Window and method of manufacturing the same

Through multi-stage toughening process and ion exchange technology, the compression stress zone is formed in the window of the electronic device, which solves the problem of weakening the structure of the light and thin window, and achieves the balance of high strength and surface durability, and improves the impact resistance.

CN112010570BActive Publication Date: 2024-11-26SAMSUNG DISPLAY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202010459006.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-05-30
Filing Date
2020-05-27
Publication Date
2024-11-26
Estimated Expiration
2040-05-27

AI Technical Summary

Technical Problem

The existing electronic device windows have weakened structure during the thinning process, making it difficult to take into account high strength and surface durability, especially in the face of external impacts.

Method used

A multi-stage toughening process is used to manufacture windows. By forming a compressive stress zone on the surface and matrix area of ​​the window, the concentration distribution and compression stress patterns of Li+, Na+ and K+ ions are used to improve the impact resistance of the windows. The specific method includes using a variety of toughened molten salts for ion exchange in the substrate glass, forming compressive stress portions with different slopes and densities, and reinforcing the surface and internal structure of the window.

Benefits of technology

The compression stress value and impact resistance of the window are significantly improved, so that it exhibits excellent stability and durability during external impact while maintaining its thin and light structural characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112010570B_ABST
    Figure CN112010570B_ABST
Patent Text Reader

Abstract

The present application relates to a window, which comprises a substrate region and a compressive stress region disposed on the substrate region. The compressive stress region comprises Li + Ion, Na + Ions and K + The compressive stress region includes a first compressive stress portion, wherein from the surface of the window toward the substrate region, the K + The concentration of Na ions decreases. + ion concentration increases, and the Li + The concentration of Na ions increases. The second compressive stress portion is adjacent to the first compressive stress portion. In the second compressive stress portion, from the first compressive stress portion toward the substrate region, the Na + ion concentration decreases and the Li + The concentration of ions increases. The window thus has high surface compressive stress values ​​and impact resistance.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Korean Patent Application No. 10-2019-0063793, filed on May 30, 2019, which is hereby incorporated by reference in its entirety. Technical Field

[0003] The present disclosure herein relates to windows and methods of making the same, and more particularly, to windows used as cover glass for electronic devices and methods of making the same. Background Art

[0004] The electronic device may include a window, a housing, and various electronic components disposed therein. One such electronic component may be a display device for displaying an image. The various electronic components may also include a touch sensor and one or more components for generating and / or detecting light and / or sound.

[0005] The window protects the electronic components and provides the user with an active area where the display can be seen and where the user can register touch input. Thus, the user provides input to the electronic components or receives information generated by the electronic components through the window. In addition, the electronic components can be stably protected from external impacts due to the window.

[0006] In recent years, the trend toward slimmer electronic devices requires lighter and thinner windows, and in order to compensate for the resulting structural weakness, methods of toughening windows have been studied, by which excellent strength and surface durability are provided. Summary of the invention

[0007] The present disclosure provides windows having surfaces with increased compressive stress and impact strength.

[0008] Additionally, the present disclosure provides methods of making windows that include a toughening process for increasing the compressive stress and impact strength of the surface.

[0009] Embodiments of the present inventive concept provide a window comprising a substrate region and a compressive stress region disposed on the substrate region. The compressive stress region comprises Li + Ion, Na + Ions and K + ions, and further comprising a first compressive stress portion, wherein from the surface of the window toward the substrate region, the K + The concentration of ions decreases, and the Na + The concentration of Li ions and the +The concentration of Na ions increases. The second compressive stress portion is adjacent to the first compressive stress portion. In the second compressive stress portion, from the first compressive stress portion toward the substrate region, the Na + The concentration of ions decreases and the Li + The concentration of ions increases.

[0010] In an embodiment of the present inventive concept, the first compressive stress portion may have a first compressive stress pattern, wherein the compressive stress value decreases from the surface toward the base region at a first slope. The second compressive stress portion may have a second compressive stress pattern, wherein the compressive stress value decreases from the first compressive stress portion toward the base region at a second slope different from the first slope. Each of the first slope and the second slope may represent an amount of decrease in the compressive stress value as the depth within the window increases in a direction from the surface toward the base region.

[0011] In an embodiment of the present inventive concept, the first slope may be greater than the second slope.

[0012] In an embodiment of the present inventive concept, the density at the first compressive stress portion may be greater than the density at the second compressive stress portion.

[0013] In an embodiment of the present inventive concept, the second compressive stress portion may not include the K + ion.

[0014] In an embodiment of the present inventive concept, the compressive stress region may have a thickness of about 130 μm to about 150 μm.

[0015] In an embodiment of the present inventive concept, the first compressive stress portion may have a thickness of about 5 μm to about 15 μm.

[0016] In an embodiment of the present inventive concept, the compressive stress value at the surface may be about 650 MPa or greater.

[0017] In an embodiment of the present inventive concept, the matrix region may include about 50 wt % to about 80 wt % of SiO 2 , about 10 wt % to about 30 wt % Al 2 O 3 and about 3 wt % to about 20 wt % Li 2 O.

[0018] In an embodiment of the present inventive concept, the window may include a flat portion and at least one curved portion adjacent to the flat portion.

[0019] In an embodiment of the present inventive concept, the window comprises a compressive stress region at its surface. The compressive stress region comprises a first compressive stress portion, wherein from the surface toward the center of the window, K + The concentration of ions decreases, and Na + Ion concentration and Li + The concentration of Na ions increases. The second compressive stress portion is adjacent to the first compressive stress portion. In the second compressive stress portion, from the first compressive stress portion toward the center, the Na + ion concentration decreases and the Li + The concentration of ions increases.

[0020] In an embodiment of the present inventive concept, the first compressive stress portion may have a first compressive stress pattern, wherein the compressive stress value decreases from the surface toward the center at a first slope. The second compressive stress portion may have a second compressive stress pattern, wherein the compressive stress value decreases from the first compressive stress portion toward the center at a second slope greater than the first slope. Each of the first slope and the second slope may represent an amount of decrease in the compressive stress value as the depth within the window increases from the surface toward the center.

[0021] In an embodiment of the present invention, a method for manufacturing a window includes providing a substrate glass and toughening the substrate glass. The toughening of the substrate glass includes performing a first toughening of the substrate glass in a first toughening molten salt, performing a second toughening of the substrate glass in a second toughening molten salt, and performing a third toughening of the substrate glass in a third toughening molten salt. The first toughening molten salt to the third toughening molten salt each contain KNO 3 and NaNO 3 , and the second toughening molten salt KNO 3 The weight percentage is greater than that of KNO in the first toughening molten salt and the third toughening molten salt. 3 weight percentage.

[0022] In an embodiment of the present invention, the KNO in the second toughening molten salt 3 and NaNO 3 The weight ratio of may be about 91:9 to about 90:10.

[0023] In an embodiment of the present invention, the KNO in the first toughening molten salt and the third toughening molten salt is 3 and NaNO 3 Each of the weight ratios of may be from about 40:60 to about 60:40.

[0024] In an embodiment of the present inventive concept, the matrix glass may include SiO 2 、Al 2 O 3 and Li 2 O.

[0025] In an embodiment of the present inventive concept, the matrix glass may include about 50 wt % to about 80 wt % of SiO 2 , about 10 wt % to about 30 wt % Al 2 O 3 and about 3 wt % to about 20 wt % Li 2 O.

[0026] In an embodiment of the present inventive concept, the matrix glass may further comprise Na 2 O.

[0027] In an embodiment of the present inventive concept, the toughening of the base glass may be performed at a temperature of about 350°C to about 450°C.

[0028] In an embodiment, the first toughening molten salt may further comprise H 2 O 3 Si or zeolite. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] A more complete appreciation of the present disclosure and its many attendant aspects will be readily obtained, while becoming better understood, by reference to the following detailed description when considered in conjunction with the accompanying drawings, in which:

[0030] Figure 1 is a perspective view showing an electronic device according to an embodiment of the inventive concept;

[0031] Figure 2 It is shown Figure 1 An exploded perspective view of the electronic device illustrated in FIG.

[0032] Figure 3 is a perspective view showing a window according to an embodiment of the present inventive concept;

[0033] Figure 4 is a cross-sectional view of a window showing an embodiment of the present inventive concept;

[0034] Figure 5A is a diagram schematically illustrating ion concentration distribution in a window according to an embodiment of the present inventive concept;

[0035] Figure 5B is a diagram schematically illustrating a compressive stress curve in a window of an embodiment of the present inventive concept;

[0036] FIG. 6A to FIG. 6CEach is a diagram schematically showing a compressive stress distribution in a window of an embodiment of the present inventive concept;

[0037] Figure 7 is a flow chart illustrating a method of manufacturing a window according to an embodiment of the present inventive concept;

[0038] Figure 8 is a flow chart illustrating a toughening process in a method of manufacturing a window according to an embodiment of the present inventive concept; and

[0039] Fig. 9 is a schematic diagram illustrating a toughening process in a method of manufacturing a window according to an embodiment of the present inventive concept. DETAILED DESCRIPTION

[0040] In describing the embodiments of the present disclosure illustrated in the drawings, specific terminology is employed for the purpose of clarity. However, the present disclosure is not intended to be limited to the specific terminology so selected, and it is to be understood that each specific element includes all technical equivalents that operate in a similar manner.

[0041] It will be understood that when an element or layer is referred to as being “on,” “connected to” or “coupled to” another element or layer, it can be directly on, directly connected to or directly coupled to another element or layer, or intervening elements or layers may be present.

[0042] The same reference numerals may refer to the same elements throughout the specification and the accompanying drawings. In the accompanying drawings, the thickness, ratio and size of the elements may be exaggerated for effective description of the technical contents.

[0043] It should be understood that although the term first, second, etc. can be used to describe various elements, components, regions, layers and / or parts in this article, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish an element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teaching of the present invention, the first element, component, region, layer or part discussed below can be referred to as the second element, component, region, layer or part. As used herein, the singular "a (a)", "an (an)" and "the (the)" are intended to also include plural forms, unless the context clearly indicates otherwise.

[0044] For ease of description, spatially relative terms such as "under," "lower," "below," "over," and "upper" may be used herein to describe the relationship of one element or feature to another element or feature, as illustrated in the accompanying drawings. It should be understood that the spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the accompanying drawings.

[0045] Hereinafter, a window according to an embodiment of the inventive concept and a method of manufacturing the window according to an embodiment of the inventive concept will be described herein with reference to the accompanying drawings.

[0046] Figure 1 is a perspective view showing an electronic device according to an embodiment of the inventive concept. Figure 1 , an electronic device including a window is shown. Figure 2 yes Figure 1 An exploded perspective view of the electronic device shown in FIG. Figure 3 is a perspective view of a window according to an embodiment of the present inventive concept. Figure 4 is a cross-sectional view of the window. Figure 5A shows the ion concentration distribution in the window, and Figure 5B The compressive stress curve in the window is shown.

[0047] The electronic device EA may be implemented as a smart phone, a smart watch, a personal computer, a tablet computer, a laptop / notebook / ultranotebook computer, a desktop computer monitor, a television, etc. The electronic device EA may include various embodiments, such as a display device, an element for generating sound / light, an element for sensing sound / light, and one or more other electronic elements.

[0048] The electronic device EA may display an image IM in a third direction DR3 on a display surface IS parallel to a plane defined by the first direction DR1 and the second direction DR2. The display surface IS on which the image IM is displayed may correspond to the front surface of the electronic device EA and the front surface FS of the window CW. In addition, the electronic device EA may have a three-dimensional shape having a predetermined thickness in a third direction DR3 perpendicular to the plane defined by the first direction DR1 and the second direction DR2.

[0049] Figure 1 The display surface IS in the electronic device EA shown in FIG. 4 may include a display area DA and a non-display area NDA adjacent to the display area DA. The non-display area NDA may at least partially surround the display area DA. The non-display area NDA is illustrated as completely surrounding the display area DA, but the inventive concept is not limited thereto. The display area DA is an area in which an image IM is provided, and thus may correspond to an active area AA of the display panel DP. The image IM may be a still image and / or a dynamic image. Figure 1 A clock window is shown in FIG. 4 as an example of an image IM.

[0050] In this embodiment, the terms front surface / top surface and rear surface / bottom surface are defined relative to the direction in which the image IM is displayed. The front surface and the rear surface may be opposite to each other relative to the third direction DR3, and the normal direction of each of the front surface and the rear surface may be parallel to the third direction DR3. The first direction DR1 to the third direction DR3 are relative concepts and can be converted into different directions.

[0051] The electronic device EA includes a window CW, a display panel DP and a housing HAU. Figure 1 and Figure 2 In the electronic device EA shown in FIG. 1 , the window CW and the housing HAU may be combined to constitute the exterior of the electronic device EA.

[0052] The front surface FS of the window CW defines the front surface of the electronic device EA, as described in detail. The front surface FS of the window CW may include a transmission area TA in which light may pass and a baffle area BZA in which light may be at least partially blocked.

[0053] The transmission area TA may be an optically transparent area. For example, the transmission area TA may be a area having a visible light transmittance of about 90% or more.

[0054] The baffle area BZA may have a lower light transmittance than the transmission area TA. The baffle area BZA may define the shape of the transmission area TA. The baffle area BZA may be adjacent to the transmission area TA and may at least partially surround the transmission area TA.

[0055] The baffle zone BZA may have a specific color, such as black. The baffle zone BZA may cover the surrounding zone NAA of the display panel DP to prevent the surrounding zone NAA from being viewed from the outside. This is illustrated by way of example in the drawings, however, according to an embodiment of the inventive concept, the baffle zone BZA may be omitted from the window CW.

[0056] The window CW may include a glass substrate. For example, the window CW may be a toughened glass substrate that has undergone a toughening process. The window CW may provide a transmission area TA by utilizing the light transmittance of the glass, and may stably protect the display panel DP from external impact by including a toughened surface.

[0057] The window CW can be manufactured according to the method described herein. The method of manufacturing a window according to an embodiment of the inventive concept may include multi-stage toughening for toughening the base glass, and a toughening molten salt may be provided in each stage of the multi-stage toughening. A detailed description of the method of manufacturing a window is provided below.

[0058] The display panel DP can be activated according to an electrical signal. In this embodiment, the display panel DP is activated to display an image IM on the display surface IS of the electronic device EA. The image IM can be viewed by the user through the transmission area TA, and the user can receive information from the image IM. However, this is illustrated by way of example, and the display panel DP can be activated to sense an external input applied to its front surface. The external input can include a user's touch, contact or proximity of an inanimate object, pressure, light or heat, and is not limited to any one specific embodiment.

[0059] The display panel DP may include an active area AA and a peripheral area NAA. The active area AA may be an area in which an image IM is provided. The transmissive area TA may overlap at least a portion of the active area AA.

[0060] The surrounding area NAA may be an area covered by the baffle area BZA. The surrounding area NAA may be adjacent to the active area AA. The surrounding area NAA may at least partially surround the active area AA. A driving circuit, a driving line, etc. for driving the active area AA may be provided in the surrounding area NAA.

[0061] The display panel DP may include a plurality of pixels PX. Each of the plurality of pixels PX displays a light spot in response to an electrical signal. The light displayed by the pixel PX realizes an image IM. The pixel PX may include a display element. For example, the display element may be an organic light emitting element, a quantum dot light emitting element, a liquid crystal display element, an electrophoretic element, an electrowetting element, etc.

[0062] The housing HAU may be disposed below the display panel DP. The housing HAU may include a relatively hard / rigid material. For example, the housing HAU may include a plurality of frames and / or plates made of glass, plastic, or a metal such as stainless steel or aluminum. The housing HAU defines a housing space for accommodating the display panel DP and other electronic components. The display panel DP may be protected from external impacts by the housing HAU.

[0063] Figure 3 is a perspective view showing a window CW-a according to an embodiment of the present inventive concept. Such a window CW-a is shown in Figure 3 In the embodiment of the present invention, the window CW-a may include a flat portion FA and a curved portion BA. As shown, the flat portion FA may be disposed between two curved portions BA, however, in some embodiments of the present invention, there may be only one curved portion BA, or there may be no flat portion when the entire front surface FS may be curved.

[0064] In an embodiment of the present inventive concept, the bending axis BX may extend in the second direction DR2 and may be provided on the rear surface RS side of the window CW-a. The flat portion FA may be parallel to a plane defined by the first direction DR1 and the second direction DR2. Each of the curved portions BA may be a curved surface portion adjacent to the flat portion FA, and each of the curved portions BA may have a curved shape. For example, referring to Figure 3 , the bent portion BA may be a portion adjacent to the opposite side of the flat portion FA and bent downward from the flat portion FA. However, the present inventive concept is not limited thereto, and the bent portion BA may be disposed adjacent to only one side of the flat portion FA, or may be disposed adjacent to all four sides of the flat portion FA when viewed on a plane.

[0065] Figure 4 is a cross-sectional view illustrating a window according to an embodiment of the present inventive concept. Figure 4 is along Figure 2 A cross-sectional view taken along line II' in the window CW shown in FIG. 1 is shown in FIG. 2. Hereinafter, a description of a cross section of the window CW will be given. Such a window may be Figure 2 The window shown is the same as that shown in FIG, but the description can also be applied to Figure 3 Window CW-a of the embodiment shown in FIG.

[0066] refer to Figure 4 The window CW includes a front surface FS and a rear surface RS, each of which is an external surface. The front surface FS of the window CW is exposed to the outside and defines the front surface of the electronic device EA. The rear surface RS of the window CW is opposite to the front surface FS in the third direction DR3.

[0067] The window CW may include one or more compressive stress regions CSL. Each of the compressive stress regions CSL may be formed adjacent to a surface of the window CW. The compressive stress region CSL may be formed to have a predetermined depth in a thickness direction of the window CW from the surface of the window CW. In this specification, the compressive stress region CSL may indicate a region from the front surface FS or the rear surface RS which is the surface of the window CW to a point where the compressive stress becomes zero. Reference Figure 4 , the window CW may include two compressive stress regions CSL, which are respectively disposed adjacent to the front surface FS and the rear surface RS and are formed to be symmetrical with respect to the center line MP of the window CW. However, the present invention is not limited thereto, and the compressive stress region CSL may be disposed only adjacent to the front surface FS of the window CW, or the compressive stress region CSL adjacent to the front surface FS and the rear surface RS may be provided asymmetrically with respect to the center line MP of the window CW.

[0068] In the window CW of the embodiment of the present inventive concept, a base region BSL may be provided between the compressive stress regions CSL. The base region BSL may be a region where ion exchange of a toughening molten salt does not occur during toughening of a base glass in manufacturing the window.

[0069] The compressive stress zone CSL may contain Li + Ion, Na + Ions and K + The compressive stress region CSL may include a first compressive stress portion CSP1 adjacent to the front surface FS or the back surface RS which is a "surface" and a second compressive stress portion CSP2 adjacent to the base region BSL. The second compressive stress portion CSP2 may be a portion disposed adjacent to the first compressive stress portion CSP1.

[0070] Figure 5A FIG. 1 shows a Li of a window CW according to an embodiment of the present inventive concept. + Ion, Na + Ions and K + The distribution of ion concentration. Figure 5A In , the abscissa represents the depth from the zero depth (the surface of the window CW) toward the center line MP, and the ordinate represents the relative ion concentration.

[0071] refer to Figure 5A The first compressive stress portion CSP1 may be where from the front surface FS and the rear surface RS toward the base area BSL, K + The concentration of ions decreases and Na + Ion concentration and Li + In the second compressive stress portion CSP2, in the direction toward the base region BSL, Na + The concentration of ions can be reduced and Li + The concentration of ions can be increased.

[0072] In the window CW, the first compressive stress portion CSP1 may include Li + Ion, Na + Ions and K + ions, and the second compressive stress portion CSP2 may include Li + Ions and Na + ions, but may not contain K + ions. On the other hand, Li + Ion concentration and Na + The concentration of ions can be maintained at a constant level.

[0073] The first compressive stress portion CSP1 may correspond to a second toughening step (S530; see Figure 8 ) and the third toughening step (S550; see Figure 8 ) formed. In addition, the second compressive stress portion CSP2 may correspond to the first toughening step (S510; see Figure 8 ) formed in the compressive stress zone.

[0074] The thickness t of the compressive stress zone CSL from the surface (front surface or back surface) DOC can be the total thickness t of the window CW CW The thickness t of the compressive stress zone CSL is DOC It is the thickness in the depth direction of the window CW from the front surface FS or the rear surface RS of the window CW to the point where the compressive stress value becomes zero.

[0075] In addition, the thickness t of the first compressive stress portion CSP1 is DOL-K It can be represented from the front surface FS or the rear surface RS of the window CW to where K + The thickness of the point where the concentration of ions becomes zero. For example, the first compressive stress portion CSP1 may be formed by K + Layer formed by ion exchange.

[0076] The thickness of the compressive stress zone CSL is t DOC It may be about 130 μm to about 150 μm. In addition, the thickness t of the first compressive stress portion CSP1 is DOL-K The window CW may be formed by including a window having a total thickness t CW The compressive stress zone CSL has an improved impact resistance due to at least about 10% of the thickness of the compressive stress zone CSL.

[0077] Thickness t of window CW CW It may be about 0.3 mm to about 1.0 mm. For example, the thickness t of the window CW of an embodiment of the present inventive concept may be about 0.3 mm to about 1.0 mm. CW The window CW may be about 0.7 mm to about 0.9 mm. The window CW may be used as the electronic device EA described in detail (see Figure 1 ) to make the electronic device EA (see Figure 1 ) thinner and lighter.

[0078] Chemical toughening can be performed to include SiO 2 、Al 2 O 3 and Li 2 O to provide the window CW. Therefore, the base region BSL may include SiO2 、Al 2 O 3 and Li 2 O. The body region BSL may include about 50 wt % to about 80 wt % of SiO 2 , about 10 wt % to about 30 wt % Al 2 O 3 and about 3 wt % to about 20 wt % Li 2 O.

[0079] Figure 5A The alkali metal ion (Li + Ion, Na + Ions and K + ions), but the alkali metal ion (Li ion) distribution from another surface to the center line MP can also be shown in the same way. + Ion, Na + Ions and K + ions) of the ion concentration distribution.

[0080] In the window CW of the embodiment, the density may be highest in the first compressive stress portion CSP1 and may become lower toward the center line MP. The density in the second compressive stress portion CSP2 may be lower than that in the first compressive stress portion CSP1 and higher than that in the base region BSL.

[0081] Figure 5B A compressive stress curve in a window CW according to an embodiment of the present inventive concept is exemplarily shown. Figure 5B It may be a graph showing a compressive stress curve of a window CW manufactured by a method of manufacturing a window to be described later. Figure 5B , the direction of the arrow representing the compressive stress corresponds to the direction in which the compressive stress increases. Figure 5B , a compressive stress curve from one surface to the center line MP is shown, but a compressive stress curve from another surface to the center line MP can also be shown similarly.

[0082] refer to Figure 5B , the window CW of the embodiment may have the highest compressive stress value on the front surface FS and the rear surface RS, and have a gradually decreasing compressive stress value toward the center line MP of the window CW. The compressive stress value may be greater than the thickness t of the compressive stress region CSL. DOC is negative. Negative compressive stress values ​​can indicate tensile forces.

[0083] The compressive stress curve in the compressive stress zone CSL may have at least one inflection point CS_T. Figure 5BIn the embodiment of the present invention, the inflection point CS_T may appear at a portion corresponding to a boundary between the first compressive stress portion CSP1 and the second compressive stress portion CSP2. The window CW may exhibit a compressive stress curve including at least one inflection point CS_T.

[0084] In the window CW of the embodiment of the present inventive concept, the first compressive stress portion CSP1 may contain a first compressive stress pattern PT1 having a first slope, and the second compressive stress portion CSP2 may contain a second compressive stress pattern PT2 having a second slope. The slopes of the compressive stress curves in the first compressive stress portion CSP1 and the second compressive stress portion CSP2 each correspond to a decrease in the compressive stress value as the depth within the window CW increases from the surface of the window CW toward the base area BSL.

[0085] The first slope of the first compressive stress pattern PT1 in the first compressive stress portion CSP1 may be a ratio of a decrease in the compressive stress value ΔCS1 to an increase in the depth Δt1 within the window CW. In addition, the second slope of the second compressive stress pattern PT2 in the second compressive stress portion CSP2 may be a ratio of a decrease in the compressive stress value ΔCS2 to an increase in the depth Δt2 within the window.

[0086] Δt1 is the thickness t from the surface to the first compressive stress portion CSP1 DOL-K The depth increase of the depth of the first compressive stress portion CSP1 corresponds to the difference between the compressive stress value K'_CS at the surface and the compressive stress value K'_CS1 at the inflection point CS_T. Here, Δt2 is the thickness t of the first compressive stress portion CSP1. DOL-K The depth increase amount is the depth of the end of the second compressive stress portion CSP2 opposite to the inflection point CS_T, and ΔCS2 corresponds to the compressive stress value K′_CS1 at the inflection point CS_T.

[0087] refer to Figure 5B , the change amount of the compressive stress value in the first compressive stress portion CSP1 may be greater than the change amount of the compressive stress value in the second compressive stress portion CSP2. For example, the first slope may be greater than the second slope. The inflection point CS_T appearing in the compressive stress curve may be a point where the first slope of the first compressive stress pattern PT1 changes to the second slope of the second compressive stress pattern PT2.

[0088] The compressive stress value at the surface of the window CW may be greater than or equal to about 650 MPa. By having a maximum surface compressive stress value of about 650 MPa or greater, the window CW may have excellent impact resistance.

[0089] FIG. 6A to FIG. 6C Embodiments of compressive stress curves in a window are each shown by way of example. FIG. 6A to FIG. 6CEach of the compressive stress curves shown in FIG. 1 may include three pattern portions, and Figure 5B The compressive stress curve shown in has two compressive stress patterns.

[0090] The first pattern portion (PT1_a, PT1_b, and PT1_c) corresponds to the second compressive stress portion CSP2 (see Figure 4 ) in the compressive stress curve. The second pattern portion (PT2_a, PT2_b and PT2_c) and the third pattern portion (PT3_a, PT3_b and PT3_c) correspond to the first compressive stress portion CSP1 (see Figure 4 ) in the compressive stress curve. The third pattern portions (PT3_a, PT3_b and PT3_c) correspond to the first compressive stress portions CSP1 (see Figure 4 ) in the compression stress curve from the surface of the window to the inflection point. The second pattern portions (PT2_a, PT2_b and PT2_c) correspond to the compression stress curves of the portions disposed between the first pattern portions (PT1_a, PT1_b and PT1_c) and the third pattern portions (PT3_a, PT3_b and PT3_c). For example, the second pattern portions (PT2_a, PT2_b and PT2_c) correspond to the compression stress curves of the portions disposed between the first pattern portions (PT1_a, PT1_b and PT1_c) and the third pattern portions (PT3_a, PT3_b and PT3_c). Figure 4 ) contains the compressive stress value K_CS to the thickness t DOL-K The compressive stress variation curve of the compressive stress value K'_CS1 at the depth.

[0091] FIG. 6A to FIG. 6C The compressive stress curve shown in can represent the compressive stress of the window manufactured by the method of manufacturing the window of the embodiment to be described later. For example, FIG. 6A to FIG. 6C The compressive stress curve shown in can be obtained by performing a three-stage toughening process performed sequentially. For example, the first pattern portion (PT1_a, PT1_b, and PT1_c) can be a compressive stress curve formed by the first toughening, and the second pattern portion (PT2_a, PT2_b, and PT2_c) and the third pattern portion (PT3_a, PT3_b, and PT3_c) can correspond to the compressive stress curves formed by performing the second toughening and the third toughening, respectively.

[0092] exist FIG. 6A to FIG. 6C, K'_CS is the final compressive stress value at the surface, and K_CS is the compressive stress value at the inflection point where the second pattern portion (PT2_a, PT2_b and PT2_c) changes into the third pattern portion (PT3_a, PT3_b and PT3_c), respectively, and K'_CS1 corresponds to the compressive stress value at the inflection point where the first pattern portion (PT1_a, PT1_b and PT1_c) changes into the second pattern portion (PT2_a, PT2_b and PT2_c), respectively.

[0093] FIG. 6A to FIG. 6C The compressive stress curves of the third pattern portions (PT3_a, PT3_b, and PT3_c) having shapes different from each other are shown. The window CW may have a compressive stress value that increases toward the surface in the third pattern portion PT3_a, such as Fig. 6A Shown in.

[0094] In addition, reference Figure 6B and Figure 6C , the compressive stress value in the third pattern portions (PT3_b and PT3_c) may decrease toward the surface. Figure 6B The case where the difference between the final compressive stress value K'_CS at the surface and the compressive stress value K_CS at the inflection point where the second pattern portion PT2_b changes into the third pattern portion PT3_b is not large is shown. Figure 6C A case where the final compressive stress value K'_CS at the surface is significantly smaller than the compressive stress value K_CS at the inflection point where the second pattern portion PT2_c changes into the third pattern portion PT3_c is shown.

[0095] Therefore, the window can behave like Figure 5B or Fig. 6A The compressive stress curve shown in FIG. 1 has a maximum compressive stress value at the surface, or may have a compressive stress curve as shown in FIG. Figure 6B or Figure 6C The compressive stress curve shown in FIG. 1 has a slightly smaller compressive stress value at the surface.

[0096] The window can have excellent surface strength by including a first compressive stress portion adjacent to the surface and having a relatively large slope, wherein the slope is defined as the amount of decrease in compressive stress value as the depth within the window increases from the surface toward the center of the window. The second compressive stress portion has a smaller slope of compressive stress value relative to the first compressive stress portion. In addition, the window can include a first compressive stress portion in the compressive stress region (wherein from the surface toward the center, K + The concentration of ions decreases, Na + Ion concentration and Li + ion concentration increases) and the second compressive stress portion (where toward the center, Na +The concentration of ions decreases and Li + ion concentration increases), thereby having excellent impact resistance with a large surface compressive stress value.

[0097] In the following, reference will be made to Figures 7 to 9 A method of manufacturing a window according to an embodiment of the present invention is described. In the description of the method of manufacturing a window according to an embodiment of the present invention, the description of certain elements has been omitted to provide a simplified disclosure. It should be assumed that those elements that are not described may be at least similar to corresponding elements described elsewhere in the present disclosure.

[0098] Figure 7 is a flow chart showing a method for manufacturing a window according to an embodiment of the inventive concept. The method for manufacturing a window may include providing a base glass (S100) and toughening the base glass (S500). In addition, the method for manufacturing a window may further include polishing the base glass (S300) after the base glass (S100) has been provided.

[0099] In the method for manufacturing a window according to an embodiment of the present invention, the provided base glass (S100) may be a base glass manufactured by a float process. In addition, the provided base glass may be manufactured by a down-draw process or a fusion process. However, the present invention is not limited thereto, and the provided base glass may be manufactured by various methods not specified herein.

[0100] Considering the purpose of use, the already provided base glass (S100) may be cut and provided before toughening (S500) of the base glass. For example, the cut base glass may be provided before polishing (S300) of the base glass, and the side surface, front surface, etc. of the cut base glass may be polished. However, the present invention is not limited thereto, and the provided base glass may have a size that does not match the size of the final product to which the provided base glass is applied, and then may be cut and processed to match the size of the final product after the process of manufacturing a window therefrom.

[0101] The base glass may be flat. Alternatively, the base glass may be curved. For example, the base glass cut and provided in consideration of the size of the final product may be curved convexly or concavely with respect to its middle portion. Alternatively, the base glass may include a curved portion in its outer portion. However, the present invention is not limited thereto, and the base glass may be provided in various shapes.

[0102] The base glass (S100) provided in this way may include SiO 2 、Al 2 O 3 and Li 2 O. For example, the matrix glass may contain about 50 wt % to about 80 wt % SiO2 , about 10 wt % to about 30 wt % Al 2 O 3 and about 3 wt % to about 20 wt % Li 2 O.

[0103] In an embodiment of the present inventive concept, the matrix glass may include SiO 2 、Al 2 O 3 , Li 2 O and Na 2 O. In addition to SiO 2 、Al 2 O 3 , Li 2 O and Na 2 In addition to O, the base glass may further contain P 2 O 5 , K 2 O, MgO and / or CaO.

[0104] Polishing of the base glass (S300) may be performed after providing the base glass (S100). The side surface of the base glass, which is a cut surface of the base glass cut in various ways, may be polished using an abrasive or the like. In addition, the front surface of the provided base glass may be processed using an abrasive or the like.

[0105] The toughening of the matrix glass (S500) may be chemical toughening of the matrix glass by providing a toughening molten salt to the matrix glass. For example, the toughening of the matrix glass (S500) may be toughening the surface of the matrix glass by an ion exchange method after immersing the matrix glass in the toughening molten salt. The toughening molten salt provided to the matrix glass may contain two or more types of alkali metal ions.

[0106] The toughening of the matrix glass can be achieved by exchanging the alkali metal ions with relatively small ionic radius on the surface of the matrix glass for alkali metal ions with larger ionic radius (S500). + Ions and Na + Ion exchange provides Na in the toughening molten salt + Ions and K + ions to achieve toughening of the surface. The window CW manufactured by toughening the base glass (S500) may include a compressive stress region CSL on its surface (see Figure 4 ). Compressive stress zone CSL (see Figure 4 ) may be formed on the front surface FS and / or the rear surface RS of the window CW.

[0107] In the method of manufacturing a window according to an embodiment of the inventive concept, toughening of the base glass ( S500 ) may include three-stage toughening. Figure 8 Flow chart showing toughening (S500) of substrate glass in a method for manufacturing a window according to an embodiment of the present invention. Toughening (S500) of substrate glass may include a first toughening (S510) in a first toughening molten salt, a second toughening (S530) in a second toughening molten salt, and a third toughening (S550) in a third toughening molten salt. The first toughening step to the third toughening step (S510, S530, and S550) in the method for manufacturing a window of the embodiment may be performed sequentially. The first toughening step to the third toughening step (S510, S530, and S550) may be performed by separate processes, respectively.

[0108] Each of the first to third toughening molten salts provided in the first to third toughening steps (S510, S530, and S550) may be a Li + Ion, Na + Ion, K + Ion, Rb + Ions and Cs + ions. For example, each of the toughening molten salts provided in the first to third toughening steps (S510, S530, and S550) may contain KNO in the form of a mixed salt. 3 and NaNO 3 of molten salt.

[0109] KNO in the toughening molten salt provided in the first toughening step to the third toughening step (S510, S530 and S550) 3 and NaNO 3 The weight percentage of KNO may be varied in stages. For example, the second toughening molten salt used in the second toughening step (S530) may contain KNO 3 and NaNO 3 The weight percentages of KNO and KNO contained in the first toughening molten salt used in the first toughening step (S510) may be different from each other. 3 and NaNO 3 In addition, the KNO contained in the second toughening molten salt used in the second toughening step (S530) 3 and NaNO 3 The weight percentages of KNO and KNO contained in the third toughening molten salt used in the third toughening step (S550) may be different from each other. 3 and NaNO 3 The weight percentage of KNO in the second toughening molten salt 3The weight percentage of KNO in the first toughening molten salt or the third toughening molten salt may be greater than 3 weight percentage.

[0110] For example, KNO in the second toughening molten salt 3 and NaNO 3 The weight ratio of KNO can be about 91:9 to about 90:10. 3 and NaNO 3 In the second toughening molten salt, a relatively large amount of KNO 3 .

[0111] The first toughening molten salt used in the first toughening step (S510) of the method for manufacturing a window may include KNO at a weight ratio of 50:50. 3 and NaNO 3 By comparison, the second toughening molten salt used in the second toughening step (S530) may include KNO at a weight ratio of 92:8. 3 and NaNO 3 In addition, the third toughening molten salt used in the third toughening step (S550) may include KNO at a weight ratio of 50:50. 3 and NaNO 3 .

[0112] In addition, in the method for manufacturing a window according to an embodiment of the inventive concept, the third toughening step (S550) can be performed for a shorter time than the first toughening step (S510) or the second toughening step (S530). For example, when the first toughening step (S510) and the second toughening step (S530) each last for about 120 minutes to about 240 minutes, the third toughening step (S550) can be performed for about 10 minutes to about 60 minutes.

[0113] In the method of manufacturing a window, the toughening of the base glass (S500) may be performed at a temperature of about 350° C. to about 450° C. For example, the toughening of the base glass (S500) may be performed at a temperature of about 380° C. to about 400° C. The processing temperature of the second toughening step (S530) may be lower than the processing temperature of the first toughening step (S510) or the third toughening step (S550).

[0114] The first toughening molten salt in the first toughening step may further contain additives. For example, in addition to KNO 3 and NaNO 3 In addition, the first toughening molten salt may further contain H 2 O 3 Si or zeolite.

[0115] Fig. 9The toughening of the base glass (S500) in the method of manufacturing the window is schematically shown, which provides a toughening molten salt to toughen the base glass. Fig. 9 The toughening processing unit HU in which the toughening step (S500) is performed is schematically shown. Fig. 9 The toughening processing unit HU in the embodiment is used to describe the toughening step (S500), and the configuration of the toughening processing unit HU is not limited to Fig. 9 The configuration shown in .

[0116] Fig. 9 The toughening processing unit HU shown in the figure may include a tank HT for containing a toughening molten salt ML in a molten form. The heating unit HP is arranged to at least partially surround the tank HT. The heating unit HP heats the toughening molten salt ML in the tank HT. The driving unit HD fixes the provided base glass BG and moves the base glass BG in the vertical direction so as to immerse the base glass BG in the toughening molten salt ML. The control unit HC controls the operation of the toughening processing unit HU. The control unit HC can control the temperature of the toughening molten salt ML contained in the tank HT. For example, the control unit HC can control the heating unit HP so that the toughening molten salt ML is heated to a predetermined temperature, and the temperature of the toughening molten salt ML is maintained at the temperature to which the toughening molten salt ML has been heated. For example, the heating unit HP can provide heat to heat the toughening molten salt ML, or can be used as an insulating unit for maintaining the temperature of the heated toughening molten salt ML. The base glass BG can be arranged to be completely immersed in the toughening molten salt ML.

[0117] Only two base glasses BG fixed to the drive unit HD and treated in the toughening molten salt ML are shown exemplarily in Fig. 9 The base glass BG treated in the toughening molten salt ML may be provided in the singular or may be provided in the plural.

[0118] refer to Fig. 9 , the toughening step (S500) can be performed in the toughening processing unit HU by immersing the base glass BG in the toughening molten salt ML. In the method for manufacturing a window according to an embodiment of the inventive concept, the first toughening step to the third toughening step (S510, S530 and S550) can be performed in separate toughening processing units HU, respectively. However, the present invention is not limited thereto, and the toughening stages using the same toughening molten salt can be performed in the same toughening processing unit HU.

[0119] Tables 1 and 2 below respectively show process conditions of methods of manufacturing windows according to comparative examples and embodiments of the present disclosure, and evaluation results of properties of windows of the comparative examples and embodiments manufactured thereby.

[0120] For the comparative examples and for the examples, the same base glass was toughened; for the comparative examples, the evaluation results of windows toughened by a two-stage toughening process are shown, and for the examples, the evaluation results of windows toughened by a three-stage toughening process are shown.

[0121] Toughening in the method of manufacturing the window was performed under the conditions shown in Table 1 below.

[0122] [Table 1]

[0123]

[0124]

[0125] Table 2 shows the evaluation results of the windows manufactured under the conditions of Examples and Comparative Examples.

[0126] [Table 2]

[0127]

[0128] The breakage threshold height shown in Table 2 is defined as a method of evaluating the surface strength of a window, and is a measured height at which the window is broken when a weight having a predetermined weight is dropped onto the ball after a ball is placed on the window to be evaluated. For example, it can be seen that as the breakage threshold height increases, the window has a higher impact strength.

[0129] Referring to the results of Table 2, compared with the compressive stress value and depth of the compressive stress zone of the window of the comparative example, the window of the embodiment has a similar compressive stress value and depth of the compressive stress zone, but shows an improved damage threshold height.

[0130] Therefore, the method of manufacturing a window according to an embodiment of the present invention may include an additional third toughening step to allow the window to have an ion concentration distribution and a compressive stress curve in the compressive stress zone that are different from the ion concentration distribution and the compressive stress curve of the window of the comparative example, so that even when the compressive stress value or the compressive stress zone at the surface is similar to the compressive stress value or the compressive stress zone of the window of the comparative example, the window of the embodiment can have improved impact resistance.

[0131] By having a high compressive stress value at the surface and by including a first compressive stress portion and a second compressive stress portion having ion concentration distributions different from each other, the window according to an embodiment of the inventive concept can have increased impact resistance. In addition, in the method of manufacturing the window, by including three-stage toughening and by increasing the second toughening step having K + The percentage of ionic salts, the window can have a high surface compressive stress value and excellent impact resistance.

[0132] In an embodiment of the present inventive concept, a window having improved surface strength characteristics may be provided by including a compressive stress portion having different concentration profiles of alkali metal ions.

[0133] In an embodiment of the present inventive concept, a method of manufacturing a window having excellent impact strength may be provided by including a toughening step having three or more stages.

[0134] Although embodiments of the present inventive concept have been described herein, it should be understood that those skilled in the art may make various changes and modifications within the spirit and scope of the present inventive concept.

Claims

1. Window, include: basal region; as well as A compressive stress region, the compressive stress region is disposed on the base region and comprises Li + Ion, Na + Ions and K + ion, The compressive stress region includes: The first compressive stress portion, wherein from the surface of the window toward the base region, the K + The concentration of Na ions decreases. + ion concentration increases, and the Li + Increased concentration of ions; and a second compressive stress portion adjacent to the first compressive stress portion, wherein in the second compressive stress portion, from the first compressive stress portion toward the base region, the Na + The concentration of ions decreases and the Li + The concentration of ions increases, and the second compressive stress portion does not contain K + ions, and The compressive stress region has a compressive stress curve, and the compressive stress curve includes: a first pattern portion corresponding to the second compressive stress portion; a second pattern portion adjacent to the first pattern portion; a third pattern portion adjacent to the surface of the window; and an inflection point separating the second pattern portion and the third pattern portion, The compressive stress curve has a maximum compressive stress value at the surface, and the compressive stress value at the surface is 650 MPa or greater.

2. The window according to claim 1, in: In the second pattern portion of the first compressive stress portion, the compressive stress value decreases from the surface toward the base region at a first slope, In the first pattern portion, the compressive stress value decreases from the first compressive stress portion toward the base region at a second slope different from the first slope, and Each of the first slope and the second slope is defined as an amount of decrease in the compressive stress value as the depth within the window increases in a direction from the surface toward the body region. The window of claim 2 , wherein the first slope is greater than the second slope.

4. The window of claim 1, wherein a density of the first compressive stress portion is greater than a density of the second compressive stress portion. The window of claim 1 , wherein the compressive stress region has a thickness of 130 μm to 150 μm. The window of claim 1 , wherein the first compressive stress portion has a thickness of 5 μm to 15 μm.

7. The window of claim 1, wherein the matrix region comprises 50 wt% to 80 wt% SiO 2 , 10wt% to 30wt% Al 2 O 3 and 3wt% to 20wt% Li 2 O.

8. The window of claim 1, wherein the window comprises a planar portion and at least one curved portion adjacent to the planar portion.

9. A method for manufacturing a window according to any one of claims 1 to 8, said method include: providing a substrate glass; as well as toughening the base glass, The toughening of the matrix glass comprises: Performing a first toughening of the base glass in a first toughening molten salt; performing a second toughening of the base glass in a second toughening molten salt; and performing a third toughening of the matrix glass in a third toughening molten salt, The first toughening molten salt to the third toughening molten salt each contain KNO 3 and NaNO 3 ,as well as The KNO in the second toughening molten salt 3 The weight percentage is greater than the KNO in each of the first toughening molten salt and the third toughening molten salt. 3 The weight percentage, The second toughening and the third toughening form the first compressive stress portion, and the first toughening forms the second compressive stress portion.

10. The method of claim 9, wherein the KNO in the second toughening molten salt 3 and the NaNO 3 The weight ratio is 91:9 to 90:

10.

11. The method of claim 9, wherein the KNO in the first toughening molten salt and the third toughening molten salt 3 and the NaNO 3 The weight ratio of each is 40:60 to 60:

40.

12. The method of claim 9, wherein the matrix glass comprises SiO 2 、Al 2 O 3 and Li 2 O.

13. The method of claim 12, wherein the matrix glass comprises 50 wt% to 80 wt% SiO 2 , 10wt% to 30wt% Al 2 O 3 and 3wt% to 20wt% Li 2 O.

14. The method of claim 12, wherein the matrix glass further comprises Na 2 O.

15. The method of claim 9, wherein the toughening of the base glass is performed at a temperature of 350°C to 450°C.

16. The method of claim 9, wherein the first toughening molten salt further comprises H 2 O 3 Si or zeolite.

Citation Information

Patent Citations

  • Display Apparatus

    KR1020190063793A

  • Method for achieving a stress profile in a glass

    CN105873871A

  • Tempered glass and preparation method thereof

    CN108046613A

  • Method of manufacturing chemically strengthened glass plate

    US20130219966A1

  • Glass substrate, fabricating method of the same, and display device having the same

    US20160326050A1