzles 249a and 249b (i.e., R1 and R2) are configured to supply gas to all the first to third partitions, respectively.

[0044] The gas ejection ports 250c of the nozzle 249c are provided in plurality only on the upper side of the nozzle 249c to correspond to the upper side region (i.e., the first partition) in the wafer arrangement direction of the wafer arrangement region. The nozzle 249c (i.e., Rt) is configured to supply gas to the first partition but not to supply gas to the partitions other than the first partition (i.e., the second partition and the third partition).

[0045] The gas ejection ports 250d of the nozzle 249d are provided in plurality only on the central side of the nozzle 249d to correspond to the central side region (i.e., the second partition) in the wafer arrangement direction of the wafer arrangement region. The nozzle 249d (i.e., Rc) is configured to supply gas to the second partition but not to the partitions (i.e., the first partition and the third partition) other than the second partition.

[0046] The gas ejection ports 250e of the nozzle 249e are provided in plurality only on the lower side of the nozzle 249e to correspond to the lower side region (i.e., the third partition) in the wafer arrangement direction of the wafer arrangement region. The nozzle 249e (i.e., Rb) is configured to supply gas to the third partition but not to the partitions (i.e., the first partition and the second partition) other than the third partition.

[0047] The gas ejection ports 250a to 250e are configured to open toward the center of the processing chamber 201, respectively, and can supply gas toward the center of the wafer 200. The gas ejection ports 250a to 250e have the same opening area, respectively, and are provided at the same opening pitch.

[0048] like Figure 2As shown, nozzles 249a to 249e are connected to gas supply pipes 232a to 232e, respectively. In the gas supply pipes 232a to 232e, mass flow controllers (MFCs) 241a to 241e as flow controllers (flow control units) and valves 243a to 243e as switch valves are respectively provided in order from the upstream side of the gas flow. On the downstream side of the gas supply pipe 232a than the valve 243a, the gas supply pipe 232g is connected. In the gas supply pipe 232g, MFCs 241g and valves 243g are respectively provided in order from the upstream side of the gas flow. On the downstream side of the gas supply pipe 232b than the valve 243b, the gas supply pipes 232f and 232h are connected. In the gas supply pipes 232f and 232h, MFCs 241f and 241h and valves 243f and 243h are respectively provided in order from the upstream side of the gas flow.

[0049] A halosilane gas as a raw material (raw material gas) is supplied from a gas supply pipe 232a into the processing chamber 201 via MFC 241a, valve 243a, and nozzle 249a. The halosilane gas contains silicon (Si) and halogen elements as main elements constituting the film to be formed.

[0050] Raw material gas refers to a raw material in a gaseous state, for example, a gas obtained by vaporizing a raw material in a liquid state at room temperature and pressure, a raw material in a gaseous state at room temperature and pressure, etc. Halogenated silane gas refers to a silane gas having a halogen group. Halogen groups include halogen elements such as chlorine (Cl), fluorine (F), bromine (Br), and iodine (I). As a halosilane gas, for example, a raw material gas containing Si and Cl, that is, a chlorosilane gas, can be used. Chlorosilane gas acts as a Si source. As a chlorosilane gas, for example, hexachlorodisilane (Si 2 Cl 6 , referred to as: HCDS) gas.

[0051] The oxygen-containing (O) gas as a reactant (reaction gas) is supplied to the processing chamber 201 via the MFC 241b, the valve 243b, and the nozzle 249b through the gas supply pipe 232b. The oxygen-containing (O) gas acts as an oxidant (oxidizing gas). The O-containing gas acts as an O source. For example, oxygen (O 2 )gas.

[0052] A nitrogen (N)-containing gas as a reactant (reaction gas) is supplied from the gas supply pipe 232f to the processing chamber 201 via the MFC 241f, the valve 243f, the gas supply pipe 232b, and the nozzle 249b. The nitrogen (N)-containing gas functions as a nitriding agent (nitriding gas). The N-containing gas functions as an N source. For example, ammonia (NH 2+) as a nitriding hydrogen-based gas can be used as the N-containing gas. 3 )gas.

[0053] The inert gas is supplied from the gas supply pipes 232c to 232e to the processing chamber 201 through the MFCs 241c to 241e, the valves 243c to 243e, and the nozzles 249c to 249e. In addition, the inert gas is supplied from the gas supply pipes 232g and 232h to the processing chamber 201 through the MFCs 241g, 241h, the valves 243g and 243h, the gas supply pipes 232a and 232b, and the nozzles 249a and 249b. The N supplied from the nozzles 249c to 249e to the processing chamber 201 2 The gas mainly functions as a dilution gas described later. In addition, N is supplied into the processing chamber 201 from the nozzles 249a and 249b. 2 The gas mainly functions as a purge gas and a carrier gas. As the inert gas, for example, nitrogen (N 2 )gas.

[0054] The raw material supply system is mainly composed of a gas supply pipe 232a, MFC241a, and a valve 243a. The oxidant supply system is mainly composed of a gas supply pipe 232b, MFC241b, and a valve 243b. The nitriding agent supply system is mainly composed of a gas supply pipe 232f, MFC241f, and a valve 243f. The inert gas supply system is mainly composed of gas supply pipes 232c to 232e, 232g, 232h, MFC241c to 241e, 241g, 241h, and valves 243c to 243e, 243g, and 243h.

[0055] The nozzle 249a for supplying raw materials is also referred to as a raw material supply unit or a raw material gas nozzle. When the oxidant is supplied by the nozzle 249b, the nozzle 249b is also referred to as an oxidant supply unit or an oxidant gas nozzle. When the nitriding agent is supplied by the nozzle 249b, the nozzle 249b is also referred to as a nitriding agent supply unit or a nitriding gas nozzle. The nozzles 249a and 249b are also collectively referred to as a processing gas supply unit or a processing gas nozzle. The nozzles 249c to 249e for supplying inert gas are also collectively referred to as an inert gas supply unit or an inert gas nozzle. In addition, as described later, the inert gas supply unit and the inert gas nozzle are also respectively referred to as a dilution gas supply unit and a dilution gas nozzle. The nozzles 249c to 249e are also referred to as a first supply unit to a third supply unit or a first nozzle to a third nozzle, respectively. The inert gas supply unit is a supply unit different from the raw material supply unit, the oxidant supply unit, and the nitriding agent supply unit, and has a plurality of supply units referred to as the first supply unit to the third supply unit. When the inert gas is supplied from the nozzles 249 a and 249 b , it may be considered that the nozzles 249 a and 249 b are included in the inert gas supply unit.

[0056] The raw material supply system is configured to supply the raw material with a controlled flow rate from the nozzle 249a to a plurality of partitions (i.e., all the first to third partitions). The oxidant supply system is configured to supply the oxidant with a controlled flow rate from the nozzle 249b to a plurality of partitions (i.e., all the first to third partitions). The nitriding agent supply system is configured to supply the nitriding agent with a controlled flow rate from the nozzle 249b to a plurality of partitions (i.e., all the first to third partitions). The inert gas supply system is configured to supply an inert gas with a controlled flow rate from each of the nozzles 249c to 249e to a plurality of partitions (i.e., each of the first to third partitions).

[0057] It should be noted that the inactive gas supply unit is constructed such that the nozzle 249c supplies the inactive gas individually after flow control to the first partition, and does not supply the inactive gas to other partitions (the second and third partitions); the nozzle 249d supplies the inactive gas individually after flow control to the second partition, and does not supply the inactive gas to other partitions (the first and third partitions); the nozzle 249e supplies the inactive gas individually after flow control to the third partition, and does not supply the inactive gas to other partitions (the first and second partitions).

[0058] On the side of the inner tube 204, an exhaust port (exhaust slit) 204c, which is formed as a slit-shaped through-hole, is elongated in the vertical direction. The exhaust port 204c is, for example, rectangular in the front view, and is provided from the lower part to the upper part of the side wall of the inner tube 204. The exhaust space 205, which is an annular space between the inner tube 204 and the outer tube 203 in the processing chamber 201 is connected via the exhaust port 204c. The exhaust port 204c is arranged on the extension line of the above-mentioned straight line L1 in the plan view. That is, the nozzle accommodating chamber 204a and the exhaust port 204c are opposite to each other with the center of the wafer 200 accommodated in the processing chamber 201 sandwiched therebetween. In addition, the gas ejection port 250a of the nozzle 249a and the exhaust port 204c are opposite to each other with the center of the wafer 200 accommodated in the processing chamber 201 sandwiched therebetween.

[0059] like Figure 1 As shown, an exhaust pipe 231 for exhausting the atmosphere in the processing chamber 201 via the exhaust space 205 is connected to the lower part of the outer tube 203. A vacuum pump 246 as a vacuum exhaust device is connected to the exhaust pipe 231 via a pressure sensor 245 as a pressure detector (pressure detection unit) for detecting the pressure in the exhaust space 205 (i.e., in the processing chamber 201) and an APC (Auto Pressure Controller, automatic pressure regulator) valve 244 as a pressure regulator (pressure regulating unit). The APC valve 244 is configured to be able to perform vacuum exhaust and stop vacuum exhaust in the processing chamber 201 by opening and closing the valve when the vacuum pump 246 is running, and further, when the vacuum pump 246 is running, the valve opening is adjusted based on the pressure information detected by the pressure sensor 245, so that the pressure in the processing chamber 201 can be adjusted. The exhaust system is mainly composed of the exhaust pipe 231, the APC valve 244, and the pressure sensor 245. It is also conceivable that the exhaust port 204c, the exhaust space 205, and the vacuum pump 246 are included in the exhaust system.

[0060] The lower end opening of the manifold 209 is hermetically sealed by the sealing cap 219 via the O-ring 220b. A rotating mechanism 267 for rotating the wafer box 217 is provided below the sealing cap 219. The rotating shaft 255 of the rotating mechanism 267 passes through the sealing cap 219 and is connected to the wafer box 217. The rotating mechanism 267 is configured to rotate the wafer 200 by rotating the wafer box 217. The sealing cap 219 is configured to be lifted and lowered in the vertical direction by means of a wafer box elevator 115 as a lifting mechanism vertically provided outside the reaction tube 210. The wafer box elevator 115 is configured as a conveying device (conveying mechanism) that moves the wafer 200 supported by the wafer box 217 into and out of the processing chamber 201 by lifting and lowering the sealing cap 219.

[0061] The wafer box 217 as a substrate support device is configured to be able to neatly arrange and support multiple stages of multiple wafers 200 (e.g., 25 to 200) in a horizontal posture and mutually aligned in the vertical direction, that is, arranged at intervals. The wafer box 217 is made of, for example, a heat-resistant material such as quartz or SiC. At the bottom of the wafer box 217, a heat insulation plate 218 made of, for example, a heat-resistant material such as quartz or SiC is supported in multiple stages.

[0062] A temperature sensor 263 as a temperature detector is provided between the outer tube 203 and the inner tube 204. The amount of current supplied to the heater 207 is adjusted based on the temperature information detected by the temperature sensor 263, so that the temperature in the processing chamber 201 reaches a desired temperature distribution. The temperature sensor 263 is provided along the inner wall of the outer tube 203.

[0063] like Figure 3 As shown, the controller 121 as a control unit (control unit) is configured as a computer having a CPU (Central Processing Unit) 121a, a RAM (Random Access Memory) 121b, a storage device 121c, and an I / O interface 121d. The RAM 121b, the storage device 121c, and the I / O interface 121d are configured to be able to exchange data with the CPU 121a via an internal bus 121e. The controller 121 is connected to an input / output device 122 configured as, for example, a touch panel.

[0064] The storage device 121c is composed of, for example, a flash memory, a HDD (Hard Disk Drive), etc. A control program for controlling the actions of the substrate processing device, and a process recipe that records the process and conditions of the substrate processing described later are readable and stored in the storage device 121c. The process recipe is combined in a manner so that the controller 121 executes each process in the substrate processing described later and obtains a predetermined result, and functions as a program. Hereinafter, such process recipes, control programs, etc. are also simply referred to as programs. In addition, the process recipe is also referred to as a recipe. When the term "program" is used in this specification, it includes the case of only a single process, the case of only a single control program, and the case of a combination of a process and a control program. RAM121b is configured as a storage area (working area) for temporarily storing programs, data, etc. read by CPU121a.

[0065] The I / O interface 121d is connected to the MFCs 241a to 241h, valves 243a to 243h, pressure sensor 245, APC valve 244, vacuum pump 246, heater 207, temperature sensor 263, rotation mechanism 267, wafer box elevator 115, and the like.

[0066] The CPU 121a is configured to read out a control program from the storage device 121c and execute it, and to read out a recipe from the storage device 121c according to input of an operation instruction from the input / output device 122. The CPU 121a is further configured to control, according to the contents of the read recipe, the flow rate adjustment operation of various gases by the MFCs 241a to 241h, the opening and closing operation of the valves 243a to 243h, the opening and closing operation of the APC valve 244 and the pressure adjustment operation by the APC valve 244 based on the pressure sensor 245, the start and stop of the vacuum pump 246, the temperature adjustment operation of the heater 207 based on the temperature sensor 263, the rotation and rotation speed adjustment operation of the wafer box 217 by the rotation mechanism 267, the lifting and lowering operation of the wafer box 217 by the wafer box elevator 115, and the like.

[0067] The controller 121 can be constructed by installing the above-mentioned program stored in the external storage device 123 into the computer. The external storage device 123, for example, includes a disk such as HDD, an optical disk such as CD, an optical disk such as MO, a semiconductor memory such as a USB memory card, etc. The storage device 121c and the external storage device 123 are configured as a recording medium that can be read by a computer. Hereinafter, these are also simply collectively referred to as recording media. When using the term "recording medium" in this specification, it includes the case of only a single storage device 121c, the case of only a single external storage device 123, or the case of both. It should be noted that providing a program to a computer does not require the use of an external storage device 123, and can also be carried out using communication methods such as the Internet and dedicated lines.

[0068] (2) Substrate processing steps

[0069] Using the substrate processing apparatus as a step in a semiconductor device manufacturing process, Figure 4 An example of a substrate processing flow, that is, an example of a film forming flow, for forming an oxynitride film on a wafer 200 as a substrate will be described. In the following description, the operations of the various components constituting the substrate processing apparatus are controlled by the controller 121 .

[0070] Figure 4 In the film forming process shown, a film containing Si, O and N as a nitride oxide film, i.e., a silicon nitride oxide film (SiON film) is formed on the wafer 200 by performing the following steps A, B and C non-simultaneously for a predetermined number of times (n times, where n is an integer greater than 1):

[0071] In step A, the nozzle 249a as the raw material supply unit supplies HCDS gas as the raw material to the wafer 200.

[0072] Step B: O as an oxidant is supplied to the wafer 200 from the nozzle 249b as an oxidant supply unit. 2 gas,

[0073] Step C: The nozzle 249b as the nitriding agent supply unit supplies NH4O as the nitriding agent to the wafer 200. 3 gas.

[0074] It should be noted that in Figure 4 In step A of the film forming process shown in FIG. 1 , N2 as an inert gas is supplied to the wafer 200 by an inert gas supply unit different from the raw material supply unit (that is, nozzles 249c to 249e different from the nozzle 249a). 2 gas, and by controlling the N 2 The concentration distribution of the HCDS gas as a raw material in the direction in which the wafers 200 are arranged is adjusted by adjusting the flow rate of the gas. N as the inert gas supplied from the nozzles 249c to 249e 2 The gas functions as a diluent gas for the raw material HCDS gas.

[0075] In this manual, for convenience, the following is sometimes displayed: Figure 4 The film forming process is shown in Figure 1. Figure 4 In the embodiment, the execution periods of step A to step C are respectively indicated as A to C. This also applies to the modified examples and other embodiments described later.

[0076]

[0077] In this specification, when the term "wafer" is used, it includes the case where it means "the wafer itself" and the case where it means "a stack of a wafer and a predetermined layer, film, etc. formed on its surface." In this specification, when the term "wafer surface" is used, it includes the case where it means "the surface of the wafer itself" and the case where it means "the surface of a predetermined layer, etc. formed on the wafer." In this specification, when it is stated that "a predetermined layer is formed on the wafer," it includes the case where it means directly forming a predetermined layer on the surface of the wafer itself and the case where it means forming a predetermined layer on a layer, etc. formed on the wafer. In this specification, when the term "substrate" is used, it has the same meaning as when the term "wafer" is used.

[0078] (Wafer loading and wafer cassette loading)

[0079] Multiple wafers 200 are loaded into the wafer box 217 (wafer loading). Then, as shown in FIG. Figure 1As shown, the wafer cassette 217 supporting the plurality of wafers 200 is lifted by the wafer cassette elevator 115 and carried into the processing chamber 201 (wafer cassette loading). In this state, the sealing cap 219 seals the lower end of the manifold 209 via the O-ring 220b.

[0080] Here, in this embodiment, if Figure 5 As shown, a large surface area wafer 200a as a first substrate and a small surface area wafer 200b as a second substrate are loaded as a plurality of wafers 200 into a wafer arrangement area of ​​a wafer box 217. The large surface area wafer 200a is a wafer having a larger surface area than the small surface area wafer 200b, for example, a device wafer (product wafer) having a pattern constituting a semiconductor device or the like formed on its surface. The small surface area wafer 200b is a wafer having a smaller surface area than the large surface area wafer 200a, for example, a dummy wafer or a test wafer having no pattern or the like formed on its surface (i.e., having a plain structure).

[0081] The wafer box 217 has slots capable of loading 120 wafers 200 in the entire wafer arrangement area. In this embodiment, 10 small surface area wafers 200b are loaded on the upper side of the first partition and 10 are loaded on the lower side of the third partition. In addition, 100 large surface area wafers 200a are loaded from the first partition to the third partition. Here, the area in the wafer arrangement area where the large surface area wafers 200a are loaded is called the first substrate area, and the area in the wafer arrangement area where the small surface area wafers 200b are loaded is called the second substrate area.

[0082] (Pressure regulation and temperature regulation)

[0083] Next, the vacuum pump 246 performs vacuum exhaust (decompression exhaust) in the processing chamber 201, so that the desired pressure (vacuum degree) is reached in the processing chamber 201 (i.e., the space where the wafer 200 is present). At this time, the pressure in the processing chamber 201 is measured by the pressure sensor 245, and the APC valve 244 is feedback-controlled based on the measured pressure information. In addition, the heater 207 heats the wafer 200 in the processing chamber 201 so that it reaches the desired temperature. At this time, the amount of power supplied to the heater 207 is feedback-controlled based on the temperature information detected by the temperature sensor 263, so that the desired temperature distribution is achieved in the processing chamber 201. In addition, the rotation of the wafer 200 is started by the rotation mechanism 267. The exhaust in the processing chamber 201, the heating and rotation of the wafer 200 are all continued until at least the processing of the wafer 200 is completed.

[0084] (Film Forming Step)

[0085] Then, the following steps A to C are sequentially performed in a state where a plurality of wafers 200 are arranged in the wafer arrangement area.

[0086] [Step A]

[0087] In this step, HCDS gas is supplied to the wafer 200 in the processing chamber 201 (HCDS gas supplying step).

[0088] Specifically, the valve 243a is opened to flow HCDS gas into the gas supply pipe 232a. The HCDS gas is regulated in flow rate by the MFC 241a, and is supplied to the processing chamber 201 from a plurality of gas ejection ports 250a provided on the side of the nozzle 249a, and is exhausted from the exhaust pipe 231 via the exhaust port 204c and the exhaust space 205. At this time, the HCDS gas is supplied to the wafer 200.

[0089] At this time, valves 243c-243e are opened, and N is supplied into the processing chamber 201 through nozzles 249c-249e. 2 At this time, by individually adjusting the N supplied by nozzles 249c to 249e, 2 The thickness of the SiON film formed on the large surface area wafer 200a is adjusted by adjusting the flow rate of the gas. The details of the flow rate adjustment and its effects will be described later.

[0090] In the HCDS gas supply step, valves 243g and 243h may be opened to supply N into the processing chamber 201 through nozzles 249a and 249b. 2 Gas. N is supplied from nozzles 249b to 249e. 2 Gas can inhibit the intrusion of HCDS gas into the nozzles 249b~249e.

[0091] The following are examples of processing conditions in this step:

[0092] HCDS gas supply flow rate: 0.01 to 2 slm, preferably 0.1 to 1 slm,

[0093] N 2 Gas supply flow rate (Rt and Rb respectively): 0.5~10slm,

[0094] N 2 Gas supply flow rate (Rc): 0~0.1slm,

[0095] N 2 Gas supply flow rate (R1): 0~10slm,

[0096] N 2 Gas supply flow rate (R2): 0~0.1slm,

[0097] Each gas supply time: 1 to 120 seconds, preferably 1 to 60 seconds,

[0098] Processing temperature: 250-800°C, preferably 400-700°C,

[0099] Processing pressure: 1-2666Pa, preferably 67-1333Pa.

[0100] The numerical range of "250 to 800°C" described in this specification means that the range includes the lower limit and the upper limit. Therefore, for example, "250 to 800°C" means "250°C or more and 800°C or less". The same applies to other numerical ranges.

[0101] By supplying HCDS gas to the wafer 200 under the above conditions, a Si-containing layer containing Cl is formed as a first layer on the outermost surface of the wafer 200. The Si-containing layer containing Cl is formed by physical adsorption of HCDS on the outermost surface of the wafer 200, or by a substance (hereinafter referred to as Si) formed by partial decomposition of HCDS. x Cl y ) chemical adsorption, or Si accumulation due to thermal decomposition of HCDS. The Si-containing layer containing Cl may also be HCDS, Si x Cl y The adsorption layer (physical adsorption layer, chemical adsorption layer) of Cl may also be a Si layer (Si accumulation layer) containing Cl. In this specification, the Si-containing layer containing Cl may be simply referred to as the Si-containing layer.

[0102] After the first layer is formed, the valve 243a is closed to stop the supply of HCDS gas into the processing chamber 201. Then, the processing chamber 201 is evacuated to remove the residual gas in the processing chamber 201 (purge step). At this time, the valves 243c to 243e, 243g, and 243h are opened to supply N into the processing chamber 201 from the nozzles 249a to 249e. 2 Gas. 2 The gas acts as a purge gas.

[0103] As a raw material (raw material gas), monochlorosilane (SiH 3 Cl, referred to as: MCS) gas, dichlorosilane (SiH 2 Cl 2 , referred to as: DCS) gas, trichlorosilane (SiHCl 3 , referred to as: TCS) gas, tetrachlorosilane (SiCl 4 , referred to as: STC) gas, octachlorotrisilane (Si 3 Cl 8 , referred to as: OCTS) gas and other chlorosilane gases.

[0104] As inert gases, except N 2 In addition to the gas, an inert gas such as Ar gas, He gas, Ne gas, or Xe gas can be used. This also applies to each step described later.

[0105] [Step B]

[0106] After step A is completed, O is supplied to the wafer 200 in the processing chamber 201, that is, to the first layer formed on the wafer 200. 2 Gas (O 2 Gas supply step).

[0107] Specifically, valve 243b is opened to allow O to flow into gas supply pipe 232b. 2 Gas. 2 The gas is regulated in flow rate by MFC 241b and supplied to the processing chamber 201 from a plurality of gas outlets 250b provided on the side of the nozzle 249b, and is exhausted by the exhaust pipe 231 through the exhaust port 204c and the exhaust space 205. 2 gas.

[0108] At this time, as in step A, N is supplied into the processing chamber 201 from the nozzles 249c to 249e. 2 In step B, in order to suppress O 2 The purpose of the gas intrusion into the nozzles 249c to 249e is to supply N into the processing chamber 201 through the nozzles 249c to 249e. 2 Gas. It should be noted that, similarly to step A, by individually adjusting the N supplied from nozzles 249c to 249e, 2 The flow rate of the gas can also adjust the film thickness of the SiON film formed on the large surface area wafer 200 a .

[0109] O 2 In the gas supply step, similarly to step A, N2 may be supplied into the processing chamber 201 through the nozzles 249a and 249b. 2 gas.

[0110] The following are examples of processing conditions in this step:

[0111] O 2 Gas supply flow rate: 0.1~10slm,

[0112] N 2 Gas supply flow rate (Rt, Rc and Rb respectively): 0~0.1slm,

[0113] N 2 Gas supply flow rate (R2): 0~10slm,

[0114] N2 Gas supply flow rate (R1): 0~0.1slm,

[0115] Each gas supply time: 1 to 120 seconds, preferably 1 to 60 seconds,

[0116] Processing pressure: 1-4000Pa, preferably 1-3000Pa.

[0117] The other processing conditions are the same as those in step A.

[0118] By supplying O to the wafer 200 under the above conditions 2 Gas is used to oxidize (modify) at least a portion of the first layer formed on the wafer 200. As the first layer is modified, a layer containing Si and O, that is, a SiO layer, is formed as a second layer on the wafer 200. When the second layer is formed, impurities such as Cl contained in the first layer are oxidized (modified) by O 2 During the reforming reaction of the first layer by the gas, a gaseous substance containing at least Cl is formed and exhausted from the processing chamber 201. As a result, the second layer becomes a layer with less impurities such as Cl than the first layer.

[0119] After the second layer is formed, the valve 243b is closed to stop supplying O into the processing chamber 201. 2 Then, the gas remaining in the processing chamber 201 is exhausted from the processing chamber 201 through the same processing procedure as the purging step in step A (purging step).

[0120] As oxidants (oxidizing gases), in addition to O 2 In addition to gases, nitrous oxide (N 2 O) gas, nitric oxide (NO) gas, nitrogen dioxide (NO 2 ) gas, ozone (O 3 ) gas, water vapor (H 2 O gas), carbon monoxide (CO) gas, carbon dioxide (CO 2 ) gas and other O-containing gases.

[0121] [Step C]

[0122] After step B is completed, NH is supplied to the wafer 200 in the processing chamber 201, that is, to the second layer formed on the wafer 200. 3 Gas (NH 3 Gas supply step).

[0123] Specifically, the valve 243f is opened to allow NH to flow into the gas supply pipe 232f. 3 Gas. NH 3The gas is regulated in flow rate by MFC241f, flows into the nozzle 249b through the gas supply pipe 232b, is supplied to the processing chamber 201 through a plurality of gas ejection ports 250b provided on the side of the nozzle 249b, and is exhausted by the exhaust pipe 231 through the exhaust port 204c and the exhaust space 205. At this time, NH is supplied to the wafer 200. 3 gas.

[0124] At this time, as in steps A and B, N is supplied into the processing chamber 201 from the nozzles 249c to 249e. 2 In step C, as in step B, in order to suppress NH 3 The purpose of the gas intrusion into the nozzles 249c to 249e is to supply N into the processing chamber 201 through the nozzles 249c to 249e. 2 Gas. It should be noted that, similarly to step A, by individually adjusting the N supplied from nozzles 249c to 249e, 2 The flow rate of the gas can also adjust the film thickness of the SiON film formed on the large surface area wafer 200 a .

[0125] In NH 3 In the gas supply step, N2 may be supplied into the processing chamber 201 through the nozzles 249a and 249b in the same manner as in step A. 2 gas.

[0126] The following are examples of processing conditions in this step:

[0127] NH 3 Gas supply flow rate: 0.1~10slm,

[0128] N 2 Gas supply flow rate (Rt, Rc and Rb respectively): 0~0.1slm,

[0129] N 2 Gas supply flow rate (R2): 0~10slm,

[0130] N 2 Gas supply flow rate (R1): 0~0.1slm,

[0131] Each gas supply time: 1 to 120 seconds, preferably 1 to 60 seconds,

[0132] Processing pressure: 1-4000Pa, preferably 1-3000Pa.

[0133] The other processing conditions are the same as those in step A.

[0134] By supplying NH to the wafer 200 under the above conditions, 3Gas is used to nitride (modify) at least a portion of the second layer formed on the wafer 200. By modifying the second layer, a layer containing Si, O, and N, i.e., a SiON layer, is formed as a third layer on the wafer 200. When the third layer is formed, impurities such as Cl contained in the second layer are nitrided (modified) by NH 3 During the reforming reaction of the second layer by the gas, a gaseous substance containing at least Cl is formed and exhausted from the processing chamber 201. As a result, the third layer becomes a layer with less impurities such as Cl than the second layer.

[0135] After the third layer is formed, the valve 243f is closed to stop the supply of NH 3 Then, the gas remaining in the processing chamber 201 is exhausted from the processing chamber 201 through the same processing procedure as the purging step in step A (purging step).

[0136] As nitriding agent (nitriding gas), in addition to NH 3 In addition to gases, hydrazine (N 2 H 2 ) gas, hydrazine (N 2 H 4 ) Gas, N 3 H 8 Gas such as N-containing gas.

[0137] [Scheduled number of implementations]

[0138] By performing steps A to C non-simultaneously (i.e., asynchronously) as a cycle, and performing the cycle more than once (n times), a SiON film of a desired film thickness and a desired composition can be formed on the wafer 200. The above cycle is preferably repeated multiple times. That is, it is preferred that the thickness of the third layer formed in each cycle is smaller than the desired film thickness, and the above cycle is repeated multiple times until the film thickness of the SiON film formed by stacking the third layer reaches the desired film thickness.

[0139] (Post-purge ~ atmospheric pressure recovery)

[0140] After the film forming step is completed, N is supplied into the processing chamber 201 through the nozzles 249a to 249e. 2 The gas is exhausted through the exhaust port 204c and the exhaust space 205 by the exhaust pipe 231. 2 The gas functions as a purge gas. Thus, the processing chamber 201 is purged to remove the residual gas and reaction by-products in the processing chamber 201 (post-purge). Then, the atmosphere in the processing chamber 201 is replaced with an inert gas (inert gas replacement), and the pressure in the processing chamber 201 is restored to normal pressure (atmospheric pressure restoration).

[0141] (Cassette unloading and wafer release)

[0142] The sealing cap 219 is lowered by the wafer box elevator 115 to open the lower end of the manifold 209. Then, the processed wafer 200 is carried out from the lower end of the manifold 209 to the outside of the reaction tube 210 while being supported by the wafer box 217 (wafer box unloading). After the processed wafer 200 is carried out to the outside of the reaction tube 210, it is taken out from the wafer box 217 (wafer release).

[0143] (3)N 2 Gas flow control and effect

[0144] Next, the N 2 The specific content of gas flow control and its effects are explained.

[0145] The HCDS gas supplied to the surface of the wafer 200 in step A is consumed due to adsorption, decomposition, etc. when a Si-containing layer is formed on the surface. At this time, the larger the surface area of ​​the wafer 200 to which the HCDS gas is supplied, the more gas is consumed per unit time. That is, the HCDS gas supplied to the surface of the large surface area wafer 200a is consumed faster than the HCDS gas supplied to the surface of the small surface area wafer 200b.

[0146] Therefore, as in the present embodiment, by using a nozzle 249a in which gas ejection ports 250a are uniformly arranged in the entire wafer arrangement region, HCDS gas of the same concentration and flow rate (especially the flow rate supplied to each wafer 200 here) is supplied to each of the first substrate region where the large surface area wafers 200a are arranged and the second substrate region where the small surface area wafers 200b are arranged, in this case, the concentration of the HCDS gas in the second substrate region is higher than the concentration of the gas in the first substrate region by an amount caused by the low consumption rate. Furthermore, the high-concentration HCDS gas in the second substrate region bypasses the region in the first substrate region adjacent to the second substrate region (hereinafter also referred to as the adjacent substrate region), thereby increasing the concentration of the HCDS gas in the adjacent substrate region. As a result, the thickness of the Si-containing layer formed on the large surface area wafers 200a arranged in the adjacent substrate region becomes greater than the thickness of the Si-containing layer formed on the large surface area wafers 200a arranged outside the adjacent substrate region. That is, the thickness of the Si-containing layer formed on the surface thereof may vary among the plurality of large surface area wafers 200 a arranged in the first substrate region.

[0147] Here, in this embodiment, in step A, N as a dilution gas is supplied to the continuous first supply region in the substrate arrangement region. 2 gas or N2 as diluent gas is not used 2At the same time as the supply of the gas, the second supply area in the substrate arrangement area is supplied with N as the dilution gas supplied to the first supply area. 2 The flow rate of the gas (more specifically, the flow rate supplied per unit length in the arrangement direction of the wafers 200) is greater than the flow rate (more specifically, the flow rate supplied per unit length in the arrangement direction of the wafers 200), and N is supplied as a dilution gas. 2 Gas, the first supply area includes an area (first substrate area) in which at least a portion of a plurality of large surface area wafers 200a are arranged and does not include an area (second substrate area) in which small surface area wafers 200b are arranged, and the second supply area includes an area (second substrate area) in which small surface area wafers 200b are arranged as an area outside the first supply area.

[0148] Figure 5 In the example shown, the first and third sub-areas where the small surface area wafers 200b are arranged are used as the second supply area, and the second sub-area where only the large surface area wafers 200a are arranged is used as the first supply area. In addition, in step A, the N supplied by the nozzle 249c (Rt) as the first dilution gas nozzle, the nozzle 249e (Rb) as the third dilution gas nozzle, and the nozzle 249d (Rc) as the second dilution gas nozzle are separately performed. 2 The gas flow rate is controlled so that the N supplied by Rt and Rb 2 The gas flow rate per unit length in the arrangement direction of the wafers 200 (second supply region flow rate) is greater than the N supplied by Rc. 2 The flow rate of the gas per unit length in the arrangement direction of the wafers 200 (first supply region flow rate) is large.

[0149] For example, Figure 5 In the example shown, the lengths of the wafers 200 in the first to third sections in the arrangement direction are substantially the same. In this case, the MFCs 241c to 241e are controlled so that N is supplied from Rt and Rb to the processing chamber 201. 2 Gas flow rate (N per nozzle) 2 The total flow rate of the gas is greater than the N supplied from Rc to the processing chamber 201. 2 The gas flow rate is large. As a result, the N supplied from Rt and Rb can be 2 The flow rate of the gas per unit length in the arrangement direction of the wafers 200 is greater than that of the N supplied from Rc. 2 The flow rate of the gas per unit length in the arrangement direction of the wafers 200 is large.

[0150] In addition, if Figure 5As shown in the example shown in the figure, when the gas outlets 250c, 250e, and 250d of Rt, Rb, and Rc are arranged at substantially the same opening pitch in the arrangement direction of the wafer 200, the MFCs 241c to 241e are controlled respectively so that each opening of the gas outlets 250c and 250e supplies N in the processing chamber 201. 2 Gas flow rate (N per opening) 2 The gas flow rate is N supplied from each opening of the gas outlet 250d to the processing chamber 201. 2 The gas flow rate is large. As a result, the N supplied from Rt and Rb can be 2 The flow rate of the gas per unit length in the arrangement direction of the wafers 200 is greater than that of the N supplied from Rc. 2 The flow rate of the gas per unit length in the arrangement direction of the wafers 200 is large.

[0151] In addition, as in the present embodiment, when the wafers 200 are arranged at equal intervals in the entire wafer arrangement region, the MFCs 241c to 241e may be individually controlled so that the N supplied from Rt and Rb to each wafer 200 is 2 Gas flow rate (N supplied to each wafer) 2 The gas flow rate) is greater than the N supplied from Rc to each wafer 200. 2 Gas flow rate (N supplied to each wafer) 2 The gas flow rate is large.

[0152] In this way, the amount of N as the dilution gas is controlled according to the position where the small surface area wafer 200b is arranged as in the present embodiment. 2 The supply flow rate of the gas can suppress the increase in the HCDS gas concentration in the adjacent substrate region in the second supply region. In other words, the influence of the HCDS gas flowing from the second substrate region into the adjacent substrate region can be reduced.

[0153] It is desirable to control N supplied by Rt to Rb separately. 2 The gas flow rate is adjusted so that the thickness of the Si-containing layer formed on the large surface area wafers 200a arranged in the first supply region is close to, and preferably substantially the same as, the thickness of the Si-containing layer formed on the large surface area wafers 200a arranged in the second supply region.

[0154] More specifically, the N supplied from Rt to Rb is controlled 2 The gas flow rate is adjusted so that the concentration (partial pressure) of the HCDS gas in the second supply area (the first and third subareas) is close to, and preferably substantially equal to, the concentration (partial pressure) of the gas in the first supply area (the second subarea). 2Gas flow rate (N per nozzle) 2 In this example, the total flow rate of the gas is Rt: 1.0 slm, Rc: 0 slm, and Rb: 1.0 slm. 2 The gas flow rate is equal, but it can also be controlled so that the N supplied to different second supply areas is 2 The gas flow rates are different.

[0155] Thus, the thickness of the Si-containing layer formed on the large surface area wafers 200a arranged in the first supply region can be made close to, and more preferably substantially the same as, the thickness of the Si-containing layer formed on the large surface area wafers 200a arranged in the second supply region. In addition, the same is true for the SiON film formed in the above-mentioned substrate processing step. The thickness of the SiON film formed on the large surface area wafers 200a arranged in the first supply region can be made close to, and more preferably substantially the same as, the thickness of the SiON film formed on the large surface area wafers 200a arranged in the second supply region.

[0156] In this embodiment, N from Rc is used as a diluent gas. 2 The gas supply flow rate (first supply region flow rate) is set to 0 slm. That is, in this case, in step A, N as a dilution gas is not supplied to the first supply region. 2 On the other hand, the supply of gas is carried out locally only in the second supply area, and N as a dilution gas is supplied. 2 However, in order to prevent HCDS gas from invading Rc and fine-tune the concentration distribution of HCDS gas in the first supply area (second subarea), a small amount of N may be supplied from Rc. 2 For example, N from Rc 2 The supply flow rate of the gas (the first supply region flow rate) was set to 0.1 slm.

[0157] In addition, in this embodiment, only in step A, the N as the dilution gas supplied to the first to third sections is controlled according to the arrangement position of the small surface area wafers 200b. 2 However, in at least one of step B and step C, by similarly adjusting the N supplied to the first to third sub-areas, 2 The gas flow rate can be such that the O supplied to the plurality of large surface area wafers 200a is 2 Gas, NH 3 The concentration of the gas is nearly equal.

[0158] In addition, when using the above raw materials other than HCDS gas, when using O 2 When using oxidants other than gases, NH3 When using the above nitriding agents other than gas, N 2 When the above-mentioned inert gas other than the gas is used, the above-mentioned effects can be obtained in the same manner.

[0159] <Modification 1 of the first embodiment>

[0160] In the first embodiment, as described above, when N is not supplied from Rc, 2 In the case of using N2 as a dilution gas, the substrate processing apparatus may be configured without Rc. In this case, Rt and Rb are used to locally supply N2 as a dilution gas only to the second supply area (the first sub-area and the third sub-area). 2 Supply of Gas This modification is suitable for the case where small surface area wafers 200 b are loaded only on the upper end side and the lower end side of the wafer array region as in the first embodiment.

[0161] <Modification 2 of the first embodiment>

[0162] In the first embodiment, the N supplied from Rt to Rb is controlled separately. 2 The concentration of HCDS gas in the first supply region and the second supply region is adjusted by adjusting the flow rate of the gas. However, except for Rt to Rb (or Rt and Rb), the N supplied from at least one of R1 and R2 is 2 The gas is used as a diluent gas, and the concentration of the HCDS gas in the first supply region and the second supply region can be further adjusted. This modification is suitable for adjusting only the N supplied from Rt to Rb (or Rt and Rb). 2 The situation where it is difficult to adjust the concentration distribution of HCDS gas in the wafer arrangement area to the desired distribution due to the gas flow rate.

[0163] <Second embodiment>

[0164] In the first embodiment described above, the wafers 200 (the large surface area wafer 200a and the small surface area wafer 200b) are Figure 5 Here, the example of loading the wafers into the wafer box 217 and processing them is described. Figure 6 An example in which the wafers 200 are loaded and processed in the arrangement shown will be described as a second embodiment.

[0165] In this embodiment, 10 small surface area wafers 200b are loaded in the center of the second partition, and 10 are loaded in the lower side of the third partition. In addition, large surface area wafers 200a are loaded in the entire first partition and the areas of the second and third partitions where small surface area wafers 200b are not arranged, and a total of 100 wafers are loaded. That is, in this embodiment, the second and third partitions where small surface area wafers 200b are arranged are used as the second supply area, and the first partition where only large surface area wafers 200a are arranged is used as the first supply area.

[0166] In this embodiment, in step A, flow rate control is performed so that N supplied from nozzles 249d (Rc) and 249e (Rb) 2 The flow rate of the gas per unit length in the arrangement direction of the wafers 200 (the second supply region flow rate) is greater than the N supplied from the nozzle 249 c (Rt). 2 The flow rate of the gas per unit length in the arrangement direction of the wafers 200 (first supply region flow rate) is large.

[0167] More specifically, the N supplied from Rt to Rb is controlled 2 The gas flow rate is adjusted so that the concentration (partial pressure) of the HCDS gas in the second supply area (second and third subareas) is close to, and preferably substantially equal to, the concentration (partial pressure) of the gas in the first supply area (first subarea). 2 Gas flow rate (N per nozzle) 2 As an example of the total flow rate of the gas, Rt: 0 slm, Rc: 1.0 slm, and Rb: 1.0 slm. As in the case of the first embodiment, the N from Rt is not implemented. 2 Gas supply, a small amount of N can also be supplied from Rt 2 Gas. For example, N supplied from Rt 2 The supply flow rate of the gas (the first supply region flow rate) can be set to 0.1 slm.

[0168] In the present embodiment, there is an area above the first partition where the large surface area wafer 200a is not arranged. If the HCDS gas flows into such an area, the unconsumed HCDS gas may flow into the first partition, causing the concentration of the HCDS gas in the first partition to increase. Therefore, considering the flow of such HCDS gas, a small amount of N2O2 may be supplied to the first partition as a dilution gas. 2 Gas. For example, N supplied from Rt 2 The supply flow rate of the gas can be set to 0.2 slm.

[0169] According to this embodiment, even if Figure 6The arrangement of the wafers 200 shown can also achieve the same effects as those of the first embodiment.

[0170] <Third embodiment>

[0171] Next, for the example different from the first embodiment, Figure 7 An example in which the wafers 200 are loaded and processed in the arrangement shown will be described as a third embodiment.

[0172] In this embodiment, 10 small surface area wafers 200b are loaded in the center of the second partition. In addition, large surface area wafers 200a are loaded in the entire first and third partitions and the area where small surface area wafers 200b are not arranged in the second partition, for a total of 110 wafers.

[0173] That is, in this embodiment, the second partition where the small surface area wafers 200b are arranged is used as the second supply area, and the first partition and the third partition where only the large surface area wafers 200a are arranged are used as the first supply area. 2 The flow rate of the gas per unit length in the arrangement direction of the wafers 200 (the second supply region flow rate) is greater than the N supplied from the nozzles 249c (Rt) and 249e (Rb). 2 The flow rate of the gas per unit length in the arrangement direction of the wafers 200 (first supply region flow rate) is large.

[0174] For example, control the N supplied from Rt to Rb respectively. 2 The gas flow rate is adjusted so that the concentration (partial pressure) of the HCDS gas in the second supply area (second sub-area) is close to, and preferably substantially equal to, the concentration (partial pressure) of the gas in the first supply area (first sub-area and third sub-area). 2 Gas flow rate (N per nozzle) 2 As an example of the total flow rate of the gas, Rt: 0 slm, Rc: 1.0 slm, and Rb: 0 slm. In addition, as in the case of the first embodiment, the N of Rt and Rb is not implemented. 2 Gas supply can also be supplied from Rt and Rb with a small amount of N 2 Gas. For example, N supplied from Rt and Rb 2 The supply flow rate of the gas (the first supply region flow rate) can be set to 0.1 slm.

[0175] In the present embodiment, there are areas above the first partition and below the third partition where the large surface area wafer 200a is not arranged. If the HCDS gas flows into such areas, unconsumed HCDS gas may flow into the first partition and the third partition, causing the concentration of the HCDS gas in the first partition and the third partition to increase. Therefore, considering such flow of HCDS gas, a small amount of N2O2 as a dilution gas may be supplied to the first partition and the third partition. 2 Gas. For example, N supplied from Rt and Rb 2 The supply flow rate of each gas can be set to 0.2 slm.

[0176] According to this embodiment, even if Figure 7 The arrangement of the wafers 200 shown can also achieve the same effects as those of the first embodiment.

[0177] <Fourth embodiment>

[0178] Next, for the example different from the first embodiment, Figure 8 An example in which the wafers 200 are loaded and processed in the arrangement shown will be described as a fourth embodiment.

[0179] In this embodiment, if Figure 8 As shown, the wafer arrangement area is divided into the first to fourth partitions from the upper side to the lower side. Moreover, 10 small surface area wafers 200b are loaded in the first partition, the second partition, and the fourth partition respectively. In addition, the large surface area wafers 200a are loaded in the entire third partition and the areas in the first partition, the second partition, and the fourth partition where the small surface area wafers 200b are not arranged, respectively, and a total of 90 wafers are loaded. That is, in this embodiment, the first partition, the second partition, and the fourth partition where the small surface area wafers 200b are arranged are used as the second supply area, and the third partition where only the large surface area wafers 200a are arranged is used as the first supply area.

[0180] In addition, the substrate processing device used in this embodiment is as follows Fig.10 As shown, nozzles 249f to 249i are provided instead of the nozzles 249c to 249e of the substrate processing apparatus used in the first to third embodiments. Gas ejection ports 250f to 250i serving as sixth to ninth gas supply ports are provided on the side surfaces of the nozzles 249f to 249i, respectively.

[0181] The gas outlets 250f of the nozzle 249f are provided in a plurality only in a portion of the nozzle 249f to correspond to the first partition in the wafer arrangement region. The nozzle 249f (i.e., Rt′) is configured to supply gas to the first partition and not to supply gas to other partitions (i.e., the second to fourth partitions).

[0182] The gas ejection ports 250g of the nozzle 249g are provided in a plurality only in a portion of the nozzle 249g to correspond to the second partition in the wafer arrangement region. The nozzle 249g (i.e., Rc′) is configured to supply gas to the second partition and not to supply gas to other partitions (i.e., the first, third, and fourth partitions).

[0183] The gas outlets 250h of the nozzle 249h are provided in a plurality only in a portion of the nozzle 249h to correspond to the third partition in the wafer arrangement area. The nozzle 249h (i.e., Rc″) is configured to be able to supply gas to the third partition and not to supply gas to other partitions (i.e., the first, second, and fourth partitions).

[0184] The gas outlets 250i of the nozzle 249i are provided in a plurality only in a part of the nozzle 249i to correspond to the fourth partition in the wafer arrangement area. The nozzle 249i (i.e., Rb′) is configured to supply gas to the fourth partition and not to supply gas to other partitions (i.e., the first to third partitions).

[0185] It should be noted that, similar to the gas ejection ports 250c to 250e, the gas ejection ports 250f to 250i are opened toward the center of the processing chamber 201 and are configured to supply gas toward the center of the wafer 200. In addition, they have the same opening area and are arranged at the same opening pitch.

[0186] Furthermore, in step A, flow control is performed so that N supplied from Rt′, Rc′, and Rb′ 2 The flow rate of the gas per unit length in the arrangement direction of the wafers 200 (the flow rate in the second supply region) is greater than the N supplied from Rc″. 2 The flow rate of the gas per unit length in the arrangement direction of the wafers 200 (first supply region flow rate) is large.

[0187] Furthermore, N supplied from Rt′, Rc′, Rc″, and Rb′ is controlled respectively. 2 The gas flow rate is adjusted so that the concentration (partial pressure) of the HCDS gas in the second supply area (first, second, and fourth subareas) is close to, and preferably substantially equal to, the concentration (partial pressure) of the gas in the first supply area (third subarea). 2 Gas flow rate (N per nozzle) 2 As an example of the total flow rate of the gas, Rt′: 0.8 slm, Rc′: 0.7 slm, Rc″: 0.1 slm, and Rb′: 0.8 slm. In addition, as in the case of the first embodiment, N from Rc″ is not not implemented. 2Gas supply can also be supplied from Rc″ with a small amount of N 2 Gas. For example, N supplied from Rc″ 2 The supply flow rate of the gas (the first supply region flow rate) can be set to 0.1 slm.

[0188] According to this embodiment, even if Figure 8 The arrangement of the wafers 200 shown can also obtain the same effects as those of the first embodiment.

[0189] <Other embodiments>

[0190] The embodiments of the present disclosure have been specifically described above, but the present disclosure is not limited to the above embodiments, and various modifications can be made without departing from the spirit and scope of the present disclosure.

[0191] For example, as a reactant, O 2 Gas, O 3 Gases containing O, H 2 Gas such as H-containing gas, etc., forms a silicon oxide film (SiO film) on the substrate according to the film formation process shown below. In this case, the same effect as the above embodiment can be obtained. The processing process and processing conditions when supplying these reactants can be the same as the processing process and processing conditions when supplying the reactants in the above embodiment.

[0192]

[0193]

[0194] In addition, for example, NH 3 Gases such as N-containing gas, propylene (C 3 H 6 ) gas and other carbon (C) gas, triethylamine ((C 2 H 5 ) 3 N, abbreviated as TEA) gas or other N and C-containing gas is used to form a SiON film, a silicon oxycarbide film (SiOC film), a silicon oxycarbonitride film (SiOCN film), etc. on a substrate according to the film forming process shown below. In this case, the same effect as in the above embodiment can be obtained. The processing process and processing conditions when supplying these reactants can be, for example, the same as the processing process and processing conditions when supplying the reactants in the above embodiment.

[0195]

[0196]

[0197]

[0198]

[0199]

[0200] In addition, for example, titanium tetrachloride (TiCl 4 ) gas, trimethylaluminum (Al(CH 3 ) 3 , referred to as TMA) gas, etc., and form a titanium oxynitride film (TiON film), an aluminum oxynitride film (AlON film), etc. on the substrate according to the film formation process shown below. In this case, the same effect as the above-mentioned embodiment can be obtained. The processing process and processing conditions when supplying these raw materials and reactants can be the same as the processing process and processing conditions when supplying raw materials and reactants in the above-mentioned embodiment.

[0201]

[0202]

[0203]

[0204]

[0205] In the above embodiment, the wafer arrangement area is divided into 3 or 4 partitions, and 3 or 4 nozzles having gas ejection ports corresponding to the respective partitions are used to supply dilution gas to each partition individually. However, the present disclosure is not limited to the above embodiment, and for example, the wafer arrangement area may be divided into 5 or more partitions, and 5 or more nozzles having gas ejection ports corresponding to the respective partitions may be used to supply dilution gas to each partition individually.

[0206] In addition, in the above embodiment, the wafer arrangement area is divided into a plurality of partitions so that the lengths in the arrangement direction of the wafers 200 are approximately equal, and the supply of the dilution gas to each partition is controlled separately. However, the present disclosure is not limited to the above embodiment, and the length of each partition (the number of wafers contained in each partition) can be set arbitrarily. For example, the partitions on the upper and lower sides of the wafer arrangement area can be set to be narrower than other partitions.

[0207] In addition, the above-mentioned various embodiments may be applied in combination as appropriate. The processing process and processing conditions in this case may be the same as the processing process and processing conditions in the above-mentioned embodiment, for example.

[0208] Example

[0209] Hereinafter, reference examples and embodiments are described. Figure 1The substrate processing apparatus shown in FIG. 1 supplies HCDS gas, O 2 Gas and H 2 The circulation of the gas is performed 100 times, thereby forming a SiO film on the wafer. In addition, the arrangement of the wafers 200 (large surface area wafers 200a and small surface area wafers 200b) loaded in the wafer box 217 is different from the arrangement in the first embodiment (ie, as shown in FIG. Figure 5 The arrangement shown is the same.

[0210] It should be noted that the substrate processing apparatus in the above embodiment is configured such that the HDCS gas is supplied through the gas supply pipe 232a, and the O gas is supplied through the gas supply pipe 232b. 2 Gas, NH 3 However, in the reference example and the present embodiment, the substrate processing apparatus used is configured such that the HDCS gas is supplied from the gas supply pipe 232b instead of the gas supply pipe 232a, and the O is supplied from the gas supply pipe 232b instead of the gas supply pipe 232a. 2 Gas, H is supplied from the gas supply pipe 232f 2 gas.

[0211] (Reference example)

[0212] In the reference example, in the step of supplying HCDS gas, the N 2 In addition, the step of supplying HCDS gas (step A') and the step of supplying O 2 Gas and H 2 The treatment conditions in the step of gas (step B') are as follows.

[0213] [Step A′]

[0214] HCDS gas supply flow rate: 0.1slm,

[0215] HCDS gas supply time: 4 seconds,

[0216] Processing pressure: 399Pa,

[0217] N 2 Gas supply flow rate (Rt, Rc and Rb respectively): 0slm.

[0218] [Step B′]

[0219] O 2 Gas supply flow rate: 3.5slm,

[0220] H 2 Gas supply flow rate: 2.0slm,

[0221] O2 Gas and H 2 Gas supply time: 6 seconds,

[0222] Processing pressure: 40Pa,

[0223] N 2 Gas supply flow rate (Rt, Rc, Rb respectively): 0slm.

[0224] (Example)

[0225] On the other hand, in the embodiment, in the step of supplying HCDS gas (step A′) and supplying O 2 Gas and H 2 In the step of generating a gas (step B′), similarly to the first embodiment, the N 2 Gas supply is not implemented by Rc N 2 Supply of Gas In addition, the processing conditions in step A' and step B' are as follows.

[0226] [Step A′]

[0227] HCDS gas supply flow rate: 0.1slm,

[0228] HCDS gas supply time: 4 seconds,

[0229] Processing pressure: 399Pa,

[0230] N 2 Gas supply flow rate (Rt, Rb respectively): 1.0slm,

[0231] N 2 Gas supply flow rate (Rc): 0slm.

[0232] [Step B′]

[0233] O 2 Gas supply flow rate: 3.5slm,

[0234] H 2 Gas supply flow rate: 2.0slm,

[0235] O 2 Gas and H 2 Gas supply time: 6 seconds,

[0236] Processing pressure: 40Pa,

[0237] N 2 Gas supply flow rate (Rt, Rc, Rb respectively): 0slm.

[0238] Fig.11The figures show the measurement results of the relationship between the position of the large surface area wafer 200a in the wafer arrangement region (the slot number in the wafer box 217) and the film thickness of the SiO film formed on the large surface area wafer 200a arranged at each position in the reference example and the embodiment. Fig.11 The horizontal axis represents the thickness of the SiO film formed on the wafer. The vertical axis represents the position of the large surface area wafer 200a in the wafer arrangement region. In addition, "120" on the vertical axis represents the upper end of the wafer arrangement region, and "0" represents the lower end of the wafer arrangement region. In addition, the points marked with "□" represent the measurement results of the reference example, and the points marked with "◆" represent the measurement results of the embodiment.

[0239] Depend on Fig.11 It can be seen that in the reference example, the thickness of the SiO film formed on the large surface area wafer 200a in the first and third partitions where the small surface area wafer 200b (i.e., including the second substrate region) is arranged is greater than the thickness of the SiO film formed on the large surface area wafer 200a in the second partition where the small surface area wafer 200b is not arranged (i.e., not including the second substrate region). That is, it can be seen that the thickness of the SiO film formed on the surface of the large surface area wafer 200a in the second partition is different from that of the large surface area wafer 200a in the first and third partitions.

[0240] On the other hand, by Fig.11 It can be seen that in the embodiment, the thickness of the SiO film formed on the large surface area wafer 200a in the first and third partitions is close to the thickness of the SiO film formed on the large surface area wafer 200a in the second partition. That is, it can be seen that the inter-substrate uniformity related to the thickness of the SiO film formed on the surface of the large surface area wafer 200a in the second partition and the large surface area wafer 200a in the first and third partitions is improved compared with the case of the reference example.

[0241] In such an embodiment, N as a dilution gas is separately supplied to the first sub-area and the third sub-area including the second substrate region. 2 The gas is supplied to the second partition that does not include the second substrate region, so that the concentration of the HCDS gas in the first partition and the third partition can be adjusted to be close to the concentration of the HCDS gas in the second partition.

Claims

1. A method for manufacturing a semiconductor device, comprising: (a) arranging a plurality of first substrates and a second substrate having a smaller surface area than the first substrate in a direction perpendicular to the surface direction and accommodating the plurality of first substrates in a processing chamber, and (b) supplying a processing gas to a substrate arrangement region where the plurality of first substrates and the second substrates are arranged, thereby forming a thin film on the plurality of first substrates; (b) comprising the following steps: (c) supplying a dilution gas to a first supply area in the substrate arrangement area or not supplying the dilution gas, the first supply area including an area where at least a portion of the plurality of first substrates are arranged and excluding an area where the second substrate is arranged, and supplying the dilution gas to a second supply area in the substrate arrangement area that is an area other than the first supply area and includes an area where the second substrate is arranged, at a flow rate greater than the dilution gas flow rate supplied to the first supply area, from a dilution gas nozzle different from a process gas nozzle that supplies the process gas, The dilution gas nozzle does not have a gas ejection port at a position corresponding to the first supply region, but has a gas ejection port at a position corresponding to the second supply region. 2 . The method for manufacturing a semiconductor device according to claim 1 , wherein in (b), the process gas is supplied to both the first supply region and the second supply region. 3 . 3 . The method for manufacturing a semiconductor device according to claim 1 , wherein in (c), supply of the dilution gas to the first supply region is not performed.

4. The method for manufacturing a semiconductor device according to claim 1, (c) at least one of the flow rate of the dilution gas supplied to the first supply region and the flow rate of the dilution gas supplied to the second supply region is adjusted so that the concentration of the process gas in the second supply region is equal to the concentration of the process gas in the first supply region.

5. The method for manufacturing a semiconductor device according to claim 1, (c) at least one of the flow rate of the dilution gas supplied to the first supply area and the flow rate of the dilution gas supplied to the second supply area is adjusted so that the thickness of the thin film formed on the plurality of first substrates arranged in the second supply area is the same as the thickness of the thin film formed on the plurality of first substrates arranged in the first supply area.

6. The method for manufacturing a semiconductor device according to claim 1, The substrate arrangement area includes a plurality of second supply areas, In (c), the dilution gas is supplied individually to the plurality of second supply regions by the plurality of dilution gas nozzles each having the gas ejection port at a position corresponding to any one of the plurality of second supply regions.

7. The method for manufacturing a semiconductor device according to claim 6, In (c), the flow rate of the dilution gas supplied to the plurality of second supply regions is adjusted individually.

8. The method for manufacturing a semiconductor device according to claim 1, The process gas nozzle is configured to supply the process gas to both the first supply region and the second supply region.

9. The method for manufacturing a semiconductor device according to claim 1, (b) comprising the step of performing the following (d) and (e) non-simultaneously as one cycle, and performing the cycle a predetermined number of times, (d) supplying a raw material gas to the substrate arrangement region, (e) supplying a reaction gas to the substrate arrangement region; (c) is carried out in (d).

10. The method for manufacturing a semiconductor device according to claim 1, wherein: The substrate arrangement area at least includes: a first partition on one end side of the substrate arrangement area, a second partition on the central side of the substrate arrangement area, and a third partition on the other end side of the substrate arrangement area. The second partition corresponds to the first supply area, and the first partition and the third partition correspond to the second supply area. In (c), the dilution gas is supplied to the first section from a first dilution gas nozzle as the dilution gas nozzle provided corresponding to the first section, and the dilution gas is supplied to the second section from a third dilution gas nozzle as the dilution gas nozzle provided corresponding to the third section.

11. The method for manufacturing a semiconductor device according to claim 10, In (c), the dilution gas is not supplied to the second section.

12. The method for manufacturing a semiconductor device according to claim 10, In (c), the dilution gas is supplied to the second section from a second dilution gas nozzle that is different from the dilution gas nozzle and is provided corresponding to the second section.

13. A substrate processing device comprising: A substrate support device supports a plurality of first substrates and a second substrate with a smaller surface area than the first substrate in a horizontal posture in multiple stages, a processing chamber configured to accommodate a substrate support device supporting the plurality of first substrates and the second substrate; a process gas nozzle disposed upright in the process chamber along a direction in which the plurality of first substrates and the second substrate are arranged and configured to supply a process gas into the process chamber, and a dilution gas nozzle disposed upright in the processing chamber along a direction in which the plurality of first substrates and the second substrate are arranged and configured to supply a dilution gas into the processing chamber, and different from the processing gas nozzle; The dilution gas nozzle does not have a gas nozzle at a position corresponding to a first supply area in a substrate arrangement area where the multiple first substrates and the second substrate are arranged, and has a gas nozzle at a position corresponding to a second supply area in the substrate arrangement area, the first supply area includes an area where the multiple first substrates are arranged and does not include an area where the second substrate is arranged, and the second supply area is an area outside the first supply area and includes an area where the second substrate is arranged.

14. The substrate processing apparatus according to claim 13, further comprising a second dilution gas nozzle, The second dilution gas nozzle is configured to supply the dilution gas to the first supply region and not to supply the dilution gas to the second supply region, and is different from the dilution gas nozzle.

15. The substrate processing apparatus according to claim 14, further comprising: a plurality of dilution gas supply systems configured to supply the dilution gas to the dilution gas nozzle and the second dilution gas nozzle, respectively; and A control unit configured to control the plurality of dilution gas supply systems so that the dilution gas is supplied from the dilution gas nozzle to the second supply region at a flow rate greater than a flow rate at which the dilution gas is supplied from the second dilution gas nozzle to the first supply region.

16. The substrate processing apparatus according to claim 13, The substrate arrangement area includes a plurality of second supply areas, The dilution gas nozzle is provided with a plurality of nozzles. The plurality of dilution gas nozzles include the gas ejection ports at positions corresponding to any of the plurality of second supply regions.

17. A computer-readable recording medium having a program recorded thereon for causing a substrate processing apparatus to execute the following process via a computer: (a) arranging a plurality of first substrates and a second substrate having a smaller surface area than the first substrate in a direction perpendicular to the surface direction and accommodating the plurality of first substrates in a processing chamber of the substrate processing apparatus, (b) forming a thin film on the plurality of first substrates by supplying a processing gas to a substrate arrangement region of the plurality of first substrates and the second substrate, (b) includes the following processes: The dilution gas is supplied to the first supply area in the substrate arrangement area by a dilution gas nozzle different from the process gas nozzle supplying the process gas, or the dilution gas is not supplied, wherein: The first supply region includes a region where at least a part of the plurality of first substrates are arranged and does not include a region where the second substrate is arranged, and the dilution gas is supplied at a flow rate greater than the flow rate of the dilution gas supplied to the first supply region to a second supply region including the region where the second substrate is arranged in the substrate arrangement region as a region other than the first supply region, The dilution gas nozzle does not have a gas ejection port at a position corresponding to the first supply region, but has a gas ejection port at a position corresponding to the second supply region.

Citation Information

Patent Citations

  • Semiconductor device manufacturing method, substrate processing apparatus, and recording medium

    WO2016110956A1

  • Substrate processing apparatus

    US20100218724A1

  • Film forming apparatus, film forming method, and non-transitory computer-readable storage medium

    US20150275366A1

  • Method of Manufacturing Semiconductor Device

    US20170067159A1