Method and device for generating control data for an apparatus for additive manufacturing

By using the optimized non-rotationally symmetric energy beam intensity distribution curve for thermal conductive welding in the additive manufacturing process, the problems of high energy consumption and serious material loss in the deep welding process are solved, the productivity and the stability of the welding depth are improved, and the High detail resolution and smooth surfaces.

CN112041766BActive Publication Date: 2024-10-15EOS GMBH ELECTRO OPTICAL SYST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980028552.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-04-27
Filing Date
2019-04-23
Publication Date
2024-10-15
Estimated Expiration
2039-04-23

AI Technical Summary

Technical Problem

In the existing additive manufacturing process, the deep welding process leads to high energy consumption, serious material loss, increased costs and frequent material defects, and has low productivity, making it difficult to achieve efficient detail resolution and stable welding depth.

Method used

By generating optimized control data, the non-rotationally symmetric intensity distribution curve of the energy beam is used for thermal welding, controlling the local target temperature distribution, avoiding deep welding processes, improving welding depth and detail accuracy, and reducing material loss.

Benefits of technology

It achieves maximum utilization of energy, reduces material loss and cost, improves productivity and stability of welding depth, and ensures smooth surface and high quality of components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112041766B_ABST
    Figure CN112041766B_ABST
Patent Text Reader

Abstract

A method for generating control data (BSD, PSD) of an apparatus (1) for additive manufacturing and a control data generating device (54, 54') are described, wherein a building material (13) is built up and selectively solidified. To this end, the building material (13) is irradiated with at least one energy beam (AL) on a building area (8), wherein an irradiation surface (22) of the energy beam (AL) moves on the building area (8) to melt the building material (13) in a target area in or around the irradiation surface (22). In order to generate the control data (BSD, PSD), a target area (Γ) of the building material (13) is determined. Z ) in order to cause the building material (13) to melt by heat conduction welding. On this basis, an optimized intensity distribution curve (IO) of the energy beam (AL) is determined, which is essentially rotationally non-symmetrical at the irradiation surface (22) on the building area (8). The building material (13) is irradiated with the energy beam (AL) having the determined optimized intensity distribution curve (IO). A method and a control device (50) for controlling an additive manufacturing device (1) and a corresponding additive manufacturing device (2) are also described.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for generating control data for an apparatus for additive manufacturing of a manufactured product in a manufacturing process in which a building material is built up and selectively solidified, wherein, for solidification on the building area, the building material is irradiated with at least one energy beam and the irradiation surface of the energy beam is simultaneously moved on the building area to melt the building material in a target area in or around the irradiation surface. The invention also relates to a method for controlling an apparatus for additive manufacturing of a manufactured product by using control data. The invention also relates to a corresponding control data generating mechanism for generating control data and a control mechanism having such a control data generating mechanism or a port to such a control data generating mechanism for receiving the control data. Background Art

[0002] Additive manufacturing processes are becoming increasingly important in the manufacture of prototypes and in mass production. In general, "additive manufacturing processes" can be understood as the construction of manufactured products (hereinafter also referred to as "components") by stacking materials ("building materials") based on digital 3D structural data. Construction here means (but not necessarily necessarily) layer by layer. A synonym for additive manufacturing is also often the term "3D printing", and the manufacture of models, patterns and prototypes using additive manufacturing processes is often called "rapid prototyping" and the manufacture of molds is also called "rapid tooling". As mentioned at the beginning of this article, the core point is the selective solidification of the building material, wherein in multiple manufacturing processes, solidification can be carried out by means of radiation energy, such as electromagnetic radiation, especially light and / or thermal radiation, but if necessary, it can also be carried out by means of particle radiation, such as electron radiation. Methods that work using irradiation include, for example, "selective laser sintering" or "selective laser melting". In this process, thin layers of the mostly powdered building material are repeatedly applied one on top of the other and in each layer are selectively solidified in a "welding process" by spatially limited irradiation of the locations that are to belong to the product to be produced after production, i.e. the powder particles of the building material are partially or completely melted by the energy introduced locally by radiation at this location. After cooling, the powder particles are connected to one another to form a solid.

[0003] In practical applications or in machines or devices known so far for additive manufacturing, an energy beam with a substantially rotationally symmetrical intensity distribution (also referred to as an intensity distribution curve) is usually used for selective solidification. This rotationally symmetrical intensity distribution usually corresponds to a (circularly symmetrical) Gaussian distribution curve. That is, the intensity is highest in the middle of the energy beam and weakens in all directions radially outward transversely to the direction of diffusion of the energy beam or the current optical path direction (hereinafter also referred to as "beam direction" or "beam axis") according to the Gaussian distribution curve. This distribution curve can be obtained from the energy beam source used so far, such as ordinary lasers, without other measures. However, the latest knowledge or research shows that the intensity distribution of the energy beam or the exact shape of the intensity distribution curve has no significant effect on the entire manufacturing process, especially for example on energy consumption and / or the quality of the manufactured product, such as its microstructure. A comparison between a laser beam with a Gaussian intensity curve and a laser beam with a non-rotationally symmetrical intensity distribution, i.e. an elliptical intensity distribution, is shown, for example, in Tien T. et al., “Modulating laser intensity profile ellipticity for microstructural control during metal additive manufacturing”, in Acta Materialia, 128 (2017), pp. 197-206.

[0004] Furthermore, currently in practice, so-called "deep welding processes" ("penetration welding methods") are mostly used during laser sintering of metals. A welding process is defined as a deep welding process when a vapor capillary, also called a "keyhole", is formed. The emitted energy beam, in particular a laser beam, generates a sea of ​​molten material or metal. If the sea level of the material reaches its boiling temperature, the vapor bubbles press the melt laterally and downwards and thus generate vapor capillaries. The diameter of the keyhole is smaller than the diameter of the energy beam or laser beam. Here, the vapor capillaries are also generated in dependence on the movement speed of the energy beam, which is usually 2 MW / cm for lasers. 2 Start at 1m / Min. The deeper the keyhole, the greater the force, at which point you want to be able to collapse more force and have absorbed more energy beam power, so that eventually an equilibrium occurs at a certain depth related to certain parameters.

[0005] The advantage of this deep welding process is the large depth effect. That is, a significantly greater penetration depth can be achieved, measured at the focal diameter, than without such evaporation. Below, welding processes without evaporation are also referred to as "conduction welding" (also called "conduction mode welding" or "conduction laser welding").

[0006] However, this deep welding process also has several disadvantages:

[0007] First, the energy beam provides a relatively high enthalpy of evaporation, which is, for example, an order of magnitude higher than the enthalpy of melting and is withdrawn from the production part of the process. Although the enthalpy of evaporation occurs again when the metal vapor condenses, it is only at a location relatively far from the geometry to be produced. Due to this spatial separation, the enthalpy of evaporation is not available to the workpiece. This energy consumption increases the costs of the energy beam.

[0008] Secondly, the evaporated substances are mostly lost, which in the case of expensive metal powders significantly increases the component costs and has an impact on the component price.

[0009] Third, the volume of the material increases by about 1000 times (under normal conditions) during evaporation. This leads to high pressure in the metal vapor in the shrinkage cavity, which in turn leads to high outflow velocities of the metal vapor in the shrinkage cavity (on the order of 0.3 Mach). The high-speed gas jet will carry away adjacent solid particles and / or droplets, which leave the molten pool at high speed and thus cause energy and material losses. These particles and / or droplets are mostly called "splash".

[0010] Fourthly, the metal gas which condenses again shortly after leaving the keyhole usually flows exactly opposite to the direction of incidence of the energy beam, so that the condensate can interact with the energy beam in an uncontrolled manner by absorption and scattering. In order to avoid process-related disturbances as much as possible, the flow direction of the metal gas can be turned as quickly and efficiently as possible. This can be achieved by a flowing curtain of protective gas tangential to the powder bed, but its speed must be high enough to sufficiently reduce undesirable effects. However, this will usually result in a flow speed so high that a large amount of powdered material can be carried away from the powder bed, just as strong winds can also carry away dust from the floor (wind erosion). With the help of a process gas circulation system, process by-products or impurities, such as metal condensate or raw material powder discharged from the process chamber, can usually be collected downstream of the process chamber in filters and, if necessary, separators in the exhaust gas system. This material is usually lost and must also be processed in a complicated and expensive manner.

[0011] The sum of the material losses caused by the various loss sources described above may be several times the weight of the component being constructed. Therefore, avoiding their use or significantly reducing their use will greatly reduce costs.

[0012] In practice, sometimes attempts are made to control the process by setting a variable focus. A variable diffuser is used here, which moves the focus of the laser beam downward so that the beam is projected on the processing plane at its waist with a larger diameter. However, as the laser power increases, this solution is more and more prone to intensity fluctuations, which occur by moving along the longitudinal direction of the laser beam. In addition, using this method, the focus diameter can only be selected to be so large that the required process detail resolution is still achieved, which is mainly determined by the focus diameter, layer thickness and powder particle size. If at this time, in order to increase productivity, an attempt is made to increase the exposure speed, that is, the feed speed of the laser beam on the surface, but the focus diameter is not increased at the same time, because this cannot be increased due to the required detail resolution, which leads to increased intensity. And the increased intensity exacerbates the undesirable adverse phenomena of the above-mentioned deep welding process. Then the keyhole becomes deeper and more unstable. The shrinking keyhole appears in the molten pool, which hardens uncontrollably and even causes material defects, such as porosity, in extreme cases. Finally, this method limits the energy that each laser beam can couple into the material. Since the number of energy beams used is also not arbitrary and can only be increased to a small extent, this method thus limits the overall system productivity and thus also the control variables for reducing production costs. Summary of the invention

[0013] The object of the present invention is to provide a method for generating control data or for additive manufacturing of a manufactured product and a suitable device therefor which solve the above-mentioned problems.

[0014] This object is achieved by a method for generating control data according to claim 1, a method for controlling an apparatus for additive manufacturing of a manufactured product according to claim 11, a control data generating mechanism according to claim 12, a control mechanism for an apparatus for additive manufacturing of a manufactured product according to claim 13, and an apparatus for additive manufacturing of a manufactured product according to claim 14.

[0015] In the method according to the invention, control data are generated for an apparatus for additive manufacturing of a manufactured product in a manufacturing process, as described at the beginning. In this manufacturing process, the building material is preferably built up layer by layer in the process chamber of the apparatus, preferably the powder is selectively solidified by means of energy irradiation, especially in the corresponding layers. For this purpose, the building material is irradiated with an energy beam on the building area as described. In this case, the irradiation surface of the energy beam moves on the building area. In this case, "movement" can be understood as a general deflection of the energy beam, for example by a galvanometer mirror, but can also be understood as a complete radiation output unit, for example in the form of a diode row, especially a laser diode row, or beam shaping by movement.

[0016] The energy introduced by means of the energy beam melts the building material in the irradiated surface and in the surrounding target region. In this context, the term "target region" is understood to mean, on the one hand, the irradiated surface, i.e., the region on the surface where the energy beam irradiates, but also the region of the depth into the material or layer, and optionally also the periphery of the irradiated surface where the energy beam acts, for example, by heat conduction in the building material. For the sake of completeness, it should also be mentioned that the energy beam can be both particle radiation and electromagnetic radiation, for example light radiation or preferably laser radiation.

[0017] The control data can therefore preferably be exposure control data, such as scanning data which define or predetermine the movement of the energy beam on the surface; control data for setting the energy level or laser intensity; control data on the "shape" of the beam or the beam distribution and / or the focus or the beam expansion perpendicular to the radiation direction. However, these controls can also include other control information, such as coating control data which predetermine the current layer thickness, information for controlling preheating or reheating by means of other energy introduction mechanisms, information for injecting inert gas, etc., as will be explained in detail below.

[0018] It should also be mentioned here that the control data can be used both for "simple" process control and for regulating the process, for example by having the control data predetermine theoretical data for further process regulation. In other words, the method according to the invention can also be used to derive variables required for a regulator, which, for example, receives actual data for feedback, which are determined by melt pool monitoring or time-resolved optical tomography.

[0019] According to the invention, in order to generate control data for at least one irradiation mode, optimization criteria and / or auxiliary conditions and / or boundary conditions are determined for a local target temperature distribution or a target temperature distribution curve in a target region of the building material, wherein the building material is melted in the target region as a heat conduction welding. In other words, the criteria and conditions for the target temperature distribution are determined in such a way that the target temperature defined thereby in the target region is within the process window of the above-mentioned heat conduction welding and a "turnover" or transition to a deep welding process or an uncertain or unstable welding method is avoided. Based on the optimization criteria and / or auxiliary and / or boundary conditions, at least one optimized intensity distribution curve or intensity distribution of the energy beam is determined, preferably within the scope of an optimization process to be described in more detail later. According to the invention, the optimized intensity distribution curve of the energy beam at the irradiation surface on the building region is essentially rotationally non-symmetrical with respect to a beam axis (or an imaginary rotation axis) extending coaxially with the energy beam. The expression "at the irradiation surface" can therefore be understood to refer to the intensity distribution curve in an imaginary plane perpendicular to the direction of incidence shortly before the irradiation surface, which in most cases does not correspond to the intensity distribution curve directly on the surface of the building area or in the working plane, because the energy beam usually impinges on the building area obliquely. However, this does not exclude that the corresponding oblique position is also taken into account when determining the optimized intensity distribution curve, because the position of the direction of incidence on the building area also determines the influence of the optimized intensity distribution curve on the local target temperature distribution.

[0020] Up to this point, the energy beam is generated as described above so that the energy beam is generally rotationally symmetric about a radiation axis coaxial with the radiation direction of the energy beam, i.e. has a Gaussian intensity distribution. The term "substantially non-rotationally symmetric" here refers to an energy beam whose intensity distribution is intentionally generated to a significant extent non-rotationally symmetric or is correspondingly changed by targeted modification of the beam (such an intensity distribution is also considered "non-rotationally symmetric" in the present invention). It should not be understood as having a common rotationally symmetric, for example Gaussian intensity distribution itself and having only undesirable deviations from the rotational symmetry, for example due to accidental deformations or other defects of the system for generating and / or moving the energy beam or within the common tolerance range. For example, if the intensity distribution of the output energy beam generated as desired is mathematically described as a function I(r, φ) of the position of the polar coordinates r and φ (in a plane perpendicular to the beam direction), then the intensity distribution can preferably be called or defined as "non-rotationally symmetric" when no origin can be found in the intensity distribution, which satisfies the following properties for any m and any r under the condition m≥2:

[0021]

[0022] Among them, ε≤0.01, preferably ε≤0.05, more preferably ε≤0.1, and further preferably ε≤0.2.

[0023] Preferably, the strength distribution is selected such that it is also non-uniform, ie, apart from the usual tolerances, does not have essentially the same strength over the entire cross-sectional area.

[0024] The control data generated in this way for the relevant irradiation mode are used to control the device for additive manufacturing in the relevant irradiation mode and, as described, optionally also for regulating the device, so that the irradiation of the building material with the energy beam is achieved essentially with a certain optimized intensity distribution curve. That is, for this purpose, the energy beam at the irradiation surface on the building area corresponds to the certain intensity distribution curve or, except for certain tolerances, at least comes as close as possible to the certain intensity distribution curve, so that the desired local target temperature distribution is also achieved (as will be described later while maintaining other process parameters of the irradiation process).

[0025] A preferred irradiation mode that can be used in the method according to the invention is the so-called "core mode", in which the component is cured on the inside. In addition, in many production methods there are other curing modes, such as contour mode, in which the (outer) contour of the component is cured, or modes for curing supporting structures that are not an actual component of the component, etc. However, this does not exclude that the method according to the invention can also be used in other modes if desired.

[0026] It should be emphasized here that "boundary conditions" are here and generally understood as conditions that can only be influenced by complex work or even cannot be influenced, and therefore must be used as given variables when determining the optimized strength distribution curve or in the optimization process. "Auxiliary conditions" mostly refer to conditions that are different from the actual main conditions, that is, the actual optimization criteria, but must be met in addition and at the same time can usually limit the set of parameter solutions that need to be mainly achieved to meet the optimization criteria. The optimization criterion is understood as a function or multiple functions that contain the parameters to be optimized as function parameters. This function forms the mathematical relationship that should be optimized in the optimization process, that is, an optimal parameter value or multiple optimal parameter values ​​should be found for it and the target variable or set value that needs to be achieved here.

[0027] By means of the method according to the invention, the manufacturing process can be controlled so that by achieving an approximately ideal surface temperature at the surface around the irradiation surface or in the target area, for example, a uniform temperature distribution can avoid the problems caused by the deep welding process described at the beginning of this article. Thus, on the one hand, the energy introduction can be maximized, and on the other hand, other process-related aspects can be considered, which are different from the conventional rotationally symmetrical Gaussian process that has been common so far. If a Gaussian laser beam with the maximum intensity in the middle and a bell-shaped and rotationally symmetrical decrease toward the edge is irradiated on the metal molten pool, this causes a maximum value of the temperature distribution somewhere in the middle area on the surface. Here, evaporation inevitably begins at a certain moment as the power gradually increases. By allowing heat to flow through the molten pool into the material, that is, into the depth of the current surface, the temperature below the molten pool surface is usually lower than the surface temperature at this time. In addition, the surface stress of the metal melt (like most fluids) is also particularly temperature-related. The locally varying surface stress causes the material to flow from an area with low surface stress to an area with higher surface stress. This effect is called thermocapillary convection (thermocapillare convection) (also known as the Marangoni effect). If, for example, the surface stress decreases with increasing temperature (where the temperature dependence of the surface stress is related to the material and the shielding gas used), the material flows from the hot area of ​​the liquid surface to the cold area. Therefore, in the case of the Gaussian intensity distribution curve described, a flow is formed from its center to its edge. The flow turns downward at the edge of the molten pool to the deeper area of ​​the molten pool, and is located in the middle again at the bottom of the molten pool, where it rises again from the center to the surface and starts the cycle again. The speed of this thermocapillary convection can reach up to 100m / s in the molten pool. By taking into account the time that the material is in the liquid phase, the simulation realizes that this annular flow circulates about twice before the metal hardens again in ordinary exposure parameters. According to the sign of the Marangoni number (i.e. the corresponding temperature / surface stress gradient), the heat energy is transported to the colder, outer or deeper area of ​​the molten pool together with the material. This flow is also the source of turbulence, which occurs in non-stationary hardening surfaces and / or even in droplets ejected from the molten pool.

[0028] Within the scope of the process according to the invention, i.e. in the optimization of the temperature profile in the target area, in particular on the building zone, by means of the optimized intensity profile, the influence of the temperature dependence can even be used in a targeted manner at the surface of the molten pool to control the convection in the molten pool by means of a suitable predetermined temperature profile or by means of the predetermined optimization criteria and / or auxiliary and / or boundary conditions required for this purpose. Thus, for example, a temperature profile can be set in a targeted manner, which diverts the thermocapillary convection relative to the above-mentioned common direction, thereby forcing the mass transport and heat transport into the depth by convection. Thus, the "effective penetration depth" or "molten pool depth" or "welding depth" can be increased, thereby allowing thicker layers to be melted and at the same time the "hardening width" ("molten pool width") can be reduced, which is beneficial to detail accuracy, wherein the "hardening width" is understood to be the maximum extension perpendicular to the direction of movement of the energy beam on the building zone. In addition, if desired, thermocapillary convection can be completely prevented or at least greatly reduced by homogenizing the surface temperature, thereby achieving a smoother component surface.

[0029] Which strategy is used specifically or how the corresponding optimization criteria and / or auxiliary and / or boundary conditions are defined for this purpose depends on the respective purpose of use, for example which irradiation mode is involved, which component is to be produced, which conditions and desired component properties are to be achieved, which materials are used, etc. In each case, the method according to the invention can be used to predetermine the desired state of the temperature profile to be provided at the surface of the melt pool, thereby optimizing the entire production process.

[0030] In the method according to the invention for controlling a production device for additive manufacturing of manufactured products, control data are first generated in the manner according to the invention and then the device is controlled using these control data. The control data can be generated in advance and transmitted to the device as a complete package or in the form of a "control protocol", which then executes the production process. However, it is also possible in principle to determine control data for subsequent process steps during an already running process, for example, during the curing of a layer, to determine control data for the next layer and use them when curing another layer.

[0031] The basis for the output of the control data is in particular data on which locations within the process space or the building zone the material should be solidified, i.e. which parts should later belong to the component or to a possible support structure, etc. and which areas should not belong. These data can be obtained, for example, from a 3D digital model of the object to be manufactured and / or the support structure. If this data and other required information are available, such as which materials are used, which solidification mechanisms are provided, in particular which energy beams or which parameter ranges can be set, etc., the desired optimized intensity distribution curve can be determined by means of pre-defined optimization criteria and / or auxiliary conditions and / or boundary conditions to define the local target temperature distribution, and the control data can therefore be determined accordingly.

[0032] The control data generating device for generating control data for an apparatus for additive manufacturing of a manufactured product according to the invention is configured to determine optimization criteria and / or auxiliary and / or boundary conditions for a local target temperature distribution of a building material in a target region to generate control data for at least one irradiation mode, wherein the building material is melted in the target region as heat conduction welding. The optimization criteria and / or auxiliary and / or boundary conditions are predefined, for example, via a user interface or by a higher-level control protocol or the like.

[0033] The control data generating device is further configured to determine at least one optimized intensity distribution curve of the energy beam based on the optimization criterion and / or the auxiliary conditions and / or the boundary conditions, wherein, as described, the optimized intensity distribution curve of the energy beam is substantially rotationally non-symmetrical at the irradiation surface on the building area. Control data are generated in this case so that when (if necessary later) the additive manufacturing device is operated in the irradiation mode, the building material is irradiated with the energy beam substantially having the determined intensity distribution curve, so that control data are created, by means of which the additive manufacturing device can be correspondingly operated by using the control data.

[0034] The control data generating device can be, for example, a part of the control device of such a production device for additive manufacturing of manufactured products. However, the control data generating device can also be implemented independently on another computer in order to subsequently transfer the data to the control device.

[0035] Therefore, the control mechanism of the device for additive manufacturing of such a manufacturing process according to the present invention has a control data generating mechanism according to the present invention or a port with such a control data generating mechanism to provide relevant control data or to receive control data by the control data generating mechanism, and the control mechanism is configured to control the mechanism for irradiating the building material with an energy beam by using the control data.

[0036] The device according to the invention for additively manufacturing a manufactured product in an additive manufacturing process has, in addition to conventional components, such as an input device for introducing building material in the form of building material layers in a process space and an irradiation device for selectively curing the building material by irradiation with the aid of an energy beam, at least one such control device.

[0037] It should be pointed out here that the device according to the invention can also have multiple irradiation means, which are then controlled in a correspondingly coordinated manner with the control data so as to achieve a local target temperature distribution. It should also be mentioned again that the intensity distribution curve of the optimized energy beam can also be formed by multiple superimposed energy beams, so that the superimposed sub-energy beams jointly have an optimized intensity distribution curve, which then optimally leads to the desired target temperature distribution or maintains auxiliary and / or boundary conditions for the local target temperature distribution and thus meets the optimization criteria as much as possible.

[0038] The control data generating device according to the invention can be implemented in the form of a computing unit with suitable software. The computing unit can, for example, have one or more cooperating microprocessors or the like for this purpose. The control data generating device can be implemented in particular in the form of a suitable software program component in the computing unit of the control device of the production device according to the invention. The advantage of basically implementing in software is that the computing units used so far, in particular the control devices of the production device for additive manufacturing, can be retrofitted in a simple manner by software or hardware upgrades, so that they work in the manner according to the invention. In this regard, the object is also achieved by a corresponding computer program product with a computer program, which can be downloaded directly into the storage device of the computing unit, in particular the control device, and the computer program has program segments so that all steps of the method according to the invention are executed when the program is executed in the computing unit or the control device. In addition to the computer program, such a computer program product may also include additional components, such as file compilations and / or additional components and hardware components, such as hardware keys (dongles, etc.) that use the software. For transport to a computing unit or a control device and / or for storage in a computing unit or a control device, a computer-readable medium can be used, such as a memory stick, a hard disk or other transportable or permanently installed data carrier, on which program segments of a computer program are stored that are readable and executable by a computing unit, in particular a control device.

[0039] Particularly advantageous further designs and improvements of the invention are given by the dependent claims and the following description, wherein an independent claim in one claim category may also be improved similarly to dependent claims and embodiments of another claim category and in particular individual features of different embodiments or variants may also be combined to form new embodiments or variants.

[0040] There are various approaches to generating an energy beam with a specific optimized intensity profile. For example, the desired beam shaping is already achieved during the generation of the energy beam.

[0041] Thus, for example, a laser can be constructed with a plurality of laser channels which can be cohesively combined so that the laser channels together act as individual cohesive laser sources and function as a laser source. This in turn provides the possibility of additionally dynamically modulating each laser channel in terms of phase and amplitude in order to achieve a desired variable beam shaping, in particular a desired intensity profile.

[0042] Furthermore, any energy beam generated by an energy beam source, ie initially rotationally symmetrical, can only be “shaped” or modified later in a beam shaping device in order to obtain a desired beam profile. Such a beam shaping device can also be realized in different ways.

[0043] Preferably, the beam shaping device can have at least one micro-optical element which can be actuated by the control device. Particularly preferred here are so-called diffractive optical elements (also known in English as “Diffractive Optical Element”, DOE).

[0044] The DOE can operate by reflection or transmission and the wavefront of the incident beam can be varied by locally modulating the phase and / or amplitude of the reflected or transmitted partial beams.

[0045] An active DOE can be understood as an assembly of multiple, in principle coherent, laser sources as described above, in which the phase and / or amplitude of each individual laser beam are related to one another but can be controlled relative to one another, thereby also making it possible to manipulate the intensity distribution generated by the superposition of individual laser beams in the far field.

[0046] DOE is particularly useful in beam shaping arrangements where it is necessary to modify an already generated incoming energy beam (afterwards).

[0047] Preferably, the beam shaping device comprises at least one beam splitter, which can also be designed as a DOE, for example, in order to split the "input energy beam" into at least two beams. The beam splitter can preferably include a thin-film polarizer. Such a thin-film polarizer generates two linearly polarized partial beams, for which there are different options for modifying the intensity distribution.

[0048] For this purpose, the beam shaping device may have, for example, at least one beam shaping element. Preferably, the beam shaping device has a plurality of such beam shaping elements, for example beam shaping elements assigned to different partial beams, in particular linearly polarized partial beams. However, this does not exclude that a plurality of beam shaping devices may also be provided for a partial beam.

[0049] Particularly preferably, at least one of the beam shaping elements, very particularly preferably all of the beam shaping elements, comprises or is an LCoS display (LCoS=Liquid Crystal on Silicon, also known as LCoS microdisplay). With such an LCoS display, it is relatively easy to shape a linearly polarized beam in a desired manner or to change its intensity distribution in a plane perpendicular to the beam axis. An LCoS display is another example of a passive DOE in the above context.

[0050] The beam shaping device preferably also has a beam combiner in order to recombine the at least two energy beams.

[0051] The beam combiner can preferably also include a polarizer, particularly preferably a thin-film polarizer. With such a beam combiner, for example, two linearly polarized partial beams can be recombined after their modification by a beam shaping element and thus generate an output energy beam again, whose intensity profile is dynamically modified in the desired manner.

[0052] In order to generate an energy beam with a desired, essentially non-rotationally symmetrical intensity distribution by means of the beam shaping device, the beam shaping device preferably has at least one control port and is more preferably designed such that the intensity distribution of the energy beam can be dynamically modified at least within a certain bandwidth by means of the control device. This allows the non-rotationally symmetrical intensity distribution to be permanently adapted to the current requirements via the control device in a nearly "real-time" manner, so that an optimal structural effect can be achieved in each curing area.

[0053] The input energy beam can come from any desired beam source. In principle, the input energy beam can also comprise a superimposed partial beam, as described. Preferably, but not necessarily, it is a laser beam.

[0054] Likewise, in the case of energy beams with a rotationally non-symmetrical intensity distribution, the intensity distribution can also be varied in the beam shaping device, ie, a combination of several methods.

[0055] Preferably, at least one of the following further process parameters, preferably a plurality of them (which may in part be further irradiation process parameters, but may also be other process parameters) is additionally determined based on the optimization criterion and / or auxiliary and / or boundary conditions:

[0056] - The radiation intensity of the energy beam. In this case, for example, the absolute value of the beam profile can be determined, for example, which maximum or minimum value the radiation intensity has, wherein one of the values ​​is determined because the other value is determined by the beam profile. In particular, the power of the energy beam is also determined in this case;

[0057] at least one beam expansion in at least one direction transverse to the direction of incidence, i.e., for example, the beam diameter or beam width, wherein the beam width is always understood to be the expansion perpendicular to the current direction of movement of the irradiated surface on the building volume. Alternatively or additionally, the entire shape of the energy beam at the irradiated surface on the building volume can also be determined. The beam expansion can be influenced, for example, by a focus adjustment mechanism;

[0058] - the speed of movement of the energy beam over the irradiation surface on the building area, which can also be modified in a position-dependent manner, ie does not need to be a constant scanning speed;

[0059] - the layer thickness of the individual applied or cured layers of building material;

[0060] - Parameters for determining the irradiation strategy. The selective irradiation or movement of the irradiation surface of the energy beam on the building area is usually carried out according to a suitable "irradiation strategy". As a result, a larger two-dimensional area, i.e. a larger surface on the building area, is usually irradiated during the curing process. Regardless of how the energy beam is generated and how the irradiation point on the building area is specifically moved, it has proven to be advantageous to first virtually "divide" this larger area to be irradiated according to a selected pattern into, for example, virtual "stripes", diamond patterns, chessboard patterns, etc. The energy beam is then mostly swept over the individual surfaces of the pattern, i.e. defined subareas, e.g. geometrically standardized surface areas, such as stripes or areas, in the form of so-called "hatches" (usually and hereinafter also referred to as "hatches"). In the stripe pattern, the building material is cured successively along parallel stripes from a macroscopic point of view and, specifically, from a microscopic point of view, the irradiation surface of the energy beam on the building area moves along hatches that are adjacent to each other, which extend back and forth in the boundaries of the irradiation stripes transversely to the extension direction of the corresponding irradiation stripes. In this case, for example, the irradiation pattern and / or the filling direction (alternating irradiation) can be selected as irradiation strategy parameters, or work can be performed with a constant filling direction (unidirectional irradiation, ie with a taper in the irradiation stripe from the filling end to the next adjacent filling start).

[0061] In this case, other process parameters can be considered variable, i.e., considered as, for example, optimizable input variables within the optimization process. This is also advantageous in many cases, especially with regard to radiation intensity and beam spread, since these ultimately influence the temperature distribution to the greatest extent together with the beam profile. However, other parameters can also be predetermined, for example as fixed target variables, such as layer thickness or irradiation strategy. In this case, it can be provided that the relevant parameters themselves become boundary conditions if boundary conditions must be maintained.

[0062] There are various options for determining the optimization criterion and / or auxiliary and / or boundary conditions:

[0063] In a preferred embodiment of the method, the target area and optionally the defined perimeter of the target area, preferably a perimeter of up to approximately five times, particularly preferably up to approximately three times, the extension of the irradiation surface, are virtually divided into spatially different process zones, wherein the extension of the irradiation surface is defined as the area within which 99% of the radiant power of the energy beam on the building area occurs. The spatial arrangement of the process zones relative to one another is defined with reference to a coordinate system that is fixed relative to the energy beam, i.e., the coordinate system moves with the energy beam on the building area surface and also rotates with the energy beam when the movement changes. Preferably, the z coordinate is located vertically on the building area at the intersection of the beam axis and the building area surface or the working plane, and the x and y coordinates are perpendicular thereto, for example, the x coordinate is always in the direction of movement of the energy beam on the irradiation surface on the building area and the y coordinate is perpendicular thereto.

[0064] Spatially different process zones can be, for example, a melting zone and a surrounding heat-affected zone, onto which the energy beam acts directly and melts the building material there. For example, the temperature in the heat-affected zone can be higher than in the material that has not yet been heated or has already cooled, for example 0.3 times the absolute solid temperature. These zones can in turn be divided into sub-zones, which will be described in more detail below, for example, based on a number of exemplary embodiments.

[0065] In this case, different optimization criteria and / or auxiliary and / or boundary conditions are preferably assigned to the individual process zones, i.e. to different subregions in the target area and the surroundings. Examples are also provided for this purpose. By dividing into different process zones, the optimization criteria or auxiliary and / or boundary conditions can be adjusted very precisely and thus a better optimized intensity distribution can be determined, which further promotes the production process.

[0066] As described, the optimization criteria and / or auxiliary and / or boundary conditions for the local target temperature distribution are material-dependent. For example, in order to carry out the process as efficiently as possible within the process window of thermal welding, it is necessary to ensure that the temperature approaches the evaporation temperature of the material used or the lowest evaporation temperature of the material components when a material combination (e.g., alloy) is used, but does not exceed it.

[0067] Therefore, preferably, at least one material characteristic value of the building material is taken into account when determining the optimization criterion and / or auxiliary and / or boundary condition with respect to the local target temperature distribution. Particularly preferably, at least one of the following parameters, preferably a plurality of them, is taken into account:

[0068] - Characteristic values ​​for describing the phase transition of the building material. For example, these include the nucleation rate and / or the nucleation growth rate;

[0069] - cooling rates and temperature stop points, e.g. in order to create and / or avoid phase changes in the building material;

[0070] - spatial temperature gradients, in particular permissible spatial temperature gradients in order to avoid damage caused by inherent stresses induced in the process;

[0071] - Thermal conductivity of the building material;

[0072] -Thermal capacity of the building material;

[0073] - Density of the building material;

[0074] - Thermal conductivity. It is calculated from the quotient of the thermal conductivity multiplied by the heat capacity and density of the building material;

[0075] -Build the surface stress of the material.

[0076] - the phase change enthalpy of the building material, i.e. the energy required to trigger a phase or released when a phase is formed;

[0077] The boiling or evaporation temperature, preferably the lowest boiling or evaporation temperature, of the building material or at least one of its components (if the building material has a plurality of components).

[0078] The melting temperature, preferably the lowest melting temperature, of the building material or at least one of its components (if the building material has a plurality of components).

[0079] In the case of temperature- and phase-dependent material characteristics, a plurality of corresponding material characteristics or tables or functions can also be predefined in principle, which define corresponding material characteristics as a function of temperature and phase. These relate, for example, to thermal conductivity, heat capacity, density or thermal conductivity and surface stress.

[0080] In principle, given material characteristic values, it is also possible to take into account that these parameters may change due to the reaction with the protective gas atmosphere, that is, the characteristic values ​​are corrected accordingly, for example with a suitable correction function, or a table is provided which can be used to find suitable values ​​depending on the protective gas, etc.

[0081] Preferably, at least one optimization criterion relates to at least one of the following parameters:

[0082] - The local temperature at the corresponding location on the building area. This temperature should preferably be as close as possible to the evaporation temperature or the lowest evaporation temperature in the material comprising multiple components, but not exceeded. In this way it can be reliably achieved that the process remains within the process window of thermal welding and is therefore very efficient since high energies can be introduced.

[0083] - The local temperature gradient at the corresponding position on the building area. This temperature gradient should be as close as possible to the local target temperature gradient.

[0084] -Cooling rate. The cooling rate should be as close as possible to the target cooling rate.

[0085] -The power of the energy beam. This power should be as low as possible in order to save energy.

[0086] - The speed of movement of the energy beam over the irradiation surface on the building area, i.e. the scanning speed. The movement speed should again be as high as possible in order to achieve a high productivity. Since the lowest possible power of the energy beam and a high scanning speed of the energy beam are prohibited relative to the energy that can be introduced, it is preferred to find the Pareto optimum in an optimization method.

[0087] Examples are also given below for objective variables belonging to different optimization criteria.

[0088] Preferably, at least one of the following target variables is determined in order to determine the optimization criterion and / or auxiliary and / or boundary conditions of the local target temperature distribution, preferably a plurality of these target variables is determined:

[0089] - The temperature change over time allowed. For example, a target cooling rate and / or a specific temperature stop point can be predetermined for this purpose. It should be noted that the temperature change for different process zones can be different as described above. In particular, the temperature change in the melting zone is mostly different from the temperature change in the adjacent heat-affected zone.

[0090] - Local target temperature gradient. This can also be determined differently for different process zones.

[0091] A target weld pool depth, ie a desired weld pool depth or weld penetration depth, which in turn can be related in particular to the layer thickness.

[0092] Target surface quality: For example, the effects to be avoided by thermocapillary convection and / or the maximum permissible local curvature of the surface can be predetermined as target variables.

[0093] - Target build rate. In this case, it can be optimized so that the desired speed is achieved in production. The target build rate is related in particular to the above-mentioned energy beam power and scanning speed.

[0094] - Permissible deviations from the (permissible) maximum temperature, especially in the melting zone.

[0095] - Target melt pool shape, i.e. the shape to be achieved in order to fill the already solidified filling structure.

[0096] As described, a plurality of auxiliary and / or boundary conditions may also be provided in order to define or limit the local target temperature distribution. Preferably, at least one auxiliary and / or boundary condition involves maintaining at least one of the following parameters or provisions:

[0097] - Maximum temperature. In general, as mentioned, the evaporation temperature of the material or material components is the maximum permissible temperature, thereby remaining within the process window of thermal soldering. The maximum temperature is predetermined by the material or material components used and does not change if the material does not change. This is therefore a boundary condition.

[0098] - Minimum temperature. In this case, the melting temperature of the respective material used or the liquidus temperature of the respective alloy used is usually predetermined. When the material is predetermined, this can also be a boundary condition.

[0099] - A continuous temperature trend at the zone boundary between two adjacent process zones. Preferably, the temperature trend should be continuously differentiable at least once. It is particularly advantageous if the temperature trend is approximately smooth, i.e. it can be continuously differentiated at least three times. A continuous temperature trend finally means that there are no sudden changes at the zone boundary or transition between two adjacent process zones, which is also impractical. This provision can be pre-given as an auxiliary or boundary condition within the optimization process. For example, the condition "continuously differentiable at least once" is pre-given as a boundary condition and is required as an auxiliary condition to achieve a temperature trend that is as smooth as possible.

[0100] - Minimum weld pool depth. This can be a weld pool depth or weld penetration depth that is to be achieved in order to ensure connection to the previously solidified layer. This can also be determined as an auxiliary or boundary condition, i.e. a specific minimum weld pool depth, but the optimum value is achieved as far as possible, for example within specific area boundaries.

[0101] All the parameters or regulations described can also be pre-set and maintained in combination in the optimization, or only partially pre-set and maintained. In particular, different parameters or parameter values ​​can also be determined as optimization criteria or target variables, auxiliary conditions and / or boundary conditions according to the strategy.

[0102] Another boundary condition that can be taken into account or preferably should be taken into account is the conditions for obtaining energy in the process. Since the energy introduced must flow away in principle, it is also preferably possible to ensure in the process optimization that the energy that can be introduced is not greater than the energy that flows away.

[0103] As boundary conditions, the maximum possible local (optical) resolution of the beam shaping device or beam generating device or the switching time or switching frequency when switching between specific beam characteristics when forming the intensity distribution curve can also be taken into account, as well as auxiliary conditions such that the scanning speed should always be greater than zero, so that the energy beam is not distorted at this location.

[0104] Depending on the material, the selected energy beam and other process conditions, such as the permissible scanning speed, the protective gas used, the target structure type and surface quality to be achieved, etc., a certain optimized intensity distribution curve of the energy beam can have completely different shapes. That is, any arbitrary shape of a rotationally asymmetric intensity distribution or intensity distribution curve is conceivable regardless of how and where a rotationally asymmetric intensity distribution is achieved.

[0105] Initial attempts have shown that, in particular, initially (e.g. for the first track or the first filling), an intensity distribution can be optimal when the intensity distribution has an axial symmetry on the building area, the axis of symmetry of which runs along the motion vector of the irradiated surface on the building area, i.e., an intensity distribution that is axially symmetrical, for example, in the scanning direction, wherein the energy beam has a higher intensity in the region moving forward from the beam axis than in the region behind (wherein the designations "forward" and "backward" relate to the current direction of motion). Such a shape can be achieved, for example, by superimposing two Gaussian distributions that are shifted relative to one another, i.e., a stronger Gaussian distribution that is located in front in the scanning direction and a larger Gaussian distribution, the center point of which is shifted in the opposite direction to the scanning direction toward the higher Gaussian distribution. In a particularly preferred optimized intensity distribution curve, this intensity distribution curve has a maximum region, i.e., a region of highest intensity, in the region of the irradiated surface on the building area. As described, this maximum region is then preferably shifted further forward in the direction of motion of the energy beam on the building area, i.e., in the scanning direction.

[0106] If the track runs near an already solidified area, this can be taken into account and therefore a deviation from an axisymmetric strength distribution can be advantageous.

[0107] The intensity distribution curve and the size of the irradiation surface of the energy beam on the building area, i.e. the beam expansion of the energy beam on the building area, can be determined or optimized together with the intensity distribution curve. Particularly preferably, the irradiation surface of the energy beam on the building area has a beam width (perpendicular to the scanning direction) of at least 400 μm, preferably at least 600 μm, particularly preferably at least 800 μm, for example about 1 mm.

[0108] As mentioned at the outset, the heat conduction welding process is to be used in at least one irradiation mode, preferably in the core mode, in which the component interior is produced. As mentioned, in this mode, work is mostly done with a filling structure.

[0109] In contrast, in contour mode, work is usually carried out with the aid of an energy beam and without a filling structure, wherein the energy beam passes through the entire structure of the component to be produced in one go in the corresponding layer plane. A similar process may be desirable in the interior of a component, for example in the region of a hole. In this special irradiation mode, a heat conduction welding process may not be desirable.

[0110] Therefore, in a preferred variant of the method, the energy beam is optionally generated in a further irradiation mode, particularly preferably in a contour mode, during the production process, so that the melting of the build material in the target region acts as deep welding.

[0111] For example, a relatively small beam diameter can be advantageous in order to enable the energy beam to pass easily through corners in the component cross section. However, since a sufficient penetration depth cannot always be achieved with a small beam diameter when working in a heat conduction welding process with a constant layer thickness, it can be advantageous to switch to another mode, for example a deep-seated welding process. BRIEF DESCRIPTION OF THE DRAWINGS

[0112] The present invention is described in detail again according to the embodiments with reference to the accompanying drawings. The same reference numerals are used for the same components in different drawings. It is shown in the drawings:

[0113] Figure 1 A schematic diagram partially in section shows an embodiment of an additive manufacturing device having a control data generating mechanism according to the present invention,

[0114] Figure 2 A flow chart showing a possible method procedure according to an embodiment of the manufacturing method of the present invention,

[0115] Figures 3 to 7 A schematic diagram showing an embodiment for dividing a target area and its surroundings into different process zones,

[0116] Figure 8 A flow chart showing a possible method sequence of an embodiment of an optimization method in a production method according to the invention,

[0117] Fig. 9 A schematic diagram showing a functional arrangement of components of an embodiment of a beam shaping mechanism to provide a desired intensity profile for an input energy beam. DETAILED DESCRIPTION

[0118] The following exemplary embodiments are described with reference to a device 1 for additive manufacturing of manufactured products in the form of a laser sintering or laser melting device 1, wherein it is expressly pointed out that the invention is not limited to laser sintering or laser melting devices. Therefore, the device is referred to below in a general and unrestricted manner as a "laser sintering device".

[0119] This laser sintering device 1 is Figure 1Schematically shown in FIG. The device has a process chamber 3 or process space 3 with a chamber wall 4, in which the manufacturing process is basically carried out. In the process chamber 3 there is a container 5 which is open upwards and has a container wall 6. The upper opening of the container 5 forms the current working plane 7. The area of ​​the working plane 7 located within the opening of the container 5 can be used to build the object 2 and is therefore called the building area 8.

[0120] The container 5 has a base plate 11 which is movable in a vertical direction V and is arranged on a carrier 10. The base plate 11 closes the container 5 downward and thus forms the bottom of the container. The base plate 11 can be formed integrally with the carrier 10, but it can also be a flat plate formed separately from the carrier 10 and fixed to the carrier 10 or simply supported on the carrier. Depending on the type of concrete building material, i.e., for example, the type of powder used and the type of manufacturing process, a building platform 12 can be mounted on the base plate 11 as a building base, on which the object 2 can be built. However, in principle, it is also possible to build an object on the base plate 11 itself, which then forms the building base.

[0121] The object 2 is built in principle by first applying a layer of building material 13 to the building platform 12, then selectively curing the building material 13 at the points where parts of the object 2 to be manufactured are required by means of the laser AL as will be explained later, then sinking the substrate 11 and the building platform 12 by means of the carrier 10 and applying a new layer of building material 13 and selectively curing it, etc. Figure 1 The object 2 built on the building platform 12 in a container is shown in an intermediate state below the working plane 7. The object already has a plurality of solidified layers and is surrounded by a remaining unsolidified building material 13. Different materials can be used as building material 13, preferably powders, in particular metal powders, plastic powders, ceramic powders, sand, filled or mixed powders or pasty materials.

[0122] Fresh building material 15 is located in a supply container 14 of the laser sintering device 1. By means of a coating device 16 movable in a horizontal direction H, the building material can be applied in the form of a thin layer in the working plane 7 or in the building region 8.

[0123] Optionally, there is an additional radiation heating device 17 in the process chamber 3. The radiation heating device can be used to heat the applied building material 13 so that the irradiation device for selective curing does not need to introduce too much energy. That is, for example, a large amount of basic energy can be introduced into the building material 13 by means of the radiation heating device 17, which is naturally lower than the energy required to melt or sinter the building material 13. For example, infrared radiators can be used as radiation heating devices 17.

[0124] For selective solidification, the laser sintering device 1 has an irradiation device 20 or, more specifically, an exposure device 20 having a laser 21. The laser 21 generates a laser beam EL, which is first fed to a beam shaping device 30 (as an input energy beam EL). The beam shaping device 30 is described later according to Fig. 9 As described in detail, the beam shaping device is designed so that the (output) energy beam AL or output laser beam AL for irradiating the building material 13 is generated from the input energy beam EL, so that the energy beam or output laser beam has an intensity distribution that is essentially non-rotationally symmetrical with respect to the beam direction R of the energy beam AL. The energy beam AL is then deflected via a subsequent deflection device 23 (scanner 23), whereby an exposure path or track set according to the exposure strategy is opened in the layer that needs to be selectively cured accordingly and energy is selectively introduced. That is, the irradiation surface 22 of the energy beam AL is moved on the building area 8 by means of the scanner 23, wherein the current movement vector or movement direction S (scanning direction) of the irradiation surface 22 can be frequently and rapidly changed on the building area 8. In this case, the laser beam AL is focused on the working plane 7 in a suitable manner by a focusing device 24. The irradiation device 20 is preferably located outside the process chamber 3 and the laser beam AL is introduced into the process chamber 3 via a coupling window 25 installed in the chamber wall 4 on the upper side of the process chamber 3.

[0125] The illumination device 20 comprises, for example, not just one but a plurality of lasers. Preferably, this can be a gas laser or a solid-state laser or any other type of laser, such as a laser diode, in particular a VCSEL (vertical cavity surface emitting laser) or a VECSEL (vertical external cavity surface emitting laser) or an array of such lasers. Very particularly preferably, one or more non-polarized single-mode lasers, such as a 3 kW fiber laser with a wavelength of 1070 nm, can be used in the present invention.

[0126] The laser sintering device 1 also includes a sensor component 18, which is suitable for detecting process radiation emitted in the working plane during the irradiation of the laser beam 22 onto the building material. The sensor component 18 operates in a position-resolved manner, i.e. the sensor component is able to detect an emission image of the corresponding layer. Preferably, an image sensor or a camera 18 is used as the sensor component 18, the camera being sufficiently sensitive in the area of ​​the emitted radiation. Alternatively or additionally, one or more sensors for detecting optical and / or thermal process radiation can also be used, such as photodiodes for detecting electromagnetic radiation emitted by the molten pool under the emitted laser beam AL or thermistors for detecting emitted thermal radiation (so-called molten pool monitoring). It is possible to correspond the signals of sensors that are not position-resolved per se to coordinates, so that the coordinates for controlling the laser beam respectively correspond in time to the sensor signals. In Figure 1The sensor arrangement 18 is arranged within the process chamber 3 . However, the sensor arrangement can also be located outside the process chamber 3 and in this case detect the process radiation through another window in the process chamber 3 .

[0127] The signals detected by the sensor arrangement 18 are transmitted as process volume sensor data sets or layer images SB to a control device 50 of the laser sintering device 1 , which also serves to actuate the various components of the laser sintering device 1 for controlling the additive manufacturing process as a whole.

[0128] To this end, the control mechanism 50 has a control unit 51, which controls the components of the irradiation mechanism 20 via an irradiation control port 53, namely, sending laser control data LS to the laser 21, sending intensity distribution control data VS to the beam shaping mechanism 30, sending scanning control data SD to the steering mechanism 23 and sending focusing control data FS to the focusing mechanism 24.

[0129] The control unit 51 also controls the radiation heater 17 by means of suitable heating control data HS, the coating machine 16 by means of coating control data ST and the movement of the carrier 10 by means of carrier control data TS, thus controlling the layer thickness.

[0130] In addition, the control device 50 has a quality data determination device 52 which receives the process volume sensor data set SB and determines quality data QD based thereon, which can be forwarded to the control unit 51 for controllable intervention in the additive manufacturing process, for example.

[0131] The control device 50 is coupled here, for example, via a bus 55 or another data connection to a terminal 56 having a display etc. An operator can control the control device 50 and the entire laser sintering device 1 via the terminal, for example by transmitting process control data PSD.

[0132] In order to optimize the production process, control data are generated or modified in a manner according to the invention with the aid of a control data generating unit 54, 54' so that the device 1 is controlled in at least one specific irradiation mode (hereinafter based on a core mode in which the interior of the object is to be solidified) so that on the one hand the process is carried out as a heat conduction welding process and not as a deep welding process and on the other hand the energy beam AL has an optimized, essentially rotationally non-symmetrical intensity distribution curve at the irradiation surface 22 on the building area.

[0133] The control data generation mechanism 54 can be, for example, part of the control mechanism 50 and can be implemented as a software component. Such a control data generation mechanism 54 integrated in the control mechanism 50 can, for example, receive process control data PSD and modify it accordingly, so that an energy beam AL with an optimized beam distribution curve is generated and then the corresponding modified control data PSD is further transmitted to the control unit 51. Here, the modified control data PSD includes, in particular, modified exposure control data BSD, but also includes other modified control data, such as changed coating control data ST or carrier control data TS, if necessary, in order to select a suitable layer thickness. Alternatively, however, only the exposure control data BSD can be modified in the control data generation mechanism 54 and forwarded to the control unit 51, whereby the irradiation control port 53 works with the modified exposure control data BSD.

[0134] However, it is also possible that the control data generation device 54' is implemented on an external computer unit, for example, here on the terminal 56, and that process control data PSD with correspondingly suitable exposure control data BSD have previously been created, with the aid of which the device 1 is controlled so that an optimized intensity distribution curve is achieved in order to carry out the process as a heat conduction welding process. In this case, the internal control data generation device 54 present here in the control device 50 can also be omitted.

[0135] As described, the process control data PSD, in particular the exposure control data BSD, generated or modified by the control data generating unit 54, 54' can also be regarded as setpoint values, which are then used in the control unit 51 for the regulation process, wherein, for example (as a feasibility) the quality data QD can be taken into account as actual values.

[0136] It should be emphasized again here that the present invention is not limited to such a laser sintering device 1. The laser sintering device can be used for any other method for generating or additively manufacturing three-dimensional objects by applying and selectively solidifying a building material, in particular layer by layer, wherein an energy beam is output to the building material to be solidified for solidification. Therefore, the irradiation device can not only be a laser as described here, but any device can be used that can selectively bring energy to or into the building material as wave or particle radiation. For example, instead of a laser, another light source, an electric splitter beam, etc. can be used.

[0137] Even in Figure 1 Only a single object 2 is shown in the figure, but a plurality of objects can and usually are produced in parallel in the process chamber 3 or in the container 5. Examples for this will be given later. For this purpose, the building material is scanned layer by layer by an energy beam at locations corresponding to the cross section of the object in the individual layers.

[0138] According to the following Figure 2A process for creating an optimized intensity profile IO as well as optimized other process parameters WP, such as eg scanning speed, focus, layer thickness etc., which may be determined by the control data generating mechanism 54, 54' is described.

[0139] In a first step I, certain optimization criteria OK as well as auxiliary and boundary conditions WB are initially determined.

[0140] As input values, for example, material characteristic values ​​MK of the building material can be provided, for example, the above-mentioned characteristic values ​​for describing the phase transition, cooling rate and temperature standstill, thermal conductivity, heat capacity, density, thermal conductivity, surface stress, phase change enthalpy, boiling or evaporation temperature, melting temperature, etc. of the building material. These characteristic values ​​can be predefined in the form of functions and / or tables or as individual values. In principle, process data containing information such as the type of material used or the product name can also be received and suitable material characteristic values ​​can be automatically selected accordingly. It is also possible to input materials and / or material characteristic values ​​via a user interface.

[0141] Furthermore, in this step, process zones PZ can be defined, for example by the user or by extracting them from predefined control records. Figures 3 to 7 A possible process zone PZ is elaborated in detail.

[0142] In addition, target variables ZG can be predefined, such as a target cooling rate or an optimal temperature stop point, desired local target temperature gradients for different process zones, a target melt pool depth, target surface properties, a target build rate, a deviation from a maximum temperature that is still permitted, and a target melt pool shape, etc.

[0143] Finally, specific boundary and / or auxiliary conditions WB can also be directly predefined as desired. These data can also be extracted, for example, from prefabricated or existing control protocols.

[0144] Then, in the next step II, the optimization criteria OK and the boundary and / or auxiliary conditions WB determined in step I for the optimal local temperature distribution TV (target temperature distribution) are introduced into an optimization process, in which an optimized intensity distribution curve IO and other process parameters WP are determined, and while maintaining these intensity distribution curves and process parameters, the target temperature distribution TV in the respective current target area of ​​the build material achieves the optimization criteria as well as possible and also maintains the auxiliary conditions and, crucially, the boundary conditions as well as possible. The other process parameters WP determined in the optimization process may include, for example, scanning speed and layer thickness, which are ideally combined with the optimized intensity distribution curve IO. An example of such an optimization process will be described later according to Figure 8 Explain.

[0145] Then, in step III, the optimized intensity distribution curve IO and other process parameters WP are used to generate control data PSD, BSD, or if part of the control data already exists, the control data is modified accordingly, so that the energy beam is emitted to the irradiation surface 22 on the building area 8 with the optimized intensity distribution curve IO and the other process parameters WP are maintained during irradiation or when building the layer.

[0146] The following is only an example of a possible calculation of an optimized intensity distribution curve IO, which in a laser welding process makes the welding process according to the heat conduction welding principle. It should be emphasized that the entire method can also be used similarly for other energy beams.

[0147] For this purpose, a plane is first defined in which there is a moving orthogonal coordinate system x, y, z, the origin of which is always located at the center of the moving laser beam AL. The z direction of the coordinate system runs perpendicular to the working plane. The x and y coordinates are arranged perpendicular to the z direction. The coordinate system is defined in such a way that it rotates with the laser beam AL so that the laser beam always moves in the positive x direction, i.e. the projection of the coordinate x on the building area 8 corresponds to the scanning direction S.

[0148] The (x- / y-) plane defined in this coordinate system is in the region around the irradiation surface 22 of the energy beam AL on the building area 8, that is, in the target area Γ Z In the target area Γ Z A certain perimeter Γ U The process is virtually divided into spatially different process zones. The optimization criteria OK and / or auxiliary and / or boundary conditions WB are then defined with respect to the process zones.

[0149] The first region or the first process zone Γ S It can be called the melting zone Γ S This may be a region where the substance or building material is in a molten state. S Can be further divided into active melting zone Γ when necessary SA and the passive melting zone Γ SP (as different first process area and second process area) (for this see Figure 3 and Figure 4 ). The active area is heated by the laser beam AL, respectively, while the passive area is not.

[0150] Furthermore, a third region or a third process zone Γ may be defined. WS , which includes the heat-affected zone Γ laterally to the laser beam or perpendicularly to the corresponding direction of movement x WS The fourth heat-affected zone directly following the laser beam can also be defined as the following heat-affected zone Γ WP .

[0151] Instead of only one lateral heat affected zone Γ WS and / or a subsequent heat affected zone Γ WP , similar to the melting zone, the active heat affected zone Γ can also be defined as desired WSA , Γ WSP and the corresponding passive heat affected zone Γ WPA , Γ WPP , as in Figures 5 to 7 As shown in the example.

[0152] The remaining area, especially the area in front of the laser beam AL in the scanning direction, is called the periphery Γ U . Especially from Figures 5 to 7 It can be seen that the beam spread d of the laser beam AL does not need to be related to the active melting zone Γ SA consistent and, for example, also wish to actively influence the heat-affected zone, ie, the process zone Γ WSA or Γ WPA In this way, for example, the cooling rate and the temperature gradient can be determined more accurately in these areas. However, the laser beam AL should cover all "actively influenced" areas.

[0153] For example, in Figure 4 The process area Γ is shown in SA , Γ SP , Γ WS , Γ WP A possible optimization is described in a slightly more detailed manner below. For other partitions, similar definitions and procedures are used as appropriate.

[0154] Firstly, the following variables for optimization can be determined or predefined from the material data of the existing workpiece:

[0155] - Cooling rate T. The cooling rate depends on the material, ie the desired material properties, such as grain size, martensitic phase transformation, etc.

[0156] - Maximum acceptable temperature T V This is usually the evaporation temperature of the material being used or, as described, the lowest evaporation temperature in a mixture of materials.

[0157] - Melting temperature T M Here too, a minimum melting temperature must be achieved when the materials are mixed.

[0158] - In the melting zone Γ S The target temperature gradient in the equation can be defined mathematically as follows:

[0159]

[0160] T S (x, y) corresponds here to the temperature at the location (x, y) on the building region 8 in the target region of the laser beam AL, This corresponds to the derivative of the temperature at the location (x, y) on the building region 8 in the target region of the laser beam AL, and are the derivatives in the x and y directions respectively.

[0161] - In the lateral heat affected zone Γ S The target temperature gradient in can be defined mathematically as follows:

[0162]

[0163] T WS (x, y) corresponds here to the temperature at the location (x, y) on the building region 8 in the target region of the laser beam AL, This corresponds to the derivative of the temperature at the location (x, y) on the building region 8 in the target region of the laser beam AL, and are the derivatives in the x and y directions respectively.

[0164] Similar to the lateral heat affected zone Γ WS The target temperature gradient can also be the heat affected zone Γ WP Define the target temperature gradient.

[0165] The temperature gradients defined above are respectively predetermined desired parameters. For example, a maximum temperature gradient can be provided depending on the material, since the corresponding temperature gradient determines the thermocapillary convection.

[0166] In particular, the following aspects can also be taken into account when determining the target temperature gradient: In principle, stresses are generated between the solid and the weld due to the temperature gradient after the weld has hardened and cooled. This stress can be so great that it can significantly deteriorate the quality of the component or even lead to cracks in extreme cases. Influencing the magnitude and distribution of the stresses in order to sufficiently reduce the stresses, for example by adjusting the exposure and beam parameters, can improve the quality of the component. The target direction here is to reduce the temperature gradient or to keep the temperature gradient sufficiently small. Since the temperature at the melt / solid boundary surface for a given material is determined, this can be achieved by appropriately increasing the solid temperature in advance or in parallel at least locally, i.e. where the weld (joining zone) is to be joined. This can also be achieved by modifying the intensity distribution curve, i.e. designing the intensity distribution curve so that the joining zone is also irradiated, to be precise, with exactly the energy that produces the desired temperature distribution there. For this purpose, for example, an active heat-affected zone Γ can be used. WSA , as in Figure 5 and Figure 6 As shown in , the process area is specifically defined.

[0167] The following are examples of variants for defining process zones according to Figure 4 Mathematical equations are described which can define the optimization goal or optimization criterion and the auxiliary conditions and boundary conditions. In this case, equations (3) to (6) show possible optimization goals or auxiliary conditions and equations (7) to (13) give auxiliary conditions or boundary conditions which should be satisfied:

[0168] For example, for the melting zone Γ S For all points x and y in the , the following optimization objectives can be defined:

[0169]

[0170] Equation (3) describes the melting zone Γ S Optimization of the target temperature distribution T(I,x,y) in the relationship T(I,x,y). The parameter I in the relationship T(I,x,y) here symbolizes the relationship between the target temperature distribution T(I,x,y) and the actual intensity distribution I(x,y) of the energy beam that needs to be optimized. The relationship between T(I,x,y) and I(x,y) can be defined, for example, by a coupling condition of two variables, as will be given later in equation (10). In principle, equation (3) or other optimization targets can also be directly converted to a relationship with the intensity distribution I(x,y) instead of the target temperature distribution T(I,x,y), but this will make the formula very complicated. Depending on the selected optimization method, this relationship can also be taken into account in a simulation step (which simulation step can simulate which intensity distribution I(x,y) and which other parameters will lead to which target temperature distribution T(I,x,y)) in an iterative optimization process. In this regard, even if the relationship between the target temperature distribution T(x,y) and the intensity distribution I(x,y) is always given below, it will not always be called the parameter I in the target temperature distribution T(x,y).

[0171] In the first term of equation (3), at the evaporation temperature T V The difference between the local temperature T(x,y) to be optimized at the surface of the molten pool is the objective function to be minimized. This makes the melting zone Γ S The temperature T(x,y) in the V However, it should also be ensured by boundary conditions not described in equation (3) that the temperature T(x,y) at the surface of the melt pool remains below the evaporation temperature T everywhere. V , thereby also maintaining the process window of thermal conductive soldering (see equation (7) below).

[0172] The second part of equation (3) defines the spatial fluctuation of the temperature T(x,y) at the surface of the melt pool as the target function. The error that causes the desired spatial fluctuation should be minimized, i.e. the desired temperature gradient is predefined according to equation (1). This desired temperature gradient should be maintained. When, for example, the goal is to suppress thermocapillary convection in the molten pool surface, the temperature gradient can be The vector is set to zero. If the desired flow and a large amount of heat conduction should be induced in the molten pool, the temperature gradient at each point x, y in the molten zone required to induce the flow is can all be determined via the temperature dependence of the surface stress. This can be done, for example, by means of numerical calculations to solve the Navier-Stokes equations. Thermocapillary convection is taken into account in the mathematical models used here. In addition, heat conduction is also simulated in such models. These models can be applied, for example, in the above-mentioned simulation steps in an iterative optimization process.

[0173] The speed factors w1 , w2 in equation (3) can be used to predetermine, for example, the dependence of the material sensitivity on the temperature gradient, whether higher values ​​bring the current temperature closer to the evaporation temperature, ie the melt is as hot as possible, or whether the temperature gradient should be taken more into account.

[0174] In the lateral heat affected zone Γ WS The optimization of the temperature distribution in can be defined by the following equation:

[0175]

[0176] In the heat affected zone Γ WS Temperature gradient The desired temperature distribution curve is pre-given. The desired distribution curve can be selected so that the inherent stress formed due to excessive local temperature gradient is reduced. The heat affected zone Γ at each point x, y and lateral is determined by the allowable temperature gradient for reducing the inherent stress. WS The temperature gradient at Vector.

[0177] Heat affected zone Γ for following WP The optimization criterion for the temperature gradient T(x,y) at position x, y in can be defined, for example, by the following equation:

[0178]

[0179] Here, the cooling rate The temperature gradient in space along the direction of motion and the scanning speed v. If we assume that at a specific point in time, the point is in the center of the laser, then for an external observer who does not move with it, the cooling rate is This cooling rate is different from the cooling rate from the perspective of an observer moving together, which can be determined by spatial or local gradients. It is expressed by multiplying the scanning speed v.

[0180] Furthermore, the scanning speed v can be an optimization criterion, since the time to set up the workpiece can be determined hereby as well as the power required for the process, which is obtained by integrating the target intensity distribution (or optimized intensity distribution) I(x,y) of the laser beam. For example, when the required minimum power becomes the optimization parameter, the system can be designed to be more energy-efficient.

[0181] To this end, the intensity distribution I(x,y) of the laser beam can be determined for all process zones or areas and must satisfy the following conditions:

[0182] min(w3∫∫I(x,y)dydx-w4v) (6)

[0183] Here, an outer integral is run for all x-coordinate values ​​and an inner integral is run for all y-coordinate values, i.e., a double integral is run for the power of the energy beam. In other words, the integral of the intensity I(x,y), i.e., the power of the energy beam, is minimized and the scanning speed v is maximized to achieve the highest possible build rate with the lowest energy consumption. Since the two conditions are contradictory, the Pareto optimum is found with the aid of optimization condition (6), wherein more weight can be placed on one or the other objective with the aid of speed coefficients w3, w4 as required. For example, it may be more advantageous to operate the laser at a higher power, thereby achieving the highest possible speed and a shorter build time. An overall consideration makes sense.

[0184] It should be pointed out in this context that this equation is only an extremely simplified version. Other factors, such as factors describing the operating costs of the machine, can also be advantageously taken into account at the same time.

[0185] In addition, the following auxiliary conditions can be defined for the optimization method:

[0186] T V -T(x, y)≥0 (7)

[0187] This is an auxiliary condition as mentioned above, so that the current local temperature T(x,y) will never be higher than the lowest evaporation temperature T V , thus remaining in the thermal conductive soldering process.

[0188] T(x, y)-T M ≥0 (8)

[0189] In a similar manner, the temperature T(x,y) should always be greater than or equal to the melting temperature T M .

[0190] For the melting zone Γ S Heat affected zone Γ in the middle and lateral directions WS The positions x, y in can also be defined (exemplarily for a section in the y direction) as:

[0191]

[0192] The auxiliary condition ensures that at the boundary of the two process zones, here in the melting zone Γ S and heat affected zone Γ WS The temperatures between the two process zones should be as equal as possible, since there are really no temperature jumps in the surface. Boundary conditions can be defined similarly for other process zone transitions.

[0193] Another auxiliary condition ensures that all energy introduced into the process also flows downwards:

[0194]

[0195] This is done through

[0196]

[0197] To ensure that it defines the energy that flows into the region Ω below the surface. α is the absorption capacity of the building material and λ is the thermal conductivity of the building material.

[0198] Once condition (10) is determined, it should apply to all positions x, y in the active region, i.e., in the melting region Γ S and, if necessary, also in the "active" heat-affected zone Γ WSA , Γ WPA (For example, in Figure 6 Definition of process area in ).

[0199] For all positions x, y, z in volume Ω, for example, we can solve the heat conduction equation

[0200]

[0201] Determine the required variables for equations (10) and (11), where is the time derivative of T(x,y,z). p,eff (T(x,y,z)) is the temperature-dependent effective heat capacity, which also takes into account the heat of transition of all phase changes, ρ(T(x,y,z)) represents the temperature-dependent density, and the temperature-dependent thermal conductivity is provided by λ(T(x,y,z)). The derivative corresponding to temperature T(x,y,z).

[0202] Finally, preferably also a minimum welding depth t min, a minimum penetration depth must be achieved to mount one layer onto the previous layer. This can be determined by the equation

[0203] t min -t igt <0 (13)

[0204] To define, where t ist is the current welding depth. Another auxiliary condition may be that the scanning speed v is always greater than 0.

[0205] Therefore, optimization criteria and auxiliary conditions and boundary conditions can be defined for other subdivided process zones. Which of the above conditions is used as optimization criteria, auxiliary conditions or boundary conditions or whether other conditions are to be added is related to the specific manufacturing task (e.g., the machine used, the building material, the manufactured product and its requirements, etc.). Usually, in particular, the above boundary conditions must be selected according to the corresponding machine or device for additive manufacturing of the product that also performs the process at this time.

[0206] Equation 12 can also be solved numerically or empirically. In adaptive control or regulation, the equation can also be compared with on-site measurements (eg by means of monitoring) and the distribution curve can be readjusted during this process by resolving the optimization problem.

[0207] According to the following Figure 8 Preferred examples of suitable optimization methods are described below. Iterative methods can be used, for example, according to Figure 2 The method is performed in step II.

[0208] Initially, in a first step II.1, starting values ​​of the (starting) intensity distribution I(x,y) are estimated.

[0209] In the next step II.2, the heat conduction equation (12) is then solved, wherein the auxiliary conditions according to equation (10) need to be met. In this case, equation (10) includes the term αI(x,y), i.e. the (starting) intensity distribution I(x,y) in step II.1. The heat conduction equation (12) describes the introduction of heat energy from the irradiated surface into the surrounding material when a given intensity distribution I(x,y) is introduced into the material by the laser. Thus, by solving the equation, the temperature distribution curve T(x,y,z) in the material that appears on the building area in the relevant intensity distribution I(x,y) of the laser is obtained. Thus, in the first cycle of the iteration, the starting temperature distribution curve T(x,y,z) in the material is calculated essentially from the (starting) intensity distribution I(x,y) of the laser.

[0210] In step II.3, a (first) optimization process of the temperature distribution curve T(x, y, z) is then carried out, wherein a "correction value" is sought for the temperature distribution curve T(x, y, z), with the aid of which the temperature distribution curve T(x, y, z) satisfies the optimization criteria and conditions defined above according to equations (3) to (9) to the greatest extent possible.

[0211] Then in step II.4, a check is made that steps II.2 and II.3 are carried out at least twice and then the interruption criterion is checked, which involves, for example, a convergence criterion, whether in the current iteration the temperature distribution curve T(x, y, z) and / or the intensity distribution I(x, y) has changed by a previously defined tolerance value (residue) relative to the previous iteration (wherein "current" describes the iteration n and "previous" describes the iteration n-1). If this is not the case or steps II.2 and II.3 have only been carried out once, a jump is made back to step II.2 and another iteration cycle is carried out again with the current intensity distribution I(x, y).

[0212] Otherwise, the optimization method ends in step II.5 and the sought optimal intensity distribution I(x,y) is present.

[0213] In the process described above, the density, effective heat capacity, thermal conductivity, maximum acceptable temperature, melting temperature, temperature gradient and cooling rate of the heat-affected zone can be pre-set as fixed parameters as described. In addition, the minimum welding depth is used as a process parameter, and the minimum welding depth is determined by the pre-set layer height of the process. In the optimization, the power required by the system is minimized and the volume remelted per time unit is maximized. The free variables are the intensity distribution and the scanning speed. However, any other standards and input values ​​can also be added as desired, which are respectively related to the machine used, the material used and other conditions and requirements. In principle, for example, the alloy components in the corresponding material specifications can also be considered as parameters to be optimized during optimization, because the alloy components affect the material characteristics and costs, so only one example is described.

[0214] The above-described method can at least significantly reduce evaporation or even completely eliminate it. As a result, the power injected into the material per laser beam can be increased by approximately one order of magnitude, but without increasing losses in detail resolution. A similar build quality is achieved, but the component costs can be significantly reduced. Another advantage is that the method can also be used in known systems with only one or a small number of exposure devices or scanners / laser beams.

[0215] Below with the help of Fig. 9The described beam shaping device 30 can be used not only to equip new machines or new devices for manufacturing products by additive manufacturing, but also to retrofit existing machines or devices having a conventional exposure device that generates a substantially rotationally symmetric Gaussian-shaped energy beam.

[0216] exist Fig. 9 The embodiment of a suitable beam shaping mechanism 30 shown in FIG. 1 receives an input energy beam EL, such as that described above with reference to FIG. Figure 1 The laser beam of the laser 21 described in the relevant description. The input energy beam EL has a substantially rotationally symmetric intensity distribution, for example a Gaussian distribution curve. The intensity distribution of the input energy beam EL is then modified in the beam shaping device 30 so that after leaving the beam shaping device 30, the intensity distribution is substantially non-rotationally symmetric with respect to the rotation of the beam axis R or the beam direction. For example, an elliptical intensity distribution can be achieved here, which has a higher intensity on one side than on the other side. Preferably, the intensity distribution of the energy beam AL has an axial symmetry, and its axial symmetry line extends along the motion vector of the irradiation surface 22 of the energy beam AL on the building area 8. A corresponding example of an elliptical intensity distribution is also described in TienT. However, any other substantially non-rotationally symmetrical intensity distribution can also be achieved with the aid of the beam shaping device 30 .

[0217] First, the beam shaping mechanism 30 has a beam splitter 32 in the form of a thin-layer polarizer 32 on the input side, which splits the input energy beam EL into two linearly polarized sub-beams TL1 and TL2. Each of these linearly polarized sub-beams TL1 and TL2 is guided to a respective beam shaping element 34 and 35, which is an LCoS microdisplay 34 and 35 respectively. The LCoS microdisplays 34 and 35 are mainly used for suitable beam shaping. This is a passive DOE, which works in a reflective manner and changes the wavefront of the incident sub-beams TL1 and TL2 by locally modulating the phase and / or amplitude. For this purpose, the LCoS microdisplays 34 and 35 are controlled by corresponding sub-shape control signals FS1 and FS2, which are transferred to the two LCoS microdisplays 34 and 35 via the control port 31. The control port 31 receives on the input side from the illumination control port 53 of the control mechanism 50 as described above. Figure 1 Combined with the described intensity distribution control data VS.

[0218] The two correspondingly modulated partial beams TL1, TL2 are then recombined in a beam combiner 33, which is here also a thin-film polarizer 33 like the beam splitter 32. At the output of the beam combiner 33 there is then an output laser beam AL shaped in a known manner with regard to the intensity distribution, which is again randomly polarized.

[0219] The intensity profiles or phase profiles of the partial beams provided on the two LCoS microdisplays 34, 35 are preferably identical. However, in order to achieve certain optical assistance criteria, for example, the maximum intensity on the optical elements of the beam shaping device can also be provided differently, so that the desired intensity profile nevertheless occurs in the target plane.

[0220] The laser beam AL modified in this way by the beam shaping device 30, ie provided with a non-rotationally symmetrical optimized intensity distribution curve IO, is shown as follows. Figure 1 The optical image is conducted, schematically illustrated in FIG. 2 , to a scanner 23 and from there to the building region 8 .

[0221] Finally, it should also be emphasized that the above-described device is only an embodiment that can be modified in different ways by a person skilled in the art without leaving the scope of the invention. For example, when using other heat sources, in addition to energy beams, such as surface heating devices and / or other heat-influencing variables, such as cooling devices, etc., the energy introduced or removed thereby is also taken into account during optimization. In addition, the use of the indefinite article "a" does not exclude that the feature in question may also exist multiple times. The term "unit" also does not exclude that the unit is composed of a plurality of cooperating subcomponents, which may also be spatially distributed.

[0222] Reference numerals list

[0223] 1 Additive manufacturing device / laser sintering device

[0224] 2. Manufacturing products / objects / components

[0225] 3 Process space / process chamber

[0226] 4 Cavity wall

[0227] 5. Container

[0228] 6 container wall

[0229] 7 Work Plane

[0230] 8 Build Area

[0231] 10 Carrier

[0232] 11 base plate

[0233] 12 Build Platform

[0234] 13 Construction materials (in container 5)

[0235] 14 Spare Container

[0236] 15 Construction materials (in spare container 14)

[0237] 16 Coating Machine

[0238] 17 Radiant Heating Mechanism

[0239] 18 Sensor assembly / camera

[0240] 20 Irradiation mechanism / Exposure mechanism

[0241] 21 Laser

[0242] 22 (laser beam) irradiation surface

[0243] 23 Steering mechanism / scanner

[0244] 24 Focus on institutions

[0245] 25 Coupling window

[0246] 30 Beam shaping mechanism

[0247] 31 Control Port

[0248] 32 Beam splitter / thin layer polarizer

[0249] 33 Beam combiner / thin layer polarizer

[0250] 34 Beam shaping element / LCoS microdisplay

[0251] 35 Beam Shaping Element / LCoS Microdisplay

[0252] 50 Control Agency

[0253] 51 Control unit

[0254] 52 Quality data determination agency

[0255] 53 Irradiation control port

[0256] 54, 54' Control data generation mechanism

[0257] 55 Bus

[0258] 56 Terminal

[0259] AL (Output) Energy beam / Laser beam

[0260] BSD Control Data / Exposure Control Data

[0261] EL Input Energy Beam / Laser Beam

[0262] FS Focus control data

[0263] FS1, FS2 sub-shape control signal

[0264] H Horizontal direction

[0265] HS Heating Control Data

[0266] LS Laser Control Data

[0267] PSD Process Control Data

[0268] QD Quality Data

[0269] R Beam axis / beam direction

[0270] S Scanning direction / movement direction of the irradiated surface

[0271] SB Process Space Sensor Data Set / Layer Pattern

[0272] SD Scan Control Data

[0273] ST exposure control data

[0274] TL1, TL2 split beam

[0275] TS Carrier Control Data

[0276] V vertical direction

[0277] VS intensity distribution control data

[0278] MK Material characteristic value

[0279] PZ Process Zone

[0280] ZG target variable

[0281] OK Optimization criteria

[0282] WB Boundary and / or auxiliary conditions

[0283] TV Local temperature distribution / target temperature distribution

[0284] IO-optimized strength profile

[0285] WP Other process parameters

[0286] x, y, z coordinate axes

[0287] Γ U Neighborhood

[0288] Γ Z Target area

[0289] d Beam expansion

[0290] Γ S Melting area / processing area

[0291] Γ SA Active melting zone / processing zone

[0292] Γ SP Passive melting zone / process zone

[0293] Γ WS Lateral heat affected zone / process zone

[0294] Γ WP Followed by the heat affected zone

[0295] Γ WSA , Γ WSP Active Heat Affected Zone

[0296] Γ WPA , Γ WPP Passive heat affected zone.

Claims

1. A method for generating control data (BSD, PSD) for an apparatus (1) for additive manufacturing of a product (2) in a manufacturing process, wherein: In the manufacturing process, a building material (13) is built up and selectively cured, wherein, for curing on a building area (8), the building material (13) is irradiated with at least one energy beam (AL), wherein an irradiation surface (22) of the energy beam (AL) moves over the building area (8) so that the building material (13) is cured in a target area (Γ) in or around the irradiation surface (22). Z ), wherein, in order to generate the control data (BSD, PSD) for at least one irradiation mode, a target area (Γ ) in the building material (13) is determined. Z ) in the target area (Γ ) in which the target temperature distribution (TV) is optimized (OK) and / or auxiliary and / or boundary conditions (WB), wherein the target area (Γ Z ) causes the building material (13) to melt and determines at least one optimized intensity distribution curve (IO) of the energy beam (AL) within the scope of the optimization process based on the optimization criterion (OK) and / or auxiliary and / or boundary conditions (WB), wherein the energy beam (AL) at the irradiation surface (22) on the building area (8) corresponds to the determined optimized intensity distribution curve (IO) or at least approaches the determined optimized intensity distribution curve (IO) as well as possible except for certain tolerances, so that a desired local objective is achieved. Temperature distribution (TV), and wherein the optimized intensity distribution curve (IO) of the irradiation surface (22) of the energy beam (AL) on the building area (8) is essentially non-rotationally symmetric about a beam axis (R) extending coaxially with the incident direction of the energy beam (AL), and wherein the control data (BSD, PSD) are generated so that when the additive manufacturing device (1) is controlled, the building material (13) is irradiated in the irradiation mode with an energy beam (AL) essentially having a determined, optimized intensity distribution curve (IO).

2. The method according to claim 1, wherein: Based on the optimization criterion (OK) and / or the auxiliary and / or boundary conditions (WB), at least one of the following process parameters (WP) is also determined: - Radiation intensity; - at least one beam expansion (d) and / or the shape of the irradiation surface (22) of the energy beam (AL) on the building area (8); - the speed of movement of the irradiation surface (22) of the energy beam (AL) over the building area (8); - layer thickness; - Irradiation strategy.

3. The method according to claim 1 or 2, wherein: The target area (Γ Z ) and optionally the target area (Γ Z )'s periphery (Γ U ) is divided into multiple process zones (PZ, Γ S , Γ SA , Γ SP , Γ WS , Γ WP , Γ WSA , Γ WSP , Γ WPA , Γ WPP ), wherein the process zone (PZ, Γ S , Γ SA , Γ SP , Γ WS , Γ WP , Γ WSA , Γ WSP , Γ WPA , Γ WPP ) are defined relative to one another in space with reference to a coordinate system (x, y, z) fixed to the energy beam (AL), and wherein for different process zones (PZ, Γ S , Γ SA , Γ SP , Γ WS , Γ WP , Γ WSA , Γ WSP , Γ WPA , Γ WPP ) is equipped with different optimization criteria (OK) and / or auxiliary and / or boundary conditions (WB).

4. The method according to claim 1 or 2, wherein: At least one material characteristic value (MK) of the building material (13) is taken into account when determining the optimization criterion (OK) and / or auxiliary and / or boundary conditions (WB) for the local target temperature distribution (TV).

5. The method according to claim 1 or 2, wherein: When determining the optimization criterion (OK) and / or auxiliary and / or boundary conditions (WB) for the local target temperature distribution (TV), at least one of the following parameters is taken into account: - characteristic values ​​for describing phase changes of the building material; -Cooling rate and temperature stop point; -Spatial temperature gradient; - thermal conductivity; -Heat capacity; -density; - thermal conductivity; - surface stress; - phase change enthalpy; - boiling or evaporation temperature; - Melting temperature.

6. The method according to claim 1 or 2, wherein: At least one optimization criterion (OK) relates to at least one of the following parameters: - local temperature; - local temperature gradient; - Cooling rate; - the power of the energy beam; - The speed of movement of the irradiation surface of the energy beam over the building area.

7. The method according to claim 1 or 2, wherein: In order to determine the optimization criterion (OK) and / or auxiliary and / or boundary conditions (WB) for the local target temperature distribution (TV), at least one of the following target variables (ZG) is determined: -Temperature variation over time; - Local target temperature gradient; - Target melt pool depth; - Target surface quality; - Target build rate; - maximum temperature deviation; - Target melt pool shape.

8. The method according to claim 1 or 2, wherein: At least one auxiliary and / or boundary condition (WB) involves maintaining at least one of the following parameters or provisions: - maximum temperature; - minimum temperature; - a continuous temperature profile at the zone boundary between two adjacent process zones; -Minimum melt pool depth.

9. The method according to claim 1 or 2, wherein: The intensity distribution curve has a maximum area in the region of the illumination surface (22) on the building area (8).

10. The method according to claim 1 or 2, wherein: The intensity distribution curve has a maximum area in the region of the irradiation surface (22) on the building area (8) moving forward from the beam axis (R) along the direction of movement (s) of the energy beam (AL) on the building area (8).

11. The method according to claim 1 or 2, wherein: The irradiation area (22) of the energy beam (AL) has a beam width (b) of at least 400 μm on the building area (8).

12. The method according to claim 1 or 2, wherein: The irradiation area (22) of the energy beam (AL) has a beam width (b) of at least 600 μm on the building area (8).

13. The method according to claim 1 or 2, wherein: The irradiation area (22) of the energy beam (AL) has a beam width (b) of at least 800 μm on the building area (8).

14. The method according to claim 1 or 2, wherein: In another irradiation mode, the energy beam (AL) is generated so as to weld the target area (Γ with a deep layer) Z ) causes the building material (13) to melt.

15. A method for controlling an apparatus (1) for additive manufacturing of a manufactured product (2), wherein: Based on the method according to any one of claims 1 to 14, control data (BSD, PSD) are generated for the device (1) and the device (1) is controlled using the control data (BSD, PSD).

16. A control data generating device (54, 54') for generating control data (BSD, PSD) for an apparatus (1) for additive manufacturing of a manufactured product (2) in a manufacturing process in which a building material (13) is built up and selectively cured, wherein: In order to perform curing on the building area (8), the building material (13) is irradiated with at least one energy beam (AL), wherein an irradiation surface (22) of the energy beam (AL) is moved over the building area (8) so that a target area (Γ) in or around the irradiation surface (22) is Z ), wherein the control data generating means (54, 54') is configured to determine the building material (13) in the target area (Γ) in order to generate the control data (BSD, PSD) for at least one irradiation mode. Z ) in the target area (Γ ) wherein heat conduction welding is performed in the target area (Γ Z ) causes the building material (13) to melt and determines at least one optimized intensity distribution curve (IO) of the energy beam (AL) in an optimization process based on the optimization criterion (OK) and / or auxiliary and / or boundary conditions (WB), wherein the energy beam (AL) at the irradiation surface (22) on the building zone (8) corresponds to the determined optimized intensity distribution curve (IO) or is at least as close as possible to the determined optimized intensity distribution curve (IO) except for certain tolerances, so that a desired local target temperature distribution (TV) is achieved, and wherein the optimized intensity distribution curve (IO) of the irradiation surface (22) of the energy beam (AL) on the building zone (8) is substantially non-rotationally symmetric about a beam axis (R) extending coaxially with the incident direction of the energy beam (AL), and wherein the control data (BSD, PSD) are generated so that when the device (1) for additive manufacturing is operated, the building material (13) is irradiated in the irradiation mode with the energy beam (AL) substantially having the determined intensity distribution curve.

17. A control mechanism (50) for an apparatus (1) for additive manufacturing of a manufactured product (2) in a manufacturing process in which a building material (13) is built up and selectively solidified, wherein: In order to perform curing on the building area (8), the building material (13) is irradiated with at least one energy beam (AL), wherein an irradiation surface (22) of the energy beam (AL) is moved over the building area (8) so that a target area (Γ) in or around the irradiation surface (22) is Z ) in which the building material (13) is melted, wherein the control mechanism (50) has a control data generating mechanism (54) according to claim 16 or a port to the control data generating mechanism (54') according to claim 16 to provide control data (BSD, PSD), and is constructed to control the device (1) for irradiating the building material (13) with the energy beam (AL) by using the control data (BSD, PSD).

18. A device (1) for additive manufacturing of a manufactured product (2) in an additive manufacturing process, comprising at least one input device (16) for introducing a building material (13) into a process space (3), an irradiation device (20) for selectively curing the building material (13) by irradiation with an energy beam (AL), and a control device (50) according to claim 17.

19. A computer program product having a computer program, which can directly download the computer program into a storage device of a control mechanism (50) of an apparatus (1) for additive manufacturing of a manufactured product (2), the computer program having program segments so that when the computer program is executed in the control mechanism (50), all steps of the method according to any one of claims 1 to 14 are performed.