Vertical semiconductor device and method for manufacturing the same

In the manufacturing process of vertical semiconductor devices, by using fluorine plasma treatment and deposition inhibitor technology, the non-conformal barrier layer is converted into a conformal layer and an adsorption layer is formed, which solves the problems of deterioration of step coverage and uneven deposition, and improves the Integration and reliability of the device.

CN112310103BActive Publication Date: 2024-11-12SK HYNIX INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911379538.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-26
Filing Date
2019-12-27
Publication Date
2024-11-12
Estimated Expiration
2039-12-27

AI Technical Summary

Technical Problem

The prior art is difficult to effectively improve the integration and reliability of vertical semiconductor devices, especially in the three-dimensional structural arrangement, where there are problems of deterioration of step coverage and uneven deposition.

Method used

By forming an alternating laminate of a dielectric layer and a sacrificial layer on the substrate, forming an opening through etching, and then forming a non-conformal barrier layer on the alternating laminate, it is converted into a conformal barrier layer by fluorine plasma treatment, and adsorption deposition suppression The agent is to form a charge storage layer, thereby forming an adsorption layer between the barrier layer and the charge storage layer, improving step coverage and deposition uniformity.

Benefits of technology

High integration and reliability of vertical semiconductor devices are achieved, step coverage of barrier and charge storage layers is improved, uniform thickness and no overhang shape of the deposit, and overall manufacturing efficiency and quality are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112310103B_ABST
    Figure CN112310103B_ABST
Patent Text Reader

Abstract

A vertical semiconductor device and a method for manufacturing the vertical semiconductor device may include: forming an alternating stack of dielectric layers and sacrificial layers above a lower structure; forming an opening by etching the alternating stack; forming a non-conformal barrier layer on the alternating stack with the opening formed; adsorbing a deposition inhibitor on the surface of the barrier layer to convert the non-conformal barrier layer into a conformal barrier layer with the deposition inhibitor adsorbed thereon; and forming a charge storage layer on the conformal barrier layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments relate to a semiconductor device, and more particularly, to a vertical semiconductor device and a method for manufacturing the vertical semiconductor device. Background Art

[0002] A semiconductor device may include a memory cell array having a plurality of memory cells. The memory cell array may include memory cells arranged in various structures. In order to improve the integration of the semiconductor device, the memory cells may be arranged in three dimensions on a substrate. Summary of the invention

[0003] Exemplary embodiments of the present invention relate to a vertical semiconductor device capable of improving reliability and a method for manufacturing the vertical semiconductor device.

[0004] According to an embodiment, a method for manufacturing a vertical semiconductor device may include: forming an alternating stack of dielectric layers and sacrificial layers above a lower structure; forming an opening by etching the alternating stack; forming a non-conformal barrier layer on the alternating stack formed with the opening; adsorbing a deposition inhibitor on the surface of the barrier layer to convert the non-conformal barrier layer into a conformal barrier layer having the deposition inhibitor adsorbed thereon; and forming a charge storage layer on the conformal barrier layer.

[0005] According to an embodiment, a method for manufacturing a vertical semiconductor device may include: forming an alternating stack of dielectric layers and sacrificial layers above a lower structure; forming an opening by etching the alternating stack; forming a non-conformal barrier layer on the alternating stack having the opening; adsorbing a first deposition inhibitor on the surface of the barrier layer to convert the non-conformal barrier layer into a conformal barrier layer; forming a charge storage layer on the conformal barrier layer having the first deposition inhibitor adsorbed thereon; and adsorbing a second deposition inhibitor on the surface of the charge storage layer.

[0006] According to an embodiment, a vertical semiconductor device may include: a lower structure; an alternating stack of dielectric layers and gate electrodes formed above the lower structure; an opening extending through the alternating stack; a blocking layer formed on a sidewall of the opening; a charge storage layer formed on a sidewall of the blocking layer; and an adsorption layer formed at an interface between the blocking layer and the charge storage layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] Figure 1 is a cross-sectional view illustrating a semiconductor device according to an embodiment.

[0008] Figures 2A to 2G is a cross-sectional view illustrating a method for manufacturing a semiconductor device according to an embodiment.

[0009] Figure 3is a cross-sectional view illustrating a vertical semiconductor device according to an embodiment.

[0010] Figures 4A to 4K is a cross-sectional view illustrating a method for manufacturing a vertical semiconductor device according to an embodiment.

[0011] Figure 5A and Figure 5B is a cross-sectional view illustrating a method for manufacturing a vertical semiconductor device according to an embodiment.

[0012] Figure 6 is a cross-sectional view illustrating a method for manufacturing a vertical semiconductor device according to an embodiment. DETAILED DESCRIPTION

[0013] Various examples and embodiments described herein are described with reference to cross-sectional views, plan views, and block diagrams representing schematic diagrams of the present teachings. Therefore, the shapes illustrated may be modified by manufacturing techniques and / or tolerances. Therefore, the embodiments of the present teachings are not limited to the specific forms shown, but also include shape changes produced according to manufacturing processes. The regions illustrated in the figures have schematic properties, and the shapes of the regions illustrated in the figures are intended to illustrate the specific types of regions of the elements, and are not intended to limit the scope of the present teachings.

[0014] Figure 1 is a cross-sectional view illustrating a semiconductor device 100 according to an embodiment.

[0015] Reference Figure 1 , the semiconductor device 100 may include a substrate 101, a mold layer 102 located on the substrate 101, an opening 103 formed in the mold layer 102, and a gap filling structure 108 filling the opening 103. The gap filling structure 108 may include a first liner layer 104 formed on the sidewall of the opening 103, a second liner layer 105 formed on the sidewall of the first liner layer 104, and a filler 106 filling the opening 103 on the second liner layer 105. The gap filling structure 108 may further include an adsorption layer 107 formed at an interface between the first liner layer 104 and the second liner layer 105.

[0016] The adsorption layer 107 may be located at the upper sidewalls and upper corners of the opening 103. The adsorption layer 107 may include a material that induces conformal deposition of the first liner layer 104 and the second liner layer 105. The adsorption layer 107 may include a deposition inhibitor. The deposition inhibitor may include fluorine. The deposition inhibitor may include Cl, N2, or HF other than fluorine.

[0017] The first liner layer 104 may include an oxide, and the second liner layer 105 may include a nitride. The first liner layer 104 may include a silicon oxide, and the second liner layer 105 may include a silicon nitride. The adsorption layer 107 may include a fluorine-adsorbed oxide or a fluorine-adsorbed nitride. The adsorption layer 107 may include a fluorine-adsorbed silicon oxide or a fluorine-adsorbed silicon nitride.

[0018] In this embodiment, when the first liner layer 104 and the second liner layer 105 include silicon oxide and silicon nitride, respectively, the adsorption layer 107 may include fluorine-adsorbed silicon oxide. Here, the adsorption layer 107 may induce conformal deposition of silicon nitride as the second liner layer 105.

[0019] In some embodiments, when the first liner layer 104 and the second liner layer 105 include silicon nitride and silicon oxide, respectively, the adsorption layer 107 may include fluorine-adsorbed silicon nitride. Here, the adsorption layer 107 may induce conformal deposition of silicon oxide as the second liner layer 105.

[0020] The filler 106 of the gap-fill structure 108 may include oxide, a silicon layer, a high-k material, or a combination thereof. The filler 106 may include silicon oxide, a polysilicon layer, aluminum oxide, or a combination thereof.

[0021] The mold layer 102 may include a dielectric material, a conductive material, or a combination thereof. The mold layer 102 may include oxide, nitride, metal, metal nitride, metal silicide, metal carbide, amorphous silicon, polysilicon, amorphous carbon, silicon oxynitride, or a combination thereof.

[0022] Figures 2A to 2G is a cross-sectional view illustrating a method for manufacturing a semiconductor device according to an embodiment.

[0023] like Figure 2A As shown, a mold layer 102 may be formed on a substrate 101. The substrate 101 may be a material suitable for semiconductor processing. The substrate 101 may include a semiconductor substrate. For example, the substrate 101 may include a silicon substrate, a single crystal silicon substrate, a polycrystalline silicon substrate, an amorphous silicon substrate, a silicon germanium substrate, a single crystal silicon germanium substrate, a polycrystalline silicon germanium substrate, a carbon-doped silicon substrate, a combination thereof, or a multilayer thereof. The substrate 101 may include another semiconductor material such as germanium. The substrate 101 may include a III / V semiconductor substrate, for example, a compound semiconductor substrate such as gallium arsenide (GaAs). The substrate 101 may include a silicon on insulator (SOI) substrate.

[0024] The mold layer 102 may include a dielectric material, a conductive material, or a combination thereof. The mold layer 102 may include oxide, nitride, metal, metal nitride, metal silicide, metal carbide, amorphous silicon, polysilicon, amorphous carbon, silicon oxynitride, or a combination thereof.

[0025] Subsequently, an opening 103 may be formed. The opening 103 may be formed in the mold layer 102. A portion of the mold layer 102 may be etched using a mask (not shown) to form the opening 103. The bottom of the opening 103 may expose the surface of the substrate 101. The opening 103 may include a vertical hole. A plurality of openings 103 may be arranged. The plurality of openings 103 may be arranged in a zigzag pattern. The plurality of openings 103 may have a uniform size. Each opening 103 may be referred to as a "contact hole", a "through hole" or a "vertical hole".

[0026] The sidewall of the opening 103 may have a vertical profile. In some embodiments, the sidewall of the opening 103 may have an inclined profile.

[0027] like Figure 2B As shown, a first liner layer 104A may be formed. The first liner layer 104A may be formed non-conformally. In other words, due to the high aspect ratio of the opening 103, the first liner layer 104A may have poor step coverage.

[0028] The first liner layer 104A may have different thicknesses, i.e., a first thickness T1 formed on the sidewall and bottom of the opening 103 and a second thickness T2 formed at the upper corner of the opening 103. For example, the second thickness T2 may be greater than the first thickness T1. Due to the thickness difference, an overhang shape 104M may be formed at the upper corner of the opening 103.

[0029] like Figure 2C As shown, a surface treatment 111 may be performed. The surface treatment 111 may include a plasma treatment. The surface treatment 111 may transform the surface profile of the first liner layer 104A. For example, the surface treatment 111 may transform the non-conformal surface of the first liner layer 104A into a conformal surface. A conformal surface may refer to having a uniform thickness along the lower profile.

[0030] The surface treatment 111 may include an etching substance 111E. The etching substance 111E may include a material capable of partially etching the surface of the first liner layer 104A. The etching substance 111E may include fluorine (F). The surface treatment 111 may include NF3 plasma treatment. Therefore, the surface treatment 111 may include fluorine plasma treatment.

[0031] As described above, the first liner layer 104A may be etched at the upper corner of the opening 103 by the surface treatment 111 using fluorine plasma. In addition, the first liner layer 104A may be etched at the middle and bottom of the opening 103. At this time, the first liner layer 104A may be etched mainly at the upper corner of the opening 103, and thus the overhang shape 104M may be removed.

[0032] As a result, the first liner layer 104 having a uniform thickness may be formed through the surface treatment 111 .

[0033] Fluorine in fluorine plasma used during the surface treatment 111 may be adsorbed on the surface of the first liner layer 104. A fluorine adsorption layer 107 may be partially formed on the surface of the first liner layer 104. The fluorine adsorption layer 107 may be used as a deposition inhibitor in subsequent processes.

[0034] like Figure 2D and Figure 2E As shown, a second liner layer 105A may be formed on the first liner layer 104 . Figure 2D illustrates an initial deposition state of the second liner layer 105A, and Figure 2E A state after the deposition of the second liner layer 105A is completed is illustrated.

[0035] Reference Figure 2D and Figure 2E During the initial deposition process, the second liner layer 105A may be deposited on the first liner layer 104 at the middle and bottom of the opening 103. As the deposition process continues, the second liner layer 105A may be deposited on the first liner layer 104 and the fluorine adsorption layer 107 to cover the upper corners of the opening 103.

[0036] After the deposition of the second liner layer 105A is completed, the second liner layer 105A may be conformally deposited without an overhanging shape. Because the deposition is partially suppressed by the fluorine adsorption layer 107, a conformal deposition process of the second liner layer 105A may be performed. For example, the deposition rate of the second liner layer 105A at the upper corner of the opening 103 may be lower than that of other portions. In other words, the deposition rate of the second liner layer 105A at the middle and bottom of the opening 103 may be higher than that of the upper corner of the opening 103.

[0037] As described above, since deposition is suppressed by the fluorine adsorption layer 107 during the deposition process of the second liner layer 105A, the second liner layer 105A may be conformally deposited to have a uniform thickness without an overhanging shape.

[0038] like Figure 2F As shown, the bottom of the second liner layer 105A may be cut. As a result, the second liner layer 105 having a spacer shape may remain.

[0039] Continuously, the first liner layer 104 may be etched. Thus, the surface of the substrate 101 may be exposed, and the first liner layer 104 may remain on the sidewall of the opening 103.

[0040] The fluorine adsorption layer 107 may be located between the first liner layer 104 and the second liner layer 105 at an upper corner or an upper sidewall of the opening 103. The fluorine adsorption layer 107 may not be located at a middle sidewall or a bottom sidewall of the opening 103.

[0041] like Figure 2G As shown, a filler 106 may be formed to fill the opening 103 . The filler 106 may completely fill the opening 103 on the second liner layer 105 .

[0042] In order to form the filler 106 , deposition and planarization of a filling material may be performed to fill the opening 103 on the second liner layer 105 .

[0043] The filler 106 may include oxide, a silicon layer, a high-k material, or a combination thereof. The filler 106 may include silicon oxide, a polysilicon layer, aluminum oxide, or a combination thereof.

[0044] According to the above-described embodiment, the step coverage of the first liner layer 104 and the second liner layer 105 can be improved by the surface treatment 111 .

[0045] Figure 3 is a cross-sectional view illustrating a vertical semiconductor device 200 according to an embodiment.

[0046] Reference Figure 3 , the vertical semiconductor device 200 may include a lower structure 201, an alternating stack 201M in which dielectric layers 202 and gate electrodes 203 are alternately stacked, and a pillar structure 211 penetrating the alternating stack 201M. The pillar structure 211 may have a pillar shape filling an opening 204 penetrating the alternating stack 201M. Each gate electrode 203 may have a shape of an outer wall surrounding the pillar structure 211.

[0047] The pillar structure 211 may include a blocking layer 205, a charge storage layer 207, a tunnel dielectric layer 208, a channel layer 209, and a core dielectric layer 210. The pillar structure 211 may also include an adsorption layer 206 formed at an interface between the blocking layer 205 and the charge storage layer 207. The blocking layer 205 may include an oxide, and the charge storage layer 207 may include a nitride. The tunnel dielectric layer 208 may include an oxide, and the channel layer 209 may include a silicon layer. The core dielectric layer 210 may include an oxide.

[0048] Adsorption layer 206 may include a material that induces conformal deposition of blocking layer 205 and charge storage layer 207. Adsorption layer 206 may include a deposition inhibitor. The deposition inhibitor may include fluorine. Adsorption layer 206 may include a fluorine-adsorbed oxide or a fluorine-adsorbed nitride. Adsorption layer 206 may include a fluorine-adsorbed silicon oxide or a fluorine-adsorbed silicon nitride.

[0049] In this embodiment, when the blocking layer 205 and the charge storage layer 207 include silicon oxide and silicon nitride, respectively, the adsorption layer 206 may include fluorine-adsorbed silicon oxide. Here, the adsorption layer 206 may induce conformal deposition of silicon nitride as the charge storage layer 207.

[0050] Figures 4A to 4K is a cross-sectional view illustrating a method for manufacturing a vertical semiconductor device according to an embodiment.

[0051] like Figure 4A As shown, an alternating stack 11M may be formed above a lower structure including a substrate 11. The substrate 11 may be a material suitable for semiconductor processing. The substrate 11 may include a semiconductor substrate. For example, the substrate 11 may include a silicon substrate, a single crystal silicon substrate, a polycrystalline silicon substrate, an amorphous silicon substrate, a silicon germanium substrate, a single crystal silicon germanium substrate, a polycrystalline silicon germanium substrate, a carbon-doped silicon substrate, a combination thereof, or a multilayer thereof. The substrate 11 may include another semiconductor material such as germanium. The substrate 11 may include a III / V semiconductor substrate, for example, a compound semiconductor substrate such as gallium arsenide (GaAs). The substrate 11 may include a silicon-on-insulator (SOI) substrate.

[0052] The alternating stack 1154 may include a first material layer and a second material layer formed sequentially. The first material layer may include a first material, and the second material layer may include a second material. The first material and the second material may be different from each other. The first material layer and the second material layer may include a dielectric layer 12 and a sacrificial layer 13, respectively. The dielectric layer 12 may include a dielectric material, and the sacrificial layer 13 may include a sacrificial material. In this article, "sacrificial material" may refer to a material to be removed in a subsequent process. The dielectric layer 12 may include at least one dielectric material of silicon oxide, silicon nitride, silicon oxynitride, a spin-on dielectric material, a dielectric metal oxide, a silicate, and a dielectric metal oxynitride.

[0053] The sacrificial layer 13 may include a sacrificial material that can be selectively removed relative to the dielectric layer 12. The sacrificial layer 13 may be selectively removed relative to the dielectric layer 12. The ratio of the removal rate of the sacrificial layer to the removal rate of the dielectric layer 12 may be referred to as the selectivity of the removal process of the sacrificial layer 13 relative to the dielectric layer 12.

[0054] The sacrificial layer 13 may include a dielectric material. The sacrificial layer 13 may be replaced with a conductive material in a subsequent process. For example, the sacrificial layer 13 may be replaced by a gate electrode or a word line of a vertical NAND device. The sacrificial layer 13 may include silicon nitride, amorphous silicon, or polycrystalline silicon. In some embodiments, the sacrificial layer 13 may include silicon nitride.

[0055] In the present embodiment, the dielectric layer 12 may include silicon oxide, and the sacrificial layer 13 may include silicon nitride.

[0056] The dielectric layer 12 may be deposited by chemical vapor deposition (CVD) or atomic layer deposition (ALD). The sacrificial layer 13 may be deposited by CVD or ALD.

[0057] The lowermost layer and the uppermost layer of the alternating stack 11M may be the dielectric layer 12. The dielectric layer 12 and the sacrificial layer 13 may have the same thickness.

[0058] Subsequently, an opening 14 may be formed in the alternating stack 11M. A portion of the alternating stack 11M may be etched using a mask (not shown) to form the opening 14. The bottom of the opening 14 may expose the surface of the substrate 11. The opening 14 may include a vertical hole. A plurality of openings 14 may be arranged. A plurality of openings 14 may be arranged in a zigzag pattern. A plurality of openings 14 may have uniform sizes.

[0059] The sidewalls of the opening 14 may have a vertical profile. In some embodiments, the sidewalls of the opening 14 may have an inclined profile.

[0060] like Figure 4B As shown, barrier layer 15A may be formed. Barrier layer 15A may be formed non-conformally. In other words, barrier layer 15A may have poor step coverage due to the high aspect ratio of opening 14.

[0061] The barrier layer 15A may have different thicknesses, i.e., a first thickness T1 formed on the sidewall and bottom of the opening 14 and a second thickness T2 formed at the upper corner of the opening 14. For example, the second thickness T2 may be greater than the first thickness T1. Due to the thickness difference, an overhang shape 15M may be formed at the upper corner of the opening 14.

[0062] The barrier layer 15A may include silicon oxide. In some embodiments, the barrier layer 15A may include aluminum oxide (Al2O3).

[0063] Silicon oxide as the barrier layer 15A can be deposited using a silicon source material and an oxygen-containing gas. As the silicon source material, SiH4, HCDS (Si2Cl6), DCS (SiH2Cl2), tris (dimethylamino) silane (TDMAS), bis (diethylamino) silane (BDEAS), bis (tert-butylamino) silane (BTBAS), etc. can be used. As the oxygen-containing gas, O2 can be used.

[0064] Silicon oxide as the barrier layer 15A may be formed by depositing silicon nitride and then oxidizing the silicon nitride. For example, Si3N4 may be formed using a silicon source material and NH3 gas, and then an oxidation process may be performed. The oxidation process may use a H2 / O2 mixed gas.

[0065] In some embodiments, silicon oxide as the barrier layer 15A may be deposited by ALD. ALD may be performed on silicon oxide using a silicon source material and an oxygen-containing gas. As the oxygen-containing gas, a H2 / O2 mixed gas may be used.

[0066] like Figure 4C As shown, surface treatment 16 may be performed. Surface treatment 16 may include plasma treatment. Surface treatment 16 may transform the surface profile of barrier layer 15A. For example, surface treatment 16 may conformally transform the surface of barrier layer 15A.

[0067] The surface treatment 16 may include an etching substance 16E. The etching substance 16E may include a material capable of partially etching the surface of the barrier layer 15A. The etching substance 16E may include fluorine (F). The surface treatment 16 may include a NF3 plasma treatment. Therefore, the surface treatment 16 may include a fluorine plasma treatment.

[0068] As described above, the barrier layer 15A may be etched at the upper corner or upper sidewall of the opening 14 by the surface treatment 16 using fluorine plasma. In addition, the barrier layer 15A may be etched in the middle and bottom of the opening 14. At this time, the barrier layer 15A may be etched mainly at the upper corner of the opening 14, and thus the overhang shape 15M may be removed.

[0069] As a result, the barrier layer 15 having a uniform thickness can be formed through the surface treatment 16 .

[0070] The fluorine in the fluorine plasma used during the surface treatment 16 may be adsorbed on the surface of the barrier layer 15. A fluorine adsorption layer 16D may be partially formed on the surface of the barrier layer 15. The fluorine adsorption layer 16D may be used as a deposition inhibitor in subsequent processes. The deposition inhibitor may be referred to as a "surface protectant". The deposition inhibitor may include Cl, N2, or HF in addition to fluorine.

[0071] like Figure 4D and Figure 4E As shown, the charge storage layer 17A may be formed on the blocking layer 15 and the adsorption layer 16D. The charge storage layer 17A may be formed on the surface of the blocking layer 15. The deposition of the charge storage layer 17A may be suppressed by the fluorine adsorption layer 16D. For example, the charge storage layer 17A may not be deposited at the upper corner of the opening 14, but may be deposited at the middle and bottom of the opening 14.

[0072] The charge storage layer 17A can also be formed on the fluorine adsorption layer 16D by continuously depositing the charge storage layer 17A. Therefore, the charge storage layer 17A can be conformally deposited without an overhanging shape.

[0073] As described above, since deposition is suppressed by the fluorine adsorption layer 16D during the deposition process of the charge storage layer 17A, the charge storage layer 17A can be conformally deposited to have a uniform thickness without an overhanging shape.

[0074] As a result, since the surface treatment 16 is performed, the step coverage of both the blocking layer 15 and the charge storage layer 17A can be improved.

[0075] like Figure 4F As shown, the bottom of the charge storage layer 17A may be cut. Thus, the charge storage layer 17 having a spacer shape may be formed.

[0076] Continuously, the bottom of the blocking layer 15 may be cut. The blocking layer 15 and the charge storage layer 17 may be formed on the sidewalls of the opening 14.

[0077] like Figure 4G As shown, a tunnel dielectric layer 18 may be formed on the charge storage layer 17. The tunnel dielectric layer 18 may include silicon oxide.

[0078] The channel layer 19 may be formed on the tunnel dielectric layer 18 , and the core dielectric layer 20 may be formed on the channel layer 19 .

[0079] Through the above series of deposition processes, the opening 14 may be filled with the blocking layer 15 , the charge storage layer 17 , the tunnel dielectric layer 18 , the channel layer 19 , and the core dielectric layer 20 .

[0080] The channel layer 19 may include a silicon layer. The channel layer 19 may include a doped silicon layer. The core dielectric layer 20 may include silicon oxide. In order to form the channel layer 19 and the core dielectric layer 20, a silicon layer and silicon oxide may be sequentially formed and then planarized. The channel layer 19 may have a cylindrical shape, and the core dielectric layer 20 may have a columnar shape filling the cylinder of the channel layer 19.

[0081] like Figure 4H As shown, the core dielectric layer 20, the channel layer 19, and the tunnel dielectric layer 18 may be planarized. Therefore, a pillar structure 21 may be formed in the opening 14. The pillar structure 21 may include a barrier layer 15 formed on a sidewall of the opening 14, a charge storage layer 17 formed on a sidewall of the barrier layer 15, a tunnel dielectric layer 18 formed on a sidewall of the charge storage layer 17, a channel layer 19 formed on a sidewall of the tunnel dielectric layer 18, and a core dielectric layer 20 formed on a sidewall of the channel layer 19.

[0082] like Fig. 4I As shown, the slit 22 may be formed. In order to form the slit 22, a portion of the alternating stack 11M may be etched. From a top view, the slit 22 may have a line shape extending in one direction.

[0083] like Figure 4J As shown, the sacrificial layer 13 may be selectively removed. Therefore, a horizontal recess 23 may be formed between the dielectric layers 12. The horizontal recess 23 may partially expose the outer wall of the pillar structure 21.

[0084] like Figure 4K As shown, a gate electrode 24 may be formed to fill the horizontal recess 23. The gate electrode 24 may include a low resistance material. The gate electrode 24 may include a metal-based material. The gate electrode 24 may include a metal, a metal silicide, a metal nitride, or a combination thereof. For example, the metal may include nickel, cobalt, platinum, titanium, tantalum, or tungsten. The metal silicide may include nickel silicide, cobalt silicide, platinum silicide, titanium silicide, tantalum silicide, or tungsten silicide. The gate electrode 24 may also include a barrier material (not shown). The barrier material may include a metal nitride. For example, the barrier material may include titanium nitride (TiN).

[0085] In some embodiments, surface treatment 16 may be performed after depositing charge storage layer 17A.

[0086] In some embodiments, the surface treatment 16 may be applied after at least one of the deposition processes of the blocking layer 15A, the deposition processes of the charge storage layer 17A, the deposition processes of the tunnel dielectric layer 18 , and the deposition processes of the channel layer 19 .

[0087] In some embodiments, the surface treatment 16 may be selectively performed on the surface of the charge storage layer 17A after sequentially depositing the blocking layer 15A and the charge storage layer 17A. In this case, the surface treatment 16 may not be performed after depositing the blocking layer 15A.

[0088] Figure 5A and Figure 5B is a cross-sectional view illustrating a method for manufacturing a vertical semiconductor device according to an embodiment.

[0089] Can be FIG. 4A to FIG. 4E The method shown conformally forms the charge storage layer 17A. A fluorine adsorption layer 16D may be formed between the charge storage layer 17A and the blocking layer 15.

[0090] Then, if Figure 5A As shown in , surface treatment 16 may be performed again. Surface treatment 16 may include plasma treatment. Surface treatment 16 may transform the surface profile of charge storage layer 17A. For example, surface treatment 16 may conformally transform the surface of charge storage layer 17A.

[0091] Surface treatment 16 may include etching substance 16E. Etching substance 16E may include a material capable of partially etching the surface of charge storage layer 17A. Etching substance 16E may include fluorine (F). Surface treatment 16 may include NF3 plasma treatment. Therefore, surface treatment 16 may include fluorine plasma treatment.

[0092] As described above, the charge storage layer 17A may be etched at the upper corner or upper sidewall of the opening 14 by the surface treatment 16 using fluorine plasma. In addition, the charge storage layer 17A may be etched at the middle and bottom of the opening 14. At this time, the charge storage layer 17A may be etched mainly at the upper corner of the opening 14.

[0093] As a result, the charge storage layer 17A having a uniform thickness can be formed by the surface treatment 16 .

[0094] The fluorine in the fluorine plasma used during the surface treatment 16 may be adsorbed on the surface of the charge storage layer 17A. A fluorine adsorption layer 16D' may be partially formed on the surface of the charge storage layer 17A. The fluorine adsorption layer 16D' may be retained to serve as a deposition inhibitor in subsequent processes. The deposition inhibitor may be referred to as a "surface protectant". The deposition inhibitor may include Cl, N2, or HF in addition to fluorine.

[0095] The fluorine adsorption layer 16D' may be fluorine-adsorbed silicon nitride. The fluorine adsorption layer 16D' may be fluorine-adsorbed silicon oxide.

[0096] Then, execute Figure 4G to Figure 4J For example, after cutting the charge storage layer 17A on which the fluorine adsorption layer 16D' has been formed, the blocking layer 15 may be cut. Continuously, the tunnel dielectric layer 18, the channel layer 19, and the core dielectric layer 20 may be sequentially deposited.

[0097] Therefore, if Figure 5B As shown in , a pillar structure 21' may be formed to fill the opening 14. The pillar structure 21' may include a barrier layer 15 formed on a sidewall of the opening 14, a charge storage layer 17 formed on a sidewall of the barrier layer 15, a tunnel dielectric layer 18 formed on a sidewall of the charge storage layer 17, a channel layer 19 formed on a sidewall of the tunnel dielectric layer 18, and a core dielectric layer 20 formed on a sidewall of the channel layer 19. The pillar structure 21' may also include fluorine adsorption layers 16D and 16D'. The fluorine adsorption layer 16D may be located between the barrier layer 15 and the charge storage layer 17. The fluorine adsorption layer 16D' may be located between the charge storage layer 17 and the tunnel dielectric layer 18.

[0098] Through the fluorine adsorption layer 16D', the tunnel dielectric layer 18 can be conformally deposited to have a uniform thickness without an overhanging shape. Therefore, since the surface treatment 16 is performed twice, the overall step coverage of the blocking layer 15, the charge storage layer 17, and the tunnel dielectric layer 18 can be improved.

[0099] Subsequently, it can be formed Figure 4K The gate electrode is shown.

[0100] Figure 6 is a cross-sectional view illustrating a method for manufacturing a vertical semiconductor device according to an embodiment. Figure 6 An opening 14 having an inclined sidewall is illustrated, and Figure 4B Another example of the surface treatment 16 of the barrier layer 15A.

[0101] Reference Figure 6 , surface treatment 16 may be performed. Surface treatment 16 may include plasma treatment. Surface treatment 16 may transform the surface profile of barrier layer 15A. For example, surface treatment 16 may conformally transform the surface of barrier layer 15A.

[0102] The surface treatment 16 may include an etching substance 16E. The etching substance 16E may include a material capable of partially etching the surface of the barrier layer 15A. The etching substance 16E may include fluorine (F). The surface treatment 16 may include a NF3 plasma treatment. Therefore, the surface treatment 16 may include a fluorine plasma treatment.

[0103] As described above, the barrier layer 15A may be etched at the upper corner or sidewall of the opening 14 by the surface treatment 16 using fluorine plasma. In addition, the barrier layer 15A may be etched in the middle and bottom of the opening 14. At this time, the barrier layer 15A may be etched mainly at the upper corner of the opening 14, and thus the overhang shape 15M may be removed.

[0104] As a result, the barrier layer 15 having a uniform thickness can be formed through the surface treatment 16 .

[0105] The fluorine in the fluorine plasma used during the surface treatment 16 may be adsorbed on the surface of the barrier layer 15. A fluorine adsorption layer 16D may be partially formed on the surface of the barrier layer 15. The fluorine adsorption layer 16D may be used as a deposition inhibitor in subsequent processes. The deposition inhibitor may be referred to as a "surface protectant". The deposition inhibitor may include Cl, N2, or HF in addition to fluorine.

[0106] According to the above-described embodiment, the process of forming the stack of the blocking layer 15 , the charge storage layer 17 , and the tunnel dielectric layer 18 may be referred to as an “ONO process”.

[0107] As a comparative example, when an ONO process is performed to deposit a layer by thermal atomic layer deposition (ALD), it may be exposed to a high temperature of 630° C. or higher. A minute chemical vapor deposition (CVD) reaction due to such a high temperature process causes the step coverage in which non-conformal deposition is performed to deteriorate. In other words, because the upper side of the opening 14 is deposited relatively thicker than the lower side of the opening 14, the step coverage may deteriorate.

[0108] According to the present embodiment, in order to improve the step coverage of the ONO process, the surface treatment 16 may be performed before the charge storage layer 17A is deposited to achieve both the etching effect and the deposition inhibition effect. The surface treatment 16 may use NF3 plasma, and when the NF3 plasma flows to the upper side of the opening 14, then the charge storage layer 17A is deposited, the step coverage of the barrier layer 15 may be improved while etching the upper portion of the barrier layer 15.

[0109] In addition, since the upper side of the charge storage layer 17 is not deposited due to the fluorine adsorption layer 16D in the initial deposition stage, the step coverage of both the blocking layer and the charge storage layer can be improved.

[0110] According to some embodiments, a surface treatment including an etching species and a deposition inhibitor is performed to gap fill an opening having a high aspect ratio.

[0111] According to some embodiments, when an oxide-nitride-oxide (ONO) stack is formed, a surface treatment including an etching substance and a deposition inhibitor is performed, thereby improving step coverage of the ONO stack.

[0112] Although the present teaching has been described with respect to a limited number of possible embodiments, it should be noted that the embodiments presented are used to describe rather than limit the present teaching. In addition, it should be noted that those skilled in the art may implement the present teaching in various ways by substitution, change and modification without departing from the scope of the present teaching as defined by the appended claims.

[0113] CROSS-REFERENCE TO RELATED APPLICATIONS

[0114] This application claims priority to Korean Patent Application No. 10-2019-0091116, filed on Jul. 26, 2019, which is hereby incorporated by reference in its entirety.

Claims

1. A method for manufacturing a vertical semiconductor device, the method comprising the following steps: forming an alternating stack of dielectric layers and sacrificial layers over the lower structure; forming openings by etching the alternating stack; forming a non-conformal barrier layer on the alternating stack having the openings formed therein; performing a surface treatment to adsorb a deposition inhibitor on the surface of the barrier layer and convert the non-conformal barrier layer into a conformal barrier layer having the deposition inhibitor adsorbed thereon; and A charge storage layer is formed on the conformal blocking layer.

2. The method according to claim 1, wherein: The surface treatment includes plasma treatment.

3. The method according to claim 1, wherein: The surface treatment is concentrated on upper corners of the opening.

4. The method according to claim 1, wherein: The surface treatment includes partially etching the non-conformal barrier layer at upper corners of the opening.

5. The method according to claim 1, wherein: The surface treatment is performed by a plasma treatment including a plasma including an etching species.

6. The method according to claim 1, wherein: The deposition inhibitor includes a plasma comprising fluorine.

7. The method according to claim 1, wherein: The deposition inhibitor includes a plasma containing nitrogen trifluoride NF3.

8. The method according to claim 1, wherein: The deposition inhibitor includes fluorine F, chlorine Cl, nitrogen N2 or hydrogen fluoride HF.

9. A method for manufacturing a vertical semiconductor device, the method comprising the steps of: forming an alternating stack of dielectric layers and sacrificial layers over the lower structure; forming openings by etching the alternating stack; forming a non-conformal barrier layer on the alternating stack having the openings formed therein; performing a first surface treatment to adsorb a first deposition inhibitor on the surface of the barrier layer and convert the non-conformal barrier layer into a conformal barrier layer; forming a charge storage layer on the conformal barrier layer having the first deposition inhibitor adsorbed thereon; as well as A second surface treatment is performed to adsorb a second deposition inhibitor on the surface of the charge storage layer.

10. The method according to claim 9, wherein: The first surface treatment includes a plasma treatment.

11. The method according to claim 9, wherein: The first surface treatment is concentrated on upper corners of the opening.

12. The method according to claim 9, wherein: The first surface treatment includes partially etching the barrier layer at an upper corner of the opening.

13. The method according to claim 9, wherein: The first surface treatment is performed by a plasma treatment including a plasma including an etching species.

14. The method according to claim 9, wherein: The first deposition inhibitor includes a plasma including fluorine.

15. The method according to claim 9, wherein: The first deposition inhibitor includes a plasma including nitrogen trifluoride NF3.

16. The method according to claim 9, wherein: The first deposition inhibitor includes fluorine F, chlorine Cl, nitrogen N2 or hydrogen fluoride HF.

17. The method according to claim 9, wherein: The barrier layer includes silicon oxide or aluminum oxide.

18. The method according to claim 9, wherein: The first deposition inhibitor and the second deposition inhibitor include plasma of the same material.

19. The method according to claim 9, wherein: The first deposition inhibitor and the second deposition inhibitor include fluorine F, chlorine Cl, nitrogen N2 or hydrogen fluoride HF.

20. The method according to claim 9, further comprising the steps of: forming a tunnel dielectric layer on the charge storage layer having the second deposition inhibitor adsorbed thereon; as well as A channel layer is formed on the tunnel dielectric layer.

21. A vertical semiconductor device, the vertical semiconductor device comprising: Substructure; an alternating stack of dielectric layers and gate electrodes, the alternating stack formed over the lower structure; an opening extending through the alternating layers; a barrier layer formed on a sidewall of the opening; a charge storage layer formed on a sidewall of the blocking layer; as well as an adsorption layer formed at an interface between the blocking layer and the charge storage layer, wherein the adsorption layer includes a deposition inhibitor, and The adsorption layer induces conformal deposition of the charge storage layer, so that the charge storage layer is conformally deposited to have a uniform thickness during surface treatment.

22. The vertical semiconductor device according to claim 21, wherein: The adsorption layer is located on the upper side wall of the opening.

23. The vertical semiconductor device of claim 21, wherein: The adsorption layer includes fluorine-containing silicon oxide or fluorine-containing silicon nitride.

24. The vertical semiconductor device of claim 21, wherein: The deposition inhibitor includes fluorine F, chlorine Cl, nitrogen N2 or hydrogen fluoride HF.