Imprint composition and method for forming a patterned layer using the same
By adjusting the pH value using the reversible reaction products of protic acid and base at the imprinting temperature, the alkalization of the sol-gel composition is promoted, solving the problems of long imprinting time and unstable patterned layer quality, and achieving efficient patterned layer formation and improved production efficiency.
Patent Information
- Application Number
- CN201980039420.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-06-04
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2039-06-04
AI Technical Summary
In existing imprint lithography technology, it is difficult to balance stability and rapid gelation of sol-gel compositions during imprinting time, resulting in low production efficiency, and the density and quality of the patterned layer are greatly affected by the conditions during the curing process.
By using the reversible reaction products of proton-accepting acids and bases as additives at the imprinting temperature, the pH of the composition is adjusted to 4 to 7, and the vapor pressure difference is utilized to promote the alkalization of the composition during imprinting, forming a three-dimensional network and shortening the imprinting time.
It enables the formation of high-quality, dense patterned layers in a short time, improves production efficiency, and reduces sensitivity to environmental conditions, making it suitable for mass production of automated nanoimprinting tools.
Smart Images

Figure CN112272795B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an embossing composition.
[0002] The present invention further relates to a method of forming a patterned layer using such an imprint composition.
[0003] The invention further relates to an optical element and an etching mask, respectively comprising such a patterned layer. Background Art
[0004] Like other imprint lithography techniques, Substrate Conformal Imprint Lithography (SCIL) involves imprinting a layer that has been applied to the surface of a substrate using a patterned stamp. For example, the stamp can be made of silicone rubber (such as polydimethylsiloxane (PDMS)). The layer can be hardened or cured using the stamp during imprinting. When sufficient curing has taken place, the stamp is removed, leaving a patterned layer on the substrate.
[0005] Various types of embossing inks can be used, such as UV curable compositions and sol-gel compositions. After patterning on a carrier (such as a semiconductor substrate), the suitability of the curable compounds used in the embossing medium is determined by its etching characteristics. For this reason, compositions based on inorganic sols and sol-gel materials (such as sols and sol-gels derived from alkoxysilanes) have been shown to be popular due to their excellent etching resistance and selectivity, excellent adhesion and good mechanical and optical properties when condensed into polysiloxane networks. And this type of composition can be used to produce a patterned layer with features having a size ranging from less than ten nanometers to hundreds of nanometers.
[0006] In such compositions, a sol (or solution) is initially formed (e.g., by hydrolysis of an inorganic hydroxide and / or alkoxide). The sol may comprise oligomeric or linear polymeric substances formed by a condensation process, during which water and / or alcohol may be released. During the manufacture of the imprint composition or during imprinting, the sol reacts to form a sol-gel by further condensation processes, which provide a three-dimensional network. Removal of solvents (including water and / or alcohol) from the network, for example by evaporation, results in the formation of a (hardened) inorganic oxide. Sols formed by the hydrolysis and polycondensation of such hydroxide or alkoxide precursors may be considered colloids. The term "colloid" may refer to a solid-liquid and / or liquid-liquid mixture in which solid or liquid particles are dispersed in a liquid medium.
[0007] Such condensation polymerization (polycondensation) reactions are generally reversible reactions which are shifted to the polycondensation side of the equilibrium during the impression of the composition with the permeable stamp. This is because some of the reaction products (e.g. water or alcohol) released when the condensation product is formed are transported away from the reaction site by diffusion into / through the stamp material and by evaporation, thereby disfavoring the reverse (hydrolysis or alcoholysis) reaction.
[0008] However, the application of such sol-gel compositions in imprint lithography is not always straightforward. An important requirement is that the imprint process must be repeatable so that the process can be widely applied on a large scale. For example, the imprint ink comprising the curable compound(s) must have a suitable viscosity to allow easy deposition on the target substrate and must maintain a suitable viscosity until the imprint ink has been imprinted with the stamp, i.e. the ink must be flexible enough to allow it to be molded into the feature pattern on the stamp surface.
[0009] Depending on the conditions, the imprint time (defined as the time during which the stamp is in contact with the ink from liquid to a cured gel layer that allows the stamp to be removed without damaging the pattern) can range from a few seconds to more than 12 hours. Various factors may affect the imprint time, such as the degree of condensation in the sol, the water content in the composition, the presence of cosolvents (Marc A. Verschuuren, "Substrate Conformal Imprint Lithography for Nanophotonics", 2010, Utrecht University, The Netherlands), environmental conditions (e.g., relative humidity during application of the composition to the substrate, temperature during imprinting), the surface chemistry of the underlying material to be imprinted, the critical time from application of the sol-gel layer (e.g., by spin coating, ink jetting, spraying, etc.) until the stamp is applied to the layer, and the pH of the composition. With regard to surface chemistry factors, imprint times for sol-gel layers on silicon can be less than 5 minutes at room temperature, but when the same material and stamp are applied to a surface coated with chrome or aluminum, imprint times can be 4 to 20 hours.
[0010] A key challenge in the application of the present technology involves balancing the requirement for a stable sol-gel imprint ink composition with a sufficiently short imprint time. A stable sol-gel imprint ink composition may include a sol that undergoes gelation relatively slowly, which is beneficial in terms of the shelf life of the ink (i.e., before it is applied to a substrate). However, relatively slow gelation means that more time may be required for hardening. Therefore, longer imprint times may be required, resulting in a loss in product throughput.
[0011] The hardening process is usually accompanied by a significant degree of shrinkage and densification. The rate at which the solvent can be removed can be determined by the porosity characteristics of the gel (e.g., pore size distribution). Moreover, the ultimate microstructure of the patterned layer may be strongly affected by the conditions during the hardening period. Controlling the conditions to obtain a patterned layer with a sufficiently high density in a relatively short imprint time remains a challenge.
[0012] KR 2017 0027926 A discloses a composition and a method for preparing an antifouling-antimicrobial barrier coating.
[0013] CN 104 165 912 A discloses the preparation and application of molecularly imprinted sol-gel polymers on the surface of graphene oxide.
[0014] WO 2008 / 053418 A2 discloses a relief layer and an embossing method for producing the relief layer.
[0015] WO 2012 / 142126 A2 discloses a method for producing a radiation-sensitive sol-gel material. Summary of the invention
[0016] The invention is defined by the claims.
[0017] According to one aspect, there is provided a stamping composition comprising: a sol; and an additive for promoting gelation of the composition during stamping at a stamping temperature between 15°C and 120°C, the additive being a reversible reaction product of a protic acid and a base that accepts protons, wherein the composition has a pH of 4 to 7 when mixed with an equal volume of deionized water and measured at 20°C and 1 atm, and wherein the vapor pressure of the acid is higher than the vapor pressure of the base at the stamping temperature. Stamping may comprise applying the composition to a surface before contacting the resulting composition layer with the stamp, or it may comprise applying the composition directly to the stamp, followed by or not followed by a step of sandwiching the composition applied to the stamp between the stamp and another surface (e.g., of a substrate). The difference in vapor pressure causes the composition to become more alkaline (alkalinized) during stamping. This in turn may promote hardening of the composition.
[0018] A measurement of the pH of a composition can be obtained by diluting a sample of the composition with an equal volume of deionized water and measuring the pH of the resulting mixture at normal temperature and pressure (NTP) (i.e., 20° C. and 1 atm). The present invention is based in part on the recognition that, when measured using this method, adjusting the pH of the composition to between 4 and 7 results in a composition having suitable properties for forming a composition layer suitable for imprinting. This is believed to be due to the fact that such a pH results in the condensation reaction being controlled so that linear oligomers are formed in the sol.
[0019] The composition further comprises an additive which is a reversible reaction product of a protic acid and a base that accepts a proton. In other words, the reaction product can be considered to be an equilibrium mixture of an acid, a base, and a salt of an acid and a base. The pH of the composition can be adjusted to a measurement range of 4 to 7, for example, by using an appropriate amount of an acid and a base, taking into account the pKa of the acid and the pKa of the conjugate acid of the base.
[0020] During stamping, at the stamping temperature, the vapor pressure of the acid is higher than the vapor pressure of the base. Acids with higher vapor pressures can evaporate at stamping temperatures (i.e., between 15°C and 120°C), which pushes the balance associated with the reaction products to one side of the acid and the base. The lower vapor pressure of the base means that it does not evaporate to the same extent as the acid under the stamping conditions. The lower vapor pressure of the base also means that the diffusion of the base into the stamp layer is carried out to a lesser extent than in the case of a more volatile acid. This may increase the alkalization of the composition during stamping. Therefore, during stamping, the concentration of the base in the composition can be increased relative to the concentration of the acid in the composition. In this way, the stamping conditions cause the composition to become alkaline, thereby promoting the formation of a three-dimensional network (i.e., gelation). For example, relative to an acidic composition that does not include a base, the time required for stamping, i.e., the time required for sufficient hardening to remove the stamp, is correspondingly reduced.
[0021] A sol may be considered a colloid. The term "colloid" may refer to a solid-liquid and / or liquid-liquid mixture in which solid or liquid particles are dispersed in a liquid medium. Preferably, a sol is a liquid-liquid mixture.
[0022] The sol may contain a hydrolyzate of at least one of a trialkoxysilane and a tetraalkoxysilane. When the sol contains a hydrolyzate of a trialkoxysilane and a tetraalkoxysilane, the molar ratio of the tetraalkoxysilane to the trialkoxysilane is preferably 1:1 to 0.45:0.55. It has been found that when a combination of alkyltrialkoxysilane and tetraalkoxysilane in the above ratio is used, a desired degree of crosslinking in the gel can be ultimately obtained. Preferably, the tetraalkoxysilane is selected from tetramethoxyorthosilicate and tetraethoxyorthosilicate, and the trialkoxysilane is selected from methyltrimethoxysilane and methyltriethoxysilane.
[0023] Alternatively or additionally, the sol may comprise a hydrolysis product of at least one of a titanium alkoxide, a zirconium alkoxide and a hafnium alkoxide.Using such metal alkoxide derived sol-gel systems, high quality patterned layers may be obtained in relatively short imprint times.
[0024] The base may, for example, include triethanolamine. This amine has a relatively low vapor pressure (<1.3 Pa at 20°C) at printing temperatures (i.e. between 15°C and 120°C), which means that when it is combined with an acid (e.g. formic acid) having a vapor pressure higher than that of the amine, the composition can be alkalized during printing, thereby reducing the printing time.
[0025] Alternatively or in addition, the base may comprise an alkoxysilyl functionalized amine and the sol-gel composition comprises the condensation product of the alkoxysilyl functionalized amine and the hydrolysis product of the above tetraalkoxysilane and / or alkoxysilane. The alkoxysilyl functionalized amine is preferably aminopropyltriethoxysilane. By incorporating the base into the polymer structure in this way, the vapor pressure of the base can be very low. Provided that the vapor pressure of the acid is high enough at the imprint temperature, the composition can be alkalized during imprinting, thereby reducing the imprinting time, as previously described.
[0026] The acid may include at least one of the compound represented by Formula 1 and the compound represented by Formula 2;
[0027] Formula 1
[0028]
[0029] Where R 1 is hydrogen, methyl or propyl;
[0030] Formula 2
[0031]
[0032] Where R 2 and R 3Each is selected from hydrogen and C1-C3 alkyl.
[0033] Regarding the compound represented by Formula 1, the compound can reversibly react with a base to form a salt, so that at the imprint temperature, by evaporating the acid from the composition, the equilibrium can be pushed to the side of the acid and the base. In this regard, formic acid (R 1 =H) has a vapor pressure of 4600 Pa at 20°C; acetic acid (R 1 =Me) has a vapor pressure of 1500 Pa at 20°C; and propionic acid (R 1 =Et) has a vapor pressure of 390 Pa at 20°C. The relatively high vapor pressure of these compounds at the printing temperature (i.e., 15°C to 120°C) may facilitate their evaporation during printing. Provided that the vapor pressure of the base is low enough at the printing temperature, the composition can be alkalized during printing, thereby reducing the printing time, as described above.
[0034] Similar considerations apply to compounds represented by Formula 2. The carbon between the two carbonyl carbons carries an acidic proton. For example, acetylacetone (R 2 =R 3 =Me) is about 9 (ionic strength = 0) at 25°C in aqueous solution, and the vapor pressure of acetylacetone is 920 Pa at 20°C.
[0035] The colloidal sol may include a solvent that is preferably selected so that the above-mentioned linear oligomers do not phase separate (i.e., remain dissolved) from the colloidal sol. The solvent may have a sufficiently low vapor pressure to avoid significant evaporation of the solvent during the deposition of the composition on the substrate, because this may cause premature phase separation of the oligomer, which may deteriorate the quality of the structure formed by the embossing process (e.g., because the uniform deposition of the composition may become a problem). Therefore, the colloidal sol may include an alcohol, preferably at least one of 1-propanol, 2-propanol, 1-butanol, 2-butanol, tert-butanol and 1-methoxy-2-propanol. Alternatively or in addition, the colloidal sol may include water, which may participate in hydrolysis during the formation of the colloidal sol.
[0036] According to another aspect, there is provided a kit for forming a composition as defined above, wherein the kit comprises a first component and a second component, the first component comprising an acid and a sol, and the second component comprising a base.
[0037] As mentioned above, acidic conditions are advantageous in terms of the shelf life of the sol. The first component of the kit comprises an acid and a sol, and thus can have a shelf life that allows, for example, storage and transportation of the kit. Prior to use in the embossing method, the first component can be combined with a second component comprising a base to provide a sol-gel embossing composition. Alternatively, the second component can be added during the final stage of forming a layer of the first component, or the second component can be applied to the first component layer immediately before the embossing step.
[0038] According to a further aspect, there is provided a method of providing a patterned layer, the method comprising: providing a composition as defined above; forming a layer of the composition; and imprinting the layer using a patterned stamp at an imprinting temperature between 15°C and 120°C, so that the layer is alkalized during imprinting.
[0039] The method may further comprise removing the patterned stamp after embossing, and optionally, after removing the patterned stamp, heating the patterned layer at a temperature between 70° C. and 400° C. This additional heating step may effect a further hardening of the patterned layer.
[0040] According to a further aspect, an optical element is provided, the optical element comprising a patterned layer obtainable by the above method. The optical element may be, for example, a grating or a diffractive optical element. In particular, the optical element may be a lens, a light scattering element, a collimator, an incoupling element, a waveguide, a photonic device (such as a ring resonator), a wavelength filter or an amplitude modifier.
[0041] According to a further aspect, an etch mask comprising a patterned layer obtainable by the above method is provided.For example, the etch mask may be compatible with both wet etching and dry etching (eg reactive ion etching) processes. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Embodiments are described in more detail by way of non-limiting examples and with reference to the accompanying drawings, in which:
[0043] Figure 1 schematically depicts a method of forming an imprint layer according to an embodiment;
[0044] Figure 2 schematically depicts a light emitting device according to an embodiment;
[0045] Figure 3 schematically depicts a light emitting device according to another embodiment;
[0046] Figure 4 schematically depicts a method of forming an imprint layer according to another embodiment;
[0047] Figure 5 schematically depicts an aspect of a method of forming an imprint layer according to another embodiment;
[0048] Figure 6 schematically depicts a method of forming an imprint layer according to further embodiments;
[0049] Figure 7 a graph showing wavelength versus refractive index for a hardened imprint layer according to an embodiment; and
[0050] Figure 8 A graph of wavelength versus refractive index is shown for a hardened imprint layer of a comparative example in which no base was used in the imprint composition. DETAILED DESCRIPTION
[0051] The present invention will be described with reference to the accompanying drawings.
[0052] It should be understood that, although exemplary embodiments of devices, systems and methods are indicated, the detailed description and specific examples are for illustrative purposes only and are not intended to limit the scope of the invention. These and other features, aspects and advantages of the devices, systems and methods of the present invention will become better understood based on the following description, the appended claims and the accompanying drawings. It should be understood that the drawings are merely schematic and are not drawn to scale. It should also be understood that the same reference numerals are used throughout the drawings to indicate the same or similar parts, unless otherwise specified.
[0053] Embodiments of the present invention provide sol-gel ink compositions for forming a patterned layer by an imprint technique, such as substrate complete imprint lithography (SCIL), wherein a stamp having a patterned surface (typically, a surface with a pattern of micro- and / or nano-sized features) is contacted with such an ink composition. For the avoidance of doubt, it is noted that the term "imprint" in this context does not necessarily mean only pressing the patterned stamp onto a layer of the composition formed on the surface of a substrate. The meaning of the term "imprint" may further extend to applying the composition directly onto an exposed pattern of the patterned stamp. This is further explained below with reference to the accompanying drawings.
[0054] The term "ink" in the context of the present invention should not be considered to limit the imprint composition of the present invention to being suitable for producing a pattern that is different in color from the substrate. Therefore, the light absorption characteristics of the imprint composition are not limited by the term "ink".
[0055] The sol-gel printing ink composition comprises: a sol and an additive for promoting gelation of the composition at the printing temperature during printing. The composition has a pH of 4 to 7 when mixed with an equal volume of deionized water and measured at 20° C. and 1 atm. The additive is a reversible reaction product of a protic acid and a base that accepts a proton. At the printing temperature, the vapor pressure of the acid is higher than the vapor pressure of the base, so that during printing, the concentration of the base in the composition increases relative to the concentration of the acid in the composition, thereby causing alkalization of the composition.
[0056] In an embodiment, the imprinting temperature is 15° C. to 120° C., such as 20° C. to 60° C. Preferably, the imprinting temperature is 20° C. to 55° C.
[0057] In an embodiment, the sol comprises a hydrolyzate of at least one of a trialkoxysilane and a tetraalkoxysilane. For example, the sol may comprise a hydrolyzate of a trialkoxysilane and a tetraalkoxysilane. The sol-gel chemistry of such a system is shown in Reaction Scheme 1, which is for illustrative purposes only. The various reactions shown in Reaction Scheme 1 are analogous to other sol-gel systems, such as those derived from titanium alkoxide, zirconium alkoxide, or hafnium alkoxide precursors.
[0058]
[0059] Reaction Scheme I
[0060] In the reaction to form the sol-gel system, alkoxysilanes can be used, which undergo the reaction steps shown in reaction scheme I in the presence of an acid or base. Reaction scheme I shows an acid-catalyzed reaction. The alkoxysilane undergoes hydrolysis, followed by a condensation reaction between two hydrolyzed alkoxysilanes (water condensation reaction) or a condensation reaction between a hydrolyzed alkoxysilane and an unreacted alkoxysilane (alcohol condensation reaction), wherein a crosslinked inorganic network is formed. The degree of crosslinking can be controlled by appropriate selection of alkoxysilanes, pH, reaction temperature, water ratio, and cosolvent.
[0061] When the sol comprises a hydrolyzate of a trialkoxysilane and a tetraalkoxysilane, the molar ratio of the tetraalkoxysilane to the trialkoxysilane is preferably from 1:1 to 0.45:0.55. It has been found that when a combination of alkyltrialkoxysilane and tetraalkoxysilane in the above ratio is used, the desired degree of crosslinking in the gel can ultimately be obtained. Preferably, the tetraalkoxysilane is selected from tetramethoxyorthosilicate and tetraethoxyorthosilicate, and the trialkoxysilane is selected from methyltrimethoxysilane and methyltriethoxysilane. Alternatively or in addition, the sol may comprise a hydrolyzate of at least one of a titanium alkoxide, a zirconium alkoxide and a hafnium alkoxide.
[0062] The sol-gel embossing ink composition may, for example, further comprise nanoparticles (i.e., dispersed in the sol). Such nanoparticles may be transition metal oxide nanoparticles (e.g., titanium dioxide nanoparticles), which may produce a patterned layer with a higher refractive index. A patterned layer with a higher refractive index is desirable for optical applications. Alkalization of the composition during embossing may change the nanoparticle agglomeration behavior of the composition and control crosslink formation and curing. Alternatively, the sol-gel embossing ink composition may not contain such nanoparticles. The sol-gel embossing ink composition may, for example, be completely dissolved before layer formation and embossing.
[0063] To obtain a measurement of the pH of a composition, a sample of the composition can be mixed with an equal volume of deionized water. In other words, the volume ratio of the sample of the composition to the deionized water is 1:1. The pH of the resulting mixture can be measured at normal temperature and pressure (NTP) (i.e., 20°C and 1 atm). For example, a suitably calibrated pH probe can be used for this purpose. Alternative reliable methods for measuring pH (e.g., pH titration) are known to the skilled person. For example, by using appropriate amounts of an acid and a base, the pH of the composition can be adjusted to a measurement range of 4 to 7. As the skilled person will readily appreciate, the pK of the acid can be considered. a The pK of the conjugate acid of the base a To adjust pH.
[0064] The present invention is based in part on the recognition that adjusting the pH of the composition so that the pH is between 4 and 7 when measured using this method results in a composition having suitable properties (e.g., viscosity) for forming a composition layer suitable for embossing. It has also been found that such a pH extends the shelf life of the composition, for example relative to a composition having a pH greater than 7 when measured using this method.
[0065] Without wishing to be bound by any particular theory, such a pH may result in the condensation reaction being controlled such that linear oligomers are present in the sol. The linear oligomers may, for example, have a degree of polymerisation of from 2 to 20.
[0066] Preferably, the composition has a pH of 4 to 6 (such as 4.5 to 5.5) when mixed with an equal volume of deionized water and measured at 20° C. and 1 atm. When the composition has a pH of 6 to 7 (as measured using the above method), the degree of network formation may be lower, so that dewetting of the composition layer initially formed on the substrate surface may occur, and the final crosslinking during imprinting may take longer, for example relative to a composition having a pH of 4 to 6 or 4.5 to 5.5 when measured using the above method.
[0067] Although a pH range of 4 to 7 may have advantages in terms of shelf life of the composition and its application to a substrate to form a dense patterned layer, such a pH may mean that the condensation reaction (i.e., which results in gel formation) proceeds relatively slowly. For example, a longer imprinting time may be required relative to the imprinting time of the alkaline sol-gel composition for crosslinking to proceed to the point where the stamp can be removed without causing damage to the patterned layer.
[0068] However, alkaline conditions can promote the formation of undesirable three-dimensional cross-linked oligomers in the sol. The cured layer formed from such cross-linked oligomers may be more susceptible to (post-processing) shrinkage. Sol-gel imprinting ink compositions containing sols that are alkaline before imprinting can produce patterned layers with relatively high porosity, which results in lower density patterned layers with poorer mechanical and optical properties.
[0069] However, when it is desired to form a three-dimensional network (i.e., a gel), alkaline conditions are desirable during imprinting. A higher vapor pressure of the acid relative to the vapor pressure of the base at the imprinting temperature (e.g., 15° C. to 120° C.) means that during imprinting, the concentration of the base in the composition increases relative to the concentration of the acid in the composition, which allows the layer to be alkalized during imprinting. Alkalization of the layer (i.e., an increase in pH to above 7) is conducive to the formation of a three-dimensional network. For example, relative to a composition that does not include an alkali, the time required for imprinting, i.e., the time required for sufficient gelation and hardening so that the stamp can be removed, is correspondingly reduced.
[0070] The condensation polymerization (polycondensation) reactions that occur in sol-gel compositions are generally reversible reactions that are shifted to the polycondensation side of the equilibrium during imprinting of the composition using a permeable stamp. This is because some of the reaction products (e.g., water or alcohol) released when the condensation products are formed are transported away from the reaction sites by diffusion into / through the stamp material and by evaporation, thereby unfavoring the reverse (hydrolysis or alcoholysis) reaction. During imprinting, acids may also diffuse into the stamp. The removal of such reaction products and acids during imprinting can further serve to increase the concentration of base in the layer, thereby promoting alkalization of the layer and thus promoting gelation and hardening.
[0071] It is evident from the foregoing that the formation of a three-dimensional network is favored under alkaline conditions. Since the solvent is removed from the layer during imprinting, a relatively high porosity (i.e., low density) layer can be avoided. Alkaline conditions can push the equilibrium (e.g., as shown in reaction scheme 1) toward condensation, thereby releasing additional alcohol and water, which can be rapidly absorbed by the stamp due to the higher concentration of these molecules in the layer compared to in the stamp. Compared to acidic or neutral stamping conditions, the two effects, namely the increased condensation rate and the removal of the reaction products, can lead to faster formation of solid material and allow the stamp to be removed in a shorter time.
[0072] Thus, the sol-gel imprint ink composition can be used in an automated nanoimprint tool such as the AutoSCIL from Philips SCIL Nanoimprint Solutions. TM Mass production series machines) allow for higher production volumes.
[0073] Moreover, the sol-gel stamping ink composition can provide a suitably dense patterned layer, which will be discussed with reference to the examples. When the sol-gel stamping ink according to the present embodiment is used, the life of the stamp can also be improved. In addition, the sol-gel stamping ink may be less sensitive to changes in the surface chemistry of different substrates and variability in other parameters such as relative humidity of the environment, the presence of co-solvents, and the critical time from applying the sol-gel layer until the stamp is applied to the layer.
[0074] The composition comprises both a protic acid and a base that accepts a proton. However, as described above, the sol-gel imprint ink composition has a pH of 4 to 7 when mixed with an equal volume of deionized water and measured at 20° C. and 1 atm. This may mean that the acid and base are in equilibrium with the salts of the acid and base. Therefore, the additive may be considered to be an equilibrium mixture of an acid, a base, and a salt of an acid and a base. In other words, the additive used to promote gelation of the composition during imprinting may be considered to be a reversible reaction product of an acid and a base. It may be advantageous to hydrolyze the salt into an acid and a base at imprinting temperatures (e.g., between 15° C. and 120° C.) so as to allow the acid to evaporate and the base to alkalize the layer during imprinting.
[0075] For example, a base can be a "weak base," which means that the base does not completely dissociate in aqueous solution. For example, at 25°C (ionic strength = 0), the pK of the conjugate acid of the base in aqueous solution is a The range may be from 3 to 11. The base may, for example, comprise or consist of an amine, since the pK of the conjugate acid of the amine in aqueous solution is a It can be within the above range.
[0076] In an embodiment, the base comprises triethanolamine. In some instances, the base consists of triethanolamine. Triethanolamine has a relatively low vapor pressure (<1.3 Pa at 20°C) at printing temperatures (i.e., between 15°C and 120°C), which means that when it is used with an acid (e.g., formic acid) having a higher vapor pressure than the base, the composition can be alkalized during printing, thereby reducing the printing time, as previously described.
[0077] Amine bases such as triethanolamine may be suitable because they are compatible with the sol-gel composition and do not undergo phase separation from the composition during coating and imprinting. Such bases may also have relatively low toxicity and extended shelf life. Importantly, amine bases such as triethanolamine may not degrade the PDMS stamp, and absorption of the base in the PDMS may be minimal, thereby helping to alkalize the layer and reduce the imprint time, as explained above. The base is preferably free of Na, K, Li, Rb, Cs, Ca, Sr, Ba. This is to ensure that the patterned layer is compatible with complementary metal-oxide-semiconductor (CMOS) processes.
[0078] Alternatively or in addition, the base may comprise an alkoxysilyl functionalized amine and the sol-gel composition comprises the condensation product of the alkoxysilyl functionalized amine and the hydrolysis product of the above tetraalkoxysilane and / or alkoxysilane. The alkoxysilyl functionalized amine is preferably aminopropyltriethoxysilane. By incorporating the base into the polymer structure in this way, the vapor pressure of the base can be very low. Provided that the vapor pressure of the acid (e.g., formic acid) is sufficiently high at the imprint temperature, the composition can be alkalized during imprinting, thereby reducing the imprint time, as previously described.
[0079] For example, an acid can be a "weak acid," which indicates that the acid does not completely dissociate in aqueous solution. In other words, the acid is not completely (i.e., irreversibly) deprotonated. For example, the pK of an acid in aqueous solution is a The range at 25°C (ionic strength = 0) can be from 2 to 10.
[0080] The acid and base are chosen such that they react reversibly at the imprinting temperature. This involves taking into account the pKa of the acid and the pKa of the conjugate acid of the base, ie the respective equilibrium constants corresponding to proton donation by the acid and proton acceptance by the base, as will be immediately apparent to the skilled person.
[0081] At the imprint temperature, the vapor pressure of the acid is higher than the vapor pressure of the base. When the acid and base are present in other ingredients (in this case, other ingredients of the sol-gel composition), the values of the respective vapor pressures of the acid and base themselves may be different. However, ensuring that the vapor pressure of the acid itself is higher than the vapor pressure of the base itself can ensure that the vapor pressure of the acid in the composition is also higher than the vapor pressure of the base. For example, the vapor pressure of the acid itself can be greater than 300 Pa at 20°C, and the vapor pressure of the base itself can be less than 10 Pa at 20°C.
[0082] ASTM E1194-17 describes the procedure for measuring the vapor pressure of pure liquids or solid compounds. No single technique is capable of measuring 1×10 -11 To 100 kPa (about 10 -10to 760 Torr). The subject of ASTM E1194–17 is gas saturation, which measures 1×10 -11 To 1kPa (about 10 -10 Other methods, such as isobaric method and differential scanning calorimetry (DSC), are suitable for measuring vapor pressures above 0.1 kPa. -1 The isobaric (standard) procedure for measuring the vapor pressure of liquids from 2 × 10 -1 A DSC (standard) procedure to 100 kPa (about 1 to 760 Torr) vapor pressure is available in Test Method E1782.
[0083] In an embodiment, the percentage difference in the respective vapor pressures of the acid and base (i.e., (vapor pressure of acid (itself) - vapor pressure of base (itself) / vapor pressure of acid (itself)) * 100) is at least 50% (such as greater than 70%, greater than 90%).
[0084] The acid may include at least one of the compound represented by Formula 1 and the compound represented by Formula 2;
[0085] Formula 1
[0086]
[0087] Where R 1 is hydrogen, methyl or propyl;
[0088] Formula 2
[0089]
[0090] Where R 2 and R 3 Each is selected from hydrogen and C1-C3 alkyl.
[0091] Regarding the compound represented by Formula 1, the compound can reversibly react with a base to form a salt, so that at the imprint temperature, by evaporating the acid from the composition, the equilibrium can be pushed to the side of the acid and the base. In this regard, formic acid (R 1 =H) has a vapor pressure of 4600 Pa at 20°C; acetic acid (R 1 =Me) has a vapor pressure of 1500 Pa at 20°C; and propionic acid (R 1=Et) has a vapor pressure of 390 Pa at 20°C. The relatively high vapor pressure of these compounds at the printing temperature (i.e., 15°C to 120°C) may facilitate their evaporation during printing. Provided that the vapor pressure of the base is low enough at the printing temperature, the composition can be alkalized during printing, thereby reducing the printing time, as described above.
[0092] Similar considerations apply to compounds represented by Formula 2. The carbon between the two carbonyl carbons carries an acidic proton. For example, acetylacetone (R 2 =R 3 =Me) is about 9 (ionic strength = 0) at 25°C in aqueous solution, and the vapor pressure of acetylacetone is 920 Pa at 20°C.
[0093] The sol may include a solvent that is preferably selected so that the above-mentioned linear oligomers do not phase separate out of the sol (i.e. they remain dissolved). The solvent may have a sufficiently low vapor pressure to avoid significant evaporation of the solvent during deposition of the ink on the substrate, as this may result in premature phase separation of the oligomers, which can deteriorate the quality of the structure formed by the imprinting process (e.g. because uniform deposition of the composition may become problematic). Thus, the sol may include an alcohol, preferably at least one of 1-propanol, 2-propanol, 1-butanol, 2-butanol, tert-butanol and 1-methoxy-2-propanol.
[0094] Alternatively or in addition, the sol may contain water, which may participate in the hydrolysis during the formation of the sol. For example, water may be included in the composition in an amount of 5 to 20 moles per mole of metal / metalloid (e.g., silicon). For example, water may be included in the composition in an amount of 1 mole per mole of alkoxy. It has been found that particularly desirable oligomeric properties are obtained when the water content is selected within this range.
[0095] In a preferred embodiment, the sol comprises the reaction product of tetramethoxyorthosilicate (TMOS) and methyltrimethoxysilane (MTMS) in a water-alcohol mixture. The acid is preferably one or more of formic acid, acetic acid and propionic acid, and the base is an amine base, in particular triethanolamine (TEA) and / or aminopropyltriethoxysilane (APTES).
[0096] In an embodiment, the ink or composition of the invention has a composition selected from the ranges as specified in Table I. In Table I, where weight percentages (wt %) are referred to, this is relative to the total weight of the composition, unless otherwise stated.
[0097] Table I
[0098]
[0099] The sol-gel precursor, protic acid, water, and solvent can be combined to achieve acid hydrolysis. A base can then be added to the hydrolysis mixture.
[0100] In an embodiment, the sol-gel embossing ink composition may be provided as a kit, wherein the kit comprises a first component comprising an acid and a sol and a second component comprising a base. As described above, acidic conditions are advantageous in terms of the shelf life of the sol. The first component of the kit comprises an acid and a sol, and thus may have a shelf life that allows, for example, storage and transportation of the kit. Prior to use in the embossing method, the first component may be combined with a second component comprising a base to provide a sol-gel embossing ink composition. Alternatively, the second component may be added during the final stage of forming a layer of the first component, or the second component may be applied to the first component layer immediately prior to the embossing step.
[0101] A method of providing a patterned layer comprises providing the above sol-gel imprint ink composition; forming a layer of the composition; and imprinting the layer using a patterned stamp at an imprinting temperature between 15° C. and 120° C., so that the layer is alkalized during imprinting.
[0102] For example, shaping may involve spin coating, ink jetting, spray coating etc. onto the substrate. Spin coating is particularly mentioned, since a layer of substantially uniform thickness (eg 20 nm to 1 μm) can be obtained in this way.
[0103] The method may further comprise removing the patterned stamp after embossing, and optionally, after removing the patterned stamp, heating the patterned layer at a temperature between 70° C. and 400° C. Such an additional heating step may effect further hardening of the patterned layer, during which further polycondensation reactions may occur and / or volatile components (e.g., alcohol(s) and water) may be evaporated from the patterned layer.
[0104] Next, we will Figure 1 Embodiments of a method of forming a patterned layer using the imprint ink composition according to one or more embodiments described above are explained with the help of FIG. 1 , which schematically describes such a method.
[0105] In step A, a substrate 10 is provided as a support for an elastomeric stamp 20 having a main surface carrying a pattern 22. The features of the pattern 22 are typically of micrometer or nanometer dimensions, i.e. width and height of such dimensions. The pattern 22 may be formed in any suitable manner, for example by producing at least a patterned surface of the elastomeric stamp 22 in a master mould, which is well known per se. The elastomeric stamp 20 is preferably permeable so that the target components of the imprint ink composition can diffuse into the stamp material, and may be made of any suitable elastomeric material, for example a polysiloxane (such as PDMS) or another rubber-like stamp material having a low Young's modulus or having a suitable high permeability to water, alcohols and solvents, such as PFPE (acryloyloxy perfluoropolyether). A suitable Young's modulus is, for example, in the range of 2 to 100 MPa. For the avoidance of doubt, it is noted that the reported Young's modulus is determined by a standard hardness test using a rigid ball penetrating a rubber material under the conditions specified in the standard according to ASTM D1415-06 (2012). The elastomeric stamp 20 may be made of bulk material, or may be constructed in layers. The elastomeric stamp 20 may be placed on a substrate 10 so that its patterned surface is exposed, as shown in step A. Any suitable substrate 10 may be used for this purpose, such as a glass substrate, a semiconductor substrate (such as a silicon substrate), sapphire, etc.
[0106] In step B, by way of non-limiting example, a stamping ink composition 30 according to an embodiment is deposited on the pattern 22 of the elastomeric stamp 20 using any suitable deposition technique, such as doctor blading, printing or spin coating. As explained previously, in addition to the evaporation of the solvent to the environment, the interaction between the stamping ink composition 30 and the elastomeric stamp 20 will initiate gelation of the stamping ink composition 30 due to diffusion of one or more solvents and / or acids into the elastomeric stamp material and evaporation of the acid, thereby resulting in hardening of the layer, as explained previously.
[0107] In an optional step C, at this stage, the substrate 10 can be replaced by a foam 15 to increase the absorption capacity of the elastomeric stamp 20, since the components diffused from the stamp ink composition 30 into the stamp reservoir can be further stored in the porous structure of the foam 15. Foams are preferred because they have a pore structure. For this purpose, any suitable type of foam can be used, such as polyurethane foam. Alternatively, the absorption capacity of the stamp can be adjusted by combining layers of different materials that absorb more solvent or using a SCIL stamp layout in which the non-permeable backing material (such as glass) is replaced by a more permeable polymer or a plate with holes.
[0108] Step D is another optional step in which a body 40, such as an optical body (e.g., a light pipe, etc.), is placed on the embossing ink composition 30. For example, this can be used to provide an optical element 100 in which a patterned layer formed from the embossing ink composition 30 is used as an optical layer on the body 40. For example, the patterned layer can act as a refractive layer or an outcoupling layer on the body 40 to shape the light output from coupling into the body 40. By curing the embossing ink composition 30 to form a patterned layer 50, the patterned layer 50 can be adhered to the body 40, for example, to produce the optical element 100 as shown in step E.
[0109] The hardening of the embossing ink composition 30 when it is in contact with the pattern 22 can be carried out at an embossing temperature between 15° C. and 120° C. The embossing time can last for a period as short as 10 seconds. Longer embossing periods (e.g., up to 60 minutes) are also conceivable, although such periods may not be necessarily long in view of the rapid hardening of the composition 30 at the above-mentioned embossing temperatures. Optionally, the embossing ink composition 30 can be subjected to further stimulation (e.g., optical stimulation, such as UV radiation). This may be advantageous, for example, if the embossing ink composition 30 contains a polymerizable content in addition to the sol.
[0110] In at least some embodiments, before or after demolding the elastomeric stamp 20 from the cured imprint layer, the cured imprint layer can undergo a (post) curing step at an elevated temperature, for example to release residual volatile compounds (e.g., solvents) from the cured imprint layer to further densify the layer. For example, the cured imprint layer can be post-cured at about 70° C. to 400° C. Any suitable period of time can be contemplated for post-curing, although extended periods of time may be avoided if the substrate (or other layer) on which the patterned layer is formed may be damaged by prolonged heating. The post-curing period can be, for example, up to about 15 minutes.
[0111] Figure 2 A light emitting device 200 including an optical element 100 according to an example embodiment is schematically depicted. The optical element 100 (here a light guide) is optically coupled to a plurality of solid-state light emitting elements 210 (e.g., LEDs). The optical coupling ensures that light emitted by the solid-state light emitting elements 210 is coupled into the light guide body 40 and directed to the patterned layer 50 formed by the imprint ink composition 30, wherein the patterned layer 50 causes the light traveling through the light guide body 40 to be coupled out of the light guide body 40. The solid-state light emitting elements 210 can be LEDs of any suitable color or color combination (e.g., white light LEDs, blue light LEDs, green light LEDs, etc.).
[0112] In an example embodiment, the light emitting device 200 is a projection device, wherein the patterned layer 50 is arranged to collect (collimate) light leaving the light guide body 40 so as to generate a collimated light beam. This produces a particularly compact collimator, for example compared to compound parabolic concentrators commonly used for this purpose. The projection device may include a plurality of modules for generating primary color light beams, which can be combined with a projection lens to generate a color image, which is well known per se. At least one of such modules may include an optical element 100 so as to generate a collimated light beam. In an embodiment, the optical element 100 is further configured as a wavelength conversion element, for example converting light from a blue light LED into green light (e.g. a conversion of about 450nm to about 500nm). Alternatively, the light emitting device 200 may form a light rod, wherein the optical element 100 acts as a light guide and optionally further acts as a wavelength conversion element.
[0113] It should be understood that many other embodiments of the optical element 100 are also possible. For example, Figure 3 Another example embodiment is schematically depicted in which an optical element 100 is optically coupled (e.g., in physical contact) with a solid-state light emitting chip or package 310 (e.g., an LED chip or package), wherein the optical element 100 is configured as a lens element or collimator to produce a light emitting device 300 (such as a light bulb, etc.).
[0114] The optical element 100 may be integrated into other types of devices (eg other types of electronic devices).For example, the optical element 100 may form a part of an optical sensor, wherein the optical element 100 may be used as a light collecting layer of the optical sensor, for example.
[0115] Alternatively, the optical element 100 may form part of a photovoltaic device (such as a solar cell or solar panel), which typically comprises one or more photovoltaic cells for converting light into electricity. In such devices, the optical element 100 may, for example, be used as an incoupling layer for one or more photovoltaic cells, for example a patterned layer of a flat silicon substrate acting as a light trapping layer. Such light trapping layers are known per se, as explained, for example, by Spinelli et al. in Applied Physics Letters 102, 233902 (2013), and therefore, for the sake of brevity only, will not be explained in further detail. For the avoidance of doubt it should be noted that a patterned light trapping layer (anti-reflective coating) such as in the present reference may be produced in a single step process using an imprint ink composition and an imprint method according to embodiments of the present invention.
[0116] It is reiterated that the optical element 100 is not limited to the aforementioned embodiments; any embodiment is contemplated in which a patterned layer 50 of appropriate dimensions can be used to interact with light in a predetermined manner. Examples of such optical elements include lenses, light scattering elements, collimators, incoupling elements, waveguides, photonic devices (such as ring resonators), wavelength filters, amplitude modulators, etc. Other embodiments will be apparent to the skilled person. It should also be noted that the optical element 100 can be integrated into a light emitting device (e.g., an electronic device), an energy harvesting device (such as a solar panel), where the optical element can be used as an incoupling device, and the like.
[0117] Figure 4 An alternative embodiment of the method of the present invention is schematically depicted in FIG. In step A, a substrate 10 (which may be any suitable substrate, for example a semiconductor substrate, such as a silicon substrate, a SiGe substrate, a silicon-on-insulator substrate, a GaAs substrate, etc.) is covered with a layer 30 of an imprint ink composition according to an embodiment of the present invention. The imprint ink composition 30 may be applied in any suitable manner (e.g. by spin coating, ink jetting, spraying, etc.), although spin coating is specifically mentioned because a layer of substantially uniform thickness may be obtained in this manner. Furthermore, ink jet printing and subsequent imprinting produce a uniform layer due to capillary forces (e.g. due to the surface tension of the polar solvent after dispensing the droplet and under the stamp), resulting in a redistribution of the imprint ink material to obtain a uniform thickness.
[0118] An elastomeric stamp 20 having a major surface carrying a pattern 22 is embossed into a curable embossing ink composition 30, thereby transferring the pattern 22 into the layer, as shown in step B. The features of the pattern 22 typically have micrometer or nanometer dimensions, i.e. widths and heights of such dimensions. The pattern 22 can be formed in any suitable manner, for example by producing at least a patterned surface of the elastomeric stamp 22 in a master mold, which is well known per se. The elastomeric stamp 20 is preferably permeable and can be made of any suitable elastomeric material, such as a polysiloxane (such as PDMS) or another rubber-like stamp material having a low Young's modulus or having a suitable high permeability to water, alcohols and solvents, such as PFPE (acryloyloxy perfluoropolyether). The elastomeric stamp 20 can be made of a bulk material, or can be constructed in the form of layers with different Young's moduli.
[0119] Next, as depicted in step C, the stamped layer of stamping ink composition 30 is cured, which may optionally involve applying a stimulus such as heat and / or UV radiation, as previously explained.
[0120] When the polymerization reaction(s) in the imprinting layer of the imprinting ink composition 30 is completed, the elastomeric stamp 20 is demoulded from the layer in step D, thereby leaving a patterned layer 50 on the substrate 10, which retains its shape due to the network formed by the polycondensation reaction. As previously described, the patterned layer 50 can be further densified, for example, by exposure to heat (e.g., to remove remaining solvent(s)).
[0121] like Figure 4 The method schematically depicted in FIG. 5 can be used to form a three-dimensional structure constructed from a patterned layer 50. Such a three-dimensional structure can be formed by depositing a sacrificial planarization material 60 (e.g., Figure 5 The sacrificial planarizing material 60 is preferably a thermally degradable material and can be any suitable thermally degradable material, such as a thermally degradable polymer (TDP). A non-limiting example of a TDP is polynorbornene or polystyrene. Alternatively, the sacrificial planarizing material 60 can be soluble in a particular solvent. In general, any sacrificial planarizing material 60 can be used that can be selectively removed from the formed multilayer structure without damaging the patterned layer 50 formed by the curable imprint ink composition 30 according to an embodiment of the present invention.
[0122] A non-limiting example of a method for making such a three-dimensional structure is Figure 6 As explained above, in step A, a planarization layer 70 is formed on a substrate or carrier 10. The patterned layer portion 50 of the planarization layer 30 may be formed according to Figure 4 The method shown in , using a curable imprint ink composition 30, is produced by imprint lithography (substrate complete imprint lithography, SCIL). The patterned layer 50 is filled, i.e. planarized with a sacrificial filling material 60, as previously described with the aid of Figure 5 In step B, a next layer of a curable stamping ink composition 30 according to an embodiment is applied on the planarization layer 70 of step A in any suitable manner, such as by spin coating, dispensing or doctor blade coating.
[0123] As shown in step C, the curable embossing ink composition 30 deposited in step B is then embossed by an appropriately patterned elastomeric stamp 20 after the stamp is aligned relative to the substrate 10. In step C, the embossing orientation of the stamp 20 and the substrate 10 has been rotated 90° relative to the embossing orientation used to form the first patterned layer 50. It should be understood that other orientation rotation angles are also possible.
[0124] For example, the curable stamping ink composition 30 is subsequently cured (densified), e.g. Figure 4 , to form a further patterned layer 50' as shown in step D. It will be apparent that the formation of the further patterned layer 50' may be completed after removal of the patterned elastomeric stamp 20, i.e. by completing the polymerization reaction(s) as previously described. Removal of the patterned elastomeric stamp 20 leaves the further patterned layer 50' on the planarization layer 70 of step A. The newly formed patterned layer 50' may be planarized again as shown in step E to form a further planarization layer 70', after which these additional layers may be formed by repeating steps B to E. The height of the patterned portions of the patterned layers 50, 50' may be reduced using additional processing steps (e.g., by reactive ion etching).
[0125] The sacrificial planarization material 60 can then be removed by, for example, dissolving the sacrificial planarization material 60 in a suitable solvent or by thermal decomposition, thereby producing the optical device 400 in the form of a stacked structure as shown in step F. The imprint ink composition 30 is particularly suitable for use in this method because it can withstand most solvents required to dissolve the sacrificial planarization material 60, and can also withstand high temperatures of up to 600° C. or even 1000° C., making it particularly suitable for use with sacrificial planarization material 60 in the form of a thermally degradable compound (such as TDP).
[0126] In any of the foregoing embodiments, it may be necessary to remove residual imprinted structures from, for example, substrate 10, such as when layers on substrate 10 have been patterned using the imprinted structures as a mask. The imprinted structures may be removed by any suitable etching technique (eg, reactive ion etching).
[0127] The invention will now be explained in more detail by means of the following non-limiting examples.
[0128] Example 1: Preparation of acidified sol
[0129] A solution of TMOS (7.941 g) and MTMS (7.107 g) in water (6.57 g) and acetic acid (0.06 gram) was prepared, and the temperature of the mixture was maintained at 20° C. Hydrolysis was then carried out at 20° C. for 30 to 120 minutes. After the hydrolysis, water (10.33 g) and 1-propanol (100.56 g) were added to form an acidified sol.
[0130] Example 2: Preparation of acidified sol-gel embossing ink
[0131] An acidified sol-gel stamping ink was prepared by adding 1-propanol (84 g) and 1-butanol (16 g) to the acidified sol (100 g) prepared in Example 1. The stamping ink was allowed to reach equilibrium by storing the stamping ink between -30°C and -20°C for at least 20 hours. The pH of the stamping ink was 4.5 to 5.5 as measured by mixing a sample of the composition with an equal volume of deionized water and measuring the pH of the resulting mixture at normal temperature and pressure (i.e., 20°C and 1 atm) (NTP). The solids content was 2.5 wt%.
[0132] Examples 3 to 9: Preparation of acidified sol-gel embossing ink compositions containing a base
[0133] APTES or TEA was added to the acidified sol-gel imprint ink prepared in Example 1 to prepare seven acidified sol-gel imprint ink compositions containing a base (Table II). The base was added in an amount of 0.1 to 1 wt % of the imprint ink composition. To compensate for the increase in pH by adding the base, the pH was adjusted to 4 to 6 using additional formic acid as measured by mixing a sample of the composition with an equal volume of deionized water and measuring the pH of the resulting mixture at normal temperature and pressure (i.e., 20° C. and 1 atm) (NTP).
[0134] The molar ratio of TEA to formic acid was 1 :4. This ratio was found to be optimal as it allowed the pH to be adjusted to between 4 and 6. The molar ratio of APTES to formic acid was between 1 :1 and 2:1, which allowed the pH to be adjusted to between 4.5 and 5.5.
[0135] The stamp ink of Example 2 and the stamp ink compositions of Examples 3 to 9 were each spin coated on a silicon substrate at a speed of 1000 rpm for 15 seconds. The spin-coated layer was then stamped using a SCIL stamp for 10 to 40 seconds. It was found that this resulted in good capillary wettability of the stamp-resist contact line, i.e., the stamp was pulled into the resist by capillary forces.
[0136] The compositions are shown in Table II, along with their minimum imprint time, i.e., the time required for crosslinking to occur to the extent that the stamp can be removed without causing damage to the patterned layer. The shelf life at room temperature (RT; about 20° C.) was also qualitatively evaluated. For example, a shelf life of 7 to 10 days means that after this time, capillary wetting is still satisfactory, which means that the capillary forces are strong enough to pull the stamp into the resist, thereby allowing the air in front of the contact line to be expelled.
[0137] Table II
[0138]
[0139] * The sol-gel composition was prepared according to Example 3, except that half the amount of acetic acid used in Example 1 was used to prepare the acidified sol.
[0140] At RT, the embossing time for the alkali-free embossing ink of Example 2 is between 15 and 30 minutes. At 50° C., the embossing time is between 10 and 15 minutes. This variation is mainly due to changes in the ambient relative humidity level.
[0141] It can be seen from Table II that the stamping ink compositions of Examples 3 to 9 were successfully stamped using much shorter stamping times. This is due to the evaporation of formic acid (and solvent) during coating and stamping resulting in the layer being alkalized by TEA or APTES, as described previously. The gelation in the alkalized layer occurs faster than in the case of the stamping ink of Example 2.
[0142] It has been found that pH adjustment to 4 to 7 controls crosslinking in the stamping ink composition, as measured using the method described above. When 1 wt % TEA relative to silica solids was added to the stamping ink of Example 2, the pH of the resist was measured to be greater than 7, up to 7.5. In this case, no additional acid was used to adjust the measured pH to 4 to 7. When used immediately, this stamping ink composition exhibited a minimum stamping time of 5 to 15 seconds. However, the shelf life of the composition was poor; 2 to 4 hours after the addition of the base, the composition could no longer be used for stamping. This was due to the fact that the composition had been over-crosslinked after spin coating. This also demonstrates the effect of alkalization on the rate of crosslinking.
[0143] Using the imprinted layers of Examples 2 and 6 that had undergone hardening (post-annealing) at RT, 75° C., 150° C., 200° C., and 300° C., using An ellipsometer (JA Woollam Ellipsometry Solutions) was used to perform wavelength-variable-angle spectroscopic ellipsometry measurements. Figure 7 The refractive index and wavelength of the hardened layer made of the imprinted layer of Example 6 are shown. Figure 8 The refractive index and wavelength of the hardened layer made of the imprinted layer of Example 2 are shown, as well as the graph of the layer after imprinting only (in Figure 8 denoted as “RT stamping” in FIG.
[0144] Comparing the hardened layers after post-curing at 200°C and 300°C, it is apparent that compared with the layer made from the ink of Example 2 (which does not include a relatively low vapor pressure base) ( Figure 8 ) compared to the layer ( Figure 7), the refractive index is higher. The higher the refractive index, the denser the patterned layer, and therefore the less porous the patterned layer. Thus, these examples show that the imprint ink composition of the present invention results in a less porous patterned layer, which is due to the control of gelation provided by the volatile base, as described above.
[0145] The stamp life test was also performed using the AutoSCIL from Philips SCILNanoimprint Solutions. TM The 200 mm tool was run with a 200 mm tool. For large scale production, die life is very important as changing the die causes downtime and additional die adds cost. Several die runs were made with the above tool using the stamping ink composition in Table II (having 0.375 wt % APTES relative to silica solids and a 1 :1 APTES:formic acid ratio). Three die achieved 700+ imprints without noticeable drop in performance. One die achieved 1200 imprints without noticeable drop in performance. The die was Features <50 nm were replicated on a pitch of 100 nm, and SEM and optical measurements confirmed that these features were identical to the previous 10 imprints to within ±0.5 nm (via optical methods).
[0146] Other variations of the disclosed embodiments may be understood and effected by those skilled in the art in practicing the claimed invention, based on a study of the drawings, the disclosure and the appended claims. In the claims, the word "comprising" does not exclude other elements or steps, and the indefinite article "a" or "an" does not exclude a plurality. The mere fact that certain measures are recited in mutually different dependent claims does not indicate that a combination of these measures cannot be used to advantage. Any reference signs in the claims should not be construed as limiting the scope.
Claims
1. A stamping composition comprising: A sol comprising a hydrolyzate of an inorganic hydroxide and / or an alkoxide; and an additive for promoting gelation of the composition during imprinting at an imprinting temperature between 15° C. and 120° C., the additive being a reversible reaction product of a protic acid and a base accepting a proton, in, The composition has a pH of 4 to 7 when mixed with an equal volume of deionized water and measured at 20° C. and 1 atm, and wherein the vapor pressure of the acid is higher than the vapor pressure of the base at the imprinting temperature, thereby enabling alkalization of the composition during the imprinting. 2 . The composition according to claim 1 , wherein the sol comprises a hydrolyzate of at least one of a trialkoxysilane and a tetraalkoxysilane. 3 . The composition according to claim 2 , wherein the sol comprises a hydrolyzate of the trialkoxysilane and the tetraalkoxysilane, and a molar ratio of the tetraalkoxysilane to the trialkoxysilane is 1:1 to 0.45:0.
55.
4. The composition according to claim 2, wherein the tetraalkoxysilane is selected from tetramethoxyorthosilicate and tetraethoxyorthosilicate, and the trialkoxysilane is selected from methyltrimethoxysilane and methyltriethoxysilane.
5. The composition according to claim 3, wherein the tetraalkoxysilane is selected from tetramethoxyorthosilicate and tetraethoxyorthosilicate, and the trialkoxysilane is selected from methyltrimethoxysilane and methyltriethoxysilane. 6 . The composition according to claim 1 , wherein the sol comprises a hydrolyzate of at least one of titanium alkoxide, zirconium alkoxide, and hafnium alkoxide.
7. The composition of any one of the preceding claims 1 to 6, wherein the base comprises triethanolamine.
8. The composition of any one of claims 2 to 4, wherein the base comprises an alkoxysilyl-functionalized amine and the sol comprises a condensation product of the hydrolysis product and the alkoxysilyl-functionalized amine.
9. The composition according to any one of claims 1 to 6, wherein the acid comprises at least one of a compound represented by Formula 1 and a compound represented by Formula 2; Formula 1 Where R 1 is hydrogen, methyl or propyl; Formula 2 Where R 2 and R 3 Each is selected from hydrogen and C1-C3 alkyl.
10. The composition according to any one of claims 1 to 6, wherein the acid comprises at least one of a compound represented by Formula 1 and a compound represented by Formula 2; Formula 1 Where R 1 is hydrogen, methyl or propyl; Formula 2 Where R 2 and R 3 are each selected from hydrogen and C1-C3 alkyl; Wherein the base comprises triethanolamine.
11. The composition according to any one of claims 1 to 6, wherein the acid comprises at least one of a compound represented by Formula 1 and a compound represented by Formula 2; Formula 1 Where R 1 is hydrogen, methyl or propyl; Formula 2 Where R 2 and R 3 are each selected from hydrogen and C1-C3 alkyl; wherein the base comprises an alkoxysilyl-functionalized amine, and the sol comprises a condensation product of the hydrolysis product and the alkoxysilyl-functionalized amine.
12. The composition according to any one of the preceding claims 1 to 6, wherein the sol comprises an alcohol, wherein the alcohol is at least one of 1-propanol, 2-propanol, 1-butanol, 2-butanol, tert-butanol, and 1-methoxy-2-propanol.
13. The composition according to any one of the preceding claims 1 to 6, wherein the sol comprises water.
14. A kit for forming the composition of any one of claims 1 to 13, wherein the kit comprises a first component and a second component, the first component comprising an acid and a sol, and the second component comprising a base.
15. A method of providing a patterned layer, the method comprising: Providing a composition as described in any one of claims 1 to 13; forming a composition layer; as well as The layer is imprinted using a patterned stamp at an imprinting temperature between 15° C. and 120° C. such that the layer is alkalized during the imprinting.
16. The method of claim 15, comprising removing the patterned stamp after the imprinting, and optionally heating the patterned layer at a temperature between 70°C and 400°C after removing the patterned stamp.
17. An optical element comprising a patterned layer obtainable from the method according to claim 15 or claim 16, optionally wherein the optical element is a lens, a light scattering element, a collimator, an incoupling element, a waveguide, a ring resonator, a wavelength filter, or an amplitude modulator.
18. An optical element comprising a patterned layer obtainable from a method according to claim 15 or claim 16, optionally wherein the optical element is a photonic device.
19. An etch mask comprising a patterned layer obtainable from the method according to claim 15 or claim 16.
Citation Information
Patent Citations
Preparation method and use of graphene oxide surface molecularly imprinted sol-gel polymer
CN104165912A
Method for preparing coating composition having antifouling-antimoist barrier nature and Method for preparing film having antifouling-antimoist barrier nature using the same
KR1020170027926A
Relief layer and imprint method for making the same
WO2008053418A2
Method of making radiation-sensitive sol-GEL materials
WO2012142126A2
Composition, imprinting ink and imprinting method
CN104870576A