A method and system for treating tar residue
By adding a mixture of sulfur gram agent and tar solvent to coking enterprises for solid-liquid separation, the problems of viscosity and water content of tar residue are solved, drying and deodorization are achieved, coke quality and tar separation rate are improved, and the solution is solved. Environmental protection and transportation difficulties of coking enterprises.
Patent Information
- Application Number
- CN202110358049.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-01
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-04-01
AI Technical Summary
Coking enterprises have problems of viscosity and strong irritating odor when dealing with tar residues, which affects the accuracy of transportation and coal distribution. The existing oil residue separation methods lead to high moisture content of tar residues, which affects environmental protection.
The mixture of gram sulfur agent and tar solvent and steam is stirred under insulation conditions to perform solid-liquid separation to obtain dry residue powder, overcome viscosity and odor, and improve the tar separation rate.
The drying and deodorization of tar residue is achieved, the content of water and tar is reduced, the quality of coke is more accurate, the transportation is more convenient, and the separation rate and revenue of tar is improved.
Smart Images

Figure CN112940768B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of degreasing, and in particular to a method and system for treating tar residue. Background Art
[0002] With the further tightening of national environmental protection policies, the energy conservation, emission reduction and environmental protection work faced by coking enterprises are becoming more severe. How to reduce pollution and emissions has always been the top priority for the development of coking enterprises. The tar residue of the coking plant belongs to the category of hazardous waste. The treatment of coking oil residue cannot be done by simply burying or dumping it into the sea to transfer pollution. At present, there is a method of treating it by separating the oil residue, and adding the separated oil residue to the coal blending for re-coking. However, the tar residue obtained by this method still contains about 10% to 15% water and about 9% to 10% tar, so it is sticky and compacted with a strong pungent smell, which affects the accuracy of transportation and coal blending, and is not good for environmental protection.
[0003] In view of this, the present invention is proposed. Summary of the invention
[0004] One purpose of the present invention is to provide a method for treating tar residue, which fundamentally solves the problem that tar residue in coking enterprises is difficult to treat, adds an appropriate amount of sulfur-reducing agent to overcome the viscosity of tar, removes odor, and dries it into slag powder with less water and tar, so that coal blending can be accurate to ensure the quality of coke; the tar separation rate is high, and tar income is increased.
[0005] Another object of the present invention is to provide a tar residue processing system that can effectively dry the tar residue with high processing efficiency.
[0006] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0007] A method for treating tar residue comprises the following steps:
[0008] The mixture of tar residue, sulfur-removing agent, tar solvent and steam is stirred under heat preservation conditions, and then solid-liquid separation is carried out.
[0009] Preferably, the amount of the sulfur-removing agent added is 0.01% to 20% of the mass of the tar residue;
[0010] Preferably, the amount of the tar solvent added is 13% to 40% of the mass of the tar residue;
[0011] Preferably, the total mass content of tar and water in the tar residue is 18% to 22%;
[0012] Preferably, the tar solvent includes at least one of tar, diesel and phenol oil.
[0013] Preferably, in the stirred mixture, the total mass content of tar and water is 38% to 42%;
[0014] Preferably, the mass content of water in the tar residue obtained after the solid-liquid separation is 1% to 2%, and the mass content of tar is 2% to 3%;
[0015] Preferably, the insulation temperature is 60-70°C.
[0016] Preferably, the stirred mixture is ground before solid-liquid separation;
[0017] Preferably, the coal tar obtained after the solid-liquid separation is recycled;
[0018] Preferably, the tar residue obtained after the solid-liquid separation is blended with coal to produce coke.
[0019] The treatment system used in the above-mentioned tar residue treatment method comprises a pretreatment tank and a separator; the pretreatment tank comprises a pretreatment tank body and a jacket arranged outside the body; a motor is arranged on the pretreatment tank, a rotating shaft is connected to the output end of the motor, a stirrer is arranged on the rotating shaft, and the stirrer is arranged in the pretreatment tank body;
[0020] Preferably, a sieve plate located above the agitator is provided in the pretreatment tank body, the rotating shaft rotates through the sieve plate, and a tar residue scraper and a tar residue liquid wheel located above the sieve plate are circumferentially arranged on the side wall of the rotating shaft.
[0021] Preferably, the pretreatment tank is provided with a feed inlet and a slag discharge outlet;
[0022] Preferably, the feed inlet includes a tar residue feed inlet, a sulfur-removing agent feed inlet, a tar solvent feed inlet and an internal steam inlet;
[0023] Preferably, the jacket is provided with a jacket steam inlet and a condensed water outlet.
[0024] Preferably, a delivery pump is provided between the pretreatment tank and the separator.
[0025] Preferably, a grinder is provided between the pretreatment tank and the separator;
[0026] Preferably, the grinder comprises a colloid mill and / or a double drum mill.
[0027] Preferably, harmful gas collection ports are respectively provided on the pretreatment tank and the separator, and the harmful gas collection ports are connected to the exhaust gas treatment system.
[0028] Preferably, the separator comprises a slag outlet and an oil outlet;
[0029] Preferably, the oil outlet is connected to the underground tank of the cold drum section through a pipeline;
[0030] Preferably, the slag outlet is connected to a cooler.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The tar residue treatment method of the present invention fundamentally solves the problem that tar residue in coking enterprises is difficult to treat. A certain amount of sulfur-reducing agent is added to overcome the viscosity of tar, remove the stench, and dry it into slag powder with less water and tar, so that coal blending is accurate and the quality of coke is ensured; the tar separation rate is high, and the tar income is increased. The tar residue powder obtained by the drying method of the present invention is dry, loose and non-sticky, and is easy to transport, so that coal blending is accurate and the quality of coke is ensured; the process is simple and convenient, and the degree of automation is high.
[0033] (2) The processing system of the present invention can effectively dry the tar residue and has high processing efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 This is a schematic diagram of a tar residue treatment system of the present invention;
[0036] Figure 2 It is a structural schematic diagram of the pretreatment tank of the present invention;
[0037] Figure 3 The present invention is a process flow chart of the method for treating tar residue.
[0038] Reference numerals:
[0039] 101-pretreatment tank, 102-grinder, 103-transfer pump, 104-separator, 105-cooler, 106-underground tank, 1-reduction motor, 2-pretreatment tank cover, 3-internal steam inlet, 4-jacket steam inlet, 5-jacket, 6-agitator, 7-condensate outlet, 8-tar residue liquid wheel, 9-tar solvent inlet, 10-tar residue scraper, 11-sieve plate, 12-slag discharge port, 13-sulfur agent feed port, 14-tar residue feed port. DETAILED DESCRIPTION
[0040] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0041] According to one aspect of the present invention, the present invention relates to a method for treating tar residue, comprising the following steps:
[0042] The mixture of tar residue, sulfur-removing agent, tar solvent and steam is stirred under heat preservation conditions, and then solid-liquid separation is carried out.
[0043] The method of the present invention fundamentally solves the problem that tar residue of coking enterprises is difficult to handle. By adding a certain amount of sulfur-reducing agent, the tar residue is overcome in viscosity, the stench is removed, and the residue is dried into a slag powder with less water and less tar (dry and odorless), so that the coal blending is accurate to ensure the quality of coke, the separation rate of tar is high, and the tar income is increased.
[0044] The sulfur-reducing agent of the present invention is composed of the following components in parts by weight: 1-100 parts of wood fiber, 1-99 parts of oil residue and 0.1-0.7 parts of washing powder, and the total weight of the wood fiber and the oil residue is 100 parts. The wood fiber is at least one of wood chips, bamboo chips, bark, thatch, fruit shell, rice husk, straw, stalk and sugarcane. The oil residue is oil residue after oil is pressed from plant oil or animals and plants; the plant oil is at least one of rapeseed, tea seed, camphor seed, white wood seed, peanut, sesame, bean, cotton seed, olive oil seed and white wax on white ash tree; the oil residue after oil is pressed from animals and plants is at least one of rapeseed dregs, tea dregs, bean dregs, peanut dregs, sesame dregs, olive oil residue and animal oil residue.
[0045] Preferably, the sulfur-removing agent is composed of the following components in parts by weight: 10-40 parts of wood fiber, 50-90 parts of oil residue and 0.1-0.7 parts of washing powder, and the total weight of the wood fiber and the oil residue is 100 parts.
[0046] Preferably, the sulfur-removing agent is composed of the following components in parts by mass:
[0047] 1-5 parts of bamboo chips, 2-5 parts of rice husks, 3-10 parts of rice straw, 2-10 parts of straw, 2-10 parts of sugarcane, 10-20 parts of camphor seeds, 10-20 parts of olive oil seeds, 20-30 parts of rapeseed dregs, 10-20 parts of animal oil residues and 0.2-0.5 parts of washing powder.
[0048] Preferably, the sulfur-removing agent is composed of the following components in parts by mass:
[0049] 5 parts of bamboo scraps, 5 parts of rice husks, 5 parts of rice straws, 10 parts of straws, 10 parts of sugar canes, 10 parts of camphor seeds, 20 parts of olive oil seeds, 20 parts of rapeseed dregs, 15 parts of animal oil residues and 0.3 parts of washing powder.
[0050] In one embodiment, the wood fiber is 1-100 parts, and can also be 1 part, 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 60 parts, 70 parts, 80 parts, 90 parts or 100 parts.
[0051] In one embodiment, the oil residue is 1-99 parts, and can also be 1 part, 5 parts, 10 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 80 parts, 90 parts or 99 parts.
[0052] In one embodiment, the washing powder is 0.1 to 0.7 parts, and can also be 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts or 0.7 parts.
[0053] Preferably, the added amount of the desulfurizing agent is 0.01% to 20% of the mass of the tar residue.
[0054] In one embodiment, the addition amount of the desulfurizing agent is 0.01% to 20% of the mass of the tar residue, and 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20% can also be selected.
[0055] Preferably, the added amount of the tar solvent is 13% to 40% of the mass of the tar residue.
[0056] In one embodiment, the tar solvent is added in an amount of 13% to 40% of the mass of the tar residue, and 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or 40% can also be selected.
[0057] Preferably, the total mass content of tar and water in the tar residue is 18% to 22%.
[0058] In one embodiment, the total mass content of tar and water in the tar residue is 18% to 22%, and 18%, 19%, 20%, 21% or 22% can also be selected.
[0059] The present invention adopts tar, diesel oil, phenol oil or other substances capable of dissolving tar to dissolve the tar in the tar residue.
[0060] Preferably, in the stirred mixture, the total mass content of tar and water is 38% to 42%.
[0061] In one embodiment, in the tar residue obtained after the stirring, the total mass content of tar and water is 38% to 42%, and can also be 38%, 39%, 40%, 41% or 42%.
[0062] Preferably, in the tar residue obtained after the solid-liquid separation, the mass content of water is 1% to 2%, and the mass content of tar is 2% to 3%.
[0063] In one embodiment, the mass content of water in the tar residue obtained after the solid-liquid separation is 1% to 2%, and can also be 1.1%, 1.3%, 1.5%, 1.8% or 2%. The mass content of tar is 2% to 3%, and can also be 2%, 2.2%, 2.5%, 2.7% or 3%.
[0064] Preferably, water vapor is used for the heat preservation, and the heat preservation temperature is 60-70°C.
[0065] In one embodiment, the insulation temperature is 60-70°C, and can also be 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C or 70°C.
[0066] Preferably, the tar solvent includes at least one of tar, diesel and phenol oil.
[0067] Preferably, the stirred mixture is ground before solid-liquid separation.
[0068] Preferably, the coal tar obtained after the solid-liquid separation is recycled.
[0069] Preferably, the tar residue obtained after the solid-liquid separation is blended with coal to produce coke.
[0070] The coal tar after solid-liquid separation in the present invention is sent to the underground tank of the cold drum section through a pipeline for collection and reuse, and the separated oil residue is condensed and dried and sent to the coal yard for re-distribution and coking.
[0071] According to another aspect of the present invention, the present invention also relates to a treatment system used for implementing the above-mentioned tar residue treatment method, comprising a pretreatment tank and a separator; the pretreatment tank comprises a pretreatment tank body and a jacket arranged outside the body; a motor is arranged on the pretreatment tank, a rotating shaft is connected to the output end of the motor, a stirrer is arranged on the rotating shaft, and the stirrer is arranged in the pretreatment tank body;
[0072] Preferably, a sieve plate located above the agitator is provided in the pretreatment tank body, the rotating shaft rotates through the sieve plate, and a tar residue scraper and a tar residue liquid wheel located above the sieve plate are circumferentially arranged on the side wall of the rotating shaft.
[0073] The processing system of the present invention can effectively dry the tar residue.
[0074] The tar residue discharged from the discharge port of the mechanical scraper trough of the present invention enters the pretreatment tank (tar residue tank) through a chute with insulation. The tar residue tank is connected to the discharge port of the mechanical scraper trough in a closed manner. The tar residue tank is insulated by a jacket, and an agitator is arranged inside to prevent the tar residue from precipitating and condensing. At the same time, the tar residue tank has steam for heating to maintain 60-70°C to produce a certain amount of distilled water, which is used to dilute the oil residue with the solvent to ensure the smoothness of the material pipeline transportation.
[0075] The sieve plate is connected to the inner wall of the pretreatment tank body, and the connection is a detachable connection; the sieve plate is arranged horizontally.
[0076] The sieve holes of the sieve plate are circular holes with a diameter of 6 to 12 mm, preferably 10 mm; the spacing between the holes is 12 mm; the distance between the tar residue scraper and the sieve plate is 0.5 to 2 mm, preferably 1 mm; the distance between the tar residue liquid wheel and the sieve plate is 0.5 to 2 mm, preferably 1 mm.
[0077] Preferably, the pretreatment tank is provided with a feed inlet and a slag discharge outlet.
[0078] Preferably, the feed inlet includes a tar residue feed inlet, a sulfur-removing agent feed inlet, a tar solvent feed inlet and an internal steam inlet.
[0079] The tar residue feed port and the desulfurizing agent feed port of the present invention are arranged on the upper cover of the pretreatment tank.
[0080] Preferably, a steam pipe is provided in the pretreatment tank.
[0081] Preferably, there are 2 to 3 steam pipes with a diameter of 20 to 50 mm.
[0082] In one embodiment, the diameter of the steam pipe is 20-50 mm, and may be 20 mm, 25 mm, 30 mm, 35 mm, 40 mm, 45 mm or 50 mm.
[0083] Preferably, the jacket is provided with a jacket steam inlet and a condensed water outlet.
[0084] Preferably, a delivery pump is provided between the pretreatment tank and the separator.
[0085] Preferably, a grinder is provided between the pretreatment tank and the separator;
[0086] Preferably, the grinder comprises a colloid mill and / or a double drum mill.
[0087] The thin tar residue discharged from the tar residue tank contains tar and distilled water, which passes through a jacketed insulation pipeline, a grinder, and a delivery pump in turn into a separator for solid-liquid separation; the separator is a high-efficiency centrifuge.
[0088] Preferably, harmful gas collection ports are respectively provided on the pretreatment tank and the separator, and the harmful gas collection ports are connected to the exhaust gas treatment system.
[0089] Harmful gas collection ports are left on the tar residue tank and high-efficiency centrifuge, which are connected to the VOC or other tail gas treatment systems in the chemical production area for unified treatment.
[0090] Preferably, the separator comprises a slag outlet and an oil outlet;
[0091] Preferably, the oil outlet is connected to the underground tank of the cold drum section through a pipeline;
[0092] Preferably, the slag outlet is connected to a cooler.
[0093] The present invention will be further explained below with reference to specific embodiments.
[0094] Example 1
[0095] A tar residue processing system, comprising a pretreatment tank 101 and a separator 104; the pretreatment tank 101 comprises a pretreatment tank body and a jacket 5 arranged outside the body; a reduction motor 1 is arranged on the pretreatment tank 101, and a rotating shaft is connected to the output end of the reduction motor 1, and a stirrer 6 is arranged on the rotating shaft, and the stirrer 6 is arranged in the pretreatment tank body; a sieve plate 11 located above the stirrer 6 is arranged in the pretreatment tank body, and the rotating shaft rotates through the sieve plate 11, and a tar residue scraper 10 and a tar residue liquid wheel 8 located above the sieve plate are arranged relatively along the circumferential direction on the side wall of the rotating shaft; the sieve plate 11 is horizontally arranged and detachably connected to the inner wall of the pretreatment tank body; the sieve holes of the sieve plate 11 are circular holes with a diameter of 10 mm, and the spacing between the holes is 12 mm; the distance between the tar residue scraper 10 and the sieve plate 11 is 1 mm, so The distance between the tar residue liquid wheel 8 and the sieve plate 11 is 1 mm; the pretreatment tank 101 is provided with a pretreatment tank upper cover 2, and the pretreatment tank upper cover 2 is provided with a desulfurizing agent feed port 13 and a tar residue feed port 14; the pretreatment tank 101 is provided with a tar solvent inlet 9, an internal steam inlet 3 and a slag discharge port 12; the jacket 5 is provided with a jacket steam inlet 4 and a condensate outlet 7; a delivery pump 103 is provided between the pretreatment tank 101 and the separator 104; a grinder 102 is provided between the pretreatment tank 101 and the separator 104; harmful gas collection ports are respectively provided on the pretreatment tank 101 and the separator 104, and the harmful gas collection ports are connected to the exhaust gas treatment system; the separator 104 includes a slag outlet and an oil outlet; the oil outlet is connected to the underground tank 106 of the cold drum section through a pipeline; the slag outlet is connected to the cooler 105.
[0096] A method for treating tar residues, using the above-mentioned tar residue treatment system, comprises the following steps:
[0097] Take 1 ton of tar residue from the bottom of the mechanized clarification tank of the coking plant and put it into the pretreatment tank through the inlet. Add 400 kg of tar and 10 kg of sulfur agent. Insert 3 rods evenly into the pretreatment tank. The steam pipe is used to allow 100℃ steam to flow in, and the temperature in the tank is maintained at 70℃. The tar slurry is stirred continuously and the hot tar slurry is pumped into the separator by a delivery pump. The separated tar water flows into the underground tank (tar tank) from the bottom. The separated tar residue is sent to the cooler. The dry powder of the tar residue from the cooler is sent to the coal blending system for blending and refining into coke.
[0098] The sulfur-reducing agent is composed of the following components in parts by mass: 5 parts of bamboo chips, 5 parts of rice husks, 5 parts of rice straw, 10 parts of straw, 10 parts of sugarcane, 10 parts of camphor seeds, 20 parts of olive oil seeds, 20 parts of rapeseed dregs, 15 parts of animal oil residues and 0.3 parts of washing powder.
[0099] The schematic diagram of the tar slag processing system in this embodiment is as follows Figure 1 As shown;
[0100] The structural schematic diagram of the pretreatment tank in this embodiment is as follows Figure 2 As shown;
[0101] The process flow chart of the tar residue treatment method of this embodiment is as follows Figure 3 shown.
[0102] Example 2
[0103] A tar residue processing system, except that there are two steam pipes with a diameter of 30 mm, other conditions are the same as those in Example 1.
[0104] A method for treating tar residues, using the above-mentioned tar residue treatment system, comprises the following steps:
[0105] 1.5 tons of oil residue from the mechanized clarification tank of the coking plant is taken into the pretreatment tank through the feed port, 200 kg of diesel and 30 kg of desulfurizing agent are added, the pretreatment tank is evenly inserted with a steam pipe to maintain the temperature in the tank at 70°C, and the mixture is stirred continuously. The hot tar slurry is pumped into the separator with a pump, and the separated oil and water flow into the underground tank (tar tank) from the bottom, and the separated tar residue is sent to the cooler, and the dry powder of the tar residue coming out of the cooler is sent to the coal blending system for blending with coal to refine coke; the desulfurizing agent is the same as that in Example 1.
[0106] Example 3
[0107] A tar residue processing system, except that the diameter of the steam pipe is 30 mm, other conditions are the same as those in Example 1.
[0108] A method for treating tar residues, using the above-mentioned tar residue treatment system, comprises the following steps:
[0109] Take 1 ton of tar residue produced during tar fractionation and refinement through the feed inlet pretreatment tank, add 300 kg of phenol oil and 200 kg of desulfurizing agent, insert steam pipes evenly vertically into the pretreatment tank to maintain 65°C in the tank, stir it continuously and fully, use a pump to pump the hot tar slurry into a separator, let the separated oil and water flow into an underground tank (tar tank) from the bottom, send the separated tar residue to a cooler, and send the dry powder of the tar residue coming out of the cooler to a coal blending system for blending with coal to produce coke; the desulfurizing agent is the same as that in Example 1.
[0110] Example 4
[0111] A method for treating tar residue, except that the amount of sulfur-removing agent added is 0.5% of the pretreated tar residue, other conditions are the same as those in Example 1.
[0112] Example 5
[0113] A method for treating tar residue, except that the amount of sulfur-removing agent added is 1% of the pretreated tar residue, other conditions are the same as those in Example 1.
[0114] Example 6
[0115] A method for treating tar residue, except that the amount of sulfur-removing agent added is 2% of the pretreated tar residue, other conditions are the same as those in Example 1.
[0116] Example 7
[0117] A method for treating tar residue, except that the amount of sulfur-removing agent added is 5% of the pretreated tar residue, other conditions are the same as those in Example 1.
[0118] Example 8
[0119] A method for treating tar residue, except that the amount of sulfur-removing agent added is 8% of the pretreated tar residue, other conditions are the same as those in Example 1.
[0120] Comparative Example 1
[0121] A method for treating tar residue, except that no sulfur-removing agent is added, other conditions are the same as those in Example 1.
[0122] Experimental Example 1
[0123] The effects of different amounts of sulfur-removing agent added on the treated tar residue are shown in Table 1.
[0124] Table 1 Effect of different amounts of sulfur-reducing agent on treated tar residue
[0125]
[0126] It can be seen from Table 1 that when no desulfurizing agent is added, the viscosity of the tar-slag mixture is 2.324, and the fluidity is very poor. Only by adding 0.5% of desulfurizing agent, the viscosity can be reduced to 1.962, and by continuing to increase the amount of desulfurizing agent to 5%, the viscosity can be further reduced to 0.30. It can be seen that the addition of an appropriate amount of desulfurizing agent in the present invention can significantly reduce the viscosity of the sulfur-salt mixture, improve its looseness, make transportation convenient, and make coal blending convenient and accurate, and the quality of coke is not affected.
[0127] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for treating tar residue, characterized in that: The following steps are involved: The mixture of tar residue, sulfur-removing agent, tar solvent and steam is stirred under heat preservation conditions, and then solid-liquid separation is performed; The tar solvent includes at least one of tar, diesel and phenol oil; The amount of the sulfur-removing agent added is 0.01% to 20% of the mass of the tar residue; The amount of the tar solvent added is 13% to 40% of the mass of the tar residue; The insulation temperature is 60-70°C; The sulfur-removing agent is composed of the following components in parts by mass: 1-5 parts of bamboo chips, 2-5 parts of rice husks, 3-10 parts of rice straws, 2-10 parts of straws, 2-10 parts of sugarcane, 10-20 parts of camphor seeds, 10-20 parts of olive oil seeds, 20-30 parts of rapeseed dregs, 10-20 parts of animal oil residues and 0.2-0.5 parts of washing powder.
2. The method for treating tar residue according to claim 1, characterized in that: The total mass content of tar and water in the tar residue is 18% to 22%.
3. The method for treating tar residue according to claim 1, characterized in that: In the stirred mixture, the total mass content of tar and water is 38% to 42%.
4. The method for treating tar residue according to claim 1, characterized in that: In the tar residue obtained after the solid-liquid separation, the mass content of water is 1% to 2%, and the mass content of tar is 2% to 3%.
5. The method for treating tar residue according to claim 1, characterized in that: The stirred mixture is ground before solid-liquid separation.
6. The method for treating tar residue according to claim 5, characterized in that: The coal tar obtained after the solid-liquid separation is recycled.
7. The method for treating tar residue according to claim 5, characterized in that: The tar residue obtained after the solid-liquid separation is mixed with coal to produce coke.
8. The method for treating tar residue according to claim 1, characterized in that: The treatment system used includes a pretreatment tank and a separator; the pretreatment tank includes a pretreatment tank body and a jacket arranged outside the body; a motor is arranged on the pretreatment tank, a rotating shaft is connected to the output end of the motor, a stirrer is arranged on the rotating shaft, and the stirrer is arranged in the pretreatment tank body; A sieve plate located above the agitator is arranged in the pretreatment tank body, the rotating shaft rotates through the sieve plate, and a tar residue scraper and a tar residue liquid wheel located above the sieve plate are arranged oppositely along the circumferential direction on the side wall of the rotating shaft.
9. The method for treating tar residue according to claim 8, characterized in that: The pretreatment tank is provided with a feed inlet and a slag discharge outlet; The feed inlets include a tar residue feed inlet, a sulfur-removing agent feed inlet, a tar solvent feed inlet and an internal steam inlet; The jacket is provided with a jacket steam inlet and a condensed water outlet.
10. The method for treating tar residue according to claim 8, characterized in that: A delivery pump is arranged between the pretreatment tank and the separator.
11. The method for treating tar residue according to claim 8, characterized in that: A grinder is arranged between the pretreatment tank and the separator.
12. The method for treating tar residue according to claim 11, characterized in that: The grinding mill includes a colloid mill and / or a double drum mill.
13. The method for treating tar residue according to claim 8, characterized in that: The pretreatment tank and the separator are respectively provided with harmful gas collecting ports, and the harmful gas collecting ports are connected to the waste gas treatment system.
14. The method for treating tar residue according to claim 8, characterized in that: The separator comprises a slag outlet and an oil outlet; The oil outlet is connected to the underground tank of the cold drum section through a pipeline; The slag outlet is connected to a cooler.