Bonding structure, semiconductor device and method for manufacturing the same

By using a combination of phosphorus-containing copper alloy and silver particles in semiconductor devices to form the Cu10Sn3 phase, the problem of poor crack resistance of existing joint materials at high temperatures is solved, and a highly reliable joint structure is achieved, which is suitable for future high-temperature operations. Semiconductor devices.

CN112997284BActive Publication Date: 2024-10-22MITSUBISHI ELECTRIC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201880099193.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-11-08
Publication Date
2024-10-22
Estimated Expiration
2038-11-08

AI Technical Summary

Technical Problem

The bonding materials used in existing semiconductor devices contain harmful lead and precious metals, and it is difficult to maintain the crack resistance of the joints at high temperatures, making them unable to meet the needs of future high-temperature operations.

Method used

Using copper alloy particles and silver particles containing 1-7% phosphorus, the Cu10Sn3 phase is formed through the combination of the Cu6Sn5 coating layer and the Ag3Sn coating layer. The proportion and amount of the Cu alloy particles and Ag particles are adjusted to improve the resistance of the joint structure. Crackability.

Benefits of technology

At high temperatures, the crack resistance of the joint portion of the semiconductor device is significantly improved, the occurrence of cracks is avoided, the change rate of the thermal resistance value is reduced, and the reliability of the joint structure is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112997284B_ABST
    Figure CN112997284B_ABST
Patent Text Reader

Abstract

A bonding structure is a bonding structure existing between a semiconductor element and a substrate, wherein the bonding structure comprises: a Sn phase, a Cu alloy particle containing 1 mass % or more and less than 7 mass % of P, and an Ag particle, the Cu alloy particle is coated with a Cu6Sn5 layer, the Ag particle is coated with an Ag3Sn layer, and the Cu alloy particle and the Ag particle are bonded to each other via a Cu 10 The Sn3 phase is at least partially combined, and the total amount of the Cu alloy particles and the Ag particles added is greater than 25 mass % and less than 65 mass % relative to the joint structure, and the mass ratio of the amount of the Ag particles added to the amount of the Cu alloy particles added is greater than 0.2 and less than 1.2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a junction structure, a semiconductor device and a method for manufacturing the same. Background Art

[0002] In recent years, the requirements for the reliability of semiconductor devices have been increasing. In particular, since the difference in thermal expansion coefficients between semiconductor elements and circuit substrates is large, it is necessary to improve the reliability of the joints between them. In the past, semiconductor elements using silicon (Si), gallium arsenic (GaAs), etc. as substrates were mostly used, and their operating temperatures were 100°C to 125°C. For the bonding materials used when bonding these semiconductor elements to the circuit substrate, a high melting point for multi-stage bonding, crack resistance against repeated thermal stress associated with start-up and stop, and contamination resistance of the semiconductor device are required. In response to these requirements, 95Pb-5Sn (mass %) is used as a bonding material in semiconductor devices using semiconductor elements using Si as a substrate. In addition, 80Au-20Sn (mass %) is used as a bonding material in semiconductor devices using semiconductor elements using gallium arsenic as a substrate. However, from the perspective of reducing environmental load, 95Pb-5Sn, which contains a large amount of harmful lead (Pb), has problems. In addition, 80Au-20Sn containing a large amount of precious metals has problems due to the high price and buried amount of precious metals. Therefore, there is a strong demand for a bonding material that can serve as an alternative to these bonding materials.

[0003] On the other hand, from the perspective of energy saving, semiconductor devices using semiconductor elements based on silicon carbide (SiC) or gallium nitride (GaN) are being actively developed as next-generation semiconductor devices. For these semiconductor devices, the operating temperature is set to 175°C or above from the perspective of reducing power loss, and it is said that it will reach 300°C in the future. Therefore, it is necessary to prevent cracks from occurring at the joint between the semiconductor element and the circuit board even when operating at a higher temperature.

[0004] Therefore, it is necessary to solve the problems of conventional bonding materials containing lead or noble metals and to improve the crack resistance of the bonding portion when the semiconductor device is operated at high temperature.

[0005] Therefore, in Patent Document 1, as a method for joining a semiconductor element in a semiconductor device to a substrate, a joining method having the following steps is disclosed: a step of applying a joining material containing Cu particles and Sn particles to the joining surface of the semiconductor element or the substrate; a step of bringing the joining surface of the semiconductor element and the joining surface of the substrate into contact (merging) via the joining material; a step of heating at a temperature higher than the melting point of Sn to cause transitional liquid phase sintering of Cu and Sn in the joining material so that the joining material becomes a composition containing Cu6Sn5 and Cu3Sn; and a step of heating to change the Cu6Sn5 of the joining material into Cu3Sn to increase the ratio of Cu3Sn.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2014-199852 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, in patent document 1, no research has been conducted on the influence of the composition ratio of Cu particles and Sn particles on the crack resistance of the joint. If a large amount of Cu particles are added, the fluidity of Sn is reduced, and it is believed that voids are generated at the position where particles are sealed to each other. When thermal shock is applied to the joint comprising the void, cracks are easily generated. And then, for the Cu-Sn alloy represented by Cu6Sn5, although considering the existence of Cu as a solid solution region of about 5 mass % from the metal phase diagram, it shows the state of 2 phase separation types. Therefore, if there is no low melting point Sn at the interface of Cu6Sn5, it becomes a void, which can become the starting point of cracks. Therefore, the crack resistance of the joint formed by the joining method of patent document 1 cannot be said to be sufficient.

[0011] The present invention has been made to solve the above-mentioned problems, and aims to provide a bonding structure with high bonding reliability that is unlikely to cause cracks even when the semiconductor device is operated at high temperatures. Another object of the present invention is to provide a semiconductor device having the bonding structure and a method for manufacturing the same.

[0012] Means for solving problems

[0013] The present invention is a bonding structure, which is a bonding structure existing between a semiconductor element and a substrate, wherein the bonding structure comprises: a Sn phase, a Cu alloy particle containing 1 mass % or more and less than 7 mass % of P, and an Ag particle, wherein the Cu alloy particle is coated with a Cu6Sn5 coating layer, the Ag particle is coated with an Ag3Sn coating layer, and the Cu alloy particle and the Ag particle are bonded to each other via a Cu 10The Sn3 phase is at least partially combined, and the total amount of the Cu alloy particles and the Ag particles added is greater than 25 mass % and less than 65 mass % relative to the joint structure, and the mass ratio of the amount of the Ag particles added to the amount of the Cu alloy particles added is greater than 0.2 and less than 1.2.

[0014] The present invention is a semiconductor device, wherein a semiconductor element and a substrate are bonded via the bonding structure.

[0015] The present invention is a method for manufacturing a semiconductor device, comprising: a process for preparing a paste, wherein Sn particles, Cu alloy particles containing 1 mass % or more and less than 7 mass % of P, Ag particles and a solvent are mixed to prepare the paste, wherein the total amount of the Cu alloy particles and the Ag particles is 25 mass % or more and less than 65 mass % relative to the total amount of the Sn particles, the Cu alloy particles and the Ag particles, and the mass ratio of the Ag particles to the Cu alloy particles is 0.2 or more and less than 1.2; a process for applying the paste on a substrate; a process for placing a semiconductor element on the paste; a process for heating to a temperature of 120° C. or more and 200° C. or less to volatilize the solvent in the paste; and a process for heating to a temperature of 340° C. or more and less than 450° C. to bond the semiconductor element to the substrate.

[0016] Effects of the Invention

[0017] According to the present invention, a highly reliable bonded structure that is less likely to crack even when the semiconductor device is operated at high temperatures can be provided. In addition, according to the present invention, a semiconductor device having a highly reliable bonded structure and a method for manufacturing the same can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic cross-sectional view of a semiconductor device including the junction structure according to the first embodiment.

[0019] Figure 2 It is a flowchart of the manufacturing method of the semiconductor device provided with the junction structure concerning Embodiment 1.

[0020] Figure 3 It is a schematic diagram showing the state of components contained in the paste.

[0021] Figure 4 This is a schematic diagram showing a step of applying a paste on a substrate in the method for manufacturing a semiconductor device according to the first embodiment.

[0022] Figure 5This is a schematic diagram showing a step of placing a semiconductor element on a paste applied on a substrate in the method for manufacturing a semiconductor device according to the first embodiment.

[0023] Figure 6 This is a schematic diagram showing a step of volatilizing the solvent in the paste by heating in the method for manufacturing the semiconductor device according to the first embodiment.

[0024] Figure 7 This is a schematic diagram showing a step of bonding a semiconductor element and a substrate by heating in the method for manufacturing a semiconductor device according to the first embodiment.

[0025] Figure 8 This is the ternary phase diagram of Ag-Sn-Cu.

[0026] Fig. 9 It is a graph showing the relationship between the total amount of Cu alloy particles and Ag particles and the rate of change of thermal resistance value at each Ag / Cu mass ratio.

[0027] Fig.10 It is a graph showing the relationship between the total amount of Cu alloy particles and Ag particles and the rate of change of thermal resistance value at the P content in each Cu alloy particle. DETAILED DESCRIPTION

[0028] Implementation method 1.

[0029] Figure 1 It is a schematic cross-sectional view of a semiconductor device including the junction structure according to the first embodiment of the present invention. Figure 1 In the embodiment, the semiconductor device is a device in which a semiconductor element 1 and a substrate 2 are bonded via a bonding structure 3. The bonding structure 3 includes: a tin (Sn) phase 4, a copper (Cu) alloy particle 5 containing 1 mass % or more and less than 7 mass % of phosphorus (P), and a silver (Ag) particle 6. The surface of the Cu alloy particle 5 is coated with a Cu6Sn5 coating layer 7. The surface of the Ag particle 6 is coated with an Ag3Sn coating layer 8. The Cu alloy particle 5 and the Ag particle 6 are bonded via a Cu 10 The Sn3 phase 9 is at least partially bonded. Between the semiconductor element 1 and the joint structure 3, an Ag layer 10 and an Ag3Sn interface layer 11 are formed in sequence from the semiconductor element 1 side. Between the substrate 2 and the joint structure 3, a Cu layer 12 and a Cu6Sn5 interface layer 13 are formed in sequence from the substrate 2 side. In addition, there are voids 14 generated in the manufacturing process of the semiconductor device in the joint structure 3. Furthermore, in the joint structure 3, fine Cu-P compound particles 15 generated in the manufacturing process of the semiconductor device can be distributed in a dotted manner.

[0030] In the joint structure 3 involved in the first embodiment, the total amount of the Cu alloy particles 5 and the Ag particles 6 added is 25 mass% or more and less than 65 mass%, preferably 30 mass% or more and 60 mass% or less, relative to the joint structure 3. When the total amount of the Cu alloy particles 5 and the Ag particles 6 added is less than 25 mass%, Sn is insufficient relative to the Cu alloy particles 5 and the Ag particles 6, and a low melting point phase is found in the joint structure 3. On the other hand, when the total amount of the Cu alloy particles 5 and the Ag particles 6 added is 65 mass% or more, a large number of voids are generated in the joint structure 3, and cracks are easily generated.

[0031] In the joint structure 3 involved in embodiment 1, the mass ratio of the addition amount of Ag particles 6 to the addition amount of Cu alloy particles 5 (Ag / Cu mass ratio) is 0.2 or more and less than 1.2, preferably 0.3 or more and 1.1 or less. When the Ag / Cu mass ratio is less than 0.2 or more than 1.2, a large number of voids are generated in the joint structure 3, and cracks are easily generated.

[0032] The cross-sectional thickness of the joined structure 3 is preferably 20 μm to 150 μm, more preferably 30 μm to 130 μm. When the cross-sectional thickness of the joined structure 3 is within the above range, there are few voids in the joined structure 3, and excellent crack resistance can be achieved.

[0033] When the phosphorus content of the Cu alloy particles 5 is less than 1% by mass and more than 7% by mass, a large number of voids are generated in the joint structure 3, and cracks are easily generated. The phosphorus content of the Cu alloy particles 5 is preferably more than 2% by mass and less than 6% by mass. There is no particular limitation on the shape of the Cu alloy particles 5, and it is preferably spherical. The average particle size of the Cu alloy particles 5 is preferably more than 5μm and less than 50μm, and more preferably more than 7μm and less than 40μm. When the average particle size of the Cu alloy particles 5 is within the above range, the solvent is easily detached from the gaps between the Cu alloy particles 5, the Ag particles 6 and the Sn particles, and the oxide film on the surface of the Cu alloy particles 5 is easily removed by the solvent, so it can form a compound with Sn. In addition, there is no particular limitation on the thickness of the Cu6Sn5 coating layer 7 that covers the surface of the Cu alloy particles 5, and it is preferably more than 3μm and less than 20μm.

[0034] The shape of the Ag particles 6 is not particularly limited, and is preferably spherical. The average particle size of the Ag particles 6 is preferably 5 μm or more and 50 μm or less, and more preferably 7 μm or more and 40 μm or less. When the average particle size of the Ag particles 6 is within the above range, the solvent is easily separated from the gaps between the Cu alloy particles 5, the Ag particles 6, and the Sn particles, and the oxide film on the surface of the Ag particles 6 is easily removed by the solvent, so that a compound can be formed with Sn. The thickness of the Ag3Sn coating layer 8 that covers the surface of the Ag particles 6 is not particularly limited, and is preferably 5 μm or more and 30 μm or less.

[0035] In addition, in this specification, the average particle size is a value measured using an apparatus in accordance with the particle size analysis-laser diffraction / scattering method described in JIS-Z-8825.

[0036] The thickness of the Ag 3 Sn interface layer 11 is not particularly limited, but is preferably 5 μm or more and 30 μm or less.

[0037] The thickness of the Cu6Sn5 interface layer 13 is not particularly limited, but is preferably 3 μm or more and 20 μm or less.

[0038] In this specification, the thicknesses of the Cu6Sn5 coating layer 7, the Ag3Sn coating layer 8, the Ag3Sn interface layer 11, and the Cu6Sn5 interface layer 13 are values ​​measured at the cross section of the bonding portion using a SEM (Scanning Electron Microscope) device.

[0039] The semiconductor element 1 may be a general semiconductor element with silicon (Si) as a substrate, preferably a wide bandgap semiconductor element with a wide bandgap semiconductor material such as silicon carbide (SiC), gallium nitride (GaN)-based materials, diamond, etc. having a wider bandgap than silicon as a substrate. On the semiconductor element 1, an Ag layer 10 is formed to ensure bonding with the bonding structure 3. The thickness of the Ag layer 10 is not particularly limited as long as it can ensure bonding with the bonding structure 3.

[0040] As the material of the substrate 2, silicon nitride (Si3N4), aluminum nitride (AlN), copper-molybdenum alloy, etc. can be listed. On the substrate 2, in order to ensure the bonding property with the bonding structure 3, a Cu layer 12 is formed. The thickness of the Cu layer 12 is not particularly limited as long as the bonding property with the bonding structure 3 can be ensured. In addition, the Cu layer 12 can be a Cu alloy such as Cu-Mo, Cu-Cr, Cu-W, Cu-P, Cu-Sn, and Cu-Zn as long as it has Cu as the main component.

[0041] Next, a method for manufacturing a semiconductor device including the junction structure according to the first embodiment will be described. Figure 2It is a flowchart of the manufacturing method of the semiconductor device provided with the junction structure concerning Embodiment 1.

[0042] First, Sn particles, Cu alloy particles containing 1 mass % or more and less than 7 mass % of P, Ag particles, and a solvent are mixed to prepare a paste ( S1 ). Figure 3 Schematic diagram showing the state of the components contained in the paste. Figure 3 As shown in , in the paste 16, the Sn particles 17, the Cu alloy particles 5 and the Ag particles 6 are in a state of being dispersed in the solvent 18. The method for producing the Sn particles 17, the Cu alloy particles 5 and the Ag particles 6 used here is not particularly limited, and a known method such as an atomization method can be listed. As the solvent 18, a solvent used in a known bonding material paste can be used, for example, terpineol, diethylene glycol monobutyl ether, methyl ethyl ketone, isophorone, etc. can be listed. The solvent 18 is preferably contained in a range of 10 mass % or more and 30 mass % or less relative to the paste 16. The total amount of the Cu alloy particles 5 and the Ag particles 6 contained in the paste 16 is 25 mass % or more and less than 65 mass %, preferably 30 mass % or more and 60 mass % or less, relative to the total amount of the Sn particles 17, the Cu alloy particles 5 and the Ag particles 6. When the total amount of the Cu alloy particles 5 and the Ag particles 6 is less than 25% by mass, Sn is insufficient relative to the Cu alloy particles 5 and the Ag particles 6, and a low melting point phase is found in the bonded structure 3. On the other hand, when the total amount of the Cu alloy particles 5 and the Ag particles 6 is 65% by mass or more, a large number of voids are generated in the bonded structure 3, and cracks are easily generated. The mass ratio of the Ag particles 6 contained in the paste 16 to the Cu alloy particles 5 (Ag / Cu mass ratio) is made to be 0.2 or more and less than 1.2, preferably 0.3 or more and 1.1 or less. When the Ag / Cu mass ratio is less than 0.2 or more than 1.2, a large number of voids are generated in the bonded structure 3, and cracks are easily generated.

[0043] Secondly, if Figure 4 As shown in , the prepared paste 16 is applied on the Cu layer 12 of the substrate 2 (S2). The coating thickness of the paste 16 can be appropriately adjusted so that the joint structure 3 has a desired cross-sectional thickness. As far as the coating method of the paste 16 is concerned, there is no particular limitation as long as the paste 16 can be uniformly coated with the desired coating thickness. For example, a method of coating using a scraper, a method of coating using a dispenser, etc. can be cited.

[0044] Secondly, if Figure 5As shown in , the semiconductor element 1 is mounted on the paste 16 applied on the Cu layer 12 of the substrate 2 so that the Ag layer 10 of the semiconductor element 1 is in contact with the paste 16 (S3). In order to mount the semiconductor element 1 on the paste 16 with high accuracy, a device capable of automatically recognizing the upper surface of the paste 16, such as a chip mounter manufactured by Astrid FA Co., Ltd., can be used.

[0045] Secondly, if Figure 6 As shown in , the laminate including the semiconductor element 1, the paste 16 and the substrate 2 is heated to a temperature of 120°C to 200°C to volatilize the solvent 18 and remove the solvent 18 from the paste 16 (S4). The obtained dried paste 19 is composed of Sn particles 17, Cu alloy particles 5 and Ag particles 6. The heating can be performed in any of a vacuum atmosphere, an air atmosphere, an inert gas atmosphere, etc., but it is necessary to perform the heating in a manner that the Sn particles 17 are not melted. The heating temperature can be appropriately set in the range of 120°C to 200°C according to the boiling point of the solvent 18.

[0046] Finally, if Figure 7 As shown in , the stacked body including the semiconductor element 1, the paste dried body 19 and the substrate 2 is heated to a temperature of 340°C or higher and less than 450°C, so that the semiconductor element 1 and the substrate 2 are bonded via the bonding structure 3 (S5). In this process, the Sn particles 17 melt at the stage where the heating temperature reaches 232°C. When the Sn particles 17 melt, an Ag3Sn interface layer 11 is formed at the interface with the Ag layer 10 of the semiconductor element 1, and a Cu6Sn5 interface layer 13 is formed at the interface with the Cu layer 12 of the substrate 2. At the same time, a Cu6Sn5 coating layer 7 is formed in a manner covering the surface of the Cu alloy particles 5, and an Ag3Sn coating layer 8 is formed in a manner covering the surface of the Ag particles 6. There is a lot of dissolved oxygen in the Cu alloy particles 5. This oxygen deteriorates the bonding property. However, when the Cu6Sn5 coating layer 7 is formed, the P contained in the Cu alloy particles 5 acts as a deoxidizer and preferentially reacts with oxygen to form phosphorus oxide. The phosphorus oxide is vaporized when the heating temperature reaches 270°C. Sometimes, a part of the P contained in the Cu alloy particles 5 does not react with oxygen and precipitates as fine Cu-P compound particles 15 in the bonded structure 3. If the P content of the Cu alloy particles 5 is 1% by mass or more and less than 7% by mass, there is no adverse effect on the bonding reliability. Then, when the heating temperature reaches 340°C or more and less than 450°C, a phase transition occurs between the Cu6Sn5 coating layer 7 and the Ag3Sn coating layer 8 to form Cu 10 Sn3 phase 9. Through this Cu 10Sn3 phase 9 at least partially bonds Cu alloy particles 5 and Ag particles 6, thereby reducing the number of voids 14 that may serve as crack starting points. As a result, cracks are less likely to occur in the bonded structure 3 even when the semiconductor device is operated at high temperatures.

[0047] The semiconductor device including the bonded structure 3 manufactured in this way is unlikely to be cracked even when operated at high temperatures and has high reliability.

[0048] Furthermore, in the above description, the form of bonding a semiconductor element to a substrate is described, but it is not limited to this, and it can also be applied to a form of bonding a semiconductor element to a lead frame, a form of bonding a substrate to a cooling fin, etc. In addition, it is not limited to the case of bonding one semiconductor element to one substrate, and multiple semiconductor elements and components can be arranged on one substrate and bonded together.

[0049] Example

[0050] <Example 1>

[0051] Sn particles with an average particle size of 20 μm, Cu alloy particles with a P content of 5% by mass and an average particle size of 20 μm, Ag particles, and terpineol as a solvent were mixed to prepare a paste. The total amount of the Cu alloy particles and the Ag particles was 50% by mass relative to the total amount of the Sn particles, the Cu alloy particles, and the Ag particles, and the Ag / Cu mass ratio was 0.67 (rounded to the third decimal place). In addition, the amount of the solvent was 20% by mass relative to the paste. In addition, the Sn particles, Cu alloy particles, and Ag particles used were manufactured by an atomization method, and their shapes were all spherical.

[0052] After arranging a stainless steel metal mask with an opening size of 10 mm × 10 mm on a DBC (Direct Bonded Copper) substrate with a size of 20 mm × 20 mm, the prepared paste was applied using a scraper to a thickness of 150 μm. In addition, as a DBC substrate, a substrate having a structure in which a 0.4 mm thick Cu layer was formed on both sides of a 0.6 mm thick ceramic (Si3N4) was used.

[0053] A semiconductor element is placed on the paste applied on the DBC substrate so that the upper surface of the paste is in contact with the Ag layer. The semiconductor element is a semiconductor element in which a 7μm thick Ag layer is formed on one side of silicon carbide (SiC) with a size of 10mm×10mm and a thickness of 0.3mm.

[0054] Next, the laminate including the DBC substrate, the paste, and the semiconductor element was heated to 180° C. in a vacuum reflow oven to volatilize the terpineol in the paste.

[0055] Next, the stacked body including the DBC substrate, the dried paste body, and the semiconductor element was heated to 340° C. at a temperature increase rate of 30° C. / min in a vacuum reflow furnace and then naturally cooled to obtain a semiconductor device.

[0056] In order to inspect the generation of voids in the bonded structure of the obtained semiconductor device in a non-destructive manner, an ultrasonic flaw detector (SAT) (Fine SAT III manufactured by Hitachi Parasol Systems Co., Ltd.) was used to observe the side of the bonded structure. The observation image was binarized using binarization software (Photoshop manufactured by Advanced Systems Co., Ltd.) to calculate the void ratio. The situation where the void ratio is less than 10% is evaluated as good initial bonding (○), and the situation where the void ratio is more than 10% is evaluated as poor initial bonding (×). The results are shown in Table 1.

[0057] <Examples 2 to 4 and Comparative Examples 1 to 3>

[0058] A semiconductor device was obtained in the same manner as in Example 1 except that the bonding temperature was changed to the temperature shown in Table 1. The occurrence of voids in the bonded structure of the obtained semiconductor device was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0059]

Table 1

[0060] Junction temperature Void ratio Initial fertility <![CDATA[Cu 10 Presence or absence of Sn3 phase]]> Comparative Example 1 300℃ 50% × none Comparative Example 2 330℃ 40% × none Example 1 340℃ 8% ○ have Example 2 380℃ 6% ○ have Example 3 400℃ 5% ○ have Example 4 440℃ 7% ○ have Comparative Example 3 450℃ 52% × none

[0061] As shown in Table 1, when the bonding temperature is less than 340°C, the initial bonding becomes poor. This is believed to be because when the Cu6Sn5 coating layer, Ag3Sn coating layer, Cu6Sn5 interface layer and Ag3Sn interface layer are formed with heating, a volume shrinkage of about 10% occurs, resulting in voids. When the bonding temperature is above 340°C and less than 450°C, the voids decrease sharply and the initial bonding becomes good. Composition analysis of the cross-sections of these bonded structures was performed, and the results showed that Cu6Sn5 was formed between the Cu6Sn5 coating layer and the Ag3Sn coating layer. 10 Sn3 phase. This is believed to be because when the bonding temperature reaches 340°C or higher, a phase transition occurs between the Cu6Sn5 coating layer and the Ag3Sn coating layer, forming a Cu 10 Sn3 phase and Sn-rich melt phase (Sn-Cu-Ag eutectic phase). 10 The mechanism of Sn3 phase can be explained by Figure 8 The Ag-Sn-Cu ternary phase diagram shown in FIG was read. When the bonding temperature was 450°C, the initial bonding became poor. The composition analysis of the cross section of the bonded structure was performed, and no Cu was found. 10Sn3 phase. This is considered to be because a Cu3Sn coating layer is formed on the surface of the Cu alloy particles instead of a Cu6Sn5 coating layer, and the above-mentioned phase transformation does not occur.

[0062] <Examples 5 to 13 and Comparative Examples 4 to 22>

[0063] A semiconductor device was obtained in the same manner as in Example 1 except that the total amount of the Cu alloy particles and the Ag particles and the Ag / Cu mass ratio were changed as shown in Tables 2 and 3 and the bonding temperature was changed to 400°C.

[0064] The bonded structure was cut out from the obtained semiconductor device, heated to 300°C using differential scanning calorimetry (DSC), and it was confirmed whether a melting peak of 210 to 240°C from the melting point of the Sn phase was generated. The bonded structure in which the melting peak was detected was evaluated as having a low melting point phase, and the bonded structure in which the melting peak was not detected was evaluated as having no low melting point phase. Specifically, in the atmosphere, the temperature was heated from room temperature to 300°C at a heating rate of 10°C / min. If the melting peak amount at 210°C to 240°C was less than 20mJ / mg, it was judged to have no low melting point phase, and if it was 20mJ / mg or more, it was judged to have a low melting point phase. The results are shown in Tables 2 and 3.

[0065] The occurrence of voids in the obtained bonded structure of the semiconductor device was evaluated in the same manner as in Example 1. The results are shown in Tables 2 and 3.

[0066] In addition, the initial thermal resistance value of the semiconductor device was measured by the laser flash method. Secondly, as a simulation of the high-temperature operation of the semiconductor device, a liquid tank type thermal shock tester was used, and one cycle was set as 1 cycle after holding at 50°C for 30 seconds and then at 175°C for 30 seconds, and it was performed for 100,000 cycles. The thermal resistance value after 100,000 cycles was measured, and the rate of change relative to the initial thermal resistance value was calculated according to the following formula. The results are shown in Tables 2 and 3. When the rate of change of the thermal resistance value is 10% or more, it can be judged that the crack resistance of the semiconductor device during high-temperature operation is poor.

[0067] Change rate of thermal resistance value (%) = (initial thermal resistance value - thermal resistance value after 100,000 cycles) / initial thermal resistance value × 100

[0068]

Table 2

[0069]

[0070]

Table 3

[0071]

[0072] As shown in Table 2, when Cu alloy particles containing 5% by mass of P are used, if the total amount of Cu alloy particles and Ag particles is 25% by mass or more and less than 65% by mass and the Ag / Cu mass ratio is 0.2 or more and less than 1.2, no low melting point phase is found in the bonded structure, and a semiconductor device with good initial bondability and crack resistance is obtained. On the other hand, as shown in Table 3, even if Cu alloy particles containing 5% by mass of P are used, if the total amount of Cu alloy particles and Ag particles is less than 25% by mass or more than 65% by mass, or the Ag / Cu mass ratio is less than 0.2 or more than 1.2, a low melting point phase is found in the bonded structure or the initial bondability becomes poor, and the crack resistance becomes poor.

[0073] <Examples 14 to 19 and Comparative Examples 23 to 36>

[0074] A semiconductor device was obtained in the same manner as in Example 1 except that the total amount of the Cu alloy particles and the Ag particles and the P content in the Cu alloy particles were changed as shown in Tables 4 and 5 and the bonding temperature was changed to 400°C.

[0075] The presence or absence of a low melting point phase, the occurrence of voids, and the rate of change in thermal resistance in the obtained semiconductor device joint structure were evaluated in the same manner as in Example 5. The results are shown in Tables 4 and 5.

[0076]

Table 4

[0077]

[0078]

Table 5

[0079]

[0080] As shown in Table 4, even if Cu alloy particles containing 1% or 6.5% P are used, if the total amount of Cu alloy particles and Ag particles is 25% or more and less than 65% by mass and the Ag / Cu mass ratio is 0.2 or more and less than 1.2, no low melting point phase is found in the bonded structure, and a semiconductor device with good initial bondability and crack resistance is obtained. On the other hand, as shown in Table 5, even if the Ag / Cu mass ratio is 0.67, if the total amount of Cu alloy particles and Ag particles is less than 25% or more than 65% by mass, or Cu alloy particles with a P content of less than 1% or more than 7% by mass are used, a low melting point phase is found in the bonded structure or the initial bondability becomes poor, and the crack resistance becomes poor.

[0081] The change rate (%) of the thermal resistance value in Tables 2 and 3 was used as the vertical axis, and the total amount of the Cu alloy particles and the Ag particles added to the bonded structure (mass %) was used as the horizontal axis. The results were plotted (plotted) for each Ag / Cu mass ratio. Fig. 9 In addition, the change rate (%) of the thermal resistance value in Tables 4 and 5 was used as the vertical axis, and the total amount of the Cu alloy particles and the Ag particles added to the bonded structure (mass %) was used as the horizontal axis, and the P content (mass %) in each Cu alloy particle was coordinate-plotted (plotted), and the results are shown in Fig.10 In. By Fig. 9 and 10 It was confirmed that for a semiconductor device using Cu alloy particles containing 1 mass % or more and less than 7 mass % of P, with the total amount of Cu alloy particles and Ag particles added being 25 mass % or more and less than 65 mass % relative to the joint structure, and with the Ag / Cu mass ratio being 0.2 or more and less than 1.2, the rate of change in thermal resistance value is less than 10%.

[0082] Description of Reference Numerals

[0083] 1 semiconductor element, 2 substrate, 3 junction structure, 4 Sn phase, 5 Cu alloy particles, 6 Ag particles, 7 Cu6Sn5 coating layer, 8 Ag3Sn coating layer, 9 Cu 10 Sn3 phase, 10 Ag layer, 11 Ag3Sn interface layer, 12 Cu layer, 13 Cu6Sn5 interface layer, 14 voids, 15 Cu-P compound particles, 16 paste, 17 Sn particles, 18 solvent, 19 dried paste.

Claims

1. A bonding structure, which is a bonding structure existing between a semiconductor element and a substrate, wherein: The bonded structure includes: a Sn phase, Cu alloy particles containing 1 mass % or more and less than 7 mass % of P, and Ag particles. The Cu alloy particles are covered with a Cu6Sn5 coating layer, and the Ag particles are covered with an Ag3Sn coating layer. The Cu alloy particles and the Ag particles are connected via Cu 10 The Sn3 phase is at least partially bonded, The total amount of the Cu alloy particles and the Ag particles added to the bonded structure is 25 mass % or more and less than 65 mass %, The mass ratio of the amount of the Ag particles added to the amount of the Cu alloy particles added is 0.2 or more and less than 1.

2.

2. The joint structure according to claim 1, wherein: Cu—P compound particles are distributed in the joint structure in a dotted manner.

3. A semiconductor device, wherein: The semiconductor element and the substrate are bonded via the bonded structure according to claim 1 or 2.

4. The semiconductor device according to claim 3, wherein: Between the semiconductor element and the bonding structure, an Ag layer and an Ag3Sn interface layer are formed in sequence from the semiconductor element side, and between the substrate and the bonding structure, a Cu layer and a Cu6Sn5 interface layer are formed in sequence from the substrate side.

5. A method for manufacturing a semiconductor device, comprising: A paste preparation step of mixing Sn particles, Cu alloy particles containing 1 mass % or more and less than 7 mass % of P, Ag particles, and a solvent to prepare the paste, wherein: The total amount of the Cu alloy particles and the Ag particles is 25 mass % or more and less than 65 mass % relative to the total amount of the Sn particles, the Cu alloy particles and the Ag particles, and the mass ratio of the Ag particles to the Cu alloy particles is 0.2 or more and less than 1.2; The process of coating the paste on a substrate; a step of placing a semiconductor element on the paste; A step of heating the paste to a temperature of 120° C. to 200° C. to volatilize the solvent in the paste; and A step of heating the substrate to a temperature of 340° C. or higher and lower than 450° C. to bond the semiconductor element to the substrate.