Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal display element
By using polymers with specific side chain structures in the liquid crystal representation element to form a liquid crystal orientation film, the problems of insufficient response speed of the liquid crystal representation element and difficulty in processing compounds in the prior art are solved, and efficient liquid crystal representation effect is achieved.
Patent Information
- Application Number
- CN201980070307.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-10-26
- Filing Date
- 2019-10-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2039-10-24
AI Technical Summary
The sulfide-based compounds used in the existing liquid crystal display element have strong odor and difficulty in processing, and the low molecular weight components of the vinyl ether compound may cause poor expression, and the response speed of the liquid crystal display element in the vertical orientation is insufficient, which is difficult to meet. High-speed response and efficient inclination angle impart the demand.
A liquid crystal alignment agent is used, which contains a polymer with a specific side chain structure. By combining specific side chains 1, side chain 2 and side chain 3, a specific copolymer or polymer mixture is formed, which optimizes the performance of the liquid crystal alignment film and improves the The liquid crystal represents the field angle, response speed and contrast of the element.
The liquid crystal representation element has a wide field of view angle, fast response speed and high contrast ratio, which meets the needs of high-speed response and efficient inclination angle, while avoiding the difficulty in handling sulfide-based compounds and the residual problems of vinyl ether compounds.
Smart Images

Figure CN112888996B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a liquid crystal alignment agent, a liquid crystal alignment film, and a liquid crystal display element. Background Art
[0002] Liquid crystal display elements are widely used in televisions, large monitors, personal computers, mobile phones, smart phones, etc. In recent years, opportunities for using liquid crystal display elements under high temperature and high humidity conditions have also increased in car navigation devices, meters, industrial equipment installed outdoors, and display parts of measuring instruments installed in vehicles.
[0003] Among them, vertical alignment liquid crystal display elements have been widely used in recent years due to their wide viewing angle, fast response speed and high contrast. For the vertical alignment method, the following technology is known: adding a photopolymerizable compound to a liquid crystal composition in advance, using it together with a liquid crystal alignment film such as a polyimide system, applying voltage to the liquid crystal unit while irradiating ultraviolet rays, thereby giving a tilt angle to the film surface and accelerating the response speed of the liquid crystal (see Patent Document 1 and Non-Patent Document 1).
[0004] Therefore, in order to promote the reaction of the above-mentioned photopolymerizable compounds, a composition for a liquid crystal display element for forming at least one of the liquid crystal layer and the liquid crystal orientation layer of a liquid crystal display element has been proposed, which contains a compound having a structure capable of exhibiting a chain transfer function (see Patent Document 2).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. WO2011 / 132752
[0008] Patent Document 2: Japanese Patent Application Publication No. 2014-186301
[0009] Non-patent literature
[0010] Non-patent document 1: K. Hanaoka, SID04 DIGEST, P. 1200-1202 Summary of the invention
[0011] Problem that the invention aims to solve
[0012] However, the sulfide-based compound disclosed as a compound having a structure capable of exhibiting a chain transfer function contained in the composition for liquid crystal display elements in Patent Document 2 has a strong odor and problems in handling, and therefore cannot be produced in large quantities industrially. In addition, the vinyl ether disclosed as a compound having a structure capable of exhibiting a chain transfer function, i.e., benzyl isopropenyl ether, is a low molecular weight component, and unreacted components remain in the liquid crystal alignment film, which may cause poor display of the liquid crystal display element.
[0013] In recent years, as the quality of liquid crystal display elements has been improved, the response speed of vertical alignment liquid crystal display elements has been required to be further increased, and the photopolymerizable compound has been required to react efficiently and have the ability to provide a tilt angle.
[0014] Solutions for solving problems
[0015] The present invention has been achieved in response to the above-mentioned needs and has the following aspects.
[0016] A liquid crystal aligning agent, characterized in that it contains a polymer having a side chain represented by the following formula (1) and a side chain represented by the following formula (2).
[0017]
[0018] (Where R 1c , R 2c Each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. c Represents a single bond or -CO-. Ar 1 represents phenylene, naphthylene or biphenylene. 1c , T 2c Each independently represents a single bond, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH2O-, -N(CH3)-, -CON(CH3)- or -N(CH3)CO-. c represents a single bond, an alkylene group having 1 to 20 carbon atoms which may be substituted with a fluorine atom, a divalent aromatic ring group having 6 to 12 carbon atoms, a divalent alicyclic group having 3 to 8 carbon atoms, or a divalent heterocyclic group selected from pyrrole, imidazole, pyridine, pyrimidine, pyrazine, pyridazine, triazine, indole, quinoline, carbazole, thiazole, purine, tetrahydrofuran and thiophene. n represents an integer of 1 to 4. * represents a bonding position to an adjacent atom. )
[0019]
[0020] (Q represents a group selected from the following formulae (q-1) to (q-4) (R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, R3 represents -CH2-, -NR-, -O- or -S-, and * represents a bond to an adjacent carbon atom.) R1r , R 2r Each independently represents an alkyl group or alkoxy group having 1 to 10 carbon atoms, a benzyl group or a phenethyl group. 2 represents a divalent aromatic hydrocarbon group selected from phenylene, naphthylene and biphenylene, and the organic group may be substituted thereon, and the hydrogen atom may be substituted with a halogen atom. 1r , T 2r Each independently represents a single bond, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH2O-, -N(CH3)-, -CON(CH3)- or -N(CH3)CO-. r represents a single bond, an alkylene group having 1 to 20 carbon atoms which may be substituted with a fluorine atom, a divalent aromatic ring group having 6 to 12 carbon atoms, a divalent alicyclic group having 3 to 8 carbon atoms, or a divalent heterocyclic group selected from pyrrole, imidazole, pyridine, pyrimidine, pyrazine, pyridazine, triazine, indole, quinoline, carbazole, thiazole, purine, tetrahydrofuran and thiophene. * represents the bonding position to the adjacent atom. )
[0021]
[0022] Effects of the Invention
[0023] The liquid crystal display element having a liquid crystal aligning film obtained from the liquid crystal aligning agent of the present invention has a wide viewing angle, a high response speed, and a large contrast. DETAILED DESCRIPTION
[0024] The liquid crystal aligning agent of the present invention contains a polymer having a side chain represented by the following formula (1) (hereinafter also referred to as a specific side chain 1) and a side chain represented by the following formula (2) (hereinafter also referred to as a specific side chain 2).
[0025]
[0026]
[0027] In the above formula (1), R 1c , R 2c , Y c ,Ar 1 , T 1c , T 2c , A c and n have the same meanings as described above.
[0028] Among them, R 1c , R 2c Each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and among them, R 1c and R 2cEach independently represents an alkyl group having 1 to 10 carbon atoms. The alkyl group having 1 to 10 carbon atoms is preferably a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a tert-pentyl group, a hexyl group, a heptyl group, an octyl group, an isooctyl group, a 2-ethylhexyl group, a tert-octyl group, a nonyl group, an isononyl group, a decyl group or an isodecyl group.
[0029] In addition, Ar 1 Preferably, it is phenylene or biphenylene. Preferably, T 1c , T 2c Each is independently a single bond, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH- or -CH2O-.
[0030] A c It is preferably a single bond, an alkylene group having 1 to 20 carbon atoms which may be substituted with a fluorine atom, a divalent aromatic ring group having 6 to 12 carbon atoms, or a divalent alicyclic group having 3 to 8 carbon atoms.
[0031] Furthermore, n is preferably 1-2.
[0032] As -Ar in formula (1) 1 -(Y c -CHR 1c R 2c ) n Preferred structures include the following (ch-1) to (ch-6).
[0033]
[0034] (R 1c , R 2c The same meaning as the above formula (1).
[0035] In the above formula (2), Q and R 1r , R 2r ,Ar 2 , T 1r , T 2r , A r The meaning is as described above.
[0036] Among them, Ar 2 From the viewpoint of high photoreactivity, phenylene or biphenylene is preferred. 1r , T 2r Each is independently a single bond, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH- or -CH2O-.
[0037] A r It is preferably a single bond, an alkylene group having 1 to 20 carbon atoms which may be substituted with a fluorine atom, a divalent aromatic ring group having 6 to 12 carbon atoms, or a divalent alicyclic group having 3 to 8 carbon atoms.
[0038] As R constituting the above formula (1) 1c , R 2c , R in the above formula (2) 1r and R 2r The alkyl group may be a straight chain or a branched chain. Specific examples thereof include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, isopentyl, tert-pentyl, hexyl, heptyl, octyl, isooctyl, 2-ethylhexyl, tert-octyl, nonyl, isononyl, decyl, isodecyl, cyclopentyl, cyclopentylmethyl, cyclopentylethyl, cyclohexyl, cyclohexylmethyl, and cyclohexylethyl.
[0039] As A constituting the above formula (1) c , A in the above formula (2) r The alkylene group having 1 to 20 carbon atoms may be any of a straight chain, a branched chain or a cyclic chain. Specific examples thereof include methylene, ethylene, n-propylene, isopropylene, cyclopropylene, 1-methyl-cyclopropylene, 2-methyl-cyclopropylene, 1,1-dimethyl-n-propylene, 1,2-dimethyl-n-propylene, 2,2-dimethyl-n-propylene, 1-ethyl-n-propylene, 1,2-dimethyl-cyclopropylene, 2,3-dimethyl-cyclopropylene, 1-ethyl-cyclopropylene, 2-ethyl-cyclopropylene, 1,1,2-trimethyl-n-propylene, 1,2,2-trimethyl- n-propylene, 1-ethyl-1-methyl-n-propylene, 1-ethyl-2-methyl-n-propylene, 2-n-propyl-cyclopropylene, 1-isopropyl-cyclopropylene, 2-isopropyl-cyclopropylene, 1,2,2-trimethyl-cyclopropylene, 1,2,3-trimethyl-cyclopropylene, 2,2,3-trimethyl-cyclopropylene, 1-ethyl-2-methyl-cyclopropylene, 2-ethyl-1-methyl-cyclopropylene, 2-ethyl-2-methyl-cyclopropylene, 2-ethyl-3-methyl-cyclopropylene and the like.
[0040] Among them, an alkylene group having 1 to 10 carbon atoms is preferred, and 1 to 3 carbon atoms is more preferred, and specifically, a methylene group, an ethylene group, or an n-propylene group is preferred.
[0041] As A constituting the above formula (1) c , A in the above formula (2) r The aromatic ring group having 6 to 12 carbon atoms includes a benzene ring, a biphenylene ring, a naphthalene ring and the like.
[0042] As A constituting the above formula (1) c , A in the above formula (2) r The alicyclic group having 3 to 8 carbon atoms includes a cyclopentane ring, a cyclohexane ring, and the like.
[0043] As -Ar in formula (1) 2 -CO-CR 1r R 2r Preferred structures of Q include formulae (ra-1) to (ra-6).
[0044] Among these, from the viewpoint of the reliability of the obtained liquid crystal display element, (ra-2) or (ra-3) is preferred.
[0045]
[0046] The polymer contained in the liquid crystal aligning agent of this invention may have the side chain represented by following formula (3) other than the specific side chain 1 and the specific side chain 2 (it may also be called a specific side chain 3 hereafter).
[0047]
[0048] In the above formula (3), l, m and n each independently represent an integer of 0 or 1. 1 Represents -(CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CH2O-, -CH2OCO-, -COO- or -OCO- or -(CH2) a1 -A1-(CH2) a2 -A2-, A1 is an oxygen atom or -COO-* (wherein the connecting bond with * is connected to (CH2) a2 bond), A2 is an oxygen atom or *-COO- (wherein the bond with * is connected to (CH2) a2 bonding), a1 is an integer of 0 or 1, and a2 is an integer of 1 to 10.
[0049] In addition, R 2 , R 3 and R 4 Each independently represents a phenylene group, a fluorine-containing phenylene group or a cycloalkylene group. 5 represents a linear alkyl group having 2 to 24 carbon atoms, a fluorinated alkyl group having 2 to 24 carbon atoms, an alkoxy group having 2 to 24 carbon atoms, an alkoxyalkyl group having 2 to 24 carbon atoms, or a structure having a steroid skeleton. 5 In the case of a linear alkyl group having 2 to 24 carbon atoms or a fluorinated alkyl group having 2 to 24 carbon atoms, l+m+n≥1 is satisfied, and in the case of a structure having a steroid skeleton, l, m, and n are 0, and R 1 Represents -(CH2) a-(a is an integer from 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CH2O-, -CH2OCO-, -COO- or -OCO-.
[0050] Specific examples of the structure having a steroid skeleton include a structure having a skeleton represented by the following formula (st).
[0051]
[0052] Preferred structures of the specific side chain 3 include the following formulae (S1-x1) to (S1-x7) and formula (S3-x).
[0053]
[0054] In the above formula, R 1 X represents a linear alkyl group having 2 to 24 carbon atoms, an alkoxy group having 2 to 24 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms. p Represents -(CH2) a -(a is an integer from 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CH2O-, -CH2OCO-, -COO- or -OCO-. A1 represents an oxygen atom or -COO-* (wherein the bond with * is the same as (CH2) a2 bond), A2 represents an oxygen atom or *-COO- (wherein the bond with * is connected to (CH2) a2 bond), a1 and a3 are each independently an integer of 0 or 1, a2 is an integer of 1 to 10, and Cy represents a 1,4-cyclohexylene group or a 1,4-phenylene group.
[0055]
[0056] In the above formula, X represents the above formula (X1) or (X2). Col represents at least one selected from the group consisting of the above formulas (Col1) to (Col4). G represents the above formula (G1) or (G2). * represents the position of bonding to other groups.
[0057] As more preferable structures of the formula (S3-x), the following formulas (S3-1) to (S3-6) are mentioned.
[0058]
[0059] <Specific polymers>
[0060] The specific polymer contained in the liquid crystal aligning agent of the present invention may be a polymer containing a unit having a specific side chain 1 and a unit having a specific side chain 2 (hereinafter also referred to as a specific copolymer), or may be a mixture containing a polymer having a specific side chain 1 and a polymer having a specific side chain 2 (hereinafter also referred to as a polymer mixture).
[0061] The specific copolymer may further contain a unit having a specific side chain 3 in addition to a unit having a specific side chain 1 and a unit having a specific side chain 2. In addition, the polymer mixture may be a mixture containing a polymer having a specific side chain 1 and a polymer having a specific side chain 2, wherein any of the polymers contains a unit having a specific side chain 3; or a mixture containing a polymer having a specific side chain 1, a polymer having a specific side chain 2, and a polymer having a specific side chain 3.
[0062] The specific copolymer may be a diamine having a specific side chain 1 and a polymer having a specific side chain 2, but is preferably a polymer having a skeleton selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane and poly(meth)acrylate. Among them, preferably, a polyamic acid formed by a polycondensation reaction of a diamine component containing a diamine having a specific side chain 1 and a diamine having a specific side chain 2 and a tetracarboxylic acid component and / or a polyimide formed by imidizing the polyamic acid.
[0063] The content ratio of the unit having the specific side chain 1 and the unit having the specific side chain 2 in the specific copolymer is preferably 5 / 95 to 95 / 5, more preferably 10 / 90 to 90 / 10 in terms of molar ratio (specific side chain 1 / specific side chain 2). When the ratio is within the above range, the light irradiation amount when imparting the tilt is reduced.
[0064] When the specific copolymer includes a unit having a specific side chain 3, the ratio of the unit having a specific side chain 1 and the unit having a specific side chain 2 is preferably 10 / 90 to 90 / 10, more preferably 10 / 90 to 80 / 20 in terms of molar ratio (specific side chain 3 / (specific side chain 1+specific side chain 2)). When the above ratio is within the above range, the liquid crystal alignment film has a high vertical orientation and the light irradiation amount when tilted is reduced.
[0065] The above-mentioned polymer mixture is preferably a polymer comprising a polyamic acid formed by a condensation reaction between a diamine component containing a diamine having a specific side chain 1 and a tetracarboxylic acid component and / or a polyimide formed by imidizing the polyamic acid; and a mixture of a polymer comprising a polyamic acid formed by a condensation reaction between a diamine component containing a diamine having a specific side chain 2 and a tetracarboxylic acid component and / or a polyimide formed by imidizing the polyamic acid.
[0066] The content ratio of the polymer having the specific side chain 1 and the polymer having the specific side chain 2 in the polymer mixture is preferably 10 / 90 to 90 / 10, more preferably 20 / 80 to 80 / 20 in terms of weight ratio (polymer 1 having the specific side chain 1 / polymer having the specific side chain 2). When the above ratio is within the above range, the light irradiation amount when the tilt is applied is reduced.
[0067] When obtaining the specific polymer of the present invention, that is, the above-mentioned specific copolymer or the above-mentioned polymer mixture, a preferred diamine having a specific side chain 1 used as a part of the raw materials thereof includes a diamine represented by the following formula (d-1).
[0068]
[0069] In the above formula (d-1), R 1c , R 2c , Y c ,Ar 1 , T 1c , T 2c , A c and n have the same meanings as in the above formula (1), including their preferred examples. 1c and R 2c The case where both groups are methyl groups is particularly preferred from the viewpoint of availability of raw materials and the like.
[0070] Preferred specific examples of the diamine represented by the formula (d-1) include the following formulas (1-a) to (1-j).
[0071]
[0072] When obtaining the specific polymer of the present invention, that is, the above-mentioned specific copolymer or the above-mentioned polymer mixture, a preferred diamine having a specific side chain 2 used as a part of the raw materials thereof includes a diamine represented by the following formula (d-2).
[0073]
[0074] In the above formula (d-2), R 1r , R 2r , Y r ,Ar 2 , T 1r , T 2r and A r The meanings of are the same as those in the aforementioned formula (2), including preferred examples thereof.
[0075] Preferred specific examples of the diamine represented by the formula (d-2) include the following formulas (2-a) to (2-d).
[0076]
[0077] When the specific polymer of the present invention is a polymer having a side chain represented by the following formula (3) in addition to the side chain represented by the above formula (1) and the side chain represented by the above formula (2), as the diamine component, a diamine represented by the following formula (d-3) is used in addition to the diamine represented by the above formula (d-1) and the diamine represented by the above formula (d-2).
[0078]
[0079] In the above formula (d-3), l, m, n and R 1 ~R 5 The definitions of are the same as those of the above formula (3) including respective preferred examples. z represents an integer of 1 to 2, and Y3 represents the following formula (Ar 3-1 )~(Ar 3-2 ) shown in the structure.
[0080]
[0081] In the above formula, A 3a represents a single bond or a divalent organic group having an aromatic group. 3b Indicates a trivalent group having an aromatic group. *1 indicates para-R 1 -(R 2 ) l -(R 3 ) m -(R 4 )nR 5 * represents the bonding position to -NH2, and *2 represents the bonding position to -NH2.
[0082] As A 3a The divalent organic group having an aromatic group in the formula (R1) may be, for example, a structure represented by the following formula (R1).
[0083] *3-X1-Q1-*2 (R1)
[0084] In the above formula, X1 includes a single bond, -O-, -C(CH3)2-, -NH-, -CO-, -NHCO-, -COO-, -(CH2) m -、-SO2-、-O-(CH2) m -O-, -OC(CH3)2-, -CO-(CH2) m -、-NH-(CH2) m -、-SO2-(CH2) m -、-CONH-(CH2) m -、-CONH-(CH2)m -NHCO-, -COO-(CH2) m -OCO-, etc. Q1 includes a group formed by removing two hydrogen atoms from an aromatic hydrocarbon having 6 to 20 carbon atoms, such as a benzene ring or a naphthalene ring. m is an integer of 1 to 8. *2 indicates a bonding position to -NH2, and *3 indicates a bonding position to a benzene ring.
[0085] As A 3b The trivalent organic group having an aromatic group in the formula (R2) may be, for example, a structure represented by the following formula (R2).
[0086]
[0087] In the above formula, X2 has the same meaning as X1 in formula (R1), and Q2 can be a group formed by removing three hydrogen atoms from an aromatic hydrocarbon having 6 to 20 carbon atoms such as a benzene ring or a naphthalene ring. 1 -(R 2 ) l -(R 3 ) m -(R 4 ) n -R 5 * represents the bonding position to -NH2, *3 represents the bonding position to the benzene ring.
[0088] Preferred specific examples of the diamine represented by the above formula (d-3) include diamines of the following formulas (V-1) to (V-13).
[0089]
[0090]
[0091] In the above formula, X v1 ~X v4 , X p1 ~X p8 Each independently represents -(CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CH2O-, -CH2OCO-, -COO- or -OCO-. X V6 ~X V7 , X s1 ~X s4 Each independently represents -O-, -COO- or -OCO-. a ~X f Represents a single bond, -O-, -NH- or -O-(CH2) m -O-.R v1 ~R v4 , R1a ~R 1h Each independently represents a linear alkyl group having 2 to 24 carbon atoms, an alkoxy group having 2 to 24 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms. m represents an integer of 1 to 8.
[0092] As the diamine component for obtaining the specific polymer, other diamines (hereinafter also referred to as other diamines) may be used in combination in addition to the diamine represented by the above formula (d-1), the diamine represented by the above formula (d-2), and the diamine represented by the above formula (d-3).
[0093] Specifically, examples thereof include diamines described in paragraph
[0169] of International Publication WO2015 / 046374, diamines having a carboxyl group or a hydroxyl group described in paragraphs
[0171] to
[0172] , diamines having a nitrogen-containing heterocyclic ring described in paragraphs
[0173] to
[0188] , diamines having a nitrogen-containing structure described in paragraph
[0050] of JP-A-2016-218149, diamines having a pyrrole structure described in International Publication WO2017 / 126627, and diamines having a structure represented by the following formula (pr):
[0094]
[0095] (R 1 represents a hydrogen atom, hydrogen, a fluorine atom, a cyano group, a hydroxyl group, a methyl group, R 2 Each independently represents a single bond or *1-R 3 -Ph-*2, R 3 represents a single bond, selected from -O-, -COO-, -OCO-, -(CH2)l-, -O(CH2) m O-, -CONH- and -NHCO- in a divalent organic group (l, m represent integers of 1 to 5), *1 represents the position of bonding to the benzene ring in the formula (pr), *2 represents the position of bonding to the amino group in the formula (pr). Ph represents a phenylene group. n represents 1 to 3.),
[0096] A diamine having a pyrrole structure described in International Publication WO2018 / 062197, preferably a diamine having a structure represented by the following formula (pn):
[0097]
[0098] (R 1 , R 2 represents a hydrogen atom or a methyl group, R 3 Each independently represents a single bond or *1-R 4 -Ph-*2, R 4 represents a single bond, selected from -O-, -COO-, -OCO-, -(CH2)l -、-O(CH2) m O-, -CONH- and -NHCO- in a divalent organic group (l, m represent integers of 1 to 5, *1 represents the position of bonding to the benzene ring in the formula (pn), *2 represents the position of bonding to the amino group in the formula (pn). Ph represents a phenylene group. n represents 1 to 3.),
[0099] A diamine having a thiophene or furan structure described in International Publication WO2018 / 092759, preferably a diamine having a structure represented by the following formula (sf):
[0100]
[0101] (Y 1 represents a sulfur atom or an oxygen atom, R 2 Each independently represents a single bond or *1-R 5 -Ph-*2, R 5 represents a single bond, selected from -O-, -COO-, -OCO-, -(CH2) l -、-O(CH2) m O-, -CONH- and -NHCO- in a divalent organic group (l, m represent integers of 1 to 5, *1 represents the position of bonding to the benzene ring in the formula (pn), *2 represents the position of bonding to the amino group in the formula (pn). Ph represents a phenylene group. n represents 1 to 3.),
[0102] A diamine having a carbazole structure described in International Publication WO2018 / 110354, preferably a diamine having a structure represented by the following formula (cz):
[0103]
[0104] (R 1 represents a hydrogen atom or a methyl group, R 2 Represents a methyl group. ),
[0105] Diamines containing organic siloxanes such as 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and 1,3-bis(4-aminobutyl)-1,1,3,3-tetramethyldisiloxane, diamines having a functional group (also called a photoreactive group) capable of forming a covalent bond by light irradiation as described in International Publication WO2015 / 033921 for improving the response speed of liquid crystal when forming a liquid crystal display element, and diamines having a benzophenone skeleton represented by the following formula (z1) or (z2).
[0106]
[0107] Specific examples of the diamine having a benzophenone skeleton include 3,3′-diaminobenzophenone, 3,4′-diaminobenzophenone, 4,4′-diaminobenzophenone, 4,4′-bis[4-(4-amino-α,α-dimethylbenzyl)phenoxy]benzophenone, and diamines represented by the following formulas (z-1) to (z-4).
[0108]
[0109] Moreover, as said other diamine, the other diamine which has the structure of following formula (11) is mentioned.
[0110]
[0111] In the formula, A is a single bond or a divalent organic group, and R1, R2 and R3 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.
[0112] In the above formula (11), A is a single bond or a divalent organic group. The divalent organic group has a structure represented by the following formula (12), for example.
[0113] *-R5-B-R6-* (12)
[0114] In the formula, B is a divalent linking group, and R5 and R6 are each independently a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms. Specific examples of B include -CH2-, -CHR7-, -CR7R8-, -CR7=CR8-, -C≡C-, -O-, -S-, -NR9-, -C(=O)O-, -OC(=O)-, -C(=O)NR 10 -、-NR 10 C(=O)-、-NR 10 C(=O)NR 11 -, but not limited to this.
[0115] The above R7, R8, R9, R 10 and R 11 Each independently represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms. Examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, butyl, tert-butyl, hexyl, octyl, and decyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; bicycloalkyl groups such as bicyclohexyl; alkenyl groups such as vinyl, 1-propenyl, 2-propenyl, isopropenyl, and hexenyl; aryl groups such as phenyl, xylyl, biphenyl, and naphthyl; and aralkyl groups such as benzyl, phenylethyl, and phenylcyclohexyl.
[0116] It should be noted that some or all of the hydrogen atoms of these monovalent hydrocarbon groups may be substituted with halogen atoms, hydroxyl groups, mercapto groups, carboxyl groups, thioester groups, amide groups, alkyl groups, cycloalkyl groups, bicycloalkyl groups, alkenyl groups, aryl groups, aralkyl groups, etc.
[0117] If R7, R8, R9, R 10 and R 11 If the structure is bulky, such as an aromatic ring or an alicyclic structure, the solubility of the polymer may be reduced. Therefore, an alkyl group such as a methyl group, an ethyl group, a propyl group, or a butyl group, or a hydrogen atom is preferred, and a hydrogen atom is more preferred.
[0118] R1, R2 and R3 in formula (11) are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 6 carbon atoms. Examples of the monovalent organic group include a monovalent hydrocarbon group, a hydroxyl group, a mercapto group, an ester group, a carboxyl group, a thioester group, an amide group, an organic oxy group, an organic silyl group, an organic thio group, an acyl group, and the like. As the monovalent organic group, a monovalent hydrocarbon group is preferred from the viewpoint of high resistance to high temperature and high humidity. Specific examples of the monovalent hydrocarbon group include the aforementioned monovalent hydrocarbons, in which a part or all of the hydrogen atoms of the monovalent hydrocarbon groups may be replaced by the aforementioned R7, R8, R9, R10, R11, R12, R13, R14, R15, R16, R17, R18, R19, R20, R21, R22, R23, R24, R25, R26, R27, R28, R29, R30, R31, R32, R33, R34, R35, R36, R37, R38, R39, R40, R41, R42, R43, R44, R45, R46, R47, R48, R49, R50, R51, R52, R53, R54, R55, R56, R57, R58, R59, R60, R70, R71, R72, R73, R74, R8 10 In addition to the substitutable groups exemplified in the above, the group may be substituted with a pyrrolyl group, an imidazolyl group, a pyrazolyl group or the like.
[0119] From the viewpoint of high resistance to high temperature and high humidity, R1 and R2 are preferably alkyl groups such as methyl, ethyl, propyl, and butyl, or hydrogen atoms, and more preferably hydrogen atoms.
[0120] From the viewpoint of high resistance to high temperature and high humidity, R3 is preferably an alkyl group such as a methyl group, an ethyl group, a propyl group or a butyl group, or a hydrogen atom, and more preferably a hydrogen atom.
[0121] As specific examples of the structure represented by formula (11), structures of the following formulae (H-1) to (H-6) are particularly preferred.
[0122]
[0123] n1, n2, n3, n4, n5, and n6 each independently represent an integer of 1 to 10.
[0124] The diamine having a structure represented by the above formula (11) is preferably a diamine represented by the following formula (M1) from the viewpoint that the high-temperature and high-humidity resistance of the liquid crystal aligning film is high.
[0125]
[0126] Z1 is a substituent having a structure represented by the above formula (11), and n is an integer of 1 to 4. Y1 is an (n+2)-valent organic group having 5 to 40 carbon atoms.
[0127] Examples of the (n+2)-valent organic group having 5 to 40 carbon atoms in the aforementioned Y1 include hydrocarbon groups such as chain hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups, groups formed by introducing functional groups such as -O-, -COO-, -OCO-, -CO-, -NHCO-, -S-, -NH-, divalent heterocyclic rings or divalent groups containing a steroid skeleton between carbon-carbon bonds in the hydrocarbon groups, (n+2)-valent heterocyclic rings, etc. In addition, each of these groups may have a substituent such as a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), an alkoxy group, etc.
[0128] Here, the (n+2)-valent chain hydrocarbon group includes R7, R8, R9, R 10 and R 11 The group formed by removing (n+1) hydrogen atoms from the aforementioned univalent alkyl group, the group formed by removing (n+1) hydrogen atoms from the aforementioned univalent alkenyl group, etc. Examples of the (n+2)-valent alicyclic hydrocarbon group include R7, R8, R9, R 10 and R 11 The group formed by removing (n+1) hydrogen atoms from the aforementioned univalent cycloalkyl group, the group formed by removing (n+1) hydrogen atoms from the aforementioned univalent bicycloalkyl group, etc. Examples of the (n+2)-valent aromatic hydrocarbon group include R7, R8, R9, R 10 and R 11 A group formed by removing (n+1) hydrogen atoms from the above-mentioned monovalent aryl group, a group formed by removing (n+1) hydrogen atoms from the above-mentioned monovalent aralkyl group, and the like.
[0129] Examples of the divalent heterocyclic ring include a divalent pyrrole ring, a divalent thiophene ring, a divalent furan ring, a 5-membered heterocyclic ring such as a pyrrolidinylene group, and a 6-membered heterocyclic ring such as a piperidinylene group, a piperazinylene group, a pyridinylene group, a pyridazinylene group, and a pyrimidinylene group.
[0130] The steroid skeleton has a skeleton represented by the following formula (st) in which three six-membered rings and one five-membered ring are bonded.
[0131]
[0132] From the viewpoint of high temperature and high humidity resistance of the liquid crystal alignment film, Y1 is preferably an (n+2)-valent organic group having 5 to 40 carbon atoms in an aromatic ring, specifically, an (n+2)-valent aromatic hydrocarbon group having 5 to 40 carbon atoms, a group formed by introducing functional groups such as -O-, -COO-, -OCO-, -CO-, -NHCO-, -S-, -NH-, a divalent heterocycle or a divalent group containing a steroid skeleton between carbon-carbon bonds in the hydrocarbon group, or an (n+2)-valent group having an aromatic heterocycle.
[0133] In the (n+2)-valent group having an aromatic heterocycle in Y1, the aromatic heterocycle is preferably a nitrogen-containing aromatic heterocycle having a nitrogen atom in the ring portion. Specifically, for example, a pyridine ring, a pyrimidine ring, a pyrazine ring, a pyridazine ring, a triazine ring, etc. are listed, and a pyridine ring, a pyrimidine ring or a triazine ring is more preferred.
[0134] From the viewpoint of high voltage holding ratio, Y1 is preferably an (n+2)-valent aromatic hydrocarbon group having 5 to 40 carbon atoms, and preferably an (n+2)-valent group having 5 to 40 carbon atoms having a structure represented by the following formula (Ar1).
[0135]
[0136] A1 represents a single bond or a divalent organic group having an aromatic ring.
[0137] As more preferable specific examples of the above formula (M1), the following formulas (M1-1) to (M1-13) can be mentioned.
[0138]
[0139] Z1 is the structure represented by the above formula (11), c is an integer of 1-4, d and e are integers of 1-2, and n is an integer of 2-6.
[0140] From the viewpoint of improving vertical alignment properties, the diamine having a structure represented by the above formula (11) is preferably at least one selected from the group consisting of diamines represented by the following formulae (M-1) to (M-6).
[0141]
[0142] n1, n2, n3, n4, n5, and n6 each independently represent an integer of 1 to 10.
[0143] Moreover, as said other diamine, the diamine which has the structure represented by following formula (21) is mentioned.
[0144]
[0145] In the above formula (21), R 1 represents hydrogen or a monovalent organic group, and * represents a site that bonds to other groups.
[0146] Examples of the diamine having an oxazoline skeleton represented by the above formula (21) include diamines selected from the group represented by the following formulas (21-1) to (21-3).
[0147]
[0148] In the above formulas (21-1) to (21-3), R1 The definition of R is the same as in the above formula (21). 2 represents a single bond, -O-, -COO-, -OCO-, -(CH2) l -、-O(CH2) l O-、-CONR 11 -、-NR 11 CO- and -NR 11 - or a divalent organic group consisting of a combination of these, W 1 represents a structure selected from the following group (3-1), W 2 represents a structure selected from the following group (3-2), W 3 represents a structure selected from the following group (3-3), W 4 represents a structure selected from the following group (3-4). 11 represents hydrogen or a monovalent organic group, l represents an integer of 1 to 12, and a represents an integer of 0 or 1.
[0149]
[0150] In the above group (3-1), *1 represents the site bonded to the amino group in formula (21-1) to (21-3), and *2 represents the site bonded to the oxazoline ring. In the group (3-2), *1 represents the site bonded to the amino group in formula (21-1) to (21-3), and *3 represents the site bonded to R 2 In group (3-3), *3 indicates the bonding site with R 2 Bonding site. In group (3-4), *2 represents the site bonded to the oxazoline ring. X represents a substituent, which is a hydrogen atom; a halogen atom; an alkyl group having 1 to 6 carbon atoms, such as methyl, ethyl, and propyl; a halogenated alkyl group having 1 to 6 carbon atoms, such as trifluoromethyl; a substituted amino group, such as dimethylamino; an alkoxy group having 1 to 6 carbon atoms, such as methoxy and ethoxy; an amide group, such as NHCOCH3, NHCOCH2CH3, and NHCOOtBu. tBu represents a tert-butyl group.
[0151] Specific examples of the diamines of the formulae (21-1) to (21-3) are as follows.
[0152]
[0153] In the above formula, R 1 The definition of R is the same as in the above formula (21), and is particularly preferably a hydrogen atom, a methyl group (Me) or an ethyl group (Et). 11 The definition of is the same as in the above formula (21), and is particularly preferably a hydrogen atom, a Me group or an Et group. n represents an integer of 1 to 6, and m represents an integer of 1 to 12.
[0154] Specific examples of the diamine component that can be used in combination with the other diamines include m-phenylenediamine, p-phenylenediamine, 4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-difluoro-4,4'-diaminobiphenyl, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylamine, N-methyl(4,4'-diaminodiphenyl)amine, 4,4'-diaminobenzophenone, 1,4-diaminonaphthalene, 2,6-diaminonaphthalene, 1,2-bis(4-aminophenyl)ethane, 1,3-bis(4-aminophenyl)propane, 1,4-bis(4-aminophenyl)butane, 1,4-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, and 1,4-bis(4-aminophenyl)propane. (4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(4-aminobenzyl)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-[1,4-phenylenebis(methylene)]diphenylamine, 1,4-phenylenebis[(4-aminophenyl)methanone], 1,4-phenylenebis(4-aminobenzoate), bis(4-aminophenyl)terephthalate, bis(4-aminophenyl)isophthalate, N,N'-(1,4-phenylene)bis(4-aminobenzamide), N,N'-bis(4-aminophenyl)terephthalamide, N,N'-bis(4-aminophenyl)isophthalamide, 9,10-bis(4-aminophenyl)anthracene, 2,2'-bis[4-(4-aminophenyl) 1,4-bis(4-aminophenoxy)butane, 1,5-bis(4-aminophenoxy)pentane, 1,6-bis(4-aminophenoxy)hexane, 1,7-bis(4-aminophenoxy)heptane, 1,8-bis(4-aminophenoxy)octane, 1,9-bis(4-aminophenoxy)nonane, 1,10-(4-aminophenoxy)decane, bis(4-aminocyclohexyl)methane, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 2,4-diaminobenzoic acid, 2,5-diaminobenzoic acid or 3,5-diaminobenzoic acid , 4,4'-diaminobiphenyl-3-carboxylic acid, 4,4'-diaminodiphenylmethane-3-carboxylic acid, 4,4'-diaminodiphenylethane-3-carboxylic acid, 4,4'-diaminobiphenyl-3,3'-dicarboxylic acid, 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid, 3,3'-diaminobiphenyl-4,4'-dicarboxylic acid, 3,3'-diaminobiphenyl-2,4'-dicarboxylic acid, 4,4'-diaminodiphenylmethane-3,3'-dicarboxylic acid, 4,4'-diaminodiphenylethane-3,3'-dicarboxylic acid, 4,4'-diaminodiphenyl ether-3,3'-dicarboxylic acid, 2,6-diaminopyridine, 3,4-diaminopyridine, 2,4-diaminopyrimidine, 3,6-diaminocarbazole, N-methyl-3,6-diaminocarbazole, 1,4-bis-(4-aminophenyl)-piperazine, 3,6-diaminoacridine, N-ethyl-3,6-diaminocarbazole, N-phenyl-3,6-diaminocarbazole, N,N'-bis(4-aminophenyl)-benzidine, N,N'-bis(4-aminophenyl)-N,N'-dimethylbenzidine, compounds represented by the following formula (D-2-1) to (D-2-23), and diamines wherein the amino groups thereof are secondary amino groups.
[0155]
[0156] The above other diamines may be used alone or in combination of two or more depending on the solubility of the specific polymer in the solvent, the coating properties of the liquid crystal aligning agent, the liquid crystal alignment when forming a liquid crystal aligning film, the voltage holding ratio, the stored charge and other properties.
[0157] As the tetracarboxylic acid component for obtaining the specific polymer of the present invention, it is preferred to use tetracarboxylic dianhydrides represented by the following formulas [4] to [6]. In this case, not only tetracarboxylic dianhydrides represented by the formulas [4] to [6] but also tetracarboxylic acids, tetracarboxylic acid dihalides, tetracarboxylic acid dialkyl esters or tetracarboxylic acid dialkyl ester dihalides which are tetracarboxylic acid derivatives thereof can be used.
[0158]
[0159] Z 1 represents at least one structure selected from the following [4a] to [4k]. In formula [5] or [6], j and k are each independently an integer of 0 or 1. x and y are each independently a single bond, a carbonyl group, an ester, a phenylene group, a sulfonyl group or an amide group.
[0160]
[0161] In formula [4a], Z 1 ~Z 4 represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom or a benzene ring, and they may be the same or different. Preferred specific examples of the formula [4a] include the following structures [4a-1] and [4a-2].
[0162]
[0163] In formula [4g], Z 5 and Z 6 represents a hydrogen atom or a methyl group, and may be the same or different.
[0164] Among Z in formula [4], tetracarboxylic dianhydride and its tetracarboxylic acid derivatives having structures represented by formula [4a], formula [4c] to formula [4g] or formula [4k] are preferred from the viewpoint of ease of synthesis and ease of polymerization reactivity when producing a polymer. Tetracarboxylic dianhydride and its tetracarboxylic acid derivatives having structures represented by formula [4a], formula [4e] to formula [4g] are more preferred. Tetracarboxylic dianhydride and its tetracarboxylic acid derivatives having structures represented by formula [4a], formula [4e] or formula [4f] are particularly preferred. As further preferred specific examples, tetracarboxylic dianhydride and its tetracarboxylic acid derivatives having structures represented by formula [4a-1], formula [4a-2], formula [4e] and formula [4f] are listed.
[0165] From the viewpoint of suppressing the accumulated charge of the liquid crystal display element, preferred specific examples of the formula [5] or [6] include tetracarboxylic dianhydrides represented by the following formulae (5a-1) to (5a-5) and (6a-1).
[0166]
[0167] The tetracarboxylic acid component represented by the formula [4] is preferably 1 to 100 mol% in 100 mol% of all tetracarboxylic acid components used, and among these, 5 to 95 mol% is preferred, and 20 to 80 mol% is more preferred.
[0168] The tetracarboxylic acid component may be used alone or in combination of two or more depending on properties such as solubility of the specific polymer in a solvent, coating properties of a liquid crystal aligning agent, liquid crystal alignment when a liquid crystal aligning film is formed, voltage holding ratio, and stored charge.
[0169] As the polyimide-based polymer of the specific polymer, other tetracarboxylic acid components other than the specific tetracarboxylic acid component may be used.
[0170] As other tetracarboxylic acid components, tetracarboxylic acid, tetracarboxylic dianhydride, tetracarboxylic acid dihalide, tetracarboxylic acid dialkyl ester, or tetracarboxylic acid dialkyl ester dihalide shown below can be mentioned.
[0171] That is, as other tetracarboxylic acid components, 1,2,5,6-naphthalenetetracarboxylic acid, 1,4,5,8-naphthalenetetracarboxylic acid, 1,2,5,6-anthracenetetracarboxylic acid, bis(3,4-dicarboxyphenyl)methane, 2,2-bis(3,4-dicarboxyphenyl)propane, bis(3,4-dicarboxyphenyl)dimethylsilane, bis(3,4-dicarboxyphenyl)diphenylsilane, 2,3,4,5-pyridinetetracarboxylic acid, 2,6-bis(3,4-dicarboxyphenyl)pyridine, 3,4,9,10-perylenetetracarboxylic acid, or 1,3-diphenyl-1,2,3,4-cyclobutanetetracarboxylic acid may be mentioned.
[0172] <Method for producing specific polymer>
[0173] The polyimide precursor as the specific polymer in the present invention is obtained by reacting a diamine component with a tetracarboxylic acid component. Specifically, a method of obtaining polyamic acid by polycondensing tetracarboxylic dianhydride with a primary diamine or a secondary diamine; a method of obtaining polyamic acid by dehydration polycondensation of tetracarboxylic acid with a primary diamine or a secondary diamine; or a method of obtaining polyamic acid by polycondensing a tetracarboxylic acid dihalide with a primary diamine or a secondary diamine.
[0174] Specific polymer can be obtained by reacting the above-mentioned tetracarboxylic acid component and diamine component together with a molecular weight modifier as required. As the molecular weight modifier, for example, monoanhydrides such as maleic anhydride, phthalic anhydride, itaconic anhydride, monoamines such as aniline, cyclohexylamine, n-butylamine, monoisocyanates such as phenyl isocyanate, naphthyl isocyanate, etc. can be listed. For the usage ratio of the molecular weight modifier, relative to a total of 100 parts by mass of the tetracarboxylic acid component and diamine component used, it is preferably less than 20 parts by mass, more preferably less than 10 parts by mass.
[0175] In order to obtain polyamic acid alkyl ester, a method of polycondensing a tetracarboxylic acid obtained by dialkyl esterifying a carboxylic acid group with a primary diamine or a secondary diamine; a method of polycondensing a tetracarboxylic acid dihalide obtained by dialkyl esterifying a carboxylic acid group with a primary diamine or a secondary diamine; or a method of converting the carboxyl group of the polyamic acid into an ester is used.
[0176] The reaction of the diamine component and the tetracarboxylic acid component is usually carried out in a solvent. The solvent used at this time is not particularly limited as long as it is a solvent in which the generated polyimide precursor dissolves. Specific examples of the solvent used in the reaction are listed below, but are not limited to these examples.
[0177] Examples include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and 1,3-dimethyl-2-imidazolidinone. In addition, when the polyimide precursor has high solvent solubility, methyl ethyl ketone, cyclohexanone, cyclopentanone, 4-hydroxy-4-methyl-2-pentanone, or solvents represented by the following formulas [D-1] to [D-3] can be used.
[0178]
[0179] In formula [D-1], D 1 represents an alkylene group having 1 to 3 carbon atoms, wherein D 2 represents an alkylene group having 1 to 3 carbon atoms, wherein D 3 It represents an alkylene group having 1 to 4 carbon atoms.
[0180] These solvents can be used alone or in combination. Furthermore, even if it is a solvent that does not dissolve the polyimide precursor, it can be mixed in the aforementioned solvent and used within the range that the generated polyimide precursor will not precipitate. In addition, the moisture in the solvent becomes the cause of hindering the polymerization reaction and then hydrolyzing the generated polyimide precursor, so the solvent is preferably a dehydrated solvent.
[0181] When the diamine component and the tetracarboxylic acid component are reacted in a solvent, the reaction can be carried out at any concentration. However, if the concentration is too low, it is difficult to obtain a high molecular weight polymer, and if the concentration is too high, the viscosity of the reaction solution is too high and it is difficult to stir uniformly. Therefore, it is preferably 1 to 50% by weight, and more preferably 5 to 30% by weight. The reaction may be carried out at a high concentration in the initial stage and then the solvent may be added.
[0182] In the polymerization reaction of the polyimide precursor, the total molar ratio of the diamine component to the tetracarboxylic acid component is preferably 0.8 to 1.2. As in a normal polycondensation reaction, the closer the molar ratio is to 1.0, the greater the molecular weight of the generated polyimide precursor.
[0183] The polyimide of the present invention is obtained by ring-closing the polyimide precursor. In the polyimide, the ring-closure ratio (also referred to as imidization ratio) of the amic acid group is not necessarily required to be 100% and can be arbitrarily adjusted according to the application and purpose.
[0184] As the polyimide which is the specific polymer in the present invention, a method of ring-closing a polyamic acid or a polyamic acid alkyl ester which is a polyimide precursor is used.
[0185] Examples of a method for imidizing a polyimide precursor include thermal imidization in which a solution of a polyimide precursor is directly heated, and catalyst imidization in which a catalyst is added to a solution of a polyimide precursor.
[0186] The temperature when the polyimide precursor is thermally imidized in a solution is 100 to 400° C., preferably 120 to 250° C., and it is preferably carried out while removing water generated by the imidization reaction to the outside of the system.
[0187] The catalyst imidization of the polyimide precursor can be carried out by adding a basic catalyst and anhydride to the solution of the polyimide precursor and stirring at -20°C to 250°C, preferably 0°C to 180°C. The amount of the basic catalyst is 0.5 to 30 times by mole, preferably 2 to 20 times by mole, of the amic acid group, and the amount of the anhydride is 1 to 50 times by mole, preferably 3 to 30 times by mole, of the amic acid group. As the basic catalyst, pyridine, triethylamine, trimethylamine, tributylamine or trioctylamine can be listed, among which pyridine is preferred because it has a suitable alkalinity for the reaction. As the anhydride, acetic anhydride, trimellitic anhydride or pyromellitic anhydride can be listed, among which, if acetic anhydride is used, purification after the reaction becomes easy, so it is preferred. The imidization rate achieved by the catalyst imidization can be controlled by adjusting the amount of catalyst, reaction temperature and reaction time.
[0188] In the case of recovering the generated polyimide precursor or polyimide from the reaction solution of the polyimide precursor or polyimide, the reaction solution can be put into a solvent for precipitation. As the solvent used in the precipitation, methanol, ethanol, isopropanol, acetone, hexane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, toluene, benzene, water, etc. can be listed. After filtering and recovering, the polymer put into the solvent and precipitated can be dried at room temperature or heated under normal pressure or reduced pressure. In addition, if the operation of re-dissolving the polymer recovered by precipitation in the solvent and re-precipitating and recovering is repeated 2 to 10 times, the impurities in the polymer can be reduced. As the solvent at this time, for example, alcohols, ketones or hydrocarbons can be listed. If more than 3 solvents selected from them are used, the efficiency of purification is further improved, so it is preferred.
[0189] The weight average molecular weight (Mw) of the polyimide precursor and the polyimide measured by gel permeation chromatography (GPC) in terms of polyethylene oxide is preferably 1000 to 500000, more preferably 2000 to 300000. In addition, the molecular weight distribution (Mw / Mn) represented by the ratio of Mw to the number average molecular weight (Mn) in terms of polyethylene oxide measured by GPC is preferably 15 or less, more preferably 10 or less. By being within this molecular weight range, good orientation of the liquid crystal display element can be ensured.
[0190] <Liquid crystal alignment agent>
[0191] The liquid crystal aligning agent of the present invention is a coating solution for forming a liquid crystal aligning film, and is a coating solution for forming a liquid crystal aligning film containing a specific polymer and a solvent. The specific polymer can be any polyimide polymer of polyamic acid, polyamic acid alkyl ester, and polyimide.
[0192] All polymers in the liquid crystal alignment agent of the present invention may all be specific polymers, or other polymers may be mixed. As other polymers, polyimide polymers without specific side chain 1, specific side chain 2 and specific side chain 3 may be listed. Cellulose polymers, acrylic polymers, methacrylic polymers, polystyrene, polyamide or polysiloxane may also be listed. At this time, the content of other polymers other than these is preferably 5 to 90 parts by mass, more preferably 10 to 60 parts by mass, relative to 100 parts by mass of the polymer formed by combining the specific polymer and the other polymers mentioned above.
[0193] Moreover, it is preferable that content of the solvent in the liquid crystal aligning agent of this invention is 70-99.9 mass %.This content can be changed suitably according to the coating method of a liquid crystal aligning agent and the film thickness of a target liquid crystal aligning film.
[0194] The solvent used for the liquid crystal aligning agent of this invention is not specifically limited as long as it is a solvent (also called a good solvent) which melt|dissolves a polymer. Although the specific example of a good solvent is given below, it is not limited to these examples.
[0195] Examples thereof include N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-butyl-2-pyrrolidone, dimethyl sulfoxide, γ-butyrolactone, γ-valerolactone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, methyl ethyl ketone, cyclohexanone, cyclopentanone, and 4-hydroxy-4-methyl-2-pentanone.
[0196] Among them, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-butyl-2-pyrrolidone, γ-butyrolactone, γ-valerolactone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropionamide or 3-butoxy-N,N-dimethylpropionamide is preferred.
[0197] Furthermore, when the solubility of the polymer in the solvent is high, it is preferable to use the solvent represented by the above formula [D-1] to formula [D-3].
[0198] The good solvent in the liquid crystal aligning agent of the present invention is preferably 5 to 99% by mass of all solvents contained in the liquid crystal aligning agent, and among them, preferably 10 to 90% by mass.
[0199] The liquid crystal aligning agent of the present invention can use a solvent (also referred to as a poor solvent) that improves the coating properties and surface smoothness of the liquid crystal aligning film when the liquid crystal aligning agent is applied. Specific examples of the poor solvent are given below, but are not limited to these examples.
[0200] Examples thereof include ethanol, isopropanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, isopentanol, tert-pentanol, 3-methyl-2-butanol, neopentyl alcohol, 1-hexanol, 2-methyl-1-pentanol, 2-methyl-2-pentanol, 2-ethyl-1-butanol, 1-heptanol, 2-heptanol, 3-heptanol, 1-octanol, 2-octanol, 2-ethyl-1-hexanol, cyclohexanol, 1-methylcyclohexanol, 2-methylcyclohexanol, 3-methylcyclohexanol, 1,2-ethanediol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 2,3-butylene glycol, 1,5-pentanediol, alcohol, 2-methyl-2,4-pentanediol, 2-ethyl-1,3-hexanediol, dipropyl ether, dibutyl ether, dihexyl ether, dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, 1,2-butoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol dibutyl ether, 2-pentanone, 3-pentanone, 2-hexanone, 2-heptanone, 4-heptanone, 3-ethoxybutyl acetate, 1-methylpentyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, ethylene glycol monoacetate, ethylene glycol diacetate, propylene carbonate, ethylene carbonate, 2-(methoxymethoxy)ethanol, ethylene glycol monobutyl ether, ethylene glycol monoisoamyl ether, ethyl glycol monohexyl ether, 2-(hexyloxy)ethanol, furfuryl alcohol, diethylene glycol, propylene glycol, the solvent represented by the above formula [D-1] to [D-3] or propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, propylene glycol monobutyl ether, 1-(butoxyethoxy)propanol, propylene glycol monomethyl ether acetate, dipropylene glycol, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, ethylene glycol mono acetate, ethylene glycol diacetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, 2-(2-ethoxyethoxy)ethyl acetate, diethylene glycol acetate, triethylene glycol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol monoethyl acetate, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, methyl ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isopentyl lactate or 4-hydroxy-4-methyl-2-pentanone, etc.
[0201] Among them, 1-hexanol, cyclohexanol, 1,2-ethylene glycol, 1,2-propylene glycol, propylene glycol monobutyl ether, ethylene glycol monobutyl ether, dipropylene glycol dimethyl ether, diethylene glycol diethyl ether, 4-hydroxy-4-methyl-2-pentanone, propylene glycol diacetate, dipropylene glycol monomethyl ether or propylene carbonate is preferred.
[0202] These poor solvents are preferably 1 to 95% by mass of the total solvents contained in the liquid crystal aligning agent, and among them, 10 to 90% by mass is preferred.
[0203] The liquid crystal aligning agent of the present invention can use a compound that improves the uniformity of the film thickness of the liquid crystal aligning film when the liquid crystal aligning agent is applied and the surface smoothness.
[0204] As the compound for improving the uniformity of the film thickness of the liquid crystal alignment film and the surface smoothness, fluorine-based surfactants, silicone-based surfactants, nonionic surfactants, etc. can be listed. More specifically, for example, EFTOPEF301, EF303, EF352 (Tochem Products Co., Ltd.), Megaface F171, F173, R-30 (Dainippon Ink Co., Ltd.), Fluorad FC430, FC431 (Sumitomo 3M Limited), Asahi Guard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, SC106 (Above Asahi Glass Co., Ltd.) etc. can be listed.
[0205] The using ratio of these surfactants is preferably 0.01 to 2 parts by mass, more preferably 0.01 to 1 part by mass, relative to 100 parts by mass of all polymer components contained in the liquid crystal aligning agent.
[0206] Furthermore, the liquid crystal aligning agent of the present invention may also be added as a compound that promotes charge transfer in the liquid crystal aligning film and promotes charge escape of the element, and nitrogen-containing heterocyclic amines represented by formulas [M1] to [M156] described in paragraphs
[0194] to
[0200] of the International Publication WO2011 / 132751, and more preferably nitrogen-containing heterocyclic amines represented by the following formulas (B-1) to (B-40). The amine can be added directly to the liquid crystal aligning agent, but it is preferably added after forming a solution with a concentration of 0.1 to 10%, preferably 1 to 7%, with an appropriate solvent. As such a solvent, there is no particular limitation if it is a solvent that dissolves the above-mentioned polyimide polymer.
[0207]
[0208] Furthermore, the liquid crystal aligning agent of the present invention may contain a crosslinking compound which is a compound that crosslinks a specific polymer, or an adhesion aid for improving adhesion between the liquid crystal aligning film and the substrate, and adhesion between the liquid crystal aligning film and the sealing material.
[0209] (Crosslinking compound)
[0210] As the crosslinking compound, it is preferred to introduce at least one compound selected from the group consisting of a crosslinking compound having the following substituents and a crosslinking compound having a polymerizable unsaturated group, wherein the substituent is at least one selected from an epoxy group, an isocyanate group, an oxetane group, a cyclocarbonate group, a blocked isocyanate group, a hydroxyl group and an alkoxy group.
[0211] It should be noted that, from the viewpoint of improving crosslinking, these substituents and polymerizable unsaturated bonds preferably have 2 or more in the crosslinking compound. As specific examples of crosslinking compounds, compounds with epoxy or isocyanate groups, compounds with oxetane groups, amino resins with hydroxyl, alkoxy or lower alkoxyalkyl groups, benzene or phenolic compounds with hydroxyl or alkoxy groups, compounds with cyclic carbonate groups, compounds with hydroxyalkylamide groups, compounds with blocked isocyanate groups, etc., are listed in paragraphs
[0103] to
[0112] of International Publication Gazette 2012 / 014898, compounds with hydroxyalkylamide groups, compounds with blocked isocyanate groups, etc., are listed in International Publication Gazette 2015 / 072554.
[0212] Preferred specific examples of the crosslinking compound include compounds represented by the following formulae (CL-1) to (CL-11).
[0213]
[0214] The content of the crosslinking compound is preferably 0.1 to 100 parts by mass, more preferably 0.1 to 50 parts by mass, further preferably 1 to 50 parts by mass, based on 100 parts by mass of all polymer components contained in the liquid crystal aligning agent, from the viewpoint of improving the orientation of the liquid crystal.
[0215] (Sealing agent)
[0216] Examples of the adhesion aid include functional silane compounds. Examples thereof include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-aminopropyltrimethoxysilane, 2-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-ureidepropyltrimethoxysilane, 3-ureidepropyltriethoxysilane, N-ethoxycarbonyl-3-aminopropyltrimethoxysilane, N-ethoxycarbonyl-3-aminopropyltriethoxysilane, N-triethoxysilylpropyltriethylenetriamine, N-trimethoxysilylpropyltriethylenetriamine, 1 0-trimethoxysilyl-1,4,7-triazadecane, 10-triethoxysilyl-1,4,7-triazadecane, 9-trimethoxysilyl-3,6-diazanonyl acetate, 9-triethoxysilyl-3,6-diazanonyl acetate, N-benzyl-3-aminopropyl trimethoxysilane, N-benzyl-3-aminopropyl triethoxysilane, N-phenyl-3-aminopropyl trimethoxysilane, N-phenyl-3-aminopropyl triethoxysilane, N-bis(oxyethylene)-3-aminopropyl trimethoxysilane, N-bis(oxyethylene)-3-aminopropyl triethoxysilane. When using these adhesion aids, the amount is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, relative to 100 parts by mass of all polymer components contained in the liquid crystal aligning agent. When the amount is less than 0.1 parts by mass, the effect of improving adhesion cannot be expected, while when the amount is more than 30 parts by mass, the orientation of liquid crystal may deteriorate.
[0217] The liquid crystal alignment agent of the present invention may contain, in addition to the above-mentioned poor solvents, cross-linking compounds, adhesion aids, compounds for improving the uniformity of the film thickness and surface smoothness of the resin coating or liquid crystal alignment film, and compounds for promoting charge escape, dielectrics and conductive substances for changing the electrical properties of the liquid crystal alignment film, such as the dielectric constant and conductivity.
[0218] <Liquid crystal alignment film / liquid crystal display element>
[0219] The liquid crystal alignment agent of the present invention can be used as a liquid crystal alignment film by applying it on a substrate, firing it, and then performing an alignment treatment by rubbing, light irradiation, etc. In addition, in the case of vertical alignment, it can be used as a liquid crystal alignment film even without performing an alignment treatment.
[0220] The liquid crystal alignment film of the present invention can be used for horizontal alignment type or vertical alignment type (VA mode, PSA mode, SC-PVA mode, etc.) liquid crystal alignment film, among which, it is a liquid crystal alignment film suitable for vertical alignment type liquid crystal display elements such as PSA mode and SC-PVA mode, and the pre-tilt can be controlled by using a small amount of light irradiation.
[0221] As the substrate used at this time, if it is a substrate with high transparency, it is not particularly limited. In addition to the glass substrate, plastic substrates such as acrylic substrates and polycarbonate substrates can also be used. From the viewpoint of process simplification, it is preferred to use a substrate formed with an ITO electrode for driving liquid crystals. In addition, in the reflective liquid crystal display element, if only a single-sided substrate, then even an opaque substrate such as a silicon wafer can also be used, as an electrode at this time, a material of reflected light such as aluminum can also be used.
[0222] There is no particular limitation on the coating method of the liquid crystal alignment agent, and it is usually industrially applied by screen printing, offset printing, flexographic printing or inkjet method, etc. Other coating methods include dipping, roll coating, slit coating, spin coating or spray coating, and they can be used according to the purpose.
[0223] After the liquid crystal alignment agent is applied to the substrate, a heating means such as a heating plate, a heat circulation oven or an IR (infrared) oven is used to evaporate the solvent at a temperature of 30 to 300°C, preferably 30 to 250°C, according to the solvent used in the liquid crystal alignment agent, to form a liquid crystal alignment film. If the thickness of the fired liquid crystal alignment film is too thick, it is disadvantageous in terms of the power consumption of the liquid crystal display element. If it is too thin, the reliability of the liquid crystal display element may be reduced, so it is preferably 5 to 300 nm, more preferably 10 to 100 nm. When the liquid crystal is horizontally oriented or tilted, the fired liquid crystal alignment film is treated by friction or polarized ultraviolet irradiation.
[0224] The liquid crystal display element of the present invention is formed by producing a liquid crystal cell by a known method after obtaining a substrate with a liquid crystal alignment film from the liquid crystal aligning agent of the present invention by the above-mentioned method.
[0225] As a method for preparing a liquid crystal unit, there can be exemplified a method of preparing a pair of substrates with liquid crystal alignment films formed thereon, dispersing spacers on the liquid crystal alignment film of one substrate, bonding the other substrate with the liquid crystal alignment film surface facing inward, injecting liquid crystal under reduced pressure and sealing; or a method of dripping liquid crystal on the surface of the liquid crystal alignment film with spacers dispersed thereon and then bonding the substrates together for sealing.
[0226] Furthermore, the liquid crystal aligning agent of the present invention is also preferably used for a liquid crystal layer between a pair of substrates having electrodes, a liquid crystal composition containing a polymerizable compound polymerized by at least one of active energy rays and heat is arranged between a pair of substrates, and a liquid crystal display element is manufactured by a process of polymerizing the polymerizable compound by irradiation of active energy rays and heat while applying a voltage between the electrodes. Here, ultraviolet rays are suitable as active energy rays. As ultraviolet rays, the wavelength is 300 to 400nm, preferably 310 to 360nm. When polymerization is performed by heating, the heating temperature is 40 to 120°C, preferably 60 to 80°C. In addition, ultraviolet rays and heating can be performed simultaneously.
[0227] The above-mentioned liquid crystal display element controls the pre-tilt of the liquid crystal molecules by means of a polymer-sustaining alignment (PSA) method. In the PSA method, a small amount of photopolymerizable compounds, such as photopolymerizable monomers, are pre-mixed into the liquid crystal material. After the liquid crystal unit is assembled, the photopolymerizable compounds are irradiated with ultraviolet rays or the like while a prescribed voltage is applied to the liquid crystal layer, and the pre-tilt of the liquid crystal molecules is controlled by the generated polymer. The orientation state of the liquid crystal molecules when the polymer is generated is stored even after the voltage is removed, so the pre-tilt of the liquid crystal molecules can be adjusted by controlling the electric field formed in the liquid crystal layer, etc. In addition, in the PSA method, no friction treatment is required, so it is suitable for the formation of a vertically oriented liquid crystal layer whose pre-tilt is difficult to control by friction treatment.
[0228] That is, the liquid crystal display element of the present invention is obtained by the above-mentioned method from the liquid crystal aligning agent of the present invention to obtain a substrate with a liquid crystal aligning film, and then a liquid crystal unit is prepared, and the polymerizable compound is polymerized by at least one of ultraviolet irradiation and heating, thereby controlling the orientation of liquid crystal molecules.
[0229] If an example of the preparation of a PSA liquid crystal unit is listed, it can be listed as a method of preparing a pair of substrates with liquid crystal alignment films formed thereon, dispersing spacers on the liquid crystal alignment film of one substrate, bonding the other substrate with the liquid crystal alignment film surface facing inside, injecting liquid crystal under reduced pressure and sealing; or a method of dripping liquid crystal on the surface of the liquid crystal alignment film with spacers dispersed thereon and then bonding the substrates together for sealing, etc.
[0230] A polymerizable compound that is polymerized by heat or ultraviolet irradiation is mixed in the liquid crystal. As the polymerizable compound, there can be cited compounds having one or more polymerizable unsaturated groups such as an acrylate group and a methacrylate group in the molecule. At this time, the polymerizable compound is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass relative to 100 parts by mass of the liquid crystal component. If the polymerizable compound is less than 0.01 parts by mass, the polymerizable compound will not polymerize, and it becomes impossible to control the orientation of the liquid crystal. If it is more than 10 parts by mass, the unreacted polymerizable compound increases and the residual image characteristics of the liquid crystal display element are reduced.
[0231] After the liquid crystal cell is manufactured, an AC or DC voltage is applied to the liquid crystal cell, and heat or ultraviolet rays are irradiated to polymerize the polymerizable compound. This allows the alignment of the liquid crystal molecules to be controlled.
[0232] Furthermore, the liquid crystal aligning agent of the present invention is also preferably used for a liquid crystal display element, i.e., SC-PVA mode, having a liquid crystal layer between a pair of substrates having electrodes, and a liquid crystal aligning film containing a polymerizable group polymerized by at least one of active energy rays and heat is arranged between the aforementioned pair of substrates, and a voltage is applied between the electrodes. Here, ultraviolet rays are suitable as active energy rays. As ultraviolet rays, the wavelength is 300 to 400 nm, preferably 310 to 360 nm. When polymerization is performed by heating, the heating temperature is 40 to 120 ° C, preferably 60 to 80 ° C. In addition, ultraviolet rays and heating can be performed simultaneously.
[0233] In order to obtain a liquid crystal alignment film containing a polymerizable group that is polymerized by at least one of active energy rays and heat, a method of adding a compound containing the polymerizable group to a liquid crystal alignment agent and a method of using a polymer component containing a polymerizable group can be cited. As a specific example of a polymer containing a polymerizable group, it is not particularly limited if it is a polymer having the aforementioned photoreactive group, and a polymer obtained using a diamine having the aforementioned photoreactive group can be cited.
[0234] If an example of the preparation of a liquid crystal unit of the SC-PVA mode is listed, it can be listed as a method of preparing a pair of substrates on which the liquid crystal orientation film of the present invention is formed, and dispersing spacers on the liquid crystal orientation film of one substrate, making the liquid crystal orientation film surface face inside to bond to the other substrate, injecting liquid crystal under reduced pressure and sealing; or a method of dripping liquid crystal on the surface of the liquid crystal orientation film on which spacers are dispersed, and then bonding the substrates together to seal, etc.
[0235] After the liquid crystal cell is manufactured, the alignment of the liquid crystal molecules can be controlled by applying an AC or DC voltage to the liquid crystal cell and irradiating the cell with heat or ultraviolet light.
[0236] Example
[0237] The following is a specific description based on Examples, but the present invention is not limited to these Examples and should not be construed as being deleted.
[0238] The abbreviations used below have the following meanings.
[0239] (Acid dianhydride)
[0240] BODA: Bicyclo[3,3,0]octane-2,4,6,8-tetracarboxylic dianhydride
[0241] CBDA: 1,2,3,4-cyclobutanetetracarboxylic dianhydride
[0242] (Diamine)
[0243] p-PDA: p-phenylenediamine, DBA: 3,5-diaminobenzoic acid
[0244] 3AMPDA: 3,5-diamino-N-(pyridin-3-ylmethyl)benzamide
[0245]
[0246] (Solvent)
[0247] NMP: N-methyl-2-pyrrolidone, BCS: butyl cellosolve
[0248] (additive)
[0249] 3AMP: 3-aminomethylpyridine
[0250] <Production of Liquid Crystal Alignment Agent>
[0251] (Example 1)
[0252] BODA (1.13 g, 4.5 mmol), DA-1 (0.60 g, 1.8 mmol), DA-3 (0.65 g, 2.7 mmol) and DA-4 (1.71 g, 4.5 mmol) were dissolved in NMP (16.3 g), reacted at 60°C for 3 hours, CBDA (0.86 g, 4.5 mmol) and NMP (3.4 g) were added, and reacted at 40°C for 12 hours to obtain a polyamic acid solution.
[0253] After adding NMP to the polyamic acid solution (19.3 g) to dilute to 6 mass%, acetic anhydride (3.6 g) and pyridine (1.1 g) as imidization catalysts were added and reacted at 80° C. for 3 hours. The reaction solution was put into methanol (220 ml) and the obtained precipitate was filtered. The precipitate was washed with methanol and dried under reduced pressure at 60° C. to obtain a polyimide powder (A). The imidization rate of the polyimide was 77%.
[0254] NMP (25.4 g) was added to the obtained polyimide powder (A) (3.2 g), and the mixture was dissolved by stirring at 70° C. for 12 hours. 3AMP (1 wt % NMP solution) 3.2 g and BCS (21.2 g) were added to the solution, and the mixture was stirred at room temperature for 5 hours to obtain a liquid crystal aligning agent (A1).
[0255] (Example 2)
[0256] BODA (1.13 g, 4.5 mmol), DA-1 (0.59 g, 1.8 mmol), DA-2 (0.67 g, 2.7 mmol) and DA-4 (1.71 g, 4.5 mmol) were dissolved in NMP (16.4 g), reacted at 60°C for 3 hours, CBDA (0.86 g, 4.5 mmol) and NMP (3.4 g) were added, and reacted at 40°C for 12 hours to obtain a polyamic acid solution.
[0257] After adding NMP to the polyamic acid solution (16.4 g) to dilute to 6 mass%, acetic anhydride (2.9 g) and pyridine (0.9 g) as imidization catalysts were added and reacted at 80° C. for 3 hours. The reaction solution was put into methanol (190 ml) and the obtained precipitate was filtered. The precipitate was washed with methanol and dried under reduced pressure at 60° C. to obtain a polyimide powder (B). The imidization rate of the polyimide was 78%.
[0258] NMP (21.3 g) was added to the obtained polyimide powder (B) (2.7 g), and the mixture was dissolved by stirring at 70° C. for 12 hours. 2.7 g of 3AMP (1 wt % NMP solution) and BCS (17.8 g) were added to the solution, and the mixture was stirred at room temperature for 5 hours to obtain a liquid crystal aligning agent (B1).
[0259] (Example 3)
[0260] BODA (2.25 g, 9.0 mmol), DA-1 (0.60 g, 1.8 mmol), DA-3 (1.74 g, 7.2 mmol) and DA-4 (3.43 g, 9.0 mmol) were dissolved in NMP (32.1 g), and reacted at 60°C for 3 hours. Then, CBDA (1.76 g, 9.0 mmol) and NMP (6.8 g) were added, and the mixture was reacted at 40°C for 12 hours to obtain a polyamic acid solution.
[0261] After adding NMP to the polyamic acid solution (15.0 g) to dilute to 6 mass%, acetic anhydride (2.8 g) and pyridine (0.9 g) as imidization catalysts were added and reacted at 80° C. for 3 hours. The reaction solution was put into methanol (174 ml) and the obtained precipitate was filtered. The precipitate was washed with methanol and dried under reduced pressure at 60° C. to obtain a polyimide powder (C). The imidization rate of the polyimide was 77%.
[0262] NMP (20.3 g) was added to the obtained polyimide powder (C) (2.5 g), and the mixture was dissolved by stirring at 70° C. for 12 hours. 2.5 g of 3AMP (1 wt % NMP solution) and BCS (16.9 g) were added to the solution, and the mixture was stirred at room temperature for 5 hours to obtain a liquid crystal aligning agent (C1).
[0263] (Example 4)
[0264] BODA (2.25 g, 9.0 mmol), DA-1 (0.60 g, 1.8 mmol), DA-2 (1.79 g, 7.2 mmol) and DA-4 (3.43 g, 9.0 mmol) were dissolved in NMP (32.3 g), reacted at 60°C for 3 hours, CBDA (1.76 g, 9.0 mmol) and NMP (6.8 g) were added, and reacted at 40°C for 12 hours to obtain a polyamic acid solution.
[0265] After adding NMP to the polyamic acid solution (15.0 g) to dilute to 6% by mass, acetic anhydride (2.8 g) and pyridine (0.9 g) were added as imidization catalysts, and the mixture was reacted at 75° C. for 2.5 hours. The reaction solution was put into methanol (174 ml), and the obtained precipitate was filtered. The precipitate was washed with methanol and dried under reduced pressure at 60° C. to obtain a polyimide powder (D). The imidization rate of the polyimide was 69%.
[0266] NMP (19.7 g) was added to the obtained polyimide powder (D) (2.5 g), and the mixture was dissolved by stirring at 70° C. for 12 hours. 2.5 g of 3AMP (1 wt % NMP solution) and BCS (16.4 g) were added to the solution, and the mixture was stirred at room temperature for 5 hours to obtain a liquid crystal aligning agent (D1).
[0267] (Comparative Example 1)
[0268] BODA (25.6 g, 102.5 mmol), DA-1 (13.5 g, 41.0 mmol), p-PDA (6.7 g, 61.5 mmol) and DA-4 (39.0 g, 102.5 mmol) were dissolved in NMP (339.4 g), reacted at 60°C for 3 hours, and then CBDA (18.9 g, 96.3 mmol) (75.6 g) was added and reacted at 40°C for 12 hours to obtain a polyamic acid solution.
[0269] After adding NMP to the polyamic acid solution (260.0 g) to dilute to 6% by mass, acetic anhydride (52.3 g) and pyridine (16.2 g) were added as imidization catalysts, and the mixture was reacted at 80° C. for 3 hours. The reaction solution was put into methanol (3040 ml), and the obtained precipitate was filtered. The precipitate was washed with methanol and dried under reduced pressure at 60° C. to obtain a polyimide powder (E). The imidization rate of the polyimide was 70%.
[0270] NMP (28.6 g) was added to the obtained polyimide powder (E) (3.6 g), and the mixture was dissolved by stirring at 70° C. for 12 hours. 3AMP (1 wt % NMP solution) 3.6 g and BCS (23.8 g) were added to the solution, and the mixture was stirred at room temperature for 5 hours to obtain a liquid crystal aligning agent (E1).
[0271] (Comparative Example 2)
[0272] BODA (2.50 g, 10.0 mmol), DA-1 (0.66 g, 2.0 mmol), p-PDA (0.87 g, 8.0 mmol) and DA-4 (3.80 g, 8.0 mmol) were dissolved in NMP (31.3 g), reacted at 60°C for 3 hours, CBDA (1.88 g, 9.6 mmol) and NMP (7.5 g) were added, and reacted at 40°C for 12 hours to obtain a polyamic acid solution.
[0273] After adding NMP to the polyamic acid solution (15.0 g) to dilute to 6% by mass, acetic anhydride (3.1 g) and pyridine (1.0 g) as imidization catalysts were added and reacted at 80° C. for 3 hours. The reaction solution was put into methanol (175 ml) and the resulting precipitate was filtered. The precipitate was washed with methanol and dried under reduced pressure at 60° C. to obtain a polyimide powder (F). The imidization rate of the polyimide was 69%.
[0274] NMP (21.3 g) was added to the obtained polyimide powder (F) (2.7 g), and the mixture was dissolved by stirring at 70° C. for 12 hours. 2.7 g of 3AMP (1 wt % NMP solution) and BCS (17.8 g) were added to the solution, and the mixture was stirred at room temperature for 5 hours to obtain a liquid crystal aligning agent (F1).
[0275] <Fabrication of Liquid Crystal Cell and Measurement of Pretilt Angle>
[0276] (Example 5)
[0277] A liquid crystal unit was prepared using the liquid crystal alignment agent (A1) obtained in Example 1 according to the steps shown below. The liquid crystal alignment agent (A1) obtained in Example 1 was spin-coated on the ITO surface of an ITO electrode substrate having an ITO electrode pattern with a pixel size of 100 μm×300 μm and a line / line spacing of 5 μm, dried on a hot plate at 80°C for 90 seconds, and then sintered in a hot air circulation oven at 230°C for 15 minutes to form a liquid crystal alignment film with a film thickness of 100 nm.
[0278] Moreover, the liquid crystal aligning agent (A1) was spin-coated on the ITO surface where no electrode pattern was formed, and it dried with a hot plate at 80 degreeC for 90 seconds, and baked with a hot air circulation oven at 230 degreeC for 15 minutes, and the liquid crystal aligning film with a film thickness of 100 nm was formed.
[0279] For the above two substrates, after 4 μm bead spacers were spread on the liquid crystal alignment film of one substrate, a sealant (solvent-based thermosetting epoxy resin) was printed thereon. Then, the surface of the other substrate on which the liquid crystal alignment film was formed was placed inside, and after being bonded to the previous substrate, the sealant was cured to produce an empty cell. Liquid crystal MLC-3023 (trade name of Merck Ltd. (liquid crystal containing a polymerizable compound)) was injected into the empty cell by a reduced pressure injection method to produce a liquid crystal cell.
[0280] Then, while a DC voltage of 15 V was applied to the liquid crystal cell, a 10 J / cm 2 UV was irradiated through a 365 nm bandpass filter. Then, the pretilt angle of the pixel portion of the cell after UV irradiation was measured. The measurement was performed using an LCD analyzer LCA-LUV42A manufactured by Meiryo Technica Corporation. The results are shown in Table 1.
[0281] (Examples 6 to 12, Comparative Examples 3 to 6)
[0282] In Example 5, instead of the liquid crystal alignment agent (A1), the liquid crystal alignment agent shown in Table 1 obtained in Examples 1 to 4 or Comparative Example 1 or 2 is used, and UV irradiation is performed under the following conditions. Otherwise, a liquid crystal unit is prepared in the same manner as in Example 5, and for the liquid crystal unit after UV irradiation, the pretilt angle is measured in the same manner as in Example 5.
[0283] It should be noted that the UV irradiation was performed at 20 J / cm2 as shown in Table 1 in Examples 6, 8, 10, 12, and Comparative Examples 4 and 6. 2 .
[0284] The measurement results of the pretilt angles are summarized in the table.
[0285] [Table 1]
[0286]
[0287] As shown in Table 1, the tilt angles of the liquid crystal cells of Examples 5 to 8 were smaller than those of Comparative Examples 3 to 4, and Examples 9 to 12 were smaller than those of Comparative Examples 5 to 6, and it was confirmed that the tilt imparting ability was improved by using the liquid crystal display element of the present invention.
[0288] Industrial Applicability
[0289] The liquid crystal display element having a liquid crystal aligning film obtained from the liquid crystal aligning agent of the present invention has a wide viewing angle, a fast response speed, and a large contrast ratio, and can therefore be suitably used for large-screen and high-definition televisions, large monitors, and the like.
[0290] It should be noted that the entire contents of the specification, patent claims, and abstract of Japanese Patent Application No. 2018-202179 filed on October 26, 2018 are incorporated herein by reference as a public introduction to the specification of the present invention.
Claims
1. A liquid crystal alignment agent, characterized in that: The copolymer comprises a unit having a side chain represented by the following formula (1) and a unit having a side chain represented by the following formula (2), wherein the molar ratio of the unit having a side chain represented by the formula (1) to the unit having a side chain represented by the formula (2) is 5 / 95 to 95 / 5, R 1c , R 2c each independently represents an alkyl group having 1 to 10 carbon atoms, and Y c Represents a single bond or -CO-, Ar 1 represents phenylene, naphthylene or biphenylene, T 1c , T 2c Each independently represents a single bond, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH2O-, -N(CH3)-, -CON(CH3)- or -N(CH3)CO-, A c represents a single bond, an alkylene group having 1 to 20 carbon atoms which may be substituted with a fluorine atom, a divalent aromatic ring group having 6 to 12 carbon atoms, a divalent alicyclic group having 3 to 8 carbon atoms, or a divalent heterocyclic group selected from pyrrole, imidazole, pyridine, pyrimidine, pyrazine, pyridazine, triazine, indole, quinoline, carbazole, thiazole, purine, tetrahydrofuran and thiophene, n represents an integer of 1 to 4, and * represents a bonding position to an adjacent atom, Q represents a group selected from the following formulae (q-1) to (q-4), R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, R3 represents -CH2-, -NR-, -O- or -S-, R 1r , R 2r Each independently represents an alkyl group or an alkoxy group having 1 to 10 carbon atoms, a benzyl group or a phenethyl group, Ar 2 represents a divalent aromatic hydrocarbon group selected from phenylene, naphthylene and biphenylene, and the organic group may be substituted thereon, and the hydrogen atom may be substituted with a halogen atom, T 1r , T 2r Each independently represents a single bond, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH2O-, -N(CH3)-, -CON(CH3)- or -N(CH3)CO-, A r represents a single bond, an alkylene group having 1 to 20 carbon atoms which may be substituted with a fluorine atom, a divalent aromatic ring group having 6 to 12 carbon atoms, a divalent alicyclic group having 3 to 8 carbon atoms, or a divalent heterocyclic group selected from pyrrole, imidazole, pyridine, pyrimidine, pyrazine, pyridazine, triazine, indole, quinoline, carbazole, thiazole, purine, tetrahydrofuran and thiophene, and * represents a bonding position to an adjacent atom, 2. The liquid crystal alignment agent according to claim 1, wherein In the formula (1), -Ar 1 -(Y c -CHR 1c R 2c ) n Indicates the following (ch-1) to (ch-6), R 1c , R 2c This has the same meaning as the above formula (1).
3. The liquid crystal aligning agent according to claim 1 or 2, wherein: In the formula (2), Ar 2 represents a phenylene group or a biphenylene group, T 1r , T 2r each independently represents a single bond, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH- or -CH2O-, A r It represents a single bond, an alkylene group having 1 to 20 carbon atoms which may be substituted with a fluorine atom, a divalent aromatic ring group having 6 to 12 carbon atoms, or a divalent alicyclic group having 3 to 8 carbon atoms.
4. The liquid crystal aligning agent according to claim 1 or 2, wherein The copolymer is at least one copolymer selected from the group consisting of a polyimide precursor and a polyimide obtained by imidizing the polyimide precursor.
5. The liquid crystal aligning agent according to claim 1 or 2, wherein The copolymer is a copolymer having a side chain represented by the following formula (3) in addition to the side chain represented by the formula (1) and the side chain represented by the formula (2), l, m and n each independently represent an integer of 0 or 1, and R1 represents -(CH2) a -, -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CH2O-, -CH2OCO-, -COO- or -OCO-, -(CH2) a1 -A1-(CH2) a2 -A2-, wherein a is an integer from 1 to 15, A1 is an oxygen atom or -COO-*, wherein the connecting bond with * is (CH2) a2 bonding, A2 is an oxygen atom or *-COO-, in which the connecting bond with * is attached to (CH2) a2 bonding, a1 is an integer of 0 or 1, a2 is an integer of 1 to 10, R 2 , R 3 and R 4 Each independently represents a phenylene group, a fluorinated phenylene group or a cycloalkylene group, and R 5 represents a linear alkyl group having 2 to 24 carbon atoms, a fluorinated alkyl group having 2 to 24 carbon atoms, an alkoxy group having 2 to 24 carbon atoms, an alkoxyalkyl group having 2 to 20 carbon atoms, or a structure having a steroid skeleton, wherein R 5 In the case of a linear alkyl group having 2 to 24 carbon atoms or a fluorinated alkyl group having 2 to 24 carbon atoms, l+m+n≥1 is satisfied, and R 5 In the case of a structure having a steroid skeleton, l, m, and n represent 0, and R 1 Represents -(CH2) a -, -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CH2O-, -CH2OCO-, -COO- or -OCO-, wherein a is an integer from 1 to 15.
6. The liquid crystal aligning agent according to claim 1 or 2, wherein: The copolymer is a copolymer obtained by using a diamine represented by the following formula (d-1) as a part of the raw material. R 1c , R 2c , Y c ,Ar 1 , T 1c , T 2c , A c , n have the same meanings as in the above formula (1).
7. The liquid crystal aligning agent according to claim 1 or 2, wherein: The copolymer is a copolymer obtained by using a diamine represented by the following formula (d-2) as a part of the raw material. R 1r , R 2r , Y r ,Ar 2 , T 1r , T 2r , A r This has the same meaning as the above formula (2).
8. The liquid crystal aligning agent according to claim 1 or 2, wherein: The copolymer is a copolymer obtained by using a diamine represented by the following formula (d-3) as a part of the raw material. l, m, n and R 1 ~R 5 The definition is the same as that of the above formula (3), z represents an integer of 1 to 2, and Y3 is the following formula (Ar 3-1 )~(Ar 3-2 ) shown in the structure, A 3a represents a single bond or a divalent organic group having an aromatic group, A 3b represents a trivalent group having an aromatic group, *1 represents a para-R 1 -(R 2 ) l -(R 3 ) m -(R 4 ) n -R 5 , and *2 indicates the bonding position to -NH2.
9. The liquid crystal alignment agent according to claim 1 or 2, wherein: The copolymer is a copolymer obtained by using tetracarboxylic dianhydride represented by the following formulas [4] to [6] as a part of the raw material. Z 1 represents at least one structure selected from the following formulae [4a] to [4k], wherein in formula [5] or [6], j and k are each independently an integer of 0 or 1, and x and y each independently represent a single bond, a carbonyl group, an ester, a phenylene group, a sulfonyl group or an amide group, Z 1 ~Z 4 Each independently represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom or a benzene ring.
10. A liquid crystal alignment film, characterized in that: This is formed using the liquid crystal aligning agent according to any one of claims 1 to 9.
11. A liquid crystal display element, characterized in that: The liquid crystal alignment film comprises the liquid crystal alignment film according to claim 10 .
12. A method for manufacturing a liquid crystal display element, comprising: A step of applying the liquid crystal alignment agent according to any one of claims 1 to 9 on a substrate to form a coating film; A step of firing the coating film; and a step of bringing the obtained fired film into contact with a liquid crystal composition to form a liquid crystal layer.
13. A method for manufacturing a liquid crystal display element, comprising: A step of applying the liquid crystal alignment agent according to any one of claims 1 to 9 on a substrate to form a coating film; A step of firing the coating film; a step of bringing the obtained fired film into contact with a liquid crystal composition containing a polymerizable compound to form a liquid crystal layer; and a step of irradiating the liquid crystal layer with ultraviolet rays.