A pure handmade silk cotton long fiber whole stretching equipment and process
Through a whole-sheet stretching quilt-making process that includes cocoon cooking, rinsing, cocoon pulling, and expansion, the problem of difficulty in stretching the entire silk quilt during the preparation process is solved, and the silk quilt is realized. Uniform laying and high elasticity avoid the generation of static electricity and reduce the cost of manual expansion.
Patent Information
- Application Number
- CN202011372755.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-11-30
AI Technical Summary
It is difficult to stretch the entire sheet of existing handmade silk quilts during the preparation process, which causes the silk to break easily, and the produced silk quilts are uneven in thickness and prone to misalignment and deformation.
A process including cocoon selection, cocoon cooking, rinsing, cocoon pulling and wadding, expansion, drying, wadding and edge locking is adopted. Double palace cocoons with a silk length of more than 1200m are selected and processed using edible alkali and purified water. Cocoon cooking and rinsing, combined with two-way parallel stretching and expansion technology, ensure even stretching and laying of silk.
It realizes the entire silk quilt laying, avoids the problems of silk breakage and uneven thickness, improves the elasticity and service life of the silk quilt, reduces the cost of manual expansion, and prevents the generation of static electricity.
Smart Images

Figure CN112411021B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a silk quilt processing technology, and specifically designs a whole-sheet stretching device and a technology for silk cotton filaments. Background Art
[0002] Silk is the lightest, softest and finest natural fiber in nature. It can easily return to its original shape after the external force is removed. The inner tube does not cake, does not feel stuffy, does not shrink, is uniform and soft, and can be used permanently without turning over. Silk quilts are made of high-quality silk with a novel fiber structure to allow water vapor to flow freely. In addition, the unique air permeability and moisture permeability of silk itself make silk quilts feel smoother, cool but not warm, warm but not dry. Mulberry silk is mainly composed of animal protein and is rich in 18 kinds of amino acids necessary for the human body. It can promote the vitality of skin cells and prevent vascular sclerosis. Long-term use can prevent skin aging. It has a special antipruritic effect on certain skin diseases and has a certain health care effect on arthritis, periarthritis of the shoulder, and asthma. It is known as the "second skin of the human body" and the "Queen of Fibers".
[0003] However, the cotton pockets used to make pure handmade silk quilts today are all relatively small, usually only about 50 cm. During the stretching process of the quilt, it is impossible to stretch the entire sheet manually, the silk is easily broken, and the entire sheet cannot be laid. Therefore, existing pure handmade silk quilts are all made by splicing, which is prone to problems such as uneven thickness, misalignment and deformation. Summary of the invention
[0004] The purpose of the present invention is to provide a quilt that can be used for whole-sheet silk laying and can be made into quilts of different sizes using pure handmade cotton of the required length of silk cotton, thereby solving the problems of the existing pure handmade silk quilts mentioned in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A pure handmade silk cotton long fiber whole stretch quilt making process, including cocoon selection, cocoon boiling, rinsing, cocoon picking and cotton application, cotton expansion, drying, cotton spreading and edge locking;
[0007] Select cocoons, select double palace cocoons with silk length of more than 1200m, and the cocoons are used as raw materials. The selected cocoons are put into dry preservation bags and placed at room temperature for use;
[0008] For cocoon boiling, edible alkali and pure water are first mixed in a weight ratio of 1 to 2:100, and the pH value is controlled at 8 to 11. Two portions of the mixed water are placed at room temperature for standby use; one portion of the mixed water is used to boil the cocoons for no less than 30 minutes, during which constant temperature control is performed, the cocoons are intermittently rolled and stirred, and the temperature is controlled to be 100°C; another portion of the mixed water is heated to a temperature between 50 and 70°C, and the cocoons are placed in the mixed water for 1 to 30 minutes for temperature difference penetration; finally, the cocoon boiling process is repeated on the infiltrated cocoons; the number of repetitions is adjusted according to the temperature, and the purpose of cocoon layer penetration is finally achieved; during this period, the external temperature is a factor that determines the number of cocoon boiling times, wherein the temperature is between 0 and 18°C for at least 4 times, between 18 and 26°C for 2 to 3 times, and above 26°C for 1 to 2 times. The whole process takes more than 3 hours, because boiling the cocoons is very important, which can not only remove the cocoons and add cotton, but also avoid damaging the cocoon silk. Maintaining the strength of the cocoon silk is very important for the service life of the cotton and silk quilt.
[0009] Rinse, first rinse the cocoons with clean water to ensure that the residual liquid is clear; soak the rinsed cocoons in a mixture of edible white vinegar and pure water for 3-4 times, wherein the amount of edible white vinegar and water is 20-30 ml of edible white vinegar and 10 L of water for 1 kg of cocoons, and the pH value is controlled at 6.5-7. After soaking, rinse again with clean water;
[0010] Cocoons are pulled out and the silk is added. The cocoons are stretched individually to remove the cocoon cakes and black moles. The thickness of the silk is even and the layers are aligned. The silk is added one by one without breaking the silk to ensure uniform stretching and make silk cotton bags.
[0011] Sponge expansion: put the prepared silk cotton bag on the stretching equipment. During the sponge expansion process, it needs to be expanded in water, where the water temperature does not exceed 60°C, and the sponge expansion is carried out by bidirectional parallel stretching;
[0012] Drying: Let the expanded cotton dry naturally and set aside;
[0013] Spreading cotton: Spread the dried cotton manually, and use the method of layer-by-layer overlapping and cross-crossing to form a mesh-shaped cotton quilt. According to the different weights of the silk quilt, a silk quilt needs to be spread with thousands of layers of cotton. In this process, it is stretched according to different size requirements;
[0014] Edge locking: Use a batten board to press the edge of the silk quilt onto the operating platform along the edge of the quilt, use a retaining spring to clamp the batten board to fix the silk and prevent it from moving, and use an electric edge locking machine to rotate and lock the edge of the silk quilt pressed by the batten board.
[0015] Preferably, the cocoon boiling is repeated twice and the cocoon boiling time is 30 minutes.
[0016] Preferably, during the rinsing process, the amount of edible white vinegar and water used is in the ratio of 20 ml of edible white vinegar to 10 L of water for soaking 1 kg of silkworm cocoons.
[0017] A whole-sheet stretching device for silk floss filaments comprises a floss expansion zone, a control zone and an adjusting bracket, wherein the control zone and the adjusting bracket are sequentially arranged below the floss expansion zone, a water inlet pipe and a water outlet pipe are respectively arranged on the floss expansion zone and the control zone, and a water inlet, a water outlet and a floss expansion unit are arranged inside the floss expansion zone; a constant temperature return water unit and a power output device are arranged inside the control zone, the constant temperature return water unit is connected to the bottom of the floss expansion zone, the constant temperature return water unit is connected to the water outlet pipe, a water outlet valve is arranged above the water outlet pipe, the constant temperature return water unit comprises a return water pipe, a return water valve, a return water pump and a heating device are sequentially arranged on the return water pipe according to the water flow direction; the power output device is connected to the floss expansion unit circuit, the floss expansion unit comprises a guide rail and a pull rod fixer, the pull rod fixer is slidably arranged above the guide rail, a pull rod is installed between the pull rod fixers, and a fixed bracket is arranged below the power output device.
[0018] Preferably, two ends of the constant temperature water return unit are connected to a water inlet and a water outlet respectively.
[0019] Preferably, both ends of the water return pipe are connected to a water inlet and a water outlet respectively.
[0020] Preferably, a thermometer and a liquid level gauge are also provided on the sponge expansion zone, and a heating device is provided at the bottom of the sponge expansion zone.
[0021] Preferably, the adjustment bracket is composed of a plurality of support blocks, and the support blocks are provided with adjustment holes, so that the overall height of the equipment can be adjusted.
[0022] Preferably, the pull rod fixer includes an adjusting fixture, and adjusting rods are respectively provided at the left and right ends of the adjusting fixture, and the two ends of the adjusting rod are respectively connected to the adjusting fixture and the roller, and telescopic adjustment keys and telescopic rods are respectively provided at the upper and lower ends of the adjusting fixture, and a fixed bin is provided at the end of the telescopic rod, and a fixing rod is penetrated through the fixed bin.
[0023] Preferably, the rollers are arranged on both sides of the guide rail and the rollers are slidably matched with the guide rail.
[0024] It is explained here that the heating device is a heater and the power output device is a servo motor.
[0025] Beneficial effects:
[0026] 1. The pure handmade silk cotton filament whole-sheet stretching quilt-making process of the present invention can be carried out in a pure handmade manner during use, and the produced pure handmade silk quilt does not need to be spliced, has uniform thickness, and is not easy to be dislocated or deformed; at the same time, during use, the silk quilt produced by the present invention is soaked in edible white vinegar for cocoon removal and cotton application, which can effectively prevent the silk quilt from easily generating static electricity, and solves the defects of silk quilts in the prior art; furthermore, the pure handmade stretching can make the silk quilt fluffy when used, and has more elasticity than the silk quilt formed by splicing.
[0027] 2. The cotton expansion equipment of the present invention can achieve homogenization and soaking through water. Cooperating with the whole stretching quilt making process of the silk cotton long fiber of the present invention, the silk quilt can be made more elastic and will not break; it can replace the splicing process and reduce the cost of manual cotton expansion. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the structure of the present invention;
[0029] Figure 2 A top view of the present invention;
[0030] Figure 3 It is a schematic diagram of the structure of the pull rod fixing device of the present invention.
[0031] In the figure: 1, thermometer, 2, liquid level gauge, 3, expansion area, 4, heating device, 5, water outlet valve, 6, water outlet pipe, 7, water return pipe, 8, water return pump, 9, water return valve, 10, water inlet pipe, 11, power output device, 12, fixed bracket, 13, control area, 14, adjustment hole, 15, guide rail, 16, water outlet, 17, water inlet, 18, pull rod holder;
[0032] 18b, roller, 18c, adjusting rod, 18d, adjusting fixing piece, 18e, telescopic rod, 18f, fixing rod, 18g, fixing bin, 18h, telescopic adjusting key. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] See also Figures 1 to 3 , the present invention provides a technical solution:
[0036] A pure handmade silk cotton long fiber whole stretch quilt making process, including cocoon selection, cocoon boiling, rinsing, cocoon picking and cotton application, cotton expansion, drying, cotton spreading and edge locking;
[0037] Select cocoons, select double palace cocoons with silk length of more than 1200m, and the cocoons are used as raw materials. The selected cocoons are put into dry preservation bags and placed at room temperature for use;
[0038] To cook the cocoons, firstly, edible alkali and pure water are mixed in a weight ratio of 1:100, and the pH value is controlled at 8. Two portions of the mixed water are placed at room temperature for standby use; first, one portion of the mixed water is used to cook the cocoons for no less than 30 minutes, during which constant temperature control is performed, and the cocoons are intermittently rolled and stirred, and the temperature is controlled at 100°C; then the other portion of the mixed water is heated to 50°C, and then the above cocoons are placed in the mixed water and placed for 15 minutes for temperature difference penetration; finally, the above cocoon cooking process is repeated for the infiltrated cocoons; the number of repetitions is adjusted according to the temperature, and finally the purpose of cocoon layer penetration is achieved; during this period, the external temperature is the factor that determines the number of cocoon cooking times, among which, the temperature is between 5°C for at least 4 times, 18-26°C for 2-3 times, and above 26°C for 1-2 times. The whole process takes more than 3 hours, because cocoon cooking is very important, which can not only remove the cocoons and put on the cotton, but also not cook the cocoon silk, and maintain the strength of the cocoon silk, which is very important for the service life of the cotton and silk quilt;
[0039] Rinse, first rinse the cocoons with clean water to ensure that the residual liquid is clear; soak the rinsed cocoons in a mixture of edible white vinegar and pure water for 3 times, wherein the amount of edible white vinegar and water is 20 ml of edible white vinegar and 10 L of water for 1 kg of cocoons, and the pH value is controlled at 6.5-7. After soaking, rinse again with clean water;
[0040] Cocoons are pulled out and the silk is added. The cocoons are stretched individually to remove the cocoon cakes and black moles. The thickness of the silk is even and the layers are aligned. The silk is added one by one without breaking the silk to ensure uniform stretching and make silk cotton bags.
[0041] Sponge expansion: put the prepared silk cotton bag on the stretching equipment. During the sponge expansion process, it needs to be expanded in water, where the water temperature does not exceed 60°C, and the sponge expansion is carried out by bidirectional parallel stretching;
[0042] Drying: Let the expanded cotton dry naturally and set aside;
[0043] Spreading cotton: Spread the dried cotton manually, and use the method of layer-by-layer overlapping and cross-crossing to form a mesh-shaped cotton quilt. According to the different weights of the silk quilt, a silk quilt needs to be spread with thousands of layers of cotton. In this process, it is stretched according to different size requirements;
[0044] Edge locking: Use a batten board to press the edge of the silk quilt onto the operating platform along the edge of the quilt, use a retaining spring to clamp the batten board to fix the silk and prevent it from moving, and use an electric edge locking machine to rotate and lock the edge of the silk quilt pressed by the batten board.
[0045] The cocoon boiling was repeated twice, and the cocoon boiling time was 30 minutes.
[0046] During the rinsing process, the amount of edible white vinegar and water used is 20 ml of edible white vinegar and 10 L of water for soaking 1 kg of silkworm cocoons.
[0047] A whole-sheet stretching device for silk floss filaments comprises a floss expansion zone 3, a control zone 13 and an adjusting bracket, wherein the control zone 13 and the adjusting bracket are sequentially arranged below the floss expansion zone 3, a water inlet pipe 10 and a water outlet pipe 6 are arranged on the floss expansion zone 3 and the control zone 13 respectively, and a water inlet 17, a water outlet 16 and a floss expansion unit are arranged inside the floss expansion zone 3; a constant temperature return water unit and a power output device 11 are arranged inside the control zone 13, the constant temperature return water unit is connected to the bottom of the floss expansion zone 3, and the constant temperature return water unit is connected to the power output device 11. The water outlet pipe 6 is connected, and a water outlet valve 5 is arranged above the water outlet pipe 6. The constant temperature return water unit includes a return water pipe 7, and a return water valve 9, a return water pump 8 and a heating device 4 are arranged on the return water pipe 7 in sequence according to the water flow direction; the power output device 11 is connected to the expansion unit circuit, and the expansion unit includes a guide rail 15 and a pull rod fixer 18. The pull rod fixer 18 is slidably arranged above the guide rail 15, and a pull rod is installed between the pull rod fixers 18. A fixed bracket 12 is arranged below the power output device 11.
[0048] The two ends of the constant temperature return water unit are respectively connected to the water inlet 17 and the water outlet 16. The two ends of the return water pipe 7 are respectively connected to the water inlet 17 and the water outlet 16. The expansion area 3 is also provided with a thermometer 1 and a liquid level gauge 2, and the bottom of the expansion area 3 is provided with a heating device 4. The adjustment bracket is composed of a plurality of support blocks, and the support blocks are provided with adjustment holes 14. The pull rod fixer 18 includes an adjustment fixing 18d, and the left and right ends of the adjustment fixing 18d are respectively provided with adjustment rods 18c, and the two ends of the adjustment rod 18c are respectively connected to the adjustment fixing 18d and the roller 18b, and the upper and lower ends of the adjustment fixing 18d are respectively provided with a telescopic adjustment key 18h and a telescopic rod 18e, and the end of the telescopic rod 18e is provided with a fixed bin 18g, and the fixed bin 18g is penetrated by a fixed rod 18f. The roller 18b is provided on both sides of the guide rail 15, and the roller 18b and the guide rail 15 are slidably matched.
[0049] During operation, water is first added to the expansion zone 3 through the water inlet pipe 10. According to actual use, the water level inside the expansion zone 3 is determined by observing the liquid level meter 2, and then a small opening is made in the silk floss bag. (It should be noted that in the prior art, in order to solve the problem that the silk floss bag cannot be completely stretched as a whole, the silk floss bag is cut and broken and combined by splicing) and the opening is put on the pull rod for stretching, which requires soaking in water. During this process, the temperature is determined by observing the display above the thermometer 1, and stretching is performed at a suitable temperature. The changes in the thermometer 1 are observed, and the temperature control is achieved by manually turning on or off the heating device 4; finally, during stretching, the water level inside the expansion zone 3 can be controlled by the return valve 9 and the outlet valve 5 to achieve resource reuse and recycling.
[0050] Example 2
[0051] See also Figures 1 to 3 , the present invention provides a technical solution:
[0052] A pure handmade silk cotton long fiber whole stretch quilt making process, including cocoon selection, cocoon boiling, rinsing, cocoon picking and cotton application, cotton expansion, drying, cotton spreading and edge locking;
[0053] Select cocoons, select double palace cocoons with silk length of more than 1200m, and the cocoons are used as raw materials. The selected cocoons are put into dry preservation bags and placed at room temperature for use;
[0054] For cocoon boiling, edible alkali and purified water are first mixed in a weight ratio of 1.5:100, and the pH value is controlled at 8-11. Two portions of the mixed water are placed at room temperature for standby; one portion of the mixed water is used to boil the cocoons for no less than 30 minutes, during which constant temperature control is performed, the cocoons are intermittently rolled and stirred, and the temperature is controlled to be 100°C; the other portion of the mixed water is heated to a temperature of 65°C, and the cocoons are placed in the mixed water and placed for 15-30 minutes for temperature difference penetration; finally, the cocoon boiling process is repeated on the infiltrated cocoons; the number of repetitions is adjusted according to the temperature, and the purpose of cocoon layer penetration is finally achieved; during this period, the external temperature is a factor that determines the number of cocoon boiling times, wherein the temperature is between 0-18°C for at least 4 times, between 18-26°C for 2-3 times, and above 26°C for 1-2 times. The whole process takes more than 3 hours, because boiling the cocoons is very important, which can not only remove the cocoons and add cotton, but also avoid damaging the cocoon silk. Maintaining the strength of the cocoon silk is very important for the service life of the cotton and silk quilt.
[0055] Rinse, first rinse the cocoons with clean water to ensure that the residual liquid is clear; soak the rinsed cocoons in a mixture of edible white vinegar and pure water for 3-4 times, wherein the amount of edible white vinegar and water is 25 ml of edible white vinegar and 10 L of water for 1 kg of cocoons, and the pH value is controlled at 6.5-7. After soaking, rinse again with clean water;
[0056] Cocoons are pulled out and the silk is added. The cocoons are stretched individually to remove the cocoon cakes and black moles. The thickness of the silk is even and the layers are aligned. The silk is added one by one without breaking the silk to ensure uniform stretching and make silk cotton bags.
[0057] Sponge expansion: put the prepared silk cotton bag on the stretching equipment. During the sponge expansion process, it needs to be expanded in water, where the water temperature does not exceed 60°C, and the sponge expansion is carried out by bidirectional parallel stretching;
[0058] Drying: Let the expanded cotton dry naturally and set aside;
[0059] Spreading cotton: Spread the dried cotton manually, and use the method of layer-by-layer overlapping and cross-crossing to form a mesh-shaped cotton quilt. According to the different weights of the silk quilt, a silk quilt needs to be spread with thousands of layers of cotton. In this process, it is stretched according to different size requirements;
[0060] Edge locking: Use a batten board to press the edge of the silk quilt onto the operating platform along the edge of the quilt, use a retaining spring to clamp the batten board to fix the silk and prevent it from moving, and use an electric edge locking machine to rotate and lock the edge of the silk quilt pressed by the batten board.
[0061] The cocoon boiling was repeated twice, and the cocoon boiling time was 30 minutes.
[0062] During the rinsing process, the amount of edible white vinegar and water used is 20 ml of edible white vinegar and 10 L of water for soaking 1 kg of silkworm cocoons.
[0063] Example 3
[0064] See also Figures 1 to 3 , the present invention provides a technical solution:
[0065] A pure handmade silk cotton long fiber whole stretch quilt making process, including cocoon selection, cocoon boiling, rinsing, cocoon picking and cotton application, cotton expansion, drying, cotton spreading and edge locking;
[0066] Select cocoons, select double palace cocoons with silk length of more than 1200m, and the cocoons are used as raw materials. The selected cocoons are put into dry preservation bags and placed at room temperature for use;
[0067] For cocoon boiling, edible alkali and purified water are first mixed in a weight ratio of 2:100, and the pH value is controlled at 8-11. Two portions of the mixed water are placed at room temperature for standby; one portion of the mixed water is used to boil the cocoons for no less than 30 minutes, during which constant temperature control is performed, the cocoons are intermittently rolled and stirred, and the temperature is controlled at 100°C; the other portion of the mixed water is heated to 70°C, and the cocoons are placed in the mixed water for 15-30 minutes for temperature difference penetration; finally, the cocoon boiling process is repeated on the infiltrated cocoons; the number of repetitions is adjusted according to the temperature, and the purpose of cocoon layer penetration is finally achieved; during this period, the external temperature is a factor that determines the number of cocoon boiling times, wherein the temperature is between 0-18°C for at least 4 times, between 18-26°C for 2-3 times, and above 26°C for 1-2 times. The whole process takes more than 3 hours, because boiling the cocoons is very important, which can not only remove the cocoons and add cotton, but also avoid damaging the cocoon silk. Maintaining the strength of the cocoon silk is very important for the service life of the cotton and silk quilt.
[0068] Rinse, first rinse the cocoons with clean water to ensure that the residual liquid is clear; soak the rinsed cocoons in a mixture of edible white vinegar and pure water for 3-4 times, wherein the amount of edible white vinegar and water is 30 ml of edible white vinegar and 10 L of water for 1 kg of cocoons, and the pH value is controlled at 7. After soaking, rinse again with clean water;
[0069] Cocoons are pulled out and the silk is added. The cocoons are stretched individually to remove the cocoon cakes and black moles. The thickness of the silk is even and the layers are aligned. The silk is added one by one without breaking the silk to ensure uniform stretching and make silk cotton bags.
[0070] Sponge expansion: put the prepared silk cotton bag on the stretching equipment. During the sponge expansion process, it needs to be expanded in water, where the water temperature does not exceed 60°C, and the sponge expansion is carried out by bidirectional parallel stretching;
[0071] Drying: Let the expanded cotton dry naturally and set aside;
[0072] Spreading cotton: Spread the dried cotton manually, and use the method of layer-by-layer overlapping and cross-crossing to form a mesh-shaped cotton quilt. According to the different weights of the silk quilt, a silk quilt needs to be spread with thousands of layers of cotton. In this process, it is stretched according to different size requirements;
[0073] Edge locking: Use a batten board to press the edge of the silk quilt onto the operating platform along the edge of the quilt, use a retaining spring to clamp the batten board to fix the silk and prevent it from moving, and use an electric edge locking machine to rotate and lock the edge of the silk quilt pressed by the batten board.
[0074] Preferably, the cocoon boiling is repeated twice and the cocoon boiling time is 30 minutes.
[0075] Preferably, during the rinsing process, the amount of edible white vinegar and water used is in the ratio of 20 ml of edible white vinegar to 10 L of water for soaking 1 kg of silkworm cocoons.
[0076] The equipment used in Examples 2 and 3 is the same as that in Example 1.
[0077] The pure handmade silk cotton long fiber stretching quilt making process of the present invention can be carried out in a pure handmade manner during use, and the produced pure handmade silk quilt does not need to be spliced, has uniform thickness, and is not easy to be dislocated and deformed; at the same time, during use, the silk quilt produced by the present invention is soaked in edible white vinegar for cocoon removal and cotton application, which can effectively prevent the silk quilt from easily generating static electricity, and solves the defects of silk quilts in the prior art; furthermore, the pure handmade stretching can make the silk quilt fluffy when used, and has more elasticity than the silk quilt formed by splicing.
[0078] Since silk is made of long fiber material, during the expansion process, as the expansion area increases, the resistance encountered becomes stronger. The silk cotton long fiber whole sheet stretching equipment proposed in the present invention is just to solve this problem. It expands the cotton mechanically to prevent the technical defects of uneven manpower or the use of splicing to expand the cotton unable to be achieved, provides a more complete whole sheet expansion technology, and improves the silk quilt production process.
[0079] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A whole-sheet stretching device for silk floss filaments, characterized in that: The invention comprises a sponge expansion area (3), a control area (13) and an adjustment bracket. The control area (13) and the adjustment bracket are arranged in sequence below the sponge expansion area (3). The sponge expansion area (3) and the control area (13) are respectively provided with a water inlet pipe (10) and a water outlet pipe (6). The sponge expansion area (3) is provided with a water inlet (17), a water outlet (16) and a sponge expansion unit. The control area (13) is provided with a constant temperature return water unit and a power output device (11). The constant temperature return water unit is connected to the bottom of the sponge expansion area (3). The constant temperature return water unit is connected to the water outlet pipe (6). A water outlet valve (5) is arranged above the water outlet pipe (6); the constant temperature water return unit comprises a water return pipe (7); a water return valve (9), a water return pump (8) and a heating device (4) are arranged on the water return pipe (7) in order according to the water flow direction; the power output device (11) is connected to the cotton expansion unit circuit; the cotton expansion unit comprises a guide rail (15) and a pull rod holder (18); the pull rod holder (18) is slidably arranged above the guide rail (15); a pull rod is installed between the pull rod holder (18); and a fixing bracket (12) is arranged below the power output device (11); The pull rod fixer (18) includes an adjusting fixing member (18d), and the left and right ends of the adjusting fixing member (18d) are respectively provided with adjusting rods (18c), and the two ends of the adjusting rod (18c) are respectively connected to the adjusting fixing member (18d) and the roller (18b), and the upper and lower ends of the adjusting fixing member (18d) are respectively provided with a telescopic adjustment key (18h) and a telescopic rod (18e), and the end of the telescopic rod (18e) is provided with a fixed bin (18g), and a fixed rod (18f) is provided through the fixed bin (18g); the roller (18b) is provided on both sides of the guide rail (15), and the roller (18b) and the guide rail (15) are slidably matched.
2. The whole-sheet stretching device for silk floss filaments according to claim 1, characterized in that: The two ends of the constant temperature water return unit are respectively connected to a water inlet (17) and a water outlet (16).
3. The whole-sheet stretching device for silk floss filaments according to claim 1, characterized in that: The two ends of the water return pipe (7) are respectively connected to a water inlet (17) and a water outlet (16).
4. The whole-sheet stretching device for silk floss filaments according to claim 1, characterized in that: A thermometer (1) and a liquid level gauge (2) are also provided on the sponge expansion area (3), and a heating device (4) is provided at the bottom of the sponge expansion area (3).
5. The whole-sheet stretching device for silk floss filaments according to claim 1, characterized in that: The adjustment bracket is composed of a plurality of support blocks, and the support blocks are provided with adjustment holes (14).
Citation Information
Patent Citations
Whole-piece stretching equipment for pure manual silk quilt
CN216514651U