Magnetic materials, permanent magnets, rotating electric machines and vehicles

By using Th2Ni17 crystal structure and rare earth element replacement technology in magnet materials, the concentration of M element and the concentration of rare earth elements is improved, and the problem of insufficient saturation magnetization of existing magnet materials is solved, and the development of high-performance permanent magnets is realized. Suitable for a variety of electrical equipment and vehicle applications.

CN112530653BActive Publication Date: 2024-11-08KK TOSHIBA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010106497.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-17
Filing Date
2020-02-21
Publication Date
2024-11-08
Estimated Expiration
2040-02-21

AI Technical Summary

Technical Problem

The saturation magnetization of existing magnet materials is insufficient, making it difficult to meet the needs of high-performance permanent magnets in the fields of miniaturization, high efficiency and high output.

Method used

The magnet material composed of R1-xYx)aMbAc is used, and the main phase has a Th2Ni17 crystal structure. The concentration of M element in the main phase is 89.6 atomic % or more. The portion of the R element is replaced by Y to increase the concentration of rare earth elements and The ratio of M element, combined with the addition of A element, optimizes the crystal structure and electronic structure to enhance magnetic anisotropy and saturation magnetization.

Benefits of technology

It significantly improves the saturation magnetization and refractory force of magnet materials, meets the needs of high-performance permanent magnets, is suitable for rotary motors, generators, vehicles and other fields, achieving high efficiency, miniaturization and low-cost applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112530653B_ABST
    Figure CN112530653B_ABST
Patent Text Reader

Abstract

The present invention improves the saturation magnetization of the magnetic material. The magnetic material is composed of the formula: (R 1‑x Y x ) a M b A c (wherein, R is one or more rare earth elements, M is at least one element selected from the group consisting of Fe and Co, A is at least one element selected from the group consisting of N, C, B, H and P, x is a number satisfying 0.01≤x≤0.8, a is a number satisfying 4≤a≤20 atomic %, b is a number satisfying b=100‑a‑c atomic %, c is a number satisfying 0≤c≤18 atomic %), and it has Th2Ni 17 The concentration of the M element in the main phase is 89.6 atomic % or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present application relate to a magnet material, a permanent magnet, a rotating electrical machine, and a vehicle. Background Art

[0002] Permanent magnets are used in a wide range of products, including rotating electrical machines such as motors and generators, electrical equipment such as speakers and measuring equipment, and vehicles such as automobiles and railway vehicles. In recent years, the above products have been required to be smaller, more efficient, and more powerful, and high-performance permanent magnets with high magnetization and high coercive force have been required.

[0003] Examples of high-performance permanent magnets include rare earth magnets such as Sm-Co magnets and Nd-Fe-B magnets. In these magnets, Fe or Co contributes to the increase of saturation magnetization. In addition, these magnets contain rare earth elements such as Nd or Sm, which result in large magnetic anisotropy due to the behavior of 4f electrons of the rare earth elements in the crystal field. As a result, large coercive force can be obtained.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 8-191006

[0007] Non-patent literature

[0008] Non-patent document 1: D. Givord et al., J. Less-Common Met., 29 (1972) 389.

[0009] Non-patent document 2: D. Givord et al., J. Less-Common Met., 29 (1972) 361. Summary of the invention

[0010] Problems to be solved by the invention

[0011] Improve the saturation magnetization of the magnet material.

[0012] Means for solving problems

[0013] The magnet material of the embodiment has a composition formula: (R 1-x Y x ) a M b A c(wherein, R is one or more rare earth elements, M is at least one element selected from the group consisting of Fe and Co, A is at least one element selected from the group consisting of N, C, B, H and P, x is a number satisfying 0.01≤x≤0.8, a is a number satisfying 4≤a≤20 atomic %, b is a number satisfying b=100-ac atomic %, c is a number satisfying 0≤c≤18 atomic %), and it has Th2Ni 17 The concentration of the M element in the main phase is 89.6 atomic % or more. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a schematic diagram showing the CaCu5-type crystal structure.

[0015] Figure 2 It is a schematic diagram showing the rare earth element sites in the CaCu5-type crystal structure.

[0016] Figure 3 It is used to illustrate Th2Zn 17 Schematic diagram of the crystal structure.

[0017] Figure 4 It is used to illustrate Th2Ni 17 Schematic diagram of the crystal structure.

[0018] Figure 5 It is a schematic diagram showing an example of a permanent magnet motor.

[0019] Figure 6 It is a schematic diagram showing an example of a variable flux motor.

[0020] Figure 7 It is a schematic diagram showing an example of a generator.

[0021] Figure 8 It is a schematic diagram showing an example of a railway vehicle.

[0022] Fig. 9 It is a schematic diagram showing an example of a car.

[0023] Explanation of symbols

[0024] 1 permanent magnet motor, 2 stator, 3 rotor, 4 core, 5 permanent magnet, 11 variable flux motor, 12 stator, 13 rotor, 14 core, 15 fixed magnet, 16 variable magnet, 21 generator, 22 stator, 23 rotor, 24 turbine, 25 shaft, 26 brush, 100 railway vehicle, 101 rotating electrical machine, 200 automobile, 201 rotating electrical machine. DETAILED DESCRIPTION

[0025] The following is an explanation of the embodiments with reference to the accompanying drawings. It should be noted that the accompanying drawings are schematic diagrams, and for example, the relationship between thickness and plane dimensions, the ratio of thickness of each layer, etc., may be different from the actual situation. In addition, in the embodiments, substantially the same components are marked with the same reference numerals and the explanation is omitted.

[0026] (First embodiment)

[0027] The magnetic material of the embodiment includes an R element (R is one or more rare earth elements) and an M element (at least one element selected from the group consisting of Fe and Co). The magnetic material has a metal structure having a main phase. The main phase is the phase with the highest volume occupancy among the crystalline phases and amorphous phases in the magnetic material.

[0028] In order to improve the saturation magnetization of the magnet material, it is effective to increase the concentration of the M element in the main phase. In addition, in order to obtain the large magnetic anisotropy required for the magnet material, it is important that the main phase contains rare earth elements. That is, forming a rare earth compound with a high M element concentration is very important for realizing high-performance permanent magnets.

[0029] The magnet material of this embodiment is obtained by replacing part of R with Y to obtain a composition formula (R 1-x Y x ) a M b A c (wherein, R is one or more rare earth elements, M is at least one element selected from the group consisting of Fe and Co, A is at least one element selected from the group consisting of N, C, B, H and P, x is a number satisfying 0.01≤x≤0.8, a is a number satisfying 4≤a≤20 atomic %, b is a number satisfying b=100-ac atomic %, and c is a number satisfying 0≤c≤18 atomic %). It should be noted that the magnet material may also contain inevitable impurities.

[0030] Furthermore, the magnet material of this embodiment has Th2Ni 17 The main phase of the quartz crystal structure has a concentration of M element of 89.6 atomic % or more. The above-mentioned structure can improve the saturation magnetization of the magnet material. The lower limit of the saturation magnetization is not particularly limited, for example, greater than 1.51T, and more preferably greater than 1.55T.

[0031] The R element is a rare earth element, which brings large magnetic anisotropy to the permanent magnet and gives the permanent magnet a high coercive force. Specifically, the R element is at least one element selected from the group consisting of lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm) and europium (Eu). Pr, Nd, and Sm are preferably used, and Sm is particularly preferred. In the case of using a plurality of elements including Sm as the R element, by setting the Sm concentration to more than 50 atomic % of the total elements applicable as the R element, the performance of the magnet material, such as coercive force, can be improved. The addition amount a of the R element is set to 4 atomic % to 20 atomic %. When it is less than 4 atomic %, the precipitation of the α-Fe phase becomes significant, resulting in a decrease in the coercive force of the permanent magnet. When it exceeds 20 atomic %, the decrease in the saturation magnetization of the permanent magnet becomes significant.

[0032] The magnet material of the embodiment requires yttrium (Y). Y is for Th2Ni 17 The Y element is an effective element for stabilizing the Th2Ni type crystal structure. That is, the Y element mainly replaces the R element in the main phase, and increases the Th2Ni 17 The stability of the type crystal structure. If the amount of Y added is too little, the effect brought by the addition of Y cannot be obtained. If the amount of Y added is too much, the anisotropic magnetic field of the permanent magnet is significantly reduced. The amount of Y added x is preferably a number that satisfies 0.01≤x≤0.8, and particularly preferably a number that satisfies 0.2≤x≤0.4.

[0033] 50 atomic % or less of the Y element may be replaced by at least one element selected from the group consisting of zirconium (Zr) and hafnium (Hf). Zr and Hf are elements effective for stabilizing the crystal phase.

[0034] The M element is at least one element selected from the group consisting of Fe and Co. By changing the ratio of Fe to Co, the saturation magnetization of the permanent magnet can be increased. In addition, by increasing the ratio of Co, the Curie temperature of the permanent magnet increases, thereby suppressing the decrease in saturation magnetization in a high temperature region.

[0035] Less than 20 atomic % of the M element may be replaced by at least one element selected from the group consisting of aluminum (Al), silicon (Si), chromium (Cr), manganese (Mn), nickel (Ni), copper (Cu) and gallium (Ga). The above elements contribute to the growth of grains constituting the main phase, for example.

[0036] In addition, a part of the M element may be replaced by at least one element selected from the group consisting of titanium (Ti), vanadium (V), chromium (Cr), niobium (Nb), tantalum (Ta), molybdenum (Mo) and tungsten (W). 17 The crystal structure is stable.

[0037] Element A is at least one element selected from the group consisting of nitrogen (N), carbon (C), boron (B), hydrogen (H) and phosphorus (P). Element A has the ability to invade Th2Ni 17 The A element has a crystal lattice structure of a type, and generates at least one of the following functions, such as expanding the crystal lattice and changing the electronic structure. This can improve the Curie temperature, magnetic anisotropy, and saturation magnetization. The A element is not necessarily added except for unavoidable impurities.

[0038] The amount c of the element A added is a number satisfying 0≤c≤18 atomic %, preferably 0≤d≤10 atomic %. If the amount of the element A added exceeds 18 atomic %, the saturation magnetization decreases.

[0039] The composition of the magnetic material is measured by, for example, high-frequency inductively coupled plasma-atomic emission spectrometry (ICP-AES), scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX), transmission electron microscope-energy dispersive X-ray spectroscopy (TEM-EDX), scanning transmission electron microscope-energy dispersive X-ray spectroscopy (STEM-EDX), etc. The volume ratio of each phase is comprehensively determined by combining observation with an electron microscope or an optical microscope with X-ray diffraction, etc. In addition, the concentration of the M element in the main phase can be measured by, for example, methods such as SEM-EDX or TEM-EDX.

[0040] As described above, the magnet material of this embodiment has Th2Ni by replacing part of the R element with Y. 17 The main phase of the Th2Ni type crystal structure has a concentration of M element of 89.6 atomic % or more. 17 The crystal phase of the Th2Ni type crystal structure is 17 The main reason for the phase and the ability to have Th2Ni 17 The main reason is that the concentration of the M element in the main phase is set to 89.6 atomic % or more.

[0041] Figure 1 This is a schematic diagram showing the CaCu5-type crystal structure. The intermetallic compound with a composition ratio of R element to M element of 1:5 has Figure 1 The hexagonal crystal structure is called CaCu5 type crystal structure. R2M with a composition ratio of R element to M element of 2:17 17 The compound has a crystal structure similar to the CaCu5 type crystal structure. When one R atom is replaced by two M atoms and the replacement ratio is 1 / 3 of the total number of R atoms, R2M is obtained as follows 17 Compound.

[0042] RM5-1 / 3(R-2M)=R 2 / 3 M (5+2 / 3) =R2M 17

[0043] The two replaced M atoms are arranged in a dumbbell shape along the c-axis, so they are called "dumbbells". 17 There are two types of substitution methods using dumbbells in compounds. Figure 2 It is a schematic diagram showing the R atom site (rare earth element site) of the CaCu5 type crystal structure. Figure 2 In the RM5 crystal lattice, only the R atoms are considered. Figure 2 In the example, the surface obtained by dumbbell replacement of the R atoms at the positions "2" and "5" is called surface A, the surface obtained by dumbbell replacement of the R atoms at the position "3" is called surface B, and the surface obtained by dumbbell replacement of the R atoms at the positions "1" and "4" is called surface C. If stacked with ABCABC... along the c-axis direction, it becomes what is called Th2Zn 17 The crystal structure of rhombohedral crystal type crystal structure. Figure 3 It is used to illustrate Th2Zn 17 Schematic diagram of the crystal structure of the type, each number corresponds to Figure 2 The numbers shown in the figure indicate the positions of the rare earth element sites. On the other hand, if stacked with ABABAB..., it becomes what is called Th2Ni 17 The crystal structure of the hexagonal crystal is of type crystal structure. Figure 4 It is used to illustrate Th2Ni 17 Schematic diagram of the crystal structure of the type, each number corresponds to Figure 2 The numbers shown in indicate the positions of the rare earth element sites.

[0044] When the M element is Fe, there is no RFe5 compound with a CaCu5 type crystal structure, but R2Fe 17 The compound exists for all R elements and has Th2Zn on the light rare earth element side compared to gadolinium (Gd). 17 Type crystal structure, with Th2Ni on the heavy rare earth element side 17 One of the main reasons for the different crystal structures depending on the type of rare earth element is the atomic radius of the rare earth element site. That is, when a light rare earth element with a relatively large atomic radius at the rare earth element site is selected, Th2Zn is easily generated. 17 On the other hand, when a heavy rare earth element with a relatively small atomic radius is selected as the rare earth element site, Th2Ni 17Type crystal structure. For high-performance magnet materials, light rare earth elements such as La, Ce, Pr, Nd, and Sm are mainly used as R elements, but by replacing part of them with Y, which has a smaller atomic radius than these R elements, the average atomic radius of the rare earth element site can be reduced. It is believed that this is because Th2Ni is generated by replacing part of the R element with Y. 17 The main reason for the phase.

[0045] Next, relative to Th2Zn 17 Type crystal structure and Th2Ni 17 The crystal structure of this type is further explained by the structure of the dumbbell. Figure 3 As shown in Th2Zn 17 In the case of a crystalline structure of the type, if the number of dumbbells is further increased, a portion where two dumbbells are connected along the c-axis direction will inevitably be generated. Regarding the portion where two dumbbells are connected along the c-axis direction, for example, when the M element is Fe, the distance between the atoms closest to Fe-Fe is too short, so it is considered to be unfavorable in terms of energy. That is, it is considered that in the case of Th2Zn 17 In the Th2Ni type crystal structure, the composition ratio of the R element to the M element is 2:17 (the concentration of the M element in the compound is 89.5 atomic %), and there is basically no solid solution region on the high iron concentration side. 17 In the case of a type crystal structure, due to Figure 4 As shown in , there are no dumbbells at the "1" and "4" positions, so it is possible to avoid connecting two dumbbells along the c-axis direction by replacing these positions with dumbbells. For example, regarding the crystal structure of LuFez (z = 8.5 to 9.5) using Lu as the R element, Th2Ni 17 The type compound has a solid solution region on the high iron concentration side when the composition ratio of R element to M element is 2:17. This is believed to be the reason for the conversion of Th2Ni 17 This is mainly because the concentration of the M element in the phase increases to 89.6 atomic % or more.

[0046] As described above, the magnet material of this embodiment can generate Th2Ni by mainly using light rare earth elements such as La, Ce, Pr, Nd, Sm, and Eu as the R element and replacing a part of them with Y. 17 phase, the concentration of the M element in the main phase can be increased to 89.6 atomic % or more.

[0047] Th2Ni is generated by using light rare earth elements such as La, Ce, Pr, Nd, Sm, and Eu as the R element and replacing part of them with Zr, Hf, and Sc. 17phase. In contrast, Y is superior to Zr, Hf, and Sc in terms of the effect of substitution with respect to the R element. The main reason for this is that even when Zr, Hf, and Sc are substituted, Th2Ni is generated by reducing the average atomic radius of the rare earth element site. 17 Phase, but because Zr, Hf, Sc are transition metal elements, part of them occupy the M element site. The occupation of the M element site by Zr, Hf, Sc results in a decrease in the concentration of the M element in the compound, and it becomes impossible to increase it to more than 89.6 atomic %. On the other hand, it is believed that although Y has a smaller atomic radius than the R element, it has a larger atomic radius than Zr, Hf, and Sc, so it can avoid occupying the M element site, thereby increasing the concentration of the M element in the main phase to more than 89.6 atomic %.

[0048] When the magnet material contains the A element, the A element has a high affinity with Zr, Hf, and Sc, and is likely to generate nitrides, carbides, borides, and the like that do not contribute to the saturation magnetization of the magnet material, such as ZrN, ZrC, and HfB2, which damage the saturation magnetization of the magnet material. In contrast, the magnet material of this embodiment can suppress the generation of nitrides, carbides, and borides, and allows the A element to penetrate into the Th2Ni 17 The crystal lattice of the phase can improve the magnetic properties such as Curie temperature and magnetic anisotropy without damaging the saturation magnetization.

[0049] Th2Ni 17 For a magnet material having a main phase of a crystalline structure of the type, due to the high concentration of the M element, it is easy to precipitate at least one heterophase selected from the group consisting of the α-Fe phase and the α-(Fe, Co) phase. If the heterophase precipitates, the concentration of the M element in the main phase decreases, resulting in a decrease in the saturation magnetization of the main phase. In addition, the precipitation of the heterophase will lead to a decrease in the coercive force of the permanent magnet. The total amount of the heterophase is preferably, for example, less than 10 volume %.

[0050] Next, an example of a method for manufacturing a permanent magnet using the magnet material of the embodiment is described. First, an ingot alloy containing a predetermined amount of R element, Y, and M element is prepared. The ingot alloy can be obtained, for example, by arc melting, high-frequency induction melting, melt spraying (gas atomization), mold casting, etc.

[0051] In addition to Th2Ni 17 In addition to the phase, many α-(Fe, Co) phases and other heterogeneous phases are precipitated, which sometimes leads to a decrease in saturation magnetization and anisotropic magnetic field. -2 K / sec~1×10 -7The quenching speed is 0.1K / sec, which can reduce the precipitation amount of α-(Fe, Co) phase. As a quenching method, for example, the quenching can be performed at a predetermined speed by a thin strip continuous casting method. By controlling the rotation speed of the roll, the cooling speed of the molten metal can be controlled. The roll can be a single roll type or a double roll type.

[0052] The step of heat treating the ingot alloy or the quenched thin strip obtained in the above step at a temperature of 400°C to 1200°C for 2 hours to 120 hours may also be included. 17 The phase is homogenized, and the two characteristics of saturation magnetization and anisotropic magnetic field are further improved.

[0053] Element A can also be made to infiltrate the ingot alloy or quenched thin strip obtained in the above process. Specifically, when nitrogen is used as element A, nitrogen gas or ammonia gas is used as a nitrogen source, and heat treatment is performed at a temperature of 200°C to 600°C for 1 hour to 24 hours to nitride it. When carbon is used as element A, C2H2 (CH4, C3H8, CO) gas or heated decomposition gas of methanol is used as a carbon source, and heat treatment is performed at a temperature of 300°C to 600°C for 1 hour to 24 hours to carbonize it. In addition, solid carburizing using carbon powder or molten salt carburizing using KCN or NaCN can also be performed. Regarding B, H and P, conventional boriding, hydrogenation and phosphating can be performed. When infiltrating element A, if the ingot alloy or quenched thin strip is crushed in advance to an average particle size of about 10μm to 100μm, element A can be efficiently infiltrated.

[0054] The magnet material is manufactured through the above process. Furthermore, the magnet material is used to manufacture a permanent magnet. For example, a sintered magnet including a sintered body of the magnet material is manufactured by crushing the magnet material and then performing a heat treatment such as sintering. In addition, a bonded magnet including the magnet material is manufactured by crushing the magnet material and curing it with a resin or the like.

[0055] (Second embodiment)

[0056] The permanent magnet using the magnetic material of the first embodiment can be used in various motors or generators. In addition, it can also be used as a fixed magnet or a variable magnet of a variable flux motor or a variable flux generator. By using the above-mentioned permanent magnet, various motors or generators are constructed. In the case where the above-mentioned permanent magnet is applied to a variable flux motor, the technology disclosed in, for example, Japanese Patent Publication No. 2008-29148 or Japanese Patent Publication No. 2008-43172 can be applied to the construction or drive system of the variable flux motor.

[0057] Next, a motor and a generator including permanent magnets will be described with reference to the drawings. Figure 5is a schematic diagram showing a permanent magnet motor. Figure 5 In the permanent magnet motor 1 shown in FIG, a rotor (rotor) 3 is arranged in a stator (stator) 2. A permanent magnet 5 is arranged in the core 4 of the rotor 3. By using the above-mentioned permanent magnets, based on the characteristics of each permanent magnet, etc., it is possible to achieve high efficiency, miniaturization, and low cost of the permanent magnet motor 1.

[0058] Figure 6 is a schematic diagram showing a variable flux motor. Figure 6 In the variable flux motor 11 shown in the figure, a rotor (rotor) 13 is arranged in a stator (stator) 12. In the core 14 of the rotor 13, permanent magnets are arranged as fixed magnets 15 and variable magnets 16. The magnetic flux density (magnetic flux) of the variable magnet 16 can be set to be variable. Since the variable magnet 16 has a magnetization direction orthogonal to the Q-axis direction, it is not affected by the Q-axis current and can be magnetized by the D-axis current. A magnetizing winding (not shown) is provided on the rotor 13. It is a structure in which a current is made to flow from a magnetizing circuit into the magnetizing winding so that its magnetic field directly acts on the variable magnet 16.

[0059] By using the above-mentioned permanent magnet, a coercive force suitable for the fixed magnet 15 can be obtained. When the above-mentioned permanent magnet is applied to the variable magnet 16, the coercive force can be controlled within the range of 100 kA / m to 500 kA / m by changing the manufacturing conditions. Figure 6 In the variable flux motor 11 shown in FIG. 1 , the permanent magnets may be used in either the fixed magnets 15 or the variable magnets 16, or in either one of the magnets. The variable flux motor 11 can output a large torque with a small device size, and is therefore suitable for motors such as hybrid vehicles and electric vehicles that require high output and miniaturization of the motor.

[0060] Figure 7 It is a schematic diagram showing an example of a generator. Figure 7 The generator 21 shown in the figure has a stator (stator) 22 using the above-mentioned permanent magnet. The rotor (rotor) 23 arranged inside the stator (stator) 22 is connected to a turbine 24 provided at one end of the generator 21 via a shaft 25. The turbine 24 is rotated, for example, by a fluid supplied from the outside. It should be noted that, instead of the turbine 24 rotating by the fluid, the shaft 25 may be rotated by dynamic rotation such as the transmission of the regenerative energy of the vehicle. Various known structures can be adopted for the stator 22 and the rotor 23.

[0061] The shaft 25 is in contact with a commutator (not shown) arranged on the opposite side of the turbine 24 relative to the rotor 23, and the electromotive force generated by the rotation of the rotor 23 is boosted to the system voltage via the phase separation bus and the main transformer (not shown) as the output power of the generator 21 and transmitted. The generator 21 can be any of a conventional generator and a variable flux generator. It should be noted that the rotor 23 is charged by the shaft current accompanied by static electricity or power generation from the turbine 24. Therefore, the generator 21 is equipped with a brush 26 for discharging the charge of the rotor 23.

[0062] As described above, by applying the above-mentioned permanent magnets to a generator, effects such as high efficiency, size reduction, and cost reduction can be obtained.

[0063] The above-mentioned rotating electrical machine may be mounted on, for example, a railway vehicle (an example of a vehicle) used in railway transportation. Figure 8 This is a schematic diagram showing an example of a railway vehicle 100 including a rotating electrical machine 101. As the rotating electrical machine 101, the above-mentioned Figure 5 , 6 Motor, Figure 7 When the rotating electric machine 101 is equipped with the rotating electric machine 101, the rotating electric machine 101 can be used as an electric motor (motor) that outputs driving force by using the power supplied from the overhead wire or the power supplied from the secondary battery installed in the railway vehicle 100, or can be used as a generator (generator) that converts kinetic energy into electricity and supplies electricity to various loads in the railway vehicle 100. By using a high-efficiency rotating electric machine such as the rotating electric machine of the embodiment, the railway vehicle can be driven in an energy-saving manner.

[0064] The above-mentioned rotating electric machine may be mounted on an automobile (another example of a vehicle) such as a hybrid automobile or an electric automobile. Fig. 9 2 is a schematic diagram showing an example of a vehicle 200 equipped with a rotating electrical machine 201. As the rotating electrical machine 201, the above-mentioned Figure 5 , 6 Motor, Figure 7 When the rotating electric machine 201 is installed, the rotating electric machine 201 can be used as a motor for outputting the driving force of the automobile 200 or a generator for converting the kinetic energy of the automobile 200 during driving into electric power.

[0065] Example

[0066] (Examples 1 to 18)

[0067] In order to obtain the compositions of Examples 1 to 18 shown in the following Table 1, the raw materials were weighed and ingot alloys were produced by arc melting. Next, using the ingot alloy, a quenched thin strip was produced by a thin strip continuous casting method using a single-roll type liquid quenching solidification device. The roller peripheral speed was set to 2 m / s. The quenched thin strip was heat treated at a temperature of 1100°C for 4 hours in an Ar atmosphere. The heat-treated thin strip was crushed in a mortar, and the crystal structure was analyzed by X-ray diffraction (XRD) measurement using X-rays with CuKα as the ray source. The results confirmed that the main phase in all samples was Th2Ni 17 In addition, it was confirmed that the precipitation amount of the α-(Fe, Co) phase in all samples was less than 10% by volume based on the area ratio of the SEM image.

[0068] The magnetization of the heat-treated ribbon was measured at room temperature using a vibrating sample magnetometer (VSM), and the saturation magnetization Ms was evaluated using the saturation law from the measurement results. The concentration of each element in the main phase was evaluated by SEM-EDX. Specifically, for the heat-treated ribbon, the concentration was measured at 5 points per field of view and at 3 fields of view, so that the concentration of each element was obtained from the average concentration of a total of 15 points. It should be noted that the concentration of the M element is the total concentration of Fe and Co.

[0069] (Comparative Examples 1 and 2)

[0070] Next, in order to obtain the compositions of Comparative Examples 1 and 2 shown in Table 1, raw materials were weighed and alloys were prepared by arc melting. Samples were prepared by the same procedure as Examples 1 to 18 except that the compositions were different. The measurement results of Examples 1 to 18 and Comparative Examples 1 and 2 are shown in Table 1.

[0071] Table 1

[0072]

[0073] As can be seen from Table 1, for example, when the R element is not replaced by Y (Comparative Example 1) and when a part of the R element is replaced by Zr (Comparative Example 2), the concentration of the M element in the main phase is less than 89.6 atomic %, and the saturation magnetization is low. On the other hand, when a part of the R element is replaced by Y (Examples 1 to 18), the concentration of the M element in the main phase is 89.6 atomic % or more, and the saturation magnetization is higher than that of Comparative Examples 1 and 2.

[0074] It should be noted that several embodiments of the present invention have been described, but these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other ways, and various omissions, substitutions, and changes can be made without departing from the scope of the subject matter of the invention. These embodiments and their variations are included in the scope and subject matter of the invention, and are also included in the invention described in the claims and their equivalents.

Claims

1. A magnetic material having a composition formula: (R 1-x Y x ) a M b A c express, In the formula, R is one or more rare earth elements, M is at least one element selected from the group consisting of Fe and Co, A is at least one element selected from the group consisting of N, C, B, H and P, x is a number satisfying 0.01≤x≤0.8, a is a number satisfying 4≤a≤20 atomic %, b is a number satisfying b=100-ac atomic %, c is a number satisfying 0≤c≤18 atomic %, And the magnet material has Th2Ni 17 The main phase of the crystal structure, The concentration of the M element in the main phase accounts for more than 89.6 atomic % of all elements in the main phase. The magnet material does not contain Ti.

2. The magnetic material according to claim 1, wherein The R element is at least one element selected from the group consisting of La, Ce, Pr, Nd, Sm, and Eu.

3. The magnetic material according to claim 1, wherein A part of the M element is substituted with at least one element selected from the group consisting of V, Cr, Nb, Ta, Mo, and W.

4. The magnetic material according to claim 1, wherein 20 atomic % or less of the M element is substituted with at least one element selected from the group consisting of Al, Si, Cr, Mn, Ni, Cu and Ga.

5. A magnetic material having a composition formula: (R 1-x Y x ) a M b A c express, In the formula, R is one or more rare earth elements, M is at least one element selected from the group consisting of Fe and Co, A is at least one element selected from the group consisting of N, C, B, H and P, x is a number satisfying 0.01≤x≤0.8, a is a number satisfying 4≤a≤20 atomic %, b is a number satisfying b=100-ac atomic %, c is a number satisfying 0≤c≤18 atomic %, And the magnet material has Th2Ni 17 The main phase of the crystal structure, The concentration of the M element in the main phase accounts for more than 89.6 atomic % of all elements in the main phase. In the M element, less than 0.89 atomic % of the composition of the magnet material is replaced by Ti, 50 atomic % or less of the Y element is substituted with at least one element selected from the group consisting of Zr and Hf. 6 . A permanent magnet comprising the magnetic material according to claim 1 . 7 . A permanent magnet comprising a sintered body of the magnet material according to claim 1 . 8 . A rotating electrical machine comprising a stator and a rotor, wherein the stator or the rotor has the permanent magnet according to claim 6 .

9. The rotating electrical machine according to claim 8, wherein: The rotor is connected to the turbine via a shaft. 10 . A vehicle comprising the rotating electrical machine according to claim 8 .

11. The vehicle according to claim 10, wherein: The rotor is connected to a shaft, and rotation is transmitted to the shaft.