Composite transmission layer and application thereof and method for preparing organic solar cell module

By combining scraping and evaporation technology in the composite transport layer of organic solar cells, the substrate holes and defects are filled, the carrier collection efficiency and surface flatness are improved, and the film inhomogeneity caused by the difference in substrate surface morphology is solved. The photoelectric conversion efficiency and stability of module devices have been significantly improved.

CN112366278BActive Publication Date: 2024-11-26SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011146336.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-23
Publication Date
2024-11-26
Estimated Expiration
2040-10-23

AI Technical Summary

Technical Problem

In the industrialization of organic solar cells, differences in the surface morphology of the composite transport layer substrate lead to poor film formation, uniformity and stability of the thin film, affecting the photoelectric conversion efficiency of module devices.

Method used

The AZO thin film substrate of alcohol solution was prepared by scraping coating and vacuum evaporated to electron transport organic small molecule materials. The PEDOT:PSS substrate of aqueous solution was vacuum evaporated to hole transport organic small molecule materials to build a composite transport layer, and through scraping coating and The combined evaporation method fills holes and defects, and improves carrier collection efficiency and surface flatness.

Benefits of technology

It improves the stability and photoelectric conversion efficiency of organic solar cell modules, simplifies the preparation process, reduces costs, is suitable for flexible batteries, and significantly improves the performance of module devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112366278B_ABST
    Figure CN112366278B_ABST
Patent Text Reader

Abstract

The present invention provides a composite transport layer and its application and a method for preparing an organic solar cell module. The composite transport layer includes a composite electron transport layer and a composite hole transport layer. The composite electron transport layer is formed by coating an AZO film in an alcohol solution as a substrate and vacuum evaporating an electron transport organic small molecule material A. The composite hole transport layer is formed by coating a PEDOT:PSS film in an aqueous solution as a substrate and vacuum evaporating a hole transport organic small molecule material B. By vacuum evaporating an organic small molecule material on the surface of a thin film substrate prepared by scraping to construct a composite interface transport layer, the holes of the thin film substrate can be filled and the defects can be passivated, the carrier collection efficiency can be improved, and the surface flatness can be improved, and the stability and photoelectric conversion efficiency of the prepared solar cell module can be effectively improved. The composite transport layer prepared by the method is also suitable for flexible batteries, and the entire battery preparation process has high repeatability and is easy to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solar cell materials, and specifically relates to an organic solar cell module with stable coating and high photoelectric conversion efficiency, and more particularly to a composite transmission layer and its application in preparing a flexible organic solar cell module. Background Art

[0002] At present, organic solar cells are developing rapidly, and their photoelectric conversion efficiency in the laboratory stage has exceeded 18%. There is an urgent need for related industrialization research, so it is necessary to study and prepare high-efficiency organic solar cell module devices. For this purpose, the organic solar cell module prepared by scraping should have good repeatability while maintaining excellent photoelectric conversion efficiency.

[0003] Due to the different surface morphologies of the composite transport layer substrate, the film forming properties, uniformity and stability of the film prepared by scraping the upper layer will be further affected. If the film thickness difference in different areas, poor surface morphology and poor blending state are caused during the large-area scraping film forming process, the performance of the module device will be attenuated. At the same time, the excellent performance of the interface transport layer can greatly reduce intrinsic defects and interface defects, improve the carrier collection efficiency, and then improve the photoelectric conversion efficiency of the module device, thereby further promoting the industrialization of organic solar cells. Summary of the invention

[0004] In order to solve the above problems, the purpose of the present invention is to provide a composite transport layer and its application in a flexible organic solar cell module. The composite interface transport layer is constructed by vacuum evaporating an organic small molecule material on the surface of a thin film substrate prepared by scraping. The method of combining scraping and evaporation can be used to fill the holes in the thin film substrate and passivate the defects, thereby improving the carrier collection efficiency and surface flatness, and effectively improving the stability of the prepared solar cell module and the photoelectric conversion efficiency. The composite transport layer is also suitable for flexible batteries.

[0005] Another object of the present invention is to provide a method for preparing an organic solar cell module based on a composite transport layer, which has a simple preparation process, low cost, good repeatability, and can improve the efficiency of the module device.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows.

[0007] A composite transport layer, comprising a composite electron transport layer and a composite hole transport layer; the composite electron transport layer is formed by using an AZO coating film of an alcohol solution as a substrate, and vacuum evaporating an electron transport organic small molecule material A; the composite hole transport layer is formed by using a PEDOT:PSS coating film of an aqueous solution as a substrate, and vacuum evaporating a hole transport organic small molecule material B.

[0008] Furthermore, the materials of the composite electron transport layer and the composite hole transport layer are both composed of hybrid organic / inorganic materials.

[0009] Furthermore, the organic small molecule material A is any one or more of BPhen, TAZ, T3T, and TST; the organic small molecule material B is any one or more of TCTA, NPD, and TMPyP.

[0010] A method for preparing an organic solar cell module based on the composite transport layer comprises the following steps:

[0011] S101, preparing a cathode on a transparent substrate, and performing laser patterning etching on the cathode electrode;

[0012] S102, preparing an AZO thin film substrate on the cathode electrode by blade coating or slit coating; and vacuum evaporating an electron transport organic small molecule material A on the AZO thin film substrate to construct a composite electron transport layer;

[0013] S103, preparing a light absorption layer on the composite electron transport layer by a scraping method, and then preparing a hole transport layer on the light absorption layer;

[0014] S104, performing pattern cutting on the hole transport layer, and vapor-depositing electrodes on the cut film layer to obtain an organic solar cell module with a reverse structure.

[0015] Or include the following steps:

[0016] S201, preparing an anode on a transparent substrate, and performing laser patterning etching on the anode electrode;

[0017] S202, preparing a PEDOT:PSS thin film substrate on the anode electrode by blade coating or slit coating; and vacuum evaporating a hole transport organic small molecule material B on the PEDOT:PSS thin film substrate to construct a composite hole transport layer;

[0018] S203, preparing a light absorption layer on the composite hole transport layer by a scraping method, and then preparing an electron transport layer on the light absorption layer;

[0019] S204, performing pattern cutting on the electron transport layer, and vapor-depositing electrodes on the cut film layer to obtain an organic solar cell module with a forward structure.

[0020] Furthermore, the light absorption range of the composite electron transport layer is 200-450nm, the film thickness is 2-60nm, and the preferred film thickness is 10nm; the light absorption range of the composite hole transport layer is 200-500nm, the film thickness is 2-60nm, and the preferred film thickness is 8nm.

[0021] Further, in S102, when preparing the AZO thin film substrate by blade coating, the coating speed is 5-60 mm / s, the slit height is 5-80 um, the substrate temperature is 10-200° C., the annealing temperature is 50-300° C., and the time is 10-90 min;

[0022] In S202, when preparing the PEDOT:PSS thin film substrate, the scraping speed is 5-50 mm / s, the slit height is 5-60 um, the substrate temperature is 10-150° C., the annealing temperature is 40-200° C., and the time is 10-90 min.

[0023] Further, in S102, the rate of vacuum evaporation of electron transport organic small molecule material A is The preferred evaporation rate is

[0024] In S202, the rate of vacuum evaporation hole transport of organic small molecule material B is The preferred evaporation rate is

[0025] Furthermore, the substrate is any one of a glass substrate, a PET plastic substrate, a PEN plastic substrate, a flexible mesh silver substrate, and a flexible silver nanowire substrate.

[0026] Further, the electrode includes a cathode and a transparent electrode, or an anode and a transparent electrode;

[0027] Wherein, the material of the cathode is indium tin oxide or fluorine-doped tin dioxide;

[0028] The material of the anode is indium tin oxide or fluorine-doped tin dioxide;

[0029] The material of the transparent electrode is any one or more of an Ag electrode, an Al electrode, a Cu electrode, a carbon electrode, a PH1000 polymer electrode, a silver nanowire electrode, and a metal oxide electrode, preferably a silver nanowire electrode.

[0030] An application of the composite transmission layer in preparing a flexible organic solar cell module.

[0031] The battery module device structure prepared by the method of the present invention mainly includes a substrate, an electrode and a functional layer; the functional layer is mainly composed of a composite electron transport layer, a light absorption layer and a composite hole transport layer; the number of layers of the functional layer is 1 to 5. Among them, the prepared functional layer is composed of a composite electron transport layer, a light absorption layer and a hole transport layer or a composite hole transport layer, a light absorption layer and an electron transport layer.

[0032] In the present invention, in the reverse organic solar cell module based on the novel composite transport layer, the hole transport layer is selected from a polymer having a triphenylamine structure such as poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], a combination of a p-type semiconductor and an organic salt such as poly-3,4-ethylenedioxythiophene / polystyrene sulfonate, and one of metal oxides such as nickel oxide and molybdenum oxide. The hole transport layer is prepared on the light absorption layer by a scraping or evaporation method.

[0033] In the present invention, in the forward organic solar cell module based on the novel composite transport layer, the electron transport layer is one or more of metal oxides such as PFN-Br, PFN, PDINO, fullerenes such as PCBM, C60 and fullerene derivatives, and the electron transport layer is prepared on the light absorption layer by a method of scraping and then annealing.

[0034] Beneficial effects of the present invention:

[0035] 1. The present invention selects to prepare the transport layer by combining the scraping solution with the vacuum evaporation of small molecule materials, which has higher carrier transport performance, can effectively fill the hole defects of the interface transport layer, can improve the density and wettability of the film and reduce the surface roughness, and can not only improve the uniformity and stability of the upper light absorption layer film coating, but also has higher electron or hole collection efficiency, and finally improves the photoelectric conversion efficiency of the module device, which provides important help for the potential application of flexible organic solar cell modules and electronic equipment integration.

[0036] 2. Compared with the traditional interface transmission layer, the composite transmission layer of the present invention has good applicability. It is not only suitable for series battery modules, but also has a significant improvement effect on parallel battery modules. It is beneficial to improve the performance of module devices prepared by different connection methods, and also has a good effect on flexible substrates.

[0037] 3. The method of the present invention has a simple preparation process, low cost, good repeatability, and can improve the stability of the solution coating, the photoelectric conversion efficiency of the organic solar cell module, and the module device efficiency. The high-performance organic solar cell module prepared by the present invention greatly meets the demand for electricity consumption in daily life, and has broad application prospects in the fields of electronic equipment integration, making it a highly competitive new generation of clean energy; at the same time, the invented new composite transmission layer provides important help for the development of stacked cells, and combined with dye-sensitized solar cells, perovskite cells, silicon cells, and copper indium gallium selenide cells, it can effectively improve the efficiency of stacked cell modules. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is the transmission curve diagram of the glass substrate / AZO and glass substrate / AZO / BPhen structures in Example 1.

[0039] Figure 2 This is a two-dimensional plane diagram of the surface roughness of the glass substrate / AZO and glass substrate / AZO / BPhen structures in Example 1.

[0040] Figure 3 This is a three-dimensional surface morphology of the glass substrate / AZO and glass substrate / AZO / BPhen structures in Example 1.

[0041] Figure 4 This is a contact angle test diagram of the glass substrate / AZO and glass substrate / AZO / BPhen structures in Example 1.

[0042] Figure 5 This is a two-dimensional plane diagram of the surface roughness of the light absorbing layer film coated on different substrates in Example 1.

[0043] Figure 6 This is a three-dimensional surface morphology diagram of a light absorption layer film scraped out on different substrates in Example 1.

[0044] Figure 7 Diagrams of different positions for measuring thickness of the organic solar cell module of Example 1.

[0045] Figure 8 It is a JV curve diagram of the rigid organic solar cell module of Example 1 and the rigid organic solar cell module prepared with a traditional transport layer.

[0046] Fig. 9 It is a JV curve diagram of the flexible organic solar cell module of Example 2 and the flexible organic solar cell module prepared with a traditional transmission layer. DETAILED DESCRIPTION

[0047] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0048] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.

[0049] Embodiment 1

[0050] A composite transport layer, comprising a composite electron transport layer and a composite hole transport layer; the composite electron transport layer is formed by using an AZO coating film of an alcohol solution as a substrate, and vacuum evaporating an electron transport organic small molecule material A; the composite hole transport layer is formed by using a PEDOT:PSS coating film of an aqueous solution as a substrate, and vacuum evaporating a hole transport organic small molecule material B.

[0051] Wherein, the composite electron transport layer and the composite hole transport layer are both composed of hybrid organic / inorganic materials. The organic small molecule material A is any one or more of BPhen, TAZ, T3T, and TST; and the organic small molecule material B is any one or more of TCTA, NPD, and TMPyP.

[0052] The method for preparing an organic solar cell module based on the composite transmission layer comprises the following steps:

[0053] S101, using a glass rigid substrate, polishing it, and then coating a layer of indium tin oxide thin film on the glass by magnetron sputtering to form ITO conductive glass as the cathode of the solar cell; then performing patterned laser etching on the ITO conductive glass;

[0054] S102, coating AZO solution on the patterned ITO conductive glass, with a slit height of 20 μm, a substrate temperature of 40° C., a coating speed of 30 mm / s, and annealing at 140° C. in air for 20 min to obtain a film of about 20 nm;

[0055] S103, place the ITO with AZO nanofilm in a nitrogen glove box and put it into a vacuum coating machine, and wait until the pressure of the chamber is pumped down to 3×10 -4 Pa, The composite transport layer is constructed by evaporating 10nm of BPhen organic small molecule material at a rate of

[0056] Among them, the chemical structure formula of BPhen is:

[0057]

[0058] S104, then take out the evaporated substrate from the warehouse, place it on a scraper in the air to scrape the light absorption layer solution, the light absorption layer solution is a binary system solution, its components are PM6 and Y6, the ratio is PM6:Y6=1:1.2, the total concentration is 16mg / mL, the solvent is pure chloroform solution; all solutions can be used after stirring for 6 hours; the slit height during scraping is 20um, the substrate temperature is 60℃, and the scraping speed is 40mm / s; then annealing at 110℃ for 10min, and the thickness of the obtained light absorption layer is 100nm;

[0059] The chemical structure of PM6 is:

[0060]

[0061] The chemical structure of Y6 is:

[0062]

[0063] S105, place the cell with the light absorption layer film coated in a vacuum evaporation machine, and wait until the pressure in the chamber is pumped down to 3×10 -4 Pa, 10 nm MoO3 was evaporated at a rate of 1.0 wt % as a hole transport layer.

[0064] S106, take out the battery cells from the chamber, place them in the mold for physical segmentation, expose 1mm of electrodes for upper and lower connections between modules, build series batteries, and then continue to place the battery cells in the coating machine until the cabin pressure is pumped to 3×10 -4 Pa, A 300nm aluminum electrode was evaporated at a rate of ; an organic solar cell module with a reverse structure was obtained.

[0065] Embodiment 2

[0066] A composite transport layer, comprising a composite electron transport layer and a composite hole transport layer; the composite electron transport layer is formed by using an AZO coating film of an alcohol solution as a substrate, and vacuum evaporating an electron transport organic small molecule material A; the composite hole transport layer is formed by using a PEDOT:PSS coating film of an aqueous solution as a substrate, and vacuum evaporating a hole transport organic small molecule material B.

[0067] Wherein, the composite electron transport layer and the composite hole transport layer are both composed of hybrid organic / inorganic materials. The organic small molecule material A is any one or more of BPhen, TAZ, T3T, and TST; and the organic small molecule material B is any one or more of TCTA, NPD, and TMPyP.

[0068] The method for preparing an organic solar cell module based on the composite transmission layer comprises the following steps:

[0069] S201, using a PET / ITO flexible substrate, using a cotton swab dipped in ethanol to wipe the surface electrode as the cathode of the solar cell, and then using a laser etcher to perform pattern cutting;

[0070] S202, coating the AZO solution on the patterned PET / ITO conductive substrate, fixing the flexible substrate by vacuum adsorption, with a slit height of 20 um, a substrate temperature of 40° C., a coating speed of 30 mm / s, and annealing at 140° C. in air for 20 min to obtain an electron transport layer;

[0071] S203, place the ITO with electron transport layer in a nitrogen glove box, attach it to the glass substrate and put it into the vacuum coating machine, and wait until the pressure of the chamber is pumped to 3×10 -4 Pa, 10 nm of BPhen was evaporated at a rate of 100 nm as an electron dense layer to construct a composite transport layer.

[0072] S204, then take out the evaporated substrate from the warehouse, place it on a scraper in the air, and scrape the light absorption layer solution, the light absorption layer solution is also a binary system solution, its components are PM6 and Y6, the ratio is PM6:Y6=1:1.2, the total concentration is 18mg / mL, and the solvent is pure chloroform solution; all solutions can be used after stirring for six hours; the slit height during scraping is 20um, the substrate temperature is 65°C, and the scraping speed is 30mm / s; then annealing on a vacuum hot stage at 110°C for 10min, and the obtained light absorption layer film thickness is about 120nm;

[0073] S205, place the cell with the light absorption layer film coated in a vacuum evaporation machine, and wait until the pressure in the chamber is pumped down to 3×10 -4 Pa, 10 nm MoO3 was evaporated at a rate of 100 nm as a hole transport layer;

[0074] S206, take out the battery cells from the chamber, place them in the mold for physical segmentation, expose 1mm of electrodes for upper and lower connections between modules, build series batteries, and then continue to place the battery cells in the coating machine until the cabin pressure is pumped to 3×10 -4 Pa, A 300nm aluminum electrode was evaporated at a rate of.

[0075] Embodiment 3

[0076] A composite transport layer, comprising a composite electron transport layer and a composite hole transport layer; the composite electron transport layer is formed by using an AZO coating film of an alcohol solution as a substrate, and vacuum evaporating an electron transport organic small molecule material A; the composite hole transport layer is formed by using a PEDOT:PSS coating film of an aqueous solution as a substrate, and vacuum evaporating a hole transport organic small molecule material B.

[0077] Wherein, the composite electron transport layer and the composite hole transport layer are both composed of hybrid organic / inorganic materials. The organic small molecule material A is any one or more of BPhen, TAZ, T3T, and TST; and the organic small molecule material B is any one or more of TCTA, NPD, and TMPyP.

[0078] The method for preparing an organic solar cell module based on the composite transmission layer comprises the following steps:

[0079] S101, using a glass rigid substrate, polishing it, and then coating a layer of indium tin oxide thin film on the glass by magnetron sputtering to form ITO conductive glass, which serves as an anode of a solar cell; and then performing patterned laser etching on the ITO conductive glass;

[0080] S102, coating the PEDOT:PSS solution on the patterned ITO conductive glass with a slit height of 20 μm, a substrate temperature of 40° C., a coating speed of 30 mm / s, and annealing at 140° C. in air for 20 min to obtain a film of about 20 nm;

[0081] S103, place the ITO with PEDOT:PSS nanofilm in a nitrogen glove box and put it into a vacuum coating machine, and wait until the pressure of the chamber is pumped down to 3×10 -4 Pa, The composite transport layer is constructed by evaporating 10nm of TCTA organic small molecule material at a rate of

[0082] Among them, the chemical structure formula of TCTA is:

[0083]

[0084] S104, then take out the evaporated substrate from the warehouse, place it on a scraper in the air to scrape the light absorption layer solution, the light absorption layer solution is a binary system solution, its components are PM6 and Y6, the ratio is PM6:Y6=1:1.2, the total concentration is 16mg / mL, the solvent is pure chloroform solution; all solutions can be used after stirring for 6 hours; the slit height during scraping is 20um, the substrate temperature is 60℃, and the scraping speed is 40mm / s; then annealing at 110℃ for 10min, and the thickness of the obtained light absorption layer is 100nm;

[0085] S105, place the cell with the light absorption layer film coated in a vacuum evaporation machine, and wait until the pressure in the chamber is pumped down to 3×10 -4 Pa, 10 nm of Cs2CO3 was evaporated at a rate of 1.0 wt % as an electron transport layer.

[0086] S106, take out the battery cells from the chamber, place them in the mold for physical segmentation, expose 1mm of electrodes for upper and lower connections between modules, build series batteries, and then continue to place the battery cells in the coating machine until the cabin pressure is pumped to 3×10 -4 Pa, A 300nm aluminum electrode was evaporated at a rate of ; and an organic solar cell module with a forward structure was obtained.

[0087] The performance test of the organic solar cell module based on the composite transport layer of Example 1 and Example 2 was carried out, and the results are as follows: Figures 1 to 8 .

[0088] Figure 1 These are the transmission curves of glass substrate / AZO and glass substrate / AZO / BPhen structures. It can be seen from the curve that when an electron-dense layer is evaporated on the surface of the AZO substrate, it does not affect the transmittance of the substrate in the range of 300-900 nanometers, which also ensures that the overall performance of the module device is not affected.

[0089] Figure 2 is the two-dimensional plane image of the surface roughness of glass substrate / AZO and glass substrate / AZO / BPhen structures, Figure 2 It can be seen that when an electron dense layer is evaporated on the electron transport layer, the surface roughness can be effectively reduced, which is more conducive to the stability and uniformity of the subsequent light absorption layer coating.

[0090] Figure 3 The three-dimensional surface morphology of glass substrate / AZO and glass substrate / AZO / BPhen structures is shown in Figure 2. Figure 3 It can be seen that the glass substrate / AZO has a wide range of thickness fluctuations, resulting in the entire surface being uneven. By adding an electron-dense layer, the hole defects and surface flatness of the AZO substrate can be effectively filled, making the entire base surface smoother, which has a significant impact on the quality of the subsequent coating film.

[0091] Figure 4 The surface wettability of glass substrate / AZO and glass substrate / AZO / BPhen structures was studied by testing the contact angle. It was found that adding a BPhen electron-dense layer on the AZO surface can effectively improve the flatness and wettability of the substrate surface, which is also beneficial to the subsequent scraping of the light absorption layer solution and improves the quality and stability of the coating.

[0092] Figure 5 is a two-dimensional plane diagram of the surface roughness of the light absorbing layer film coated on different substrates. Figure 5 It can be seen that when an electron dense layer is added on the electron transport layer, the surface roughness of the light absorption layer film scraped out as a substrate is significantly reduced, indicating that a flat substrate is conducive to scraping out a film with a uniform surface.

[0093] Figure 6 In order to obtain the three-dimensional surface morphology of the light absorbing layer film by scraping on different substrates, Figure 6 It can be seen that the film coated on the composite transmission layer has a uniform surface thickness, without a large range of height differences, and has a better surface morphology.

[0094] Figure 7 Table 1 shows the film thickness values ​​in different regions.

[0095] Table 1 Thickness of different regions of the light absorption layer film based on different substrates

[0096]

[0097]

[0098] according to Figure 7 As can be seen from Table 1, by measuring the film thickness of the scraped light absorbing layer in different areas, it can be more intuitively found that when the new composite transmission layer is used as the substrate, the film thickness uniformity of the scraped light absorbing layer is greatly improved, which is crucial to improving the performance of the module device. It shows that the performance of each battery in the prepared series battery module is equivalent, thereby ensuring the overall device performance.

[0099] Figure 8 It is a JV curve diagram of the rigid organic solar cell module prepared in Example 1 and the rigid organic solar cell module prepared with a traditional transport layer.

[0100] Among them, the rigid organic solar cell module prepared with a traditional transmission layer is used as the control group I, and the rigid organic solar cell module prepared in Example 1 is used as the experimental group I. The test results are shown in Table 2.

[0101] The rigid organic solar cell module structure of the control group I is:

[0102] Glass substrate / AZO / light absorption layer / MoO3 / aluminum.

[0103] The rigid organic solar cell module structure of experimental group I is:

[0104] Glass substrate / AZO / BPhen / light absorption layer / MoO3 / aluminum.

[0105] Table 2 Photovoltaic performance test results of rigid organic solar cell modules of experimental group I and control group I

[0106]

[0107] Depend on Figure 8 It can be seen from the JV curve and the photovoltaic parameters in Table 2 that when the composite transport layer is used, the morphology and thickness uniformity of the scraped film are well improved and the carrier mobility is enhanced, so the device performance is greatly improved, mainly manifested in the increase of short-circuit current density. This shows that the film scraped out based on the new transport layer substrate has better film forming properties, fewer defects inside, and higher conversion efficiency for absorbed photons. The photoelectric conversion efficiency of the new module device finally prepared is about 0.9% higher than that of the traditional module device.

[0108] Fig. 9It is a JV curve diagram of the flexible organic solar cell module prepared in Example 2 and the flexible organic solar cell module prepared with a traditional transmission layer.

[0109] Among them, the flexible organic solar cell module prepared with a traditional transmission layer is the control group II, and the flexible organic solar cell module prepared in Example 2 is the experimental group II. The test results are shown in Table 3.

[0110] The flexible organic solar cell module structure of control group II is:

[0111] PET substrate / AZO / light absorption layer / MoO3 / aluminum.

[0112] The flexible organic solar cell module structure of experimental group II is:

[0113] PET substrate / AZO / BPhen / light absorption layer / MoO3 / aluminum.

[0114] Table 3 Photovoltaic performance test results of flexible organic solar cell modules of experimental group II and control group II

[0115]

[0116] Depend on Fig. 9 From the JV curve and the photovoltaic parameters in Table 3, it can be seen that the new composite transmission layer also has good device performance on the flexible substrate. Compared with the traditional module device, the flexible module device based on the new composite transmission layer has greatly improved the open circuit voltage and short circuit current density, and finally the photoelectric conversion efficiency of the module device has increased by about 1.2%. It shows that adding an electron dense layer on the rough PET substrate surface can effectively increase the surface flatness, and has great application potential in improving the performance of flexible module devices in the future.

[0117] In summary, by introducing an electron-dense layer into the traditional transport layer to construct a new composite transport layer, the method of combining scraping and evaporation not only improves the photoelectric performance of the film, but also reduces the roughness of the substrate and increases the substrate wettability, which helps the film-forming property of the light absorption layer during the scraping process, making the film thickness uniform and the morphology good. Ultimately, the overall photoelectric conversion efficiency of the module device can be improved. At the same time, it also has a good performance improvement effect on a flexible substrate, indicating that this preparation method has an important impact on promoting the development of organic photovoltaic industrialization.

[0118] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an organic solar cell module based on a composite transport layer, characterized in that: The following steps are involved: S101, preparing a cathode on a transparent substrate, and performing laser patterning etching on the cathode electrode; S102, preparing an AZO thin film substrate on the cathode electrode by a doctor blade coating method; and constructing a composite electron transport layer by vacuum evaporating an electron transport organic small molecule material A on the AZO thin film substrate; the composite electron transport layer is formed by coating an AZO film with an alcohol solution as a substrate and vacuum evaporating an electron transport organic small molecule material A; the organic small molecule material A is any one or more of BPhen, TAZ, T3T, and TST; the light absorption range of the composite electron transport layer is 200-450nm, and the film thickness of the composite electron transport layer is 2-60nm; S103, preparing a light absorption layer on the composite electron transport layer by a scraping method, and then preparing a hole transport layer on the light absorption layer; S104, performing pattern cutting on the hole transport layer, and evaporating electrodes on the cut film layer to obtain an organic solar cell module with a reverse structure; Or include the following steps: S201, preparing an anode on a transparent substrate, and performing laser patterning etching on the anode electrode; S202, preparing a PEDOT:PSS thin film substrate on the anode electrode by blade coating; and constructing a composite hole transport layer by vacuum evaporating a hole transport organic small molecule material B on the PEDOT:PSS thin film substrate; the composite hole transport layer is formed by coating a PEDOT:PSS film in an aqueous solution as a substrate, and vacuum evaporating a hole transport organic small molecule material B; the organic small molecule material B is any one or more of TCTA, NPD, and TMPyP; the light absorption range of the composite hole transport layer is 200-500nm, and the film thickness of the composite hole transport layer is 2-60nm; S203, preparing a light absorption layer on the composite hole transport layer by a scraping method, and then preparing an electron transport layer on the light absorption layer; S204, performing pattern cutting on the electron transport layer, and vapor-depositing electrodes on the cut film layer to obtain an organic solar cell module with a forward structure.

2. The method for preparing an organic solar cell module based on a composite transport layer according to claim 1, characterized in that: In S102, the scraping speed of the AZO thin film substrate prepared by scraper coating is 5 to 60 mm / s, the slit height is 5 to 80 um, and the substrate temperature is 10 to 200 o C, annealing temperature is 50~300 o C, time is 10 to 90 minutes; In S202, the scraping speed when preparing the PEDOT:PSS thin film substrate is 5-50 mm / s, the slit height is 5-60 um, and the substrate temperature is 10-150 o C, annealing temperature is 40~200 o C, time is 10 to 90 min.

3. The method for preparing an organic solar cell module based on a composite transport layer according to claim 1, characterized in that: In S102, the rate of vacuum evaporation of electron transport organic small molecule material A is 0.1-10 Å / s; In S202, the rate of vacuum evaporation hole transport of organic small molecule material B is 0.2-8 Å / s.

4. The method for preparing an organic solar cell module based on a composite transport layer according to claim 1, characterized in that: The substrate is any one of a glass substrate, a PET plastic substrate, a PEN plastic substrate, a flexible mesh silver substrate, and a flexible silver nanowire substrate.

5. An organic solar cell module based on a composite transport layer prepared by the preparation method according to claim 1.