Low permeability polybenzimidazole (PBI) membrane for redox flow batteries
By using a polybenzimidazole gel membrane formed by a combination of polyphosphoric acid and aromatic compounds, the problems of low efficiency and high cost of redox flow battery membranes under high current loads are solved, and high conductivity and stability are achieved. The size and cost of the battery stack are reduced.
Patent Information
- Application Number
- CN201980073268.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-09-14
- Filing Date
- 2019-09-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-09-13
AI Technical Summary
Existing redox flow battery membranes exhibit low efficiency and high cost under high current loads. Traditional PBI membranes have low ion conductivity and are not durable, making it difficult to operate stably under high current conditions.
Polyphosphoric acid (PPA) and aromatic or heteroaromatic tetraamino compounds are combined with aromatic or heteroaromatic carboxylic acid compounds to form a polybenzimidazole (PBI) gel film through heating and polymerization, which is then hydrolyzed to form phosphoric acid and solidified. Forming a PBI gel film capable of maintaining structure at high liquid content, and improving its conductivity and stability through densification.
A redox flow battery membrane that operates efficiently under high current loads is achieved, with high ionic conductivity and low permeability, reducing the cost and volume of the battery stack while improving the mechanical and chemical stability of the membrane.
Smart Images

Figure CN112956056B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of U.S. Provisional Patent Application Serial No. 62 / 731,152, filed on September 14, 2018, entitled “Low Permeability Polybenzimidazole (PBI) Gel Membranes for Flow Batteries,” which is incorporated herein by reference for all purposes.
[0003] Federal Research Statement
[0004] This invention was made with government support under Grant No. DE-AR0000767 awarded by the Department of Energy. The government has certain rights in this invention.
[0005] background
[0006] The increasing demands on the energy sector have created new demands for large-scale energy storage devices that have additional impacts in grid management and backup power while seamlessly integrating with new renewable energy devices. Redox flow batteries have unmet potential for efficiently storing large amounts of energy and meeting cost requirements for meeting such demands. Redox flow batteries are charged and discharged by using a positive electrode electrolyte solution and a negative electrode electrolyte solution separated by an ion exchange membrane, each electrolyte solution containing metal ions (active materials) that form a redox pair (also known as a redox couple), the valence state of which is changed by oxidation-reduction.
[0007] Unfortunately, widespread adoption of redox flow batteries has been limited by the high cost of device manufacturing. For example, in vanadium redox flow batteries (VRBs), a major portion of the cost is attributed to the vanadium electrolyte. Such costs can be reduced by reducing the size of the electrochemical stack. However, in order to achieve this efficiently and maintain high power density, the battery must be able to operate at high current loads for many cycles. Conventional membranes used in redox flow batteries (usually perfluorosulfonic acid membranes such as ) are poor ion conductors and cannot sustain operation at high current loads, and therefore cells incorporating these membranes require larger cell stacks at higher costs. There has been a surge in membrane development activity in an attempt to reduce the cost of redox flow batteries and improve overall performance, with limited success.
[0008] Ion exchange membranes are the main components of redox flow batteries and have a significant impact on the output, capacity, life and cost of the battery. In addition to the requirements for low crossover of redox pairs to electrolyte ions and the ability to function at high current loads, ion exchange membranes must exhibit mechanical and chemical stability and high durability. The ion exchange membranes of redox flow batteries are always immersed in the electrolyte solution and therefore must be able to resist degradation due to oxidation, etc., and the durability of the membrane becomes the main factor determining the life of the redox flow battery.
[0009] Certain types of phosphoric acid (PA)-doped polybenzimidazole (PBI) membranes have been considered for a variety of electrical applications. Conventional PBI membranes are most notably known for their performance as high temperature polymer electrolyte membranes. Conventional PBI membranes have also been considered for a variety of new devices, such as electrochemical hydrogen separation, SO2 depolarized electrolyzers, and redox flow batteries. To date, research on PBI membranes for redox flow batteries has focused on conventional meta-polybenzimidazole (m-PBI) and its derivatives. Conventional PBI membranes for electrochemical applications have been prepared by solution casting in N,N'-dimethylacetamide (DMAc) to form a dense membrane, followed by absorption of the formed membrane into the desired electrolyte, known as the "conventional absorption process". Unfortunately, these conventional PBI membranes have shown extremely low ionic conductivity (less than 20 mS·cm) when absorbed into electrolyte solutions. -1 ) and cannot exceed about 100mAcm -2 Furthermore, the conventional absorption process for conventional PBI membranes is a time-consuming, environmentally unfriendly technology, which increases the cost of the membrane manufacturing process.
[0010] Recently, a process for preparing PBI membranes has been developed, which includes directly casting a polymeric composition containing a PBI polymer in a polyphosphoric acid (PPA) solvent. The PPA solvent is then hydrolyzed to PA (PA is a poor solvent for PBI) to induce the solidification of the PBI membrane, which is formed by absorption of PA.
[0011] What is needed in the art is an ion exchange membrane for a redox flow battery that exhibits low permeability to the active redox species of the battery combined with high ionic conductivity and can operate at high current loads while being highly stable and durable in the challenging environment of a redox flow battery.
[0012] Overview
[0013] According to one embodiment, a method for forming a redox flow battery membrane is disclosed. The method may include forming a polymeric composition comprising polyphosphoric acid (PPA), an aromatic or heteroaromatic tetraamino compound, and an aromatic or heteroaromatic carboxylic acid compound. The aromatic carboxylic acid compound may be an aromatic or heteroaromatic polycarboxylic acid or its ester, anhydride or acid chloride, or an aromatic or heteroaromatic diamino carboxylic acid. The method also includes polymerizing the compounds of the polymeric composition, such as by heating the polymer, to affect the polymerization of the compounds and the formation of a polybenzimidazole (PBI) solution.
[0014] After polymerization, the PBI solution can be shaped to form a membrane precursor, and the PPA of the solution can be hydrolyzed to form phosphoric acid (PA) and water, and the polymer of the membrane precursor is cured to form a PBI gel membrane that absorbs PA and water. The PBI gel membrane is different from previously known conventional PBI membranes because it can incorporate high liquid content and maintain structure, i.e., can maintain a self-supporting structure even at a low solid content of, for example, about 40 wt.% or less.
[0015] The method may also include treating the gel membrane to densify the gel membrane and form a densified PBI gel membrane or a dried PBI membrane.After densification, the method may include re-swelling the PBI membrane by absorbing a redox flow battery supporting electrolyte, one example of which is sulfuric acid.
[0016] Also disclosed is a redox flow battery membrane, which includes a densified PBI gel membrane and a redox flow battery supporting electrolyte absorbed in the densified PBI gel membrane. The redox flow battery membrane can exhibit high ionic conductivity, such as about 50 mS / cm or more, and can also exhibit VO 2+ Low ion permeability, for example about 10 -7 cm 2 / s or lower.
[0017] A redox flow battery incorporating a densified PBI gel membrane is also described. The redox flow battery may include a densified PBI gel membrane as described that separates an anolyte solution and a catholyte solution and may be operated at high current densities, such as about 50 mA / cm 2 or greater operating under low crossover of redox couple ions. The redox flow battery may include other battery components as known in the art (eg, electrodes, current collectors, flow lines, etc.) and may include a single cell or multiple cells in a single cell stack or multiple cell stacks. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] A full and enabling disclosure of the subject matter, including the best mode thereof, as would occur to one of ordinary skill in the art, is more particularly set forth in the remainder of this specification (including with reference to the accompanying drawings), wherein:
[0020] Figure 1 The dimensions of the membranes used in this disclosure are defined.
[0021] Figure 2 A redox flow battery as may be incorporated into a membrane as described herein is schematically illustrated.
[0022] Figure 3 A multi-cell stack that may be included in a redox flow battery as described is schematically illustrated.
[0023] Figure 4 The voltage efficiency (VE), coulombic efficiency (CE), and energy efficiency (EE) of VRBs incorporating membranes as described herein are presented.
[0024] Figure 5 The VE, CC, and EE of VRB incorporated into films as described herein are presented.
[0025] Figure 6 The VE, CC, and EE of VRB incorporated into films as described herein are presented.
[0026] Figure 7 The VE, CC, and EE of VRB incorporated into films as described herein are presented.
[0027] Figure 8 The VE, CC, and EE of VRB incorporated into films as described herein are presented.
[0028] Fig. 9 The VE, CC, and EE of VRB incorporated into comparative films are presented.
[0029] Repeat use of reference characters in the present specification and drawings is intended to represent same or analogous features or elements of the invention.
[0030] Details
[0031] The various embodiments of the disclosed subject matter will now be referred to in detail, one or more examples of which are set forth below. Each embodiment is provided by way of explanation of this subject matter rather than by way of limitation. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made in this disclosure without departing from the scope or spirit of this subject matter. For example, a feature shown or described as a part of one embodiment may be used in another embodiment to produce yet other embodiments.
[0032] The present disclosure generally relates to redox flow battery ion exchange membranes, methods for forming the membranes, and redox flow batteries incorporating the membranes. The redox flow battery membranes are based on polybenzimidazole (PBI) membranes, and more specifically, on PBI gel membranes. As used herein, the term "gel" generally refers to a polymer matrix that can incorporate a high liquid content and maintain a self-supporting structure. For example, a PBI gel membrane as described herein can incorporate about 60 wt.% or more, about 65 wt.% or more, about 75 wt.% or more, about 80 wt.% or more, or about 85 wt.% or more of liquid by weight of the composite membrane (total solids plus liquid content) without losing the structure of the polymer matrix. In one embodiment, the PBI gel membrane can incorporate from about 60 wt.% to about 95 wt.% of liquid while maintaining a self-supporting semi-rigid structure, i.e., a structure that can be manipulated and exhibits flexibility without losing the polymer matrix, such as Figure 1 As indicated in Figure 1 The figure shows a membrane 12 as described herein in both a flat and slightly curved configuration. In addition, the PBI gel can be processed to remove liquid from the gel and then reabsorb the liquid to re-swell without losing the structure of the polymer matrix.
[0033] The redox flow battery membrane can exhibit low permeability to redox couple ions while maintaining high ionic conductivity, allowing for the formation of cells that can operate at high performance under high current load conditions, which can translate into redox flow batteries having smaller and lower cost electrochemical stacks that provide the same or better performance than the prior art. For example, in some embodiments, the redox flow battery membrane as described can be permeable to members of the redox couple, such as VO 2+ or VO 4+ Shows about 10 -7 cm 2 / s or lower, such as about 5×10 -8 cm 2 / s or lower, about 10 - 8 cm 2 / s or lower or about 5×10 -9 cm 2 / s or lower permeability.
[0034] Beneficially, the redox flow battery membrane can exhibit low redox couple crossover characteristics while maintaining electrochemical activity. For example, the redox flow battery membrane as described can exhibit an in-plane ionic conductivity of about 50 mS / cm in 2.6 M sulfuric acid solution or even higher in some embodiments, such as about 100 mS / cm or about 200 mS / cm in some embodiments.
[0035] Furthermore, in some embodiments, cells incorporating the disclosed membranes can be operated at high current densities, such as about 50 mA / cm 2 or higher, for example, from about 100 mA / cm 2 To about 500mA / cm 2 In addition, cells incorporating redox flow battery membranes can be operated at high efficiencies. By way of example, at 242 mA / cm 2 At current densities of 483 mA / cm2, cells incorporating membranes as described can exhibit coulombic efficiencies (CE) of about 90% or greater, such as from about 94% to about 99% in some embodiments; energy efficiencies (EE) of about 70% or greater, such as from about 73% to about 84% in some embodiments; and voltage efficiencies (VE) of about 75% or greater, such as from about 78% to about 80%. At 483 mA / cm2, cells incorporating membranes as described can exhibit coulombic efficiencies (CE) of about 90% or greater, such as from about 94% to about 99% in some embodiments; energy efficiencies (EE) of about 70% or greater, such as from about 73% to about 84% in some embodiments; and voltage efficiencies (VE) of about 75% or greater, such as from about 78% to about 8 2 At current densities of about 100 % or more, cells incorporating membranes as described can exhibit a CE of 85% or greater, for example in some embodiments from about 87% to about 99%; an EE of about 50% or greater, for example in some embodiments from about 54% to about 75%; and a VE of about 60% or greater, for example from about 62% to about 77%.
[0036] The performance characteristics of the disclosed redox flow battery membranes are based on the use of densified PBI gel membranes. Batteries incorporating the membranes are greatly improved as compared to batteries incorporating ion exchange membranes based on conventional PBI polymer membranes, which exhibit very low ionic conductivities, e.g., less than 20 mS / cm. In addition, batteries incorporating conventional PBI polymer membranes are unable to operate at temperatures above about 80 mA / cm. 2The current density works. Without wishing to be bound by any particular theory, it is believed that the excellent properties of the disclosed redox flow battery membrane are due to the morphology of the polymer matrix forming the membrane structure. As further described herein, the disclosed PBI membrane is formed according to a method comprising hydrolysis of a PPA polymer solvent and subsequent solidification of the PBI polymer in a hydrolyzate (PA), followed by densification of the gel film thus formed. It is believed that this initial in-situ hydrolysis and polymer solidification lead to the formation of an ordered polymer matrix, which is different in molecular structure from the conventional organic solution cast PBI membrane, which is cast as a solution of an organic solvent, followed by solidification by removing the organic solvent via, for example, heating. In particular, it is believed that as compared with conventional PBI membranes, the PBI gel membrane structure includes a more open and ordered framework, wherein the framework of the PBI matrix provides a stable gel membrane, which presents improved electrochemical properties as described. After the densification of the gel membrane, for example, by reducing the membrane thickness and / or drying to form the PBI membrane, the porosity of the membrane to large redox ions can be reduced without destroying the framework of the matrix initially formed. Therefore, after imbibing a redox flow battery supporting electrolyte into the PBI membrane, the re-swollen membrane can maintain the desired electrochemical functionality and ionic conductivity while exhibiting reduced permeability to large ions of active redox couple species in the electrolyte solution.
[0037] In addition to highly desirable electrochemical properties, PBI polymer-based redox flow battery membranes are highly resistant to degradation in a redox flow battery environment. For example, the disclosed membranes can show little or no degradation in vanadium oxide solutions. Thus, the disclosed membranes can provide long-term activity, further reducing the cost of redox flow batteries incorporating the membranes.
[0038] To form a redox flow battery membrane, a polymeric composition can be formed that includes PPA and a selected PBI-forming compound, such as a PBI-forming monomer. In some embodiments, the monomer content of the polymeric composition can be generally low, such as about 10 wt.% or less, about 8 wt.% or less, or about 5 wt.% or less.
[0039] The PBI polymer of the PBI gel film can have any PBI structure as generally known in the art, and can be formed by polymerization of a PBI forming compound comprising at least one aromatic or heteroaromatic tetraamino compound and at least one aromatic or heteroaromatic polycarboxylic acid or its ester, anhydride or acid chloride or at least one aromatic or heteroaromatic diaminocarboxylic acid. The heteroaromatic compounds encompassed herein include aromatic systems containing at least one nitrogen, oxygen, sulfur or phosphorus atom in the aromatic ring.
[0040] Examples of aromatic and heteroaromatic tetraamino compounds that can be used to form PBI gel films can include, but are not limited to, 2,3,5,6-tetraaminopyridine; 3,3',4,4'-tetraaminodiphenyl sulfone; 3,3',4,4'-tetraaminodiphenyl ether; 3,3',4,4'-tetraaminobiphenyl; 1,2,4,5-tetraaminobenzene; 3,3',4,4'-tetraaminobenzophenone; 3,3',4,4'-tetraaminodiphenylmethane; and 3,3',4,4'-tetraaminodiphenyldimethylmethane and salts thereof, such as the monohydrochloride, dihydrochloride, trihydrochloride, and tetrahydrochloride, and any combination of aromatic or heteroaromatic tetraamino monomers.
[0041] In one embodiment, aromatic polycarboxylic acid can include dicarboxylic acid.Dicarboxylic acid can be used alone or with one or more other polycarboxylic acid compounds such as tricarboxylic acid and / or tetracarboxylic acid combination use.When incorporated, based on the amount of used dicarboxylic acid compound, the content of tricarboxylic acid or tetracarboxylic acid can be about 30mol% or less generally, for example from about 0.1mol% to about 20mol% or from about 0.5mol% to about 10mol%.Polycarboxylic acid esters can be used, such as C1-C20 alkyl esters or C5-C12 aryl esters of polycarboxylic acids.The anhydride of polycarboxylic acids or the acyl chlorides of polycarboxylic acids can be polymerized according to disclosed method.
[0042] Examples of aromatic dicarboxylic acids may include, but are not limited to, pyridine-2,5-dicarboxylic acid; pyridine-3,5-dicarboxylic acid; pyridine-2,6-dicarboxylic acid; pyridine-2,4-dicarboxylic acid; 4-phenyl-2,5-pyridinedicarboxylic acid; 3,5-pyrazoledicarboxylic acid; 2,6-pyrimidinedicarboxylic acid; 2,5-pyrazinedicarboxylic acid; 2,4,6-pyridinetricarboxylic acid; benzimidazole-5,6-dicarboxylic acid; 5-hydroxyisophthalic acid; 4-hydroxy Isophthalic acid; 2-hydroxyterephthalic acid; 5-aminoisophthalic acid; 5-N,N-dimethylaminoisophthalic acid; 5-N,N-diethylaminoisophthalic acid; 2,5-dihydroxyterephthalic acid; 2,6-dihydroxyisophthalic acid; 4,6-dihydroxyisophthalic acid; 2,3-dihydroxyphthalic acid; 2,4-dihydroxyphthalic acid; 3,4-dihydroxyphthalic acid; 1,8-dihydroxy 3,6-naphthalene dicarboxylic acid; diphenyl sulfone-4,4'-dicarboxylic acid; isophthalic acid; terephthalic acid; phthalic acid; 3-fluorophthalic acid; 5-fluoroisophthalic acid; 2-fluoroterephthalic acid; tetrafluorophthalic acid; tetrafluoroisophthalic acid; tetrafluoroterephthalic acid; 3-sulfophthalic acid; 5-sulfoisophthalic acid; 2-sulfoterephthalic acid; tetrasulfophthalic acid; tetrasulfoisophthalic acid; tetrasulfo Terephthalic acid; 1,4-naphthalene dicarboxylic acid; 1,5-naphthalene dicarboxylic acid; 2,6-naphthalene dicarboxylic acid; 2,7-naphthalene dicarboxylic acid; biphenyl carboxylic acid; diphenyl ether 4,4'-dicarboxylic acid; benzophenone-4,4'-dicarboxylic acid; biphenyl-4,4'-dicarboxylic acid; 4-trifluoromethylphthalic acid; 2,2-bis(4-carboxyphenyl)hexafluoropropane; 4,4'-stilbene dicarboxylic acid; and 4-carboxycinnamic acid or any combination thereof.
[0043] Examples of aromatic tricarboxylic acids and their esters, anhydrides and acid chlorides include, but are not limited to, 1,3,5-benzenetricarboxylic acid (trimellitic acid); 1,2,4-benzenetricarboxylic acid (trimellitic acid); (2-carboxyphenyl)iminodiacetic acid; 3,5,3′-biphenyltricarboxylic acid; and 3,5,4′-biphenyltricarboxylic acid; or any combination thereof.
[0044] Examples of aromatic tetracarboxylic acids and their esters, anhydrides and acid chlorides include, but are not limited to, 3,5,3′,5′-biphenyltetracarboxylic acid; benzene-1,2,4,5-tetracarboxylic acid; benzophenonetetracarboxylic acid; 3,3′,4,4′-biphenyltetracarboxylic acid; 2,2′,3,3′-biphenyltetracarboxylic acid; 1,2,5,6-naphthalenetetracarboxylic acid; and 1,4,5,8-naphthalenetetracarboxylic acid; or any combination thereof.
[0045] Heteroaromatic carboxylic acids may include heteroaromatic dicarboxylic acids, heteroaromatic tricarboxylic acids, and heteroaromatic tetracarboxylic acids, including their respective esters such as C1-C20 alkyl esters, C5-C12 aryl esters, or anhydrides or acyl chlorides of heteroaromatic carboxylic acids. Examples of heteroaromatic carboxylic acids include, but are not limited to, pyridine-2,5-dicarboxylic acid; pyridine-3,5-dicarboxylic acid; pyridine-2,6-dicarboxylic acid; pyridine-2,4-dicarboxylic acid; 4-phenyl-2,5-pyridinedicarboxylic acid; 3,5-pyrazoledicarboxylic acid; 2,6-pyrimidinedicarboxylic acid; 2,5-pyrazinedicarboxylic acid; 2,4,6-pyridinetricarboxylic acid; benzimidazole-5,6-dicarboxylic acid; and also their C1-C20 alkyl esters or their C5-C12 aryl esters, or their anhydrides or their acyl chlorides, or any combination thereof.
[0046] In one embodiment, the polymeric composition may include a diaminocarboxylic acid, examples of which include, but are not limited to, diaminobenzoic acid and mono- and dihydrochloride derivatives of the acid, and 1,2-diamino-3'-carboxylic acid 4,4'-diphenyl ether, or any combination thereof.
[0047] The PPA that can be used in the polymeric composition can be commercial PPA, such as available from Riedel-de Haen, for example. The PPA can include concentrated grades of PA (H3PO4) exceeding 100%. At high concentrations, individual H3PO4 units polymerize by dehydration, and the PPA can be of the formula H n+2 P n O 3n+1 (n>1) indicates.
[0048] In some embodiments, PPA[H n+2 P n O 3n+1 (n>1)] may have a P2O5 content of about 70 wt.% or more, such as about 75 wt.% or more or about 82 wt.% or more, such as from about 70 wt.% to about 86 wt.%, as calculated by acid titration. The polymeric composition may be in the form of a solution of the monomers / compounds, or a dispersion / suspension of the monomers / compounds in the PPA, which generally depends on the nature of the compound to be polymerized and any additional components of the polymerization solution.
[0049] Polymerization can be carried out at a certain temperature and for a period of time until suitable polymerization of the compound has occurred, which can generally be determined by the increase in viscosity of the polymerized composition. The increase in viscosity can be determined by visual inspection, by determining the intrinsic viscosity, or by any other suitable means. For example, in some embodiments, polymerization can continue until the polymerized composition exhibits an intrinsic viscosity of about 0.8 dL / g or greater, such as about 1.0 dL / g or greater or about 1.5 dL / g or greater. In some embodiments, the polymerization temperature can generally be about 220°C or lower, for example, about 200°C or lower, such as about 100°C to 195°C. Polymerization can be carried out in a time from a few minutes (for example, about 5 minutes) to several hours (for example, about 100 hours). In one embodiment, the polymerized composition can be heated in a stepwise manner, for example, in three or more steps, each step lasting from about 10 minutes to about 5 hours, and the temperature is increased by about 15°C or more for each step. Of course, specific polymerization conditions can vary, generally depending on the reactivity and concentration of specific monomers, as will be apparent to those skilled in the art, and specific polymerization conditions are not required in the formation of redox flow battery membranes.
[0050] Exemplary PBI polymer repeating units of the PBI gel film may include, but are not limited to:
[0051]
[0052]
[0053]
[0054] or any combination thereof, wherein in some embodiments, n and m are each independently 1 or greater, about 10 or greater, or about 100 or greater.
[0055] The PBI polymer of the membrane as disclosed herein may include any repeating unit, including any derivatization thereof as generally known in the art, examples of which are well within the knowledge of those skilled in the art, representative examples of which have been described, for example, in U.S. Patent Application Publication No. 2013 / 0183603 to Benicewicz et al., which is incorporated herein by reference.
[0056] After polymerization, the polymer can be dissolved in the PPA solvent and the PBI polymer solution can be processed to form a gel film precursor having a desired thickness. Advantageously, the polymer solution and the gel film precursor and final gel film and redox flow battery membrane formed therefrom can be free of organic solvents.
[0057] The film precursor may be formed according to any suitable forming process such as, but not limited to, casting, spraying, doctor blading, etc. For example, in one embodiment, the gel film precursor may be formed to a thickness of from about 20 micrometers (μm) to about 4,000 μm, such as in some embodiments, from about 30 μm to about 3,500 μm or from about 50 μm to about 1,000 μm.
[0058] In order to cure the polymer of the film precursor and form a PBI gel film, the PBI polymer solution can be treated in the presence of water and / or moisture to hydrolyze at least a portion of the PPA of the solution. After hydrolysis, the PPA will hydrolyze to form PA and water, thereby causing a sol-gel transition of the PBI polymer solution and curing of the polymer, since the PBI polymer is less soluble in PA as compared to PPA.
[0059] The hydrolysis treatment can be carried out at a temperature and for a time sufficient to solidify the gel film so as to be self-supporting and capable of being manipulated without damage, while incorporating a high liquid content (e.g., a liquid content of about 60 wt.% or more of the total solid and liquid content of the film). By way of example, the hydrolysis treatment can be carried out at a temperature from about 0°C to about 150°C, such as from about 10°C to about 120°C or from about 20°C to about 90°C, such as in some embodiments at ambient temperature (e.g., in contact with an environment at a relative humidity of from about 35% to 100%).
[0060] The hydrolysis can be carried out by contacting the gel film precursor with H2O, e.g., in liquid or vapor form and / or in the presence of other components. For example, the gel film precursor can be contacted with water vapor and / or liquid water and / or steam and / or aqueous PA (e.g., a PA solution having a PA concentration from about 10 wt.% to about 90 wt.%, e.g., about 30 wt.% to about 70 wt.% or about 45 wt.% to about 55 wt.%). The treatment can be carried out at standard pressure, but this is not a requirement of the formation process, and in some embodiments, the hydrolysis treatment can be carried out at a modified pressure.
[0061] In one embodiment, the hydrolysis can be carried out in a climate-controlled environment, wherein the HO content can be strictly controlled. For example, the moisture content of the local environment can be controlled by controlling the temperature or saturation of the fluid contacting the precursor film. For example, a carrier gas such as air, nitrogen, carbon dioxide or other suitable gas can carry HO (e.g., steam) in controlled amounts for contact with the precursor film.
[0062] The hydrolysis treatment time can generally vary depending on parameters such as, for example, the H2O content and the form of contact, the film thickness, the contact temperature, etc. Typically, the hydrolysis treatment can be carried out over a period of time between a few seconds and a few minutes, for example when the hydrolysis treatment uses superheated steam, or alternatively over a period of time of several days, for example when the hydrolysis treatment is carried out at ambient temperature and low relative atmospheric humidity. In some embodiments, the hydrolysis treatment can be carried out over a period of time between about 10 seconds and about 300 hours, for example from about 1 minute to about 200 hours. By way of example, in an embodiment in which at least partial hydrolysis of the PPA of the PBI polymer solution is carried out at room temperature (e.g., about 20°C) in ambient air with a relative atmospheric humidity (i.e., relative humidity) content of from about 20% to 100%, for example from about 40% to about 80%, the treatment time can generally be between about 5 hours and about 200 hours.
[0063] After hydrolysis of at least a portion of the PPA of the PBI polymer solution, the polymer can solidify, which forms a PBI gel film. In one embodiment, the PBI gel film can have a thickness from about 15 μm to about 3000 μm, for example from about 20 μm to about 2000 μm or from about 20 μm to about 1500 μm, although any particular film thickness is not critical. In some embodiments, the PBI gel film can have a thickness less than the thickness of the film precursor. As previously discussed, after hydrolysis, the PBI gel film can be self-supporting, even at high liquid content, which is believed to be due to the intramolecular polymer structure and intermolecular polymer structure present in the solidified polymer matrix.
[0064] In one embodiment, the PBI gel film formed can have a PBI solid content of from about 5 wt.% to about 40 wt.%, such as from about 8 wt.% to about 30 wt.% or from about 10 wt.% to about 25 wt.% of the total weight of the film (including liquid content). The PBI gel film formed can be self-supporting, such as having a Young's modulus of about 2.0 MPa or greater, such as about 3.0 MPa or greater or about 4.5 MPa or greater in some embodiments, as determined for a PBI gel film (e.g., polybenzimidazole) having a thickness of 0.43 mm and a PBI content of 5 wt.%.
[0065] To form a redox flow battery membrane from a PBI gel membrane, the PBI gel membrane can be densified, and the PA and PPA incorporated into the membrane can be removed and replaced with a redox flow battery supporting electrolyte. In one embodiment, the PBI gel membrane can be processed to remove the PA and PPA incorporated into the gel membrane prior to the densification process. In other embodiments, the PBI gel membrane can undergo a densification process prior to removing the PA and PPA.
[0066] There is no particular limitation on the manner in which PA and PPA are removed from the membrane. For example, the PBI gel membrane can be simply washed with water several times to remove any PA and PPA remaining in the gel membrane. For example, the PBI gel membrane can be immersed in a series of water baths, each of which keeps the PBI gel membrane for a period of time ranging from a few minutes (e.g., about 5 minutes) to several hours (e.g., about 24 hours). Optionally, the bath can be heated, for example, to a temperature from about 20°C to about 150°C, for example, from about 25°C to about 90°C, although in other embodiments, the membrane can be rinsed at ambient temperature without special temperature control. In order to confirm the removal of PA and PPA, the pH of the washing solution can be determined, and washing / rinsing can continue until the pH of the washing solution is neutral.
[0067] The PBI gel membrane can be densified according to any suitable method. As used herein, the term "densification" generally refers to any process that reduces the molecular porosity of the membrane. The densification process will generally be accompanied by a permanent reduction in at least one dimension of the membrane after the membrane is re-swelled to a similar liquid content after the densification process. For example, after densification, a fully liquid-incorporated membrane (i.e., unable to absorb any additional liquid) can exhibit a reduction in size (e.g., thickness) as compared to a fully liquid-incorporated membrane prior to densification. As used herein, the term "thickness" generally refers to a decrease in size (e.g., thickness) as compared to a fully liquid-incorporated membrane prior to densification. Figure 1 Dimensions of the membrane 12 in the z-direction are shown in FIG.
[0068] Advantageously, the PBI gel membrane can be densified without changing the basic morphology of the polymer matrix of the membrane formed according to the gel forming process. Thus, the membrane can exhibit reduced porosity for large ions and particularly redox couple ions that may be found in redox flow batteries, with little or no reduction in the ionic conductivity of the membrane. This can provide for the formation of redox flow batteries that can exhibit high current density and low redox couple crossover.
[0069] There is no particular limitation on the manner in which the gel film is densified. For example, in one embodiment, the densification process may include densifying the film in one or more directions (i.e., by Figure 1 In some embodiments, the gel film can be actively stretched in one or more directions of the x, y plane of the film to about 200%, about 190%, about 180%, about 170%, about 160%, or about 150% of the original size, such as from about 110% to about 200% or from about 120% to about 190%.
[0070] In other embodiments, the film can be densified without actively stretching the film. For example, the film can be maintained in one or more dimensions (e.g., x-direction, y-direction, or e ... Figure 1 , which can densify the film. By way of example, a relatively small film can be held on two opposing sides or, optionally, on all four sides as liquid is removed from the film, which can densify the film. In another embodiment, the film can be in the form of a substantially annular sheet, such as on a roller, and the film can be held on opposing sides (e.g., in a cross direction), and optionally held under tension along at least a portion of the length of the sheet (e.g., in a machine direction), while liquid is removed from the film, which can densify the film.
[0071] Optionally, pressure can be applied to the film surface (in the z direction) during the densification process. For example, pressure can be applied to the film surface by sandwiching the film between substrates, and liquid can be removed from the film while the film is maintained in at least one surface direction to densify the film. In such an embodiment, when the film is densified, the sandwich substrate can allow liquid to be discharged from the film. For example, at least one of the substrates can define holes, channels, etc. to allow liquid to be discharged from the film. Alternatively, liquid can simply be discharged from the edge of the film between the pressed substrates.
[0072] Removing liquid from the gel film during the densification process can be active liquid removal or passive liquid removal, or some combination of the two. For example, simply keeping the film in the ambient atmosphere while keeping the film on one or more surface dimensions can passively remove liquid and densify the film. Similarly, in those embodiments where the film is stretched on one or more surface dimensions and those embodiments where pressure is applied across the surface of the film, liquid will be removed from the gel film only by the stretching / pressing action performed on the film.
[0073] In some embodiments, the membrane can be processed by adding heat, contacting with a relatively dry gas stream such as air, nitrogen, argon, etc., or a combination thereof, to actively remove liquid from the gel film. In addition, active removal of liquid from the membrane can be combined with stretching / pressing the membrane or simply holding the membrane in one or more directions on the membrane surface at the same time.
[0074] The amount of liquid to be removed from the film can make the film dry, i.e., there is no additional liquid except the liquid caused by the surrounding atmosphere, to form a PBI film. As used herein, the term "film" generally refers to a polymer structure that is significantly smaller than the surface size (x, y plane) in thickness (z direction) and incorporates little or no moisture, such as about 5wt.% or less moisture, in the polymer matrix. In one embodiment, the densification of the film can include removing a large portion of the liquid of the gel film, but it is not necessary to reach the degree that is considered "dry". For example, about 50wt.% or more, about 60wt.% or more, about 70wt.% or more, or about 80wt.% or more of the liquid content of the gel film can be removed during the densification process.
[0075] The densification process can be performed as a single-step process or a multi-step process. By way of example, a multi-step process may include a first step during which the film may be stretched in one or more directions on the film surface, and / or during which pressure may be applied to the surface area across the film thickness; followed by a second step during which the film may be maintained in one or more dimensions while liquid is actively or passively removed from the film. A single-step process may include only stretching or pressing the film, or alternatively stretching the film, pressing the film, or simply maintaining the film in one or more dimensions, together with actively or passively removing liquid from the film. Any combination of liquid removal, stretching the film, pressing the film, and maintaining the film in one or more dimensions may be used individually or in combination and in a single step or in multiple steps to densify the film.
[0076] Optionally, the PBI membrane may be cross-linked, which may reduce the permeability of the membrane to redox pairs of ions of the battery electrolyte solution without strongly affecting the desired electrochemical properties of the membrane. The manner of cross-linking and the point in the formation process when the membrane is cross-linked are not particularly limited. For example, the gel membrane may be cross-linked prior to rinsing / washing the formed gel membrane or after rinsing / washing the formed gel membrane to remove PA and PPA and prior to densification of the membrane. In other embodiments, the membrane may be cross-linked after densification and allowing the membrane / film to absorb the supporting electrolyte.
[0077] In one embodiment, the PBI film can be crosslinked simply by heating in the presence of atmospheric oxygen. Crosslinking can also be achieved by the action of radiation, such as infrared (IR) radiation (having a wavelength from about 700 nm to about 1 mm), including near IR (having a wavelength from about 700 nm to about 2000 nm or radiation with an energy in the range of from about 0.6 eV to about 1.75 eV).
[0078] In order to achieve crosslinking, the PBI polymer can incorporate reactive functional groups on the polymer chain so as to crosslink with itself, or optionally crosslink with a crosslinker (i.e., a polyfunctional compound that can react with one or more functional groups (e.g., amines) of the PBI polymer). The crosslinker can include any suitable functional group to achieve crosslinking. Suitable crosslinkers are not particularly limited, and examples thereof may include, but are not limited to, epichlorohydrin, diepoxides, diisocyanates, α,ω-dihaloalkanes, diacrylates, and bisacrylamides, and specific examples thereof may include, but are not limited to, α,α'-dichloro-p-xylene, chloromethyl methyl ether, bis(chloromethyl) ether, terephthaloyl chloride, succinyl chloride, and dimethyl succinate, as well as combinations of crosslinkers. In one embodiment, from 1 equivalent to 20 equivalents of crosslinker can be used for each available aromatic ring, but the crosslinking embodiment of the membrane is not limited to any particular crosslinking density.
[0079] In order to form a redox flow battery membrane, the membrane / membrane can absorb a supporting electrolyte after densification. The selected supporting electrolyte can generally depend on the specific characteristics of the redox flow battery in which the membrane is to be used, and can include an acidic supporting electrolyte, an alkaline supporting electrolyte, and a neutral substance (e.g., water). For example, the membrane / membrane can absorb an inorganic acid (e.g., a strong inorganic acid) such as hydrochloric acid, nitric acid, fluorosulfonic acid, or sulfuric acid or a mixture thereof, or a strong organic acid such as acetic acid, formic acid, p-toluenesulfonic acid, or trifluoromethanesulfonic acid or a mixture thereof, and a mixture of different types of acids such as a combination of inorganic acids and organic acids. Other examples of supporting electrolytes that can be absorbed in the membrane may include, but are not limited to, sodium chloride, potassium chloride, sodium hydroxide, potassium hydroxide, sodium sulfide, potassium sulfide, and combinations thereof. By way of example, the supporting electrolyte may include H2SO4, HBr, HBr / HCl mixtures, HCl, NaS2, NaS2 / NaBr mixtures, Br2 in HBr, Br2 in H2SO4, Br2 in HBr / H2SO4 mixtures, etc. In one embodiment, a tetraalkylammonium supporting cation may be absorbed in the membrane, wherein Et4N + and Bu4N + are two non-limiting examples. Tetrafluoroborate (BF 4- ), perchlorate (ClO 4- ) or hexafluorophosphate (PF 6- ) or a combination thereof are additional examples of supporting electrolytes that can be absorbed in the membrane.
[0080] The concentration of the supporting electrolyte in the redox flow battery membrane is not particularly limited, and in some embodiments, can typically be up to about 25 moles / liter (M), such as from about 0.1 M to about 25 M, from about 0.5 M to about 10 M, or from about 1 M to about 5 M.
[0081] The membrane / film can absorb the supporting electrolyte according to any suitable method. For example, a densified PBI membrane or a densified and dried PBI membrane can absorb the supporting electrolyte by soaking in a solution of the supporting electrolyte for a period of time ranging from a few minutes up to a few hours or days in one embodiment, optionally in an environment of increased temperature.
[0082] The redox flow battery membrane may include one or more additives that may be incorporated into the membrane during membrane formation or in combination with a supporting electrolyte. By way of example, small organic molecules such as small C1-C4 alcohols (e.g., glycerol), small organic acids, urea, etc. may be incorporated into the redox flow battery membrane in combination with absorption of a supporting electrolyte.
[0083] In one embodiment, the redox flow battery membrane can incorporate microparticles, such as titanium dioxide or PBI microparticles, typically in an amount of about 2 wt.% or less, which can reduce the porosity of the membrane. For example, nano-sized PBI microparticles can be incorporated into the polymer matrix during the curing of the PBI gel membrane by adding the microparticles to the polymer solution during hydrolysis.
[0084] Densified membranes as described can be incorporated into redox flow batteries for any purpose and in combination with any suitable electrolyte solution and redox couple. For example, redox flow battery membranes as described can be incorporated into batteries for use in the renewable energy sector and / or in current power grids for backup / reduction of energy outages during peak usage times.
[0085] One embodiment of the redox flow battery 10 is Figure 2 As shown, the battery can be in liquid communication with a first tank 100 that can hold a first electrolyte solution and a second tank 200 that can hold a second electrolyte solution. Tanks 100, 200 can be in liquid communication with either side of the redox flow battery membrane 12 of the battery 10 by using conduits 110, 210, pumps 112, 212, valves, control systems, etc. The electrolyte solutions stored in tanks 100, 200 can be circulated to either side of the battery 10 by pumps 112 and 212, respectively, during charging and discharging to contact either side of the membrane 12.
[0086] As is known, the electrolyte solutions of the battery can each incorporate one member of a redox pair. In a specific embodiment, as is known in the art, a redox flow battery membrane can be used for a VRB. The VRB includes a vanadium-based compound in the first electrolyte solution, wherein the vanadium alternates between +5 valence (pentavalent) and +4 valence (tetravalent) vanadium, such as, for example, (VO2)2SO4, VO(SO4), or a combination thereof. The second electrolyte solution may include a vanadium-based compound as an active material, wherein the vanadium alternates between +2 valence (divalent) to +3 valence (trivalent) vanadium, such as, for example, VSO4, V2(SO4)3, or a combination thereof.
[0087] The charge / discharge chemistry of a VRB can be represented in one embodiment as:
[0088] Positive Electrode:
[0089] VO 2+ +H2O-e - →VO2 + +2H + (Charge)
[0090] VO 2+ +H2O-e - ←VO2 + +2H + (Discharge)
[0091] E 0 = +1.00 V relative to standard hydrogen electrode (SHE)
[0092] Negative electrode
[0093] V 3+ +e - →V 2+ (Charge)
[0094] V 3+ +e - ←V 2+ (Discharge)
[0095] E 0 =-0.26V vs. SHE
[0096] Overall chemical reaction:
[0097] VO 2+ +V 3+ +H2O→VO2 + +2H + +V 2+ (Charge)
[0098] VO 2+ +V 3+ +H2O←VO2+ +2H + +V 2+ (Discharge)
[0099] E 0 电池 =1.26V relative to SHE
[0100] Of course, the redox flow batteries described herein are not limited to VRBs, and other batteries including other redox pairs are contemplated herein. Exemplary redox pairs may include, but are not limited to, Zn / Br2; Zn / Fe; Fe / Cr; polysulfide / Br2; polysulfide / I2; 9,10-anthraquinone-2,7-disulfonic acid (AQDS) / Br2; poly(methyl viologen) (poly(MV)) / poly(2,2,6,6-tetramethylpiperidinyloxy-4-yl methacrylate) (poly(TEMPO)); bis-(trimethylammonio)propyl tetrachloroviologen (BTMAP-Vi) / BTMAP-dichloroferrocene (BTMAP-Fc); 2,6-dihydroxyanthraquinone (2,6–DHAQ) / ferrocyanide; and alloxazine 7 / 8-carboxylic acid (ACA) / ferrocyanide.
[0101] By way of example, in one embodiment, the battery may include an electrolyte system including ferrocyanide such as [Fe(CN)6]3 / [Fe(CN)6]4 as an active anode electrolyte material and Fe 2+ and Fe 3+ The catholyte in such a system may include an iron / ligand complex, examples of which may include, but are not limited to, triethanolamine, diethanolamine, ethanolamine, N,N-bis-(2-hydroxyethyl)-(iminotris)-(hydroxymethyl)-methane, and mixtures thereof, wherein the catholyte may have a ligand to iron ratio of from about 3:1 to about 10:1.
[0102] The electrolyte solution may generally include the active material (e.g., vanadium ions, iron ions, etc.) at a concentration from about 0.5 M to about 10 M. For example, the electrolyte solution may include the active material at about 0.5 M or more, about 0.6 M or more, or about 0.7 M or more, such as from about 1 M to about 3 M.
[0103] In one embodiment, the electrolyte solution may include the corresponding active material at a concentration of the active material in the range from 1M to 10M. In one embodiment, when the active material has a concentration in this range, it can promote the high energy density and high power density at which the redox flow battery membrane is capable of operating. In one embodiment, when the active material has a concentration of less than 1M, the amount per unit volume of the active material included in the liquid may be too small, thereby reducing the energy density. In one embodiment, when the active material has a concentration greater than 10M, the electrolyte solution may have a sharply increased viscosity and therefore a significantly reduced oxidation / reduction reaction rate, thereby reducing the power density. The paired electrolyte solutions of the redox flow battery may include their corresponding redox pair active materials at the same concentration as each other or at different concentrations, wherein the preferred concentration generally depends on the specific redox pair to be used, the application of the battery, and the presence of any additional additives in the electrolyte solution.
[0104] The electrolyte solution of the battery may include additives, such as one or more redox flow battery supporting electrolytes as previously discussed. In one embodiment, the electrolyte solution of the battery may include a supporting electrolyte that has been absorbed in a redox flow battery membrane.
[0105] In one embodiment, the electrolyte solution may include a sulfuric acid supporting electrolyte. For example, the electrolyte solution may include a mixture of sulfuric acid and water, i.e., an aqueous sulfuric acid solution, together with an active material of the solution, such as a solvent. In one embodiment, a mixture of a supporting electrolyte and water, such as an aqueous sulfuric acid solution, may include a supporting electrolyte at a concentration from about 1M to about 5M. In one embodiment, the concentration of the supporting electrolyte may be selected so as to provide a suitable solubility for the active material of the electrolyte solution. Therefore, the solution may exhibit a desired ionic conductivity and viscosity, and may avoid overvoltage problems in the battery.
[0106] like Figure 2 As indicated in , each side of the battery 10 may include additional components adjacent to the membrane 12 as known in the art, including a conductive separator 14, such as porous carbon paper, carbon cloth, carbon felt or metal cloth (a porous membrane made of fiber-type metal or a metal film formed on the surface of a polymer fiber cloth) and others. As known, the battery may also include electrodes 16, which may be the same or different from each other and may be made of a conductive substrate (e.g., graphite) suitable for the corresponding electrolyte solution of the battery. A current collector 18 (e.g., gold-plated copper) may be electrically connected to the electrode 16, and the battery may include an end plate 20 (e.g., a stainless steel end plate), which is on either side of the 1 / 2 cell and relatively away from the separator. The current collector 18 provides electrical communication between the battery 10 and an external circuit, as shown.
[0107] Figure 3 The figure shows more than one cell 10 arranged in a typical cell stack 150 of a redox flow battery. As shown, a first circulation path 300 may pass through one side of each of the cells 10 of the stack 150, so that the electrolyte solution of that portion of the cell flows through the path 300 and returns to the first tank 100. A second circulation path 400 passes through the other side of each of the cells 10 of the stack 150, so that the electrolyte solution of that portion of the cell flows through the path 400 and returns to the second tank 200. As shown in FIG. Figure 2 As indicated in , the redox flow battery may also include corresponding charge / discharge circuits, as well as converters, controllers, etc., as known in the art to collect and supply power by using batteries.
[0108] The redox flow battery membrane as described herein can allow for higher performance flow batteries operating at high current loads. Such improved operating conditions can alleviate the need for large electrochemical stacks and thereby reduce the overall cost of commercial flow battery devices. In addition, the membrane of the present invention exhibits excellent performance due to its high ionic conductivity. This in turn can reduce the cost of the overall construction by reducing the necessary stack size.
[0109] The present disclosure may be better understood with reference to the examples set forth below.
[0110] Materials and methods
[0111] 3,3',4,4'-Tetraaminobiphenyl (TAB, polymer grade, -97.5%) was donated by BASF Fuel Cell, Inc. and used as received. Additional monomers were purchased and used as received. PPA (115%) was supplied by FMC Corporation and used as received. α,α'-Dichlorop-xylene (>98.0% purity) was purchased from TCI and used as received.
[0112] Polymer synthesis and membrane fabrication
[0113] A typical polymerization includes the following: The monomers are combined with TAB in a reaction kettle, mixed with an overhead stirrer and purged with dry nitrogen. The contents are heated in a high temperature silicone oil bath, and the temperature is controlled by a programmable temperature controller with ramp and soak features. After the reaction is complete as determined by visual inspection of the viscosity, the polymer solution is cast onto a clear glass plate using a doctor blade with a controlled gate thickness of 15 mils. The cast solution is hydrolyzed into a film at 25°C in a humidity chamber adjusted to 55% RH.
[0114] rinse
[0115] The cast membrane was placed in a DI water bath and the pH of the water was monitored using pH strips. The water bath was changed every 8 hours until a pH of 7 was recorded.
[0116] Densification
[0117] The two-step densification includes a first step in which the membrane is cut into a size of 10 cm x 12 cm and then folded twice to provide a four-layer membrane. The four-layer membrane is then densified using 5843 Tensile Tester. During the second step, the stretched membrane was placed between two porous glass plates and clamped down around the perimeter to maintain the xy dimensions of the membrane and allowed to dry overnight.
[0118] One-step densification involves placing the rinsed membrane between two porous polyethylene sheets and clamping along the perimeter to maintain the xy dimensions. The sandwiched membrane is placed upright at room temperature to dry for 24 hours.
[0119] absorb
[0120] The densified membrane was placed in a 2.6 M sulfuric acid bath for 24 hours to ensure equilibrium of the acid doping.
[0121] Characterization
[0122] The composition of the sulfuric acid-doped PBI membrane is determined by measuring the relative amounts of polymer solids, water and acid in the membrane. The sulfuric acid (SA) content of the membrane is determined by titrating the membrane sample with a standardized sodium hydroxide solution (0.10 M) using a Metrohm 888DMS Titrando automatic titrator. After titration, the sample is washed thoroughly with DI water and dried overnight at 120°C under reduced pressure. The dried sample is then weighed to determine the polymer solids content of the membrane.
[0123] Using Equation 1 and Equation 2, determine the polymer weight percent and sulfuric acid weight percent, respectively;
[0124]
[0125]
[0126] Where W 样品 is the weight of the sample before titration, W 干燥 is the final dry sample weight after titration, M 酸 is the molecular weight of sulfuric acid, and V NaOH and c NaOH is the volume and concentration of sodium hydroxide solution required to neutralize sulfuric acid to the first equivalence point. It is important to note that although the second proton of sulfuric acid is much less acidic than the first proton, it is still a strong enough acid to cause both protons to be titrated simultaneously, pKa1 =-3 and pK a2 =2.
[0127] The number of moles of sulfuric acid per mole of PBI repeating unit (or SA doping level, X) is calculated by the following equation:
[0128]
[0129] Where V NaOH and c NaOH is the volume and concentration of sodium hydroxide solution required to neutralize sulfuric acid to the first equivalence point, W 干燥 is the final weight of the dried sample after titration, and M 聚合物 is the molecular weight of the repeating unit of the polymer.
[0130] Conductivity
[0131] The in-plane conductivity of the membrane was measured by a four-probe electrochemical impedance spectroscopy (EIS) method using a FuelCon (TrueData-EISPCM) electrochemical workstation in a frequency range from 1 Hz to 50 kHz. A membrane sample with a typical geometry of 1.0 cm × 4.0 cm was fixed into the 4-electrode measurement head of the measurement. The conductivity of the membrane was calculated using the following equation:
[0132]
[0133] where d is the distance between the two inner probes, l is the thickness of the membrane, w is the width of the membrane, and R m is the ohmic resistance determined by the model fit. The conductivity was performed at room temperature to replicate the normal operating conditions of the VRB.
[0134] Vanadium permeability
[0135] The crossover of vanadium(IV) (VOSO4) was measured using a PermeGear "side-by-side" direct osmosis cell. The cell had two chambers of 45 mL volume separated by the membrane under test. The chamber temperature was regulated to 25°C using a circulating water bath. A typical test experiment contained 1.5 M VOSO4 in 2.6 M sulfuric acid in the donor chamber and 1.5 M MgSO4 in 2.6 M sulfuric acid in the acceptor chamber. Vanadium(IV) has a strong absorption property at 248 nm; utilizing this property, the concentration in the acceptor chamber was measured at different time intervals using a Shimadzu UV-2450 UV / Vis spectrometer. 2+ Permeability can be calculated using Fick's law of diffusion, Equation 5,
[0136]
[0137] Where: c r(t) is the receptor VOSO4 concentration at time t, c r (0) is the initial VOSO4 concentration of the donor, V is the volume of the donor and acceptor solutions, d is the membrane thickness, A is the effective area of the membrane, and P s is salt permeability.
[0138] Vanadium Test Cell
[0139] VRB test cells are assembled into 24cm 2 active area, and an interdigitated flow field was utilized to process the liquid electrolyte solution into the carbon plate. During use, the membrane was sandwiched between identical commercial carbon paper electrodes that had previously been heat treated to 400°C in air for 30 hours and lined with a polytetrafluoroethylene (PTFE) membrane. The cell was equipped with two 100 mL reservoirs of electrolyte solution on each side consisting of 1.60 M vanadium material with an average oxidation state of 3.55 and a total sulfur content of 4.2 M. The electrolyte was circulated through the cell at a constant flow rate of 120 mL / min via two acid-resistant membrane pumps. The charge / discharge cycle performance was measured using a multichannel potentiostat (Model BT2000, Arbin Instruments Inc., College Station, TX) at a flow rate of 120 mL / min from 72 mA / cm 2 Up to 484mA / cm 2 Constant current density measurement within a range of .
[0140] Example 1
[0141] The para-PBI gel membranes formed by polymerization of 2.25wt% monomer concentration of terephthalic acid, 3,3',4,4'-tetraaminobiphenyl at 220°C for 24 hours as described above were rinsed in a series of deionized water baths to remove phosphoric acid. pH indicator paper was used to ensure that all acids had been removed before proceeding. The membranes were densified according to a two-step procedure during which the membranes were stretched to 1.7 times their original length during the first densification step. After densification, the dried dense PBI membranes were removed and placed in a 2.6M sulfuric acid solution for 24 hours before characterization.
[0142] The in-plane ionic conductivity was measured to be 175 mS / cm at room temperature, and the VOSO4 permeability was determined to be 1.93 × 10 - 8 cm 2 / s. The film was characterized by using a VRB test cell as described. VE, CE and EE were measured. The results are Figure 4 and are shown in Table 1 below.
[0143] Table 1
[0144]
[0145] Example 2
[0146] The para-PBI membrane formed as described in Example 1 was rinsed in a series of deionized water baths to remove phosphoric acid. pH indicator paper was used to ensure that all acid had been removed before proceeding. The membrane was densified according to a two-step procedure during which the membrane was stretched to 1.5 times its original length during the first densification step. After densification, the dried dense PBI membrane was removed and placed in a 2.6M sulfuric acid solution for 24 hours before characterization.
[0147] The in-plane ionic conductivity was measured to be 207.6 mS / cm at room temperature. The VOSO4 permeability was determined to be 4.55×10 - 8 cm 2 / s. The film was characterized by using a VRB test cell. VE, CE and EE were measured. The results are Figure 5 and are shown in Table 2 below.
[0148] Table 2
[0149]
[0150] Example 3
[0151] The para-PBI membrane formed as described in Example 1 was rinsed in a series of deionized water baths to remove phosphoric acid. pH indicator paper was used to ensure that all of the acid had been removed before proceeding. The wet thickness was measured to be 356.67 ± 5.8 μm, and the membrane size was cut to 45.72 cm × 30.48 cm. The wet membrane was densified according to a one-step densification process. The dried membrane had a uniform thickness of 30 μm.
[0152] Prior to characterization, the first sample of the dried dense membrane was placed in 2.6 M sulfuric acid for 24 hours. The in-plane ionic conductivity was measured to be 95.17 mS / cm at room temperature. The VOSO4 permeability was measured to be 2.65×10 -8 cm 2 / s. The film was characterized by using a VRB test cell. VE, CE and EE were measured. The results are Figure 6 and are shown in Table 3.
[0153] Table 3
[0154]
[0155] Prior to characterization, a second sample of the dried dense membrane was placed in 85wt.% phosphoric acid for 24 hours. The through-plane ionic conductivity was measured with an amplitude of 5mV using a Zahner IM6e spectrometer in a frequency range of 1Hz to 100kHz by a four-probe AC impedance spectroscopy method. A two-component model with an ohmic resistor in parallel with a capacitor was used to fit the experimental data. The conductivity of the membrane at different temperatures was calculated using the previously described equation by the membrane resistance obtained from the model simulation. The membrane sample was subjected to two heating ramps to 180°C. The conductivity measured at 180°C on the second heating ramp was 215.68mS / cm.
[0156] Example 4
[0157] 11.0824g of TAB (51.72mmol), 13.9034g of 2-sulfoterephthalic acid monosodium salt (2STPA, 51.85mmol) and 600g of PPA were added to a 1000mL reactor (4wt% monomer charge). Polymerization was carried out at 220°C in a nitrogen atmosphere for 48 hours. The solution was applied to a glass substrate by a scraper with a 20 mil gate thickness, and then hydrolyzed for 24 hours. The s-PBI membrane absorbed in phosphoric acid was rinsed as described and densified according to a two-step densification process, during which the membrane was stretched to 1.5 times its original length. Before characterization, the dried dense PBI membrane was placed in a 2.6M sulfuric acid solution for 24 hours.
[0158] The in-plane ionic conductivity was measured to be 179.7 mS / cm at room temperature. The VOSO4 permeability was tested as described and was measured to be 2.60×10 -9 cm 2 / s. The film was characterized by using a VRB test cell. VE, CE and EE were measured. The results are Figure 7 and are shown in Table 4 below.
[0159] Table 4
[0160]
[0161] Example 5
[0162] 11.0824g of TAB (51.72mmol), 13.9034g of 2STPA (51.85mmol) and 600g of PPA were added to a reactor (4wt% monomer charge). Polymerization was carried out at 220°C for 48 hours in a nitrogen atmosphere. The solution was applied to a glass substrate by a scraper with a 20 mil gate thickness, and then hydrolyzed for 24 hours. The s-PBI film was rinsed, and the wet thickness was measured to be 251.8±34μm. The wet film was densified according to a one-step densification process. The dried densified film had a uniform thickness of 37.7μm. Before characterization, the dry film was placed in 2.6M sulfuric acid for 24 hours.
[0163] The in-plane ionic conductivity was measured to be 65.71 mS / cm at room temperature. The VOSO4 permeability was measured to be 7.76×10 - 9 cm 2 / s. The film was characterized by using a VRB test cell. VE, CE and EE were measured. The results are Figure 8 and are shown in Table 5 below.
[0164] Table 5
[0165]
[0166] Example 6
[0167] 6.615g of TAB (30.87mmol), 6.119g of 2,5-dihydroxyterephthalic acid (diOH-TPA, 30.88mmol) and 401.29g of PPA were added to the reactor and polymerized as described. Polymerization was carried out at 220°C for 24 hours in a nitrogen atmosphere. The solution was applied to a glass substrate by a scraper with a 20 mil gate thickness, and then hydrolyzed for 24 hours. The film was rinsed and densified according to a one-step densification process. Before densification, the wet thickness was measured to be 404.44 ± 10 μm. The dried densified film had a uniform thickness of 31.1 μm. Before characterization, the dry film was placed in 2.6M sulfuric acid for 24 hours.
[0168] The in-plane ionic conductivity was measured to be 218.48 mS / cm at room temperature. The VOSO4 permeability was measured to be 3.92×10 - 8 cm 2 / s.
[0169] Comparative Example 1
[0170] The para-PBI membrane made by the PPA process was first rinsed several times in a deionized water bath to remove phosphoric acid. pH indicator paper was used to ensure that all the acid had been removed before proceeding. The neutralized membrane was then placed in a 2.6 M sulfuric acid solution for at least 24 hours before characterization. The VOSO4 permeability was determined to be 5.73 × 10 -7 cm 2 / s.
[0171] Comparative Example 2
[0172] 1.0824 g of TAB (51.72 mmol), 13.9034 g of 2STPA (51.85 mmol) and 600 g of PPA were added to a 1000 mL reactor (4 wt.% monomer charge) equipped with an overhead mechanical stirrer. Polymerization was carried out at 220 ° C for 48 hours in a nitrogen atmosphere. The solution was applied to a glass substrate by a spatula with a 20 mil gate thickness and then hydrolyzed for 24 hours. The sPBI membrane absorbed in phosphoric acid was rinsed in a series of deionized water baths to remove phosphoric acid. pH indicator paper was used to ensure that all acid had been removed. Prior to characterization, the sPBI membrane was placed in 2.6 M sulfuric acid for 24 hours. VOSO4 permeability was measured to be 4.89×10 -7 cm 2 / s.
[0173] Comparative Example 3
[0174] 6.615 g of TAB (30.87 mmol), 6.119 g of diOH-TPA (30.88 mmol) and 401.29 g of PPA were added to the reactor and stirred with an overhead mechanical stirrer under a nitrogen atmosphere. Polymerization was carried out at 220 ° C for 24 hours in a nitrogen atmosphere. The solution was applied to a glass substrate by a spatula with a 20 mil gate thickness and then hydrolyzed for 24 hours. The membrane absorbed in phosphoric acid was rinsed in a series of deionized water baths to remove phosphoric acid. pH indicator paper was used to ensure that all acid had been removed. Prior to characterization, the membrane was placed in 2.6 M sulfuric acid for 24 hours. VOSO4 permeability was measured to be 7.23 × 10 -7 cm 2 / s.
[0175] Comparative Example 4
[0176] A commercially available m-PBI membrane prepared from a cast and dried N,N-dimethylacetamide solution was used as received. The membrane was placed in a 2.6 M sulfuric acid solution for 24 hours prior to characterization. The in-plane ionic conductivity in sulfuric acid was measured to be 13.1 mS / cm at room temperature. VO 2+ The permeability was determined to be 2.53×10-11 cm 2 / s.
[0177] The membrane was characterized by using a VRB test cell. 2 Measure VE, CE and EE. The results are Fig. 9 and are shown in Table 6 below.
[0178] Table 6
[0179]
[0180] As shown, at higher current densities, the cell does not perform and cannot operate above about 72 mA / cm 2 This is because the voltage is related to the membrane conductivity, which is very low for this membrane.
[0181] While certain embodiments of the disclosed subject matter have been described using specific terms, such description is for illustrative purposes only, and it is to be understood that changes and variations may be made without departing from the spirit or scope of the subject matter.
[0182] This article also provides the following items:
[0183] 1. A method for forming a redox flow battery membrane, comprising:
[0184] forming a polymeric composition comprising polyphosphoric acid, an aromatic or heteroaromatic tetraamino compound, and an aromatic or heteroaromatic carboxylic acid compound, wherein the aromatic or heteroaromatic carboxylic acid compound comprises an aromatic or heteroaromatic polycarboxylic acid or an ester, anhydride or chloride thereof and / or comprises an aromatic or heteroaromatic diaminocarboxylic acid;
[0185] polymerizing the aromatic or heteroaromatic tetraamino compound and the aromatic or heteroaromatic carboxylic acid compound to form a polymer solution comprising polybenzimidazole dissolved in the polyphosphoric acid;
[0186] shaping the polymer solution to form a membrane precursor comprising the polymer solution;
[0187] hydrolyzing at least a portion of the polyphosphoric acid solution to form phosphoric acid and water, whereupon the membrane precursor forms a gel membrane comprising the polybenzimidazole, the gel membrane being a self-supporting membrane capable of incorporating a liquid content of about 60 wt.% or more without loss of structure;
[0188] densifying the gel film; and
[0189] The densified gel film is made to absorb the redox flow battery supporting electrolyte.
[0190] 2. The method according to item 1, wherein the step of densifying the gel film comprises reducing the thickness of the gel film.
[0191] 3. The method according to item 1 or item 2, wherein the step of densifying the gel film comprises drying the gel film.
[0192] 4. The method according to any of the preceding items, wherein the step of densifying the gel film comprises stretching the gel film in one or more directions along a film surface.
[0193] 5. The method according to any one of the preceding items, wherein the aromatic or heteroaromatic tetraamino compound comprises 2,3,5,6-tetraaminopyridine; 3,3',4,4'-tetraaminodiphenyl sulfone; 3,3',4,4'-tetraaminodiphenyl ether; 3,3',4,4'-tetraaminobiphenyl; 1,2,4,5-tetraaminobenzene; 3,3',4,4'-tetraaminobenzophenone; 3,3',4,4'-tetraaminodiphenylmethane; and 3,3',4,4'-tetraaminodiphenyldimethylmethane or a salt thereof, or any combination thereof.
[0194] 6. The method according to any one of the preceding items, wherein the aromatic or heteroaromatic carboxylic acid compound comprises pyridine-2,5-dicarboxylic acid; pyridine-3,5-dicarboxylic acid; pyridine-2,6-dicarboxylic acid; pyridine-2,4-dicarboxylic acid; 4-phenyl-2,5-pyridinedicarboxylic acid; 3,5-pyrazoledicarboxylic acid; 2,6-pyrimidinedicarboxylic acid; 2,5-pyrazinedicarboxylic acid; 2,4,6-pyridinetricarboxylic acid; benzimidazole-5,6-dicarboxylic acid; 5 -Hydroxyisophthalic acid; 4-hydroxyisophthalic acid; 2-hydroxyterephthalic acid; 5-aminoisophthalic acid; 5-N,N-dimethylaminoisophthalic acid; 5-N,N-diethylaminoisophthalic acid; 2,5-dihydroxyterephthalic acid; 2,6-dihydroxyisophthalic acid; 4,6-dihydroxyisophthalic acid; 2,3-dihydroxyphthalic acid; 2,4-dihydroxyphthalic acid; 3,4-dihydroxyphthalic acid Acid; 1,8-dihydroxynaphthalene-3,6-dicarboxylic acid; diphenylsulfone-4,4'-dicarboxylic acid; isophthalic acid; terephthalic acid; phthalic acid; 3-fluorophthalic acid; 5-fluoroisophthalic acid; 2-fluoroterephthalic acid; tetrafluorophthalic acid; tetrafluoroisophthalic acid; tetrafluoroterephthalic acid; 3-sulfophthalic acid; 5-sulfoisophthalic acid; 2-sulfoterephthalic acid; tetrasulfophthalic acid; tetrasulfoisophthalic acid ; tetrasulfonaterephthalic acid; 1,4-naphthalene dicarboxylic acid; 1,5-naphthalene dicarboxylic acid; 2,6-naphthalene dicarboxylic acid; 2,7-naphthalene dicarboxylic acid; biphenyl carboxylic acid; diphenyl ether 4,4'-dicarboxylic acid; benzophenone-4,4'-dicarboxylic acid; biphenyl-4,4'-dicarboxylic acid; 4-trifluoromethylphthalic acid; 2,2-bis(4-carboxyphenyl)hexafluoropropane; 4,4'-stilbene dicarboxylic acid; and 4-carboxycinnamic acid or any combination thereof.
[0195] 7. The method according to any of the preceding items, wherein the hydrolysis is carried out at a temperature from about 0°C to about 150°C and at a relative humidity from about 20% to 100%.
[0196] 8. A redox flow battery membrane comprising:
[0197] A densified polybenzimidazole gel film that is a self-supporting film capable of incorporating about 60 wt. % or more of liquid content without loss of structure; and
[0198] A redox flow battery supporting electrolyte, wherein the redox flow battery supporting electrolyte is absorbed in the polybenzimidazole gel membrane;
[0199] The redox flow battery membrane exhibits a conductivity of about 50 mS / cm in a 2.6 M sulfuric acid solution. 2 or greater in-plane ionic conductivity; and wherein
[0200] The redox flow battery membrane exhibits about 10 -7 cm 2 VO / s or lower 2+ Permeability.
[0201] 9. The redox flow battery membrane according to item 8, wherein the polybenzimidazole of the densified polybenzimidazole gel membrane comprises one or more of the following repeating units:
[0202]
[0203]
[0204]
[0205] or any combination thereof, wherein n and m are each independently 1 or greater, about 10 or greater, or about 100 or greater.
[0206] 10. According to the redox flow battery membrane of item 8 or item 9, the supporting electrolyte comprises an inorganic acid, such as hydrochloric acid, nitric acid, fluorosulfonic acid or sulfuric acid or a mixture thereof; a strong organic acid, such as acetic acid, formic acid, p-toluenesulfonic acid or trifluoromethanesulfonic acid or a mixture thereof; or a combination of one or more inorganic acids and / or one or more organic acids; or the supporting electrolyte comprises sodium chloride, potassium chloride, sodium hydroxide, potassium hydroxide, sodium sulfide, potassium sulfide or any combination thereof; or the supporting electrolyte comprises a tetraalkylammonium cation.
[0207] 11. A redox flow battery membrane according to any one of items 8 to 10, wherein the densified polybenzimidazole gel membrane is cross-linked.
[0208] 12. A redox flow battery comprising:
[0209] The densified polybenzimidazole gel film exhibits a thermal conductivity of about 50 mS / cm in a 2.6 M sulfuric acid solution. 2 or greater in-plane ionic conductivity and about 10 -7 cm 2 VO / s or lower 2+ Permeability; and
[0210] a redox flow battery supporting electrolyte, wherein the redox flow battery supporting electrolyte is absorbed in the densified polybenzimidazole gel membrane;
[0211] The redox flow battery is capable of operating at approximately 50 mA / cm 2 or greater current density operation.
[0212] 13. The redox flow battery according to item 12, wherein the redox flow battery is a vanadium flow battery.
[0213] 14. The redox flow battery membrane according to item 12 or item 13, wherein the redox flow battery is 2 The current density has a coulombic efficiency of about 90% or greater and / or an energy efficiency of about 70% or greater and / or a voltage efficiency of about 75% or greater.
[0214] 15. A redox flow battery membrane according to any one of items 12 to 14, wherein the redox flow battery is 2 The current density has a coulombic efficiency of about 85% or greater and / or an energy efficiency of about 50% or greater and / or a voltage efficiency of about 60% or greater.
Claims
1. A method for forming a redox flow battery membrane, comprising: forming a polymeric composition comprising polyphosphoric acid, an aromatic or heteroaromatic tetraamino compound, and an aromatic or heteroaromatic carboxylic acid compound, wherein the aromatic or heteroaromatic carboxylic acid compound comprises an aromatic or heteroaromatic polycarboxylic acid or an ester, anhydride or chloride thereof and / or comprises an aromatic or heteroaromatic diaminocarboxylic acid; polymerizing the aromatic or heteroaromatic tetraamino compound and the aromatic or heteroaromatic carboxylic acid compound to form a polymer solution comprising polybenzimidazole dissolved in the polyphosphoric acid; shaping the polymer solution to form a membrane precursor comprising the polymer solution; hydrolyzing at least a portion of the polyphosphoric acid to form phosphoric acid and water, after which the membrane precursor forms a gel membrane comprising the polybenzimidazole, the gel membrane being a self-supporting membrane capable of incorporating 60 wt.% or more of a liquid content without loss of structure; washing the gel membrane to remove the phosphoric acid and remaining polyphosphoric acid; densifying the gel film; as well as The rinsed and densified gel membrane is allowed to absorb a redox flow battery supporting electrolyte. 2 . The method of claim 1 , wherein the step of densifying the gel film comprises reducing the thickness of the gel film.
3. The method of claim 1, wherein the step of densifying the gel film comprises drying the gel film.
4. The method of claim 1, wherein the step of densifying the gel film comprises stretching the gel film in one or more directions along a film surface.
5. The method according to any one of claims 1 to 4, wherein the aromatic or heteroaromatic tetraamino compound is selected from 2,3,5,6-tetraaminopyridine; 3,3',4,4'-tetraaminodiphenyl sulfone; 3,3',4,4'-tetraaminodiphenyl ether; 3,3',4,4'-tetraaminobiphenyl; 1,2,4,5-tetraaminobenzene; 3,3',4,4'-tetraaminobenzophenone; 3,3',4,4'-tetraaminodiphenylmethane; or 3,3',4,4'-tetraaminodiphenyldimethylmethane or a salt thereof.
6. The method according to any one of claims 1 to 4, wherein the aromatic or heteroaromatic carboxylic acid compound is selected from pyridine-2,5-dicarboxylic acid; pyridine-3,5-dicarboxylic acid; pyridine-2,6-dicarboxylic acid; pyridine-2,4-dicarboxylic acid; 4-phenyl-2,5-pyridinedicarboxylic acid; 3,5-pyrazoledicarboxylic acid; 2,6-pyrimidinedicarboxylic acid; 2,5-pyrazinedicarboxylic acid; 2,4,6-pyridinetricarboxylic acid; benzimidazole-5,6-dicarboxylic acid; formic acid; 5-hydroxyisophthalic acid; 4-hydroxyisophthalic acid; 2-hydroxyterephthalic acid; 5-aminoisophthalic acid; 5-N,N-dimethylaminoisophthalic acid; 5-N,N-diethylaminoisophthalic acid; 2,5-dihydroxyterephthalic acid; 2,6-dihydroxyisophthalic acid; 4,6-dihydroxyisophthalic acid; 2,3-dihydroxyphthalic acid; 2,4-dihydroxyphthalic acid; 3,4-dihydroxy 1,8-Dihydroxynaphthalene-3,6-dicarboxylic acid; diphenylsulfone-4,4'-dicarboxylic acid; isophthalic acid; terephthalic acid; phthalic acid; 3-fluorophthalic acid; 5-fluoroisophthalic acid; 2-fluoroterephthalic acid; tetrafluorophthalic acid; tetrafluoroisophthalic acid; tetrafluoroterephthalic acid; 3-sulfophthalic acid; 5-sulfoisophthalic acid; 2-sulfoterephthalic acid; tetrasulfophthalic acid; tetrasulfophthalic acid isophthalic acid; tetrasulfoterephthalic acid; 1,4-naphthalene dicarboxylic acid; 1,5-naphthalene dicarboxylic acid; 2,6-naphthalene dicarboxylic acid; 2,7-naphthalene dicarboxylic acid; biphenyl carboxylic acid; diphenyl ether 4,4'-dicarboxylic acid; benzophenone-4,4'-dicarboxylic acid; biphenyl-4,4'-dicarboxylic acid; 4-trifluoromethylphthalic acid; 2,2-bis(4-carboxyphenyl)hexafluoropropane; 4,4'-stilbene dicarboxylic acid; or 4-carboxycinnamic acid.
7. The process according to any one of claims 1 to 4, wherein the hydrolysis is carried out at a temperature of from 0°C to 150°C and at a relative humidity of from 20% to 100%.
8. The method of any one of claims 1-4, wherein the porous substrate comprises a porous glass plate.
9. The method of any one of claims 1-4, wherein the porous substrate comprises a porous polyethylene sheet.
10. A redox flow battery membrane formed by the method according to claim 1, wherein The redox flow battery membrane exhibited a 50 mS / cm 2 or greater in-plane ionic conductivity; and wherein The redox flow battery membrane exhibits 10 -7 cm 2 VO / s or lower 2+ Permeability.
11. The redox flow battery membrane of claim 10, wherein the polybenzimidazole of the densified polybenzimidazole gel membrane comprises one or more of the following repeating units: or any combination thereof, wherein n and m are each independently 1 or greater, 10 or greater, or 100 or greater.
12. According to the redox flow battery membrane of claim 10 or claim 11, the redox flow battery supporting electrolyte comprises an inorganic acid; a strong organic acid; or a combination of one or more inorganic acids and / or one or more organic acids; or the redox flow battery supporting electrolyte comprises sodium chloride, potassium chloride, sodium hydroxide, potassium hydroxide, sodium sulfide, potassium sulfide or any combination thereof; or the redox flow battery supporting electrolyte comprises tetraalkylammonium cations.
13. A redox flow battery membrane according to claim 10 or claim 11, wherein the densified polybenzimidazole gel membrane is cross-linked.
14. The redox flow battery membrane according to claim 12, wherein the inorganic acid is selected from hydrochloric acid, nitric acid, fluorosulfonic acid or sulfuric acid or a mixture thereof.
15. The redox flow battery membrane of claim 12, wherein the strong organic acid is selected from acetic acid, formic acid, p-toluenesulfonic acid or trifluoromethanesulfonic acid or a mixture thereof.
16. A redox flow battery comprising the redox flow battery membrane according to claim 10, wherein The redox flow battery is capable of operating at 50 mA / cm 2 or greater current density operation.
17. The redox flow battery of claim 16, wherein the redox flow battery is a vanadium flow battery.
18. The redox flow battery according to claim 16 or claim 17, wherein the redox flow battery is 2 The current density has a coulombic efficiency of 90% or greater and / or an energy efficiency of 70% or greater and / or a voltage efficiency of 75% or greater.
19. The redox flow battery according to claim 16 or claim 17, wherein the redox flow battery is at 483 mA / cm 2 The current density has a coulombic efficiency of 85% or greater and / or an energy efficiency of 50% or greater and / or a voltage efficiency of 60% or greater.