Photovoltaic cell and method for manufacturing the same

By using customized POx and Al layers and their cover layer structures in photovoltaic cells, the surface composite problem of photovoltaic cells is solved, the carrier life and charge density are improved, and the battery efficiency is improved.

CN112424951BActive Publication Date: 2024-11-29TECH UNIV EINDHOVEN
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN201980030694.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-03-11
Publication Date
2024-11-29
Estimated Expiration
2039-03-11

AI Technical Summary

Technical Problem

The surface recombination of existing photovoltaic cells results in the loss of charge carriers, reducing energy conversion efficiency, especially the surface passivation effect of n-type semiconductors, making it difficult to effectively reduce surface recombination.

Method used

Using a POx layer containing phosphorus, aluminum and oxygen as the passivation layer stack, a photovoltaic cell structure with excellent passivation effect is formed by customizing the atomic ratio of phosphorus to aluminum and applying a cover layer, including deposition of POx on a silicon substrate and A layer of Al and a cover structure is applied to its top to improve stability and passivation effect.

Benefits of technology

It realizes effective reduction of surface recombination in photovoltaic cells, improves carrier life and fixed charge density, reduces interface state density, and improves battery efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112424951B_ABST
    Figure CN112424951B_ABST
Patent Text Reader

Abstract

A photovoltaic cell is disclosed comprising a silicon substrate having two opposing main surfaces, wherein a first main surface of the two main surfaces is covered by a passivation layer stack, the passivation layer stack comprising a PO-containing layer covering the first main surface. x and Al layer and covers the PO x A method for manufacturing a photovoltaic cell is also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to photovoltaic cells and to a method for manufacturing a photovoltaic cell. Background Art

[0002] Photovoltaic cells having a passivation layer are known, for example, from WO 2016022026 A1. Summary of the invention

[0003] The limiting factor of the performance of silicon-based photovoltaic cells (hereinafter also referred to as solar cells) is the recombination of charge carriers at the surface due to the presence of surface states that promote such recombination. Such surface recombination is a problem for solar cells because the charge carriers that recombine at the surface are lost and cannot contribute to the collector current, thereby reducing the energy conversion efficiency. In order to reduce surface recombination, it is necessary to passivate the surface so that the recombination activity of the surface states is suppressed. This is usually achieved by depositing or growing a thin film layer or stack of dielectric or other materials on the semiconductor surface, so that the density of surface states at the interface between the semiconductor and the layer or stack is reduced. Typically, the layer or stack also induces band bending at the semiconductor surface, so that the surface concentration of one type of charge carrier (electron or hole) is reduced. This will also reduce surface recombination because recombination requires the presence of two types of carriers.

[0004] Currently, a large number of materials are known to be effective for passivation of semiconductor surfaces. These materials include silicon oxide, silicon nitride, amorphous silicon, aluminum oxide, aluminum nitride, hafnium oxide, gallium oxide, titanium oxide and tantalum oxide. Sometimes these materials are combined into stacks.

[0005] Most of these materials experience upward band bending (hole accumulation) at the semiconductor surface due to the fact that they contain negative charge states in the bulk or near the semiconductor interface (see Figure 1 ). This is beneficial for the passivation of p-type semiconductor surfaces, but detrimental for the passivation of n-type semiconductor surfaces. This is because on n-type surfaces, such upward band bending leads to the formation of an inversion layer at the surface, which promotes the lateral transport of minority carriers to high recombination regions (e.g., edges), which may lead to shunting. On heavily doped n-type surfaces, upward band bending may even increase rather than reduce surface recombination, because the induced band bending is not sufficient to produce a complete inversion of the surface charge, but only leads to depletion or weak inversion of the semiconductor surface.

[0006] Known passivation materials that induce downward band bending (electron accumulation) at the semiconductor surface and are therefore beneficial for the passivation of n-type surfaces include silicon oxide and silicon nitride, due to the fact that both contain positive charge states. However, the former contains only a relatively low concentration of charge states (typically <5×10 11 cm-2 ), making the contribution of the induced band bending to reducing surface recombination quite small. Silicon nitride can have a larger charge concentration (>5×10 12 cm -2 [Hezel 1989]), however, the charge concentration in passivated silicon nitride films (also characterized by low interface state density) is typically slightly smaller, about 5 × 10 11 cm -2 Up to 2×10 12 cm -2 [Hezel 1989, Schuurmans 1996, Aberle 1999, Dauwe 2002, Wan2013].

[0007] This is significantly less than the charge concentration observed for the best passivating negative charge material, alumina, which typically has a charge concentration of 2-10×10 12 cm -2 Therefore, there is a gap between the availability of passivation materials with strong negative charge and those with strong positive charge.

[0008] A second important function of thin film materials in semiconductor device fabrication is as a source of dopants for forming highly doped surface regions in semiconductor substrates. This has been demonstrated, for example, using the deposition of silicon oxides doped with phosphorus and boron, and for growing phosphosilicate and borosilicate glasses on silicon during standard diffusion processes. This can be accomplished by heating the sample surface to high temperatures (either across the entire surface, such as in a combustion furnace, or using, for example, laser-induced heating ( Figure 2 ) and only local heating) to initiate diffusion of dopant species into the semiconductor substrate. A particularly advantageous situation occurs when such a thin film dopant source also functions as a surface passivation layer. This is the case of aluminum oxide, which both provides effective passivation of p-type surfaces due to its large negative charge and has also been shown to function as a dopant source for aluminum doping of silicon via laser doping. This situation is advantageous because it allows the formation of localized diffusion contact areas that are self-aligned with the surrounding passivation layer, thereby simplifying processing.

[0009] Aluminum and phosphorus are located on either side of silicon in the periodic table. In silicon, aluminum is a p-type dopant, while phosphorus is an n-type dopant. Aluminum oxide (Al2O3) films are known to have a large negative fixed charge concentration when deposited on silicon. Stoichiometric aluminum phosphate (AlPO4) can be considered isoelectronic with silicon oxide (SiO2), characterized by a small positive charge concentration at its interface with silicon.

[0010] The invention relates to a photovoltaic cell comprising a silicon substrate having two opposite main surfaces, wherein a first of the two main surfaces is covered by a passivation layer stack comprising:

[0011] The first major surface is covered with a PO-containing x and Al layers; and

[0012] Covering PO x and a covering layer structure of an Al layer.

[0013] Containing PO x The layer of Al is a layer comprising phosphorus, aluminum and oxygen, more specifically a layer comprising a mixture of phosphorus, aluminum and oxide. Such a passivation layer stack can be tailored to obtain an effective excess carrier lifetime τ eff (s), fixed charge density Q f (cm -2 ) and interface state density D it (eV -1 cm -2 ) is the best balance between the effective excess carrier lifetime τ eff Relatively long and interface state density D it Relatively low. The desired fixed charge density Q f Depending on the PO x and the doping type of the main surface of the layer of Al, ie, n-silicon or p-silicon.

[0014] For example, containing PO x The layer of Al may have a large positive fixed charge and may provide excellent passivation of the crystalline silicon surface. The silicon at the first main surface of the silicon substrate may be coated with PO x Phosphorus doping in the layer containing PO and Al. This method can form local heavily doped regions, which facilitate the formation of electrical contact with the silicon substrate. The capping layer structure acts as a moisture barrier and is resistant to PO x and Al layers provide chemical stability to the PO x The layer of Al may be unstable with respect to the environment depending on its content.

[0015] In some cases, it appears as a mixed AlP x O y Membrane mixed with PO x In view of this, the present invention also relates to a photovoltaic cell comprising a silicon substrate having two opposite main surfaces, wherein a first main surface of the two main surfaces is covered by a passivation layer stack, the passivation layer stack comprising a PO-containing layer covering the first main surface. x and Al layer, which contains PO x The layer with Al is a mixed AlP x O y Therefore, you can choose PO xThe ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer containing PO and Al (P / (P+Al)) is such that x The layer of phosphorus and aluminum is stable with respect to the outside air. The ratio is therefore the number of atoms of phosphorus divided by the number of atoms of phosphorus plus aluminum.

[0016] The following embodiments are embodiments of both PV-cells with a cover layer and PV-cells without a cover layer. When the PV-cell has no cover layer, it is necessary to contain PO x The Al layer itself is stable with respect to the outside air.

[0017] In a first embodiment, the PO x The layer with Al is a mixed AlP x O y Membrane. Customized PO x The ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer of Al (P / (P+Al)) is used to obtain the effective excess carrier lifetime τ eff (s), fixed charge density Q f (cm -2 ) and interface state density D it (eV -1 cm -2 ) to achieve the best balance between

[0018] As from Figure 9b It is clear that the atomic percentage of phosphorus and phosphorus + aluminum (P / (P+Al)) in the layer has an effect on the fixed charge density (Q f ) has an impact. By tailoring this ratio, the fixed charge density can be changed from negative to positive, in the example, from -12*10 12 cm -2 Up to +14*10 12 cm -2 . Effective excess carrier lifetime τ eff is preferably long, and this can also be obtained by tailoring the ratio between the atomic percentages of phosphorus and phosphorus + aluminum (P / (P+Al)), as obtained from Figure 9a The effective excess carrier lifetime τ can even be improved by forming gas annealing and by applying an Al2O3 capping layer and optionally performing a subsequent annealing. eff Interface state density (D it ) is preferably relatively low, and this can also be achieved by tailoring the PO x The atomic percentage of phosphorus in the layer of phosphorus and Al is achieved by phosphorus + aluminum (P / (P+Al)).

[0019] In an embodiment, the ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer (P / (P+Al)) is 0.6 to 1.0. Within this range, the effective excess carrier lifetime τ eff is relatively large, fixed charge density Q f is positive, and the interface state density D it different and can be relatively small. This will result in a PV-cell with good efficiency.

[0020] In an embodiment, the ratio between the atomic percentage of phosphorus to phosphorus + aluminum in the layer (P / (P+Al)) is at least 0.5.

[0021] In an embodiment, the PO x The layer of Si and Al additionally contains at least one of H, Si, and C.

[0022] For example, H may be beneficial in reducing the interface state density with the silicon substrate.

[0023] Si and additional Al can be used in PO-containing x and Al in the contact region between the layer and the silicon substrate and on the other hand in the PO x The PO-containing layer diffuses into the contact area between the layer containing Al and Al and the cover layer structure containing Al2O3. x and Al layers.

[0024] In the embodiment, the Si substrate is x A thin SiO2 layer may be present between the films (either intentionally or as a byproduct of the deposition process) to minimize the concentration of electrical interface states (D it ).

[0025] In an embodiment, the thin SiO2 layer may have a thickness of 0.5-2 nm.

[0026] In an embodiment, the capping layer structure may be an aluminum oxide (Al2O3) layer. However, it is noted that other materials may also be used for the capping layer structure, in particular other oxides or nitrides (e.g., silicon nitride, titanium oxide, silicon oxide, etc.). The capping layer structure may also be present as a stack of layers, for example, an Al2O3 layer and a SiN x A stack of layers.

[0027] In an embodiment, the PO-containing x The layer of Al may have a thickness of less than 10 nm.

[0028] In an embodiment, the top cover structure comprises an aluminum oxide (Al2O3) layer having a thickness of 2-30 nm, more preferably 2-5 nm.

[0029] In an embodiment, the second main surface of the two main surfaces of the silicon substrate may be covered by an Al2O3 layer.

[0030] The Al2O3 layer provides excellent passivation of the crystalline silicon surface and has a negative fixed charge.

[0031] In embodiments, a photovoltaic cell having an Al2O3 layer on a second major surface may include a SiO2 layer between the second major surface and an aluminum oxide (Al2O3) layer covering the second major surface.

[0032] In an embodiment, the SiO2 layer may have a thickness of 0.5-2 nm.

[0033] In further elaboration of an embodiment having an aluminum oxide (Al2O3) layer covering the second major surface, the Al2O3 layer may include, in order from the second major surface to the top, an Al2O3 layer, an optional SiO2 layer on the top of the Al2O3 layer, and a SiN2 layer on the top thereof. x A portion of a stack of covering layers.

[0034] The present invention also relates to a method for manufacturing a photovoltaic cell, the method comprising:

[0035] providing a silicon substrate having two opposing major surfaces;

[0036] A PO-containing x and Al layers;

[0037] In the presence of PO x A capping layer structure is applied on top of the layer of Al to cover the PO x and Al layers.

[0038] Containing PO x and Al layers passivate the Si and can be tailored to obtain an effective excess carrier lifetime τ eff (s), fixed charge density Q f (cm -2 ) and interface state density D it (eV -1 cm -2 ) is the best balance between the effective excess carrier lifetime τ eff is relatively long and the interface state density D it is relatively low. The desired fixed charge density Q f Depending on the PO x and the doping type of the main surface of the layer of Al, ie, n-silicon or p-silicon.

[0039] As described above with respect to PV-cells, in some cases, a hybrid AlP xO y Membrane mixed with PO x The layer of Al and Al can be stable, and in this case no covering layer needs to be applied. In view of this, the present invention also relates to a method for manufacturing a photovoltaic cell, the method comprising:

[0040] providing a silicon substrate having two opposing major surfaces;

[0041] A PO-containing x and Al layer, which contains PO x The layer with Al is a mixed AlP x O y Therefore, you can choose to contain PO x The ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer containing PO and Al (P / (P+Al)) is such that x The layer of Al is stable with respect to the outside air.

[0042] The following embodiments of the method according to the invention relate both to embodiments of the method for producing a PV-cell with a cover layer and to embodiments of the method for producing a PV-cell without a cover layer. When the PV-cell has no cover layer, it is necessary to x The Al layer itself is stable with respect to the outside air.

[0043] In an embodiment, the PO x The layer with Al is a mixed AlP x O y A membrane formed by:

[0044] Apply a certain amount of PO x layer and a number of Al-containing layers, wherein the customized PO x The ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer of Al (P / (P+Al)) is calculated to obtain the effective excess carrier lifetime τ eff (s), fixed charge density Q f (cm -2 ) and interface state density D it (eV -1 cm -2 ), where customization is achieved by applying the desired amount of PO x layer and the desired number of Al-containing layers to form a mixed AlP x O y Membrane to achieve.

[0045] The desired amount of PO can be applied x layer and the desired number of Al-containing layers (e.g., Al2O3 layers), and the desired amount of Al-containing layers (e.g., Al2O3 layers) is obtained precisely in the PO-containingx In particular, when the layer is formed by ALD (e.g. in a space-based atmospheric system such as sold under the trade name Levitrack), the P / (P+Al) ratio in the layer is 1.5 wt% and 2.5 wt% respectively. x The Al2O3 layer is a single layer and can be precisely defined in the PO x and Al layers.

[0046] In an embodiment, the ratio between the atomic percentages of phosphorus and phosphorus + aluminum (P / (P+Al)) in the layer is from 0.6 to 1.0.

[0047] In an embodiment, the PO x and Al layers can be formed by applying at least one PO x layer and applying at least one Al-containing layer, followed by annealing at least one PO x A stack of layers and at least one Al-containing layer to mix Al and P to obtain a mixed AlP x O y membrane.

[0048] In an embodiment, PO is applied alternately x layer and an Al-containing layer to form a stack of layers. x The alternating stack of layers and Al-containing layers results in a very well mixed AlP x O y membrane.

[0049] In an embodiment, at least one PO is applied x layer and at least one Al-containing layer and subsequently PO x An intermediate annealing step is performed between the layer and the subsequent Al-containing layer in order to mix the at least one PO previously applied x Al and P in the layer and at least one Al-containing layer to obtain a mixed AlP x O y film, in the mixed AlP x O y The subsequent PO x layer and a subsequent Al-containing layer.

[0050] When AlP is formed x O y When multiple annealing is performed during the film formation, a very uniformly mixed AlP x O y membrane.

[0051] In the embodiment, PO is first applied alternately xThe stack of layers is then annealed to mix Al and P to obtain a mixed AlP x O y In this embodiment, after applying the PO x Annealing is performed after all layers of the PO and Al layers. It can be decided whether intermediate annealing is preferred or whether it is preferred to apply the PO x The entire stack of layers and Al-containing layers is then annealed. In space-based atmospheric systems such as those sold under the trade name Levitrack, intermediate annealing is possible with hardly any delay in the formation of the PV-cell.

[0052] In an embodiment, the PO-containing phase can be deposited by pulsed, spatial or batch atomic layer deposition (ALD); or pulsed, spatial or batch chemical vapor deposition (CVD). x A layer of A1 and Al is applied on the first main surface.

[0053] In further elaboration of this embodiment, the pulsed, spatial or batch chemical vapor deposition (CVD) may be pulsed, spatial or batch plasma enhanced chemical vapor deposition (PECVD).

[0054] In an embodiment, for the x The pulsed, spatial or batch atomic layer deposition (ALD) or pulsed, spatial or batch chemical vapor deposition (CVD) of a layer of O and Al applied on the first major surface can be carried out by alternately exposing the surface to trimethyl phosphate (TMP) and an O-containing reactant selected from O2 plasma, H2O, O3 and H2O2; and alternately exposing the surface to trimethylaluminum (TMA) and an O-containing reactant selected from O2 plasma, H2O, O3 and H2O2.

[0055] In an embodiment, the first major surface can be exposed to a purge gas, such as N2, between each exposure to trimethyl phosphate and exposure to the reactant containing O. Thus, the first major surface can also be exposed to a purge gas, such as N2, between each exposure to trimethylaluminum and exposure to the reactant containing O. In an embodiment, pulsed, spatial, or batch atomic layer deposition (ALD) or pulsed, spatial, or batch chemical vapor deposition (CVD) can be performed in an atmospheric ALD or CVD system, such as a spatial atmospheric system sold under the trade name of Levitrack.

[0056] In embodiments, pulsed, spatial, or batch atomic layer deposition (ALD) or pulsed, spatial, or batch chemical vapor deposition (CVD) may be performed in a low pressure deposition system.

[0057] A low pressure deposition system is one in which the pressure is sub-atmospheric.

[0058] In an embodiment, the PO-containing x A layer of A1, A2 and A1 is applied to the first main surface of the silicon substrate.

[0059] In an embodiment, the application of the cover layer structure may include the application of an Al2O3 layer.

[0060] In embodiments, the application of the Al2O3 layer can be carried out with a PO-containing x The application of the Al layer is achieved in the same atmospheric space ALD system and is immediately followed by a PO x and Al layers without removing the substrate from the atmospheric space ALD system, so that the Al2O3 capping layer structure is applied to the PO-containing x Before the Al layer, the PO x The layers of A1 and Al are not exposed to air or moisture.

[0061] In an embodiment, the PO x The application of the Al and Al2O3 layers can be realized in different modules of an ALD, CVD and / or PECVD system, wherein the substrate is exposed to the PO4-containing substrate in an inert atmosphere or in a vacuum. x and Al layer to the module where the Al2O3 layer is applied to avoid the PO x and the Al layer is air exposed.

[0062] In embodiments, application of the Al2O3 capping layer is achieved at a temperature of 20-300°C, more preferably 150-250°C and even more preferably 180-220°C.

[0063] The invention is further described in the detailed description with reference to the following drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] Figure 1 .At a fixed charge Q f and the interface trap density D it A summary of the work on passivation coatings on silicon is provided by Cuevas et al. [Cuevas 2015], to which our PO x / Al2O3 data(D it and Q f The exact value of will depend on the details of the deposition process conditions).

[0065] Figure 2Schematic illustration of the laser doping process from a film containing dopants. The laser pulse locally heats the film, creates local openings in the film and causes the dopant to diffuse into the silicon, forming local heavily doped regions at the surface.

[0066] Figure 3a Image of a silicon surface passivated by Al2O3, a currently known structure for surface passivation. Negative fixed charges in the film repel negatively charged electrons from the interface, resulting in effective passivation especially for p-type surfaces.

[0067] Figure 3b By the suggested PO x Figure 3. Image of a silicon surface passivated by a Si / Al2O3 stack. The positive fixed charges in the film repel positively charged holes from the interface, resulting in effective passivation, especially for n-type surfaces.

[0068] Figure 4a At a temperature of 25°C and a TMP injection time of 500 ms (bubbler temperature 25°C), PO x Film thickness versus deposition process cycle number.

[0069] Figure 4b At 25°C, 500ms, 1s and 2s injection times (bubbler temperature 25°C), PO x Film thickness versus cycle number.

[0070] Figure 4c Steady state GPC versus TMP injection time at 25°C (bubbler temperature 25°C).

[0071] Figure 4d At deposition temperatures of 25°C, 100°C, and 200°C and bubbler temperatures of 25°C and 70°C, PO x Film thickness versus cycle number.

[0072] Figure 5 PO deposited on polished (100)Si substrate at 100°C x Relative atomic composition of the / Al2O3 stacks determined by XPS versus sputtering time.

[0073] Figure 6a The PO deposited at 25°C x / Al2O3 stacks and the same Al2O3 film but without PO x Effective excess carrier lifetime τ of passivated n-type Si(100) eff (Δn=10 15 cm -3 ) relative to the annealing temperature. Annealing was performed continuously for 10 minutes at each temperature in N2.

[0074] Figure 6b The PO deposited at 100°C x / Al2O3 stacks and the same Al2O3 film but without PO x Effective excess carrier lifetime τ of passivated n-type Si(100) eff (Δn=10 15 cm -3 ) relative to the annealing temperature. Annealing was performed continuously for 10 minutes at each temperature in N2.

[0075] Figure 7a The PO deposited at 25°C x Effective excess carrier lifetime τ of n-type FZ Si(100) wafers passivated by / Al2O3 stacks eff Relative to the excess carrier concentration Δn as a function of the cumulative annealing temperature. The dashed line shows the intrinsic Si lifetime τ int As parameterized by Richter et al. [Richter 2012].

[0076] Figure 7b The PO deposited at 100°C x Effective excess carrier lifetime τ of n-type FZ Si(100) wafers passivated by / Al2O3 stacks eff Relative to the excess carrier concentration Δn as a function of the cumulative annealing temperature. The dashed line shows the intrinsic Si lifetime τ int As parameterized by Richter et al. [Richter 2012].

[0077] Figure 8a PO deposited on silicon at 100 °C x / Al2O3 stacks and the same Al2O3 film but without PO x High frequency capacitance-voltage curves were measured where the samples were annealed in N2 at various temperatures for 10 min prior to metallization.

[0078] Figure 8b Depend on Figure 8a The corresponding fixed charge density determined from the data as a function of annealing temperature.

[0079] Figure 9a Effective excess carrier lifetime τ eff Relative to the ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer (P / (P+Al)).

[0080] Figure 9b Fixed charge density Q f Relative to the ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer (P / (P+Al)).

[0081] Fig.9c Interface state density D it Relative to the ratio between the atomic percentage of phosphorus and (phosphorus + aluminum) in the layer (P / (P+Al)). DETAILED DESCRIPTION

[0082] PO 4 was deposited on the main surface of the silicon substrate by exposing the sample alternately to trimethyl phosphate (TMP) and O 2 plasma reactants and a separate N 2 purge in a cyclic manner at temperatures ranging from 25°C to 100°C in an atomic layer deposition (ALD) reactor. x The process produces linear film growth after an initial nucleation delay, and depending on the temperature and TMP exposure time, the growth per cycle (GPC) is to (At least at a deposition temperature of 25°C, no saturation of the GPC relative to the precursor injection was observed, so that this process should be considered a pulsed chemical vapor deposition method rather than a true ALD.) Note that other phosphorus-containing precursors and other reactants (e.g., H2O, O3, H2O2) can potentially be used in place of TMP and O2 plasma to deposit PO in a similar manner. x Other deposition methods can also be used instead of ALD to deposit PO x Layers are deposited by, for example, chemical vapor deposition, evaporation, sputtering or solution-based methods.

[0083] In PO x Immediately after deposition, an Al2O3 capping layer was deposited in situ using trimethylaluminum (TMA) and O2 plasma at the same temperature. In principle, the Al2O3 film can also be deposited using other precursors or reactants or by other deposition methods. The Al2O3 capping layer can also be replaced by other materials with suitable moisture barrier properties (e.g., silicon nitride or titanium oxide).

[0084] At low pressure (~10 -6 The deposition of the passivation stack is carried out in a deposition system with a base pressure of 100 to 100°. Alternatively, the stack can also be deposited in an atmospheric ALD or CVD system such as, for example, the Levitrack tool currently sold for Al2O3 deposition. x The films were observed to deteriorate significantly within minutes after exposure to the atmosphere, with the formation of fractal crack patterns and blisters, presumably due to atmospheric moisture. x The films are stable to atmospheric exposure over weeks and months. xFilms (~5-10 nm) were observed to gradually form bubbles in the as-deposited state. Annealing the stack in N2 at 200°C for 1 minute immediately after deposition produced improved stability and bubble-free films. PO4 thicker than 10 nm and covered with Al2O3 x The film showed obvious cracking within minutes of exposure to the atmosphere and obvious blistering upon annealing. x The film thickness is preferably kept below 10 nm.

[0085] In order to avoid the rather reactive PO x Air exposure of the film can be performed in an integrated process flow in a spatial ALD system (e.g., Levitrack tool). x / Al2O3 stack deposition. In such a system, different precursors can be injected at different points along a track that is heated to different temperatures. In this method, two processes can be performed at different temperatures, for example, PO at 100°C x and AlO at 200°C x , without being exposed to air.

[0086] PO x X-ray photoelectron spectroscopy (XPS) compositional depth profiling of / Al2O3 stacks (using sputtering) ( Figure 5 ) shows that there is a PO-containing layer under the Al2O3 cover layer. x and Al layers, i.e., AlP x O y There is also a thin silicon oxide (SiO x ) layer, which is likely formed during the initial deposition cycle on the PO x Formed by O2 plasma exposure while still nucleating. Carbon concentration throughout the stack is below the detection limit (<1%).

[0087] To investigate the passivation properties of these layers, PO4 layers with a thickness of 5-6 nm were deposited from trimethyl phosphate (TMP) using an O2 plasma reactant at temperatures ranging from 25°C to 100°C in an atomic layer deposition (ALD) reactor. x At the same temperature, a ~15 nm thick Al2O3 capping layer was deposited in situ using trimethylaluminum (TMA) and O2 plasma. x A symmetric carrier lifetime test structure was fabricated on a 280 μm thick double-sided polished float tape (100) 1-5 Ω cm n-type Si wafer and immediately exposed to PO x / Al2O3 or Al2O3 received standard RCA cleaning and HF soaking before deposition. After deposition, the samples were annealed in N2 for 10 minutes at a series of increasing temperatures. Carrier lifetime measurements were performed using a Sinton WCT-120TS photoconductive lifetime tester.

[0088] Figure 6 shows that the x The measured effective excess carrier lifetime τ of the samples passivated with Al2O3 or the samples passivated with Al2O3 alone eff As a function of post-deposition annealing temperature, two points become immediately clear. First, PO x / Al2O3 provides an excellent degree of surface passivation that is comparable or better than plasma ALD Al2O3 films deposited at the same temperature, with peak lifetimes of 1.9 ms and 5.2 ms for stacks deposited at 25°C and 100°C, respectively (note that these temperatures are not optimal for Al2O3 passivation). x The dependence of the passivation quality of the / Al2O3 stack on the annealing temperature is fundamentally different. In particular, a clear increase in the lifetime is observed at significantly lower annealing temperatures, with lifetimes of the order of 1 ms already observed after annealing at 250°C for 10 minutes. The second point clearly shows that the passivation quality of the / Al2O3 stack is significantly different from that of the PO4 stack. x The passivation provided by the Si / Al2O3 stack is not simply due to the Al2O3 capping layer, but rather to the fundamentally different interfaces formed by these two materials with c-Si. The passivation of films deposited at 25°C was already observed to deteriorate when annealed at 400°C, but the lifetime of films deposited at 100°C only degraded at 550°C.

[0089] A careful examination of the implant-dependent lifetime data (Figure 7) reveals some additional differences between films deposited at 25°C and 100°C. The lifetime of the sample passivated at 25°C after annealing at 250°C is well described by a single-diode model, with a saturation current density J0 of 44 fA / cm per side. 2 , indicating that the surface is strongly accumulated or reversed due to the charge in the dielectric stack. After annealing at higher temperatures, the lifetime increases synchronously at high injection and decreases at low injection, such that the surface recombination can no longer be properly parameterized by J0. In contrast, the stack deposited at 100°C exhibits single diode behavior over a wider temperature range, with an unusually low J0 of ~6 fA / cm per side observed after annealing at 450°C. 2. It is thus shown that a deposition temperature of 100°C is preferred. These differences in injection dependence can be related to differences in the amount of fixed charge. Interestingly, the stacks deposited at both temperatures show similarly high lifetimes at high injection, and the corresponding 1-Sun indicates an open circuit voltage of ˜725 mV. These represent unusually high values ​​and show a significant passivation potential for such stacks.

[0090] Use high frequency (1MHz) capacitance-voltage measurements to determine PO x / Fixed charge concentration Q of Al2O3 stack f (Figure 8). It was found that PO deposited at 100°C and annealed at 250-400°C x The positive fixed charge of the Al2O3 stack is 4×10 12 cm -2 to 4.6×10 12 cm -2 , with the same Al2O3 film but without PO x About 2×10 12 cm -2 This charge ratio is usually used to passivate n-type silicon surfaces. x ) films are significantly larger. Capacitance-voltage measurements also indicate that the investigated PO x / Al2O3 stacks are characterized by a very low interface state density (D it ), which is comparable to or lower than the interface state density of Al2O3 and higher than that of SiN x The interface state density is significantly lower, which together with the large fixed charge explains the excellent passivation of these stacks. This is probably due to the formation of well-controlled SiO x Interface and efficient hydrogenation.

[0091] Figure 9a The effective excess carrier lifetime τ eff With respect to the ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer (P / (P+Al)). As is clear from the figure, the effective excess carrier lifetime is high when the P / (P+Al) ratio is 0-0.15 and 0.7-1.0. Forming gas annealing and applying an Al2O3 capping layer improve the excess carrier lifetime, so that good effective excess carrier lifetime values ​​can be obtained even along the entire ratio range.

[0092] Figure 9b Shows a fixed charge density Q f (cm -2) relative to the ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer (P / (P+Al)). As is clear from the figure, the fixed charge density can be tailored from negative to positive as desired by changing the ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer (P / (P+Al)). In the range of 0.6-1.0, the fixed charge density is 14 to 2. In this range of 0.6-1.0, good fixed charge density values ​​can be obtained and at the same time very low interface state density can also be obtained, which is advantageous.

[0093] Fig.9c The interface state density D it (eV -1 cm -2 ) relative to the ratio between the atomic percentages of phosphorus and (phosphorus + aluminum) in the layer (P / (P+Al)). When the ratio between the atomic percentages of phosphorus and phosphorus + aluminum in the layer (P / (P+Al)) is 0.6-1.0, a low interface state density and a relatively high positive fixed charge density can be obtained.

[0094] The invention is not limited to the embodiments described in the detailed description.

[0095] References

[0096] [Hezel 1989]:Hezel,R.,and K.Jaeger."Low-temperature surfacepassivation of silicon for solar cells."Journal of the ElectrochemicalSociety 136,no.2(1989):518-523.DOI:10.1149 / 1.2096673

[0097] [Schuurmans 1996]: Schuurmans, FM, A. Schonecker, JAEikelboom, and W.C. Sinke. "Crystal-orientation dependence of surface recombination velocity for silicon nitride passivated silicon wafers." In Photovoltaic Specialists Conference, 1996., Conference Record of the Twenty Fifth IEEE, pp. 485-488. IEEE, 1996.

[0098] DOI:10.1109 / PVSC.1996.564049

[0099] [Alerbe 1999]:Aberle,Armin G.Crystalline silicon solar cells:advancedsurface passivation and analysis.Centre for PhotovoltaicEngineering.University of New South wales,1999.

[0100] [Dauwe 2002]:Dauwe,Stefan,Jan Schmidt,Axel Metz,and Rudolf Hezel."Fixed charge density in silicon nitride films on crystalline silicon surfacesunder illumination."In Photovoltaic Specialists Conference,2002.ConferenceRecord of the Twenty-Ninth IEEE,pp.162-165.IEEE,2002.

[0101] DOI:10.1109 / PVSC.2002.1190481

[0102] [Wan 2013]:Wan,Yimao,Keith R.McIntosh,and Andrew F.Thomson."Characterisation and optimisation of PECVD SiNx as an antireflection coatingand passivation layer for silicon solar cells."AIP Advances 3,no.3(2013):032113.DOI:10.1063 / 1.4795108

[0103] [Richter 2012]:A.Richter,S.W.Glunz,F.Werner,J.Schmidt,and A.Cuevas,“Improved quantitative description of Auger recombination in crystallinesilicon,”Phys.Rev.B vol.86,no.165202,2012

[0104] [Cuevas 2015]Cuevas,Andres,Thomas Allen,James Bullock,Yimao Wan,andXinyu Zhang."Skin care for healthy silicon solar cells."In PhotovoltaicSpecialist Conference(PVSC),2015 IEEE 42nd,pp.1-6.IEEE,2015。

[0105] DOI:10.1109 / PVSC.2015.7356379。

Claims

1. A photovoltaic cell comprising a silicon substrate having two opposite main surfaces, wherein a first main surface of the two main surfaces is covered by a passivation layer stack, the passivation layer stack comprising: - a PO-containing x and Al layers; as well as - Cover the PO x and the capping structure of the Al layer, The ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer (P / (P+Al)) is 0.6 to 1.

0.

2. The photovoltaic cell according to claim 1, wherein the PO x The layer with Al is a mixed AlP x O y membrane, wherein the customized PO x The ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer of Al (P / (P+Al)) is used to obtain the effective excess carrier lifetime τ eff (s), fixed charge density Q f (cm -2 ) and interface state density D it (eV -1 cm -2 ) to achieve the best balance between 3. The photovoltaic cell according to any one of claims 1 to 2, wherein the PO-containing x The layer of Si and Al additionally contains at least one of H, Si, and C.

4. The photovoltaic cell according to claim 1, comprising: - on the first main surface and the PO x and SiO2 layer between the Al layers. 5 . The photovoltaic cell according to claim 4 , wherein the SiO 2 layer is a layer having a thickness of 0.5 nm to 2 nm. The photovoltaic cell of claim 1 , wherein the capping layer structure comprises an aluminum oxide Al 2 O 3 layer.

7. The photovoltaic cell of claim 1, wherein the superstrate structure comprises a stack of layers.

8. The photovoltaic cell according to claim 1, wherein the cover layer structure comprises an Al2O3 layer and a SiN x A stack of layers.

9. The photovoltaic cell according to claim 1, wherein the cover layer structure comprises a selected from SiN x 、TiO x 、SiO x layer.

10. The photovoltaic cell according to claim 1, wherein the PO-containing x The layer of Al has a thickness of less than 10 nm.

11. The photovoltaic cell of claim 1, wherein the capping layer structure is an aluminum oxide Al2O3 layer having a thickness of 2 nm to 30 nm. 12 . The photovoltaic cell of claim 1 , wherein the capping layer structure is an aluminum oxide Al 2 O 3 layer having a thickness of 2 nm to 5 nm.

13. The photovoltaic cell according to claim 1, wherein the second of the two main surfaces is covered by an aluminum oxide Al2O3 layer.

14. The photovoltaic cell according to claim 13, comprising: - a SiO 2 layer between the second main surface and the aluminum oxide Al 2 O 3 layer covering the second main surface.

15. The photovoltaic cell according to claim 14, wherein the SiO2 layer is a layer having a thickness of 0.5 nm to 2 nm.

16. The photovoltaic cell of claim 13, wherein the Al2O3 layer is part of a stack, the stack comprising, from the second major surface to the top: Al2O3 layer; an optional SiO2 layer on top of the Al2O3 layer; and SiN x Covering layer.

17. A method for manufacturing a photovoltaic cell, the method comprising: - providing a silicon substrate having two opposing main surfaces; - applying a PO-containing x and Al layers; - In the PO x A capping layer structure is applied on top of the Al layer to cover the PO x and Al layers, The ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer (P / (P+Al)) is 0.6 to 1.

0.

18. The method of claim 17, wherein the PO-containing x The layer with Al is a mixed AlP x O y The mixed AlP x O y The membrane is formed by: Apply a certain amount of PO x layer and a number of Al-containing layers, wherein the PO-containing x The ratio between the atomic percentage of phosphorus and phosphorus + aluminum in the layer of Al (P / (P+Al)) is used to obtain the effective excess carrier lifetime τ eff (s), fixed charge density Q f (cm -2 ) and interface state density D it (eV -1 cm -2 ), where the desired amount of PO x layer and a desired number of Al-containing layers to form the hybrid AlP x O y The customization is achieved by using a membrane.

19. The method according to any one of claims 17 to 18, wherein the PO-containing x and Al layers are formed by applying at least one layer of PO x layer and applying at least one Al-containing layer, and subsequently annealing the at least one PO layer x and the at least one Al-containing layer so as to mix the Al and P to obtain a mixed AlP x O y membrane.

20. The method of claim 17, wherein the PO x layer and the Al-containing layer to form a stack of layers.

21. The method of claim 20, wherein during said applying of at least one layer of PO x layer and at least one Al-containing layer and the subsequent PO x An intermediate annealing step is performed between the layer and the subsequent Al-containing layer in order to mix the at least one previously applied PO layer x The Al and P in the layer and at least one Al-containing layer to obtain a mixed AlP x O y film, in the mixed AlP x O y The subsequent PO x layer and a subsequent Al-containing layer.

22. The method of claim 20, wherein the PO x A layer and an Al-containing layer to form a stack of layers, and then annealing the stack of layers to mix the Al and P to obtain a mixed AlP x O y membrane.

23. The method of claim 17, wherein the PO-containing x and a layer of Al are applied on the first main surface.

24. The method of claim 23, wherein the pulsed, spatial or batch chemical vapor deposition (CVD) is pulsed, spatial or batch plasma enhanced chemical vapor deposition (PECVD).

25. The method according to claim 23 or 24, wherein the PO-containing x The pulsed, spatial or batch atomic layer deposition ALD or the pulsed, spatial or batch chemical vapor deposition CVD applied on the first main surface with a layer of Al and O is carried out by alternately exposing the surface to trimethyl phosphate (TMP) and an O-containing reactant selected from O2 plasma, H2O, O3 and H2O2, and alternately exposing the surface to trimethylaluminum (TMA) and an O-containing reactant selected from O2 plasma, H2O, O3 and H2O2.

26. The method of claim 25, wherein the first major surface is exposed to a purge gas between each exposure to trimethyl phosphate and exposure to the O-containing reactant.

27. The method of claim 25, wherein the first major surface is exposed to a purge gas between each exposure to trimethylaluminum and exposure to the O-containing reactant.

28. The method of claim 23, wherein the pulsed, spatial or batch atomic layer deposition (ALD) or pulsed, spatial or batch chemical vapor deposition (CVD) is performed in an atmospheric ALD or CVD system.

29. The method of any one of claims 26 to 27, wherein the pulsed, spatial or batch atomic layer deposition ALD or pulsed, spatial or batch chemical vapor deposition CVD is performed in a low pressure deposition system.

30. The method of claim 17, wherein the PO-containing x A layer of A1, A2 and A1 is applied on the first main surface of the silicon substrate.

31. The method of claim 17, wherein the PO-containing x A layer of A1, A2 and A1 is applied on the first main surface of the silicon substrate.

32. The method of claim 17, wherein applying the cover layer structure comprises applying an Al2O3 layer.

33. The method of claim 32, wherein the Al2O3 layer is applied on the surface of the PO-containing x The application of the Al layer is achieved in the same atmospheric space-type ALD system and is immediately followed by the PO x and Al layers without removing the substrate from the atmospheric space ALD system, so that when the Al2O3 capping layer is applied to the PO-containing x and Al layers, the PO x The layers of A1 and Al are not exposed to air or moisture.

34. The method of claim 32, wherein the PO-containing x and Al2O3 layer, wherein the substrate is applied in an inert atmosphere or in a vacuum from which the PO-containing x and Al layer to the module where the Al2O3 layer is applied to avoid the PO x and the Al layer is air exposed.

35. The method of claim 32, wherein applying the Al2O3 capping layer is achieved at a temperature of 20°C to 300°C.

36. The method of claim 32, wherein applying the Al2O3 capping layer is accomplished at a temperature of 150°C to 250°C.

37. The method of claim 32, wherein applying the Al2O3 capping layer is accomplished at a temperature of 180°C to 220°C.

Citation Information

Patent Citations

  • A photovoltaic cell with a passivation layer as well as a method for manufacturing such a photovoltaic cell

    WO2016022026A1

  • Precursors for photovoltaic passivation

    CN103000755A

  • Semiconductor device i.e. mono or polycrystalline silicon-based solar cell, for generating current from solar energy, has aluminum oxide passivation layer comprising beryllium, gallium or iron ion layer applied on surface of substrate

    DE102012214442A1

  • Method of deposition of Al2O3 / SiO2 stacks, from aluminium and silicon precursors

    EP2484803A1

  • Surface passivation of high-efficiency crystalline silicon solar cells

    US20150101662A1