A metal contact structure of a two-dimensional semiconductor material and a preparation method thereof
By using a combination of tooth-shaped metal electrodes with edge contacts and top contacts on two-dimensional semiconductor materials, combined with plasma bombardment and in-situ metal deposition technology, the problem of poor metal-two-dimensional material interface performance under traditional contact methods is solved. , achieving the effects of low contact resistance and high switching ratio.
Patent Information
- Application Number
- CN202011282535.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-16
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-11-16
AI Technical Summary
The traditional metal contact method of two-dimensional semiconductor materials makes it difficult to form strong covalent bonds at the metal-two-dimensional material interface, resulting in high contact resistance and poor device performance. In addition, direct metal deposition will damage the crystal lattice of the two-dimensional material and introduce interface state and defect state.
It adopts a structure of substrate, dielectric layer, ordinary metal electrode, tooth-shaped metal electrode and top metal electrode, in which the tooth-shaped metal electrode is in contact with the edge of the two-dimensional semiconductor material, and the top metal electrode is located above the tooth-shaped metal electrode and bombarded by plasma and in-situ metal deposition to prepare source and drain metal electrodes to increase the contact area between metal and two-dimensional semiconductor materials.
It achieves ohmic contact, reduces contact resistance, improves the switching ratio of the device, reduces lattice damage and the generation of interface states, alleviates the charge congestion effect, and improves the electrical performance of the device.
Smart Images

Figure CN112466930B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of semiconductor devices, and in particular relates to a metal contact structure of a two-dimensional semiconductor material and a preparation method thereof. Background Art
[0002] Since the invention of integrated circuits, they have developed rapidly and the technology has been continuously iterating. The characteristic size of devices based on semiconductor silicon has gradually shrunk according to "Moore's Law" to maximize the number of devices per unit area, while reducing the cost of chip production and maintaining the advantages of high performance and low power consumption. However, when the characteristic size of the device is reduced to below sub-10 nanometers, problems such as short channel effects, quantum effects, and reduced switching frequencies become increasingly serious. Two-dimensional semiconductor materials can effectively avoid the above problems. Their good mechanical properties, electrical properties, photoelectric effects and other characteristics are conducive to the preparation of high-performance logic devices, sensors and detectors. The combination with mature silicon-based processes can expand the functions and application scenarios of chips.
[0003] Since the zero bandgap characteristic of graphene limits its application in the field of electronic devices, two-dimensional semiconductor materials have a larger bandgap width range, higher mobility, and effectively overcome the limitation of short channel effect, becoming a research hotspot in academia and industry. Currently, the two-dimensional semiconductor materials obtained by mechanical exfoliation and chemical vapor deposition mainly include MoS2, MoTe2, MoSe2, WSe2 and WS2.
[0004] The traditional method of metal contact of two-dimensional semiconductor materials is to contact the metal with the surface of the two-dimensional material, that is, top contact. However, since there are no dangling bonds on the surface of the two-dimensional material, after the metal is deposited on the surface of the two-dimensional material, it is difficult to form a strong covalent bond at the metal-two-dimensional material interface. Instead, a van der Waals gap is formed at the interface, which is combined by weak van der Waals forces. This van der Waals gap acts as a barrier for electrons / holes, hindering the injection and output of charges, thereby forming a large contact resistance, which is not conducive to improving the performance of the device. In addition, when the metal is directly deposited on the surface of the two-dimensional material, it is easy to damage the lattice of the two-dimensional material, thereby introducing interface states and defect states, resulting in a Fermi level pinning effect, which is not conducive to improving the electrical performance of the device. Summary of the invention
[0005] The purpose of the present invention is to provide a metal contact structure of a two-dimensional semiconductor material and a preparation method thereof, so as to solve the existing technical problems existing in the metal-two-dimensional semiconductor material top contact method mentioned in the background technology.
[0006] The metal contact structure of the two-dimensional semiconductor material provided by the present invention comprises a substrate, a dielectric layer located on the substrate, a common metal electrode, a toothed metal electrode, a top metal electrode and a two-dimensional semiconductor material located on the dielectric layer. The common metal electrode and the toothed metal electrode are connected, the toothed metal electrode contacts the edge of the two-dimensional semiconductor material, and the top metal electrode is located above the toothed metal electrode.
[0007] The method for preparing the metal contact structure of the two-dimensional semiconductor material provided by the present invention comprises the following specific steps:
[0008] (1) forming a dielectric layer on a substrate and preparing a two-dimensional semiconductor material on the surface of the dielectric layer;
[0009] (2) defining source and drain electrode regions on the two-dimensional semiconductor material through a masking layer, wherein the source and drain electrode regions include a common metal electrode region and a toothed metal electrode region;
[0010] (3) etching the source-drain electrode region defined by the masking layer to remove the two-dimensional semiconductor material in the source-drain electrode region;
[0011] (4) using plasma to bombard the edge of the two-dimensional semiconductor material exposed after the etching, and then performing in-situ source and drain metal deposition to prepare source and drain metal electrodes; the source and drain metal electrodes include ordinary metal electrodes and toothed metal electrodes;
[0012] (5) depositing a top metal electrode on the surface of the toothed metal electrode;
[0013] (6) Define a channel and etch away the two-dimensional semiconductor material outside the channel.
[0014] In step (1) of the present invention, the substrate is a commonly used substrate in the art, such as a glass substrate, a sapphire substrate, a quartz substrate, a silicon substrate or any one of flexible substrates.
[0015] In step (1) of the present invention, the preparation method of the two-dimensional semiconductor material is chemical vapor deposition, physical vapor deposition, atomic layer deposition or mechanical exfoliation.
[0016] In step (2) of the present invention, the masking layer is a photoresist or a mask.
[0017] Preferably, the masking layer is patterned by using a photolithography process to pattern the photoresist by exposure, development and the like; or a mask is used to pattern the mask containing the electrode pattern closely against the surface of the two-dimensional semiconductor material.
[0018] In step (4) of the present invention, the plasma bombardment and source / drain metal deposition processes are both completed in a magnetron sputtering chamber in the same vacuum environment.
[0019] Preferably, the plasma bombardment is to bombard the edge of the two-dimensional semiconductor material with plasma generated on the surface of the target in a magnetron sputtering vacuum chamber. The bombardment method is: the high-purity argon gas flow rate is 30 sccm-50 sccm, the sputtering pressure is 0.8 Pa and the sputtering power is 10W-40 W, and the edge of the two-dimensional semiconductor material is bombarded with plasma generated on the surface of the target for 10 seconds to 60 seconds. The distance between the target and the two-dimensional semiconductor material is 5 cm-20 cm.
[0020] In step (5) of the present invention, the method for preparing the top metal electrode is: using a photolithography process or a mask to define the pattern of the top metal electrode, and then using a vacuum evaporation or sputtering coating method to prepare the top metal electrode.
[0021] In step (3) or step (6) of the present invention, the etching method is dry etching commonly used in the art, such as inductively coupled plasma etching, reactive ion etching or ion milling etching.
[0022] Compared with the prior art, the present invention has the following advantages and effects: The present invention provides a metal contact structure of a two-dimensional semiconductor material and a preparation method thereof, so that the metal electrode contacts the two-dimensional semiconductor material through edge contact and partial top contact. Compared with the traditional full top contact method, the configuration of a toothed metal electrode (edge contact) plus a top metal electrode (partial top contact) can reduce the lattice damage and interface state caused by the top contact; at the same time, compared with the linear full edge contact method, the toothed edge contact configuration can increase the contact area between the metal and the edge of the two-dimensional semiconductor material. The method provided by the present invention can increase the contact area between the metal and the two-dimensional semiconductor material from both the edge and the top, thereby alleviating the charge crowding effect existing in the linear full edge contact method. The present invention can enable metal-two-dimensional semiconductor materials to achieve ohmic contact, reduce contact resistance, and improve the switching ratio of the device, and is expected to be used in the production of large-scale integrated circuits in the future. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The diagram is a schematic diagram of the structure of the semiconductor device and the contact method of the present invention, wherein (a) is a top view of the transistor and (b) is a side view of the transistor.
[0024] Figure 2The figure is a schematic diagram of the process of preparing the device and forming the metal contact of the present invention. Among them, (a) is a schematic diagram of the original prepared two-dimensional semiconductor material, (b) is a schematic diagram of the structure of defining the source and drain electrodes with a masking layer, (c) is a schematic diagram of the structure after etching away the two-dimensional semiconductor material below the source and drain electrode area, (d) is a schematic diagram after depositing the source and drain metal electrodes, (e) is a schematic diagram of the structure after depositing the additional top metal electrode, and (f) is a top view of the device structure after defining the channel and etching away the two-dimensional semiconductor material outside the channel.
[0025] Figure 3 It is a schematic diagram of the plasma bombardment treatment of the edge of a two-dimensional semiconductor material and the in-situ source-drain metal deposition method of the present invention.
[0026] Numbers in the figure: 1001 is the substrate, 1002 is the dielectric layer, 2001 is the ordinary metal electrode, 2002 is the toothed metal electrode, 2003 is the top metal electrode, 3001 is the two-dimensional semiconductor material, 4001 is the masking layer, 5001 is the vacuum chamber, 5002 is the rotating tray, 5003 is the target material I, 5004 is the target material II, and 6001 is the sample for defining the source and drain electrodes. DETAILED DESCRIPTION
[0027] Embodiments of the present invention are described in detail below, and the examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals represent the same or similar materials or the methods with the same or similar functions from beginning to end. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention. In order to simplify the disclosure of the present invention, the materials and methods of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the various specific processes and material examples provided by the present invention, but those of ordinary skill in the art can appreciate the applicability of other processes and / or the use of other materials.
[0028] Hereinafter, an example of a metal contact structure of a two-dimensional semiconductor material and a preparation method thereof according to the present invention will be described with reference to the attached drawings.
[0029] According to one embodiment of the present invention, a metal contact structure of a two-dimensional semiconductor material and a method for preparing the same are provided.
[0030] exist Figure 11 shows a semiconductor device and a contact method of the present invention, including a substrate 1001, a dielectric layer 1002 located on the substrate, a common metal electrode 2001, a toothed metal electrode 2002, a top metal electrode 2003, and a two-dimensional semiconductor material 3001 located on the dielectric layer. The common metal electrode 2001 is connected to the toothed metal electrode 2002, the toothed metal electrode 2002 is in contact with the edge of the two-dimensional semiconductor material 3001, and the top metal electrode 2003 is located above the toothed metal electrode 2002.
[0031] exist Figure 2 The process of preparing the device of the present invention and forming the metal contact is shown in FIG. Figure 3 FIG. 2 shows the plasma bombardment treatment of the edge of the two-dimensional semiconductor material 3001 and the in-situ source-drain metal deposition method of the present invention. Figure 2 The steps of device preparation shown in Figure 3 , a specific example is described. The specific steps of preparation are as follows:
[0032] First, if Figure 2 (a), a dielectric layer 1002 is formed on a substrate 1001, and a two-dimensional semiconductor material 3001 is prepared on the surface of the dielectric layer 1002. The substrate 1001 is a commonly used substrate in the art, such as a glass substrate, a sapphire substrate, a quartz substrate, a silicon substrate or any one of flexible substrates, and the preparation method of the two-dimensional semiconductor material 3001 is chemical vapor deposition, physical vapor deposition, atomic layer deposition or mechanical stripping. As a specific example, in this embodiment, heavily doped p-type silicon is selected as the substrate 1001, silicon dioxide is used as the dielectric layer 1002, and the two-dimensional semiconductor material 3001 is prepared by chemical vapor deposition. The two-dimensional semiconductor material 3001 selected in this embodiment is molybdenum disulfide.
[0033] Figure 2 (b) shows a structure in which a source-drain electrode is defined by a masking layer 4001. The source-drain electrode region is defined on the two-dimensional semiconductor material 3001 by the masking layer 4001, and the source-drain electrode region includes a common metal electrode region and a toothed metal electrode region, and the masking layer 4001 is a photoresist or a mask. The masking layer 4001 is patterned by using a photolithography process to pattern the photoresist by means of exposure, development, etc.; or a mask is used to pattern the mask containing the electrode pattern closely against the surface of the two-dimensional semiconductor material 3001. As a specific example, in this embodiment, a photolithography process is selected, and a photoresist is used as the masking layer 4001, and the pattern of the source-drain region is obtained on the surface of the molybdenum disulfide of the two-dimensional semiconductor material 3001 by exposure and development.
[0034] Figure 2(c) shows the structure after etching away the two-dimensional semiconductor material 3001 below the source and drain electrode region. Under the patterned selective protection of the mask layer 4001, the source and drain electrode region defined by the mask layer 4001 is etched to remove the two-dimensional semiconductor material 3001 in the source and drain electrode region. In this embodiment, the inductively coupled plasma etching method is used to etch the two-dimensional semiconductor material 3001 in the source and drain region.
[0035] Figure 3 and Figure 2 (d) shows the plasma bombardment treatment of the edge of the two-dimensional semiconductor material 3001 and the in-situ source-drain metal deposition. The sample 6001 with the source-drain electrode defined after the above steps is placed on the rotating tray 5002 in the vacuum chamber 5001. Under high vacuum conditions, the edge of the two-dimensional semiconductor material 3001 exposed after the above etching is bombarded with the plasma generated by the target material I 5003. Then, without destroying the vacuum, the target material I 5003 and the target material II 5004 are used to perform in-situ source-drain metal deposition to prepare the source-drain metal electrode. The source-drain metal electrode includes a common metal electrode 2001 and a toothed metal electrode 2002. The plasma bombardment and source-drain metal deposition process are completed in the same vacuum environment magnetron sputtering chamber. As a specific example, the target material I 5003 in this embodiment uses a titanium (Ti) target, the target material II 5004 uses a gold (Au) target, and the metal electrode is Ti / Au with a thickness of 5 nm / 30 nm. The plasma bombardment is to bombard the edge of the two-dimensional semiconductor material 3001 with the plasma generated on the surface of the target in the magnetron sputtering vacuum chamber 5001. The bombardment method is: the high-purity argon gas flow rate is 40 sccm, the sputtering pressure is 0.8 Pa and the sputtering power is 20 W, and the edge of the two-dimensional semiconductor material 3001 is bombarded for 30 seconds with the plasma generated on the surface of the titanium target. The distance between the titanium target and the two-dimensional semiconductor material 3001 is 10 cm.
[0036] Figure 2 (e) shows the structure after depositing the additional top metal electrode 2003. The top metal electrode 2003 is deposited on the surface of the toothed metal electrode 2002. The preparation method of the top metal electrode 2003 is: define the pattern of the top metal electrode 2003 by using a photolithography process or a mask, and then use a vacuum evaporation or sputtering coating method to prepare the top metal electrode 2003. As a specific example, in this embodiment, the pattern of the top metal electrode 2003 is defined by a photolithography process, and the top metal electrode 2003 is prepared by a magnetron sputtering method. The top metal electrode 2003 is a 30 nm thick gold electrode.
[0037] Figure 2(f) shows the device structure after the channel is defined and the two-dimensional semiconductor material 3001 outside the channel is etched away. The channel is defined by a photolithography process and the two-dimensional semiconductor material 3001 outside the channel is etched away. The etching method is a dry etching commonly used in the art, such as inductively coupled plasma etching, reactive ion etching or ion milling etching. In this embodiment, inductively coupled plasma etching is used to etch the two-dimensional semiconductor material 3001 outside the channel.
[0038] In the above, a metal contact structure of a two-dimensional semiconductor material and a preparation method thereof are described in detail for the present invention, but the present invention is not limited to the above examples. Various improvements and deformations can of course be made without departing from the gist of the present invention.
Claims
1. A method for preparing a metal contact structure of a two-dimensional semiconductor material, It is characterized in that The metal contact structure comprises a substrate, a dielectric layer located on the substrate, a common metal electrode, a toothed metal electrode, a top metal electrode and a two-dimensional semiconductor material located on the dielectric layer; the common metal electrode and the toothed metal electrode are connected, the toothed metal electrode is in contact with the edge of the two-dimensional semiconductor material, and the top metal electrode is located above the toothed metal electrode; The specific steps of the method are as follows: (1) forming a dielectric layer on a substrate and preparing a two-dimensional semiconductor material on the surface of the dielectric layer; (2) defining source and drain electrode regions on the two-dimensional semiconductor material through a masking layer, wherein the source and drain electrode regions include a common metal electrode region and a toothed metal electrode region; (3) etching the source-drain electrode region defined by the masking layer to remove the two-dimensional semiconductor material in the source-drain electrode region; (4) using plasma to bombard the edge of the two-dimensional semiconductor material exposed after the etching, and then performing in-situ source and drain metal deposition to prepare source and drain metal electrodes; (5) depositing a top metal electrode on the surface of the toothed metal electrode; (6) Define a channel and etch away the two-dimensional semiconductor material outside the channel.
2. The preparation method according to claim 1, It is characterized in that The substrate is any one of a glass substrate, a sapphire substrate, a quartz substrate, a silicon substrate or a flexible substrate.
3. The preparation method according to claim 2, It is characterized in that The preparation method of the two-dimensional semiconductor material is any one of chemical vapor deposition, physical vapor deposition, atomic layer deposition or mechanical stripping.
4. The preparation method according to claim 2, It is characterized in that The masking layer is any one of photoresist and mask.
5. The preparation method according to claim 2 or 4, It is characterized in that The masking layer is patterned by using a photolithography process to pattern the photoresist by exposure and development; or by using a mask to closely attach the mask containing the electrode pattern to the surface of the two-dimensional semiconductor material for patterning.
6. The preparation method according to claim 2, It is characterized in that The plasma bombardment and source / drain metal deposition processes in step (4) are both completed in a magnetron sputtering chamber in the same vacuum environment.
7. The preparation method according to claim 1 or 6, It is characterized in that The plasma bombardment is to bombard the edge of the two-dimensional semiconductor material with the plasma generated on the surface of the target material in the magnetron sputtering vacuum chamber; the bombardment method is: the high-purity argon gas flow rate is 30 sccm-50 sccm, at a sputtering gas pressure of 0.8Pa and a sputtering power of 10W-40W, the edge of the two-dimensional semiconductor material is bombarded with the plasma generated on the surface of the target material for 10 seconds to 60 seconds; the distance between the target material and the two-dimensional semiconductor material is 5 cm-20 cm.
8. The preparation method according to claim 1, It is characterized in that The preparation method of the top metal electrode is: using a photolithography process or a mask to define the pattern of the top metal electrode, and then using a vacuum evaporation or sputtering coating method to prepare the top metal electrode.
9. The preparation method according to claim 1, It is characterized in that In step (3) or step (6), the etching method is any one of inductively coupled plasma etching, reactive ion etching or ion milling etching.
Citation Information
Patent Citations
TFT (thin film transistor) array substrate and manufacturing method therefor, and liquid crystal display apparatus
CN105895638A
Thin film transistor with high effective power
CN106549041A
Thin film transistor and manufacturing method therefor, array substrate and manufacturing method therefor, and display apparatus
CN111670503A
Metal contact structure of two-dimensional semiconductor material
CN213782022U
Semiconductor device
JP2010114171A