Method for preparing all-vanadium electrolyte from multi-mixed acid
Through the polymixed acid preparation method, combined with sulfuric acid, oxalic acid and methylsulfonic acid-hydrochloric acid, the all-vana electrolyte is prepared, which solves the problem of narrow temperature range of the electrolyte and insufficient thermal stability, and achieves higher energy density and wider The temperature range of the use temperature reduces the power cost and the generation of side-reacting gases.
Patent Information
- Application Number
- CN202411019858.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
The current all-vanadium liquid flow battery electrolyte has a narrow temperature range. V (V) is easy to precipitate at high temperatures, and V (II), V (III), and V (IV) is easy to crystallize at low temperatures, resulting in thermal stability of the electrolyte. The properties and energy density are insufficient, and the high concentration of a single sulfuric acid system will increase the viscosity and cost of the electrolyte, disrupt the valence equilibrium, and reduce capacity.
By using the polymixed acid preparation method, 3.5 valent vanadium sulfate stock solution was prepared by dissolving V2O5 powder in water-sulfuric acid solution at a certain temperature, and adding mixed solutions of oxalic acid and methylsulfonic acid-hydrochloric acid, and 3.5 valent vanadium was obtained by electrolysis. The electrolyte broadens the temperature range of the electrolyte and improves thermal stability and energy density.
The use temperature range of electrolyte is broadened, thermal stability and energy density is improved, power costs and generation of side reaction gases are reduced, and large-scale production is easy, the risk of vanadium ion precipitation is reduced, and the charge and discharge performance is improved.
Smart Images

Figure CN118970126A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of all-vanadium liquid flow batteries, and in particular relates to a method for preparing an all-vanadium electrolyte with multiple mixed acids. Background Art
[0002] With the proposal of my country's "dual carbon" goals, the new energy storage industry has a full-scale layout in the national strategy. Among them, the all-vanadium liquid flow battery has become one of the most popular and practical liquid flow energy storage industries with the best industrial production due to its relatively flexible use environment, relatively independent energy modules and power modules, long service life, high safety, and different valence states of a single substance. At present, there are many ways to prepare the electrolyte of the all-vanadium liquid flow battery, which can be divided into direct electrolysis and indirect electrolysis according to the preparation path. The direct electrolysis method is to use a vanadium sulfate slurry containing high-purity V2O5 as the negative electrode liquid, and use a sulfuric acid solution of the same concentration as the positive electrode liquid for direct electrolysis through parameter control. The negative electrode liquid is electrolyzed and reduced to the target 3.5-valent electrolyte, and the positive electrode liquid precipitates oxygen. The indirect electrolysis method is prepared in two steps. First, the required concentration of tetravalent vanadium sulfate is prepared, and then the positive and negative electrode barrels are filled with the same concentration and volume of tetravalent vanadium sulfate and then electrolyzed (charged). The electrolyte obtained in the negative electrode barrel after electrolysis is the target 3.5-valent electrolyte.
[0003] As an important component of the all-vanadium flow battery system, the electrolyte determines the energy module of the vanadium battery system. The oxidation / reduction of the active substance in the electrolyte - vanadium ions is the only source of chemical energy conversion into electrical energy. Theoretically, the higher the vanadium ion concentration, the higher the energy conversion. However, the higher the vanadium ion concentration, the greater the energy density. At low temperatures, V(Ⅱ), V(Ⅲ), and V(Ⅳ) are prone to crystallization as the vanadium ion concentration increases. At high temperatures, V(Ⅴ) is prone to crystallization as the vanadium ion concentration increases. The best goal is to increase the vanadium ion concentration while expanding the high and low temperature use boundaries of the electrolyte. Common industrial and large-scale all-vanadium electrolytes often use sulfuric acid solution as a supporting electrolyte. The boundary temperature of the all-vanadium electrolyte in this sulfuric acid system is generally in a narrow range of -5 to 40°C. Above 40°C, high-valent V(Ⅴ) is easy to precipitate. Below -5°C, low-valent V(Ⅱ), V(Ⅲ), and V(Ⅳ) vanadium ions are easy to crystallize. Increasing the concentration of sulfuric acid can increase the solubility of V(Ⅴ), V0 2+ / VO2 + The reversibility and thermal stability of the reaction will inhibit the dissolution of V(II), V(III) and V(IV). At the same time, the excessively high sulfuric acid concentration increases the viscosity of the electrolyte, which increases the piping and cost of the circulation system. In a circulation module, no matter which valence state of vanadium ions is precipitated, the valence balance will be destroyed, resulting in capacity decay. In view of the above problems, the present invention proposes a method for preparing an all-vanadium electrolyte with a multi-mixed acid. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing an all-vanadium electrolyte from a multi-mixed acid, aiming to solve the problems raised in the above-mentioned background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing an all-vanadium electrolyte using a multi-mixed acid, comprising the following steps:
[0007] At a certain temperature, V2O5 powder with a concentration of ≧99.9% is dissolved in a sulfuric acid solution prepared by water-sulfuric acid, fully activated for a certain time, cooled to a certain temperature and then oxalic acid is added, reacted for a certain time and then cooled, and then a certain amount of methanesulfonic acid-hydrochloric acid mixed solution is added to make up the volume to prepare a tetravalent vanadium sulfate stock solution, and then the tetravalent vanadium sulfate stock solution is evenly divided into positive and negative electrode barrels, and electrolyzed with an electrolysis device to obtain a 3.5-valent all-vanadium electrolyte.
[0008] Furthermore, the initial temperature of the V2O5 addition is 75-95°C.
[0009] Furthermore, the sulfuric acid and water are configured into a sulfuric acid solution in a volume ratio of 1:1 to 1:3.
[0010] Furthermore, the activation time of the V2O5 is 0.5 to 3 hours.
[0011] Furthermore, when the oxalic acid is added, the temperature of the solution is cooled to 55-65°C.
[0012] Furthermore, after adding the oxalic acid, the reduction reaction time is 0.5 to 3 hours.
[0013] Furthermore, the adding speed of the oxalic acid is 4-8 kg / min; if a variable frequency feeder device is used to feed the oxalic acid, the feeding frequency is 10-22 Hz.
[0014] Furthermore, when the methanesulfonic acid-hydrochloric acid mixed acid is added, the solution temperature is 40° C., wherein the mass percentage concentration of hydrochloric acid is 32-40%, and the molar ratio of the methanesulfonic acid to the hydrochloric acid is 1:1-1:5.
[0015] Furthermore, the total vanadium concentration of the all-vanadium electrolyte is 1.5-1.8 mol / L, the sulfuric acid concentration is 2-4.5 mol / L, the methanesulfonic acid concentration is 0.1-0.6 mol / L, and the hydrochloric acid concentration is 0.5-1.5 mol / L.
[0016] Furthermore, the electrolysis equipment is a Xinwei CTE-4008D-5V30A charge-discharge instrument, with a charge cut-off voltage of 1.55V, a discharge cut-off voltage of 1.00V, and a current density of 50-120mA / cm 2, the electrode area is 48cm 2 , using single battery charging and discharging.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The method for preparing all-vanadium electrolyte by multi-mixed acid uses sulfuric acid-methanesulfonic acid-hydrochloric acid as supporting electrolyte and indirect electrolytic reduction as the path. Compared with single sulfuric acid system electrolyte, it broadens the use temperature range and use area of the electrolyte, improves the thermal stability of the electrolyte, and improves the energy density to a certain extent; compared with pure direct electrolysis, it saves electricity costs, reduces the generation of side reaction gases, and is easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a performance diagram of the 1# electrolyte prepared in Example 1.
[0020] Figure 2 This is the performance diagram of 2# electrolyte prepared in Example 2.
[0021] Figure 3 This is the performance diagram of 3# electrolyte prepared in Example 3.
[0022] Figure 4 This is the performance diagram of 4# electrolyte prepared in Example 4. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0024] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.
[0025] One embodiment of the present invention provides a method for preparing an all-vanadium electrolyte with a multi-mixed acid, comprising the following steps:
[0026] Sulfuric acid (concentration of 2-4.5 mol / L) and water are prepared into a sulfuric acid solution in a volume ratio of 1:1-1:3. High-purity V2O5 (≧99.9%) powder and sulfuric acid solution are fully activated at 75-95°C for 0.5-3h, then cooled to 55-65°C, and oxalic acid is added at a ratio of 55-74% of the mass of the V2O5 powder (the rate of oxalic acid addition is 4-8 kg / min; if a variable frequency feeder device is used to feed oxalic acid, the feeding frequency is 10-22 Hz); react for 0.5-3h, then cool to 40°C, and then add a mixed solution of methanesulfonic acid and hydrochloric acid. The mixture was diluted to volume (the mass percentage concentration of hydrochloric acid was 32-40%; the molar ratio of methanesulfonic acid to hydrochloric acid was 1:1-1:5; the concentration of methanesulfonic acid was 0.1-0.6 mol / L, and the concentration of hydrochloric acid was 0.5-1.5 mol / L), a tetravalent electrolyte with the mixed acid as a supporting electrolyte was prepared, and the tetravalent vanadyl sulfate stock solution was used as the initial electrolyte for the positive and negative electrodes at a volume ratio of 1:1, and an electrolysis device (a Xinwei CTE-4008D-5V30A charge and discharge instrument, with a charge cut-off voltage of 1.55 V, a discharge cut-off voltage of 1.00 V, and a current density of 50-120 mA / cm 2 , the electrode area is 48cm 2 , using single cell charge and discharge) for electrolysis, the cathode liquid after electrolytic reduction is the target electrolyte, that is, 3.5-valent all-vanadium electrolyte (total vanadium concentration is 1.5-1.8 mol / L).
[0027] In the embodiment of the present invention, the present invention uses sulfuric acid-hydrochloric acid-methanesulfonic acid tri-mixed acid as the supporting electrolyte and oxalic acid as the reducing agent. The indirect electrolytic reduction method, that is, chemical reduction combined with electrolysis, is used to prepare the 3.5-valent target electrolyte. A very important point about the capacity decay of the all-vanadium electrolyte is that the valence state is unbalanced after the thermal stability of the positive electrode electrolyte is reduced. The present invention introduces methanesulfonic acid and hydrochloric acid on the basis of a single sulfuric acid system. Both acids can improve the thermal stability of the positive electrode liquid and broaden the operating temperature range of the electrolyte. Cl - It can form soluble VO2Cl(H2O) with pentavalent vanadium ions, which inhibits the precipitation of V2O5 in the cathode liquid to a certain extent. Methanesulfonic acid is a small molecule organic acid that can balance HSO4 - The ionization of ions promotes the electrochemical process. At the same time, the introduction of small molecule organic acids avoids the entry of difficult-to-separate impurity ions.
[0028] Example 1: One embodiment of the present invention provides a method for preparing an all-vanadium electrolyte using a multi-mixed acid, comprising the following steps:
[0029] Sulfuric acid (concentration of 3.8 mol / L) and water are prepared into a sulfuric acid solution in a volume ratio of 1:2. At 85°C, fully activate the V2O5 powder with a concentration of ≥99.9% in the sulfuric acid solution for 1.5 hours, then cool down. When the temperature drops to 60°C, add the reducing agent oxalic acid (68% of the mass of the V2O5 powder) at a feeding rate of 5 kg / min. Stir the reaction for 1.5 hours to obtain a tetravalent vanadium sulfate stock solution. The volume is adjusted to a total vanadium concentration of 1.6 mol / L. Tetravalent vanadium accounts for more than 98% of the total vanadium, meeting the requirements of GB / T 37204-2018. Then the electrolysis equipment is used at 50 mA / cm 2 Electrolysis was performed at a current density of 1. After electrolysis, the negative electrode solution was recorded as 1# electrolyte. The 1# electrolyte was used to assemble the all-vanadium battery system using the Xinwei CTE-4008D-5V30A charge and discharge tester. The performance of 1# electrolyte was tested. Figure 1 At the same time, when the SOC (battery state of charge) is 70%, the positive electrode solution is taken and the V 总 and V (V) Concentration, specific data see Table 1.
[0030] Embodiment 2: One embodiment of the present invention provides a method for preparing an all-vanadium electrolyte using a multi-mixed acid, comprising the following steps:
[0031] Prepare sulfuric acid (concentration of 3.8 mol / L) and water in a volume ratio of 1:2 to form a sulfuric acid aqueous solution. At 85°C, fully activate the V2O5 powder with a concentration of ≥99.9% in the sulfuric acid solution for 1.5 hours, then cool it down. When the temperature drops to 60°C, add the reducing agent oxalic acid (68% of the mass of the V2O5 powder) at a feeding rate of 5 kg / min. Stir the reaction for 1.5 hours to obtain a tetravalent vanadium sulfate stock solution. Make the volume to a total vanadium concentration of 1.6 mol / L. Tetravalent vanadium accounts for more than 98% of the total vanadium, meeting the requirements of GB / T 37204-2018. Then pass through the electrolysis equipment at 80 mA / cm 2 Electrolysis was performed at a current density of 1.5 %. After electrolysis, the negative electrode solution was recorded as 2# electrolyte. The 2# electrolyte was used to assemble the all-vanadium battery system using the Xinwei CTE-4008D-5V30A charge and discharge tester. The performance of 2# electrolyte was tested. Figure 2 At the same time, when the SOC (battery state of charge) is 70%, the positive electrode solution is taken and the V 总 and V (V) Concentration, specific data see Table 1.
[0032] Example 3: One embodiment of the present invention provides a method for preparing an all-vanadium electrolyte using a multi-mixed acid, comprising the following steps:
[0033] Sulfuric acid (concentration of 3.8 mol / L) and water are prepared into a sulfuric acid aqueous solution in a volume ratio of 1:2. At 85°C, V2O5 powder with a concentration of ≥99.9% is fully activated in the sulfuric acid solution for 1.5 hours, then cooled. When the temperature drops to 60°C, oxalic acid (68% of the mass of V2O5 powder) as a reducing agent is added at a feeding rate of 5 kg / min. After stirring for 1.5 hours, a tetravalent vanadium sulfate stock solution is obtained. Methanesulfonic acid and hydrochloric acid (the mass percentage concentration of hydrochloric acid is 32%; the concentration of methanesulfonic acid is 0.4 mol / L, and the concentration of hydrochloric acid is 0.8 mol / L) are added in a molar ratio of 1:2, and the total vanadium concentration is 1.6 mol / L. Tetravalent vanadium accounts for more than 98% of the total vanadium, meeting the requirements of GB / T 37204-2018. Then, the electrolysis equipment is used at 50 mA / cm 2 Electrolysis was performed at a current density of 1.5 %. After electrolysis, the negative electrode solution was recorded as 3# electrolyte. The 3# electrolyte was used to assemble the all-vanadium battery system using the Xinwei CTE-4008D-5V30A charge and discharge tester to test the performance of the 3# electrolyte. The performance is as follows: Figure 3 At the same time, when the SOC (battery state of charge) is 70%, the positive electrode solution is taken and the V 总 and V (V) Concentration, specific data see Table 1.
[0034] Embodiment 4: One embodiment of the present invention provides a method for preparing an all-vanadium electrolyte using a multi-mixed acid, comprising the following steps:
[0035] Sulfuric acid (concentration of 3.8 mol / L) and water are prepared into a sulfuric acid aqueous solution in a volume ratio of 1:2. At 85°C, V2O5 powder with a concentration of ≥99.9% is fully activated in the sulfuric acid solution for 1.5 hours, then cooled. When the temperature drops to 60°C, oxalic acid (68% of the mass of V2O5 powder) as a reducing agent is added at a feeding rate of 5 kg / min. After stirring for 1.5 hours, a tetravalent vanadium sulfate stock solution is obtained. Methanesulfonic acid and hydrochloric acid (the mass percentage concentration of hydrochloric acid is 32%; the concentration of methanesulfonic acid is 0.4 mol / L, and the concentration of hydrochloric acid is 0.8 mol / L) are added in a molar ratio of 1:2, and the total vanadium concentration is set to 1.6 mol / L. Tetravalent vanadium accounts for more than 98% of the total vanadium, meeting the requirements of GB / T 37204-2018. Then, the electrolysis equipment is used at 80 mA / cm 2 Electrolysis was performed at a current density of 1.5 %. After electrolysis, the negative electrode solution was recorded as 4# electrolyte. The 4# electrolyte was used to assemble the all-vanadium battery system using the Xinwei CTE-4008D-5V30A charge and discharge tester to test the performance of the 4# electrolyte. The performance is as follows: Figure 4 At the same time, when the SOC (battery state of charge) is 70%, the positive electrode solution is taken and the V 总 and V(V) Concentration, specific data see Table 1.
[0036] Table 1 Performance and V of electrolytes 1# to 4# prepared in Examples 1 to 4 (V) and V 总 Concentration statistics
[0037]
[0038] As can be seen from Table 1, at the same current density, the mixed acid electrolyte with the addition of methanesulfonic acid-hydrochloric acid can improve the three major efficiency of battery charge and discharge, reduce the precipitation of pentavalent vanadium, and reduce the charging open circuit voltage to varying degrees; under the same system of electrolytic solvents (single acid or mixed acid type), the increase in current density will reduce the charge and discharge performance of vanadium batteries to a certain extent. In summary, compared with pure sulfuric acid electrolyte, the sulfuric acid-methanesulfonic acid-hydrochloric acid mixed acid system electrolyte can improve the three major efficiencies to a certain extent, reduce the charging open circuit voltage, and reduce the precipitation of pentavalent vanadium, thereby improving the charge and discharge performance.
[0039] The above are only preferred embodiments of the present invention. It should be pointed out that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention. These should also be regarded as the protection scope of the present invention. These will not affect the effect of the implementation of the present invention and the practicality of the patent.
Claims
1. A method for preparing all-vanadium electrolyte using multi-mixed acid, It is characterized in that The following steps are involved: At a certain temperature, the concentration is ≧99.9%V 2 O 5 The powder is dissolved in a sulfuric acid solution prepared by water-sulfuric acid, fully activated for a certain period of time, cooled to a certain temperature and then oxalic acid is added, reacted for a certain period of time and then cooled, and then a certain amount of methanesulfonic acid-hydrochloric acid mixed solution is added to make up the volume to prepare a tetravalent vanadium sulfate stock solution, and then the tetravalent vanadium sulfate stock solution is evenly divided into positive and negative electrode barrels, and electrolyzed with an electrolysis device to obtain a 3.5-valent all-vanadium electrolyte.
2. The method for preparing all-vanadium electrolyte by using poly-mixed acid according to claim 1, It is characterized in that The V 2 O 5 The initial temperature of the feed is 75-95°C.
3. The method for preparing all-vanadium electrolyte by using poly-mixed acid according to claim 1, It is characterized in that The sulfuric acid and water are configured into a sulfuric acid solution in a volume ratio of 1:1 to 1:
3.
4. The method for preparing all-vanadium electrolyte by using multi-mixed acid according to claim 1, It is characterized in that The V 2 O 5 The activation time is 0.5 to 3 hours.
5. The method for preparing all-vanadium electrolyte by using multi-mixed acid according to claim 1, It is characterized in that When the oxalic acid is added, the temperature of the solution is cooled to 55-65°C.
6. The method for preparing all-vanadium electrolyte by using poly-mixed acid according to claim 1, It is characterized in that After the oxalic acid is added, the reduction reaction time is 0.5 to 3 hours.
7. The method for preparing all-vanadium electrolyte by using multi-mixed acid according to claim 1, It is characterized in that The adding speed of the oxalic acid is 4-8 kg / min; if a variable frequency feeder device is used to feed the oxalic acid, the feeding frequency is 10-22 Hz.
8. The method for preparing all-vanadium electrolyte by using multi-mixed acid according to claim 1, It is characterized in that When the methanesulfonic acid-hydrochloric acid mixed acid is added, the solution temperature is 40° C., wherein the mass percentage concentration of hydrochloric acid is 32-40%, and the molar ratio of the methanesulfonic acid to the hydrochloric acid is 1:1-1:
5.
9. The method for preparing all-vanadium electrolyte by using multi-mixed acid according to claim 1, It is characterized in that The total vanadium concentration of the all-vanadium electrolyte is 1.5-1.8 mol / L, the sulfuric acid concentration is 2-4.5 mol / L, the methanesulfonic acid concentration is 0.1-0.6 mol / L, and the hydrochloric acid concentration is 0.5-1.5 mol / L.
10. The method for preparing all-vanadium electrolyte by using poly-mixed acid according to claim 1, It is characterized in that The electrolysis equipment is a Xinwei CTE-4008D-5V30A charge and discharge instrument, with a charge cut-off voltage of 1.55V, a discharge cut-off voltage of 1.00V, and a current density of 50-120mA / cm 2 , the electrode area is 48cm 2 , using single battery charging and discharging.
Citation Information
Cited By
A high-temperature-resistant electrolyte for a vanadium flow battery, a preparation method thereof and a vanadium flow battery
CN122696725A