Biobattery with fuel storage

By using solid block enzyme electrodes and porous membrane structures in biofuel cells, combined with hydrophilic porous materials to store biofuels, the problems of miniaturization and efficient output are solved, and stable application and environmental protection characteristics in disposable devices are achieved .

CN112236891BActive Publication Date: 2024-10-08CENT NAT DE LA RECH SCI (C N R S) +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980038313.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-06-08
Filing Date
2019-05-31
Publication Date
2024-10-08
Estimated Expiration
2039-05-31

AI Technical Summary

Technical Problem

It is difficult for existing biofuel cells to achieve miniaturization, low-cost manufacturing and high current density output, and it is difficult to operate stably in complex circuit integration, which affects their application in disposable devices.

Method used

The anode and cathode are made of solid briquettes, containing enzymes and conductive materials that catalyze the oxidation of biofuels and the reduction of oxidants respectively, and are in contact with the liquid medium through a separating porous membrane. Hydrophilic porous materials are used to store biofuels and realize electricity. chemical reaction.

Benefits of technology

A small, efficient biofuel cell is realized that can operate stably in a disposable device, provide reliable voltage and high current density output, and is biodegradable and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112236891B_ABST
    Figure CN112236891B_ABST
Patent Text Reader

Abstract

The present invention relates to a biobattery (1) having a biofuel reservoir intended to be in contact with a liquid medium and in contact with a fluid medium comprising an oxidant. The biobattery comprises a first electrochemical cell, the first electrochemical cell comprising: an anode (5) comprising a first enzyme capable of catalyzing the oxidation of the biofuel; a cathode (7) comprising a second enzyme capable of catalyzing the reduction of the oxidant; and a separating porous membrane (3) disposed between the anode (5) and the cathode (7), the membrane being electrically insulating and permeable to the liquid medium. The biobattery (1) is characterized in that it comprises a biofuel storage member for storing the biofuel (3) and for providing the liquid medium to the anode (5), the member comprising a hydrophilic porous material in contact with the anode (5), and the member having a hydrophilicity of 500 to 900 g / m 2 Surface density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an enzymatic fuel cell or biocell, to its use for detecting or oxidizing a biofuel such as glucose, to a kit comprising the same and to an electrical or electronic device incorporating the biocell. The invention also relates to a method for manufacturing such a biocell and to an assembly comprising at least two biocells according to the invention. Background Art

[0002] Fuel cell technology is based on the conversion of chemical energy into electrical energy. Organic molecules such as glucose are one of the most important energy sources for many living organisms and can be considered as safe, tractable and consumable, and therefore biodegradable, biofuels.

[0003] Biofuel enzyme cells (also referred to as biobatteries) use enzymes to generate energy or electricity from biological substrates such as oxygen, methanol, glucose or starch. Biobatteries convert biofuels in the presence of enzyme compounds to produce electricity. The most well-known biobatteries that work by glucose oxidation (GBFC) are such cells that convert glucose to produce electricity by oxidation at the anode using enzymes incorporated therein and having a catalytic function of the reaction. The function of the cathode is generally to reduce oxygen and may or may not include an enzyme that catalyzes this reaction.

[0004] Enzymes are promising alternatives to precious metal catalysts, as they mostly work at neutral pH and room temperature and offer little or no toxicity, which is not the case with other metal-based catalysts. Such biofuel biocells can therefore be very easily recycled and present an ecological alternative as electric current generators, especially for disposable devices.

[0005] The invention more precisely relates to the manufacture of bio-batteries of the "button" type, that is to say of smaller size and capable of providing power equivalent to that of metal-based button cells, and which can optionally be discarded without environmental risk. This is not the case with button cells and alkaline batteries today. This green technology could offer an original solution to the problems associated with the recycling of zinc, lithium or manganese-based batteries used every day. In the absence of metal, the device according to the invention also describes a portable energy source that is invisible to metal detectors.

[0006] Alternatively or additionally, the device according to the invention is intended to generate electrical energy for specific needs when other conventional energy sources (wind, solar energy, etc.) are unavailable. In fact, enzymes have a unique selectivity that enables the generation of electricity in a complex medium, which can allow the use of liquids and especially various biological fluids: sugar (glucose), syrup drinks, physiological fluids (animal saliva, blood, urine) or plant sources (juice), etc.) as activators and / or fuels. In this case, the terms "fuel" and "biofuel" are interchangeable.

[0007] In these regards, important challenges must be overcome before such biofuel cells can be put into commercial applications.

[0008] Specifically, it should preferably be small in size (1 cm in area). 2 Up to 5cm 2 ), or even very small (less than 0.5 cm 2 ), and is designed to replace the "button" type batteries frequently used in disposable devices. It should be easy to recycle and preferably inexpensive.

[0009] The present invention therefore aims in particular at solving the problem of providing a biofuel cell, in particular a design that allows its use in a disposable device that is cheap (button cell type) or designed for single use, preferably of small size, and preferably allows for an optimized entry of fuel and oxidant into the electrochemical cell to produce a maximum amount of energy. In addition, advantageously, such a biofuel cell can be used in an assembly of several biofuel biocells or electrochemical cells to produce sustainable and regenerative energy.

[0010] In general, therefore, the present invention aims to solve the problem of easy and low-cost manufacture of biobatteries, and their integration into more or less complex circuits, wherein the current density generated is high enough to operate the device. Advantageously, the voltage delivered is sufficient to operate the device reliably. Summary of the invention

[0011] According to one embodiment, the invention comprises a biocell having a biofuel reservoir, the biocell being intended to be in contact with a liquid medium, the liquid medium optionally comprising a biofuel, and the biocell being intended to be in contact with a fluid medium comprising an oxidant, the biocell comprising a first electrochemical cell, the first electrochemical cell comprising:

[0012] - an anode made of a solid mass comprising a conductive material mixed with a first enzyme capable of catalyzing the oxidation of a biofuel; and

[0013] a cathode consisting of a solid mass comprising a conductive material mixed with a second enzyme capable of catalyzing the reduction of an oxidant, and

[0014] - a separating porous membrane disposed between the anode and the cathode, which is electrically insulating and permeable to said liquid medium.

[0015] The biobattery also includes an electrical connection member for electrically connecting the biobattery electrical receiver, the electrical connection member allowing current to flow between the anode and the cathode. The biobattery is characterized in that it includes a biofuel storage member for storing biofuel and providing a liquid medium to the anode, the member includes a hydrophilic porous material in contact with the anode, and the member has a hydrophilicity of 500 g / m 2 Up to 900g / m 2 Surface density.

[0016] Thus, the storage member can act as a reservoir for the biofuel and / or the liquid containing it. Preferably, the storage member has a volume that can be 650 g / m 2 Up to 750g / m 2 The surface density (or grammage) within the range is preferably 703 g / m 2 , optionally ±20%. It can be especially chosen from the group consisting of 655, 660, 665, 670, 675, 680, 685, 690, 695, 696, 697, 698, 699, 700, 701, 702, 703, 704, 705, 707, 708, 709, 710, 711, 712, 713, 714, 715, 720, 725, 730, 735, 740, 745, 750, 755 and 760 g / m 2 Therefore, the storage medium is a very porous material.

[0017] The storage member can be a porous pad, in the form of a pad, or in the form of an English "pad". The material constituting the storage member is preferably an electrical insulator. This material can contain textile fibers or non-woven fibers (felt) or be made of textile fibers or non-woven fibers (felt). These fibers are preferably natural and / or biodegradable fibers, for example, it can be a material comprising cellulose and especially cotton fabric or mainly consisting of cellulose and especially cotton fabric, or based on cellulose and especially cotton fabric in addition. It can also be a natural polymer (cellulose, cotton fabric, sponge, chitosan, etc.) or synthetic (polyacrylic acid foam, polyvinyl alcohol, etc.). The statement "based on X" can be interpreted as referring to a material consisting of more than 90 mass %, preferably more than 95%, even more than 98% relative to the total mass of component X. Therefore, the storage member can advantageously include or be essentially composed of a piece of paper, preferably blotting paper type, such as super thick blotting paper. It is also preferred that this pad and / or paper do not have additives. The gram weight can be measured according to the standard NF EN ISO 536 of November 2012.

[0018] The thickness of the storage member is preferably as small as possible to allow miniaturized use. However, for other uses, this thickness can be greater and of the same order of magnitude as one centimeter or half a centimeter. This thickness can therefore be 1 cm to 0.1 mm, preferably 8 mm to 2 mm, and more precisely about 2.6 mm, optionally ±20%. It can especially be selected as a thickness selected from the group consisting of: 1; 1.5; 1.6; 1.7; 1.8; 1.9; 2; 2.1; 2.2; 2.3; 2.4; 2.6; 2.7; 2.8; 2.9; 3; 3.1; 3.2; 3.3; 3.4; 3.5; 3.6; 3.7; 3.8; 3.9 and 4 mm.

[0019] Advantageously, the storage member is a sheet of blotting paper, the thickness of which is 2.6 mm ± 0.2 mm. Its porosity must allow good absorption of liquids containing fuel (e.g. water, urine, syrupy drinks, blood, etc.), and in particular sugars. According to a preferred variant of the invention, it must be rigid enough for the embedding or maintenance of the bioanode or biocathode.

[0020] Advantageously, the storage member has a liquid filtration time which may be in the range of 100 s / ml to 140 s / ml, preferably 110 s / ml to 130 s / ml, and conveniently about 120 s / 100 ml, optionally ±20%; measured according to the Herzberg method (with a water column of 100 mm).

[0021] The electrochemical cell included in the biobattery according to the present invention comprises an anode and a cathode. These electrodes are in the form of a solid mass, which comprises at its substrate a preferably porous conductive material and at least one enzyme of a half-reaction to be catalyzed. This porous material can be any recyclable porous conductive material, such as carbon felt, microporous carbon, carbon nanotubes, activated carbon, carbon black, conductive polymers, etc. In an example, a sheet based on single-walled or more advantageous multi-walled carbon nanotubes (MWCNT) or carbon black provides excellent porosity associated with excellent conductivity. "Carbon nanotube" means a carbon nanotube having at least one dimension less than 1500nm. Preferably, the carbon nanotube has a length (L) / diameter ratio expressed as L / diameter between 100 and 5000. Preferably, the carbon nanotube has a length of about 1.5 μm and a diameter of about 10 nm, for example.

[0022] In the exemplary embodiment of the invention of the present application, the biofuel of choice is glucose due to the high availability of this compound and its minimal impact on the environment. However, the structure of the biocell according to the present invention can be adapted to substrates other than glucose, as long as the relevant enzyme compounds are also suitable.

[0023] The theoretical reaction balance of the glucose / O2 enzyme biobattery is as follows:

[0024] Anode: Glucose → Gluconolactone + 2H + +2e -

[0025] Cathode: O2+4H + +4e - →2H2O

[0026] Biobattery: 2 glucose + O2 → 2 gluconolactone + 2H2O

[0027] Therefore, according to a preferred aspect of the present invention, the enzyme system used at the anode may include at least one glucose oxidase. Glucose oxidase (GOx) is an oxidoreductase of EC 1.1.3.4 type (classified in April 2018), which catalyzes glucose, more specifically, β-D-glucose (or dextrose) oxidation to hydrogen peroxide and D-glucono-δ-lactone, which is then hydrolyzed to gluconic acid. Glucose oxidase specifically binds to β-D-pyranose glucose (the hemiacetal form of glucose) and does not work on 1'α-D-glucose. However, it can work on its enantiomeric glucose because it is mainly in its cyclic form (at pH 7: 36.4% α-D-glucose and 63.6% β-D-glucose, 0.5% in linear form) in solution glucose. In addition, the oxidation and consumption of the β form shifts the α-D-glucose / β-D-glucose balance toward this form. The term GOx extends to natural proteins and their derivatives, mutants and / or functional equivalents. The term extends especially to proteins that do not differ substantially in structure and / or enzymatic activity.

[0028] Glucose oxidase contains and requires a cofactor to achieve catalysis. This cofactor is Flavin Adenine Dinucleotide (FAD), which is the main redox component in the battery. FAD acts as an initial electron acceptor, which is reduced to FADH2, which will be reoxidized to FAD (regeneration) by molecular oxygen (O2, which is more reducing than FAD). Finally, O2 is reduced to hydrogen peroxide (H2O2). The cofactor is included in the commercially available GOx enzyme and the terms GOx and FAD-GOX are equivalent.

[0029] The most widely used glucose oxidase is that extracted from Aspergillus niger. However, GOx from other sources may be used, for example, certain strains of the species Penicillium or Aspergilius terreus.

[0030] Glucose oxidase from Aspergillus niger is a dimer composed of 2 equal subunits each having a molecular weight of 80 kDa (by gel filtration). Each subunit contains flavin adenine dinucleotide and an iron atom. This glycoprotein contains approximately 16% neutral sugars and 2% amino sugars. It also contains 3 cysteine ​​residues and 8 potential sites for N-glycosylation.

[0031] The specific activity of GOx is preferably greater than or equal to 100,000 units / g solid (without added O2). One unit is defined as the oxidation capacity of 1.0 micromole of β-D-glucose to D-gluconolactone and H2O2 per minute at 35°C at pH 5.1. (Km=33-110 mM; 25°C; pH 5.5-5.6).

[0032] To the extent that the use of GOx involves the generation of hydrogen peroxide, catalase can be added to the enzyme system.

[0033] Catalase is a tetrameric enzyme that catalyzes the following reaction: 2H2O2→O2+2H2O. Each subunit contains iron bound to a protoheme type IX group. Each subunit is identical and consists of a polypeptide chain of approximately 500 amino acids. The molecular weight of each subunit is typically 60 kDa (gel filtration). Catalase can bind strongly to NADP and NADP, and the heme groups are then separated from each other. Positioning. It can react with other hydrogenated alkyl peroxides (such as methyl peroxide or ethyl peroxide). The activity of catalase is usually constant in the pH range of 4 to 8.5. Its specific activity is preferably greater than 2000 units / mg, especially greater than 3000 units / mg, for example about 5000 units / mg protein. One unit is defined as the ability to decompose 1.0 micromole of hydrogen peroxide (H2O2) per minute at pH 7.0 at 25°C, and the H2O2 concentration is preferably between 10.3 millimolar and 9.2 millimolar. The term catalase extends to natural proteins and their derivatives, mutants and / or functional equivalents. This term is particularly extended to proteins that do not differ substantially in structure and / or enzymatic activity. The catalase used is preferably of bovine origin.

[0034] It is also possible to use other enzymes to convert glucose, and in particular at least one dehydrogenase. In fact, hydrogen peroxide is not produced during the reaction catalyzed by this enzyme, which is advantageous. Dehydrogenases also work in combination with FAD (see above). A particularly preferred dehydrogenase is flavin adenine dinucleotide-glucose dehydrogenase (FAD-GDH) (EC 1.1.5.9). The term FAD-GDH extends to natural proteins and their derivatives, mutants and / or functional equivalents. This term extends in particular to proteins that do not differ substantially in structure and / or enzymatic activity. Therefore, in order to produce the anode of the electrochemical cell of the biobattery according to the invention, a GDH enzyme protein having an amino acid sequence with at least 75%, preferably 95% and even more preferably 99% identity to one or more GDH sequences shown in a database (e.g. SWISS PROT) can be used in combination with a cofactor. FAD-GDH of aspergillus sp. is particularly preferred and effective, but other FAD-GDH from Glomerella cingulata (GcGDH) or recombinant forms expressed in Pichia pastoris (rGcGDH) may also be used. The FAD-GDH used in the exemplary embodiment is a FAD-GDH from aspergillus sp. (SEKISUIDIAGNOSTICS, Lexington, Massachusetts, catalog number GLDE-70-1192) having the following characteristics:

[0035] Appearance: Freeze-dried yellow powder.

[0036] Activity: >900U / mg powder at 37°C.

[0037] Solubility: Easily soluble in water, concentration: 10mg / mL.

[0038] Unit activity: The amount of enzyme that converts one micromole of glucose per minute at 37°C.

[0039] Molecular weight (gel filtration) 130 kDa.

[0040] Molecular weight (SDS Page): Diffuse 97 kDa band indicating glycosylated protein.

[0041] Isoelectric point: 4.4.

[0042] K m Value: 5.10 -2 M (D-glucose).

[0043] The porous conductive material can also include aromatic molecules acting as redox mediators, such as 1,4-naphthoquinone, to improve electron exchange. Other molecules selected from the group formed by the following can also be considered: 9,10-phenanthroline, 1,10-phenanthroline-5,6-dione, 9,10-anthraquinone, phenanthrene, 1,10-phenanthroline, 5-methyl-1,10-phenanthroline, pyrene, 1-aminopyrene, pyrene-1butyric acid and a mixture of two or more of these. In the case of an enzyme system including FAD-GDH or GOx, it is particularly advantageous to use such compounds.

[0044] The oxidant of the biofuel cell may advantageously be molecular oxygen, and in particular the oxygen contained in air.

[0045] When the oxidant is molecular oxygen O2, the enzyme system that can be used at the cathode can advantageously include bilirubin oxidase (BOD). BOD is an oxidoreductase (EC classification 1.3.3.5, CAS number 80619-01-8; April 2018) that catalyzes the following reaction:

[0046] 2bilirubin+O(2)<=>2bililiverdin+2H(2)O.

[0047] The most widely used bilirubin oxidase is the bilirubin oxidase extracted from Myrothecium verrucaria. However, it is contemplated that BOD from other sources may be used. The activity of BOD is preferably greater than 15 units / mg protein, preferably greater than 50 units / mg, such as about 65 units / mg protein. One unit is defined as the ability to oxidize 1.0 micromole of bilirubin per minute at 37°C at pH 8.4. The term BOD refers to native proteins and derivatives, mutants and / or functional equivalents thereof. This term is particularly extended to proteins that have no substantial differences in structure and / or enzymatic activity.

[0048] Protoporphyrin IX (CAS No. 553-12-8; April 2018) is a compound with a porphyrin unit, and its crude chemical formula is C 34 H 34 N4O4. It is used to functionalize porous conductive materials, and in particular nanotubes, and allows better orientation of enzymes such as BOD. Therefore, it is preferably included in the material constituting the cathode.

[0049] The solid mass combining the porous conductive material with at least one enzyme and / or an enzyme system is preferably in the form of a block or a sheet (for example, a circle) advantageously obtained by compressing a mixture of the elements. The mass can be easily obtained by compression and adopt any desired specific shape. Specifically, the bioanode and / or biocathode according to the invention can take the form of a relatively small (1 cm to 2 cm in diameter) or even very small (less than 0.5 cm in diameter) sheet (for example a circle or a polygon). The thickness of such a sheet can vary between 3.5 mm and 0.2 mm, for example 0.25 mm. Therefore, the biobattery according to the invention can have different shapes and smaller sizes. Specifically, it can occupy only less than or equal to 2 cm. 3 , preferably less than or equal to 1 cm 3 or even less than or equal to 0.75cm 3 It can be designed in particular to be able to replace "button-type" batteries.

[0050] According to a particularly preferred aspect of the invention, the anode thus comprises a GOx enzyme, preferably in combination with a catalase or FAD-GDH enzyme. In this case, the biofuel is therefore glucose. In both cases, the bioanode also comprises a glucose oxidation mediator, such as a 1,4-naphthoquinone compound. Preferably, the biocathode comprises an enzyme that reduces oxygen, and more precisely BOD, which is preferably combined with protoporphyrin IX. The terms biocathode and bioanode refer to the presence of biological material, such as an enzyme, in their structure. In the case of the biofuel cell of the invention, they will be used in a manner equivalent to the cathode and anode.

[0051] The device according to the invention comprises a separating porous membrane arranged between the anode and the cathode, which is electrically insulating and permeable to the liquid medium. This membrane allows in particular ionic substances to pass between the anode and the cathode.

[0052] According to a particular variant of the invention, this film may be a thin sheet (less than 200 μm thick) of paper having a low surface density (for example less than or equal to 150 g / m 2 ). Specifically, such membranes have a thickness of less than 150 μm, preferably less than 100 μm, preferably less than 75 μm, which is preferably biodegradable. This option is particularly preferred when the means for storing biofuel and providing liquid medium to the anode surrounds and supports the bioanode and / or anode sheet, and optionally the biocathode of one or more biocells.

[0053] According to another preferred variant of the invention, the separating porous membrane, which is electrically insulating and permeable to the liquid medium, is also a member for storing the biofuel and making the liquid available. Advantageously, this storage member is as described above.

[0054] The biobattery according to the invention also comprises electrical connection means, which are usually incorporated with a conductive material. These means may be in the form of a layer, tab or wire. Such layers, tabs or wires preferably have a low thickness, a high thermal conductivity and / or electrical conductivity, and may comprise or be (substantially) made of highly oriented graphite. Thus, it is possible to use flakes or tabs of pyrolytic graphite (pyrolytic graphite flakes). Its thickness may be selected from 10 μm to 500 μm, preferably 17 μm to 300 μm, and preferably in the range of 40 μm to 100 μm. It may be selected from the group consisting of a thickness of 10, 17, 25, 40, 50, 70 and 100 μm. Its thermal conductivity (in the longitudinal plane of the flake) may be 500 W / (mK) to 2000 W / (mK), preferably 700 W / (mK) to 1950 W / (mK), and preferably 900 W / (mK) to 1350 W / (mK). It may be selected from the group consisting of the following thermal conductivity values: 700, 1000, 1300, 1350, 1600, 1850 and 1950 W / (mK). This layer may also have an electrical conductivity of more than 5,000 S / cm, preferably greater than or equal to 8,000 S / cm, for example about 10,000 S / cm. However, it may have a higher conductivity, for example about 20,000 S / cm, especially if the thickness of the layer is less than 40 μm. This layer may also have heat resistance, for example resistance to temperatures greater than 200° C., preferably greater than 300° C., for example about 400° C.

[0055] The device according to the invention advantageously comprises an external coating, which may be a protective layer or membrane, which partially covers one or more electrochemical cells of the device. The external coating is preferably flexible, adhesive, non-toxic, chemically stable, electrically insulating, radiation-insensitive and / or has a wide operating temperature range (e.g., from -150°C to 200°C, or even a temperature of about 260°C). This coating or external protective membrane may comprise or be made (essentially) of a glass fabric impregnated with a relatively inert material, such as a perfluorinated polymeric material of the PTFE (polytetrafluoroethylene) type or a silicone-based material. The PTFE may be a polytetrafluoroethylene from Du Pont de Nemours. From Asahi Glass From Dyneon The membrane or coating is preferably impregnated with more than 50% by weight, preferably 50% to 70% by weight, preferably 57% to 64% by weight of said material relative to the total weight of the membrane. Its thickness may be one tenth of a millimeter or even one hundredth of a millimeter. For example, it may be selected from the range of 0.03 mm to 0.50 mm, preferably 0.05 mm to 0.30 mm and preferably 0.06 mm to 0.14 mm, for example 0.07 mm (NF EN ISO 2286-Dec. 3, 2016). According to a preferred aspect of the invention, the coating or protective film comprises an adhesive layer, preferably water-resistant, so that it adheres to the outer surface of one or more electrochemical cells of the biobattery according to the invention. According to a specific aspect, this membrane can be directly attached to a surface of the anode and / or cathode, or directly attached to a part of the circuit member. According to another preferred aspect, this external coating, which is preferably flexible and insulating, comprises one or more openings positioned and dimensioned to allow liquid to pass to the anode and / or gas to pass to the cathode. This opening may be pre-cut in the coating: for example, it may be in the form of a series of small circular openings located opposite the biocathode. Additionally or alternatively, this opening may be formed by the fact that the coating does not completely surround the biobattery comprising one or more electrochemical cells and the storage member, but leaves an opening that allows access to these elements. Thus, for a device of generally planar shape, the opening may be left on the edge of the device.

[0056] According to an advantageous aspect of the invention, when the bioanode and / or biocathode (which may be in the form of a sheet or button) is held in a frame, the frame is the means for storing biofuel and making the liquid medium available, or the frame is an electrically insulating material, such as PTFE.

[0057] Thus, according to a first embodiment, the anode is inserted into a storage member, which may be, for example, a sheet of absorbent material as described above. This storage member will therefore also act as a frame and / or support and maintain the bioanode and possible biocathode in place, and will generally keep them in contact with the liquid medium and the biofuel contained therein, in direct contact with the latter. According to this variant of the invention, the device may comprise several electrochemical cells of the type described in the present application, which are connected in series. Such a device therefore consists of a stack of electrochemical cells, the number of cells being generally not greater than ten. For example, three or four individual cells may be stacked.

[0058] According to another embodiment described above, the storage member is also the membrane of the biobattery. In this case, the anode (and possibly the cathode) can be inserted into a frame or fixture made of an insulating material, such as PTFE (polytetrafluoroethylene). This frame preferably has an opening sized to receive one or more bioelectrodes and making it possible to accommodate and / or position the electrodes (anode or cathode). In fact, according to this variant of the invention, the frame can contain several electrodes that can be of anode or cathode type. The frame is sized so that when two frames are placed opposite each other, it is possible to place the anode and cathode opposite each other and thus create several electrochemical cells. It is then appropriate to position the switch member to connect these electrochemical cells in series.

[0059] The object of the invention is also a method for manufacturing a biobattery as described in the present application. This method comprises the use of the described external coating sheet and comprises the steps of positioning the means for switching on, at least one electrode facing said switching means (bioanode or biocathode), the storage means and possibly the membrane on the inner face (preferably adhesive) of the external coating. The external coating sheet is dimensioned so that once the elements of the biobattery are positioned on the adhesive surface, there is a free surface around the periphery of these elements. This free surface is positioned and dimensioned so that these elements join together and constitute the biobattery.

[0060] According to a variant of the method according to the invention, the switching member is first positioned on the inner face of the coating and then the frame (or template) is superimposed. Next, the mixture in the form of a powder or paste constituting the anode or cathode according to the invention is positioned inside the opening of the frame and this assembly is compressed in situ to obtain a solid mass constituting the anode or cathode. Once the storage member is positioned between the layers, this step can be repeated to form the missing electrode (cathode or anode) and to assemble the two coatings to form a biobattery according to the invention. The two parts are advantageously joined by an adhesive present on the inner part of the outer coating.

[0061] The invention also relates to a biobattery as described in the present application and also including an aqueous liquid, the liquid optionally including a biofuel. In practice, the biofuel may already be present in the device in a dry and / or solid and / or insoluble form, and / or be able to migrate to the enzyme site. For example, it can be incorporated into a fuel storage member or positioned near the fuel storage member. When water (pure or impure) is added, the biofuel (e.g., sugar) thus present dissolves in the medium, which allows electrochemical exchange to occur. Alternatively or additionally, the added liquid includes the biofuel. This can be, for example, a physiological fluid, such as blood, urine or saliva or an alcohol or glucose drink.

[0062] A subject of the invention is also a method for obtaining a biobattery, said method comprising placing a biobattery according to the invention as described in the present application in the presence of a liquid, preferably an aqueous liquid, optionally comprising a biofuel such as glucose, starch or ethanol.

[0063] Another object of the invention is a device comprising a biobattery according to the invention and an electrical receiver (that is to say a device using (receiving) electric current), to which the biobattery is electrically connected. Such a device may be a test, in particular a test for biological fluids: for example a pregnancy test or a blood sugar test. Alternatively or additionally, the biobattery (and / or the device) according to the invention may be incorporated into an electronic device with an electronic display and / or light emission. More generally, the device according to the invention is of the type that uses metal derivatives to work with button-type batteries. Such a device according to the invention may advantageously be disposable and / or biodegradable.

[0064] Another subject of the invention is a kit for producing a biobattery as described in the present application and comprising a biobattery as described in the present application, the associated instructions for use and possibly a container comprising an aqueous liquid as described above.

[0065] Another object of the invention is the use of a thick blotting paper as described above for the manufacture of a biobattery or for the manufacture of a device for obtaining a biobattery, preferably a biobattery according to the invention. Preferably, the blotting or blotting paper is 2.6 mm ± 0.2 mm thick.

[0066] Another subject of the invention is the use of a biobattery according to the invention for generating electric current. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] Figure 1 A partially exploded view of the device according to the present invention as described in Example 1.

[0068] Figure 2 Shown are polarization and power curves of a GOx / BOD biobattery according to Example 1 produced using the apparatus of Example 1 and a 5 mM glucose solution.

[0069] Figure 3 Indicated by Figure 1 Device and polarization and power curves of the FAD-GDH / BOD biobattery according to Example 1 generated from 5 mM glucose solution.

[0070] Figure 4 Graphs showing polarization and power curves of a GOx / BOD biobattery according to an embodiment of Example 2, with a 5 mM glucose solution as the fuel.

[0071] Figure 51 shows the polarization and power curves of the GOx / BOD biobattery according to the embodiment of Example 2, with the fuel being 150 mM glucose solution.

[0072] Figure 6 According to Example 3, Polarization and power curves of FAD-GDH / BOD biocell produced on carbon and fueled by 150 mM glucose solution.

[0073] Figure 7 Shows the polarization and power curves of the FAD-GDH / BOD biocell produced on MWCNTs according to Example 1, with the fuel being 150 mM glucose solution.

[0074] Figure 8 Energy production by continuous discharge at 6 kΩ in μW.h versus time (minutes) is shown for the biobattery of Example 3 and total glucose consumption of the mat immersed in 5 mM and 150 mM glucose.

[0075] Fig. 9 Energy production by continuous discharge at 6 kΩ in μW.h versus time (minutes) and total glucose consumption of the mat immersed in 150 mM glucose are shown for the biobattery of Example 3 (carbon black) and the biobattery of Example 1 FAD-GDH / BOD on MWCNTs.

[0076] Fig.10 Contains a partially exploded view of the structure of the biobattery 10 shown in Example 4 and a front view thereof, and a cross-sectional view on the left.

[0077] Fig.11 Contains a partially exploded view of the structure of the biobattery 20 shown in Example 5 and a front view thereof, and a cross-sectional view on the left.

[0078] Fig.12 1 shows the polarization and power curves of the biobattery according to Example 4 at t=0, t=7 days and t=1 month for 150 mM glucose solution.

[0079] Fig.13 Energy production by continuous discharge at 6 kΩ in μW.h versus time (minutes) and total glucose consumption of 150 mM glucose solution are shown for the biobattery of Example 4.

[0080] Fig.14 For 150 mM glucose solution, Example 5 and Fig.11 Polarization and power curves of the biobattery described in .

[0081] Fig.15Shown are the polarization and power curves of the biobattery described in Example 6 for 150 mM glucose solution. DETAILED DESCRIPTION

[0082] Reagents:

[0083] Type VII glucose oxidase (GOx) from Aspergillus niger (April 2018: EC number: 1.1.3.4, CAS number: 9001-37-0, molecular weight: 160 kDa (gel filtration) > 100,000 units / g) was from the company Sigma-Aldrich (product code G2133).

[0084] Catalase from bovine liver (April 2018: EC number: 1.11.1.6, CAS number: 9001-05-2, molecular weight 250 kDa, 2000 units / mg to 5000 units / mg) was also from Sigma-Aldrich, Colorado (product code C1345).

[0085] Bilirubin oxidase (BOD) from Myrocera verrucosa (April 2018, EC No. 1.3.3.5, CAS No.: 80619-01-8, 15-65 units / mg) was obtained from Sigma-Aldrich (product code B0390).

[0086] 95% pure protoporphyrin IX was also obtained from Sigma-Aldrich, Colorado (product code P8293).

[0087] Flavin adenine dinucleotide-dependent glucose dehydrogenase (FAD-GDH, 11580 units / mg solid (one unit of activity: the amount of enzyme that converts one micromole of glucose (β-dextrose) per minute at 37°C) from Aspergillus species (April 2018: EC number 1.1.5.9) was from the company SEKISUI.

[0088] Multi-walled carbon nanotubes (MWCNTs) were purchased from Nanocyl (purity > 95%, diameter 10 nm, length 1.5 μm).

[0089] The brand of carbon black XC72R was purchased from CABOT corporation.

[0090] The current collecting microporous gas diffusion (GDL) layer was purchased from Paxitech. It consisted of a narrow network of carbon fibers in the form of carbon felt and had a thickness of 210 μm and a through resistivity of 8 mΩ cm. 2 and a permeability to air of 70 seconds.

[0091] The porous paper used as pad is an extra thick blotter paper (grade 707) from VWR reference 732-0604. This is 100% cotton blotter paper, free of additives, and made with ultrapure water. Its texture is smooth and regular, and its structure is uniform. For a thickness of 2.6 mm, its areal density is 703 g / m 2 Its given technical characteristics are a filtration time (according to Herzberg) of 120 seconds / 100 ml (with a water column of 100 mm) and a rise of 75 mm in 96 seconds according to the Klemm test (capillary permeability).

[0092] The 140 μm thick cellulose sheets used were of the Whatman type (Qualitative filter papers for technical use, grade 0903) published by Sigma Aldrich (ref WHA10334885).

[0093] The protective film is an adhesive sheet of a fabric or glass film impregnated with 70 μm thick PTFE (TISOFLON 3AD; ISOFLON) and having a PTFE impregnation rate of 61% by weight. The adhesive surface of this film is covered with protective PTFE (Teflon TM This membrane is covered with a protective Teflon sheet which can serve as a holding frame or template for the bioanode and / or bio-cathode sheets according to the invention.

[0094] The enzyme was stored at -20°C. Distilled water was obtained by using Millipore Ultrapure TM The system was obtained by purifying water to a resistivity of 15 MΩ×m. High purity oxygen and argon were from MESSER. Before use, the glucose solution was converted to β-D-glucose overnight. All other reagents (including 1,4-naphthoquinone) were from Sigma-Aldrich.

[0095] For the electrochemical characterization of the biobattery, the anode was defined as the working electrode, while the cathode was connected as the reference electrode. All experiments were performed at pH 7 in Mcllvaine or phosphate buffer with 5 mmol L -1 (close to the concentration of some body fluids) or 150mmol L -1 The solution was dripped onto the edge of the reservoir, at least onto one edge that was not completely covered with the insulating coating. The biocell was connected to a computer running EC-lab10.39 software. VMP3 multi-channel potentiostat. Polarization and power curves were recorded after 30 seconds of discharge. All experiments were performed at room temperature (about 20°C).

[0096] The biocathode and bioanode exemplified below are solids formed into compressed disks.

[0097] Example 1 ( piece Inserted into porous sheet)

[0098] For the biocathode, carbon nanotubes (MWCNT) were mixed with protoporphyrin IX in the presence of DMF (dimethylformamide), followed by heating at 80°C for about 12 hours. Protoporphyrin IX promotes the orientation of the enzyme protein relative to the nanotubes. The nanotubes functionalized in this way were rinsed and filtered several times with distilled water. 35 mg of MWCNT functionalized with protoporphyrin IX were ground in the presence of 15 mg of BOD and 100 μl of distilled water.

[0099] For the bioanode, 35 mg MWCNT, 15 mg GOx, 10 mg catalase from bovine liver and 5 mg 1,4-naphthoquinone were ground with 100 μL distilled water. For the other bioanode based on FAD-GDH, 35 mg functionalized MWCNT, 15 mg FAD-GDH and 5 mg 1,4-naphthoquinone were ground with 100 μL distilled water.

[0100] Each homogenous slurry was then compressed separately onto an electrical contact GDL tab using a hydraulic press to obtain a sheet of 1 cm in diameter and 2 mm in thickness. In this case, this 9 or 9' GDL tab acts both as a current collector and as a support for the compression of the carbon paste.

[0101] Holes of the size and shape corresponding to the anode and cathode sheets are made in a pad of 2.6 mm thickness and 25 mm x 25 mm in size. Each pad or "mat" will act as a frame for the sheets. The biobattery device is then assembled: each of the resulting sheet / tab associations is positioned from its rear inside the opening of the pad so that the GDL tab is positioned on the outside and protrudes relative to its corresponding pad. The bioanode and biocathode are thus formed. A thin sheet of Whatman cellulose, acting as an electrical insulator, is placed between the bioanode and the biocathode. This assembly forms the basis of the electrochemical cell. Figure 1 is a semi-exploded view of such a device. An enzyme sheet or bioanode 5 comprising GOx or FAD-GDH is positioned in the fuel tank 3, with the GDL tab 9 protruding from the rear. Symmetrically, an enzyme sheet or biocathode 7 comprising BOD is positioned in the 3' pad, with the 9' GDL tab also protruding from its rear. A porous sheet of electrical insulation 8 is placed between the bioanode 5 and biocathode 7 and their respective frames 3 and 3'.

[0102] This device is then encapsulated by an adhesive protective film of glass fabric and PTFE 70 μm thick (not shown) covering the back of both electrodes. The protruding GDL tab portion is substantially covered with this protective film. In addition, 4 holes of 2 mm in diameter made in the protective film are located at the back of the biocathode and allow oxygen to diffuse from the air inside the device and supply it to the biocathode 7.

[0103] Figure 2 and 3 GOx BiopIies( Figure 2 ) and FAD-GDH( Figure 3 ). The power obtained in the case of FAD-GDH (0.38 mW) is greater than that obtained in the case of GOx (0.27 mW). This is due to the fact that FAD-GDH is more active than GOx and it does not produce H2O2 as a byproduct. In fact, H2O2 can increase the instability of the cell and inhibit the activity of the BOD enzyme at the cathode.

[0104] Example 2: Stacking

[0105] Figure 3 and Figure 4 A stack of 3 cells with FAD-GOX / BOD biocathode / anode is schematically shown in FIG. 1 (GDL tabs not shown). This stack is produced by leaving only the external tabs protruding to close the circuit. Once the cells are juxtaposed, the stack is covered with an adhesive film made of glass fiber and PTFE fabric in the same manner as the device of Example 1.

[0106] This example shows the ease of stacking these cells, from 0.27 mW and 0.62 V fem for a single cell to 0.82 mW and 1.7 V fem for a stack of 3 cells with a pad immersed in a 5 mM glucose solution ( Figure 4 ). Concentrated glucose solution (150 mM) resulted in a high power of 2.2 mW ( Figure 5 ). Figure 4 and 5 The effect of these two different glucose concentrations on the obtained performance is shown.

[0107] Example 3: FAD-GDH / BOD biobattery using carbon black support

[0108] To overcome the problems that may be associated with carbon nanotubes in terms of obtaining commercial samples or suspicion of their toxicity, MWCNTs have been replaced by carbon black, which is already used in many commercial products.

[0109] The enzyme tablets were obtained by the same method as in Example 1, but with carbon black The method of Example 1 was then used to produce a 1-cell biobattery. Figure 6 When placed in the presence of 150 mM glucose solution, the Polarization and power curves of this FAD-GDH biobattery on carbon.

[0110] Figure 7 The polarization and power curves of the FAD-GDH biobattery on MWCNTs of Example 1 are shown when introduced with a glucose solution of the same concentration (150 mM). For a recharge of 150 mM glucose (approximately 0.5 mL), the power delivered by the MWCNT- and Vulcan carbon (carbon black)-based cells were 1.3 mW and 1.2 mW, respectively. Both materials provide similar power and therefore can be used depending on the technology and environmental constraints necessary to manufacture these cells.

[0111] Figure 8 Shown are energy production in μW.h versus time (minutes) at continuous discharge at 6 kΩ for the biobattery of Example 3 (carbon black) and total glucose consumption for mats immersed in 5 mM and 150 mM glucose. Fig. 9 Energy production at continuous discharge at 6 kΩ in μWh versus time (minutes) and total glucose consumption of the mat immersed in 150 mM glucose are shown for the biobattery of Example 3 (carbon black) and the biobattery of Example 1 FAD-GDH / BOD on MWCNTs.

[0112] The best performance of the MWCNT-based cells was obtained, which made it possible to produce 400 μWh after continuous discharge, which consumed all the available glucose of 150 mM.

[0113] Example 4: Single-reservoir biobattery

[0114] Fig.10 A diagram of the structure of a biobattery 10 according to this particular example is included.

[0115] For the biocathode, 8.75 mg MWCNTs functionalized with protoporphyrin IX as described in Example 1 were ground in the presence of 3.75 mg BOD and 25 μΐ distilled water. For the bioanode, 8.75 mg MWCNTs, 3.75 mg GOx, 2.5 mg catalase from bovine liver and 1.25 mg 1,4-naphthoquinone were ground with 25 μΐ distilled water.

[0116] Each sheet 15 and 17 is formed in situ on a frame comprising a PTFE sheet 12 or 12' having a thickness of 0.25 mm and pierced with circular holes having a diameter of 1 cm. This template is placed on a support consisting of an adhesive sheet of glass fiber and a PTFE 11 or 11' having a thickness of 70 μm. The GDL tab 19 or 19' is positioned between the circular holes and the adhesive sheet 11 or 11' relative to the circular holes of the PTFE sheet 12 or 12'. This sheet 11 and 11' is not shown in the exploded view. A sufficient amount of each homogenous paste of the bioanode or biocathode (an amount of about 12 mg per sheet makes it possible to fill the template) is positioned in the hole and compressed directly onto the support by a press. This makes it possible to obtain sheets having a diameter of 1 cm and a thickness of 0.25 mm. These sheets on the support formed in situ can then be used as bioanode and biocathode.

[0117] The adhesive sheet 11' of the biocathode is perforated with 4 holes 14 of 2 mm diameter to allow oxygen to diffuse from the air to the biocathode. Fig.10 The adhesive cover sheet 11 or 11 ' is not shown in the exploded view of , but the position of the holes is indicated therein. The dimensions of the PTFE sheet 12 or 12' acting as a frame are approximately 20 mm x 20 mm. The outer support sheets 11 and 11 ' acting as protection have larger dimensions and enable the fixing or joining of the elements of the device by contact of their facing adhesive surfaces. Their adhesive faces are face to face, which can join each other and fix the biobattery on some of its sides. An example of this variant is Fig.10 The subject of the photograph framed in . It is possible to see a flexible outer sheet 11 ' pierced with holes 14 and extending laterally from the right and left sides to cover and adhere to the symmetrical parts of the sheet 11 overlapping each other. A 10 euro cent coin allows to observe the size of the biobattery obtained.

[0118] A thick ink absorbing sheet 13 of substantially the same size as the PTFE sheet (as used in the previous examples) acting as a frame is then placed between the anode sheet 15 and cathode sheet 17. The GDL tabs 19 and 19' act as current collectors and supports for the sheet 15 or 17.

[0119] The GDL tab 19 is thus positioned facing the anode sheet 15 and the GDL tab 19' is also positioned facing the cathode sheet 17. These two tabs 19 and 19' protrude from their respective supports 12 and 12'. They are positioned between the PTFE sheet 12 or 12' and the external support sheet 11 or 11'. These tabs 19 and 19' act as current collectors and supports for the pads associated therewith and make it possible to connect the device to an electrical receiver. In the front view of the biobattery 10, the tabs 19 and 19' protrude from opposite sides of the device according to the invention, while in the exploded view, these tabs 19 and 19' are shown protruding from the same side. Both arrangements are possible.

[0120] Regardless of the final specific shape of the biocell according to the invention, it comprises a channel allowing the glucose based fuel to contact the pad 13. Here, the glucose solution is added by injecting it using a syringe.

[0121] Fig.12 Demonstrating that whether measured after one week or one month, the biobattery maintained its performance. Fig.13 It was confirmed that by testing the discharge of the biobattery, whether it was started after a week or a month, it still maintained 100% of its performance. This verified the ability of the biobattery to power a device without performance loss for at least 1 month after its manufacture.

[0122] Example 5 Series Connection piece Biobattery

[0123] Fig.11 A diagram of the structure of a biobattery 20 according to this particular example is included.

[0124] The anode and cathode sheets used were of the same type as those used in the apparatus of Example 4.

[0125] Four sheets, two anode sheets 25 and 35 and two cathode sheets 27 and 37, were placed on the bonding surface of the first bonding sheet of glass fiber and PTFE 31 and placed in four circular openings of a PTFE sheet 32 ​​having a size of 35 mm×35 mm. These sheets had the same material and thickness as those described in Example 4. The four sheets were positioned in a quadrilateral pattern, and each anode sheet 25 and 35 was arranged diagonally to each other, as were the cathode sheets 27 and 37.

[0126] Another set of four sheets of PTFE sheet 32' is arranged on the second sheet of fibers and PTFE 31'. On the second sheet 32', the four sheets alternate in a symmetrical arrangement: two anode sheets 45 and 55, and two cathode cells 47 and 57 are each diagonal to each other.

[0127] The electrochemical cells are arranged in series by using GDL tabs 29, 29' and 29" positioned between the adhesive outer sheet 31 and the PTFE sheet 32 ​​and tabs 39 and 39' positioned between the outer adhesive sheet 31 and the PTFE sheet 32'. It should be noted that Fig.11 In the exploded view of the PTFE sheet 32, the position of the tabs on the PTFE sheet 32 ​​is seen by means of transparency: the tabs are actually positioned behind the face of the frame shown. This is done to be able to understand the corresponding positioning of the tabs. Their relative position is better explained in the relevant cross-sectional view. On the PTFE sheet 32', the tab 39 horizontally positioned between the sheets 45 and 57 makes it possible to connect the electrochemical cell composed of the anode 45 and the cathode 27 to the electrochemical cell composed of the anode 35 and the cathode 57. Similarly, the tab 29" vertically positioned between the sheets 35 and 37 makes it possible to connect the battery composed of the anode 35 and the cathode 57 to the battery composed of the anode sheet 55 and the cathode sheet 37. The tab 39' horizontally positioned between the sheets 55 and 47 makes it possible to connect the battery composed of the anode sheet 55 and the cathode sheet 37 to the battery composed of the anode sheet 25 and the cathode sheet 47. The tabs 29 and 29', which are in contact with the cathode sheet 27 and the anode sheet 25, respectively, protrude in opposite directions to the outside of the circuit and allow the device to be connected to an electrical receiver (not shown).

[0128] As in Example 4, the sheets are formed by adding a certain amount of paste in a 10 mm diameter circular hole preformed in the sheet 32 ​​or 32' for in situ compression. Tabs 29, 29', 29", 39 and 39' are pre-positioned between the sheets of glass fiber and PTFE 31 and 31" and PTFE sheets 32 and 32' acting as supports.

[0129] At the back of each of the 4 biocathodes 27, 37, 47 and 57 (and the corresponding parts of the GDL tabs), a set of 4 holes 24 with a diameter of 2 mm are made on the glass fiber and PTFE support sheets 31 and 31 ' and allow oxygen to diffuse from the air to the biocathode. Although the openings are formed in the sheets 31 and 31 ' and are not shown in the partially exploded view, the position of these series of openings 24 is also indicated on the partially exploded view of the biobattery 20.

[0130] A reservoir or pad 3 mm thick and substantially the same size as the PTFE sheets 32 and 32' or slightly smaller is inserted between the two sheets carrying the PTFE sheets 31 and 31', sheets 27, 35, 37, 25 and 45, 57, 55, 47, and the sheets carrying the tabs 29, 29' and 29". This pad 23 is in direct contact with one side of the sheets 27, 35, 37, 25, 45, 57, 55 and 47. This pad is made of thick blotting paper of the same type as previously described in Example 4.

[0131] The outer coating sheets 31 and 31 ', acting as protection and support, are larger in size than the PTFE sheets and therefore protrude from these sheets 32 and 32'. These sheets 31 and 31 ' thus make it possible to fix or join the elements of the biobattery by contact with their opposing adhesive surfaces. Their adhesive faces are opposite, they can join each other and fix the biobattery on some of its sides. An example of this variant is Fig.11 A flexible outer sheet 31 ′ pierced with a series of holes 14 can be seen, the edges of which extend transversely to the right and to the left to cover and adhere to symmetrical parts of the sheet 31 by overlapping each other.

[0132] The sheets 32 and 32' are placed face to face so that each anode sheet 25, 35 placed on the first sheet 32 ​​is opposite to the cathode block 47 and 57 placed on the other PTFE sheet 32. Likewise, each anode sheet 27, 37 placed on the first PTFE sheet 32 ​​is opposite to the cathode sheet 45 and 55 placed on the other PTFE sheet 32'. Then, a reservoir 23 made of a thick water-absorbing sheet of the same size as the PTFE sheets 32 and 32' is placed therebetween. Then, the biobattery 30 is obtained by bringing the outer covering sheets 31 and 31' into contact with each other.

[0133] Example 6: Comparison of the previous example of tandem biobattery with a single cell

[0134] A biobattery 40 according to the invention was produced to compare the efficiency of the tandem device described in Example 5 to that of a pair of cells comprising only equal amounts of material. piece Instead of 4 series installation piece A biobattery of the same type as in Example 5 was produced, comprising a pair of circular bioanodes and biocathodes identical in all respects to Example 5 except for their diameters. piece of biobatteries. piece The diameter is 20mm.

[0135] Fig.14 Display 20mm piece Polarization and power curves of biobatteries. piece If the size of is doubled, then it is approximately multiplied by two. Fig.15 The polarization and power curves are shown for the biobattery described in Example 5. They show that if two biobatteries are placed in series in the same device, the emf and battery power increase by a factor of two.

Claims

1. A biobattery (1, 10, 20) having a biofuel reservoir, the biobattery comprising a first electrochemical cell, the first electrochemical cell comprising: - an anode (5, 15, 25, 35, 45, 55) made of a solid mass comprising a conductive material mixed with a first enzyme capable of catalyzing the oxidation of said biofuel; and a cathode (7, 17, 27, 37, 47, 57) made of a solid mass comprising a conductive material mixed with a second enzyme capable of catalyzing the reduction of an oxidant, and - a separating porous membrane (8) disposed between the anode (5, 15, 25, 35, 45, 55) and the cathode (7, 17, 27, 37, 47, 57), the membrane being electrically insulating and permeable to a liquid medium, the liquid medium comprising a biofuel, - the biobattery further comprises an electrical connection member (9, 9', 19, 19', 29, 29', 29", 39, 39') for electrically connecting the biobattery to an electrical receiver, the electrical connection member allowing current to flow from the cathode (7, 17, 27, 37, 47, 57) to the anode (5, 15, 25, 35, 45, 55); The biobattery (1, 10, 20) is characterized in that it includes a biofuel storage member (3, 3', 13, 23) for storing the biofuel and for providing a liquid medium to the anode (5, 15, 25, 35, 45 and 55), the member includes a hydrophilic porous material in contact with the anode (5, 15, 25, 35, 45 and 55), and the member has a hydrophilic porous material of 500 to 900 g / m 2 Surface density.

2. The biobattery (1, 10, 20) according to claim 1, wherein the biofuel storage member (3, 3', 13, 23) has a thickness of 1 cm to 0.1 mm.

3. The biobattery (1, 10, 20) according to claim 1 or 2, wherein the hydrophilic porous material is a cellulose-based material.

4. The biobattery (1, 10, 20) according to claim 1 or 2, wherein the biofuel storage member for storing biofuel and providing liquid is also the separating porous membrane, and the membrane is electrically insulating and permeable to the liquid medium.

5. The biobattery (1, 10, 20) according to claim 1 or 2, wherein the electrical contact member for contacting the device comprises a tab made of pyrolytic graphite.

6. The biobattery (1, 10, 20) according to claim 1 or 2, wherein the anode (5, 15, 25, 35, 45 and 55) is in the form of a sheet.

7. The biobattery (1, 10, 20) according to claim 1 or 2, wherein the anode is held in a frame, the frame being the biofuel storage member (3, 3', 13 and 23) for storing the biofuel and making the liquid medium available, or the frame being an electrically insulating material.

8. The biobattery (1, 10, 20) according to claim 7, wherein the electrically insulating material is PTFE.

9. The biobattery (1, 10, 20) according to claim 1 or 2, wherein the biobattery comprises an outer covering comprising openings positioned and dimensioned to enable liquid to access the anode and / or gas to access the cathode.

10. The biobattery (1, 10, 20) according to claim 9, wherein the outer covering is flexible and insulating.

11. The biobattery (1, 10, 20) according to claim 1 or 2, further comprising an aqueous liquid medium.

12. The biobattery (1, 10, 20) according to claim 11, wherein the aqueous liquid medium comprises a biofuel.

13. Use of a biobattery according to any one of claims 1 to 12 for generating electric current.