Cell culture substrate, method for producing cell culture substrate, and method for producing spheroid

By forming island-shaped cell proliferative areas and non-cell proliferative areas on the cell culture substrate, and using external stimulation to peel off the cell colonies, the problems of uneven size and limited shape of spheroids in the existing technology are solved and achieved It achieves efficient and uniform spheroid formation and is suitable for differentiation applications of pluripotent stem cells.

CN112840016BActive Publication Date: 2024-10-25TOSOH CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980067821.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-10-16
Filing Date
2019-10-15
Publication Date
2024-10-25
Estimated Expiration
2039-10-15

AI Technical Summary

Technical Problem

It is difficult to form spheroids of uniform size and arbitrary shape with existing technology, especially in mass production and differentiation applications of pluripotent stem cells, and existing methods are limited to spheroids and are difficult to form spheroids of other shapes.

Method used

Using a cell culture substrate with a stimulus-responsive polymer, island-like cell proliferative areas and non-cell proliferative areas are formed on the substrate, and the cell colonies are exfoliated by external stimulation to form cells with uniform size and arbitrary shape. Spheroid.

Benefits of technology

It achieves a high survival rate of cells, the formation of spheroids with uniform size and arbitrary shape, and improves mass productivity and application efficiency of cell culture substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112840016B_ABST
    Figure CN112840016B_ABST
Patent Text Reader

Abstract

Provided are: a cell culture substrate that enables cells to effectively form spheroids, has a high cell survival rate, and can form spheroids of uniform size and arbitrary shape; and a method for producing the cell culture substrate; and a method for producing spheroids with excellent cell survival rate inside spheroids using the cell culture substrate. A cell culture substrate, characterized in that it has a substrate and a stimulus-responsive polymer coated on the substrate, the stimulus-responsive polymer is a block copolymer having a water-insoluble block segment and a stimulus-responsive block segment, and the cell culture substrate has the following two regions (A) and (B). (A) is a region having cell proliferation and stimulus responsiveness, and an area of ​​0.001 to 5 mm 2 (B) is an island-like region adjacent to the region (A) and without cell proliferation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a cell culture substrate capable of efficiently forming spheroids and capable of forming spheroids of uniform size and arbitrary shape; a method for producing the cell culture substrate; and a method for producing spheroids using the cell culture substrate. Background Art

[0002] Pluripotent stem cells such as embryonic cells (ES cells) and artificial cells (iPS cells) are cells with the ability to differentiate into various tissues of an organism (differentiation omnipotence), and are widely used as the source of cells for the field of regenerative medicine and drug discovery screening. In order to apply pluripotent stem cells to regenerative medicine and drug discovery screening, pluripotent stem cells must be differentiated into target cells, and at this time, spheroids (embryoids) of pluripotent stem cells need to be formed. In addition, although pluripotent stem cells can differentiate into various cells, it is known that the optimal size of the spheroid will be different according to the type of differentiated cells, and it is desired to control the size and make spheroids with more uniform size.

[0003] As a method for forming spheroids, a method of spontaneously forming aggregates of pluripotent stem cells by using a substrate to which pluripotent stem cells do not adhere is currently known (for example, see Patent Document 1). Although this method is excellent in mass productivity of spheroids, it has the problem that spheroids of uniform size cannot be obtained.

[0004] As a method for forming spheroids of uniform size, a method of using a cell culture substrate having fine concavoconvex shapes on the surface is known (for example, see Patent Document 2). However, such a cell culture substrate having fine concavoconvex shapes lacks mass production and is not suitable for forming a large number of spheroids. In addition, the spheroids that can be formed are limited to spherical shapes, and there is a problem that spheroids of shapes other than spherical shapes cannot be formed.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 8-140673

[0008] Patent Document 2: Japanese Patent Application Publication No. 2015-073520 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] The present invention aims to provide a cell culture substrate that can efficiently form spheroids from cells and can form spheroids of uniform size and arbitrary shape; a method for producing the cell culture substrate; and a method for producing spheroids using the cell culture substrate.

[0011] Solutions for solving problems

[0012] The present inventors have conducted intensive studies in view of the above circumstances and have found that the above-mentioned problems can be solved by a substrate having a specific region having stimuli-responsiveness, thereby completing the present invention.

[0013] That is, the present invention lies in the following [1] to

[12] .

[0014] [1] A cell culture substrate comprising a substrate and a stimuli-responsive polymer coated on the substrate, wherein the stimuli-responsive polymer is a block copolymer having a water-insoluble block segment and a stimuli-responsive block segment, and the cell culture substrate has the following two regions (A) and (B),

[0015] (A) has cell proliferation and stimulus response, and the area is 0.001 to 5 mm 2 island-like area.

[0016] (B) is a region adjacent to the region (A) above and having no cell proliferation.

[0017] [2] The cell culture substrate according to [1], wherein the region (A) includes two regions (A1) and (A2), and the region (B) includes two regions (B1) and (B2).

[0018] (A1) Cell proliferative area

[0019] (A2) Stimulus-responsive area

[0020] (B1) Substrate bonding area

[0021] (B2) Stimulus-responsive area

[0022] [3] The cell culture substrate according to [1] or [2], wherein the region (A) is a region in which temperature-responsive regions with diameters of 10 to 500 nm are dispersed in a region in which cells proliferate, or a region in which temperature-responsive regions with diameters of 10 to 500 nm are dispersed in a region in which cells do not proliferate.

[0023] [4] A cell culture substrate according to any one of [1] to [3], comprising a substrate and a layer comprising a stimuli-responsive polymer formed on the substrate, wherein the substrate comprises two regions: a region having cell proliferation and a region having no cell proliferation, and a ratio of average roughness / layer thickness of the layer is greater than or equal to 0.5 and less than or equal to 1.

[0024] [5] The cell culture substrate according to [4] above, wherein the stimuli-responsive polymer is a block copolymer having a water-insoluble block segment and more than 90 wt % of a stimuli-responsive block segment.

[0025] [6] The cell culture substrate according to any one of [1] to [5], wherein the region (A) is a plasma treatment region.

[0026] [7] The cell culture substrate according to any one of [1] to [6], which is used for forming spheroids of pluripotent stem cells.

[0027] [8] The method for producing a cell culture substrate according to any one of [1] to [7], characterized in that it comprises the following steps (1) and (2):

[0028] (1) Forming a cell-proliferative region with an area of ​​0.001 to 5 mm on the surface of a substrate without cell-proliferative activity 2 The process of the island-shaped area,

[0029] (2) A step of forming a layer based on a stimuli-responsive substance on the surface of a substrate.

[0030] [9] The method for producing a cell culture substrate according to the above-mentioned [8] is characterized in that in the above-mentioned step (1), a region with cell proliferation is formed on the surface of the substrate without cell proliferation by any one of plasma treatment, UV treatment, corona treatment or a combination of multiple thereof.

[0031]

[10] The method for producing a cell culture substrate according to [8] or [9] above, wherein the substrate used in the step (1) has cell adhesive properties but does not have cell proliferation properties.

[0032]

[11] The method for producing a cell culture substrate according to [9] or

[10] , wherein the step (1) comprises a step of laminating a surface protection film on the substrate, wherein the surface protection film has an area of ​​0.001 to 10 mm 2 hole.

[0033]

[12] A method for producing a spherical body, characterized in that the method comprises the following steps (i) to (iii):

[0034] (i) A step of seeding cells on the cell culture substrate according to any one of [1] to [8] above.

[0035] (ii) culturing the seeded cells to form colonies of cells adhered to the cell culture substrate,

[0036] (iii) a step of applying an external stimulus to detach at least a portion of the colony from the cell culture substrate to form a cell spheroid.

[0037] Effects of the Invention

[0038] The present invention can provide a cell culture substrate that can efficiently form spheroids with high cell survival rate, uniform size and arbitrary shape of spheroids, a method for producing the cell culture substrate, and a method for producing spheroids with excellent cell survival rate inside spheroids using the cell culture substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a schematic diagram (stereoscopic view) of the cell culture substrate of the present invention.

[0040] Figure 2 This is a schematic diagram (cross-sectional view) of a cell culture substrate having a layer based on a stimuli-responsive polymer.

[0041] Figure 3 This is a schematic diagram showing the state of cells after step (i) of the method for producing a spheroid of the present invention.

[0042] Figure 4 This is a schematic diagram showing the state of cells after step (ii) of the method for producing spheroids of the present invention.

[0043] Figure 5 This is a schematic diagram showing the state of cells after step (iii) of the method for producing spheroids of the present invention.

[0044] Figure 6 3 is a phase contrast microscope image showing the spheroid of Example 1.

[0045] Figure 7 1 is a phase contrast microscope image showing the colonies of Example 2.

[0046] Figure 8 3 is a phase contrast microscope image showing the spheroids of Example 2.

[0047] Fig. 9 3 is a phase contrast microscope image showing the spheroids of Example 4.

[0048] Fig.10 3 is a phase contrast microscope image showing the spheroid of Example 5.

[0049] Fig.11 This is an atomic force microscope image showing the cell culture substrate of Example 7.

[0050] Fig.12 This is an atomic force microscope image showing the cell culture substrate of Example 8.

[0051] Fig.13 3 is a phase contrast microscope image showing the spheroids of Example 8. DETAILED DESCRIPTION

[0052] Hereinafter, a method for implementing the present invention (hereinafter referred to as "this embodiment") is described in detail. The following embodiment is an example for illustrating the present invention and is not intended to limit the present invention to the following contents. The present invention can be implemented with appropriate modifications within the scope of its purpose.

[0053] In this specification, "spheroid" is a three-dimensional cell aggregate formed by a plurality of cells aggregating, and does not include a cell sheet formed by cells adhering to a substrate. Preferably, it has a spherical shape, or it may be a spherical or hollow shape with a gap formed by folding a sheet of cells. In addition, in this specification, "colony" means a cell group in the form of a cell sheet formed by cells adhering to a substrate.

[0054] In addition, in this specification, "stimulus responsiveness" means that the structure changes or the degree of hydrophilicity / hydrophobicity changes due to external stimulation. Here, in this specification, "external stimulation" means: mechanical stimulation such as ultrasound, vibration, convection; electromagnetic stimulation such as light, electricity, magnetism; thermodynamic stimulation such as heating and cooling, and does not include stimulation caused by biological reactions such as enzyme reactions.

[0055] In this specification, "temperature responsiveness" means that the degree of hydrophilicity / hydrophobicity changes due to temperature changes. Furthermore, the critical temperature at which the degree of hydrophilicity / hydrophobicity changes is referred to as "response temperature."

[0056] In addition, in this specification, "biologically derived substances" are substances existing in the body of an organism, and may be natural substances, or substances artificially synthesized by gene recombination technology, etc., or substances obtained by chemical synthesis based on the aforementioned biologically derived substances. Biologically derived substances are not particularly limited, and examples thereof include nucleic acids, proteins, polysaccharides, and nucleotides, nucleosides, amino acids, various sugars, or lipids, vitamins, and hormones that are the basic materials constituting organisms.

[0057] In addition, in this specification, "cell adhesion" means that the cell is easy to adhere to the cell culture substrate at the culture temperature, and "having cell adhesion" means that the cell can adhere to the substrate or cell culture substrate directly or through the biological material at the culture temperature. In addition, "not having cell adhesion" means that the cell cannot adhere to the substrate or cell culture substrate at the culture temperature.

[0058] In addition, in this specification, "cell proliferation" means that cells easily proliferate at the culture temperature, and "having cell proliferation" means that cells can adhere to the substrate or cell culture substrate directly or with the aid of a biological substance at the culture temperature and proliferate. In addition, "not having cell proliferation" means that cells cannot adhere to the substrate or cell culture substrate at the culture temperature, or adhere but cannot proliferate. Furthermore, "high cell proliferation" means that when compared with the same culture period, more cells proliferate.

[0059] A cell culture substrate according to one embodiment of the present invention has the following two regions (A) and (B).

[0060] (A) has cell proliferation and stimulus response, and the area is 0.001 to 5 mm 2 island-like area.

[0061] (B) A region adjacent to the region (A) above and without cell proliferation.

[0062] The aforementioned (A) region has cell proliferation and stimulus responsiveness. Due to the cell proliferation and stimulus responsiveness, the cell culture substrate of the present invention can form colonies by culturing cells and peel off colonies by external stimulation to produce spheroids. In the case of not having cell proliferation or stimulus responsiveness, it is impossible to culture cells to form colonies or to peel off colonies by external stimulation, so it is impossible to produce spheroids.

[0063] The aforementioned stimulus responsiveness is not particularly limited as long as the colonies can be detached by external stimulation, and the examples include temperature responsiveness, light responsiveness, pH responsiveness, magnetic responsiveness, electric field responsiveness, and mechanical stimulus responsiveness. Preferably, it is any one of temperature responsiveness, light responsiveness, pH responsiveness, and mechanical stimulus responsiveness, or a combination of multiple thereof; more preferably, it is any one of temperature responsiveness, light responsiveness, and mechanical stimulus responsiveness, or a combination of multiple thereof; particularly preferably, it is any one of temperature responsiveness and mechanical stimulus responsiveness, or a combination of multiple thereof; and most preferably, it is temperature responsiveness.

[0064] (A) The area is also 0.001 to 5 mm 2 The island-shaped area is 0.001 to 5 mm 2 The island-like region can form colonies of a size and shape suitable for producing spheroids when culturing cells. In addition, the shape of the colonies can be controlled by the shape of the island-like region, and spheroids other than spheres can be produced. The area is less than 0.001 mm 2 or more than 5mm 2In the case of 0.005 to 1 mm2 of the spheroid, the optimal size of colonies cannot be formed when the cells are cultured, the shape of the spheroid is deformed, or the spheroid cannot be produced. In addition, from the perspective of being suitable for forming spheroids suitable for differentiation induction of pluripotent stem cells, the area is preferably 0.005 to 1 mm2. 2 , and the preferred area is 0.01 to 0.5 mm 2 , the area is particularly preferably 0.015 to 0.25 mm 2 The most preferred area is 0.02 to 0.2 mm 2 .

[0065] In addition, from the perspective of suitability for producing spheroids having uniform size and shape, the standard deviation of the area of ​​the (A) region / average area is preferably 80% or less, more preferably 50% or less, particularly preferably 20% or less, and most preferably 5% or less.

[0066] In the present invention, "island-like" means an independent region arranged on a plane like an island structure existing in a sea-island structure (for example, Figure 1 The part shown in the symbol A.). Since (A) region is island-shaped, the cell culture substrate of the present invention can form colonies by culturing cells, and peel off colonies by external stimulation to make spheroids. When (A) region is not island-shaped, such as in the case of stripe-like structures, the colonies are easily broken when peeling off and spheroids with uniform size and shape cannot be manufactured. As the shape of the island, there is no particular limitation, and it can be suitably set according to the shape of the target spheroid, for example, a circle, an ellipse, a polygon, a closed shape formed by a straight line or a curve of an irregular shape, etc. can be listed. In addition, from the aspect of being suitable for manufacturing a spheroid close to a spherical shape, as the shape of the island, preferably a circle or an ellipse, a polygon, further preferably a circle or an ellipse, a rectangle, particularly preferably a circle or an ellipse, a square, and most preferably a circle or an ellipse.

[0067] In addition, in the present invention, from the perspective of being suitable for manufacturing a spherical body close to a sphere, the aspect ratio of the island shape is preferably 5 or less, more preferably 2 or less, particularly preferably 1.5 or less, and most preferably 1.1 or less. Here, in the present invention, the "aspect ratio" represents the major diameter / minor diameter as the ratio of the maximum diameter (major diameter) to the minimum diameter (minor diameter) of the shape.

[0068] The aforementioned (B) region is adjacent to the aforementioned (A) region and does not have cell proliferation. Since it is an area adjacent to the (A) region and does not have cell proliferation, when culturing cells, colonies are formed only in the (A) region, and a state where no colonies exist can be formed around the (A) region, and colonies are peeled off by external stimulation to manufacture spheroids. When the (B) region is not adjacent to the (A) region or has cell proliferation, when culturing cells, colonies also exist around the (A) region, so when the colonies in the (A) region are peeled off by external stimulation, the colonies in the (A) region are fixed by the surrounding colonies and spheroids cannot be manufactured, or the surrounding colonies adhere to the colonies in the (A) region and spheroids with uniform size and shape cannot be manufactured. In addition, from the aspect of being suitable for making the size and shape of the manufactured spheroids uniform, it is preferred that the (B) region not only has cell proliferation but also has cell adhesion.

[0069] The shape of the (B) region is not limited except that it is adjacent to the (A) region. However, from the perspective of being suitable for producing spheroids of uniform size and shape, it is preferred that 20% or more of the length of the boundary line with the (A) region is adjacent to the (B) region, more preferably 50% or more, particularly preferably 80% or more, and most preferably the entire periphery of the (A) region is the (B) region. In addition, from the perspective of being suitable for improving the mass productivity of the cell culture substrate, it is preferred that the (A) region is an island-shaped structure and the (B) region is a sea-shaped structure (for example, Figure 1 The region other than the region (B) adjacent to the region (A) includes a region having cell proliferation but not responsive to stimulation.

[0070] The aforementioned (B) region also preferably has stimulus responsiveness. When (B) region and (A) region have stimulus responsiveness in the same manner, when manufacturing the cell culture substrate of the present invention, it is not necessary to pattern by covering stimulus responsiveness material in (A) region and (B) region, as long as the stimulus responsiveness material is uniformly covered on the whole surface of the cell culture substrate, the mass production of the cell culture substrate can be improved. In addition, by covering stimulus responsiveness material in (B) region, the cell adhesion in (B) region can be reduced, so it is easy to make colonies with uniform shape, and it is easy to manufacture spheroids with uniform size and shape, so it is preferred.

[0071] The area ratio of the (A) region and the (B) region is not particularly limited, but from the perspective of increasing the amount of spheroids that can be produced per unit area of ​​the culture substrate, the area of ​​the (A) region is preferably 10% or more of the entire substrate, more preferably 30% or more, particularly preferably 50% or more, and most preferably 70% or more. In addition, from the perspective of providing a sufficient distance between multiple (A) regions and inhibiting the fusion of colonies in multiple (A) regions to form an uneven shape, the area of ​​the (B) region is preferably 20% or more of the entire substrate, more preferably 40% or more, particularly preferably 60% or more, and most preferably 80% or more.

[0072] In the present invention, from the perspective of improving the mass productivity of the cell culture substrate, it is preferred that the stimuli-responsiveness is caused by a layer containing a stimuli-responsive polymer. Here, when the term "substrate" is used in the present invention, it means the base substrate (e.g., Figure 2 1.) In addition, when "cell culture substrate" is mentioned, it means the entire article for forming spheroids (for example, Figure 2 The part indicated by symbol 10. ).

[0073] There is no particular limitation on the type of the stimuli-responsive polymer, and suitable examples include block copolymers coated on a substrate; copolymers immobilized on a substrate via reactive groups such as an azide group; polymers immobilized on a substrate by coating a monomer on a substrate and subjecting the substrate to electron beam polymerization or free radical polymerization, etc.

[0074] As the aforementioned stimulus-responsive polymer, a temperature-responsive polymer is preferred from the perspective of being suitable for detaching colonies with relatively weak stimulation and producing spheroids without damaging the cells. In addition, when culturing cells on a cell culture substrate, from the perspective of being able to culture cells at a temperature close to body temperature, the response temperature is preferably 50°C or less, more preferably 35°C or less, and from the perspective of being suitable for inhibiting cell detachment during operations such as medium replacement during the culture process, it is particularly preferably 25°C or less, and most preferably 15°C or less. Furthermore, from the perspective of being able to form spheroids by cooling operations at a temperature that does not damage the cells, the response temperature is preferably 0°C or more, more preferably 5°C or more, particularly preferably 10°C or more, and most preferably 15°C or more.

[0075] The type of the temperature-responsive polymer is not particularly limited. Examples of the monomer unit include (meth)acrylamide compounds such as acrylamide and methacrylamide; N,N-diethylacrylamide, N-ethylacrylamide, N-n-propylacrylamide, N-n-propylmethacrylamide, N-isopropylacrylamide, N-isopropylmethacrylamide, N-cyclopropylacrylamide, N-cyclopropylmethacrylamide, N-tert-butylacrylamide, N-ethoxyethylacrylamide, N-ethoxyethylmethacrylamide, N-tetrahydrofurfurylacrylamide, N-tetrahydrofurfurylmethacrylamide and other N-alkyl-substituted (meth)acrylamide derivatives; N,N-dimethyl (meth)acrylamide, N,N-ethylmethacrylamide, N,N-diethylacrylamide and other N,N-dialkyl-substituted (meth)acrylamide derivatives; 1-(1-oxo-2-propenyl)-pyrrolidone; (Meth)acrylamide derivatives having a cyclic group such as pyrrolidine, 1-(1-oxo-2-propenyl)-piperidine, 4-(1-oxo-2-propenyl)-morpholine, 1-(1-oxo-2-methyl-2-propenyl)-pyrrolidine, 1-(1-oxo-2-methyl-2-propenyl)-piperidine, and 4-(1-oxo-2-methyl-2-propenyl)-morpholine; vinyl ethers such as methyl vinyl ether; and proline derivatives such as N-proline methyl ester acrylamide. From the viewpoint of being suitable for setting the response temperature to 0 to 50° C., N,N-diethylacrylamide, N-n-propylacrylamide, N-isopropylacrylamide, N-n-propylmethacrylamide, N-ethoxyethylacrylamide, N-tetrahydrofurfurylacrylamide, and N-tetrahydrofurfurylmethacrylamide are preferred, N-n-propylacrylamide and N-isopropylacrylamide are more preferred, and N-isopropylacrylamide is particularly preferred. When a room temperature medium is used for medium replacement during culture operation, N-n-propylacrylamide and N-proline methyl ester acrylamide are preferred from the viewpoint of being suitable for setting the response temperature of the block copolymer to a temperature lower than room temperature.

[0076] In addition, the temperature-responsive polymer may be a copolymer, for example, a copolymer comprising at least two or more monomer units selected from the aforementioned monomer units, particularly a copolymer of N-isopropylacrylamide and N-tert-butylacrylamide, which is preferred because the response temperature can be controlled within the range of 5 to 30°C by changing the content of N-tert-butylacrylamide within the range of 5 to 60 mol%. Furthermore, it may be a copolymer of the aforementioned monomer units constituting the temperature-responsive segment and other monomer units, for example, by making a copolymer with a hydrophilic monomer unit, the response temperature can be shifted to the high temperature side, and by making a copolymer with a hydrophobic monomer unit, the response temperature can be shifted to the low temperature side. It should be noted that the arrangement of the copolymer may be any of a random arrangement, an alternating arrangement, and a block arrangement.

[0077] In the present invention, from the perspective of being suitable for rapidly performing the process of forming spheroids from colonies, the ratio of temperature-responsive structural units contained in the temperature-responsive polymer is preferably 70 wt% or more, more preferably 80 wt% or more, particularly preferably 90 wt% or more, and most preferably 92 wt% or more.

[0078] As the aforementioned stimulus-responsive polymer, preferably: a block copolymer having a stimulus-responsive block segment and a water-insoluble block segment or a block copolymer having a stimulus-responsive block segment and a reactive segment. By making the stimulus-responsive polymer the aforementioned block copolymer, it is possible to improve the mass productivity of the cell culture substrate and inhibit the stimulus-responsive polymer from being mixed into the manufactured spheroid. As the aforementioned stimulus-responsive block segment, there is no particular limitation, and polymers containing monomeric units of the aforementioned temperature responsiveness can be cited. In addition, by making the block copolymer contain a water-insoluble block segment or a reactive segment, it is possible to inhibit the block copolymer from being mixed into the culture fluid, and it is possible to culture without contaminating cells, so that the stimulus-responsive polymer can be inhibited from being mixed into the spheroid, so it is preferred. Here, in this specification, the block segment "having water insolubility" means that at least a portion of the homopolymer consisting only of the monomeric units constituting the block segment is insoluble in water. Furthermore, the term "reactive segment" means that the block segment has a reactive group and can be immobilized on a substrate by external stimulation such as heat, pH change, or light irradiation.

[0079] Examples of the monomer units constituting the water-insoluble block segments include n-butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, n-hexyl acrylate, n-hexyl methacrylate, n-octyl acrylate, n-octyl methacrylate, n-decyl acrylate, n-decyl methacrylate, n-dodecyl acrylate, n-dodecyl methacrylate, n-tetradecyl acrylate, n-tetradecyl methacrylate, etc. In addition, from the perspective of being suitable for firmly fixing the block copolymer to a substrate, it is preferred to have a reactive group, and examples thereof include 4-azidophenyl acrylate, 4-azidophenyl methacrylate, 2-((4-azidobenzoyl)oxy)ethyl acrylate, and 2-((4-azidobenzoyl)oxy)ethyl methacrylate. Furthermore, from the perspective of suitability for improving cell proliferation, a structure having an aromatic ring is preferred, and examples thereof include 2-hydroxyphenyl acrylate, 2-hydroxyphenyl methacrylate, 3-hydroxyphenyl acrylate, 3-hydroxyphenyl methacrylate, 4-hydroxyphenyl acrylate, 4-hydroxyphenyl methacrylate, N-(2-hydroxyphenyl)acrylamide, N-(2-hydroxyphenyl)methacrylamide, N-(3-hydroxyphenyl)acrylamide, N-(3-hydroxyphenyl)methacrylamide, N-(4-hydroxyphenyl)acrylamide, N-(4-hydroxyphenyl)methacrylamide, and styrene.

[0080] In the present invention, examples of the monomer unit constituting the reactive block segment include 4-azidophenyl acrylate, 4-azidophenyl methacrylate, 2-((4-azidobenzoyl)oxy)ethyl acrylate, and 2-((4-azidobenzoyl)oxy)ethyl methacrylate.

[0081] In the present invention, the water-insoluble block segment or the reactive block segment may further include a repeating unit for controlling the response temperature of the block copolymer. As the repeating unit for controlling the response temperature of the block copolymer, hydrophilic or hydrophobic components may be listed, without particular limitation, for example, 2-dimethylaminoethyl acrylate, 2-dimethylaminoethyl methacrylate, 2-diethylaminoethyl acrylate, 2-diethylaminoethyl methacrylate, N-[3-(dimethylamino)propyl]acrylamide and the like having an amino group; N-(3-sulfopropyl)-N-methacryloyloxyethyl-N,N-dimethylammonium betaine, N-methacryloyloxyethyl-N,N-dimethylammonium-α-N-methylcarboxy betaine and the like having Betaine; hydroxyethyl acrylate, hydroxyethyl methacrylate, N-(2-hydroxyethyl) acrylamide, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, polypropylene glycol monoacrylate, polypropylene glycol monomethacrylate, methoxy polyethylene glycol monoacrylate, methoxy polyethylene glycol monomethacrylate, diethylene glycol monomethyl ether acrylate, diethylene glycol monomethyl ether methacrylate, diethylene glycol monoethyl ether acrylate, diethylene glycol monoethyl ether methacrylate, 2-methoxyethyl acrylate, 2-methoxyethyl methacrylate, 2-ethoxyethyl acrylate, methyl acrylate 2-ethoxyethyl acrylate, 3-butoxyethyl acrylate, 3-butoxyethyl methacrylate, 3-butoxyethyl acrylamide, furfuryl acrylate, furfuryl methacrylate, tetrahydrofurfuryl acrylate, tetrahydrofurfuryl methacrylate, etc. having a polyethylene glycol group, methoxyethyl group; methoxymethyl acrylate, methoxymethyl methacrylate, 2-ethoxymethyl acrylate, 2-ethoxymethyl methacrylate, 3-butoxymethyl acrylate, 3-butoxymethyl methacrylate, 3-butoxymethyl acrylamide, etc. having an acrylate group; 2-methacryloyloxyethyl phosphorylcholine, 2-acryloyloxyethyl Those having a phosphorylcholine group such as acyloxyethyl phosphorylcholine, 3-(meth)acryloyloxypropyl phosphorylcholine, 4-(meth)acryloyloxybutyl phosphorylcholine, 6-(meth)acryloyloxyhexyl phosphorylcholine, 10-(meth)acryloyloxydecyl phosphorylcholine, ω-(meth)acryloyl(poly)oxyethylene phosphorylcholine, 2-acrylamideethyl phosphorylcholine, 3-acrylamidepropyl phosphorylcholine, 4-acrylamidebutyl phosphorylcholine, 6-acrylamidehexyl phosphorylcholine, 10-acrylamidedecyl phosphorylcholine and ω-(meth)acrylamide(poly)oxyethylene phosphorylcholine.

[0082] The water-insoluble block segments or reactive block segments may be copolymers, and the arrangement of the copolymers may be any of a random arrangement, an alternating arrangement, and a block arrangement.

[0083] The structural unit ratio of the aforementioned water-insoluble block segment or reactive block segment is preferably 1 wt% or more, further preferably 2 wt% or more, particularly preferably 5 wt% or more, and most preferably 10 wt% or more, from the viewpoint of preventing the block copolymer from mixing into the culture medium and contaminating the cells, and from the viewpoint of maintaining a high rate of undifferentiation in subculture.

[0084] The molecular weight of the stimuli responsive polymer in the present invention is not particularly limited, but is preferably 1,000 to 1,000,000, more preferably 2,000 to 500,000, particularly preferably 5,000 to 300,000, and most preferably 10,000 to 200,000 in terms of number average molecular weight in order to improve the strength of the stimuli responsive polymer.

[0085] In the present invention, from the aspect of being suitable for inhibiting the mixing of stimulus-responsive polymers into spheroids, the components with a number average molecular weight of 5000 or less contained in the stimulus-responsive polymer are preferably 50% or less, more preferably 30% or less, particularly preferably 10% or less, and most preferably 5% or less. In addition, the components with a number average molecular weight of 10000 or less are preferably 50% or less, more preferably 30% or less, particularly preferably 10% or less, and most preferably 5% or less. Furthermore, the components with a number average molecular weight of 30000 or less are preferably 50% or less, more preferably 30% or less, particularly preferably 10% or less, and most preferably 5% or less. The content of the components below the specific molecular weight contained in the block copolymer can be measured by gel permeation chromatography.

[0086] In the present invention, from the perspective of being suitable for inhibiting the mixing of the stimuli-responsive polymer into the spheroid, the dissolution amount of the stimuli-responsive polymer in water is preferably 50% or less, more preferably 30% or less, particularly preferably 10% or less, and most preferably 5% or less. The dissolution amount of the stimuli-responsive polymer in water represents the weight loss ratio of the stimuli-responsive polymer when the substrate formed with the layer based on the stimuli-responsive polymer is immersed in water at 25°C for about 1 hour. Here, there is no particular limitation on the method for measuring the weight loss of the stimuli-responsive polymer, and it can be measured by a commonly used method, for example, a method based on FT-IR, a method based on measuring the average film thickness, etc.

[0087] The stimulus-responsive polymer in the present invention may contain a chain transfer agent, a polymerization initiator, a polymerization inhibitor, etc. as needed. As a chain transfer agent, there is no particular limitation, and a common user can be suitably used, for example, dithiobenzoate, trithiocarbonate, 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid, 2-cyanopropane-2-yl-N-methyl-N-(pyridine-4-yl)dithiocarbamate, (methyl-2-[methyl (4-pyridine) dithiocarbonate] propionate). In addition, as a polymerization initiator, there is no particular limitation, and a common user can be suitably used, for example, azobisisobutyronitrile, 1,1'-azobis(cyclohexanecarbonitrile), di-tert-butyl peroxide, tert-butyl hydroperoxide, hydrogen peroxide, potassium persulfate, benzoyl peroxide, triethyl boron, diethyl zinc, etc. can be cited. Furthermore, the polymerization inhibitor is not particularly limited and any commonly used inhibitor can be appropriately used. Examples thereof include hydroquinone, p-methoxyphenol, 1,2,4,5-tetrazine-1(2H)-yl, 3,4-dihydro-2,4,6-triphenylverdazyl, 2,2,6,6-tetramethylpiperidinyl-1-oxyl, and 4-hydroxy-2,2,6,6-tetramethylpiperidinyl-1-oxyl.

[0088] The method for synthesizing the stimuli-responsive polymer in the present invention is not particularly limited, and the living radical polymerization technique described in "Radical Polymerization Handbook", published by NTS Inc., pp. 161-225 (2010) can be used.

[0089] In the present invention, from the perspective of being suitable for improving cell proliferation, the thickness of the layer based on the stimuli-responsive polymer is preferably 1000 nm or less, more preferably 200 nm or less, particularly preferably 100 nm or less, and most preferably 50 nm or less. In addition, from the perspective of being suitable for rapidly performing the process of forming spheroids from colonies, the thickness of the layer based on the stimuli-responsive polymer is preferably 5 nm or more, more preferably 20 nm or more, particularly preferably 30 nm or more, and most preferably 35 nm or more. Here, the "thickness" of the layer based on the stimuli-responsive polymer in the present invention represents the length in the out-of-plane direction from the interface between the substrate and the layer based on the stimuli-responsive polymer to the peak portion in the surface structure of the layer based on the stimuli-responsive polymer. For the layer thickness of the layer based on the stimulus responsive polymer, it can be calculated as follows: the cell culture substrate is immersed in water at the culture temperature for more than 24 hours, and it is quickly dried by blowing air, etc. For the obtained sample, when the layer thickness exceeds the range of 10nm, the ultrathin section of the cell culture substrate made by the microtome is used to measure the cross-sectional image using a transmission electron microscope, and the distance of 10 randomly selected positions is measured, and the average value is obtained, thereby calculating. In addition, when the layer thickness is in the range below 10nm, an ellipsometer can be used for measurement.

[0090] In the present invention, from the perspective of being suitable for improving cell proliferation and rapidly performing the process of forming spheroids from colonies, the ratio of the average roughness of the surface / layer thickness of the layer based on the stimuli-responsive polymer is preferably 0.3 or more. By making the ratio of the average roughness of the surface of the stimuli-responsive polymer to the layer thickness to be 0.3 or more, it is possible to set areas where cells strongly adhere and areas where they do not, so that the cell proliferation can be improved and the process of forming spheroids from colonies can be rapidly performed. From the perspective of being suitable for improving cell proliferation and rapidly performing the process of forming spheroids from colonies, the ratio of the average roughness of the surface of the layer based on the stimuli-responsive polymer to the layer thickness is further preferably 0.5 or more, particularly preferably 0.7 or more, and most preferably 0.9 or more. Here, the "average roughness" of the surface of the layer based on the stimuli-responsive polymer in the present invention means the average height of the profile curve determined in accordance with JIS B0601:2013, and can be calculated by measuring an atomic force microscope image of a representative surface of the cell culture substrate, and obtaining the average height with 1 μm as a reference length in the roughness curve of 10 randomly selected positions. Similar to the above-mentioned layer thickness measurement, the cell culture substrate is immersed in water at the culture temperature for more than 24 hours, and it is quickly dried by blowing air, etc., and the obtained sample is measured.

[0091] In the cell culture substrate of one embodiment of the present invention, it is preferred that the region (A) includes two regions (A1) and (A2) described below, and the region (B) includes two regions (B1) and (B2) described below.

[0092] (A1) Cell proliferative area

[0093] (A2) Stimulus-responsive area

[0094] (B1) Substrate bonding area

[0095] (B2) Stimulus-responsive area

[0096] Here, "substrate bonding region" means that the component covering the cell culture substrate adheres to the region on the substrate. The stimulus responsive region has the effect of reducing cell proliferation, so by making (A) region include (A1) and (A2) these 2 regions, it is possible to suitably carry out the spheroid formation of the pluripotent stem cells that are difficult to adhere to the cell culture substrate and proliferate and the peeling from the cell culture substrate by stimulus response. In addition, since (B) region has (B1), it is suitable for the component covering the cell culture substrate to be firmly immobilized on the substrate. And then, since (B) region has (B2) region, it is suitable for suppressing the proliferation of pluripotent stem cells in (B) region, and is suitable for forming uniform spheroids. For (A1) and (A2), (B1) and (B2) regions, it is possible to determine the principal component present in each region by measuring the atomic force microscope image or the transmission electron microscope image on the cell culture substrate surface, so as to confirm. For example, in the case of covering a copolymer including a cell proliferation monomer unit and a stimuli-responsive monomer unit, the monomer unit present in each region can be determined based on the phase image in an atomic force microscope image or the contrast in a transmission electron microscope image.

[0097] The aforementioned (A1) and (A2), (B1) and (B2) regions can be suitably formed by covering a block copolymer comprising a combination of monomer units having greatly different degrees of hydrophilicity / hydrophobicity. Among them, the composition and coverage of the copolymers capable of forming the (A1) and (A2), (B1) and (B2) regions vary depending on the type of block copolymer. When the block copolymer is a diblock of butyl methacrylate and N-isopropylacrylamide, a diblock having more than 90% of one component is preferred, more preferably N-isopropylacrylamide exceeds 90%, particularly preferably N-isopropylacrylamide exceeds 92%, and most preferably N-isopropylacrylamide exceeds 94%. In addition, it is preferably covered with a film thickness of 1 to 200 nm, more preferably a film thickness of 5 to 100 nm, particularly preferably a film thickness of 10 to 50 nm, and most preferably a film thickness of 15 to 35 nm.

[0098] In the present invention, the aforementioned (A) region preferably has a cell proliferative region with a temperature responsive region having a diameter of 10 to 500 nm dispersed therein, or a cell proliferative region with a diameter of 10 to 500 nm dispersed therein in a temperature responsive region not having cell proliferative activity. By making the (A) region dispersed with the aforementioned region with a diameter of 10 to 500 nm, spheroid formation of pluripotent stem cells and peeling from the cell culture substrate by stimulus response can be appropriately performed.

[0099] In the present invention, the aforementioned region (A) is preferably a plasma-treated region from the viewpoint of improving the mass productivity of spheroids and forming uniform spheroids. By making the region (A) a plasma-treated region, a large number of cells can be gathered only in the region (A), and a large number of uniform spheroids can be easily formed.

[0100] In the present invention, from the perspective of improving the mass productivity of spheroids and further forming uniform spheroids, the difference in zeta potential between the (A) region and the (B) region is preferably 5 mV or more, more preferably 10 mV or more, particularly preferably 20 mV or more, and most preferably 40 mV or more.

[0101] In the present invention, from the perspective of improving the mass productivity of spheroids, it is preferred that there is no partition wall that cells cannot cross around the aforementioned (A) region. By making the absence of a partition wall that cells cannot cross around the (A) region, cells can move freely and a large number of cells can be gathered in the (A) region, thereby improving the mass productivity of spheroids. In addition, from the perspective of improving the mass productivity of spheroids, it is further preferred that there is no partition wall with a height of 1 μm or more, particularly preferably no partition wall with a height of 0.1 μm or more, and most preferably no partition wall with a height of 0.05 μm or more.

[0102] In the present invention, the cell culture substrate may contain a biologically derived substance on its surface as required. The biologically derived substance is not particularly limited, and examples thereof include matrigel, laminin, fibronectin, vitronectin, collagen, and the like.

[0103] These biologically derived substances may be natural substances, or may be artificially synthesized by gene recombination technology, or may be fragments obtained by cleavage with restriction enzymes, or synthetic proteins or synthetic peptides based on these biologically derived substances.

[0104] In the present invention, as the aforementioned matrigel, for example, commercially available products such as Matrigel (manufactured by Corning Incorporated) and Geltrex (manufactured by Thermo Fisher Scientific) can be preferably used from the viewpoint of easy availability.

[0105] The type of the laminin is not particularly limited, and for example, laminin 511, laminin 521, or laminin 511-E8 fragments reported to show high activity against α6β1 integrin expressed on the surface of human iPS cells can be used. The laminin can be a natural product, or it can be artificially synthesized by gene recombination technology, etc., or it can be a synthetic protein or synthetic peptide based on the laminin. From the perspective of ease of acquisition, for example, iMatrix-511 (manufactured by Nippi, Inc.) which is a commercially available product can be appropriately used.

[0106] The vitronectin may be a natural product, or may be artificially synthesized by gene recombination techniques, or may be a synthetic protein or synthetic peptide based on the vitronectin. From the perspective of ease of acquisition, for example, commercially available vitronectin, human plasma source (Wako Pure Chemical Industries, Ltd.), synthemax (Corning Incorporated), and vitronectin (VTN-N) (Thermo Fisher Scientific) may be suitably used.

[0107] The aforementioned fibronectin may be a natural product, or may be artificially synthesized by gene recombination techniques, or may be a synthetic protein or synthetic peptide based on the aforementioned fibronectin. From the aspect of ease of acquisition, for example, a commercially available fibronectin solution, a human plasma source (Wako Pure Chemical Industries, Ltd.), or Retronectin (Takara Bio Inc.) may be suitably used.

[0108] The type of the aforementioned collagen is not particularly limited, for example, type I collagen and type IV collagen can be used. The aforementioned collagen can be a natural product, or it can be artificially synthesized by gene recombination techniques, or it can be a synthetic peptide based on the aforementioned collagen. From the aspect of ease of acquisition, for example, human collagen I (Corning Incorporated) and human collagen IV (Corning Incorporated) as commercial products can be suitably used.

[0109] In the present invention, in order to suppress the denaturation of biologically derived substances and to improve cell proliferation, it is preferred that biologically derived substances are immobilized on a cell culture substrate by non-covalent bonds rather than covalent bonds. Here, in the present invention, "non-covalent bonds" refer to binding forces other than covalent bonds derived from intermolecular forces such as electrostatic interactions, hydrophobic interactions (Japanese: water-insoluble interactions), hydrogen bonds, π-π interactions, dipole-dipole interactions, London dispersion forces, and other van der Waals interactions. The immobilization of biologically derived substances on block copolymers can be caused by a single binding force or a combination of multiple ones.

[0110] In the present invention, the method for immobilizing the biogenic substance is not particularly limited. For example, the following methods can be suitably used: a method of immobilizing the biogenic substance by applying a solution of the biogenic substance on a cell culture substrate for a predetermined time; a method of immobilizing the biogenic substance by adding the biogenic substance to the culture solution during cell culture so that the biogenic substance is adsorbed to the cell culture substrate.

[0111] In the present invention, the material of substrate is not particularly limited, and not only materials such as glass and polystyrene used in common cell culture can be used, but also materials that can usually give form, such as polymer compounds such as polycarbonate, polyethylene terephthalate, polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, polymethyl methacrylate, ceramics, metals, etc. can be used. From the ease of culture operation, the material of substrate preferably includes at least one of glass, polystyrene, polycarbonate, polyethylene terephthalate, polyethylene, and polypropylene, and further preferably includes at least one of glass, polystyrene, polycarbonate, polyethylene terephthalate, and polyethylene. From the aspect suitable for improving flexibility, polystyrene, polycarbonate, polyethylene terephthalate, and polyethylene are particularly preferred. In addition, from the aspect suitable for patterning by using the hydrophilic treatment described later and giving cell proliferation, polystyrene, polycarbonate, and polyethylene are most preferred.

[0112] As the shape of substrate, there is no particular restriction, can be a plane shape such as plate, film, can also be fiber, porous particles, porous membrane, hollow fiber. In addition, it can also be the container (cell culture dishes such as petri dishes, flasks, culture plates, etc.) used in common cell culture, etc. Consider from the aspect of the ease of culture operation, preferably a plane shape such as plate, film or a porous membrane as a flat membrane. In addition, as required, the structure for distinguishing each spheroid can be provided by arranging a partition plate, etc. on substrate.

[0113] In the present invention, from the perspective of being suitable for rapidly performing the process of forming spheroids from colonies and being able to distribute nutrients to the inside of colonies without leaving any residue when manufacturing larger spheroids, it is preferred that the substrate is a porous substrate and the pore size of the porous substrate is smaller than that of the cells. In addition, from the perspective of being suitable for rapidly performing the process of forming spheroids from colonies, the pore size is preferably 0.01 to 8 μm, more preferably 0.01 to 3 μm, particularly preferably 0.01 to 1 μm, and most preferably 0.1 to 1 μm. Here, the "pore size" of the porous substrate in the present invention represents the average value of the diameter of the pores of the porous substrate along the in-plane direction of the porous substrate, and can be calculated by measuring the diameters of more than 20 pores in the laser microscope image, scanning electron microscope image, and transmission electron microscope image of the porous substrate and finding the average value.

[0114] As the aforementioned porous substrate, in addition, from the aspect of being suitable for rapidly performing the process of forming spheroids from colonies, the porosity is preferably 0.01 to 60%, more preferably 0.01 to 20%, particularly preferably 0.01 to 4%, and most preferably 0.01 to 1.5%. Here, the "porosity" of the porous substrate in the present invention is a value obtained by dividing the total area of ​​the pore portion by the substrate area for one main surface of the surface of the porous substrate, indicating the extent of pores present in the substrate surface in terms of area ratio, and can be measured by observing a square area with a side length of 200 times or more of the pore diameter of the porous substrate in a laser microscope image, a scanning electron microscope image, or a transmission electron microscope image of the porous substrate.

[0115] The cell culture substrate of the present invention can be sterilized. The method of sterilization is not particularly limited, and high pressure steam sterilization, UV sterilization, gamma ray sterilization, ethylene oxide gas sterilization, etc. can be used. From the aspect of being suitable for suppressing the denaturation of the block copolymer, high pressure steam sterilization, UV sterilization, ethylene oxide gas sterilization are preferred, from the aspect of being suitable for suppressing the deformation of the substrate, UV sterilization or ethylene oxide gas sterilization are further preferred, and from the aspect of excellent batch productivity, ethylene oxide gas sterilization is particularly preferred.

[0116] As cells cultured using the cell culture substrate of the present invention, as long as the surface can be adhered to before applying temperature reduction stimulation, there is no particular limitation. For example, in addition to various cell line cells such as Chinese hamster ovary-derived CHO cells, mouse connective tissue L929, human embryonic kidney-derived HEK293 cells, and human cervical cancer-derived HeLa cells, it is also possible to use, for example: as epithelial cells and endothelial cells constituting each tissue and organ in the organism; Skeletal muscle cells, smooth muscle cells, and cardiomyocytes showing contractility; Neuronal cells, glial cells, and fibroblasts constituting the nervous system; Hepatic parenchymal cells, liver non-parenchymal cells, and fat cells participating in the metabolism of the organism; Mesenchymal stem cells, bone marrow cells, and Muse cells as cells with differentiation ability are present in various tissues, and then ES cells, iPS cells, etc. have stem cells (pluripotent stem cells) with differentiation pluripotency, cells induced by differentiation of these cells, etc. From the viewpoint of the proliferation and exfoliation of the cells of the culture substrate of the present invention, preferably stem cells or pluripotent stem cells, further preferably mesenchymal stem cells or pluripotent stem cells, particularly preferably pluripotent stem cells, and most preferably iPS cells.

[0117] The present invention also relates to a method for producing the cell culture substrate with excellent mass productivity. The method is characterized by comprising the following steps (1) and (2).

[0118] (1) Forming a cell-proliferative area of ​​0.001 to 5 mm on the surface of a substrate that does not have cell-proliferative properties 2 The process of forming an island-like area.

[0119] (2) A step of forming a layer based on a stimuli-responsive substance on the surface of a substrate.

[0120] Hereinafter, steps (1) to (2) in the method for producing a cell culture substrate of the present invention will be described in detail.

[0121] In the step (1) of the method for producing a cell culture substrate of the present invention, a substrate without cell proliferation is used, and a layer having cell proliferation and an area of ​​0.001 to 5 mm is formed on the surface of the substrate. 2 Island-shaped regions. By using a substrate without cell proliferation and forming a cell proliferation region by patterning, a cell proliferation region of any shape and size can be effectively prepared. As a method for forming a cell proliferation region, from the aspect of being suitable for improving the mass productivity of the cell culture substrate, a method of hydrophilizing treatment such as plasma treatment, UV treatment, corona treatment, or covering the substrate with a substance having cell proliferation is preferred, and a method of imparting cell proliferation to a part of the substrate by hydrophilizing treatment such as plasma treatment, UV treatment, corona treatment, etc. is further preferred, among which plasma treatment is particularly preferred.

[0122] The patterning method is not particularly limited, and the following methods can be cited: a method of hydrophilizing the desired shape by performing a plasma treatment, UV treatment, corona treatment, etc. under a state covered with a metal mask, a silicon mask, a surface protection film, etc.; a method of covering a cell-proliferating substance on a substrate in a desired shape by photolithography or inkjet. In order to improve the mass productivity of the cell culture substrate, it is preferred to perform a plasma treatment, UV treatment, corona treatment, etc. hydrophilizing treatment under a state where a surface protection film with holes formed by laser processing is attached to the substrate.

[0123] In addition, as a method for patterning by a method other than the above-mentioned step (1), a method of forming a region without cell proliferation on the surface of a substrate with cell proliferation may be used. As this method, for example, the following method can be cited: using a substrate with cell proliferation, or after imparting cell proliferation to the entire surface of a substrate without cell proliferation, a substance without cell proliferation is coated on the substrate in a desired shape by photolithography or inkjet method.

[0124] In the process (2) of the manufacturing method of the cell culture substrate of the present invention, a layer based on a stimulus-responsive substance is formed on the surface of the substrate. At this time, by forming a layer based on a stimulus-responsive substance on the surface of the substrate with a layer thickness of less than 100nm, even if the process (2) is performed after the process (1), the molecular chains of the stimulus-responsive substance are easily covered in a sparse state on the surface of the cell proliferation formed in the patterning process, which is suitable for maintaining the effect of the patterning while also giving stimulus responsiveness. In addition, by setting the layer thickness to more than 1nm, thereby giving sufficient stimulus responsiveness, it is suitable to manufacture a cell culture substrate that can quickly perform a spheroid formation process.

[0125] As a method for covering the aforementioned stimulus-responsive substance, the following methods can be performed alone or in combination: a method for forming a layer by covering the stimulus-responsive substance on the substrate by chemical bonding; a method for forming a layer by covering the stimulus-responsive substance on the substrate by physical interaction. That is, as a method based on chemical bonding, ultraviolet irradiation, electron beam irradiation, gamma ray irradiation, plasma treatment, corona treatment, etc. can be used. Furthermore, when the stimulus-responsive polymer and the substrate have suitable reactive functional groups, organic reactions commonly used such as free radical reactions, anionic reactions, and cationic reactions can be used. As a method based on physical interaction, a matrix with good compatibility and good coating properties with the stimulus-responsive polymer can be used as a medium and various known methods such as coating, brushing, dip coating, spin coating, rod coating, flow coating, spray coating, roller coating, air knife coating, blade coating, gravure coating, micro-gravure coating, and slit coating can be used.

[0126] As a method for covering the aforementioned stimulus-responsive substance, it is also preferred to cover the entire surface of the cell culture substrate with the stimulus-responsive substance. When the stimulus-responsive substance is covered, patterning is not performed, but the stimulus-responsive substance is covered using a commonly used coating method, so that the mass production of the cell culture substrate can be improved. In addition, by covering the entire surface of the cell culture substrate with the stimulus-responsive substance, the (A) region is given stimulus responsiveness, and the (B) region is also covered with the stimulus-responsive substance. By covering the (B) region with the stimulus-responsive substance, the cell adhesion of the (B) region can be reduced. Therefore, in the case of using a substrate with cell adhesion but not cell proliferation as a substrate, it is possible to achieve that the (B) region has cell adhesion only in the aforementioned patterning process, and by also covering the (B) region with the stimulus-responsive substance, the (B) region can be made into a region that also does not have cell adhesion, and it is easy to form a uniform spheroid of size and shape and is preferred. At this time, the difference between the coverage amount of the (A) region and the (B) region is preferably 1μg / cm 2 Below, more preferably 0.8 μg / cm 2 Below, particularly preferably 0.6 μg / cm 2 Below, most preferably 0.4 μg / cm 2 In addition, the coverage of the (A) region and the (B) region is preferably 0.1 to 10 μg / cm 2 , more preferably 0.5 to 7 μg / cm 2 , particularly preferably 1 to 5 μg / cm 2 , most preferably 2 to 4 μg / cm 2 .

[0127] In the method for producing a cell culture substrate of the present invention, the order of step (1) and step (2) may be either one or the other. From the perspective of reducing the effects of step (1) such as scratches on the surface of the layer of the stimuli-responsive substance, it is preferred that step (2) be performed after step (1).

[0128] The present invention also relates to a method for producing spheroids using the above-mentioned cell culture substrate. The above-mentioned method is characterized in that the spheroids are produced through the following steps (i) to (iii).

[0129] (i) A step of seeding cells on the aforementioned cell culture substrate.

[0130] (ii) a step of culturing the seeded cells to form colonies of cells adhered to the cell culture substrate.

[0131] (iii) A step of applying an external stimulus to cause the colonies to detach from the cell culture substrate to form cell spheroids.

[0132] Hereinafter, steps (i) to (iii) in the method for producing a spheroid of the present invention will be described in detail.

[0133] The process (i) in the method for manufacturing spheroids of the present invention is a process of using the aforementioned cell culture substrate and inoculating cells in the aforementioned cell culture substrate. In the present invention, "inoculating cells" means that a culture medium (hereinafter, referred to as "cell suspension") dispersed with cells is applied to a cell culture substrate or injected into a cell culture substrate, so that a cell suspension is contacted with a cell culture substrate. By using a cell culture substrate with a cell proliferation region, it is possible to culture cells in the step (ii) described later. In the case where the cell culture substrate does not have a cell proliferation region, cells cannot be cultured in the step (ii). In addition, by making the aforementioned cell proliferation region further have a stimulus-responsive region, colonies can be peeled off from the cell culture substrate and formed into spheroids by external stimulation in the step (iii) described later. In the case of not having stimulus-responsiveness, spheroids cannot be formed by external stimulation in the step (iii).

[0134] In the above steps (i) to (iii), the culture is carried out under conditions effective for maintaining the undifferentiated nature of the cells. There are no particular restrictions on the conditions effective for maintaining the undifferentiated nature, and examples thereof include setting the cell density at the start of the culture to the preferred range described below as the cell density at the time of inoculation, and carrying out the culture in the presence of a suitable liquid culture medium, etc. As a culture medium effective for maintaining the undifferentiated nature of the cells, for example, a culture medium to which one or more of insulin, transferrin, selenium, ascorbic acid, sodium bicarbonate, basic fibroblast growth factor, transforming growth factor β (TGFβ), CCL2, activin, and 2-mercaptomethanol, which are known factors for maintaining the undifferentiated nature of the cells, can be suitably used. From the perspective of being particularly suitable for maintaining the undifferentiated nature of the cells, it is further preferred to use a culture medium containing insulin, transferrin, selenium, ascorbic acid, sodium bicarbonate, basic fibroblast growth factor, and transforming growth factor β (TGFβ), and it is most preferred to use a culture medium to which basic fibroblast growth factor is added.

[0135] The type of the culture medium to which the basic fibroblast growth factor is added is not particularly limited. For example, commercially available products include DMEM (manufactured by Sigma-Aldrich Co. LLC), Ham's F12 (manufactured by Sigma-Aldrich Co. LLC), D-MEM / Ham's F12 (manufactured by Sigma-Aldrich Co. LLC), Primate ES Cell Medium (manufactured by ReproCELL Incorporated), StemFit AK02N (manufactured by AJINOMOTO CO., INC.), StemFit AK03 (manufactured by AJINOMOTO CO., INC.), mTeSR1 (manufactured by STEMCELL TECHNOLOGIES), TeSR-E8 (manufactured by STEMCELL TECHNOLOGIES), ReproNaive (manufactured by ReproCELL Incorporated), ReproXF (manufactured by ReproCELL Incorporated), ReproFF (manufactured by ReproCELL Incorporated), and ReproFF2 (manufactured by ReproCELL Incorporated). Incorporated), NutriStem (Biological Industries Ltd.), iSTEM (Takara Bio Inc.), GS2-M (TakaraBio Inc.), hPSC Growth Medium DXF (PromoCell Co., Ltd.), etc. From the perspective of being suitable for maintaining the undifferentiated state of cells, Primate ES Cell Medium (ReproCELL Incorporated), StemFit AK02N (AJINOMOTO CO., INC.) or StemFit AK03 (AJINOMOTO CO., INC.) is preferred, StemFit AK02N (AJINOMOTO CO., INC.) or StemFit AK03 (AJINOMOTO CO., INC.) is more preferred, and StemFit AK02N (AJINOMOTO CO., INC.) is particularly preferred.

[0136] In the above step (i), the method of inoculating cells is not particularly limited, and it can be performed, for example, by injecting a cell suspension into a cell culture substrate. The cell density at the time of inoculation is not particularly limited, but in order to maintain and proliferate the cells, it is preferably 1.0×10 2 ~1.0×10 6 Cells / cm 2, and more preferably 5.0×10 2 ~5.0×10 5 Cells / cm 2 , particularly preferably 1.0×10 3 ~2.0×10 5 Cells / cm 2 , the most preferred is 1.2×10 3 ~1.0×10 5 Cells / cm 2 .

[0137] As the culture medium used in the aforementioned step (i), in addition, from the perspective of being suitable for maintaining cell survival, it is preferred to use a culture medium in which a Rho binding kinase inhibitor is further added to the aforementioned culture medium to which basic fibroblast growth factor is added. In particular, when human cells are used and the cell density of the human cells is low, the addition of a Rho binding kinase inhibitor is sometimes effective for maintaining the survival of human cells. As a Rho binding kinase inhibitor, for example, (R)-(+)-trans-N-(4-pyridyl)-4-(1-aminoethyl)-cyclohexanecarboxamide·2HCl·H2O (Y-27632 manufactured by Wako Pure Chemical Industries, Ltd.), fasudil hydrochloride (1-(5-Isoquinolinesulfonyl)homopiperazine hydrochloride) (HA1077 manufactured by Wako Pure Chemical Industries, Ltd.) can be used. The concentration of the Rho-binding kinase inhibitor added to the culture medium is within a range that is effective for maintaining the survival of human cells and does not affect the undifferentiated state of human cells, preferably 1 μM to 50 μM, more preferably 3 μM to 20 μM, further preferably 5 μM to 15 μM, and most preferably 8 μM to 12 μM.

[0138] Soon after the start of the above step (i), cells begin to adhere to the cell culture substrate.

[0139] In step (ii) of the method for producing spheroids of the present invention, the seeded cells are cultured at a temperature of preferably 30 to 42°C, more preferably 32 to 40°C, particularly preferably 36 to 38°C, and most preferably 37°C, from the perspective of maintaining the proliferation ability, physiological activity, and function of the cells.

[0140] Preferably, the initial culture medium replacement is performed 22 to 26 hours after the start of the aforementioned step (ii). Preferably, the second culture medium replacement is performed 48 to 72 hours thereafter, and then the culture medium replacement is performed every 24 to 48 hours. During this period, cells proliferate to form flat cell masses called colonies. Colonies are a state of adhesion to the cell culture substrate. Continue to culture until the size of the colony becomes about the size of the (A) area, and then enter step (iii).

[0141] In step (iii) of the method for producing spheroids of the present invention, an external stimulus is applied to the cell culture substrate on which the cells are cultured, so that at least a portion of the aforementioned colony is peeled off from the cell culture substrate. At this time, by gradually peeling off from the periphery of the colony, the colony is folded into a round block, and a spheroid with a uniform shape is easily formed. In the case where a colony is peeled off from the substrate on its entire surface, a suspended spheroid can be obtained. In addition, by peeling off only the outer periphery of the colony from the substrate without peeling off the center of the colony, a spheroid adhering to the substrate can be formed. When cooling is used as an external stimulus, in order to peel off the cells in a short time and reduce the damage caused by cooling, the temperature during cooling is preferably 0 to 30°C, more preferably 3 to 25°C, and further preferably 5 to 20°C. In addition, in order to reduce damage to the cells, the cooling time is preferably 120 minutes or less, more preferably 60 minutes or less, particularly preferably 30 minutes or less, and most preferably 15 minutes or less.

[0142] The method for cooling the cell culture substrate in the aforementioned step (iii) is not particularly limited, and for example, the following methods can be used: a method of cooling the cell culture substrate in a refrigerator; a method of cooling the cell culture substrate on a cold plate; a method of replacing the cell culture substrate with a cooled culture medium or buffer and leaving it to stand for a predetermined time, etc.

[0143] In addition, in the aforementioned step (iii), in order to peel off the cells in a short time and reduce the damage caused by external stimulation, a step of generating convection in the liquid containing the cultured cells may also be included. The method of generating convection is not particularly limited, and examples thereof include a method of mechanically generating forced convection in the liquid by pipetting the culture liquid and using a pump, a stirring blade, etc.

[0144] As for the spheroids produced by the spheroid production method of the present invention, from the perspective of being suitable for uniformly treating all cells in the culture process after spheroid formation such as differentiation induction, the deviation of the particle size of the spheroids (standard deviation of the particle size / average particle size) is preferably 20% or less, more preferably 15% or less, particularly preferably 10% or less, and most preferably 5% or less.

[0145] Example

[0146] Below, enumerate the mode for implementing the present invention to describe the present invention in detail, but it is to be used to illustrate the example of the present invention, and is not used to limit the present invention to the following content. In addition, can be implemented in the scope of the gist of the present invention with suitable changes. It should be noted that, as long as there is no special statement, reagent uses commercially available products.

[0147] <Polymer composition>

[0148] The results were analyzed by proton nuclear magnetic resonance spectroscopy (1H-NMR) using a nuclear magnetic resonance measuring apparatus (manufactured by JEOL Ltd., trade name JNM-GSX400) or carbon nuclear magnetic resonance spectroscopy ( 13 C-NMR) spectral analysis.

[0149] <Polymer molecular weight and molecular weight distribution>

[0150] The weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) were measured by gel permeation chromatography (GPC). The GPC apparatus used HLC-8320GPC manufactured by Tosoh Corporation, and two TSKgel Super AWM-H manufactured by Tosoh Corporation were used as columns. The column temperature was set to 40°C, and the eluent was measured using 1,1,1,3,3,3-hexafluoro-2-isopropanol containing 10mM sodium trifluoroacetate or N,N-dimethylformamide containing 10mM lithium bromide. The measurement sample was prepared at 1.0 mg / mL and measured. The molecular weight standard curve used polymethyl methacrylate (manufactured by Polymer Laboratories Ltd.) with a known molecular weight.

[0151] <Polymer layer thickness>

[0152] The thickness of the polymer layer covering the substrate was measured using an AFM device (SPM-9600 manufactured by Shimadzu Corporation). BL-AC40TS-C2 cantilever was used, and the surface was scratched with tweezers to measure the depth of the scratch to measure the thickness of the polymer layer.

[0153] [Example 1]

[0154] 0.40 g (0.1 mmol) of 4-cyano-4-[(dodecylsulfanylthiocarbonyl)thio]pentanoic acid, 7.11 g (50 mmol) of n-butyl methacrylate, and 33 mg (0.2 mmol) of azobis(isobutyronitrile) were added to a test tube and dissolved in 50 mL of 1,4-dioxane. After degassing by nitrogen bubbling for 30 minutes, the mixture was reacted at 70°C for 24 hours. After the reaction was completed, the reaction solvent was distilled off under reduced pressure using a rotary evaporator, and the reaction solution was concentrated. The concentrated solution was injected into 250 mL of methanol, and the precipitated yellow oily substance was recovered and dried under reduced pressure to obtain an n-butyl methacrylate polymer.

[0155] Add 0.9 g (0.3 mmol) of the above-mentioned n-butyl methacrylate polymer, 8.14 g (72 mmol) of N-isopropylacrylamide, and 5 mg (0.03 mmol) of azobisisobutyronitrile to a test tube and dissolve in 15 mL of 1,4-dioxane. After degassing by nitrogen bubbling for 30 minutes, react at 65°C for 17 hours. After the reaction is completed, dilute the reaction solvent with acetone, inject into 500 mL of hexane, recover the precipitated solid and dry it under reduced pressure. In addition, dissolve it in acetone again, inject into 500 mL of pure water, recover the precipitated solid and dry it under reduced pressure to obtain a diblock copolymer of N-isopropylacrylamide and n-butyl methacrylate.

[0156] A culture dish (manufactured by AS ONE CORPORATION., material: polystyrene) with a diameter of 10 cm and without cell proliferation was covered with a metal mask having a plurality of circular holes with a diameter of 0.3 mm, and a plasma irradiation device (manufactured by VACUUM DEVICE, trade name: Plasma ion bomber PIB-20) was used to perform plasma treatment from the metal mask (under a gas pressure of 20 Pa, a conductive current of 20 mA, and an irradiation time of 10 seconds), thereby patterning the area in which cell proliferation is formed. The aforementioned block copolymer was dissolved in ethanol to prepare a 0.6wt% solution, and the solution was spin-coated at 2000 rpm for 60 seconds on the surface of the patterned substrate. After drying at room temperature for 1 hour, a substrate covered with the block copolymer was prepared.

[0157] It should be noted that the structural unit ratio of the block copolymer is 4 wt% of n-butyl methacrylate and 96 wt% of N-isopropylacrylamide, and the molecular weight is Mn77,000. The thickness of the layer of the block copolymer covering the polystyrene petri dish is 25 nm.

[0158] A culture medium, StemFitAK02N (manufactured by AJINOMOTO CO., INC.), was added to the substrate patterned and covered with the block copolymer at a volume of 0.2 mL / cm. 2 , and then 1300 pieces / cm 2 Human iPS cell line 201B7 was added, and iMatrix-511 solution (manufactured by Nippi, Inc.) was added at a concentration of 2.5 μL / mL. The cells were cultured at 37°C and a CO2 concentration of 5%. In addition, Y-27632 (manufactured by Wako Pure Chemical Industries, Ltd.) (concentration 10 μM) was added to the culture medium 24 hours after cell inoculation.

[0159] After 24 hours, 96 hours, and 144 hours from the cell inoculation, the cell state was observed using a phase contrast microscope to confirm that the cells adhered and proliferated along the patterned shape in any case, and replaced with a new aforementioned culture medium. After 144 hours from the cell inoculation and after the culture medium was replaced, the substrate was cooled at room temperature for 20 minutes and observed again using a phase contrast microscope. The following state was observed: with cooling, the colony began to peel off from the surroundings, and a spheroid was formed on the substrate. Furthermore, by knocking the side of the substrate with the hand to peel off the spheroid from the substrate, a spheroid with uniform size and spherical shape can be recovered.

[0160] [Example 2]

[0161] As the metal mask in Example 1, a metal mask having a plurality of rectangular holes of 0.5 mm×1 mm was used, and a cell culture substrate was prepared in the same manner as in Example 1 otherwise.

[0162] Cell culture was performed in the same manner as in Example 1. After 24 hours, 96 hours, and 144 hours from the cell inoculation, the cell state was observed using a phase contrast microscope. It was confirmed that the cells adhered and proliferated along the patterned shape in any case, and the culture medium was replaced with a new one. After 144 hours from the cell inoculation and after the culture medium was replaced, the substrate was cooled at room temperature for 20 minutes, and the side of the substrate was tapped by hand. Spheroids of uniform size and elongated coiled shape were recovered.

[0163] [Example 3]

[0164] As the metal mask in Example 1, a metal mask having a plurality of circular holes with a diameter of 0.5 mm was used, and a cell culture substrate was prepared in the same manner as in Example 1 otherwise.

[0165] Cell culture was performed in the same manner as in Example 1. After 24 hours, 96 hours, and 144 hours from cell inoculation, the cell state was observed using a phase contrast microscope. It was confirmed that the cells adhered and proliferated along the patterned shape in any case, and the culture medium was replaced with a new one. After 144 hours from cell inoculation and after the culture medium was replaced, the substrate was cooled at room temperature for 20 minutes and cultured again at 37°C for 1 hour. As the cooling progressed, the colonies began to peel off from the periphery to form spheroids, and spheroids adhered to the substrate could be obtained.

[0166] [Example 4]

[0167] As the metal mask in Example 1, a metal mask having a plurality of circular holes with a diameter of 0.2 mm was used. In addition, a VUV Aligner (trade name) manufactured by Ushio Inc. was used instead of the plasma ion bomber PIB-20. A cell culture substrate was prepared in the same manner as in Example 1 except that

[0168] Cell culture was carried out in the same manner as in Example 1. After 24 hours, 96 hours, and 144 hours from the cell inoculation, the cell state was observed using a phase contrast microscope to confirm that the cells adhered and proliferated along the patterned shape in any case, and the culture medium was replaced with a new one. After 144 hours from the cell inoculation and after the culture medium was replaced, the substrate was cooled at room temperature for 20 minutes and the side of the substrate was tapped by hand. Spheroids of uniform size and spherical shape can be recovered. The particle size of the recovered spheroids was measured, and the deviation of the particle size (standard deviation of the particle size / average particle size) was obtained. The result was 6.6%, which was a small deviation.

[0169] [Example 5]

[0170] As the metal mask in Example 1, a metal mask having a plurality of circular holes with a diameter of 0.5 mm was used. In addition, a VUV Aligner (trade name) manufactured by Ushio Inc. was used instead of the plasma ion bomber PIB-20. A cell culture substrate was prepared in the same manner as in Example 1 except that

[0171] Cell culture was carried out in the same manner as in Example 1. After 24 hours, 96 hours, and 144 hours from the cell inoculation, the cell state was observed using a phase contrast microscope to confirm that the cells adhered and proliferated along the patterned shape in any case, and the culture medium was replaced with a new one. After 144 hours from the cell inoculation and the culture medium was replaced, the substrate was cooled at room temperature for 20 minutes, the side of the substrate was tapped by hand to peel off the cells, and then cultured for another day. Spheroids of uniform size and spherical shape can be recovered. The particle size of the recovered spheroids was measured, and the deviation of the particle size (standard deviation of the particle size / average particle size) was calculated. The result was 14.2%, which was a small deviation.

[0172] [Example 6]

[0173] Instead of the metal mask in Example 1, a mask having a plurality of circular holes with a diameter of 0.2 mm was formed on a surface protection film (E-MASK manufactured by Nitto Denko) by laser processing, and the surface protection film was attached to the substrate and plasma treated, and then the surface protection film was peeled off. Then, the block copolymer was covered in the same manner as in Example 1 to prepare a cell culture substrate.

[0174] Cell culture was carried out in the same manner as in Example 1. After 24 hours, 96 hours, and 144 hours from the cell inoculation, the cell state was observed using a phase contrast microscope to confirm that the cells adhered and proliferated along the patterned shape in any case, and the culture medium was replaced with a new one. After 144 hours from the cell inoculation and after the culture medium was replaced, the substrate was cooled at room temperature for 20 minutes and the side of the substrate was tapped by hand. Spheroids of uniform size and spherical shape can be recovered. The particle size of the recovered spheroids was measured, and the deviation of the particle size (standard deviation of the particle size / average particle size) was obtained. The result was 4.2%, which was a small deviation.

[0175] [Example 7]

[0176] As the metal mask in Example 1, a metal mask having a plurality of circular holes with a diameter of 0.2 mm was used, and a cell culture substrate was prepared in the same manner as in Example 1 otherwise.

[0177] The atomic force microscope image of the prepared cell culture substrate was measured, and the (A) region had a region (A2) with a diameter of about 90 nm and other regions with a large amount of N-isopropylacrylamide polymer. In addition, the (B) region also had a region (B2) with a diameter of about 90 nm and other regions with a large amount of N-isopropylacrylamide polymer.

[0178] Cell culture was carried out in the same manner as in Example 1. After 24 hours, 96 hours, and 144 hours from the cell inoculation, the cell state was observed using a phase contrast microscope to confirm that the cells adhered and proliferated along the patterned shape in any case, and the culture medium was replaced with a new one. After 144 hours from the cell inoculation and after the culture medium was replaced, the substrate was cooled at room temperature for 20 minutes and the side of the substrate was tapped by hand. Spheroids of uniform size and spherical shape can be recovered. The particle size of the recovered spheroids was measured, and the deviation of the particle size (standard deviation of the particle size / average particle size) was obtained. The result was 4.5%, which was a small deviation.

[0179] [Example 8]

[0180] As the metal mask in Example 1, a metal mask having a plurality of circular holes with a diameter of 0.2 mm was used, and the synthesis and coating of the block copolymer were performed by the following method.

[0181] 0.40 g (0.1 mmol) of 4-cyano-4-[(dodecylsulfanylthiocarbonyl)thio]pentanoic acid, 7.11 g (50 mmol) of n-butyl methacrylate, and 33 mg (0.2 mmol) of azobis(isobutyronitrile) were added to a test tube and dissolved in 50 mL of 1,4-dioxane. After degassing by nitrogen bubbling for 30 minutes, the mixture was reacted at 70°C for 24 hours. After the reaction was completed, the reaction solvent was distilled off under reduced pressure using a rotary evaporator, and the reaction solution was concentrated. The concentrated solution was injected into 250 mL of methanol, and the precipitated yellow oily substance was recovered and dried under reduced pressure to obtain an n-butyl methacrylate polymer.

[0182] Add 0.9 g (0.3 mmol) of the above-mentioned n-butyl methacrylate polymer, 0.26 g (2.4 mmol) of N-isopropylacrylamide, and 5 mg (0.03 mmol) of azobisisobutyronitrile to a test tube and dissolve in 15 mL of 1,4-dioxane. After degassing by nitrogen bubbling for 30 minutes, react at 65°C for 17 hours. After the reaction is completed, dilute the reaction solvent with acetone, inject into 500 mL of hexane, recover the precipitated solid and dry under reduced pressure. In addition, dissolve in acetone again, inject into 500 mL of pure water, recover the precipitated solid and dry under reduced pressure to obtain a copolymer of N-isopropylacrylamide and n-butyl methacrylate.

[0183] A culture dish (manufactured by AS ONE CORPORATION., material: polystyrene) with a diameter of 10 cm and without cell proliferation was covered with a metal mask having a plurality of circular holes with a diameter of 0.2 mm, and a plasma irradiation device (manufactured by VACUUM DEVICE, trade name: Plasma ion bomber PIB-20) was used to perform plasma treatment from the metal mask (under a gas pressure of 20 Pa, a conductive current of 20 mA, and an irradiation time of 10 seconds), thereby patterning the area where cell proliferation is formed. The aforementioned block copolymer was dissolved in ethanol to prepare a 1wt% solution, and the solution was spin-coated at 2000 rpm for 60 seconds on the surface of the patterned substrate. After immersion in pure water for 1 hour, it was dried at room temperature for 24 hours to prepare a substrate covered with a block copolymer.

[0184] It should be noted that the structural unit ratio of the block copolymer is 50 wt% of n-butyl methacrylate and 50 wt% of N-isopropylacrylamide, and the molecular weight is Mn 0.6000. The thickness of the layer of the block copolymer covering the polystyrene petri dish is 50 nm.

[0185] The atomic force microscope images of the prepared cell culture substrate were measured, and it was confirmed that the regions (A) and (B) were uniform.

[0186] Cell culture was carried out in the same manner as in Example 1. After 24 hours, 96 hours, and 144 hours from the cell inoculation, the cell state was observed using a phase contrast microscope to confirm that the cells adhered and proliferated along the patterned shape in any case, and the aforementioned culture medium was replaced with a new one. After 144 hours from the cell inoculation and after the culture medium was replaced, the substrate was cooled at room temperature for 20 minutes, and the side of the substrate was tapped by hand, but the cells were not peeled off, so the peeling was performed by pipetting 20 times. Spheroids with uniform size and elongated curled shapes can be recovered. The particle size of the recovered spheroids was measured, and the deviation of the particle size (standard deviation of the particle size / average particle size) was calculated. The result was 14.6%, which is small, but larger than that of Example 7.

[0187] [Comparative Example 1]

[0188] A cell culture substrate was prepared in the same manner as in Example 1 except that the plasma treatment in Example 1 was not performed. Since there was no cell proliferation region, the iPS cells died 24 hours after seeding and spheroids could not be formed.

[0189] [Comparative Example 2]

[0190] In Example 1, the cell culture substrate was prepared in the same manner as in Example 1 without coating with block copolymer. Since there was no stimulus-responsive region, the colonies were not detached from the substrate and spheroids could not be recovered. In addition, the shapes of the colonies were not uniform.

[0191] [Comparative Example 3]

[0192] The cell culture substrate was prepared in the same manner as in Example 1 except that the whole area of ​​the substrate was subjected to plasma treatment without patterning as in Example 1. The size and shape of the colonies were not uniform. The particle size of the recovered spheroids was measured, and the deviation of the particle size (standard deviation of the particle size / average particle size) was calculated. The result was 36.5%, which was a large deviation.

[0193] [Comparative Example 4]

[0194] As the metal mask in Example 1, a metal mask having a plurality of circular holes with a diameter of 4 mm was used, and the cell culture substrate was prepared in the same manner as in Example 1. The size and shape of the colonies were not uniform. The particle size of the recovered spheroids was measured, and the deviation of the particle size (standard deviation of the particle size / average particle size) was calculated. The result was 31.1%, which was a large deviation.

[0195] [Comparative Example 5]

[0196] A commercially available cell culture container for spheroid formation (AGC TECHNO GLASS Co., Ltd., trade name EZSPHERE) having a surface with a concavoconvex shape and a cell non-adhesive surface was used, and cell inoculation was performed in the same manner as in Example 1, and spheroids were formed by suspension culture. The spheroids formed were roughly spherical, but a large number of aggregates formed by agglomeration of multiple spheroids were observed. The particle size of the recovered spheroids was measured, and the deviation of the particle size (standard deviation of the particle size / average particle size) was calculated, and the result was 22.3%, which was a large deviation.

[0197] [Reference example]

[0198] The zeta potential of the (A) region and the (B) region in Example 1 was measured by the following method. A plasma irradiation device (manufactured by VACUUM DEVICE, trade name Plasma ion bomber PIB-20) was used to treat the entire surface of a culture dish with a diameter of 10 cm that does not have cell proliferation (under a gas pressure of 20Pa, a conductive current of 20mA, and an irradiation time of 10 seconds), thereby treating the entire surface of the substrate with plasma. The block copolymer was covered on the plasma-treated substrate and the substrate that was not subjected to the aforementioned plasma treatment by the same method as in Example 1, thereby preparing a sample in which the entire surface of the substrate was the (A) region of Example 1, and a sample in which the entire surface of the substrate was the (B) region of Example 1. The zeta potential of these substrates was measured (using SurPASS manufactured by Anton Paar Co., Ltd.), and the zeta potential of the (B) region was 8mV greater than that of the (A) region.

[0199] [Table 1]

[0200]

[0201] Although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention.

[0202] It should be noted that the entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2018-194841 filed on October 16, 2018 are incorporated herein as the contents of the specification of the present invention.

[0203] Description of Reference Numerals

[0204] A (A) area

[0205] B (B) Area

[0206] 1. Substrate

[0207] 2 Stimuli-responsive polymers

[0208] 10 Cell culture substrate

[0209] 20 cells

[0210] 21 colonies

[0211] 22 spheroids

Claims

1. A cell culture substrate, characterized in that The invention relates to a cell culture substrate comprising a substrate and a stimuli-responsive polymer covering the substrate, wherein the stimuli-responsive polymer is a block copolymer having a water-insoluble block segment and a stimuli-responsive block segment, wherein the cell culture substrate comprises the following two regions (A) and (B), and comprises a substrate and a layer comprising the stimuli-responsive polymer formed on the entire surface of the substrate, wherein the substrate comprises two regions: a region having cell proliferation and a region having no cell proliferation. (A) has cell proliferation and stimulus response, and the area is 0.001 to 5 mm 2 The island-like area (B) a region adjacent to the region (A) and not having cell proliferation, The layer thickness is 25 nm or more and 50 nm or less, The ratio of average roughness of the surface of the layer to layer thickness is 0.3 or more and 1 or less.

2. The cell culture substrate according to claim 1, characterized in that The region (A) includes the following two regions (A1) and (A2), and the region (B) includes the following two regions (B1) and (B2). (A1) Cell proliferative area (A2) Stimulus-responsive area (B1) Substrate bonding area (B2) Stimulus-responsive area.

3. The cell culture substrate according to claim 1 or 2, characterized in that The (A) region is a region in which temperature-responsive regions with a diameter of 10 to 500 nm are dispersed in a cell-proliferative region, or a region in which cell-proliferative regions with a diameter of 10 to 500 nm are dispersed in a temperature-responsive region not having cell-proliferative activity.

4. The cell culture substrate according to claim 1 or 2, characterized in that: The ratio of average roughness / layer thickness of the layer is 0.5 or more and 1 or less.

5. The cell culture substrate according to claim 4, characterized in that The stimulus-responsive polymer is a block copolymer having a water-insoluble block segment and more than 90 wt % of a stimulus-responsive block segment.

6. The cell culture substrate according to claim 1 or 2, characterized in that: The (A) region is a plasma processing region.

7. The cell culture substrate according to claim 1 or 2, characterized in that: It is used to form spheroids of pluripotent stem cells.

8. The method for producing a cell culture substrate according to any one of claims 1 to 7, characterized in that: It has the following steps (1) and (2): (1) Forming a cell-proliferative region with an area of ​​0.001 to 5 mm on the surface of a substrate without cell-proliferative activity 2 The process of the island-shaped area, (2) A step of forming a layer based on a stimuli-responsive substance on the surface of a substrate.

9. The method for producing a cell culture substrate according to claim 8, characterized in that: In the step (1), a region having cell proliferation ability is formed on the surface of the substrate having no cell proliferation ability by any one of plasma treatment, UV treatment, and corona treatment or a combination of two or more thereof.

10. The method for producing a cell culture substrate according to claim 8 or 9, characterized in that: The substrate used in the step (1) has cell adhesiveness but does not have cell proliferation property.

11. The method for producing a cell culture substrate according to claim 8 or 9, characterized in that: The step (1) comprises the step of laminating a surface protection film on a substrate, wherein the surface protection film has an area of ​​0.001 to 10 mm 2 hole.

12. A method for producing a spherical body, characterized in that: It goes through the following steps (i) to (iii): (i) a step of seeding cells on the cell culture substrate according to any one of claims 1 to 7 or the cell culture substrate obtained by the production method according to any one of claims 8 to 11, (ii) a step of culturing the seeded cells to form colonies of cells adhered to the cell culture substrate, (iii) a step of applying an external stimulus to detach at least a portion of the colony from the cell culture substrate to form a cell spheroid.