Method for making hard mask that can be used in next generation photolithography

By forming a hydrocarbon-ended SnOx film on the substrate surface and irradiating it with EUV light, combining hydroxyl groups to enhance radiation absorption, the problems of low light source power and pattern collapse in the EUV lithography process are solved, and efficient patterning and Etching resistance.

CN113039486BActive Publication Date: 2024-11-12LAM RES CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN201980075389.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-11-14
Filing Date
2019-11-11
Publication Date
2024-11-12
Estimated Expiration
2039-11-11

AI Technical Summary

Technical Problem

The existing EUV lithography processes face the problems of low light source power and light loss. Traditional organic chemical amplification photoresist has a low absorption coefficient in the EUV region and the disadvantages of potentially causing blur or rough line edges, and conventional material thickness leads to pattern collapse. High risk.

Method used

A hydrocarbon-terminated SnOx film is used to form a hydrocarbon-terminated SnOx film on the substrate surface, cleavage the alkyl group by EUV light irradiation, form Sn-H bonds, and enhance radiation absorption by hydroxyl groups, and combine with self-limiting characteristics of atomic layer deposition process or chemical vapor phase. Deposition process prepares an imaging layer with high absorption and etch resistance.

Benefits of technology

It improves the sensitivity and resolution of the EUV lithography process, reduces the exposure dose requirement of the imaging layer, reduces the risk of pattern collapse, and improves the problem of rough line edges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113039486B_ABST
    Figure CN113039486B_ABST
Patent Text Reader

Abstract

The imaging layer on the surface of the substrate can be patterned using next generation photolithography techniques, and the resulting patterned film can be used, for example, as a photolithography mask for semiconductor device production.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Incorporated by Reference

[0002] The PCT application form is filed concurrently with this specification as a part of this application. Each application to which this application claims the benefit or priority as identified in the concurrently filed PCT application form is incorporated herein by reference in its entirety and for all purposes. Technical Field

[0003] The present disclosure relates to systems and methods for fabricating an imaging layer on a surface of a substrate. Such an imaging layer can be patterned using next generation photolithography techniques, and the resulting patterned film can be used, for example, as a photolithography mask for semiconductor device production. Background Art

[0004] The background description provided here generally presents the background of the present technology. The work of the presently designated inventors is not admitted as prior art to the present technology to the extent it is described in this background section and in aspects of the specification that were not determined to be prior art at the time the application was filed.

[0005] The fabrication of semiconductor devices, such as integrated circuits, is a multi-step process involving photolithography. Generally, the process involves depositing material on a wafer and patterning the material by photolithographic techniques to form structural features (e.g., transistors, conductors, and other circuit features) of a semiconductor device. The steps of a typical photolithographic process known in the art include: preparing a substrate; applying a photoresist, such as by spin coating; exposing the photoresist to light having a desired pattern to render the exposed areas of the photoresist more or less soluble in a developer solution; developing by applying a developer solution to remove the exposed or unexposed areas of the photoresist; and performing subsequent processing (e.g., by etching or material deposition) to produce features on the areas of the substrate from which the photoresist has been removed.

[0006] The evolution of semiconductor design has created the need for, and has been driven by, the ability to create smaller and smaller features on semiconductor substrate materials. This technological progress has been characterized as "Moore's Law," with the density of transistors in dense integrated circuits doubling every two years. Indeed, chip design and manufacturing have advanced so that modern microprocessors can accommodate billions of transistors and other circuit features on a single chip. Individual features on such chips can be about 22 nanometers (nm) or smaller, and in some cases less than 10 nm.

[0007] One challenge in fabricating devices with such small features is the ability to reliably and reproducibly produce photolithographic masks with sufficient resolution. Current lithographic processes generally use 193 nm ultraviolet (UV) light to expose the photoresist. Inherent problems arise when the wavelength of the light is significantly larger than the desired size of the features to be produced on the semiconductor substrate. Complex resolution enhancement techniques (e.g., multiple patterning) are required to achieve feature sizes smaller than the wavelength of the light. Therefore, there is a great deal of attention and research effort in developing so-called "next generation lithography" techniques that use electron beam radiation or shorter wavelength light, such as extreme ultraviolet (EUV) radiation having a wavelength of less than 20 nm (e.g., 13.5 nm).

[0008] However, challenges may arise with next generation lithography. For example, the performance of EUV lithography processes may be limited by the low power output of the light source and light loss during patterning. Conventional organic chemically amplified photoresists (CARs) similar to those used in 193 nm UV lithography have potential disadvantages when used in EUV lithography, in particular, for example, they have low absorption coefficients in the EUV region and diffusion of photoactivated chemicals may result in blurring or line edge roughness. In addition, in order to provide the etch resistance required to pattern the underlying device layers, the required thickness of conventional CAR materials may result in high aspect ratios that are at risk of pattern collapse. Therefore, there remains a need for improved EUV photoresist materials having properties such as reduced thickness, greater absorbance, and greater etch resistance. Summary of the invention

[0009] The present disclosure provides methods for making an imaging layer on the surface of a substrate. Such an imaging layer can be patterned into chemically distinct regions (i.e., surface imaging) using next generation lithography techniques (typically such as DUV, EUV, X-ray, and electron beam). The resulting patterned film can be used, for example, as a lithography mask for semiconductor device production.

[0010] In certain implementations, methods according to the present disclosure may include generating SnO x The imaging layer of the thin film, the SnO x The film is terminated with alkyl groups selected so that it will undergo tin-carbon bond cleavage, such as a beta-hydride elimination reaction, when irradiated with EUV light. During the EUV patterning step, the alkyl groups can be cleaved, leaving areas of Sn-H bonds, while the unexposed surface remains alkyl terminated.

[0011] In one embodiment, a method of making an imaging layer on a substrate comprises: providing a substrate having a surface comprising exposed hydroxyl groups; and forming a hydrocarbyl-terminated SnO xThe film is used as an imaging layer, and the hydrocarbon-terminated SnO x The film has tin-carbon bonds that can be cleaved by irradiating the imaging layer.

[0012] In some embodiments, the substrate surface may include hydrocarbyl-terminated SnO x SnO film imaging layer x Hydroxyl terminated SnO on the surface of the substrate material x The underlayer can enhance the absorption of radiation when irradiating the imaging layer and generate secondary electrons from the substrate to further obtain additional EUV photons to make the EUV patterning process more sensitive and reduce the required EUV dose required for imaging layer exposure.

[0013] In various embodiments, the imaging layer can be deposited by an atomic layer deposition process that exhibits self-limiting characteristics. In other embodiments, the imaging layer is a thin film deposited by a (non-self-limiting) chemical vapor deposition process.

[0014] For example, an alkyl-substituted tin capping agent may have the formula:

[0015] R n S X 4-n

[0016] Where R is C2-C 10 Alkyl or substituted alkyl substituents. X can be any suitable leaving group that is easily replaced by water to form a hydroxyl intermediate, which then reacts with other Sn-X functional groups to produce Sn-O-Sn crosslinks. In various embodiments, R is branched, has multiple β-hydrogen atoms (the maximum number corresponds to the tert-butyl substituent). For example, R can be tert-butyl, tert-pentyl, tert-hexyl, cyclohexyl, isopropyl, isobutyl, sec-butyl, n-butyl, n-pentyl, or n-hexyl or derivatives thereof, and similar materials containing one or more heteroatoms (e.g., fluorine, chlorine, bromine, iodine, nitrogen, and oxygen).

[0017] The present technology also provides methods for forming patterns on the surface of a coated substrate using EUV or other radiation, the coated substrate being produced by the methods of the present technology. Further processing of the coated substrate can take advantage of the chemical differences between exposed and unexposed areas, especially in the exposed areas of the imaging layer, to cause the hydrocarbon-terminated SnO x Transformed into hydrogen-terminated SnO x The difference in properties between exposed and unexposed areas can be exploited in subsequent processing, such as by reacting the irradiated areas, the unirradiated areas, or both with one or more reagents to selectively add material to or remove material from the imaging layer.

[0018] In various embodiments, the present technology provides a method of patterning a thin etch-resistant hard mask layer on a surface of a substrate, comprising:

[0019] providing a substrate comprising a substrate material having a surface comprising exposed hydroxyl groups;

[0020] An imaging layer is deposited on the surface, the imaging layer comprising a hydrocarbon-terminated SnO x ;

[0021] The imaging layer is selectively irradiated so that the imaging layer comprises an irradiated area and a non-irradiated area, wherein the SnO x The hydrocarbyl substituents on some of the SnO x , and in the non-irradiated areas, the imaging layer comprises the hydrocarbon-terminated SnO x ;as well as

[0022] The imaging layer is treated by reacting the irradiated areas, the non-irradiated areas, or both with one or more reagents to selectively add materials to or remove materials from the imaging layer.

[0023] The irradiation may include the use of DUV, EUV, X-ray or electron beam radiation. In some embodiments, the treatment further includes oxidizing the hydrogen terminated (Sn—H) functional groups in the irradiated areas to form Sn—OH hydroxyl terminated SnO x .

[0024] Further scope of applicability of the present technology will become apparent from the detailed description, claims and drawings.The detailed description and specific examples are intended for purposes of illustration only and are not intended to limit the scope of the present technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present technology will be fully understood from the detailed description and accompanying drawings, in which:

[0026] Figure 1 is a flow chart of an exemplary process of the present technology.

[0027] Figure 2 is a diagram depicting the overall architecture of a substrate as it is formed in an exemplary process of the present technology.

[0028] Figure 3 Detailed description of the overall structure of another substrate when it is formed in an exemplary process of the present technology.

[0029] Figure 4 Detailed description is given of the overall structure of another substrate when it is formed in an exemplary process of the present technology.

[0030] Figure 5 FIG. 1 is a flow chart of an exemplary negative tone resist process of the present technology.

[0031] Figure 6 The mask is schematically depicted when it is in Figure 5 The overall structure when being formed in a negative photoresist process.

[0032] Fig. 7A -B is a mask depicting the chemical structure of the sample when it is Figure 5 The overall structure when being formed in a negative photoresist process.

[0033] Figure 8 is a flow chart of an alternative exemplary negative photoresist process of the present technology.

[0034] Fig. 9 Depicts the mask when it is in Figure 8 The overall structure when being formed in a negative photoresist process.

[0035] Fig.10 is a flow chart illustrating a process of the present technology for forming a self-assembled sol-gel on a substrate.

[0036] Fig.11 is a flow chart illustrating a process of the present technology for forming a self-assembled block copolymer on a substrate.

[0037] Fig.12 is a flow chart illustrating a process of the present technology for selectively growing a metal device structure on a substrate.

[0038] Fig.13 It is a description of when metal Fig.12 The overall structure of the substrate when it is deposited in the process. DETAILED DESCRIPTION

[0039] Specific embodiments of the present disclosure are described in detail herein. Examples of these specific embodiments are shown in the accompanying drawings. Although the present disclosure will be described together with these specific embodiments, it should be understood that this is not intended to limit the present disclosure to such specific embodiments. On the contrary, this is intended to cover substitutions, modifications, and equivalents that may be included in the spirit and scope of the present disclosure. In the following description, many specific details are proposed in order to provide a thorough understanding of the present disclosure. The present disclosure may be implemented without some or all of these specific details. In other cases, known process operations are not described in detail to avoid making the present disclosure unnecessarily difficult to understand.

[0040] As described above, the present disclosure provides methods for making imaging layers on semiconductor substrates that can be patterned using EUV or other next generation lithography techniques. In addition to EUV (which generally includes the standard 13.5nm EUV wavelength when used and developed), the radiation sources most relevant to this lithography are DUV (deep UV) (which generally involves the use of 248nm or 193nm excimer laser sources), X-rays (which formally include EUV in the lower energy range of the X-ray range), and electron beams (which can cover a wide energy range). This method includes the following method: contacting a substrate having exposed hydroxyl groups with a hydrocarbyl-substituted tin capping agent to form a hydrocarbyl-terminated SnO as an imaging layer on the surface of the substrate. x In various embodiments, the imaging layer is a thin layer that can serve as an adhesion layer on the substrate, such as when forming a hard mask for a photolithography process, to facilitate the selective deposition of additional materials on the substrate. These specific methods may depend on the specific materials and applications used in the semiconductor substrate and the final semiconductor device. Therefore, the methods described in this application are only examples of methods and materials that can be used in the present technology.

[0041] Substrate

[0042] Substrates that can be used in the methods of the present technology may include any material structure suitable for photolithographic processing (particularly suitable for the production of integrated circuits and other semiconductor devices). In some embodiments, the substrate is a silicon wafer. The substrate can be a silicon wafer on which features with irregular surface morphology ("underlying morphological features") have been produced. (As referred to herein, a "surface" is a surface on which a film of the present technology is to be deposited or a surface to be exposed to EUV during processing.) Such underlying morphological features may include areas where material has been removed during processing (e.g., by etching) or areas where material has been added (e.g., by deposition) before performing the methods of the present technology. Such previous processing may include other processing methods in the methods of the present technology or iterative processes (through which features of two or more layers are formed on the substrate).

[0043] In some embodiments, the substrate is a hard mask that is used for photolithographic etching of the underlying semiconductor material. The hard mask may comprise any of a variety of materials including amorphous carbon (aC), SnO x 、SiO2、SiO x N y 、SiO x C, Si3N4, TiO2, TiN, W, W-doped C, WO x , HfO2, ZrO2 and Al2O3. For example, the substrate may preferably contain SnO x, such as SnO 2. In various embodiments, the layer can be from 1 nm to 100 nm thick, or from 2 nm to 10 nm thick.

[0044] In various embodiments, the substrate comprises exposed hydroxyl groups on its surface. In general, the surface may be any surface comprising exposed hydroxyl groups or being treated to produce exposed hydroxyl groups. (As referred to herein, "surface" refers to a portion of a substrate that defines a boundary between a substrate and another material (or lack of another material (e.g., a gas, a coating, or a vacuum)), and in various embodiments, can be used to be exposed to radiation or react with components in other materials.) Therefore, the method may include "providing" such a substrate, wherein, in addition to the method of the present technology, as mentioned above and further described below, a substrate with exposed hydroxyl groups is obtained as a starting material, or is produced as part of a single process (the process includes forming hydroxyl groups on a substrate and then contacting the surface with a hydroxy-substituted tin capping agent). For example, such hydroxyl groups can be formed on the surface of a substrate by treating the substrate surface using oxygen plasma, water plasma, or ozone.

[0045] In some embodiments, the substrate comprising exposed hydroxyl groups comprises: a surface layer or film comprising hydroxyl-terminated SnO x For example, the substrate may include SnO with hydroxyl terminated x Without limiting the mechanism, function or utility of the present technology, it is believed that the hydroxyl-terminated SnO x The SnO layer may provide benefits such as improved adhesion of materials deposited on the surface of the substrate and enhanced absorption of EUV (or other radiation) during patterning. Sensitivity and resolution to EUV or other radiation may depend on the SnO x The properties of the layer, such as thickness, density, and short-range charge transfer characteristics. In various embodiments, SnO x The layer has a thickness of from 0.1 nm to 20 nm, or from 0.2 nm to 10 nm, or from 0.5 nm to 5 nm.

[0046] In some embodiments, hydroxyl terminated SnO is deposited on the surface of the substrate by a vapor deposition process. x In this method, the deposition process includes making Sn-X nReacting with an oxygen-containing counter-reactant, wherein X is a ligand, such as a dialkylamide (e.g., dimethylamide, methylethylamide, and diethylamide), an alcohol (e.g., tert-butoxy and isopropoxy), a halogen (e.g., F, Cl, Br, and I), or other organic substituents (e.g., acetylacetone, N2,N3-di-tert-butyl-butane-2,3-diamide). For example, Sn-X n It can be SnCl4, SnI4, or Sn(NR2)4 (wherein R is =methyl or ethyl), or Sn(t-BuO)4. In some embodiments, there are multiple types of ligands. The oxygen-containing relative reactant can be selected from the group consisting of water, hydrogen peroxide, formic acid, alcohol, oxygen, ozone, and combinations thereof.

[0047] Suitable vapor deposition processes include chemical vapor deposition (CVD), atomic layer deposition (ALD), plasma enhanced chemical vapor deposition (PECVD), or plasma enhanced atomic layer deposition (PEALD). In some embodiments, the deposition process is used to deposit Sn-X n In some embodiments, the deposition process is CVD, which is performed by simultaneously flowing Sn-X n With oxygen-containing phase reactants. In this paper, it can be used to deposit SnO x The materials and processes of the layers are described in Nazarov et al., Atomic Layer Deposition of Tin Dioxide Nanofilms: A Review, 40 Rev. Adv. Mater. Sci 262 (2015).

[0048] In an exemplary continuous CVD process, Sn-X n Two or more gas streams with an oxygen-containing reactant source are introduced into a deposition chamber of a CVD apparatus where the gas streams mix and react in the gas phase to form SnO on the substrate. x The streams can be introduced, for example, using a double-gassing nozzle. The apparatus is configured so that the Sn-X n The flow of the reactant source with the oxygen-containing phase is mixed in the chamber to allow Sn-X n Reacts with oxygen-containing reactant sources to form SnO xThe CVD process is generally performed at a reduced pressure, for example, from 0.1 Torr to 10 Torr. In some embodiments, the process is performed at 1-2 Torr. The temperature of the substrate is preferably lower than the temperature of the reactant stream. For example, the substrate temperature can be from 0°C to 250°C, or from ambient temperature (e.g., 23°C) to 150°C.

[0049] SnO x The substrate can also be deposited by ALD process. For example, Sn-X n The reactants are introduced at different times than the oxygen-containing counterparts. For each pulse, these precursors react on the surface, forming a monolayer of material each time. This can provide excellent control over the uniformity of film thickness across the surface. The ALD process is generally performed at a reduced pressure, for example, from 0.1 Torr to 10 Torr. In some embodiments, the process is performed at 1-2 Torr. The substrate temperature can be from 0°C to 250°C, or from ambient temperature (e.g., 23°C) to 150°C. The process can be a thermal process, or preferably a plasma assisted deposition process.

[0050] Tin Capping Agent

[0051] Hydrocarbyl-substituted tin capping agents useful herein include substituents that undergo tin-carbon bond cleavage upon exposure to the imaging layer. Such cleavage may be homolytic. In some embodiments, the cleavage may occur by a β-hydride elimination reaction to release an olefin fragment leaving a hydrogen atom bonded to the tin atom that originally bears an alkyl substituent.

[0052] The specific tin capping agent can be selected based on the desired lithographic process (i.e., the specific radiation to be used). In addition, the hydrocarbyl-substituted tin capping agent can be selected so as to act as a barrier to subsequent material deposition onto the substrate. Thus, in some embodiments, the hydrocarbyl-substituted tin capping agent is an atomic layer deposition blocking agent to prevent attachment or growth of soluble metal oxide precursors from solution in contact with the surface.

[0053] In various embodiments, the hydrocarbyl-substituted tin capping agent is alkyl-substituted, such as an agent having the general formula:

[0054] R n S X m

[0055] Where R is C2-C 10alkyl or substituted alkyl with β-hydrogen, X is a suitable leaving group when reacting with the hydroxyl group in the exposed hydroxyl group, and in various embodiments, n=1-3, and m=4-n. For example, R can be tert-butyl, tert-pentyl, tert-hexyl, cyclohexyl, isopropyl, isobutyl, sec-butyl, n-butyl, n-pentyl, or n-hexyl or a derivative thereof having a heteroatom substituent at the β position. Suitable heteroatoms include halogen (F, Cl, Br, or I), or oxygen (-OH or -OR). X can be a dialkylamide (e.g., dimethylamide, methylethylamide, or diethylamide), an alcohol (e.g., tert-butoxy, isopropoxy), a halogen (e.g., F, Cl, Br, or I), or another organic ligand. Examples of hydrocarbyl-substituted tin capping agents include t-butyltris(dimethylamino)tin, n-butyltris(dimethylamino)tin, t-butyltris(diethylamino)tin, di(t-butyl)di(dimethylamino)tin, sec-butyltris(dimethylamino)tin, n-pentyltris(dimethylamino)tin, tin), t-butyltris(t-butoxy)tin, n-butyl(tris(t-butoxy)tin or isopropyltris(t-butoxy)tin.

[0056] Method for making imaging layer

[0057] In various aspects, the methods of the present technology include:

[0058] providing a substrate having a surface, wherein the surface comprises exposed hydroxyl groups; and

[0059] The surface is contacted with a hydrocarbyl-substituted tin capping agent to form a hydrocarbyl-terminated SnO on the surface of the substrate. x film as an imaging layer.

[0060] In general, contacting the surface with the hydrocarbyl-substituted tin capping agent can be performed using any suitable technique, preferably to produce a uniform distribution of the capping agent on the surface. Such methods include vapor deposition techniques such as ALD and CVD. Water can also be dosed to promote the reaction of the capping agent with the exposed hydroxyl groups of the substrate. Such methods can use repeated applications of the capping agent and water to form a surface that is fully covered with hydrocarbyl-substituted tin capping functional groups. Exposure to additional alky-based reagents (e.g., alkylthiols) can be used to form a surface with an increased number of hydrocarbyl substituents on the surface of the substrate.

[0061] In an exemplary continuous CVD process, R n Sn-X m Two or more gas streams with an oxygen-containing reactant source are introduced into the deposition chamber of the CVD apparatus, where the gas streams mix, react in the gas phase, and condense on the substrate to form SnO x The equipment is set up so that RnSn-X m The flow of the reactant source with the oxygen-containing phase is mixed in the chamber to allow R n Sn-X m Reacts with oxygen-containing reactant sources to form SnO x The CVD process is generally performed at a reduced pressure, for example, from 0.1 Torr to 10 Torr. In some embodiments, the process is performed at 1-2 Torr. The temperature of the substrate is preferably lower than the temperature of the reactant stream. For example, the substrate temperature may be from 0°C to 250°C, or from ambient temperature (e.g., 23°C) to 150°C.

[0062] SnO x The imaging layer can also be deposited by an ALD process. In this case, R n Sn-X m The reactants are introduced at different times than the oxygen-containing counterparts, which represents an ALD cycle. For each ALD cycle, the precursors react on the surface, forming a monolayer of material each time. This can provide excellent control over the uniformity of film thickness across the wafer. The ALD process is generally performed at a reduced pressure, for example, from 0.1 Torr to 10 Torr. In some embodiments, the process is performed at 1-2 Torr. The substrate temperature can be from 0°C to 250°C, or from ambient temperature (e.g., 23°C) to 150°C. The process will be a thermally driven process. The film is not expected to grow significantly after the first cycle, and subsequent cycles are designed to further fill the surface with R-terminated Sn.

[0063] Patterning

[0064] The present technology also provides methods in which the imaging layer is patterned by exposing areas of the imaging layer to radiation (e.g., EUV, DUV, or electron beam). In such patterning, the radiation is concentrated in one or more areas of the imaging layer. Generally, the exposure is performed so that the imaging layer film includes one or more areas that are not exposed to the radiation. The resulting imaging layer may include multiple exposed or unexposed areas to produce a pattern consistent with the production of transistors or other features of semiconductor devices, which is formed by adding materials or removing materials from the substrate in subsequent processing of the substrate. EUV, DUV, and electron beam radiation methods and apparatus that can be used herein include methods and apparatus that are well known in the art.

[0065] In particular, patterning is used to create regions of the imaging layer that have altered physical or chemical properties relative to unexposed regions. In particular, in various embodiments, particularly when exposure is performed using EUV in a vacuum, hydrocarbon-terminated SnO present on the surface is modified in the exposed regions of the imaging layer. x Transformed into hydrogen-terminated SnO x However, moving the exposed imaging layer from a vacuum to air, or the controlled introduction of oxygen, ozone, H2O2, or water, can result in oxidation of the surface Sn-H to Sn-OH. The difference in properties between the exposed and unexposed areas can be exploited in subsequent processing, such as by reacting the irradiated areas, the unirradiated areas, or both with one or more reagents to selectively add materials to or remove materials from the imaging layer.

[0066] Thus, in various embodiments, the present technology provides a method of making a photolithographic hard mask on a surface of a substrate, comprising:

[0067] providing a substrate comprising a substrate material having a surface comprising exposed hydroxyl groups;

[0068] An imaging layer is deposited on the surface, the imaging layer comprising a hydrocarbon-terminated SnO x ;

[0069] The imaging layer is selectively irradiated so that the imaging layer comprises an irradiated area and a non-irradiated area, wherein the hydrocarbon-terminated SnO x Has been converted into hydrogen-terminated SnO x , and in the non-irradiated areas, the imaging layer comprises the hydrocarbon-terminated SnO x ; and treating the imaging layer by reacting the irradiated areas, the non-irradiated areas, or both with one or more reagents to selectively add materials to or remove materials from the imaging layer.

[0070] In various embodiments, the substrate material comprises amorphous carbon or SnO x .

[0071] Optionally, the imaging layer is heated or "baked" to remove excess moisture and drive the Sn-O-Sn crosslinking reaction. For example, the sample can be baked under conditions (e.g., between 50°C and 200°C for 5 minutes, or between 70°C and 150°C for 2 minutes) such that the R-Sn bonds will not be significantly cleaved.

[0072] Photolithography

[0073] As described above, after irradiation, subsequent processing of the imaging layer will depend on the substrate material and the desired features of the semiconductor device fabricated using the substrate. For example, features can be produced on the substrate by various photolithographic techniques such as using spin coating of films that become selectively soluble in a liquid developer in exposed (positive tone) or unexposed (negative tone) areas defined by a patterned exposure tool.

[0074] The photolithography method of this technology is roughly described in Figure 1 As shown in the figure, by depositing hydroxyl-terminated SnO on the substrate material x The "underlayer" is formed to form a substrate (110). The hydroxyl-terminated SnO x The underlayer can enhance the absorption of radiation when irradiating the imaging layer and generate secondary electrons from the substrate to further obtain additional EUV photons to make the EUV patterning process more sensitive and reduce the required EUV dose required for imaging layer exposure.

[0075] Next, an imaging layer is formed by depositing a hydrocarbyl-substituted tin capping agent on the surface to form a hydrocarbyl-capped SnO x The substrate is then exposed to radiation (eg, using EUV) (130), and optionally, baked (140). The imaging layer surface is then processed (150). Figure 2 The overall architecture of the substrate as it is formed in this process is depicted schematically and with sample chemical structures. Figure 3 A specific example of this process is depicted in Figure 1, where the imaging layer is formed from a hydrocarbyl-substituted tin capping agent (tert-butyl Sn(N(CH3)2)3). Figure 4 An alternative scheme is depicted for an active (EUV-releasing) PR adhesion imaging layer formed by a tin capping agent, which is n-BuSn(OtBu)3.

[0076] In some methods, the treatment comprises causing the hydrogen terminated SnO xOxidation to form hydroxyl-terminated SnO x The oxidation may include exposing the irradiated area to oxygen or water. In some methods, the subsequent treatment includes removing the hydroxyl-terminated SnO x , to expose and etch the underlying substrate material. The etching may be performed by treating the patterned film with a dilute aqueous hydrofluoric acid solution or a dilute aqueous tetramethylammonium hydroxide (TMAH) solution. The treatment may also include etching of the underlying substrate layer using an oxygen plasma.

[0077] In some embodiments, the treatment further comprises hydroxyl terminated SnO x A metal oxide is deposited on the substrate, which can be used as a hard mask. The hard mask material may include a material selected from SnO2, SiO2, TiO2, WO x , HfO 2 , ZrO 2 , Ta 2 O 5 , Nb 2 O 5 , B 2 O 3 , GeO 2 , ZnO, V 2 O 5 , and Al 2 O 3. The deposition may be performed, for example, by ALD.

[0078] In some methods of the present technology, the hydrocarbon-terminated SnO is removed from the unirradiated areas by hydrogen or methane plasma. x , to expose the underlying amorphous carbon layer. The processing may also include etching of the underlying substrate material using an oxygen plasma.

[0079] Without limiting the mechanism, functionality, or utility of the present technology, it is believed that in some embodiments, the lithography methods of the present technology provide benefits over methods known in the art, such as avoiding the need to apply and remove wet photoresist formulations (e.g., avoiding scumming and pattern deformation), simplifying processes such as developing exposed substrates under vacuum in a continuous process after EUV or other radiation, reducing pattern collapse through the use of very thin metal oxide structures, improving line edge roughness, and providing the ability to tune hard mask chemistry to specific substrates and semiconductor device designs.

[0080] Additional Implementations

[0081] As described above, specific post-imaging methods and applications of the present technology may include any of a wide variety of materials and processes depending on the substrate and the desired device design. The processing of the imaging layer may depend on the substrate material and the desired features of the semiconductor device to be fabricated using the substrate. For example, features may be produced on the substrate by various standard photolithographic techniques (generally involving the coating of films that become selectively soluble in a developer in exposed (positive) or unexposed (negative) areas defined by a patterned exposure tool). Processing may also include the preparation of photolithographic masks comprising directed self-assembly (DSA) of block co-polymers (BCPs), directed self-assembly of sol-gels, and selective deposition of materials (e.g., metals or metal oxides) by atomic layer deposition or chemical vapor deposition.

[0082] For example, in some embodiments, the processing of the imaging layer and the substrate is to produce a positive mask. Such a method may include:

[0083] selectively irradiating areas of an imaging layer of a substrate fabricated by the methods of the present technology;

[0084] Oxidation of hydrogen-terminated SnO in the irradiated area x , to form hydroxyl-terminated SnO x , for example by reacting the irradiated area with air or water;

[0085] contacting the irradiated area with a dilute aqueous hydrofluoric acid (HF) solution or a dilute aqueous tetramethylammonium hydroxide (TMAH) solution to etch the exposed hydroxyl terminated surface to expose the underlying substrate material (e.g., amorphous carbon); and

[0086] The bottom layer is exposed by etching with oxygen plasma.

[0087] In some embodiments, the processing of the imaging layer and the substrate is to produce a negative photoresist. For example, such a method may include:

[0088] selectively irradiating areas of an imaging layer of a substrate fabricated by the methods of the present technology;

[0089] Oxidation of hydrogen-terminated SnO in the irradiated area x , to form hydroxyl-terminated SnO x , for example by reacting the irradiated area with air or water;

[0090] A metal oxide hard mask is selectively deposited on the hydroxyl terminated regions, for example by ALD;

[0091] For example, H2, CH4, or BCl3 based plasma is used to remove the unexposed areas of the substrate (i.e., the SnO with hydrocarbon-terminated x) to expose an underlying substrate (e.g., amorphous carbon); and

[0092] The underlying substrate is exposed by etching with oxygen plasma.

[0093] The elements of one such process are described in Figure 5 in the manufacturing process. Figure 6 ,as well as Fig. 7A -B depicts the overall architecture of the mask as it is formed in one such negative photoresist process (starting with a hydroxylation reaction of the exposed surface) in a schematic manner and with a sample chemical structure, respectively.

[0094] The elements of the alternative negative photoresist process are described in Figure 8 In this process, the hydrogen-terminated SnO x Instead, a metal or metal oxide hard mask is deposited, for example by ALD, on the Sn-H surface of the irradiated area. General methods and conditions for ALD deposition of metals on hydride surfaces are described in Kwon, et.al., Substrate Selectivity of ( t Bu-Allyl)Co(CO)3during Thermal AtomicLayer Deposition of Cobalt,24Chem.Mater.1025(2012),and Lemaire,et.al.,Understanding inherent substrate selectivity during atomic layer deposition:Effect of surface preparation,hydroxyl density,and metal oxide composition onnucleation mechanisms during tungsten ALD,146J.Chem.Phys.052811(2017). In this process, from irradiation to ALD deposition, the substrate can be maintained under vacuum to simplify the material handling procedures during the process and potentially provide manufacturing efficiency. Fig. 9 Depicted is the general architecture of a mask as it is formed in an alternative negative photoresist process.

[0095] In some embodiments, processing of the imaging layer and substrate is performed using negative tone patterning.

[0096] For example, such a method could contain:

[0097] selectively irradiating areas of an imaging layer of a substrate fabricated by the methods of the present technology;

[0098] Oxidation of hydrogen-terminated SnO in the irradiated area x , to form hydroxyl-terminated SnO x , for example by reacting the irradiated area with air or water;

[0099] selectively depositing a solution of a metal sol-gel oxide (e.g., spin coating tetraethyl orthosilicate with nitric acid at pH 2) on the hydroxyl terminated regions to form a metal oxide etch mask on the irradiated regions;

[0100] removing (e.g., by rinsing) unreacted sol-gel solution;

[0101] For example, hydrogen or methane plasma is used to remove the unexposed areas of the substrate (i.e., the SnO x ) to expose an underlying substrate (e.g., amorphous carbon); and

[0102] The underlying substrate is exposed by etching with oxygen plasma.

[0103] Materials and methods for making sol-gels are described in Hench, et al., The Sol-Gel Process, 90 Chem. Rev. 33 (1990), and Lu, et al., Continuous formation of supported cubic and hexagonal mesoporous films by sol-gel dip-coating, 389 Nature 364 (1997). The elements of this process are described in Fig.10 in the manufacturing process.

[0104] In some embodiments, the processing of the imaging layer and substrate comprises the deposition and self-assembly of block copolymers to pattern the hydrophilic and hydrophobic regions of the imaging surface to produce a hard mask. For example, such a method for producing a hard mask may comprise:

[0105] selectively irradiating areas of an imaging layer of a substrate fabricated by the methods of the present technology;

[0106] Oxidation of hydrogen-terminated SnO in the irradiated area x , to form hydroxyl-terminated SnO x , for example by reacting the irradiated area with air or water;

[0107] coating the surface with a block copolymer reactant;

[0108] annealing the surface to produce assembled block copolymers;

[0109] selectively removing substituents of the block copolymer to form a mask; and

[0110] The bottom layer is exposed by etching with oxygen plasma.

[0111] In some embodiments, a hydrophilic metal oxide may be deposited on the hydrophilic areas of the imaging surface (i.e., the irradiated areas) prior to coating with the block copolymer reactants to create a topography that directs the self-assembly of the block copolymers. Materials and methods for making self-assembling block copolymers are described in Hamley, Nanostructure fabrication using block copolymers, 14 Nanotechnology R39 (2003). The elements of this process are described in Fig.11 This approach can reduce the size of features and potentially reduce the defects associated with BCP self-assembly.

[0112] The present technology also provides methods for selectively growing electroless metal device structures, such as for hard masks, on substrates. For example, the surface can be exposed to oxidizing metal ions (such as Pd +2 In other embodiments, the exposed "deprotected" areas of the thin tin-based imaging layer (which are no longer hydrophobic) can be selectively etched away by brief exposure to an aqueous acid etchant (e.g., concentrated HF or oxalic acid solution).

[0113] For example, such a method contains:

[0114] selectively irradiating areas of an imaging layer of a substrate fabricated by the methods of the present technology;

[0115] selectively depositing a palladium (Pd) activation layer on the exposed regions of the substrate (i.e., regions having Sn—H surface portions); and

[0116] A metal (eg, cobalt) is deposited on the Pd activation layer by electroless deposition.

[0117] In various embodiments, the deposited metal is a late transition metal such as cobalt, nickel, copper, or mixtures thereof. Without limiting the mechanism, function, or utility of the present technology, it is believed that in some embodiments, this method can provide a simple additive patterning method for depositing metal features on substrates where only such features are desired, compared to subtractive techniques known in the art (which involve blanket deposition of metal followed by patterned removal). The elements of this process are depicted in Fig.12 in the manufacturing process and is shown in Fig.13 middle.

[0118] in conclusion

[0119] Methods are provided for making imaging layers on the surface of substrates that can be patterned into chemically distinct regions (ie, surface imaging) using next generation photolithography techniques. The resulting patterned films can be used, for example, as photolithographic masks for semiconductor device production.

[0120] It should be understood that the examples and embodiments described herein are for illustrative purposes only, and those skilled in the art will associate various modifications or variations based on these examples and embodiments. Although various details have been omitted for the purpose of clarity, various design alternatives can be implemented. Therefore, the present examples will be regarded as illustrative rather than restrictive, and the present disclosure will not be limited to the details set forth herein, but may be modified within the scope of the present disclosure and the appended claims.

Claims

1. A method for producing an imaging layer on a substrate, the method comprising: providing a substrate having a surface comprising exposed hydroxyl groups; and Forming a hydrocarbon-terminated SnO x The film is used as an imaging layer, and the hydrocarbon-terminated SnO x The film has tin-carbon bonds that can be cleaved by irradiating the imaging layer.

2. The method according to claim 1, wherein the hydrocarbon-terminated SnO x The film comprises contacting said surface of said substrate with a hydrocarbyl-substituted tin capping agent that undergoes tin-carbon bond cleavage upon said irradiation of said imaging layer.

3. The method of claim 2, wherein the hydrocarbyl-substituted tin capping agent acts as a blocking agent to prevent attachment or growth of soluble metal oxide precursors from a solution in contact with the surface.

4. The method of claim 2 or 3, wherein the hydrocarbyl-substituted tin capping agent has the formula: R n S X 4-n in, R is C2-C 10 alkyl or a substituted alkyl containing β-hydrogen, X is a leaving group upon reaction with the hydroxyl group of the exposed hydroxyl group, and n=1-3.

5. The method according to claim 4, wherein R is selected from the group consisting of tert-butyl, tert-pentyl, tert-hexyl, cyclohexyl, isopropyl, isobutyl, sec-butyl, n-butyl, n-pentyl, n-hexyl, and derivatives thereof having a heteroatom substituent at the β position.

6. The method of claim 4, wherein X is selected from the group consisting of dialkylamide, alcohol, and halogen.

7. The method of claim 2, wherein the hydrocarbyl-substituted tin capping agent is selected from the group consisting of tert-butyl tris(dimethylamino)tin, n-butyl tris(dimethylamino)tin, tert-butyl tris(diethylamino)tin, di(tert-butyl)di(dimethylamino)tin, sec-butyl tris(dimethylamino)tin, n-pentyl tris(dimethylamino)tin, isobutyl tris(dimethylamino)tin, isopropyl tris(dimethylamino)tin, tert-butyl tris(tert-butoxy)tin, n-butyl tris(tert-butoxy)tin, and isopropyl tris(tert-butoxy)tin.

8. The method according to any one of claims 1 to 3, wherein the substrate comprises amorphous carbon (aC), SnO x 、SiO2、SiO x N y 、SiO x C, Si3N4, TiO2, TiN, W, W-doped C, WO x、HfO2, ZrO2, Al2O3 or Bi2O3.

9. The method according to any one of claims 1 to 3, wherein the providing comprises forming a hydroxyl-terminated SnO x layer.

10. The method of claim 9, wherein the forming comprises depositing hydroxyl terminated SnO on the surface by vapor deposition. x layer.

11. The method of claim 10, wherein the deposited n Reaction with an oxygen-containing reactant wherein X is a dialkylamide, an alcohol, or a halogen.

12. The method according to claim 11, wherein Sn-X n It is SnCl4, SnI4 or Sn(NR2)4, wherein R is methyl or ethyl, or Sn(t-BuO)4.

13. The method of claim 11, wherein the oxygen-containing phase reactant is selected from the group consisting of water, hydrogen peroxide, formic acid, alcohol, oxygen, ozone, oxygen plasma, water plasma, and combinations thereof.

14. The method of claim 10, wherein the vapor deposition is chemical vapor deposition (CVD), atomic layer deposition (ALD), plasma enhanced chemical vapor deposition (PECVD), or plasma enhanced atomic layer deposition (PEALD).

15. The method according to claim 11, wherein the depositing is depositing the Sn-X n and an ALD cycle process for depositing the oxygen-containing phase reactant.

16. The method of claim 11, wherein the depositing comprises simultaneously depositing the Sn-X n A CVD process with said oxygen-containing phase reactants.

17. The method of any one of claims 1-3, wherein the imaging layer has a thickness of from 0.5 nm to 5 nm.

18. The method of any one of claims 1-3, wherein the substrate comprises underlying topographical features.

19. The method of any one of claims 1 to 3, further comprising irradiating the imaging layer to form at least one exposed region, wherein in the exposed region, the hydrocarbon-terminated SnO x Transformed into hydrogen-terminated SnO x .

20. The method of claim 19, wherein the irradiating comprises the use of DUV, EUV, X-ray or electron beam radiation.

21. The method of claim 19, wherein the hydroxyl-terminated SnO x The layer enhances the absorption of radiation when the imaging layer is irradiated.

22. The method of claim 1, wherein the irradiating comprises use of EUV radiation.

23. The method of claim 6, wherein X is selected from the group consisting of dimethylamide, methylethylamide, diethylamide, tert-butoxy, isopropoxy, F, Cl, Br, and I.

24. The method of claim 11, wherein X is selected from the group consisting of dimethylamide, methylethylamide, diethylamide, tert-butoxy, isopropoxy, F, Cl, Br, and I.

25. A method for making a photolithography hard mask on a surface of a substrate, comprising: providing a substrate comprising a substrate material having a surface comprising exposed hydroxyl groups; An imaging layer is deposited on the surface, the imaging layer comprising a hydrocarbon-terminated SnO x ; The imaging layer is selectively irradiated so that the imaging layer includes an irradiated area and a non-irradiated area, wherein the SnO x The hydrocarbyl substituents on some of the SnO x , and in the non-irradiated areas, the imaging layer comprises the hydrocarbon-terminated SnO x ;as well as The imaging layer is treated by reacting the irradiated areas, the non-irradiated areas, or both with one or more reagents to selectively add materials to or remove materials from the imaging layer.

26. The method of claim 25, wherein the providing comprises: depositing hydroxyl-terminated SnO on the surface of the substrate material by vapor deposition. x layer.

27. The method of claim 25, wherein depositing the imaging layer comprises contacting the surface of the substrate with a hydrocarbyl-substituted tin capping agent that undergoes tin-carbon bond cleavage upon the selective irradiation of the imaging layer.

28. The method of claim 27, wherein the hydrocarbyl-substituted tin capping agent has the formula: R n S X 4-n in, R is C2-C 10 alkyl or substituted alkyl having β-hydrogen, X is a suitable leaving group upon reaction with the hydroxyl group of the exposed hydroxyl group, and n=1-3.

29. The method of claim 28, wherein the hydrocarbyl-substituted tin capping agent is tert-butyl tris(dimethylamino)tin, n-butyl tris(dimethylamino)tin, tert-butyl tris(diethylamino)tin, isopropyl tris(dimethylamino)tin, tert-butyl tris(tert-butoxy)tin, and n-butyl tris(tert-butoxy)tin.

30. The method of any one of claims 25-29, wherein the selective irradiation comprises the use of DUV, EUV, X-ray or electron beam radiation.

31. The method of claim 30, wherein the irradiating comprises the use of EUV radiation.

32. The method of claim 25, wherein the SnO x The hydrocarbyl substituents on the SnO moiety are converted to hydrogen-terminated SnO by β-hydride elimination reaction. x .

33. The method of any one of claims 25-29, wherein the treating comprises causing the hydrogen terminated SnO x Oxidation to form hydroxyl-terminated SnO x .

34. The method of claim 33, wherein the oxidizing comprises exposing the irradiated area to oxygen or water.

35. The method of claim 33, wherein the treating comprises removing the hydroxyl terminated SnO in the irradiated area. x , to expose an underlying substrate material, and wherein the underlying substrate material comprises amorphous carbon.

36. The method of claim 35, wherein the removing comprises treating the irradiated area with dilute hydrofluoric acid or dilute aqueous tetramethylammonium hydroxide (TMAH).

37. The method of claim 35, wherein the processing further comprises etching the underlying substrate material using an oxygen plasma.

38. The method of claim 33, wherein the treating further comprises treating the hydroxyl terminated SnO x A metal oxide hard mask is deposited thereon.

39. The method of claim 38, wherein the metal oxide hard mask comprises a metal oxide selected from the group consisting of SnO x 、SiO2、SiO x N y 、SiO x C, TiO2, WO x、 A group consisting of HfO2, ZrO2, Al2O3 and Bi2O3.

40. The method of claim 25, further comprising treating only the hydrogen terminated SnO x Atomic layer deposition is used to selectively deposit metal layers on the surface of the substrate.

41. The method of claim 25, wherein the hydrocarbyl-terminated SnO x , to expose an underlying substrate material, and wherein the underlying substrate material comprises amorphous carbon.

42. The method of claim 41, wherein the processing further comprises etching the underlying substrate material using an oxygen plasma.

Citation Information

Patent Citations

  • Method for manufacturing mask, method for manufacturing wiring pattern, and method for manufacturing plasma display

    CN101098575A

  • Vacuum-integrated hardmask processes and apparatus

    CN105047541A

  • Patterning Process of a Semiconductor Structure with a Middle Layer

    CN106558477A

  • EUV photopatterning of vapor-deposited metal oxide-containing hardmasks

    US20170146909A1

  • Process for obtaining semiconductor nanodevices with patterned metal-oxide thin films deposited onto a substrate, and semiconductor nanodevices thereof

    US20180294155A1