Lithium-ion batteries with high-performance electrolytes and silicon oxide active materials
By using silicon oxide-based materials and graphite negative electrodes in lithium-ion batteries, combined with specific electrolytes and high tensile strength polymer binders, the problem of poor cycle stability of silicon-based negative electrode materials is solved, and high capacity and high energy density are achieved. long life battery performance.
Patent Information
- Application Number
- CN202010044645.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-30
- Filing Date
- 2020-01-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-01-15
AI Technical Summary
In existing lithium-ion batteries, silicon-based anode materials have poor cycle stability due to structural changes and volume expansion, and cannot effectively achieve high capacity and high energy density with long life.
Using a negative electrode containing silicon oxide-based materials and graphite, combined with a specific electrolyte combination such as non-aqueous solvents containing fluoroethylene carbonate, dimethyl carbonate and diethyl carbonate, high tensile strength polymer binders and nano-scale Conductive carbon to engineer lithium-ion batteries with remarkable cycle performance.
The long-term cycle stability of lithium-ion batteries under high discharge rates is achieved, and the capacity is maintained above 80% for more than 800 times, making it suitable for high-capacity applications such as electric vehicles.
Smart Images

Figure CN112151788B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. patent application No. 16 / 556,670 of the same name filed by Dong et al. on August 30, 2019, which claims priority to U.S. provisional patent application No. 62 / 866,978 of “Lithium-ion battery with high performance electrolyte and silicon oxide active material achieving very long cycle life performance” filed by Dong et al. on June 26, 2019, both of which are incorporated herein by reference.
[0003] Federally Funded Research and Development
[0004] This invention was made with government support under U.S. Government Grant Agreement No. DE-EE0006250 awarded by the U.S. Department of Energy under the Advanced Battery Alliance Program No. 18-2216-ABC. The government has certain rights in this invention. Technical Field
[0005] The present invention is directed to forming a battery utilizing an electrolyte which has been found to work in conjunction with a negative electrode incorporating a high capacity silicon oxide active material while achieving good cycling performance. Background Art
[0006] Lithium batteries are widely used in consumer electronics due to their higher energy density. For some current commercial batteries, the negative electrode material can be graphite, and the positive electrode material can include lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium iron phosphate (LiFePO4), lithium nickel oxide (LiNiO2), lithium cobalt nickel oxide (LiNiCoO2), lithium cobalt manganese nickel oxide (LiNiMnCoO2), lithium aluminum cobalt nickel oxide (LiNiCoAlO2), etc. For the negative electrode, lithium titanate is a substitute for graphite with good cycle properties, but it has a lower energy density. Other graphite substitutes such as tin oxide and silicon have the potential to provide improved energy density. However, it has been found that some high-capacity negative electrode materials are commercially unsuitable due to high irreversible capacity losses and poor discharge and recharge cycles associated with structural changes and abnormally large volume expansion, especially for silicon, which is related to lithium embedding / alloying. Structural changes and large volume changes may destroy the structural integrity of the electrode, thereby reducing the cycle efficiency. Summary of the invention
[0007] In a first aspect, the present invention relates to a lithium ion battery, the lithium ion battery comprising:
[0008] a negative electrode comprising about 75 wt % to about 92 wt % of an active material, about 1 wt % to about 7 wt % of nanoscale conductive carbon, and about 6 wt % to about 20 wt % of a polymer binder, wherein the active material comprises about 35 wt % to about 95 wt % of a silicon oxide-based material and about 5 wt % to about 65 wt % of graphite;
[0009] The positive electrode comprises lithium nickel cobalt manganese oxide, conductive carbon and a polymer binder, wherein the lithium nickel cobalt manganese oxide is approximately of the formula LiNi x Mn y Co z O2 represents, where x+y+z≈1, 0.3≤x, 0.025≤y≤0.35, 0.025≤z≤0.35;
[0010] a separator between the negative electrode and the positive electrode;
[0011] an electrolyte comprising about 1 M to about 2 M lithium salt and a non-aqueous solvent, wherein the non-aqueous solvent comprises at least about 5 volume % of fluoroethylene carbonate and at least about 25 volume % of a total amount of dimethyl carbonate, methylethyl carbonate, and diethyl carbonate; and
[0012] Container that encloses other battery components.
[0013] In another aspect, the present invention relates to a lithium ion battery, comprising:
[0014] a negative electrode comprising about 75 wt % to about 92 wt % of an active material, about 1 wt % to about 7 wt % of nanoscale conductive carbon, and about 6 wt % to about 20 wt % of a polymer binder, wherein the active material comprises about 40 wt % to about 95 wt % of a silicon oxide-based material and about 5 wt % to about 60 wt % of graphite;
[0015] A positive electrode comprising a nickel-rich lithium nickel cobalt metal oxide, conductive carbon and a polymer binder, wherein the nickel-rich lithium nickel cobalt oxide is approximately of the formula LiNi x M y Co z O2 represents, wherein x+y+z≈1, 0.3≤x, 0.025≤v≤0.35, 0.025≤z≤0.35, and M is Mn, Al, Mg, Sr, Ba, Cd, Zn, Ga, B, Zr, Ti, Ca, Ce, Y, Nb, Cr, Fe, V or a combination thereof;
[0016] a separator between the negative electrode and the positive electrode;
[0017] an electrolyte comprising about 1 M to about 2 M lithium salt and a non-aqueous solvent, wherein the non-aqueous solvent comprises at least about 5 volume % fluoroethylene carbonate and at least about 25 volume % of the total amount of dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate; and
[0018] Container that encloses other battery components.
[0019] In some embodiments, the lithium ion battery can be cycled for at least about 700 cycles at a charge rate of 1C and a discharge rate of 1C without a capacity decrease of no more than 20% relative to the 3rd cycle capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is an expanded view of a pouch battery, with the battery core separated from the two parts of the pouch case.
[0021] Figure 2 It is assembled Figure 1 A perspective bottom surface view of a pouch cell.
[0022] Figure 3 yes Figure 2 Bottom plan view of the pouch battery.
[0023] Figure 4 is a diagram of one embodiment of a battery cell including an electrode stack.
[0024] Figure 5 is a set of graphs of the specific discharge capacity (as a function of cycle number) of three button cell formats having a negative electrode containing a blend of silicon oxide / carbon composite particles and graphite and having a negative electrode containing LiNi 0.6 Mn 0.2 Co 0.2 O2(NMC622) or LiNi 0.8 Mn 0.1 Co 0.1 Positive electrodes of O2 (NMC811) cycled within the voltage window of (NMC622) 4.35V to 2.5V or 4.30V to 2.5V or (NMC811) 4.20V to 2.5V, resulting in the initial discharge capacities listed in the order from highest to lowest.
[0025] Figure 6 is used to generate Figure 5 A set of graphs of the normalized specific discharge capacity (as a function of cycle number) for three coin cells with the results plotted in .
[0026] Figure 7 is a graph of normalized capacity (as a function of cycle number) of coin cells cycled at a charge / discharge rate of 1C, the coin cells having NMC622 positive active material and SiOx composite / graphite mixed negative active material and formed using six different electrolytes, two of which contained ethylene carbonate and four of which did not contain ethylene carbonate.
[0027] Figure 8 In addition to cycling at a 2C charge / discharge rate, Figure 7 Plot of the normalized capacity as a function of cycle number for five equivalent coin cells used in.
[0028] Fig. 9 is a graph of the normalized capacity (as a function of cycle number) of coin cells cycled at a charge / discharge rate of 1 C, where one of the six electrolytes has a different amount of fluoroethylene carbonate as indicated in Table 3, as for Figure 7 The battery was formed as described.
[0029] Fig.10 is corresponding to Fig. 9 A graph of the unnormalized specific capacity relative to the positive electrode active material weight reference.
[0030] Fig.11 is a graph of the normalized capacity (as a function of cycle number) of coin cells cycled at a charge / discharge rate of 1 C, except that one of the six electrolytes with different amounts of dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate solvent as described in Table 3 was used. Figure 7 Batteries were formed as indicated.
[0031] Fig.12 Yes Fig.11 Plot of normalized capacity as a function of cycle number for an equivalent button cell used, where the cell was cycled at a charge / discharge rate of 2C.
[0032] Fig.13 is a graph of the normalized capacity (as a function of cycle number) of coin cells cycled at a charge / discharge rate of 1 C, except that one of the three electrolytes with optional additives was used, such as Figure 7 Batteries were formed as indicated.
[0033] Fig.14 is corresponding to Fig.13 A graph of the unnormalized specific capacity relative to the positive electrode active material weight reference.
[0034] Fig.15The NMC811 positive electrode active material and the Figure 7 A graph of the normalized capacity (as a function of cycle number) of button cells formed with the same negative electrode used in the battery, wherein the electrolyte is Electrolyte 2 in Table 3.
[0035] Fig.16 In the case of cycling at a charge / discharge rate of 2C, Fig.15 Plot of normalized capacity as a function of cycle number for the equivalent coin cells used.
[0036] Fig.17 is a front view of a pouch cell designed to operate at approximately 11 Ah.
[0037] Fig.18 yes Fig.17 Side view of a pouch cell.
[0038] Fig.19 Graph of the discharge capacity as a function of cycle number for two pouch cells cycled within the 4.3V to 2.3V voltage window using silicon oxide / carbon blended with graphite and NMC622 based cathodes.
[0039] Fig. 20 is used to generate Fig.19 The results in Figure 2 are graphs of the normalized discharge capacity (as a function of cycle number) of the two pouch cells.
[0040] Fig.21 is a graph of the capacity as a function of cycling for a cell using a positive electrode having NMC811 active material and an improved silicon oxide based negative electrode as described herein.
[0041] Fig. 22 is used to generate Fig.21 A graph of the normalized capacity of a battery as a function of cycles.
[0042] Fig.23 is a graph of the normalized capacity (as a function of cycle number) of pouch cells formed with NMC622 positive active material, SiOx composite graphite mixture negative active material and one of the three electrolyte formulations of Table 3 at a charge / discharge rate of 1C.
[0043] Fig.24 is used to generate Fig.23 A graph of the discharge capacity of a pouch cell as a function of cycle number.
[0044] Fig.25is a graph of normalized discharge capacity as a function of cycle for coin cells formed with positive electrodes having a blend of nickel-rich NCM and lithium- and manganese-rich NCM and with negative electrodes as used in the Examples, wherein the graph represents five different electrolytes.
[0045] Fig.26 is used to generate Fig.25 A graph of the unnormalized discharge capacity of a battery as a function of cycles. DETAILED DESCRIPTION
[0046] A new electrolyte composition has been discovered that provides unprecedented cycling performance for a battery including a negative electrode with a significant amount of silicon-based active material to achieve a high specific capacity. This achievement relies on early work that provides substantial improvements in negative electrode design, which provides a major leap in cycling performance. The new electrolyte formulation uses a significant amount of fluoroethylene carbonate solvent and does not contain other unstable components, and the other solvent components are appropriately selected to provide the stability achieved. In the negative electrode, the active material can be designed to include a blend with a silicon-based active material such as silicon oxide but without a significant graphite component. In addition, it has been found that the binder properties also contribute significantly to the cycling stability. In early work, for reasonable discharge rates and at high specific capacities, more than 600 cycles were obtained before reaching 80% of the initial capacity. In the case of further improved work herein, more than 800 cycles were obtained before reaching 80% of the initial capacity at reasonable discharge rates and at high specific capacities. Improved cycling performance is an important achievement for batteries used in electric vehicles.
[0047] Lithium has been used in both primary and secondary batteries. The striking features of lithium for battery or battery applications are its light weight and the fact that it is the most electropositive metal, and aspects of these features can also be advantageously carried in lithium-based batteries. Certain forms of metals, metal oxides, and carbon materials are known to incorporate lithium ions from electrolytes into their structures by embedding, alloying, or similar mechanisms. The positive electrode of a lithium-based battery typically contains an active material that is reversibly embedded / alloyed with lithium. A lithium-ion battery typically refers to a battery in which the negative electrode active material is also a lithium embedding / alloying material. Unless some clear distinctions are recorded, as used herein and for convenience, the terms cell and battery and variants thereof are used interchangeably.
[0048] The battery described herein is a lithium ion battery using a non-aqueous electrolyte solution containing lithium cations and suitable anions. For a secondary lithium ion battery during charging, oxidation occurs at the cathode (positive electrode), where lithium ions are extracted and electrons are released. During discharge, reduction occurs at the cathode, where lithium ions are inserted and electrons are consumed. Similarly, during charging, reduction occurs at the anode (negative electrode), where lithium ions are sucked in and electrons are consumed, and during discharge, oxidation occurs at the anode, where lithium ions and electrons are released. Unless otherwise specified, the performance values mentioned herein are at room temperature, i.e., about 23±2°C.
[0049] The word "element" is used herein in its conventional manner to refer to a member of the Periodic Table of the Elements, wherein if the element is in the composition, the element has the appropriate oxidation state, and wherein when stated to be in elemental form, the element is in its elemental form. 0 Thus, a metallic element is generally only a metal in its elemental form, or a suitable alloy of the metal in elemental form. In other words, except for metal alloys, metal oxides or other metal compositions are generally non-metals.
[0050] When a lithium-ion battery is in use, the absorption and release of lithium from the positive and negative electrodes causes structural changes in the electroactive materials. As long as these changes are reversible in nature, the capacity of the material does not change with cycling. However, it has been observed that the capacity of the active material decreases to varying degrees with cycling. Therefore, after a number of cycles, the performance of the battery drops below an acceptable value and the battery is replaced. In addition, there is usually an irreversible capacity loss in the first cycle of the battery, which is significantly greater than the capacity loss per cycle in subsequent cycles. The irreversible capacity loss (IRCL) is the difference between the charge capacity and the first discharge capacity of a new battery. Lithium metal oxide-based positive electrodes may exhibit some IRCL, which results in some compensation of the negative electrode with respect to the lithium available for cycling. The irreversible capacity loss may result in a corresponding decrease in the capacity, energy and power of the battery due to changes in the battery materials during the initial cycle.
[0051] Elemental silicon and other silicon-based active materials have attracted a great deal of attention as potential negative electrode materials due to their very high specific capacity for uptake and release of lithium relative to that of silicon. Elemental silicon forms alloys with lithium that can theoretically have lithium contents corresponding to greater than 4 lithium atoms per silicon atom (e.g., Li 4.4Si). Therefore, the theoretical specific capacity of silicon is on the order of 4000 to 4400 mAh / g, which is significantly greater than the theoretical capacity of graphite of about 370 mAh / g. It is believed that lithium is embedded in graphite to a level of about 1 lithium atom for 6 carbon atoms (LiC6). In addition, elemental silicon, silicon alloys, silicon composites, etc. can have a low potential relative to lithium metal similar to graphite. However, silicon undergoes a very large volume change when alloyed with lithium. Large volume expansions of the order of two to three times or more of the original volume have been observed, and large volume changes are associated with a significant reduction in the cycle stability of batteries with silicon-based negative electrodes. It has also been found that silicon suboxides (i.e., SiO x , x<2) is an ideal active material for lithium-based batteries, which in some embodiments can have a high specific capacity relative to lithium alloying. The reference to silicon suboxide provides recognition of silicon dioxide as a fully oxidized form of silicon. Unless otherwise specified, for convenience, silicon suboxides may generally be referred to as silicon oxides, which are not limited to silicon monoxide (SiO).
[0052] In an embodiment of particular interest, the silicon-based active material may comprise elemental silicon and / or silicon suboxide as the primary active material. Silicon suboxides have been found to be particularly effective for achieving longer cycle stability. In order to stabilize the silicon-based active material and to improve conductivity, carbon may be incorporated into the composite active material. For carbon composites with nanoscale elemental silicon and / or silicon oxide, long-term cycle stability is still rare, although the applicant has achieved moderate cycle stability for consumer electronics applications. Based on a mixture of electroactive graphite and silicon-based composites together with other electrode design improvements, longer cycle stability is described herein. As discussed in detail below, stable silicon-based electrodes may also comprise additional conductive sources, such as nanoscale carbon and improved binder blends that also make outstanding contributions to cycle stability.
[0053] Although the improved electrode design has significantly improved cycle performance, it has been found that further cycle stabilization can be achieved due to the improved electrolyte formulation.The improved electrolyte is based on a solvent comprising at least 5% by volume fluoroethylene carbonate and at least 25% by volume dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate or their mixture.In addition, in some embodiments, the electrolyte should be substantially free of ethylene carbonate.The electrolyte also comprises an electrolyte salt of about 1M to about 2M.
[0054] Fluorinated solvents have been found to be particularly useful for silicon-based active materials. Previous results have been obtained using commercial electrolytes containing specialized fluorinated solvents, as described in co-pending U.S. patent application Ser. No. 15 / 948,160 to Venkatachalam et al., entitled "Electrodes with silicon oxide active materials for lithium-ion batteries achieving high capacity, high energy density and long cycle life performance," now published as US 2019 / 0207209A1 (hereinafter referred to as the '209 application), which is incorporated herein by reference. The use of fluoroethylene carbonate as a solvent suitable for low temperature battery performance was recognized in published US patent application 2013 / 0157147 to Li et al., entitled "Low capacity electrodes for high capacity lithium-based batteries," (hereinafter referred to as the '147 application), which is incorporated herein by reference.
[0055] The effects of using fluoroethylene carbonate in forming a solid electrolyte interphase layer are described in Markevich et al., "Fluoroethylene Carbonate as an Important Component for the Formation of an Effective Solid Electrolyte Interphase on Anodes and Cathodes for Advanced Li-Ion Batteries," ACS Energy letters 2017, 2, 1137-1345, which is incorporated herein by reference. The Markevich article demonstrates the utility of silicon nanowire-based anodes. The primary focus of the Markevich article is on use with high voltage cathodes compared to ethylene carbonate-based electrolytes. The work herein extends the earlier work of the '147 application in combination with excellent electrode formation to achieve unprecedented silicon-based battery performance. In particular, the present work demonstrates that FEC-based electrolytes are effectively used at high loadings for silicon oxide / graphite blend anodes and commercially suitable electrode designs.
[0056] The active materials used in the lithium ion secondary battery herein generally include, for example, positive electrode (i.e., cathode) active materials having a moderately high average voltage relative to lithium and silicon-based active materials for the negative electrode (i.e., anode). Generally, a variety of cathode materials can be used. For example, commercially available cathode active materials can be used with existing commercial production availability. Such cathode active materials include, for example, lithium cobalt oxide (LiCoO2), LiNi 1 / 3 Mn 1 / 3 Co 1 / 3O2 (L333 or NMC111), LiNiCoAlO2 (NCA), other lithium nickel manganese cobalt oxides (NMC), LiMn2O4 (lithium manganese oxide spinel), their modified forms or their mixtures.
[0057] Nickel-rich lithium nickel cobalt manganese oxide (LiNi x Mn y Co z O2, 0.45≤x, 0.05≤y, z≤0.35) may be of interest due to lower cost and lower flammability risk relative to lithium cobalt oxide and the ability to cycle at higher voltages. The following results are presented: nickel-rich lithium nickel manganese cobalt oxide active materials paired with improved silicon-based negative electrodes form batteries with excellent cycling stability. In addition, for example, in U.S. Patent 8,389,160, entitled "Positive Electrode Materials for Lithium Ion Batteries with High Discharge Specific Capacity and Methods for Synthesizing These Materials" by Venkatachalam et al. (hereinafter referred to as the '160 patent) and U.S. Patent 8,465,873, entitled "Positive Electrode Materials for High Discharge Capacity Lithium Ion Batteries" by Lopez et al. (hereinafter referred to as the '873 patent), lithium metal oxide materials with high specific capacity that have a layered crystal structure and are rich in lithium relative to a LiMO2 (M=non-lithium metal) reference composition are described, both of which are incorporated herein by reference. These materials can be referred to as high capacity manganese-rich compositions (HCMRs) TM ). In addition, a blend of lithium-rich + manganese-rich NMC and nickel-rich NMC positive active compositions may be used.
[0058] Specifically, the desired cycling results can be obtained from nickel-rich lithium nickel manganese cobalt oxide (N-NMC), which can be made of the formula LiNi x Mn y Co z O2 represents, where x ≥ 0.3 and x + y + z ≈ 1. Commercially available preparations of these compounds include, for example, LiNi 0.33 Mn 0.33 Co 0.33 O2 (BASF and Targray (Canada)), LiNi 0.5 Mn 0.3 Co 0.2 O2(BASF), LiNi 0.6 Mn 0.2 Co 0.2 O2 (Targray (Canada), Umicore (Belgium), and L&F (South Korea)), LiNi 0.8 Mn 0.1 Co 0.1O2 (Targray, Canada, LG Chem, Umicore (Belgium) and L&F Corporation (South Korea)). In the industry, both NCM and NMC are currently used interchangeably when listing cobalt and manganese in the corresponding order, and at this time, the statements are equivalent and are based solely on personal preference.
[0059] As mentioned above, silicon-based electrodes present challenges in obtaining cycles suitable for commercial applications. For consumer electronics applications, a reasonable cycle target may be about 250-450 cycles without unacceptable performance loss, but for vehicles and similar larger capacity applications, greater cycle stability is required. Applicants have achieved a battery design suitable for consumer electronics applications that can achieve suitable performance by using silicon-based anodes. These batteries are described in the published U.S. patent application 2015 / 0050535 (hereinafter referred to as the '535 application) by Amiruddin et al., which is incorporated herein by reference. The new battery design herein provides cycles that exceed the target cycle stability for consumer electronics and achieves performance suitable for vehicles and other high-capacity applications.
[0060] Regarding silicon, oxygen-deficient silicon oxide, such as silicon oxide SiO x , 0.1≤x≤1.9, can be embedded in lithium / alloyed with lithium, so that oxygen-deficient silicon oxide can act as an active material in a lithium-based battery. Silicon oxide can be doped with a relatively large amount of lithium so that the material can exhibit a large specific capacity. However, it is also generally observed that the capacity of silicon oxide decays faster as the battery cycles. Commercial silicon-based materials containing SiO that can be composited with carbon and silicon nanocrystals from some suppliers can be obtained from AlfaAesar (USA), Sigma-Aldrich (USA), Shin-Etsu (Japan), Osaka Titanium Corporation (Japan) and Nanostructured and Amorphous Materials Corp. (USA). Other specific suitable formulations of silicon-based compositions are further described below. The applicant has achieved cyclic stability of silicon oxide-based active materials by using the electrode formulation described herein. In some embodiments, it may be desirable to have a negative electrode comprising a combination of graphite carbon active materials and silicon-based active materials to extend the cycle life at an acceptable specific capacity reduction, and the excellent cycle performance herein uses such an active material blend.
[0061] In order to achieve the results described herein, the negative electrode includes a plurality of design improvements, which can be considered to provide improved cycle performance independently or in combination, and at least for some embodiments, the combination of specific electrode features can provide unexpected synergistic performance improvements for longer cycle stability. The electrolyte described herein further utilizes these electrode improvements. In particular, the negative electrode can be designed to have a high tensile strength while introducing a composite binder with some elongation capabilities. It has been found that nano-scale conductive carbon such as carbon nanotubes, carbon black, carbon nanofibers or their combination as conductive electrode additives improves the cycle of the negative electrode using silicon-based active materials. These features can be combined with the design of electrode load and density that provide good energy density class performance for the resulting consumer electronics battery design. The cycle can be further improved by adding supplementary lithium to the battery and / or by adjusting the balance of the active materials in each electrode.
[0062] The graphite component of the active material blend in the negative electrode can provide conductivity. However, it is found that an appropriate amount of nanoscale carbon can further stabilize the negative electrode in terms of cycling. The nanoscale carbon can be in the form of carbon nanotubes, carbon nanofibers, or carbon nanoparticles such as carbon black. As described in U.S. Pat. No. 9,190,694 B2, entitled "High Capacity Anode Materials for Lithium Ion Batteries" by Lopez et al. and U.S. Pat. No. 9,780,358 B2, entitled "Battery Design Using High Capacity Anode Materials and Cathode Materials" by Masarapu et al., the usefulness of nanoscale conductive carbon for the cycling stability of silicon-based negative electrodes has been previously discovered, both of which are incorporated herein by reference. Typically, the electrode contains at least about 1% by weight of nanoscale conductive carbon to achieve stable cycling.
[0063] In lithium-ion batteries, reactive lithium for cycling is usually provided in the positive electrode active material, which is transferred to the negative electrode during the initial charge of the battery and then available for discharge of the battery there. Silicon-based negative electrodes may generally exhibit large irreversible capacity losses during the first charge of the battery. The capacity loss may generally be associated with corresponding irreversible material changes during the first charge of the battery. For example, as a result of the reaction with the typical electrolyte used in the battery, a solid electrolyte interface (SEI) layer is formed together with the negative electrode active material. If a stable SEI layer is formed, the SEI layer can stabilize the battery during the cycle. It can be inferred that other irreversible changes occur with respect to the silicon-based active composition. The first cycle irreversible capacity loss is generally significantly greater than any per-cycle capacity loss associated with subsequent cycles of the battery, although the second, third, and other cycles may also have larger per-cycle capacity losses because the initial changes are carried into the previous few cycles rather than being completed completely in the first cycle. Large irreversible capacity loss (IRCL) may reduce the cycle capacity and the energy output and power output of the battery during the cycle. In larger format cells, capacity may increase at lower cycle numbers due to practical effects, which may be, for example, improved penetration of electrolyte through the electrode stack.
[0064] In order to reduce the loss of energy output and power output of the battery due to irreversible capacity loss, supplementary lithium can be added to provide additional lithium to the battery. The introduction of supplementary lithium can reduce the introduction of cathode active materials that are not cycled due to active lithium capacity loss associated with IRCL. Supplementary lithium refers to active lithium that is directly or indirectly introduced into the battery to replace lithium lost by irreversible processes and provide other beneficial effects, which is different from the positive electrode active material. Applicants have found that supplementary lithium provided in an amount greater than the amount corresponding to compensating for irreversible capacity loss can further stabilize the cycle. In the case where the positive electrode active material is lithium-rich + manganese-rich nickel-manganese-cobalt oxide, the cycle stabilization is described in U.S. Patent No. 9,166,222 (hereinafter referred to as the '222 patent) entitled "Lithium Ion Battery Using Supplementary Lithium" by Amiruddin et al., which is incorporated herein by reference.
[0065] A variety of methods for introducing supplemental lithium can be used, including, for example, adding a lithium active material (e.g., lithium metal powder or foil) to the negative electrode, adding a sacrificial lithium source to the positive electrode, including a sacrificial lithium electrode into the battery structure, electrochemical pre-lithiation of the negative electrode, and the like. These methods are further described in the '222 patent and in U.S. Pat. No. 9,190,694, entitled "High Capacity Anode Materials for Lithium Ion Batteries" to Lopez et al. (hereinafter referred to as the '694 patent), both of which are incorporated herein by reference. In some embodiments, it has been found that electrochemical methods can be convenient, such as the methods described in the published PCT application WO 2013 / 082330 to Grant et al. entitled "Methods for Alkylating Anodes", which is incorporated herein by reference. Generally, supplemental lithium can be introduced in an amount to compensate for a portion of the irreversible capacity loss, nearly all of the irreversible capacity loss, or an amount greater than the irreversible capacity loss, but it is generally not more than 30% of the capacity of the negative electrode active material higher than the irreversible capacity loss. In some embodiments, the supplemental lithium can compensate for about 90% to about 200% of the anode first cycle irreversible capacity loss.
[0066] The applicant's previous work has found that the circulation of silicon-based anodes is significantly facilitated by the use of high tensile strength polymer binders, which can be satisfied by appropriate polyimides. Specifically, the tensile strength of the polymer binder can be at least about 60MPa. In order to extend the cycle stability even longer, it is found that polymer binder blends can provide further improved cycle performance. One component of the polymer binder blend can be a high tensile strength polymer, such as polyimide, and the second polymer can have a lower Young's modulus (elastic modulus) value to provide a more elastic polymer, such as polyvinylidene fluoride, carboxymethyl cellulose, styrene-butadiene rubber, lithiated polyacrylic acid or a mixture thereof. While providing tensile strength, the polymer binder should also provide good adhesion so that the electrode remains laminated with the collector. The required blend can include at least about 50% by weight of a high tensile strength polymer and at least about 5% by weight of a polymer binder, the Young's modulus of the polymer binder not exceeding about 2.4GPa and the elongation for some embodiments is at least about 35%.
[0067] Anode design typically involves a balance of multiple factors to achieve a target capacity while still providing a reasonable cycle. The incorporation of an ideal electrolyte herein significantly further extends cycle stability. As seen in the results in the following examples, a battery with a silicon-based anode active material is able to cycle more than seven hundred and fifty cycles while maintaining more than 80% of the battery capacity. At the same time, a realistic negative electrode design can be matched with a reasonable positive electrode design to achieve good cycling and high energy density values. The following describes in detail the balance of battery design and design features used to achieve these achievements.
[0068] Typically, the battery design described herein can be suitable for cylindrical batteries or more rectangular or prismatic style batteries. Cylindrical batteries typically have a wound electrode structure, while prismatic batteries can have wound or stacked electrodes. Typically, in order to achieve the desired performance using a suitable electrode design in terms of electrode load and density, the battery can include multiple electrodes of various polarities, which can be stacked together with the separator material between the battery electrodes. The winding of the electrode can provide a similar effect with a reasonable internal resistance due to the good stacking of the electronic conductivity and ion mobility and the electrodes in a suitable container. The size of the battery generally affects the total capacity and energy output of the battery. The design described herein is based on obtaining an ideal high energy density while providing an ideal cycle of a battery based on a silicon-based active material.
[0069] By discovering an improved electrolyte formulation, a significant extension of cycling stability has been achieved. In particular, cells with significant amounts of silicon-based active materials have been cycled at least 800 times without the capacity dropping below 80% of the third cycle capacity at a C discharge rate. The resulting cycling stability is suitable for use in electric vehicle applications and similar high capacity uses.
[0070] General Battery Characteristics
[0071] The negative electrode structure and the positive electrode structure can be assembled into a suitable battery. As further described below, the electrodes are generally formed in conjunction with a current collector to form an electrode structure. A separator is positioned between the positive electrode and the negative electrode to form a battery. The separator is electrically insulating while providing at least selected ion conduction between the two electrodes. A variety of materials can be used as separators. Some commercial separator materials can be formed from polymers such as polyethylene and / or polypropylene, which are porous sheets prepared for ion conduction. Commercial polymer separators include, for example, those from Asahi Kasei (Japan). A series of separator materials. In addition, ceramic-polymer composites have been developed for separator applications. These ceramic composite separators can be stable at higher temperatures, and the composites can reduce the risk of fire. Polymer-ceramic composites for lithium-ion battery separators are marketed under the trademark of Evonik Industries (Germany). and Tiejin Lielsort Korea Co., Ltd. Sold. In addition, a porous polymer sheet coated with a gel-forming polymer can be used to form a separator. Such a separator design is further described in U.S. Pat. No. 7,794,511 B2, entitled "Battery Separator for Lithium Polymer Batteries" by Wensley et al., which is incorporated herein by reference. Suitable gel-forming polymers include, for example: polyvinylidene fluoride (PVDF), polyurethane, polyethylene oxide (PEO), polypropylene oxide (PPO), polyacrylonitrile, gelatin, polyacrylamide, polymethyl acrylate, polymethyl methacrylate, polyvinyl acetate, polyvinyl pyrrolidone, polytetraethylene glycol diacrylate, copolymers thereof, and mixtures thereof.
[0072] The electrolyte provides ion transport between the anode and cathode of the battery during the charge and discharge process. The electrolyte used in lithium-ion batteries contains a non-aqueous solvent and a lithium salt. The improved electrolyte for silicon-based electrodes is described in detail below. The electrolyte is usually poured into the battery before the housing is sealed.
[0073] Electrodes as described herein can be assembled into a variety of commercial battery / battery designs, such as prismatic batteries, wound cylindrical batteries, button cells or other reasonable battery / battery designs. The battery can include a single pair of electrodes or multiple pairs of electrodes assembled with one or more parallel and / or series electrical connections. The electrode stack can have additional electrodes to end the stack with the same polarity as the other end of the stack, so as to facilitate placement in a container. Although the electrode structure as described herein can be used in a battery for one or single charge purposes, the resulting battery generally has an ideal cycle performance for secondary battery purposes during multiple cycles of the battery.
[0074] In some embodiments, the positive electrode and the negative electrode can be stacked together with the separator between them, and the resulting stacked structure can be rolled into a cylindrical or prismatic configuration to form a battery structure. Suitable conductive tabs can be welded to or connected to the current collector in a similar manner, and the resulting jellyroll structure can be placed in a metal can or polymer packaging, wherein the negative tab and the positive tab are welded to suitable external contacts. Electrolyte is added to the can, and the can is sealed to complete the battery. Some currently used rechargeable commercial batteries include, for example: cylindrical 18650 batteries (18 mm in diameter and 65 mm in length) and 26700 batteries (26 mm in diameter and 70 mm in length), but other battery / battery sizes and prismatic batteries and foil bag batteries / batteries of selected sizes can be used.
[0075] Pouch cells can be particularly desirable for a variety of applications, including certain vehicle applications, due to their stacking convenience and lower container weight. Pouch cell designs for automotive batteries incorporating high capacity cathode active materials are further described in U.S. Pat. No. 8,187,752 to Buckley et al., entitled "High Energy Lithium Ion Secondary Battery," and U.S. Pat. No. 9,083,062 B2 to Kumar et al., entitled "Battery Pack for Vehicles and High Capacity Pouch Secondary Battery for Incorporation into Compact Battery Packs," both of which are incorporated herein by reference. Although the pouch cell design is particularly convenient for use in a particular battery pack design, pouch cells can also be effectively used in other situations.
[0076] Figures 1 to 4 A representative embodiment of a pouch cell is shown in FIG. In this embodiment, the pouch cell 100 includes a pouch housing 102, an electrode core 104, and a pouch cover 106. The electrode core is discussed further below. The pouch housing 102 includes a cavity 110 and an edge 112 surrounding the cavity. The cavity 110 has a size such that the electrode core 104 can fit within the cavity 110. The pouch cover 106 can be sealed around the edge 112 to seal the electrode core 104 within a sealed cell, such as Figure 2 and 3 Terminal tabs 114 , 116 extend outwardly from the sealed bag for electrical contact with the electrode core 104 . Figure 3 It is taken along line 3-3 Figure 2 Schematic diagram of a cross section of a battery. Various additional embodiments of pouch cells with differently configured edges and seals are possible.
[0077] Figure 4An embodiment of an electrode core 104 that generally includes an electrode stack is shown. In this embodiment, the electrode stack 130 includes negative electrode structures 132, 134, 136, positive electrode structures 138, 140, and separators 150, 152, 154, 156 disposed between adjacent positive and negative electrodes. The separator can be provided as a single folded sheet, and the electrode structure is placed in the separator fold. The negative electrode structures 132, 134, 136 include negative electrodes 160, 162, negative electrodes 164, 166, and negative electrodes 168, 170 disposed on both sides of the collectors 172, 174, 176, respectively. The positive electrode structures 138, 140 include positive electrodes 180, 182, and positive electrodes 184, 186 disposed on opposite sides of the collectors 188, 190, respectively. Tabs 192, 194, 196, 198, 200 are connected to current collectors 172, 188, 174, 190, 176, respectively, to facilitate connection of the respective electrodes in series or in parallel. For vehicle applications, the tabs are typically connected in parallel so that tabs 192, 196, 200 will be electrically connected to an electrical contact accessible outside the container, and tabs 194, 198 will be electrically connected to an electrical contact accessible outside the container as the opposite pole.
[0078] The electrode stack may have an additional negative electrode so that both outer electrodes adjacent to the container are negative electrodes. Typically, a battery having stacked electrodes of the size described herein has 5 to 40 negative electrode elements (active material is coated on both sides of the current collector), and in further embodiments has 7 to 35 negative electrode elements, wherein the number of corresponding positive electrode elements is generally one less than the number of negative electrode elements. Those of ordinary skill in the art will recognize that additional ranges of electrode numbers within the above-defined ranges are to be considered and within the present disclosure.
[0079] As described above, the wound electrodes can be used for cylindrical cells or roughly prismatic cells, respectively. Wound cells for cylindrical lithium-ion batteries are further described in U.S. Pat. No. 8,277,969, entitled “Lithium-ion Secondary Battery,” to Kobayashi et al., which is incorporated herein by reference. Prismatic cells with wound electrodes are described in U.S. Pat. No. 7,700,221 (the '221 patent), entitled “Electrode Assembly and Lithium-ion Secondary Battery Using the Electrode Assembly,” to Yeo et al., which is incorporated herein by reference. Kobayashi's '969 patent and Yeo's '221 patent do not describe how to achieve reasonable cycling or high energy density with silicon-based active materials. For example, the design of a prismatic cell with wound electrodes is further described in the '221 patent cited above. The specific design of the stacked electrode group or wound cell may be affected by the target size and target capacity of the battery.
[0080] The improved negative electrode can be used for a variety of applications and battery / battery designs. For an electrode stack, the area of the electrode can be reasonably selected based on the volume and design constraints of a specific application. The following discussion focuses on larger batteries that are typically designed for vehicle applications such as drones, cars, trucks, or other vehicles. However, the improved negative electrode described herein can be effectively used for consumer electronics applications that can be based on smaller battery forms. In addition, it should be noted that vehicles can use smaller consumer electronics batteries, and Tesla cars are currently famous for using thousands of small consumer electronics batteries in their battery packs. Typically, larger forms of batteries / batteries can achieve a larger energy density within a specific range. Positive active materials can be ideally selected based on specific applications to balance multiple considerations such as energy density.
[0081] For selecting electrode parameters, the design of high gravimetric energy density batteries can combine considerations of multiple factors such as electrode area, number of electrode structures and balance of battery capacity. Electrode area refers to the spatial extent of one of the electrodes along one side of the current collector. Figure 1 The length "L" of the electrode is depicted, and Figure 3 The width "W" of the electrode is depicted. As shown, the area of the electrode can be defined as L x W. In some embodiments, the area of each electrode can be similar so that the size of the battery including the electrode stack can have a length and width similar to the length and width of each electrode in the stack. In some embodiments, the separator can be in the form of a sheet with an area slightly larger than the area of the electrode, and in some embodiments, the separator can be folded, pleated, or formed to have a pocket, wherein the electrode is placed in the fold or pocket of the separator.
[0082] Electrolytes
[0083] The inventors refer to solutions containing solvated ions as electrolytes, and ionic compositions that dissolve in a suitable liquid to form solvated ions are referred to as electrolyte salts. Electrolytes for lithium-ion batteries may include one or more selected lithium salts, a non-aqueous solvent, and optional additives. The electrolytes required to achieve the unprecedented cycling described herein have appropriately selected solvents and specifically avoid ingredients that have been found to reduce cycling performance.
[0084] Suitable lithium salts generally have inert anions. Suitable lithium salts include, for example, lithium hexafluorophosphate, lithium hexafluoroarsenate, bis(trifluoromethylsulfonyl imide) lithium, lithium trifluoromethanesulfonate, tris(trifluoromethylsulfonyl) methyl lithium, lithium tetrafluoroborate, lithium perchlorate, lithium tetrachloroaluminate, lithium chloride, lithium difluoro oxalate borate, and combinations thereof. Lithium hexafluorophosphate and lithium tetrafluoroborate are of particular interest. In some embodiments, the electrolyte comprises a lithium salt at a concentration of about 1 M to about 2 M, in further embodiments comprising about 1.1 M to about 1.9 M and in other embodiments comprising about 1.25 M to about 1.8 M. One of ordinary skill in the art will recognize that additional ranges of lithium salt concentrations within the above-specified ranges are to be considered and are within the present disclosure.
[0085] For lithium-ion batteries of interest, non-aqueous liquids are typically used to dissolve one or more lithium salts in a non-aqueous solvent. The solvent typically does not dissolve the electroactive material. Solvent selection is important for the electrolytes described herein, which provide unexpectedly improved cycling performance. Typically, the solvent comprises about 5 wt % to about 30 wt % of fluoroethylene carbonate (FEC), in further embodiments comprising about 7 wt % to about 27 wt % and in further embodiments comprising about 8 wt % to about 25 wt % of FEC. Accordingly, the solvent is typically substantially free of ethylene carbonate, as it has been found that ethylene carbonate is detrimental to cycling. Ethylene carbonate is a room temperature solid with a melting point of about 35° C. Fluoroethylene carbonate melts near room temperature, i.e., 18-23° C. In addition, it has been found that electrolytes with fluoroethylene carbonate have excellent low temperature performance as described in the '147 application cited above.
[0086] Electrolyte solvents also include room temperature liquid components usually, and the solvent of special concern also includes straight-chain carbonate and optional additives.Ideal straight-chain carbonate includes for example dimethyl carbonate, methyl ethyl carbonate and diethyl carbonate.In some embodiments, the total volume that dimethyl carbonate, methyl ethyl carbonate and diethyl carbonate contribute to solvent can be about 50 volume % to about 95 volume %, about 55 volume % to about 92.5 volume % in further embodiments and about 60 volume % to about 91 volume % total contribution from dimethyl carbonate, methyl ethyl carbonate and diethyl carbonate in other embodiments.In some embodiments, solvent is mainly composed of fluoroethylene carbonate and one or more selected from dimethyl carbonate, methyl ethyl carbonate and diethyl carbonate.Those of ordinary skill in the art will recognize that the other scope of the solvent component in the above-mentioned clear and definite scope will be considered and in the present disclosure.
[0087] In some embodiments, the solvent may also include propylene carbonate and / or fluorobenzene. If any one or two of these optional solvent components are present, the solvent may typically independently include one or two of these solvent components of about 0.5 volume % to about 12 volume %, about 0.75 volume % to about 10 volume % in further embodiments, and about 1 volume % to about 8 volume % in other embodiments. Although the PC or FB solvent components do not significantly change the cycle performance, these solvent components may be ideal for processing advantages such as reducing gas formation. Those of ordinary skill in the art will recognize that additional ranges of PC and / or FB solvent concentrations within the above-mentioned clear ranges are to be considered and within the present disclosure.
[0088] Typically, the solvent may include other minor components typically no more than about 20% by volume of these other solvent components, no more than about 10% by volume in some embodiments, about 0.01% by volume to about 5% by volume in other embodiments, and about 0.1% by volume to about 1% by volume in further embodiments. One of ordinary skill in the art will recognize that additional ranges of solvent components within the above-defined ranges are to be considered and within the present disclosure. In some embodiments, other suitable solvent components that may optionally exist in minor amounts include, for example: 2-methyltetrahydrofuran, dioxolane, tetrahydrofuran, γ-butyrolactone, dimethyl sulfoxide, acetonitrile, formamide, dimethylformamide, triethylene glycol dimethyl ether (tri(ethylene glycol) dimethyl ether), diethylene glycol dimethyl ether (diethylene glycol dimethyl ether), DME (monoethylene glycol dimethyl ether or 1,2-dimethyloxyethane or ethylene glycol dimethyl ether), nitromethane, and mixtures thereof. Other minor fluorinated solvent components may include, for example, fluorinated ethylene carbonate, monochloroethylene carbonate, monobromoethylene carbonate, 4-(2,2,3,3-tetrafluoropropoxymethyl)-[1,3]dioxolane-2-one, 4-(2,3,3,3-tetrafluoro-2-trifluoromethyl-propyl)-[1,3]dioxolane-2-one, 4-trifluoromethyl-1,3-dioxolane-2-one, bis(2,2,3,3-tetrafluoro-propyl) carbonate, bis(2,2,3,3,3-pentafluoro-propyl) carbonate, or mixtures thereof. Additional fluorinated secondary solvent components include, for example, fluorinated ethers as described in published U.S. patent applications 2018 / 0062206 to Li et al., entitled “Fluorinated Ethers as Electrolyte Co-Solvents for Lithium Metal-Based Anodes” and WO 2018 / 051675 to Takuya et al., entitled “Lithium Secondary Batteries,” both of which are incorporated herein by reference.
[0089] It has been found that commonly used solvent compounds that are generally considered to be ideal solvent components for lithium-ion batteries are not conducive to the improved cycling of the electrodes described herein. Specifically, ethylene carbonate is generally excluded from the electrolytes described herein. Therefore, the electrolyte generally contains no more than 0.1% by volume of ethylene carbonate.
[0090] Electrode structure
[0091] The electrodes of a battery contain active materials as well as a binder and a conductive additive. The electrodes are formed into sheets, dried and pressed to achieve the desired density and porosity. The electrode sheets are usually formed directly on a metal collector such as a metal foil or a thin metal grid. For a variety of battery structures, electrode layers are formed on both sides of the collector to provide ideal performance in an assembled battery or battery pack. The electrode layers on each side of the collector can be considered elements of the same electrode structure because they are at the same potential in the battery, but the collector itself, although part of the electrode structure, is not usually considered to be part of the electrode because it is electrochemically inert. Therefore, reference to the physical aspects of an electrode generally refers to a layer of electrode composition within the electrode structure. A conductive collector can facilitate the flow of electrons between the electrode and an external circuit.
[0092] In some embodiments, when the positive or negative electrode uses a high load level, the density of the electrode can be reduced to provide good electrode cycle stability. The density of the electrode is a function of the pressing pressure within a reasonable range. Generally, the density of the electrode cannot be increased arbitrarily without sacrificing the performance of the load level and achieving the desired cycle performance and the capacity at a higher discharge rate at the same time. The features of a specific negative electrode layer and a positive electrode layer are provided in the following section.
[0093] In some embodiments, the current collector can be formed of nickel, aluminum, stainless steel, copper, etc. The electrode material can be cast onto the current collector as a film. The electrode material with the current collector is then dried, for example, in an oven, to remove the solvent from the electrode. In some embodiments, the dried electrode material in contact with the current collector foil or other structure can be subjected to about 2 to about 10 kg / cm 2(kg / cm2) pressure. The thickness of the current collector for the positive electrode can be about 5 microns to about 30 microns, about 10 microns to about 25 microns in other embodiments, and about 14 microns to about 20 microns in further embodiments. In one embodiment, the positive electrode uses an aluminum foil current collector. The thickness of the current collector for the negative electrode can be about 2 microns to about 20 microns, about 4 microns to about 14 microns in other embodiments, and about 6 microns to about 10 microns in further embodiments. In one embodiment, the negative electrode uses copper foil as a current collector. Those of ordinary skill in the art will recognize that additional ranges of current collector thickness within the above-defined ranges are to be considered and are within the present disclosure.
[0094] negative electrode
[0095] The basic electrode design includes a blend of an active composition, a polymer binder and a conductive diluent. As described above, in some embodiments, the improved electrode design may involve a blend of a polymer binder blend and an active composition and a nano-scale conductive carbon additive. In some embodiments, the active material blend may include a majority of silicon-based active materials such as silicon oxide composites and at least 10% by weight of distinct graphite. In addition, it has been found that the stabilization of the electrode cycle using silicon-based active materials can be obtained by using a blend of a polyimide providing high mechanical strength and a portion of a more deformable polymer that still provides good electrode performance in a synergistic binder blend. Although graphite can provide conductivity to the electrode, it has also been found that in some embodiments, a certain amount of distinct nano-scale conductive carbon can be important for the ability to produce a long-cycled negative electrode. Typically, nano-scale conductive carbon is not considered to be electrochemically active, while graphite is electrochemically active. These improved design aspects are then combined into electrodes that further have previously discovered silicon-based electrode improvements.
[0096] Significant attention has been directed toward high capacity negative electrode active materials based on silicon. For cells containing significant amounts of silicon, silicon-based active materials have generally not achieved cycling stability suitable for automotive use. The '535 application has demonstrated successful cycling suitable for consumer electronics applications, among others, with cycling up to about 200 to 300 cycles at values of at least 80% of the initial capacity. Applicants have been particularly successful in cycling stability, which has been achieved using materials based primarily on silicon oxide composites. In this article, electrodes are provided that can be successfully cycled for more than 600 cycles at reasonable rates over a large voltage range without the capacity dropping below 80%. Thus, the present work is directed to extending the cycling stability to a range suitable for automotive use.
[0097] As described herein, improved cycling results are obtained using active compositions blended with silicon-based active materials and graphitic carbon. Typically, the total capacity of the negative electrode blended active material can be at least about 750 mAh / g, at least about 900 mAh / g in further embodiments, at least about 1000 mAh / g in other embodiments, and at least about 1100 mAh / g in other embodiments, at a rate of C / 3 relative to lithium metal from 5 millivolts (mV) to 1.5 V. The blended active material can contain at least about 40% by weight of silicon-based active material, at least about 50% by weight of silicon-based active material in further embodiments, about 55% by weight to about 95% by weight of silicon-based active material in other embodiments, and about 60% by weight to about 90% by weight of silicon-based active material in other embodiments. Accordingly, the blended active material may contain from about 5 wt % graphite to about 65 wt % graphite, in further embodiments from about 7 wt % graphite to about 60 wt % graphite, in other embodiments from about 8 wt % graphite to about 55 wt %, and in other embodiments from about 10 wt % graphite to about 50 wt % graphite. One of ordinary skill in the art will recognize that additional ranges of specific discharge capacities and concentrations of silicon-based active materials within the above explicit ranges are to be considered and are within the present disclosure.
[0098] As described above and described in detail below, suitable silicon-based active materials may include composites with carbon components. Silicon-based active materials are discussed in detail in the following sections. Unlike blends involving mixtures held together by polymer binders, composites refer to granular materials whose components are closely combined into an integral material with effective uniformity within an appropriate scale. Composite components may include, for example, silicon, oxygen, carbon, etc. Although it is not desired to be limited by theory, it is generally believed that the carbon component of the composite with silicon is electrochemically active and is generally not graphitic, although considering the close combination in the composite, activity is an abstract concept, and the crystal structure may be extremely complex and difficult to evaluate. In any case, it is easy for a person of ordinary skill in the art to understand that the carbon component of the composite material is distinguishable from the graphite in the composite that is not in the active material blend. The following examples are based on commercial composite compositions that are believed to contain mainly silicon suboxides with some amount of elemental silicon crystals and elemental carbon in the combined composite granular material.
[0099] Graphite is commercially available in natural and synthetic forms, and suitable graphites include natural graphite or synthetic graphite, etc. Graphite is a crystalline form of carbon with flake covalently bonded carbon. As used herein, graphite refers to graphitic carbon that does not require perfect crystallinity, and some natural graphite materials may have some crystalline impurities. However, graphite generally refers to a material dominated by a graphite structure, as will be recognized in the art. Graphite is conductive along the planes of the covalent carbon sheets stacked in the crystal. Crystalline carbon in graphite form can be intercalated with lithium, so that it is a determined electrochemically active material for lithium-ion batteries.
[0100] The average particle size of the graphite particles can be from about 1 micron to about 30 microns, from about 1.5 microns to about 25 microns in further embodiments, and from about 2 microns to about 20 microns in other embodiments. Generally, it is desirable for graphite not to include particles larger than the thickness of the electrode to avoid an uneven electrode surface, and graphite particles having a size significantly smaller than a micron may be less crystalline. In some embodiments, the D50 (mass median diameter) of the graphite carbon can be from about 5 microns to about 50 microns, from about 7 microns to about 45 microns in further embodiments, and from about 8 microns to about 40 microns or from about 10 microns to 40 microns in other embodiments. In addition, in some embodiments, the BET surface area of the graphite carbon active material (which can be evaluated according to ISO 4652) can be about 1 m 2 / g to about 100m 2 / g, in further embodiments about 5m 2 / g to about 85m 2 / g, and in other embodiments about 7.5m 2 / g to about 60m 2 / g. One of ordinary skill in the art will recognize that other ranges of particle size and surface area of graphitic carbon active materials are contemplated and are within the present disclosure. In contrast, conductive carbon black, etc. (which are referred to as paracrystalline) typically has a surface area of at least about 40 m 2 / g to 1000m 2 / g or greater.
[0101] Regarding polymer binders, applicants have obtained reasonable cycles of silicon-based batteries using high tensile strength binders such as polyimide binders. See U.S. Patent 9,601,228 (hereinafter referred to as the '228 patent) entitled "Silicon Oxide High Capacity Anode Materials for Lithium Ion Batteries" by Deng et al., which is incorporated herein by reference. In some embodiments where longer cycle stability is obtained, it has been unexpectedly found that polymer binder blends further stabilize the cycle. In particular, a second polymer or combination of polymers providing a lower elastic modulus (corresponding to greater elasticity) can be blended with a high tensile strength polyimide. The binder blend typically comprises at least about 50% by weight of polyimide, at least about 55% by weight in further embodiments, and about 60% by weight to about 95% by weight of polyimide in other embodiments. Similarly, the binder blend generally comprises at least about 5% by weight of a polymer with a relatively low elastic modulus, at least about 10% by weight in a further embodiment, and about 12% by weight to about 40% by weight of a polymer with a relatively low elastic modulus in other embodiments, as further described below. One of ordinary skill in the art will recognize that the additional range of polymer amounts within the above-mentioned clear and distinct ranges will be considered and within the present disclosure. The polymer of the blend can be selected to be soluble in the same solvent.
[0102] Polyimides are polymers based on repeating units of the imide monomer structure. The polyimide polymer chain can be aliphatic, but for high tensile strength applications, the polymer backbone is typically aromatic, with the polymer backbone extending along the N atoms of the polyimide structure. For silicon-based anodes that exhibit significant morphological changes during cycling, heat-curable polyimide polymers have been found to be ideal for high capacity negative electrodes, likely due to their high mechanical strength. The following table provides suppliers of high tensile strength polyimide polymers and the names of the corresponding polyimide polymers.
[0103]
[0104] The tensile strength of polyimide polymer can be at least about 60MPa, at least about 100MPa in further embodiments, and at least about 125MPa in other embodiments. Some commercial polyimides with high tensile strength can also have higher elongation values, which are the amount of elongation borne before the polymer tears. In some embodiments, the elongation of polyimide can be at least about 40%, at least about 50% in further embodiments, and at least about 55% in other embodiments. Tensile strength and elongation values can be measured according to the ASTM D638-10 standard test method for the tensile properties of plastics or the ASTM D882-91 standard test method for the tensile properties of thin plastic sheets, both of which are incorporated herein by reference. Based on the values reported by commercial suppliers, the results from these alternative ASTM schemes of polyimide look similar to each other. Those of ordinary skill in the art will recognize that the other scope of polymer properties within the above-mentioned clear range is to be considered and within the present disclosure.
[0105] Suitable more flexible polymer components can be selected to be inert in the electrochemistry of the battery and compatible with processing using polyimide. In particular, suitable more flexible polymer components include, for example: polyvinylidene fluoride (PVdF), carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), lithiated polyacrylic acid (LiPAA) or mixtures thereof. Regarding polymer properties, some important properties for high capacity negative electrode applications are summarized in the following table.
[0106] Binder Elongation Tensile strength(MPa) Elastic modulus(GPa) PVDF 5-50% 30-45 1.0-2.5 Polyimide 30-100% 60-300 2.5-7 CMC 30-40% 10-15 1-5 SBR 400-600% 1-25 0.01-0.1 LiPAA 1-6% 90 1-4
[0107] PVDF refers to polyvinylidene fluoride, CMC refers to sodium carboxymethylcellulose, SBR refers to styrene-butadiene rubber, and LiPAA refers to lithiated polyacrylic acid. PVDF, CMC and SBR are commercially available from a variety of sources. LiPAA can be made from LiOH and commercial polyacrylic acid (PAA). For example, a stoichiometric amount of LiOH can be added to a solution of PAA in an amount of one mole of LiOH per monomer unit of PAA. The formation and use of LiPAA are further described in Li et al., "Lithium polyacrylate as a binder for tin-cobalt-carbon negative electrodes in lithium-ion batteries", Electrochemica Acta 55 (2010) 2991-2995, which is incorporated herein by reference.
[0108] Elongation refers to the elongation percentage before the polymer tears. Generally, in order to adapt to silicon-based materials, it is necessary to have an elongation of at least about 30%, at least about 50% in some embodiments and at least about 70% in further embodiments. For polymer binder blends, for more elastic polymer binder components, it may be necessary to have an elastic modulus (alternatively, referred to as Young's modulus or tensile modulus) of no more than about 2.4 GPa, no more than about 2.25 GPa in further embodiments, no more than about 2 GPa in other embodiments and no more than about 1.8 GPa. Those of ordinary skill in the art will recognize that the other range of more elastic polymer component properties within the above-mentioned clear range is to be considered and within the present disclosure.
[0109] In order to form an electrode, the powder can be blended with the polymer in a suitable liquid such as a solvent for dissolving the polymer. Polyimide and PVdF can usually be processed in N-methylpyrrolidone (NMP), although other suitable organic solvents can be used. Water-processable polyimides are commercially available, and these water-processable polyimides are suitable for blending with various other polymers. The granular components of the electrode, i.e., active materials and nano-scale conductive carbon, can be blended with a polymer binder blend in a solvent to form a paste. The resulting paste can be pressed into an electrode structure.
[0110] The active material loading in the binder can be large. In some embodiments, the negative electrode has about 75% by weight to about 92% by weight of the negative electrode active material, about 77% by weight to about 90% by weight of the negative electrode active material in other embodiments, and about 78% by weight to about 88% by weight of the negative electrode active material in further embodiments. In some embodiments, the negative electrode has about 6% by weight to about 20% by weight of the polymer binder, about 7% by weight to 19% by weight of the polymer binder in other embodiments, and about 8% by weight to 18% by weight of the polymer binder in further embodiments. In addition, in some embodiments, the negative electrode comprises about 1% by weight to about 7% by weight of nano-scale conductive carbon, about 1.5% by weight to about 6.5% by weight in further embodiments, and about 2% by weight to about 6% by weight of nano-scale conductive carbon in other embodiments. Those of ordinary skill in the art will recognize that the additional range of polymer loading within the above-mentioned clear range is to be considered and within the present disclosure.
[0111] For the improved cycle of the negative electrode, it has been found that nano-scale carbon additives or combinations thereof are particularly desirable. Nano-scale conductive carbon generally refers to particles of high surface area elemental carbon having at least two sizes of submicron primary particles. Suitable nano-scale conductive carbons include, for example, carbon black, carbon nanotubes, and carbon nanofibers. In some embodiments, the nano-scale conductive carbon additives used in the negative electrode may include carbon nanotubes, carbon nanofibers, carbon nanoparticles (e.g., carbon black), or a combination thereof. In some embodiments, in order to achieve improved performance, the conductive additive may have a conductivity of at least about 40S / cm, at least about 50S / cm in some embodiments, and at least about 60S / cm in further embodiments. Those of ordinary skill in the art will recognize that additional ranges of particle loading and conductivity within the above-mentioned clear ranges are to be considered and within the present disclosure.
[0112] Conductivity, which is the inverse of resistivity, may be reported by the distributor and is usually measured using a specific technique developed by the distributor. For example, the resistance of carbon black is measured between two copper electrodes with a Super P TM Carbon black, see Imerys Graphite & Carbon, A Synopsis of Analytical Procedures, 2019
[0113] (http: / / www.imerys-graphite-and-carbon.com / wordpress / wp-app / uploads / 2019 / 02 / Analytical-Procedures_Web_21Feb19.pdf). Suitable supplemental conductive additives may also be added to facilitate longer term cycling stability. Alternatively, some suppliers describe a conductive carbon concentration that achieves a conductive percolation threshold.
[0114] Carbon black refers to a synthetic carbon material and may be alternatively referred to as acetylene black, furnace black, thermal black or other names indicating the method of synthesis. Carbon black usually refers to amorphous carbon, but refers to small domains with short or medium range sequences corresponding to the crystal structures of graphite or diamond in at least some forms of carbon black, but for practical purposes the material can be considered to be amorphous. Under ISO Technical Specification 80004-1 (2010), carbon black is a nanostructured material. The primary particles of carbon black can be on the order of tens of nanometers or less, but the primary particles are generally hard fused into chains or other aggregates, and the smallest dispersible unit can be considered to be about 80nm to 800nm, which is still submicron. Carbon blacks are commercially available and have been synthesized to provide the desired level of conductivity, such as (Imerys), (AkzoNobel), Shawinigan (Chevron-Phillips) and Black Pearls (Cabot).
[0115] Carbon nanofibers are high aspect ratio fibers that typically include graphene layers in the form of plates, cones, or other shapes, and carbon nanotubes include graphene sheets folded into tubes. Carbon nanofibers can have diameters below 250 nm and are commercially available, for example, Carbon nanofibers (Pyrograf Products, Inc.), or from American Elements, Inc. Carbon nanotubes have been found to be ideal conductive additives that can improve the cycling performance of the positive or negative electrode. Single-walled or multi-walled carbon nanotubes can also be obtained from American Elements, Inc, (CA, USA), Cnano Technologies (China), Fuji, Inc. (Japan), Alfa Aesar (MA, USA) or NanoLabs (MA, USA).
[0116] The negative electrode for the battery described herein can have a high active material loading level and a reasonably high electrode density. For a specific active material loading level, density is inversely related to thickness, so that an electrode with a greater density is thinner than an electrode with a lower density. The loading amount is equal to the density multiplied by the thickness. In some embodiments, the negative electrode of the battery has a negative electrode active material loading level of at least about 1.5 mg / cm 2 , in other embodiments about 2 mg / cm 2 About 8mg / cm 2 , in other embodiments about 2.5 mg / cm 2 About 6 mg / cm 2 , and in other embodiments about 3 mg / cm 2 to about 4.5 mg / cm 2 In some embodiments, the active material density of the negative electrode of the battery is about 0.5 g / cc (cc = cubic centimeter (cm 3 )) to about 2 g / cc, in other embodiments about 0.6 g / cc to about 1.5 g / cc, and in other embodiments about 0.7 g / cc to about 1.3 g / cc. Similarly, the average dry thickness of the silicon oxide-based electrode can be at least about 15 microns, in further embodiments at least about 20 microns, and in other embodiments about 25 microns to about 75 microns. The resulting silicon oxide-based electrode can exhibit at least about 3.5 mAh / cm 2In further embodiments, at least about 4.5 mAh / cm 2 and in further embodiments at least about 6 mAh / cm 2 One of ordinary skill in the art will recognize that additional ranges of active material loading levels and electrode densities within the explicit ranges above are contemplated and are within the present disclosure.
[0117] High Capacity Silicon Anode Materials
[0118] Typically, the battery designs herein are based on high-capacity anode active materials. Specifically, when cycled from 0.005V to 1.5V relative to lithium metal at a rate of C / 10, the specific capacity of the positive active material is typically at least about 800mAh / g, at least about 900mAh / g in further embodiments, at least about 1000mAh / g in other embodiments, at least about 1150mAh / g in some embodiments, and at least about 1400mAh / g in other embodiments. As implied, the specific capacity of the negative electrode active material can be evaluated in a battery with a lithium metal counter electrode. However, in the battery described herein, when cycled relative to a high-capacity lithium metal oxide positive electrode active material, the negative electrode can exhibit a reasonably comparable specific capacity. In a battery with a non-lithium metal electrode, the specific capacity of each electrode can be evaluated by dividing the battery capacity by the weight of each active material. As described herein, ideal cycling results can be obtained using a combination of silicon-based active materials and graphite carbon active materials, and good capacity is observed.
[0119] Elemental silicon, silicon alloys, silicon composites, etc. can have a low potential relative to lithium metal similar to graphite. However, elemental silicon generally undergoes a very large volume change when alloyed with lithium. Large volume expansions of the order of two to four times the original volume or more have been observed, and large volume changes are associated with significant reductions in the cycling stability of batteries with silicon-based negative electrodes.
[0120] Commercially available silicon suboxides, composites of elemental silicon and carbon can be used in the cells described herein. In addition, other formulations of silicon-based negative electrode active materials with high capacity and reasonable cycle performance have been developed. Some silicon-based compositions are described below, which provide possible and promising alternatives to commercially available SiO-based compositions. It is found that the improved electrolyte formulations described herein are particularly effective for silicon-based negative electrode active materials and blends of silicon-based active materials with graphite.
[0121] In addition, silicon-based high-capacity materials in the negative electrode of lithium-based batteries may exhibit large irreversible capacity loss (IRCL) in the first charge / discharge cycle of the battery in some formulations. The high IRCL of silicon-based anodes can consume a large portion of the capacity available for the energy output of the battery. Since the cathode (i.e., the positive electrode) supplies all of the lithium in conventional lithium-ion batteries, a high IRCL in the anode (i.e., the negative electrode) may result in a low-energy battery. In order to compensate for the large anode IRCL, supplemental lithium can be added directly or indirectly to the negative electrode material to offset the IRCL. The use of supplemental lithium to improve the performance of silicon-based electrodes is also described in the '694 patent and the '228 patent, both of which are cited above and incorporated herein by reference. The use of supplemental lithium in improved battery designs is further described below.
[0122] The anode (i.e., negative electrode) of the battery described herein can use nanostructured active silicon-based materials to better adapt to volume expansion and thereby maintain the mechanical electrode stability and cycle life of the battery. Nanostructured silicon-based negative electrode compositions are disclosed in the '694 application, the '228 patent, and U.S. Pat. No. 9,139,441 (the '441 patent) entitled "Porous silicon-based anode materials formed using metal reduction" by Anguchamy et al. (these are incorporated herein by reference). Suitable nanostructured silicon may include, for example, nanoporous silicon and nanogranular silicon. In addition, nanostructured silicon may be formed into a composite with carbon and / or into an alloy with other metal elements. The goal of the design of improved silicon-based materials is to further stabilize the negative electrode material during the cycle process while maintaining a high specific capacity and, in some embodiments, reducing the irreversible capacity loss in the first charge and discharge cycle. In addition, it has been observed that pyrolytic carbon coatings stabilize silicon-based materials in terms of battery performance.
[0123] Ideal high-capacity negative electrode active materials may include porous silicon (pSi)-based materials and / or composites of porous silicon-based materials. Typically, pSi-based materials include highly porous crystalline silicon, which can provide high surface area and / or high void volume relative to bulk silicon. Although nanostructured porous silicon can be formed by a variety of methods such as electrochemical etching of silicon wafers, particularly good battery performance has been obtained from nanostructured porous silicon obtained by metal reduction of silicon oxide powder. In particular, the material has particularly good cycle performance while maintaining a high specific capacity. The formation of a composite of a pSi-based material with a carbon-based material or metal can additionally stabilize the negative electrode mechanically to improve cycling. Additional descriptions of pSi-based materials from silicon oxide reduction can be found in the '441 patent cited above.
[0124] With regard to composite materials, nanostructured silicon components can be combined with, for example, carbon nanoparticles and / or carbon nanofibers in a compact composite material. For example, the components can be ground to form a composite in which the materials are tightly associated. Typically, it is believed that the association has mechanical characteristics, such as a softer silicon coated on a harder carbon material or mechanically attached to a harder carbon material. In an additional or alternative embodiment, silicon can be ground together with a metal powder to form an alloy, which can have a corresponding nanostructure. The carbon component can be combined with a silicon-metal alloy to form a multi-component composite.
[0125] In addition, carbon coatings can be applied to silicon-based materials to improve conductivity, and carbon coatings are shown to stabilize silicon-based materials in terms of improving cycles and reducing irreversible capacity loss. Ideal carbon coatings can be formed by pyrolyzing an organic composition. The organic composition can be pyrolyzed at a higher temperature, such as about 800°C to about 900°C, to form a hard amorphous coating. In some embodiments, the desired organic composition can be dissolved in a suitable solvent such as water and / or a volatile organic solvent for combination with a silicon-based component. The dispersion can be fully mixed with the silicon-based composition. After the mixture is dried to remove the solvent, the dry mixture of the silicon-based material coated with a carbon precursor can be heated in an oxygen-free atmosphere to pyrolyze an organic composition such as an organic polymer, some lower molecular solid organic compositions, and the like, and thereby form a carbon coating.
[0126] Regarding silicon, oxygen-deficient silicon oxide, such as silicon oxide SiO x , 0.1≤x≤1.9, can be embedded in lithium / alloyed with lithium so that the oxygen-deficient silicon oxide can function as an active material in a lithium-ion battery. These oxygen-deficient silicon oxide materials are generally referred to as silicon oxide-based materials, and in some embodiments may contain different amounts of silicon, silicon oxide, and silicon dioxide. The oxygen-deficient silicon oxide can be doped with a relatively large amount of lithium so that the material can exhibit a large specific capacity. However, it is observed that silicon oxide generally has a capacity that decreases rapidly with battery cycling, as observed for elemental silicon.
[0127] Silicon oxide based compositions have been formed into composite materials with high capacity and very good cycling performance, as described in the '228 patent cited above. In particular, oxygen deficient silicon oxide can be formed into composites with conductive materials such as conductive carbon or metal powders, which surprisingly significantly improves cycling while providing high specific capacity values. In addition, grinding silicon oxide into smaller particles such as submicron structured materials can further improve the performance of the material.
[0128] In general, a variety of composites may be used and may include silicon oxide, carbon components such as graphite particles (Gr), inert metal powders (M), elemental silicon (Si), especially nanoparticles, pyrolytic carbon coatings (HC), carbon nanofibers (CNF), or combinations thereof. The component structure may or may not correspond to the structure of the components in the composite material. Thus, the general composition of the composite may be expressed as Among them α, β, χ, δ, ε and is a relative weight and can be chosen so that Typically, 0.35<α<1, 0≤β<0.6, 0≤χ<0.65, 0≤δ<0.65, 0≤ε<0.65, and Certain subgroups of these composite ranges are of particular interest. In some embodiments, composites having SiO and one or more carbon-based components are desirable and can be represented by the formula αSiO-βGr-χHC-εCNF, where 0.35<α<0.9, 0≤β<0.6, 0≤χ<0.65, and 0≤ε<0.65 (δ=0 and ), in further embodiments 0.35<α<0.8, 0.1≤β<0.6, 0.0≤χ<0.55, and 0≤ε<0.55, in some embodiments 0.35<α<0.8, 0≤β<0.45, 0.0≤χ<0.55, and 0.1≤ε<0.65, and in other embodiments 0.35<α<0.8, 0≤β<0.55, 0.1≤χ<0.65, and 0≤ε<0.55. In additional or alternative embodiments, a composite having SiO, an inert metal powder, and optionally one or more conductive carbon components can be formed, which can be represented by the formula αSiO-βGr-χHC-δM-εCNF, wherein 0.35<α<1, 0≤β<0.55, 0≤χ<0.55, 0.1≤δ<0.65, and 0≤ε<0.55. In further additional or alternative embodiments, a composite of SiO with elemental silicon and optionally one or more conductive carbon components may be formed, which may be represented by the formula represents, where 0.35<α<1, 0≤β<0.55, 0≤χ<0.55, 0≤ε<0.55, and And in a further embodiment 0.35<α<1, 0≤β<0.45, 0.1≤χ<0.55, 0≤ε<0.45, and One of ordinary skill in the art will recognize that additional ranges within the explicit ranges above are to be considered and are within the present disclosure. As used herein, reference to a composite implies the application of significant binding forces, such as by HEMM grinding, to intimately associate the materials, as opposed to simple blending which is not considered to form a composite.
[0129] In published U.S. Patent Application 2014 / 0308585 by Han et al., entitled “Silicon-based active materials for lithium-ion batteries and synthesis using solution processing,” a method for synthesizing various Si-SiO x A solution-based method for preparing a Si-CM (M=metal) composite is described in published U.S. Patent Application 2014 / 0370387 to Anguchamy et al., entitled "Silicon-Silicon Oxide-Carbon Composite for Lithium Battery Electrode and Method of Forming the Composite," which is incorporated herein by reference. The battery in the examples uses a SiO-containing carbon composite believed to contain SiO x -Si-C or SiO x -Commercial materials of Si composites.
[0130] The capacity of the anode significantly affects the energy density of the battery. In batteries of the same output, the higher the specific capacity of the anode material, the lower the weight of the anode. When the negative electrode is made of a silicon-based material, the discharge specific capacity of the electrode at a rate of C / 3 relative to lithium metal from 1.5V to 5mV can be about 800mAh / g to 2500mAh / g, about 900mAh / g to about 2300mAh / g in further embodiments, and about 950mAh / g to about 2200mAh / g in other embodiments. Those of ordinary skill in the art will recognize that additional ranges of discharge specific capacity within the above-specified ranges are to be considered and are within the present disclosure.
[0131] positive electrode
[0132] With the improved negative electrode described above, a variety of positive electrode chemistries can be effectively introduced. The selected composition can be blended into the positive electrode together with a suitable binder and conductive material. This section focuses on positive electrode active materials that are particularly ideal for high-voltage cycling and moderately high capacity. In addition, this section describes the overall electrode composition and properties.
[0133] To some extent, the desired application of the final battery can influence the choice of the positive electrode composition. From this perspective, a wide range of compositions are described below. For automotive use and for similar applications, it has been found that specific positive electrode chemistry is ideal for achieving high energy density and cycling to more than 600 cycles while maintaining at least 80% capacity, although some materials provide promising results with slightly lower cycle stability. Specifically, it is found that nickel-rich lithium nickel manganese cobalt oxide provides very long-lasting cycle performance based on the improved electrolyte described herein. In an alternative embodiment, a blend of nickel-rich lithium nickel manganese cobalt oxide and (lithium + manganese)-rich lithium nickel manganese cobalt oxide is blended to provide reasonable positive electrode performance. In addition, when paired with the silicon-based negative electrode described herein, the nickel-rich lithium nickel manganese cobalt oxide alone as an active material can provide an ideally high energy density due to the average discharge voltage with good cycling. An example of a separate nickel-rich lithium nickel manganese cobalt oxide is provided below.
[0134] Nickel-rich lithium nickel manganese cobalt oxide (N-NMC) can provide desirable cycling and capacity performance for the lithium-ion batteries described herein. In particular, the nickel-rich composition can be approximately represented by the formula LiNi x Mn y Co z O2 represents, x+y+z≈1, 0.45≤x, 0.025≤y, z≤0.35, in further embodiments, 0.50≤x, 0.03≤y, z≤0.325, and in further embodiments, 0.55≤x, 0.04≤v, z≤0.3. The amount of nickel can affect the selected charging voltage, thereby balancing the cycle stability and discharge energy density. For values of x in the range of 0.525≤x≤0.7, the selected charging voltage can be 4.25V to 4.375V. For values of x in the range of 0.7≤x≤0.9, the selected charging voltage can be 4.05V to 4.325V. Those of ordinary skill in the art will recognize that additional ranges of compositions within the above-specified ranges and selected charging voltages are to be considered and within the present disclosure. It has been found that these compositions provide relatively stable higher voltage cycles, good capacity and ideal impedance. N-NMC powders can be synthesized using techniques such as co-precipitation as described further below, and are commercially available, for example, from BASF (Germany), TODA (Japan), L&F Materials Corp. (South Korea), Umicore (Belgium), and Jinhe Materials Corp. (China).
[0135] For N-NMC compositions, the average voltage tends to be slightly higher with increasing amounts of nickel, but the charge voltage for stable cycling tends to be slightly lower with increasing nickel. Thus, there may be a tradeoff with active material selection, although N-NMC active materials can provide good cycling and reasonably high capacity and energy density.
[0136] As mentioned above, an ideal blend may include N-NMC and (lithium-rich + manganese-rich) lithium nickel manganese cobalt oxide (LM-NMC or ). These compositions can be approximated by the formula Li 1+b Ni α MnβCo γ A δ O 2-z F z , wherein b+α+β+γ+δ≈1, b is in the range of about 0.04 to about 0.3, α is in the range of 0 to about 0.4, β is in the range of about 0.2 to about 0.65, γ is in the range of 0 to about 0.46, δ is in the range of about 0 to about 0.15, and z is in the range of 0 to 0.2, provided that α and γ are not simultaneously 0, and wherein A is a metal other than lithium, manganese, nickel, and cobalt. In some embodiments, A may be Mg, Sr, Ba, Cd, Zn, Al, Ga, B, Zr, Ti, Ca, Ce, Y, Nb, Cr, Fe, V, or a combination thereof. Additionally or alternatively, wherein 0.05≤b≤0.125, 0.225≤α≤0.35, 0.35≤β≤0.45, 0.15≤γ≤0.3, 0≤δ≤0.05 and Li with up to 5 mol % oxygen 1+b Ni α Mn β Co γ A δ O2 may be replaced with a fluorine dopant. One of ordinary skill in the art will recognize that additional ranges of composition within the explicit ranges above are to be considered and are within the present disclosure. Long-term cycling stability has been achieved at higher cycling voltages for (lithium + manganese)-rich NMC active materials, as described in U.S. Pat. No. 8,928,286, entitled "Extremely Long Cycling of Lithium Batteries with Lithium-Rich Cathode Materials" by Amiruddin et al., which is incorporated herein by reference.
[0137] LM-NMC cathode materials can advantageously be synthesized by coprecipitation and sol-gel processes detailed in the '160 patent and the '873 patent. In some embodiments, the cathode material is synthesized by precipitating a mixed metal hydroxide or carbonate composition from a solution containing +2 cations, wherein the hydroxide or carbonate composition has a selected composition. The metal hydroxide or carbonate precipitate is then subjected to one or more heat treatments to form a crystalline layered lithium metal oxide composition. The carbonate coprecipitation process described in the '873 patent yields the desired lithium-rich metal oxide material having cobalt in the composition and exhibiting high specific capacity performance as well as excellent tap density. These patents also describe the effective use of metal fluoride coatings to improve performance and cycling.
[0138] It was found that for LM-NMC positive active materials, the coating on the material can improve the performance of the corresponding battery. Suitable coating materials that are generally considered to be electrochemically inert during battery cycling may include metal fluorides, metal oxides, or halides of metal non-fluorides. The results for LM-NMC in the following examples were obtained using LM-NMC materials coated with metal fluorides. Improved metal fluoride coatings with suitably designed thicknesses are described in U.S. Patent 9,843,041, entitled "Coated Positive Electrode Materials for Lithium Ion Batteries" by Lopez et al., which is incorporated herein by reference. For example, suitable metal oxide coatings are further described in U.S. Patent 8,535,832B2, entitled "Metal Oxide Coated Positive Electrode Materials for Lithium Batteries" by Karthikeyan et al., which is incorporated herein by reference. The discovery of non-fluoride metal halides as ideal coatings for cathode active materials is described in U.S. Patent No. 8,663,849 B2 to Venkatachalam et al., entitled "Metal Halide Coatings on Lithium Ion Battery Cathode Materials and Corresponding Batteries," which is incorporated herein by reference.
[0139] With respect to active material blends for positive electrodes, the active material may comprise from about 3 wt % to about 85 wt % LM-NMC, in further embodiments from about 5 wt % to about 75 wt % LM-NMC, in further embodiments from about 6 wt % to about 70 wt % LM-NMC, and in other embodiments from about 7 wt % to about 65 wt % LM-NMC. Similarly, in the positive electrode active material blend, the active material may comprise from about 15 wt % to about 97 wt % N-NMC, in further embodiments from about 25 wt % to about 95 wt %, in further embodiments from about 30 wt % to about 94 wt %, and in other embodiments from about 35 wt % to about 93 wt % N-NMC. The positive electrode active material may optionally comprise 0 to 25 wt % of additional active materials, such as lithium cobalt oxide, LiNi 0.33 Mn 0.33 Co 0.33 O2(NMC111), LiNi 0.8 Co 0.15 Al 0.05 O2(NCA), mixtures thereof, etc. One of ordinary skill in the art will recognize that additional ranges of composition blends within the explicit ranges above are contemplated and within the present disclosure.
[0140] As described above, the positive electrode generally comprises an active material, and a conductive material in a binder. The active material load in the electrode can be large. In some embodiments, the positive electrode comprises about 85% to about 99% of the positive electrode active material, about 90% to about 98% of the positive electrode active material in other embodiments, and about 95% to about 97.5% of the positive electrode active material in further embodiments. In some embodiments, the positive electrode has about 0.75% to about 10% of a polymer binder, about 0.8% to about 7.5% of a polymer binder in other embodiments, and about 0.9% to about 5% of a polymer binder in further embodiments. The positive electrode composition may also generally include a conductive additive different from the electroactive composition. In some embodiments, the positive electrode may have 0.4% to about 12% by weight of a conductive additive, about 0.45% to about 7% by weight in further embodiments, and about 0.5% to about 5% by weight of a conductive additive in other embodiments. Those of ordinary skill in the art will recognize that additional ranges of particle loading within the above-defined ranges are to be considered and are within the present disclosure. The positive electrode active material is described above. Suitable polymer binders for positive electrodes include, for example, polyvinylidene fluoride, polyethylene oxide, polyimide, polyethylene, polypropylene, polytetrafluoroethylene, polyacrylates, rubbers such as ethylene-propylene-diene monomer (EPDM) rubber or styrene-butadiene rubber (SBR), their copolymers or their mixtures. For positive electrodes, good results can be obtained using polyvinylidene fluoride (PVDF), and the positive electrodes in the embodiments use PVDF binders. Conductive additives for negative electrodes are described in detail, and nano-scale conductive carbon can be effectively used for positive electrodes.
[0141] For a particular loading level, the electrode density (of active material) is inversely related to the thickness, such that an electrode with a greater density is thinner than an electrode with a lower density. The loading level is equal to the density multiplied by the thickness. In some embodiments, the positive electrode of the battery has a positive electrode active material loading level of about 10 to about 40 mg / cm 2 , in other embodiments from about 12 to about 37.5 mg / cm 2 , in other embodiments from about 13 to about 35 mg / cm 2 , and in other embodiments 20 to about 32.5 mg / cm 2. In some embodiments, the active material density of the positive electrode of the battery is from about 2.5 g / cc to about 4.6 g / cc in some embodiments, from about 3.0 g / cc to 4.4 g / cc in other embodiments, and from about 3.25 g / cc to about 4.3 g / cc in other embodiments. In further embodiments, the thickness of the positive electrode on each side of the collector after compression and drying of the positive electrode active material can be from about 45 microns to about 300 microns, from about 80 microns to about 275 microns in some embodiments, and from about 90 microns to about 250 microns in other embodiments. Those of ordinary skill in the art will recognize that other ranges of active material loading levels, electrode thicknesses, and electrode densities within the above explicit ranges are to be considered and are within the present disclosure.
[0142] Lithium supplementation
[0143] The improved high energy battery designs described herein generally include supplemental lithium, and this section relates to methods for incorporating supplemental lithium of appropriate embodiments. Generally, the inclusion of supplemental lithium is ideal for batteries with silicon-based negative electrode active materials because the materials exhibit higher irreversible capacity losses during the initial charge of the battery. In addition, the supplemental lithium unexpectedly also stabilizes the cycle of the LM-NMC. A variety of methods can be used to introduce supplemental lithium into the battery, although after the corresponding initial reaction and / or charging, the negative electrode becomes associated with excess lithium for cycling from the supplemental lithium. With respect to the negative electrode in a battery with supplemental lithium, after the first cycle and after additional cycles, the structure and / or composition of the negative electrode may change relative to its initial structure and composition.
[0144] According to the method for introducing the supplementary lithium, the positive electrode may initially contain a source of supplementary lithium, and / or a sacrificial electrode containing supplementary lithium may be introduced. Additionally or alternatively, the supplementary lithium may be associated with the negative electrode. In some embodiments, unlike pure chemical or mechanical methods, an electrochemical method may be used to introduce the supplementary lithium into the negative electrode. If the supplementary lithium is initially located in the positive electrode or a separate electrode, the negative electrode may be in an unchanged form in the absence of lithium until the battery is charged, or at least until the circuit between the negative electrode and the electrode with supplementary lithium is closed in the presence of an electrolyte and a separator. For example, in addition to other electrode components, the positive electrode or supplementary electrode may contain elemental lithium, lithium alloys, and / or other sacrificial lithium sources.
[0145] If sacrificial lithium is included in the positive electrode, lithium from the sacrificial lithium source is loaded into the negative electrode during the charging reaction. The voltage during charging based on the sacrificial lithium source can be significantly different from the voltage when charging based on the positive electrode active material. For example, the elemental lithium in the positive electrode can charge the negative electrode active material without applying an external voltage, because as long as the circuit is closed, the oxidation of the elemental lithium can drive the reaction. For some sacrificial lithium source materials, an external voltage is applied to oxidize the sacrificial lithium source in the positive electrode and drive lithium into the negative electrode active material. Charging can generally be carried out using constant current, stepwise constant voltage charging or other convenient charging schemes. However, at the end of the charging process, the battery should be charged to the desired voltage, so it also involves the removal of lithium from the positive electrode active material (e.g., deintercalation or dealloying).
[0146] In a further embodiment, at least a portion of the supplemental lithium is initially associated with the negative electrode. For example, the supplemental lithium may be in the form of metallic lithium, a lithium alloy, or other lithium sources that are more electronegative than the negative electrode active material. Elemental lithium may be in the form of a thin film, such as a thin film formed by evaporation, sputtering, or ablation, lithium or lithium alloy foil, and / or powder. Elemental lithium, especially elemental lithium in powder form, may be coated to stabilize lithium for processing purposes, and commercial lithium powders, such as powders from Livent Corporation, may be sold with a special coating for stability. The coating generally does not change the properties of lithium powders for electrochemical applications. After the negative electrode is in contact with the electrolyte, a reaction may occur, and the supplemental lithium is transferred to the negative electrode active material. Because the electrode is internally conductive, a closed circuit is not required to provide the electron flow resulting from the reaction. During this process, a solid electrolyte interface (SEI) layer may also be formed. Therefore, the supplemental lithium is loaded into the negative electrode active material, and at least a portion is usually consumed in the formation of the SEI layer. The supplemental lithium located in the negative electrode should be more electronegative than the active material in the negative electrode, because there is no way to react the supplemental lithium source with the active material in the same electrode by applying a voltage.
[0147] In some embodiments, the supplementary lithium associated with the negative electrode can be incorporated into the negative electrode as a powder. Specifically, the negative electrode may include an active negative electrode composition and a supplementary lithium source in a polymer binder matrix, as well as any conductive powder (if present). In additional or alternative embodiments, the supplementary lithium is arranged along the surface of the electrode. For example, the negative electrode may include an active layer having an active negative electrode composition and a supplementary lithium source layer on the surface of the active layer. The supplementary lithium source layer may include a foil of lithium or a lithium alloy, a supplementary lithium powder in a polymer binder, and / or particles of a supplementary lithium source material arranged on the surface of the active layer. In an alternative configuration, the supplementary lithium source layer is between the active layer and the collector. In addition, in some embodiments, the negative electrode may include a supplementary lithium source layer on both surfaces of the active layer.
[0148] An arrangement for electrochemical preloading of lithium may include an electrode having a silicon-based active material formed on a current collector, which is placed in a container containing a lithium source material sheet containing an electrolyte and a contact electrode. The lithium source material sheet may include a lithium foil, a lithium alloy foil, or a lithium source material in a polymer binder, optionally together with a conductive powder, which is directly in contact with the negative electrode to be preloaded with lithium so that electrons can flow between the materials, thereby maintaining electrical neutrality while various reactions occur. In the subsequent reaction, lithium is loaded into the silicon-based active material by embedding, alloying, etc. In an alternative or additional embodiment, the negative electrode active material can be mixed into the electrolyte and the lithium source material for incorporating supplementary lithium before forming an electrode with a polymer binder so that each material can react spontaneously in the electrolyte.
[0149] In some embodiments, the lithium source in the electrode can be assembled into a battery together with the electrode to be preloaded with lithium. The separator can be placed between the electrodes. The current can be made to flow between the electrodes to provide controlled electrochemical pre-lithiation. Depending on the composition of the lithium source, a voltage may or may not be applied to drive the lithium deposition in the silicon-based active material. The device for carrying out the lithiation process may include a container for accommodating an electrolyte and a battery, the battery including an electrode to be used as a negative electrode in the final battery, a current collector, a separator, and a sacrificial electrode containing a lithium source such as a lithium metal foil, wherein the separator is between the sacrificial electrode and the electrode with the silicon-based active material. Convenient sacrificial electrodes may include lithium foil, lithium powder or lithium alloy embedded in a polymer, although any electrode with removable lithium can be used. The container for the lithiated battery may include a conventional battery housing, a beaker, or any other convenient structure. This configuration provides the advantage of being able to measure the current to measure the degree of lithiation of the negative electrode. In addition, the negative electrode can be cycled once or more than once, wherein the negative electrode active material is loaded with lithium to close to full load. In this way, the SEI layer can be formed with a desired controlled degree during lithium preloading of the negative electrode active material.The negative electrode is then fully formed with the selected lithium preloading during preparation of the negative electrode.
[0150] Typically, for embodiments in which supplemental lithium is used, the amount of supplemental lithium preloaded or available for loading into the active composition can be an amount of at least about 2.5% of the capacity of the negative electrode active material, in further embodiments about 3% to about 55% of the capacity, in further embodiments about 5% to about 52.5% of the capacity, and in some embodiments about 5% to about 50% of the capacity of the negative electrode active material. The supplemental lithium can be selected to approximately balance the IRCL of the negative electrode, although other amounts of supplemental lithium can be used as desired. In some embodiments, the supplemental lithium is added in an amount having an oxidation capacity corresponding to 60% to 180% of the first cycle IRCL of the negative electrode, in further embodiments it is 80% to 165%, and in other embodiments 90% to 155%. One of ordinary skill in the art will recognize that additional ranges of percentages within the above explicit ranges are to be considered and are within the present disclosure. Thus, the contribution to the IRCL of the negative electrode can be effectively reduced or eliminated due to the addition of the supplemental lithium, such that the measured IRCL of the battery partially or mostly represents the contribution from the IRCL of the positive electrode, which is not reduced due to the presence of the supplemental lithium. One of ordinary skill in the art will recognize that additional ranges of IRCL within the explicit ranges above are contemplated and are within the present disclosure.
[0151] Balance of cathode and anode
[0152] It has been found that the overall performance of the battery depends on the capacity of both the negative electrode and the positive electrode and their relative balance. It has been found that the balance of the electrodes is important for achieving particularly high battery energy density and achieving good cycle performance. In some embodiments, there may be a trade-off for achieving longer cycle stability and energy density. In order to achieve longer cycle stability, it may be ideal to balance the battery to achieve a relatively low energy density, but the battery is suitable for stable long-term use under a wide range of operating parameters. With appropriately selected active materials, ideal electrode design and improved electrolyte formulations, high energy density can still be achieved while obtaining more than 800 cycles without more than 80% capacity drop. Electrode balance can be evaluated in a variety of alternative ways, which can work effectively when the specific evaluation method is properly considered.
[0153] Testing of active materials can be performed in lithium cells with lithium metal electrodes, and such cells are often referred to as half-cells, compared to lithium-ion cells with two electrodes containing lithium alloying or intercalation materials, known as full cells. In a half-cell with a silicon-based electrode, the lithium electrode acts as the negative electrode, and the silicon-based electrode acts as the positive electrode, as opposed to its usual role as the negative electrode in lithium-ion cells.
[0154] The capacity of the positive electrode active material can be estimated by the capacity of the material, which can be measured by cycling the material relative to lithium metal foil. For example, for a given positive electrode, the capacity can be evaluated by determining the insertion and extraction capabilities during the first charge / discharge cycle, where lithium is deintercalated or extracted from the positive electrode at a rate of C / 20 to a voltage selected based on the material chemistry and the charging voltage of the selected battery design (typically 4.2V to 4.5V), and intercalated or inserted back into the positive electrode to 2V, with a slight adjustment based on the final anode voltage relative to lithium metal, such as typically 0.1V, to a higher charging voltage relative to lithium metal. Similarly, for a given silicon-based electrode, the insertion and extraction capabilities can be evaluated with a battery having a positive electrode containing a silicon-based active material and a lithium foil negative electrode. The capacity is evaluated by determining the insertion and extraction capabilities of the battery during the first charge / discharge cycle, where lithium is intercalated / alloyed to the silicon-based electrode at a rate of C / 20 to 5mV and deintercalated / de-alloyed to 1.5V. In actual use, the observed capacity may vary from the tested capacity due to factors such as high rate operation and voltage range changes, which may be due to the cell design and due to the composition of the counter electrode that is not lithium metal. For some evaluation methods, subsequent capacity after the first cycle can be used to evaluate electrode balance, and larger discharge rates such as C / 3 or C / 10 can be used if necessary. The use of balance after a formation cycle or several formation cycles can be ideal because the balance is more based on the conditions during the use of the cell.
[0155] In most commercially available carbon-based cells, about 7% to 10% excess anode relative to cathode is used to prevent lithium plating. An important problem with too much excess anode is that the weight of the cell will increase, reducing the energy density of the cell. High capacity silicon-based anodes can have an IRCL of about 10% to about 40%, compared to graphite, which has a first cycle IRCL of ~7%. After the first charge-discharge cycle, a large portion of the capacity in the cell may become inactive and add a large amount of dead weight to the cell.
[0156] For high-capacity anode materials, the irreversible capacity loss of the negative electrode is generally greater than the irreversible capacity loss of the positive electrode, which creates additional lithium availability for the battery. If the negative electrode has an irreversible capacity loss significantly higher than that of the positive electrode, the initial charge of the negative electrode consumes lithium irreversibly, so that during subsequent discharge, the negative electrode cannot supply enough lithium to provide sufficient lithium for the positive electrode, thereby satisfying the full lithium acceptance capacity of the positive electrode. This results in a waste of positive electrode capacity, which correspondingly increases the weight that does not contribute to the cycle. As described above, most or all of the lithium loss from the net IRCL (negative electrode IRCL minus positive electrode IRCL) can be compensated by replenishing lithium. The evaluation of the electrode balance during the first formation cycle may or may not take into account the replenishment of lithium. In subsequent cycles after the formation cycle or several cycles, any excess replenishment lithium that is not consumed for IRCL is generally alloyed into the anode material. The electrode balance can be evaluated at the cycle stage after formation, such as the 4th cycle at a selected rate, and these capacities can be estimated from the electrode performance.
[0157] From the perspective of providing stable longer term cycling performance, it may be desirable to balance the electrodes to provide efficient use of both electrode capacities and to avoid plating of lithium metal during cycling. Typically, the balance of the electrodes is considered during electrode assembly, with reference to the initial capacity of the electrode relative to the lithium metal.
[0158] Typically, the battery life can be selected to end when the energy output drops by about 20% from the initial capacity at a constant discharge rate, although other values can be selected as desired. For the materials described herein, the capacity drop under negative electrode cycling is generally greater than that of the positive electrode, so the avoidance of lithium metal deposition with cycling indicates a larger excess capacity of the negative electrode, thereby further stabilizing the cycle. In general, if the rate of negative electrode capacity decay is about twice the rate of positive electrode capacity decay, it is ideal to include at least 10% additional negative electrode capacity for cycling. In a robust battery design, at least about 10% additional negative electrode may be required under a variety of discharge conditions. Typically, the balance can be selected so that the initial negative electrode charge capacity evaluated at a C / 20 rate from the open circuit voltage to 1.5V relative to lithium is about 110% to about 195%, in further embodiments about 120% to about 185%, and in further embodiments about 130% to about 190%, relative to the sum of the initial positive electrode charge capacity at a C / 20 rate from the open circuit voltage to the battery design charge voltage (typically 4.2V to 4.6V) plus the oxidation capacity of any supplemental lithium. Alternatively, the electrode balance can be evaluated at a discharge rate of C / 10 or C / 3 at the fourth cycle, where the negative electrode capacity relative to the positive electrode capacity is about 110% to 195%, in further embodiments about 120% to about 185%, and in further embodiments about 130% to about 190%. One of ordinary skill in the art will recognize that additional ranges of balance within the above explicit ranges are to be considered and are within the present disclosure. Such a balance is described in the battery design described below.
[0159] Performance properties
[0160] The improved electrolyte formulations described herein can further extend the cycle improvements obtained using negative electrode designs that are particularly effective for silicon-based materials. The combination of design features described herein can provide longer cycle stability while maintaining ideal battery performance. The realization of long-term cycles involves the combined use of improved electrode designs with battery design parameter balance described herein and improved electrolyte formulations, which unexpectedly further extend the cycle with unprecedented stability.
[0161] The selected charging voltage can be affected by the positive electrode active material. Typically, the charging voltage selected for these batteries is about 4.05V to 4.4V. The battery can exhibit very good cycle performance. In some embodiments, the battery can show a discharge capacity of at least about 80% of the 6th cycle capacity at the 700th cycle when discharged from the selected charging voltage to 2.5V at a 1C rate at 30°C, in other embodiments at least about 82%, and in other embodiments, when cycled from the selected charging voltage to 2.5V at 1C at 30°C, the 700th cycle is at least about 84% of the discharge capacity relative to the 6th cycle. Similarly, the battery can exhibit a discharge capacity at the 725th cycle of at least about 80% of the 6th cycle capacity when discharged at 1C rate from a selected charge voltage to 2.5V at 30°C, in other embodiments a discharge capacity at the 750th cycle of at least about 80%, and in other embodiments, a discharge capacity at the 800th cycle of at least about 80% relative to the 6th cycle discharge capacity when cycled at C / 3 from a selected charge voltage to 2.5V at 30°C. Comparable results were obtained at 2C charge and discharge rates. One of ordinary skill in the art will recognize that additional ranges within the above explicit ranges are to be considered and are within the present disclosure.
[0162] Example
[0163] General Methods and Materials. The electrolyte formulations were tested by incorporating them into coin cells using an NMC positive electrode and a negative electrode comprising a blend of a silicon oxide-based composite and graphite as the active material. Specifically, the active material for the positive electrode was a LiNi 0.6 Mn 0.2 Co 0.2 O2(NMC622) or LiNi 0.8 Mn 0.1 Co 0.1 The negative electrode active material is a commercial SiO-Si-C (SiOx) composite blended with electrochemically active graphite.
[0164] Unless otherwise specified, to form a negative electrode having a silicon oxide-based active material, 65 wt % to 80 wt % of a commercial silicon oxide / silicon / carbon composite material (hereinafter referred to as SiO x / Si / C) powder and the balance (20 wt % to 35 wt %) of graphite (KS 6 synthetic graphite, Imerys) to form an active material. The negative electrode active material is fully mixed with 1 wt % to 7 wt % of a nano-scale carbon conductive additive to form a uniform powder mixture. The negative electrode has 2 wt % to 6 wt % of carbon nanotubes as a conductive additive. The powder components of the electrode, active material and carbon nanotubes are mixed to form a uniform powder mixture. The negative electrode has 1 wt % to 7 wt % of a lower elastic modulus binder and 7 % to 15 % of polyimide. The weight ratio of the lower elastic modulus binder to the polyimide is 0.714.
[0165] To form the negative electrode, a blend of a polymer binder, a polyimide binder, and a lower elastic modulus binder is mixed with N-methyl-pyrrolidone ("NMP") (Sigma-Aldrich) and stirred overnight to form a polymer binder-NMP solution. The uniform powder mixture is then added to the polymer binder-NMP solution and stirred for about 2 hours to form a uniform slurry. The slurry is applied to a copper foil collector to form a thin wet film, and the laminated collector is dried in a vacuum oven to remove the NMP and cure the polymer. The laminated collector is then pressed between the rollers of a sheet mill to obtain the desired laminate thickness. The dried laminate contains 2% to 20% by weight of the binder, with the remainder of the electrode being contributed by the powder. The negative electrode is electrochemically pre-lithiated with sufficient lithium to compensate for 100% to 160% of the lithium loss caused by the irreversible capacity loss of the anode.
[0166] The positive electrode has about 93 wt % to 97.5 wt % of the active material loaded blended with 1 wt % to 4 wt % of the pvdf binder, and 1 wt % to 3 wt % of nanoscale carbon. The cathode material is blended with NMP solvent, spread onto an aluminum foil current collector, pressed and dried.
[0167] To form a button cell, a portion of the negative electrode is cut to size along the separator, and a portion of the positive electrode is also cut to size. The separator used for these cells is A porous polymer film is prepared. The electrodes with a separator in between are placed in a button cell housing. An electrolyte selected as described below is placed in the cell and the cell is sealed.
[0168] The assembled cells were cycled at 23° C. from 4.3 V to 2.5 V for NMC622 cells and from 4.2 V to 2.5 V for NMC811 cells. The cells were charged and discharged at a rate of C / 10 in the first cycle, at a rate of C / 5 in the second cycle, and then cycled at a rate of C / 3.
[0169] Examples 8 and 9 relate to pouch cells, and the formation of these cells is further described below.
[0170] Example 1 - Cell with NMC cathode and commercial electrolyte
[0171] This example illustrates the cycling performance in a coin cell with a blend of NCM cathode active materials, anode active materials, and a commercial electrolyte.
[0172] In the first group of cells, the negative electrodes of these cells were as described in the Materials and Methods section above. The positive electrodes comprised LiNi 0.8 Mn 0.1 Co 0.1 O2(NMC811) or LiNi 0.6 Mn 0.2 Co 0.2 O2 (NMC622) was used as the positive active material for the battery. Batteries were formed with different loadings of the positive active material. The NMC 622 battery was cycled within 4.30V to 2.5V or 4.35V to 2.5V, and the NMC 811 battery was cycled within a voltage range of 4.20V to 2.5V.
[0173] The initial charge-discharge cycles were performed at a rate of C / 10. The results for all samples are also summarized in Table 1.
[0174] Table 1
[0175]
[0176] In addition, the batteries corresponding to samples C1-C8 were cycled. Specifically, the batteries were charged and discharged at a rate of C / 10 in the first cycle, charged and discharged at a rate of C / 5 in the second cycle, and then cycled at a rate of C / 3. The rate performance of the battery samples based on the discharge capacity at the specified discharge rate is summarized in Table 2.
[0177] Table 2
[0178]
[0179] exist Figure 5 The discharge capacity of samples C2, C4 and C7 as a function of cycle is plotted in Figure 6 The normalized capacity as a function of cycle is plotted in . The best cycling performance of these coin cells is based on the sample of NMC622 cycled from 4.30 V to 2.5 V, while the worst cycling performance over the entire cycling range is based on NMC622 cycled from 4.35 V to 2.5 V.
[0180] Example 2 - Electrolyte formulation for silicon oxide-based lithium-ion batteries
[0181] This example provides a set of electrolyte formulations for silicon oxide based active materials designed for use in conjunction with NMC active materials and their ionic conductivity measurements.
[0182] Electrolyte formulations. Table 3 provides electrolyte formulations with different lithium hexafluorophosphate (LiPF6) concentrations and solvent contents. The concentration of LiPF6 used in each electrolyte formulation and the weight percentage ranges of fluoroethylene carbonate (FEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), fluorobenzene (FB), propylene carbonate (PC), 1,3-methane sultone (MS) and ethyl carbonate (EC) are shown in Table 3 (the percentage values are the volume percentages of the solvent), and the conductivity measurements (25°C) of each formulation are provided.
[0183] Table 3
[0184]
[0185]
[0186] *Contains 25% fluorinated additives.
[0187] A=1-1.25M,B=1.3-1.75M
[0188] FA=16%-25%
[0189] DM1=75%-85%, DM2=45%-55%, DM3=40%-50%, DM4=35-45%, DM5=30%-40%, DM6=25%-35%, DM1>DM2>DM3>DM4>DM5>DM6
[0190] EM1=75%-85%, EM2=30%-50%
[0191] DE1=30%-50%, DE2=75%-85%
[0192] Example 3 - Rate performance of electrochemical cells with selected electrolyte formulations
[0193] This example illustrates the rate capability achievable using the electrolyte selected from Example 2.
[0194] The cells were formed as described in Example 1 above, except that an electrolyte selected from Table 3 was used. Table 4 shows the relationship between electrolyte conductivity and rate performance for the five electrolyte formulations of Table 3. For electrolyte formulations Nos. 1, 2, 3, 7, and 10, the assembled cells were cycled at different charge / discharge rates, such as 0.333C / 0.333C, 1C / 1C, and 2C / 1C, after the first two formation cycles.
[0195] Table 4
[0196]
[0197] Example 4 - Electrolyte dependence on the cycling performance of NMC622 / SiOx lithium-ion batteries
[0198] In this example the cycling performance of button cells based on various electrolyte formulations is described.
[0199] Effect of ethylene carbonate. Figure 7 (1C / 1C) and 8 (2C / 2C) show the adverse effect on the rate performance of the lithium-ion battery system when the electrolyte formulation contains ethylene carbonate. The button cell of this embodiment is based on NMC622 positive electrode active material. The negative electrode and button cell were formed as described in Example 1. For example, for the button cell with electrolyte No. 1 (Table 3), the rate performance of the system deteriorated significantly after ethylene carbonate was added to the formulation. Compared with the commercial electrolytes (Product 1 and Product 2) listed in Table 3, formulations No. 1 and No. 2 contain 0% ethylene carbonate and exhibit excellent performance at both 1C and 2C cycles. Electrolyte 1 exhibits slightly better cycling performance relative to electrolyte 2.
[0200] Effect of Fluoroethylene Carbonate Concentration. Fig. 9 and 10 The normalized ( Fig. 9 ) and unnormalized ( Fig.10 ) 1C charge and discharge cycle performance. The data show that at least 5% to 10% FEC additive is needed for silicon-based cells to obtain greater than 700 cycles with 80% capacity retention. Electrolytes with 10% or 15% FEC have the best cycling performance relative to electrolytes with less or more FEC. Electrolytes without FEC cycle poorly.
[0201] Effect of solvents. For 1C cycling applications, different amounts of dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate in the electrolyte formulations showed relatively consistent performance over the battery cycle life, such as 765 to 805 cycles at 80% capacity retention in button cells ( Fig.11(1C / 1C) and 12 (2C / 2C)), although the best results were obtained with at least some DMC and not too much DEC. However, for 2C cycling applications, the cycling performance was more affected by the different solvent ratios. For example, when the electrolyte contained more than 70% DEC, the cycling performance decreased. High weight percentages of DMC or EMC did not negatively affect the cycling performance, although the best results were obtained with some blends of room temperature liquid solvent components, i.e., solvent components mixed with FEC.
[0202] Effects of solvents and additives.
[0203] The effects of fluorobenzene and propylene carbonate as additives were investigated. They are referred to as electrolytes 12-14 in Table 3. In all additive formulations tested, the coin cells showed consistent cycling performance, e.g., 770 to 780 cycles at 80% capacity retention ( Fig.13 (normalized) and 14 (unnormalized capacity)). The results are also similar to the performance of electrolyte 7 (which is the closest electrolyte without additives), as shown in Fig.11 shown.
[0204] Example 5 - Cycling performance of NMC811 / SiOx button cell
[0205] This example shows the cycle performance in the case of using NMC811 active material in the positive electrode / cathode for one of the electrolytes developed for silicon oxide-based negative electrode active materials.
[0206] Electrolyte 2 was also used to cycle similar button cells formulated with NMC811 positive active material and SiOx negative electrode as described in Examples 1, 3 and 4. These cells were cycled from 2.5 V to 4.2 V. The cycling performance was Fig.15 The results are shown in Figures 16 (1C / 1C) and 16 (2C / 2C). When using Electrolyte 2 as the electrolyte, both 1C and 2C coin cell applications provide cycling performance of more than 700 cycles with 80% capacity retention. This cycling performance is comparable to the NMC622 results, while the cycling of the NMC811 electrode at 1C / 1C is slightly better, and the cycling of the NMC811 electrode at 2C / 2C is slightly worse.
[0207] Example 6 - High Capacity Long Cycle Batteries with Commercial Electrolytes
[0208] This example illustrates the long term cycling stability based on the improved negative electrode loaded into large scale batteries.
[0209] The pouch cell is designed to have a target capacity of approximately 11Ah. The prismatic pouch cell has an approximate size of 145mm x 64mm x 7.7mm (thick), ignoring the tabs. The cell design is Fig.17 and 18The electrodes are formed as described in the Materials and Methods section above, and the separator sheet is pleated, with the plate-shaped electrodes placed in the separator folds. The separator for the pouch cell is a porous polymer composite sheet with a gel-forming polymer coating. The lithium powder ( Livent Corp.) was applied to the negative electrode surface to provide supplemental lithium to roughly compensate for 100% to 160% of the IRCL of the silicon-based negative electrode active material. The battery was designed to have a total capacity of approximately 11 Ah at a discharge rate of C / 3 at 30°C. The battery was cycled with a charge and discharge rate of C / 20 with one formation cycle. The battery was then cycled at 30°C at a charge rate and discharge rate of C / 3.
[0210] The 11Ah cell was formed with the same anode as described above for the button cell and an NMC811 based positive electrode, and an NMC622 based positive electrode and a SiO containing 75 wt % to 90 wt %. x An anode is formed of an active material of a Si / C composite and 10 wt% to 25 wt% graphite. The negative electrode capacity is initially 130% to 160% of the positive electrode capacity based on the low rate (C / 20) capacity. The negative electrode has a blend of polyimide and a lower elastic modulus binder and a carbon nanotube conductive material. A commercial fluorinated electrolyte is also used. For an electrode with an NMC622 positive electrode, two comparable representative cells are cycled from 4.3V to 2.5V. Fig.19 and 20 The loop results are plotted in . Fig.19 and 20 In , the specific capacity and the normalized specific capacity are plotted as a function of the cycles.
[0211] For cells with NMC811 positive electrode, comparable cells were cycled at a rate of C / 3 from 4.15 V to 2.5 V and from 4.20 V to 2.5 V. Fig.21 and 22 The loop results are plotted in . Fig.21 and 22 In , the specific capacity and the normalized specific capacity are plotted as a function of the cycles.
[0212] Example 7 - Cycling performance of NMC622 / SiOx pouch cells with improved electrolyte
[0213] This example examines the cycling performance of a pouch cell format having a silicon oxide based active material with the improved electrolyte described herein.
[0214] The cycling performance of NMC622 / SiOx based 11Ah 285Wh / kg pouch cells was tested using three different electrolyte formulations from Table 3. The pouch cell construction was the same as described in Example 6 except that electrodes formulated as described above in the Materials and Methods section and new electrolyte formulations were used. Fig.23 and 24 The normalized discharge capacities ( Fig.23 ) and unnormalized discharge capacity ( Fig.24 ). Cells formed using electrolyte 2 were shown to provide cycling performance of greater than 1000 cycles with 80% capacity retention. For 1C pouch cell applications, this result indicates that greater than 70% by weight of DMC is preferred in electrolyte formulations containing LiPF6 and FEC when compared to formulations 7 and 10.
[0215] Example 8 - Blended positive electrode active materials
[0216] This example illustrates the usefulness of the improved electrolyte for cycling using a battery having a positive electrode containing a blend of active materials.
[0217] A positive electrode was formed using a blend of nickel-rich lithium nickel manganese cobalt oxide (N-NMC) combined with lithium + manganese-rich NMC (LM-NCM). It has been found that some LM-NMC compositions can exhibit lower DC resistance while maintaining higher capacity and excellent cycling, as described in U.S. Pat. No. 9,552,901 B2, entitled "Lithium Ion Battery with High Energy Density, Excellent Cycling Performance and Low Internal Impedance" by Amiruddin et al. (hereinafter referred to as the '901 patent), which is incorporated herein by reference. The negative electrode was the same as described in Example 2, and a button cell was formed as described in Example 2.
[0218] The cycling results of the batteries using the 5 different electrolytes in Table 3, specifically electrolytes 1, 2, 3, 7 and 8, were obtained. The batteries were cycled from 4.25 V to 2.3 V at a 1C / 1C-charge / discharge rate after the first cycle. Fig.25 The cycling results are plotted in 26 (normalized capacity) and 26 (unnormalized discharge capacity). Similar cycling results were obtained for the electrolytes except for electrolyte 1. For all electrolytes, improved cycling was obtained relative to equivalent results obtained using commercial fluorinated electrolytes, see the '209 application cited above, where the results for electrolytes 2, 3, 7, and 8 were significantly better. However, the cycling results were not as good as in the case of the N-NMC based cathodes.
[0219] The above embodiments are intended to be illustrative rather than restrictive. Other embodiments are also within the claims. In addition, although the present invention has been described with reference to specific embodiments, those skilled in the art will recognize that changes can be made in form and detail without departing from the spirit and scope of the present invention. Any combination cited by the above documents is limited so that the subject matter incorporated herein will not be contrary to the explicit disclosure of this article. The extent to which specific structures, compositions and / or processes are described herein with components, elements, ingredients or other divisions, it should be understood that, unless otherwise explicitly stated, the disclosure herein covers specific embodiments, embodiments comprising specific components, elements, ingredients, other divisions or combinations thereof, and embodiments consisting mainly of such specific components, ingredients or other divisions or combinations thereof, which may include other features that do not change the basic properties of the subject matter, as indicated in the discussion.
Claims
1. A lithium ion battery, comprising: A negative electrode comprising 75 to 92 wt % of an active material, 1 to 7 wt % of nanoscale conductive carbon, and 6 to 20 wt % of a polymer binder, wherein the active material comprises 35 to 95 wt % of a silicon oxide-based material and 5 to 65 wt % of graphite; The positive electrode comprises lithium nickel cobalt manganese oxide, conductive carbon and a polymer binder, wherein the lithium nickel cobalt manganese oxide is of the formula LiNi x Mn y Co z O2 represents, where x+y+z≈1, 0.3≤x, 0.025≤y≤0.35, 0.025≤z≤0.35; a separator between the negative electrode and the positive electrode; an electrolyte comprising 1M to 2M lithium salt and a non-aqueous solvent, wherein the non-aqueous solvent comprises at least 5% by volume of fluoroethylene carbonate and at least 25% by volume of a total amount of dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate, wherein the amount of diethyl carbonate is 20% to 50% by volume, wherein the electrolyte is substantially free of ethylene carbonate; as well as A container that encloses other battery components.
2. The lithium ion battery of claim 1, wherein the lithium ion battery can be cycled for at least 700 cycles at a charge rate of 1C and a discharge rate of 1C without a capacity reduction of no more than 20% relative to the capacity at the third cycle.
3. The lithium ion battery according to claim 1 or 2, wherein the negative electrode active material comprises 40 wt % to 90 wt % of a silicon oxide-based material and 10 wt % to 60 wt % of graphite, wherein the BET surface area of the graphite is 2 m 2 / g to 100m 2 / g.
4. The lithium ion battery of claim 3, wherein the silicon oxide-based material comprises a silicon-silicon oxide carbon composite material.
5. The lithium ion battery of claim 1 or claim 2, wherein the polymer binder of the negative electrode comprises a blend of polyimide and a second binder polymer selected from the group consisting of polyvinylidene fluoride, carboxymethyl cellulose, styrene-butadiene rubber, lithiated polyacrylic acid, copolymers thereof, and mixtures thereof.
6. The lithium ion battery of claim 1 or claim 2, wherein the electrolyte comprises 1.25M to 1.8M lithium salt, and wherein the nonaqueous solvent comprises 8% to 25% by volume of fluoroethylene carbonate and at least 50% by volume of the total amount of dimethyl carbonate, ethyl methyl carbonate and diethyl carbonate.
7. The lithium ion battery of claim 1 or claim 2, wherein the electrolyte further comprises 2 to 12 wt% of propylene carbonate and 2 to 12 wt% of fluorobenzene.
8. The lithium ion battery of claim 1 or claim 2, wherein the lithium nickel cobalt manganese oxide is of the formula LiNi x Mn y Co z O2 represents, where x+y+z≈1, 0.50≤x, 0.03≤y≤0.325, 0.03≤z≤0.
325.
9. The lithium ion battery of claim 1 or claim 2, further comprising supplementary lithium in an amount accounting for 80% to 180% of the irreversible capacity loss of the negative electrode in the first cycle, wherein the ratio of the negative electrode capacity divided by the positive electrode capacity at the fourth cycle of the lithium ion battery at a discharge rate of C / 3 is 1.10 to 1.
95.
10. The lithium ion battery of claim 1 or claim 2, wherein the positive electrode further comprises 20 wt % to 80 wt % of a 1+b Ni α Mn β Co γ A δ O 2-z F z A (lithium + manganese) rich lithium metal oxide represented by b + α + β + γ + δ ≈ 1, b is in the range of 0.04 to 0.3, α is in the range of 0 to 0.4, β is in the range of 0.2 to 0.65, γ is in the range of 0 to 0.46, δ is in the range of 0 to 0.15, and z is in the range of 0 to 0.2, provided that α and γ are not 0 at the same time, and wherein A is a metal different from lithium, manganese, nickel and cobalt.
11. A lithium ion battery, comprising: A negative electrode comprising 75 to 92 wt % of an active material, 1 to 7 wt % of nanoscale conductive carbon, and 6 to 20 wt % of a polymer binder, wherein the active material comprises 40 to 95 wt % of a silicon oxide-based material and 5 to 60 wt % of graphite; A positive electrode comprising a nickel-rich lithium nickel cobalt metal oxide, a conductive carbon and a polymer binder, wherein the nickel-rich lithium nickel cobalt metal oxide is of the formula LiNi x M y Co z O2 represents, wherein x+y+z≈1, 0.3≤x, 0.025≤y≤0.35, 0.025≤z≤0.35, and M is Mn, Al, Mg, Sr, Ba, Cd, Zn, Ga, B, Zr, Ti, Ca, Ce, Y, Nb, Cr, Fe, V or a combination thereof; a separator between the negative electrode and the positive electrode; an electrolyte comprising 1M to 2M lithium salt and a non-aqueous solvent, wherein the non-aqueous solvent comprises at least 5% by volume of fluoroethylene carbonate and at least 25% by volume of a total amount of dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate, wherein the amount of diethyl carbonate is 20% to 50% by volume, wherein the electrolyte is substantially free of ethylene carbonate; as well as Containers for enclosing other battery components, The lithium ion battery can be cycled for at least 700 cycles at a charge rate of 1C and a discharge rate of 1C without its capacity decreasing by more than 20% relative to the capacity at the third cycle.
12. The lithium ion battery of claim 11, wherein the lithium ion battery can be cycled for at least 750 cycles at a charge rate of 1C and a discharge rate of 1C without a capacity reduction of no more than 20% relative to the capacity at the third cycle.
13. The lithium ion battery according to claim 11 or 12, wherein the negative electrode active material comprises 50 wt % to 90 wt % of a silicon oxide-based material and 10 wt % to 50 wt % of graphite, wherein the BET surface area of the graphite is 2 m 2 / g to 100m 2 / g.
14. The lithium ion battery of claim 13, wherein the silicon oxide-based material comprises a silicon-silicon oxide carbon composite material.
15. The lithium ion battery of claim 11 or claim 12, wherein the polymer binder of the negative electrode comprises a blend of a polyimide and a second binder polymer selected from the group consisting of polyvinylidene fluoride, carboxymethyl cellulose, styrene-butadiene rubber, lithiated polyacrylic acid, copolymers thereof, and mixtures thereof.
16. The lithium ion battery of claim 11 or claim 12, wherein the electrolyte comprises 1.25M to 1.8M lithium salt, and wherein the non-aqueous solvent comprises 8% to 25% by volume of fluoroethylene carbonate and at least 50% by volume of the total amount of dimethyl carbonate, ethyl methyl carbonate and diethyl carbonate.
17. The lithium ion battery of claim 11 or claim 12, wherein the electrolyte further comprises 2 to 12 wt% propylene carbonate and 2 to 12 wt% fluorobenzene.
18. The lithium ion battery of claim 11 or claim 12, wherein the nickel-rich lithium nickel cobalt metal oxide is of the formula LiNi x Mn y Co z O2 represents, where x+y+z≈1, 0.50≤x, 0.03≤y≤0.325, 0.03≤z≤0.
325.
19. The lithium ion battery of claim 11 or claim 12, further comprising supplementary lithium in an amount accounting for 80% to 180% of the irreversible capacity loss of the negative electrode in the first cycle, wherein the ratio of the negative electrode capacity divided by the positive electrode capacity at the fourth cycle of the lithium ion battery at a discharge rate of C / 3 is 1.10 to 1.
95.
20. The lithium ion battery of claim 11 or claim 12, wherein the lithium ion battery can be cycled for at least 800 cycles at a charge rate of 1C and a discharge rate of 1C without its capacity decreasing by more than 20% relative to the capacity at the third cycle.
Citation Information
Patent Citations
Lithium ion cells with high performance electrolyte and silicon oxide active materials achieving very long cycle life performance
US11973178B2
Low Temperature Electrolyte for High Capacity Lithium Based Batteries
US20130157147A1
Silicon-based active materials for lithium ion batteries and synthesis with solution processing
US20140308585A1
Silicon-silicon oxide-carbon composites for lithium battery electrodes and methods for forming the composites
US20140370387A1
Lithium ion batteries with high capacity anode active material and good cycling for consumer electronics
US20150050535A1