Sensor device, sensor package and method of forming the same

By forming a sacrificial layer on the sensor die and removing it using an etching process, combined with the redistribution structure of conductive vias and dielectric layers, the problem of difficulty in miniaturization and high-density integration with traditional packaging technology is solved, and high mechanical reliability is achieved. and manufacturing efficiency of sensor packaging.

CN113140535BActive Publication Date: 2024-10-15TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011344978.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-05-04
Filing Date
2020-11-26
Publication Date
2024-10-15
Estimated Expiration
2040-11-26

AI Technical Summary

Technical Problem

Existing semiconductor packaging technology is difficult to achieve smaller and more creative packaging systems, especially with the demand for increased integration density and shrinking electronic devices. Traditional packaging methods are difficult to meet the requirements for higher mechanical reliability and manufacturing yield.

Method used

Using the method of combining the sacrificial layer and the redistribution structure, the sacrificial layer is removed through dry etching or wet etching process to form conductive vias and dielectric layers to achieve redistribution and sealing of the sensor die, and then build an integrated fan-out (InFO) package system, exposing the sensor area to improve sensing sensitivity and response speed.

Benefits of technology

A smaller size sensor package is achieved, improving mechanical reliability and manufacturing yield, increasing sensitivity and response speed of the sensor area, while reducing manufacturing cost and total processing time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113140535B_ABST
    Figure CN113140535B_ABST
Patent Text Reader

Abstract

The device includes: a sensor die having a sensing area at a top surface of the sensor die; an encapsulant that at least laterally encapsulates the sensor die; a conductive via that passes through the encapsulant; and a front-side redistribution structure that is located on the encapsulant and on the top surface of the sensor die, wherein the front-side redistribution structure is connected to the conductive via and the sensor die, wherein an opening in the front-side redistribution structure exposes the sensing area of ​​the sensor die, and wherein the front-side redistribution structure includes: a first dielectric layer that extends over the encapsulant and the top surface of the sensor die; a metallization pattern that is located on the first dielectric layer; and a second dielectric layer that extends over the metallization pattern and the first dielectric layer. Embodiments of the application also relate to sensor devices, sensor packages, and methods of forming the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present application relate to sensor devices, sensor packages, and methods of forming the same. Background Art

[0002] The semiconductor industry has experienced rapid growth due to the increasing integration density of individual electronic components (e.g., transistors, diodes, resistors, capacitors, etc.). In most cases, iterative reductions in minimum component size can increase integration density, thereby allowing more components to be integrated into a given area. As the demand for shrinking electronic devices grows, there has been a demand for smaller and more creative semiconductor die packaging technologies. An example of such a packaging system is the Integrated Fan-Out (InFO) technology. Summary of the invention

[0003] Some embodiments of the present application provide a sensor device, comprising: a sensor die having a sensing area located at a top surface of the sensor die; an encapsulant that at least laterally seals the sensor die; a conductive via that extends through the encapsulant; and a front-side redistribution structure located on the encapsulant and on the top surface of the sensor die, wherein the front-side redistribution structure is connected to the conductive via and the sensor die, wherein an opening located in the front-side redistribution structure exposes the sensing area of ​​the sensor die, and wherein the front-side redistribution structure comprises: a first dielectric layer extending above the encapsulant and the top surface of the sensor die, a metallization pattern located on the first dielectric layer, and a second dielectric layer extending above the metallization pattern and the first dielectric layer.

[0004] Other embodiments of the present application provide a sensor package, comprising: a semiconductor die, comprising a contact pad located on the top surface of the semiconductor die and a sensing area located on the top surface of the semiconductor die; an encapsulant surrounding the semiconductor die, wherein the top surface of the semiconductor die is free of the encapsulant; a conductive via extending through the encapsulant, the conductive via being separated from the semiconductor die by the encapsulant; a first dielectric layer extending above the top surface of the encapsulant, along the sidewalls of the encapsulant, and above the top surface of the semiconductor die, wherein the first dielectric layer has a first opening exposing the sensing area of ​​the semiconductor die; a conductive layer located above the top surface of the first dielectric layer, the conductive layer extending through the first dielectric layer to contact the conductive via, and extending through the first dielectric layer to contact the contact pad; and a second dielectric layer located above the conductive layer, wherein the second dielectric layer has a second opening exposing the sensing area of ​​the semiconductor die through the first opening in the first dielectric layer.

[0005] Still other embodiments of the present application provide a method for forming a sensor package, comprising: forming a sacrificial layer on a semiconductor die, the semiconductor die including a sensor; forming a conductive via on the first redistribution structure; placing the semiconductor die on the first redistribution structure adjacent to the conductive via; sealing the semiconductor die, the sacrificial layer and the conductive via with a sealant; planarizing the sealant to expose the conductive via and the sacrificial layer; removing the sacrificial layer using an etching process; and forming a second redistribution structure above the sealant and above the semiconductor die, wherein the second redistribution structure is electrically connected to the conductive via and to the semiconductor die, and wherein the second redistribution structure includes an opening that exposes the sensor of the semiconductor die. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] When read in conjunction with the accompanying drawings, various aspects of the present invention can be best understood from the following detailed description. It should be noted that, in accordance with standard practice in the industry, the various components are not drawn to scale. In fact, for clarity of discussion, the size of the various components may be arbitrarily increased or reduced.

[0007] Figures 1 to 4 Cross-sectional views of intermediate steps during a process for forming a sensor die having a sacrificial layer are shown in accordance with some embodiments.

[0008] Figures 5 to 18 Cross-sectional views are shown of intermediate steps during a process for forming a sensor package using a dry etching process, according to some embodiments.

[0009] Fig.19 Cross-sectional views of intermediate steps during a process for forming a sensor device are shown in accordance with some embodiments.

[0010] Figures 20 to 27 Cross-sectional views are shown of intermediate steps during a process for forming a sensor package using a wet etching process, according to some embodiments.

[0011] Fig.28 Cross-sectional views of intermediate steps during a process for forming a sensor device are shown in accordance with some embodiments. DETAILED DESCRIPTION

[0012] The following disclosure provides many different embodiments or examples for implementing different features of the present invention. Specific examples of components and arrangements are described below to simplify the present invention. Of course, these are merely examples and are not intended to limit the present invention. For example, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly in contact with each other, and may also include an embodiment in which an additional component may be formed between the first component and the second component so that the first component and the second component may not be in direct contact. In addition, the present invention may repeat reference numerals and / or characters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.

[0013] Furthermore, for ease of description, spatially relative terms such as "below," "beneath," "lower," "above," "upper," etc. may be used herein to describe the relationship of one element or component to another (or additional) elements or components as shown in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein should likewise be interpreted accordingly.

[0014] In accordance with some embodiments, a sacrificial layer is formed over the sensor die before packaging the sensor die as part of a sensor package. During the packaging process, the sacrificial layer is removed using a dry etching process or a wet etching process. A redistribution structure can be formed to connect to the sensor die, thereby forming the sensor package into an integrated fan-out (InFO) package. The sensor package may include an opening that exposes a sensing area of ​​the sensor die. Packaging the sensor die in this manner can allow a smaller form factor for the final sensor package, can improve the mechanical reliability of the packaged sensor, and can improve manufacturing yield compared to other (e.g., wire bonding) packaging schemes. The sensing area of ​​the sensor die can also be formed closer to the outside of the sensor package, which can increase the sensitivity and responsiveness of the sensing operation.

[0015] Figures 1 to 4 A cross-sectional view of an intermediate step during a process for forming sensor die 100 having sacrificial layer 112 is shown, according to some embodiments. Figures 5 to 18 Cross-sectional views of intermediate steps during a process for forming the sensor package 200 using a dry etching process are shown in accordance with some embodiments. Fig.19 A sensor device 300 is shown implementing the sensor package 200 according to some embodiments. Figures 20 to 27 Cross-sectional views of intermediate steps during a process for forming a sensor package 400 using a wet etching process are shown in accordance with some embodiments. Fig.28 A sensor device 500 is shown implementing the sensor package 400 according to some embodiments.

[0016] Figures 1 to 4 The formation of sensor die 100 with sacrificial layer 112 is shown in accordance with some embodiments. Figure 1 A plurality of sensor dies 100 are shown prior to singulation. Thus, the sensor dies 100 are formed on a single substrate 102. Figure 1 A single sensor die 100 is shown in FIG. 1 and is separated by scribe line regions 108 .

[0017] The sensor die 100 may be formed in a substrate 102 using an applicable manufacturing process. The substrate 102 may be, for example, a semiconductor substrate such as doped or undoped silicon, and may be an active layer of a silicon wafer or a semiconductor-on-insulator (SOI) substrate, etc. The semiconductor substrate may include other semiconductor materials such as germanium; compound semiconductors including silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, and / or indium antimonide; alloy semiconductors including SiGe, GaAsP, AlInAs, AlGaAs, GaInAs, GaInP, and / or GaInAsP; or combinations thereof. Other substrates may also be used, such as multilayer or gradient substrates. Devices such as transistors, diodes, capacitors, resistors, etc. may be formed in and / or on the active surface of the substrate 102, and may be interconnected by interconnect structures formed by, for example, metallization patterns in one or more dielectric layers on the substrate 102.

[0018] Each sensor die 100 may include one or more sensors, integrated circuits, logic circuits (e.g., central processing units, microcontrollers, etc.), memories (e.g., dynamic random access memory (DRAM), static random access memory (SRAM), etc.), power management circuits (e.g., power management integrated circuits (PMIC)), radio frequency (RF) components, microelectromechanical systems (MEMS) components, signal processing circuits (e.g., digital signal processing (DSP) circuits), front-end circuits (e.g., analog front-end (AFE) circuits), etc., or a combination thereof.

[0019] In some embodiments, each sensor die 100 includes a sensor region 110 in which a sensor is formed. The sensor region 110 may include a portion formed within and / or formed above the substrate 102, and the sensor formed in the sensor region 110 may be physically and / or electrically connected to an integrated circuit, a metallization pattern, a device, etc. of the associated sensor die 100. The sensor region 110 may include an image sensor, an acoustic sensor, a pressure sensor, a temperature sensor, a MEMS sensor, etc. The sensor region 110 may include one or more transducers, and may also include one or more components that transmit signals for measurement during operation. For example, the sensor region 110 may include a fingerprint sensor that operates by transmitting ultrasonic waves and measuring reflected waves.

[0020] Each sensor die 100 also includes a pad 104, such as an aluminum pad, a copper pad, etc., to make an external connection. The pad 104 is located on the active surface of the sensor die 100. One or more passivation films 106 are located on the sensor die and on portions of the pad 104. An opening extends through the passivation film 106 to expose the pad 104. In some embodiments, the opening in the passivation film 106 exposes the sensor area 110. In some embodiments, the opening in the passivation film 106 can have a width W1 between about 5 μm and about 100 μm. In some embodiments, the sensor die 100 is packaged in an InFO package and packaged in a manner that allows the sensor area 110 to be exposed.

[0021] exist Figure 2 In some embodiments, a sacrificial layer 112 is formed over the substrate 102 to cover the sensor die 100. In some embodiments, the sacrificial layer 112 may be cured after being formed over the substrate 102. The sacrificial layer 112 may include, for example, a material that may be subsequently removed by an etching process, such as a wet etching process and / or a dry etching process. In some embodiments, the sacrificial layer 112 includes a material that allows the sacrificial layer 112 to be cured and then subsequently removed using an etching process. In some embodiments, the sacrificial layer 112 includes a material that allows the sacrificial layer 112 to be cured and then subsequently planarized using, for example, a chemical mechanical polishing (CMP) process or a grinding process. The sacrificial layer 112 may include a polymer, such as a polyimide, an epoxy resin, a polyolefin, etc., or a composite material, such as a polymer having one or more additives (e.g., a stress release agent, a plasticizer, etc.) synthesized to adjust one or more material properties of the polymer. The sacrificial layer 112 may be formed by any acceptable deposition process, such as spin coating, lamination, dispensing in liquid form, etc., or a combination thereof. In some embodiments, the sacrificial layer 112 may have a thickness T1 between about 2 μm and about 50 μm over the substrate 102.

[0022] exist Figure 3 and Figure 4 In some embodiments, a singulation process is performed to singulate individual sensor dies 100. The singulation process is performed along the scribe line regions 108 and may include sawing, laser drilling, etc., or a combination thereof. In some embodiments, the singulation process includes forming grooves in the scribe line regions 108 using a laser process, and then performing a sawing process to completely singulate the sensor dies 100. For example, Figure 3 FIG. 2 shows the substrate 102 after the laser process has been performed. Figure 3 As shown in , a laser process may be performed along scribe area 108 to form a groove extending through sacrificial layer 112 and into substrate 102. In some embodiments, the laser process may include, for example, a UV laser operating at a power between about 1 W and about 30 W.

[0023] After the laser process is performed, a sawing process may be performed along the scribe line region 108 to completely separate the sensor die 100 . Figure 4 As shown in . Using a laser process to remove a portion of the sacrificial layer 112 before the sawing process can reduce damage to the sacrificial layer 112 during the separation process. In some embodiments, the sacrificial layer 112 located above the sensor die 100 can have a convex or rounded upper surface, such as Figure 4 In this manner, a single sensor die 100 covered with a sacrificial layer 112 is formed.

[0024] Go to Figures 5 to 26 According to some embodiments, a sensor package 200 (see Fig.18 ), sensor device 300 (see Fig.19 )、Sensor package 400 (see Fig. 27 ) and sensor device 500 (see Fig.28 ). According to some embodiments, Figures 5 to 9 An intermediate step is shown that is performed before removing the sacrificial layer 112. According to some embodiments, Figures 10 to 19 An intermediate step in removing the sacrificial layer 112 using a dry etching process to form the sensor package 200 and the sensor device 300 is shown. According to some embodiments, Figures 20 to 28 An intermediate step in removing the sacrificial layer 112 using a wet etching process to form the sensor package 400 and the sensor device 500 is shown.

[0025] exist Figure 5In the embodiment of the present invention, a carrier substrate 202 is provided, and a release layer 204 is formed on the carrier substrate 202. The carrier substrate 202 may be, for example, a glass carrier substrate, a ceramic carrier substrate, etc. The carrier substrate 202 may be a wafer, so that a plurality of packages may be formed simultaneously on the carrier substrate 202. The release layer 204 may be formed of a polymer-based material, which may be removed from the upper structure to be formed in a subsequent step together with the carrier substrate 202. In some embodiments, the release layer 204 is an epoxy-based thermal release material that loses its adhesiveness when heated, such as a light-to-heat conversion (LTHC) release coating. In other embodiments, the release layer 204 may be an ultraviolet (UV) glue that loses its adhesiveness when exposed to UV light. The release layer 204 may be dispensed and cured in the form of a liquid, may be a laminated film laminated to the carrier substrate 202, etc. The top surface of the release layer 204 may be flush and may have a high degree of coplanarity.

[0026] exist Figure 6 In the embodiment shown, according to some embodiments, a backside redistribution structure 206 and a conductive via 216 are formed on the release layer 204. In the embodiment shown, the backside redistribution structure 206 includes a dielectric layer 208 and a metallization pattern 210 (sometimes referred to as a redistribution layer or redistribution line). The backside redistribution structure 206 is optional. In some embodiments, the metallization pattern 210 is omitted and only the dielectric layer 208 is formed.

[0027] A dielectric layer 208 is formed on the release layer 204. The bottom surface of the dielectric layer 208 may be in contact with the top surface of the release layer 204. In some embodiments, the dielectric layer 208 is formed of a polymer, such as polybenzoxazole (PBO), polyimide, benzocyclobutene (BCB), etc. In other embodiments, the dielectric layer 208 is formed of a nitride, such as silicon nitride; an oxide, such as silicon oxide, phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), etc.; or the like. The dielectric layer 208 may be formed by any acceptable deposition process, such as spin coating, chemical vapor deposition (CVD), lamination, etc., or a combination thereof.

[0028] A metallization pattern 210 is formed on the dielectric layer 208. As an exemplary process for forming the metallization pattern 210, a seed layer is formed above the dielectric layer 208. In some embodiments, the seed layer is a metal layer, which may be a single layer or a composite layer including multiple sublayers formed of different materials. In a specific embodiment, the seed layer includes a titanium layer and a copper layer located above the titanium layer. The seed layer may be formed using, for example, PVD. A photoresist is formed and patterned on the seed layer. The photoresist may be formed by spin coating, etc., and may be exposed to light for patterning. The pattern of the photoresist corresponds to the metallization pattern 210. Patterning forms an opening through the photoresist to expose the seed layer. Conductive material is formed in the opening of the photoresist and on the exposed portion of the seed layer. The conductive material may be formed by plating, such as electroplating or chemical plating, etc. The conductive material may include a metal, such as copper, titanium, tungsten, aluminum, etc., or a combination thereof. The portion of the photoresist and the seed layer on which the conductive material is not formed is removed. The photoresist may be removed by an acceptable ashing or stripping process, such as using oxygen plasma, etc. Once the photoresist is removed, the exposed portions of the seed layer are removed, such as by using an acceptable etching process, such as by wet etching or dry etching. The remaining portions of the seed layer and the conductive material form the metallization pattern 210.

[0029] It should be understood that the backside redistribution structure 206 may include any number of dielectric layers and metallization patterns. Additional dielectric layers and metallization patterns may be formed by repeating the process used to form the dielectric layer 208 and the metallization pattern 210. The metallization pattern may include wires and conductive vias. The conductive vias may be formed by forming a seed layer and a conductive material of the metallization pattern in an opening in the underlying dielectric layer during the formation of the metallization pattern. Thus, the conductive vias may interconnect and electrically connect the various wires. In some embodiments, the backside redistribution structure 206 includes a topmost dielectric or passivation layer that covers and protects the metallization pattern 210. In the embodiment shown, the topmost layer is omitted, and the subsequently formed sealant 242 is used to protect the metallization pattern 210.

[0030] Still refer to Figure 6, a conductive via 216 extending away from the dielectric layer 208 is formed on the dielectric layer 208. As an exemplary process for forming the conductive via 216, a seed layer is formed above the backside redistribution structure 206, for example, on the dielectric layer 208 and the metallization pattern 210. The seed layer for the conductive via 216 may be different from the seed layer for the metallization pattern 210, and may be further formed above the metallization pattern 210. In some embodiments, the seed layer is a metal layer, which may be a single layer or a composite layer including multiple sublayers formed of different materials. In a specific embodiment, the seed layer includes a titanium layer and a copper layer located above the titanium layer. The seed layer may be formed using, for example, PVD. A photoresist is formed and patterned on the seed layer. The photoresist may be formed by spin coating, etc. and may be exposed to light for patterning. The pattern of the photoresist corresponds to the conductive via. Patterning forms an opening through the photoresist to expose the seed layer. A conductive material is formed in the opening of the photoresist and on the exposed portion of the seed layer. The conductive material may be formed by plating, such as electroplating or chemical plating, etc. The conductive material may include a metal, such as copper, titanium, tungsten, aluminum, etc., or a combination thereof. The photoresist and the portion of the seed layer on which the conductive material is not formed are removed. The photoresist may be removed by an acceptable ashing or stripping process, such as using an oxygen plasma, etc. Once the photoresist is removed, the exposed portion of the seed layer is removed, such as by using an acceptable etching process, such as by wet etching or dry etching. The remaining portion of the seed layer and the conductive material form a conductive via 216. In the embodiment shown, the conductive via 216 is formed directly on the dielectric layer 208 and connected to the metallization pattern 210 by a wire. In other embodiments, the conductive via 216 is plated from a component of the metallization pattern 210. The conductive via 216 may be formed to have a height above the backside redistribution structure 206 that is greater than the height of the attached sensor die 100, as described below.

[0031] exist Figure 7 , the sensor die 100 is bonded to the backside redistribution structure 206 by an adhesive 228. The adhesive 128 is formed on the back side of the sensor die 100, and the sensor die 100 is bonded to the dielectric layer 208 of the backside redistribution structure 206. The adhesive 228 may be any suitable adhesive, epoxy, die attach film (DAF), etc. The adhesive 228 may be applied to the backside of the sensor die 100, or may be applied over the dielectric layer 208. For example, the adhesive 228 may be applied to the backside of the sensor die 100 before singulation to separate the sensor die 100.

[0032] Although one sensor die 100 is shown as being bonded to the backside redistribution structure 206, it should be understood that multiple sensor dies 100 may be bonded and present in the final sensor package 200. In such an embodiment, the sensor die 100 may vary in size and type. In some embodiments, the sensor die 100 may be a die with a large footprint, such as a system-on-chip (SoC) device. In embodiments where the sensor die 100 has a large footprint, the spacing available for the conductive vias 216 may be limited. When the sensor package 200 has limited spacing available for the conductive vias 216, the use of the backside redistribution structure 206 allows for an improved interconnect arrangement. In embodiments where a single sensor die 100 is used, a logic die, a memory die, or a combination thereof may also be included with the sensor die 100.

[0033] exist Figure 8 In some embodiments, a sealant 242 is formed on the various components. After formation, the sealant 242 at least laterally seals the conductive vias 216 and the sensor die 100. Thus, the metallization pattern 210 is disposed between the sealant 242 and the dielectric layer 208. The sealant 242 may be a molding compound, an epoxy, a resin, or the like. In some embodiments, the sealant 242 includes a filler material, such as particles of silicon oxide, or the like. The sealant 242 may be applied by compression molding, transfer molding, or the like. The sealant 242 may then be cured. Fig. 9 In some embodiments, a planarization process is performed. The planarization process may include a CMP process, a grinding process, etc. The planarization process may expose the conductive via 216 and the sacrificial layer 112. In some cases, after the planarization process, the surfaces of the conductive via 216, the sacrificial layer 112, and the sealant 242 are flush.

[0034] According to some embodiments, Figures 10 to 19 The formation of the sensor package 200 and the sensor device 300 is shown. According to some embodiments, the sensor package 200 (see Fig.18 ) is a package incorporating the sensor die 100, and the sensor device 300 (see Fig.19 ) is a device incorporating a sensor package 200. Figures 10 to 19 A process flow is described in which a dry etching process is used to remove the sacrificial layer 112. Therefore, the material of the sacrificial layer 112 may be a material selected to be removable by a dry etching process.

[0035] Go to Fig.10 According to some embodiments, a dry etching process is performed to Fig. 9 The structure shown in FIG. 1 is free of sacrificial layer 112. Fig.10As shown in , the dry etching process removes sacrificial layer 112 from above sensor die 100, thereby forming a recess 244 in encapsulant 242 that exposes sensor region 110 and pad 104 of sensor die 100. In some cases, the dry etching process also etches portions of encapsulant 242, which can form recess 244 with sloped sidewalls, such as Fig.10 . In some embodiments, the upper portion of the sidewall of the groove 244 may have an angle A1 between about 5 degrees and about 60 degrees relative to the lateral direction. In some embodiments, the lower portion of the sidewall of the groove 244 may have an angle A2 between about 0 degrees and about 15 degrees relative to the vertical direction. In some cases, by forming the groove 244 with the inclined sidewall, the subsequently formed layers, such as the dielectric layer 246 (described below), can have a more uniform morphology, which can reduce lithographic variations (e.g., of the openings 248, 250, and 252 described below) and reduce thickness variations of subsequently formed conductive features (e.g., the metallization pattern 256 described below).

[0036] In some embodiments, the dry etching process includes a plasma etching process. The plasma etching process may include, for example, oxygen, argon, CF4, CHF3, SF6, etc. or a combination thereof to form a plasma. In some embodiments, the plasma etching process includes an ion bombardment process. In some embodiments, the plasma etching process is implemented using a power between about 100 watts and about 1000 watts. Other process gases, powers or other process conditions are also possible.

[0037] In some cases, the dry etching process etches the encapsulant 242 so that the conductive via 216 protrudes above the encapsulant 242, such as Fig.10As shown in . In some cases, the conductive via 116 may protrude between about 0.5 μm and about 5 μm above the sealant 242. In some cases, the surface of the sealant 242 is roughened by the dry etching process, just as those surfaces are etched by the dry etching process. In some cases, after those surfaces of the passivation film 106 have been exposed by the dry etching process, the dry etching process roughens the surface of the passivation film 106. In some cases, after the dry etching process is implemented, the roughness of the surface of the sealant 242 and / or the roughness of the surface of the passivation film 106 may be between about Ra=1 μm and about Ra=10 μm. For example, the roughness of the surface of the passivation film 106 may be about Ra=1.03 μm, but other amounts of roughness are also possible. After the dry etching process is implemented, the sealant 242 may have a wavy surface. In addition, the dry etching process may expose the filling material of the sealant 242, and due to the dry etching process, the exposed filling material may have a rounded or rough exposed surface. In some embodiments, a cleaning process (eg, wet chemical process, rinsing, etc.) may be performed after the dry etching process to remove residues or particles. In some embodiments, no cleaning process is performed after the dry etching process.

[0038] According to some embodiments, Figures 11 to 16 The front side redistribution structure 264 is shown formed over the conductive via 216, the encapsulant 242 and the sensor die 100 (see FIG. Fig.16 ). The front side redistribution structure 264 includes a dielectric layer 246, a metallization pattern 256, and a dielectric layer 262. The metallization pattern may also be referred to as a redistribution layer or a redistribution line. The front side redistribution structure 264 is shown as an example, and an exemplary process for forming the front side redistribution structure 264 is discussed herein. More or fewer dielectric layers and metallization patterns may be formed in the front side redistribution structure 264. If more dielectric layers and metallization patterns are to be formed, the steps and processes discussed below may be repeated. The front side redistribution structure 264 as described herein may be used to electrically connect a conductive component (e.g., a conductive via 216) to the sensor die 100. By forming the front side redistribution structure 264 as described herein, a sensor package may be formed to have a smaller size (e.g., thickness or area). For example, instead of using wire bonding technology, the front side redistribution structure 264 may be used to form an electrical connection in a sensor package. The front side redistribution structure 264 may have a smaller total thickness than wire bonding, thereby producing a thinner sensor package. Furthermore, using relatively thin front side redistribution structures 264 can allow sensor region 110 of sensor die 100 to be closer to the outer surface of the sensor package. This allows sensor region 110 to be closer to the environment to be sensed, which can improve the sensitivity and response speed of the sensing operation.

[0039] exist Fig.11In some embodiments, a dielectric layer 246 is deposited over the structure. In some embodiments, the dielectric layer 246 is formed of a material such as PBO, polyimide, BCB, etc. In some embodiments, the dielectric layer 246 is formed of a photosensitive material that can be patterned using a photolithography mask. The dielectric layer 246 can be formed by spin coating, lamination, CVD, etc., or a combination thereof. Fig.11 As shown, the top surface of the dielectric layer 246 may be higher in the area above the encapsulant 242 and may be lower in the area above the sensor die 100. In other embodiments, the top surfaces of the dielectric layer 246 above the encapsulant 242 and above the sensor die 100 are substantially flush. In some embodiments, the dielectric layer 246 may have a thickness T2 between about 2 μm and about 50 μm above the sensor die 100. In some embodiments, the dielectric layer 246 above the sensor die 100 may have a height above the backside redistribution structure 206 that is less than the height of the encapsulant 242 above the backside redistribution structure 206. In other words, the thickness T2 may be such that the top surface of the dielectric layer 246 is below the top surface of the encapsulant 242. In some embodiments, the thickness T3 between the upper corner area of ​​the encapsulant 242 and the top surface of the dielectric layer 246 is between about 2 μm and about 10 μm. In some cases, sufficient thickness of dielectric layer 246 near the upper corner of sealant 242 can reduce thickness variation of subsequently formed conductive features (e.g., metallization pattern 256 described below). In some cases, due to the roughness of sealant 242, dielectric layer 246 located above sealant 242 can have a roughness between about Ra=2 μm and about Ra=7 μm.

[0040] like Fig.11 As shown, a region of dielectric layer 246 extending generally from above encapsulant 242 to above sensor die 100 can have a sloped top surface. In some embodiments, an upper region of the sloped top surface can have an angle A3 between about 20 degrees and about 60 degrees relative to the lateral direction. In some embodiments, a lower portion of the sloped top surface can have an angle A4 between about 105 degrees and about 170 degrees relative to the top surface of dielectric layer 246 located above sensor die 100. In some cases, by forming dielectric layer 246 with a sloped top surface extending above encapsulant 242 and sensor die 100, subsequently formed layers, such as dielectric layer 262 (described below), can have a more uniform topography and thickness variations of subsequently formed conductive features (e.g., metallization pattern 256 described below) can be reduced.

[0041] exist Fig.12, according to some embodiments, dielectric layer 246 is patterned to form openings 248, 250, and 252. Opening 248 is formed to expose conductive via 216, opening 250 is formed to expose sensor region 110 of sensor die 100, and opening 252 is formed to expose pad 104 of sensor die 100. Patterning may be performed using an acceptable photolithography process, such as when dielectric layer 246 is a photosensitive material, by exposing dielectric layer 246 to light and developing dielectric layer 246. Alternatively, patterning may be optionally performed by forming a patterned mask over dielectric layer 246 and then etching dielectric layer 246 using, for example, anisotropic etching.

[0042] exist Figures 13 to 15 In some embodiments, a metallization pattern 256 of a front side redistribution structure 264 is formed. To form the metallization pattern 256, a seed layer (not shown) is first formed over the dielectric layer 246 and in the openings 248, 250, and 252 extending through the dielectric layer 246. In some embodiments, the seed layer is a metal layer that can be a single layer or a composite layer including multiple sub-layers formed of different materials. In a specific embodiment, the seed layer includes a titanium layer and a copper layer located above the titanium layer. The seed layer can be formed using, for example, PVD.

[0043] refer to Fig.13 According to some embodiments, a photoresist 254 is then formed and patterned over the seed layer. The photoresist 254 may be formed by spin coating, lamination, etc. The patterning of the photoresist 254 may be performed using an acceptable photolithography process, such as by exposing the photoresist 254 to light and developing the dielectric layer 246. The patterning forms openings through the photoresist 254 to expose areas of the seed layer corresponding to the metallization pattern 256. Fig.13 As shown, photoresist 254 may be patterned to expose conductive vias 216 through openings 248 and to expose contact pads 104 through openings 252. Openings 250 may remain at least partially filled with photoresist 254 to protect sensor region 110 of sensor die 100.

[0044] Go to Fig.14, according to some embodiments, a conductive material is then formed in the opening of the photoresist 254 and on the exposed portion of the seed layer. The conductive material can be formed by plating, such as electroplating or chemical plating. The conductive material can be a metal, such as copper, titanium, tungsten, aluminum, etc. or a combination thereof. In some cases, conductive materials with different thicknesses can be formed in different regions. For example, a portion of the conductive material located above the sensor die 100 can have a greater thickness than a portion of the conductive material located above the sealant 242. The combination of the conductive material and the portion of the seed layer below forms a metallization pattern 256. The metallization pattern 256 includes conductive wires located on the main surface of the dielectric layer 246 and extending along the main surface of the dielectric layer 246. The metallization pattern 256 also includes: a conductive via 258 extending through the dielectric layer 246 to be physically and electrically connected to the conductive via 216; and a conductive via 260 extending through the dielectric layer 246 to be physically and electrically connected to the contact pad 104 of the sensor die 100.

[0045] Go to Fig.15 , and then removing the photoresist 254 and the portion of the seed layer on which the conductive material is not formed. The photoresist can be removed by an acceptable ashing or stripping process, such as using an oxygen plasma, etc. Once the photoresist is removed, the exposed portion of the seed layer is removed, such as by using an acceptable etching process, such as by wet or dry etching. Removing the photoresist 254 and the seed layer exposes the sensor region 110 through the opening 250 in the dielectric layer 246.

[0046] exist Fig.16 In the embodiment of the present invention, a dielectric layer 262 is deposited and patterned on the metallization pattern 256 and the dielectric layer 246 to form a front side redistribution structure 264 according to some embodiments. The dielectric layer 262 can be formed in a manner similar to the dielectric layer 246 and can be formed of the same material as the dielectric layer 246. The dielectric layer 262 is patterned to expose the sensor region 110 of the sensor die 100. In this manner, the opening 250 is extended through the dielectric layer 262. The patterning of the dielectric layer 262 can be implemented in a manner similar to the patterning of the dielectric layer 246. After the dielectric layer 262 is patterned, the opening 250 has a depth D1 extending from the main surface of the dielectric layer 262 to the topmost surface of the sensor die 100. In some embodiments, the depth D1 is in a range between about 2 μm and about 100 μm.

[0047] The opening 250 extends through the dielectric layers 246 and 262 of the front side redistribution structure 264. The metallization pattern 256 is not formed in the opening 250, so that the opening 250 is free of the material of the front side redistribution structure 264 (e.g., the material of the metallization pattern 256 and the dielectric layers 246 and 262). In some embodiments, the dielectric layer 262 is patterned so that the portion of the opening 250 extending through the dielectric 262 has a greater width than the portion of the opening extending through the dielectric layer 246. For example, the sidewalls of the dielectric layer 262 can be offset from the sidewalls of the dielectric layer 246 by a width W2 between about 0 μm and about 100 μm, such as about 20 μm. In some cases, the greater offset can allow greater exposure of the sensor region 110 to the sensed environment, which can increase the sensitivity and responsiveness of the sensing operation.

[0048] exist Fig.17 202 from the adhesive 228 and the backside redistribution structure 206 (e.g., the dielectric layer 208). According to some embodiments, an opening is then formed through the dielectric layer 208 to expose portions of the metallization pattern 210 and / or the conductive vias 216. In some embodiments, the stripping process includes projecting light, such as laser or UV light, on the release layer 204 so that the release layer 204 decomposes under the heat of the light and the carrier substrate 202 can be removed. The structure is then flipped over and placed on the tape 160. The opening in the dielectric layer 208 can be formed, for example, using laser drilling, etching, etc. A cleaning process can be performed after the laser drilling process to remove any remaining residue (e.g., of the dielectric layer 208).

[0049] exist Fig.18 In some embodiments, a conductive connector 266 is formed in an opening in the dielectric layer 208 to form the sensor package 200. The conductive connector 266 can be physically and electrically connected to the metallization pattern 210 and / or the conductive via 216. The conductive connector 266 may include a conductive material, such as solder, copper, aluminum, gold, nickel, silver, palladium, tin, etc., or a combination thereof. In some embodiments, the conductive connector 266 is formed by first forming a solder layer by such commonly used methods (such as evaporation, electroplating, printing, solder transfer, solder ball placement, etc.). Once the solder layer is formed on the structure, reflow can be implemented to shape the material into a desired bump shape. In some embodiments, the conductive connector 266 includes a flux and is formed in a flux dipping process. In some embodiments, the conductive connector 266 includes a conductive paste, such as a solder paste, a silver paste, etc., and is dispensed in a printing process.

[0050] In some embodiments, a plurality of sensor packages 200 are formed on a single carrier substrate 202, and a singulation process is performed to form individual sensor packages 200. The singulation process may be, for example, sawing, laser drilling, etc. By forming the sensor package 200 as described herein (e.g., using a sacrificial layer 112 and removing the sacrificial layer 112 using a dry etching process), the thickness of the sensor package 200 may be reduced. In addition, the sensor region 110 may be formed closer to the top of the sensor package 200 (e.g., the top of the dielectric layer 262), which may improve sensing performance.

[0051] exist Fig.19 In some embodiments, the sensor package 200 is mounted to the packaging substrate 302 using the conductive connector 266 to form the sensor device 300. The packaging substrate 302 can be made of semiconductor materials such as silicon, germanium, diamond, etc. Optionally, composite materials such as silicon germanium, silicon carbide, gallium arsenide, indium arsenide, indium phosphide, silicon germanium carbide, gallium arsenide phosphide, gallium indium phosphide, combinations of these, etc. can also be used. In addition, the packaging substrate 302 can be an SOI substrate. Typically, the SOI substrate includes a semiconductor material layer such as epitaxial silicon, germanium, silicon germanium, SOI, SGOI, or a combination thereof. In an optional embodiment, the packaging substrate 302 is based on an insulating core, such as a glass fiber reinforced resin core. An exemplary core material is a glass fiber resin, such as FR4. Optional materials for the core material include bismaleimide-triazine BT resin, or alternatively, other PCB materials or films. A build-up film (such as ABF) or other laminates can be used for the packaging substrate 302.

[0052] The packaging substrate 302 may include active and passive devices (not shown). As will be appreciated by one of ordinary skill in the art, a variety of devices (such as transistors, capacitors, resistors, combinations thereof, etc.) may be used to produce the structural and functional requirements of the design of the sensor device 300. The devices may be formed using any suitable method.

[0053] The package substrate 302 may also include metallization layers and vias (not shown) and bonding pads 304 located above the metallization layers and vias. The metallization layers may be formed above the active and passive devices and are designed to connect the various devices to form functional circuits. The metallization layers may be formed of alternating layers of dielectric (e.g., low dielectric constant material) and conductive material (e.g., copper) (wherein the vias interconnect the conductive material layers) and may be formed by any suitable process (such as deposition, metal damascene, dual metal damascene, etc.). In some embodiments, the package substrate 302 is substantially free of active and passive devices.

[0054] In some embodiments, the conductive connectors 266 are reflowed to attach the sensor package 200 to the bonding pads 304. The conductive connectors 266 electrically and / or physically connect the package substrate 302, including the metallization layers in the package substrate 302, to the sensor package 200. In some embodiments, a passive device (e.g., a surface mount device (SMD), not shown) can be attached to the sensor device 300 (e.g., bonded to the bonding pads 304) before being mounted on the package substrate 302. In such embodiments, the passive device can be bonded to the same surface of the sensor device 300 as the conductive connectors 266.

[0055] The conductive connector 266 may have an epoxy flux (not shown) formed thereon before reflow, and at least some epoxy portions of the epoxy flux remain after attaching the sensor package 200 to the package substrate 302. These remaining epoxy portions may be used as an underfill to reduce stress and protect the joints created by the reflow of the conductive connector 266. In some embodiments, an underfill (not shown) may be formed between the sensor package 200 and the package substrate 302 and around the conductive connector 266. The underfill may be formed by a capillary flow process after attaching the sensor package 200, or may be formed by a suitable deposition method before attaching the sensor package 200.

[0056] According to some embodiments, Figures 20 to 28 The formation of the sensor package 400 and the sensor device 500 is shown. According to some embodiments, the sensor package 400 (see Fig. 27 ) is a package incorporating the sensor die 100, and the sensor device 500 (see Fig.28 ) is a device incorporating a sensor package 400. Figures 20 to 28 The process shown is similar to Figures 10 to 19 The processes for forming sensor package 200 and sensor device 300 are shown, except that a wet etching process is used to remove sacrificial layer 112 from sensor die 100. Therefore, the material of sacrificial layer 112 can be selected to be removable by a wet etching process. In some cases, Figure 20 to Figure 26 Certain process steps or features of the illustrated embodiments are similar to those of Figures 10 to 19 The illustrated embodiments simulate process steps or features, and therefore the details are not repeated.

[0057] Go to Fig. 20 According to some embodiments, a wet etching process is performed to remove Fig. 9 The sacrificial layer 112 of the structure shown. Fig. 20As shown, the wet etching process removes sacrificial layer 112 from above sensor die 100, thereby forming a recess 244 in encapsulant 242 that exposes sensor region 110 and pad 104 of sensor die 100. In some cases, the wet etching process etches little or no portion of encapsulant 242, which can form recess 244 having an inwardly inclined upper sidewall, such as Fig. 20 As shown. In some embodiments, the upper portion of the sidewall of recess 244 can have an angle A5 between about 105 degrees and about 150 degrees relative to the lateral direction. In some cases, by forming recess 244 with an inwardly inclined upper sidewall, subsequently formed layers (such as dielectric layer 246) can have a more uniform morphology, which can reduce lithographic variations (e.g., of openings 248, 250, and 252) and reduce thickness variations of subsequently formed conductive features (e.g., metallization pattern 256).

[0058] The wet etching process may include, for example, immersing the structure in a wet chemical mixture including a solvent (such as DMSO, NMP, IPA, etc.) and one or more additives (such as copper corrosion inhibitors, stabilizers, etc., or combinations thereof). In some embodiments, during the wet etching process, the wet chemical mixture may be at a temperature between about 25° C. and about 90° C., such as about 50° C. In some embodiments, the wet etching process may be performed for a time between about 30 seconds and about 600 seconds, such as about 120 seconds. In some cases, performing the wet etching process for about 120 seconds may be sufficient to fully etch the sacrificial layer 112, and a drying time of 10 minutes or less may be sufficient to dry the structure after performing the wet etching process. In some cases, removing the sacrificial layer 112 using a wet etching process may reduce the overall processing time or cost for the sensor package.

[0059] In some cases, after the wet etching process is implemented, the conductive via 216 is recessed below the top surface of the sealant 242. In some cases, the conductive via 216 can be recessed between about 0.7 μm and about 2 μm below the sealant 242. In some cases, after the wet etching process is implemented, the surface of the sealant 242 and / or the passivation film 106 maintains a low roughness (e.g., Ra is less than about 0.5 μm, such as about 0.03 μm). In some embodiments, after the wet etching process is implemented, the surface of the sealant 242 is substantially flat. In some cases, the filling material of the sealant 242 is exposed by the wet etching process, and after the wet etching process is implemented, the exposed surface of the filling material is substantially flat. In some embodiments, the wet etching process is also used as a cleaning process to remove residues or particles, and a separate cleaning process is not implemented after the wet etching process.

[0060] According to some embodiments, Figure 21 to Figure 26The front side redistribution structure 264 is shown formed over the conductive via 216, the encapsulant 242 and the sensor die 100 (see FIG. Fig.26 ). The front side redistribution structure 264 includes a dielectric layer 246, a metallization pattern 256, and a dielectric layer 262. The front side redistribution structure 264 as described herein can be used to electrically connect a conductive component (e.g., a conductive via 216) to the sensor die 100. By forming a front side redistribution structure 264 as described herein, a sensor package having a smaller size (e.g., thickness or area) can be formed. For example, instead of using wire bonding technology, the front side redistribution structure 264 can be used to form an electrical connection in a sensor package. The front side redistribution structure 264 can have a smaller total thickness than wire bonding, resulting in a thinner sensor package. In addition, using a relatively thin front side redistribution structure 264 can allow the sensor area 110 of the sensor die 100 to be closer to the outer surface of the sensor package. This allows the sensor area 110 to be closer to the environment to be sensed, which can improve the sensitivity and response speed of the sensing operation.

[0061] exist Fig.21 In some embodiments, a dielectric layer 246 is deposited over the structure. Fig.21 As shown, the top surface of the dielectric layer 246 may be higher in the area above the encapsulant 242 and may be lower in the area above the sensor die 100. In other embodiments, the top surfaces of the dielectric layer 246 above the encapsulant 242 and above the sensor die 100 are substantially flush. In some embodiments, the dielectric layer 246 may have a thickness T4 between about 5 μm and about 150 μm above the sensor die 100. In some embodiments, the dielectric layer 246 above the sensor die 100 may have a height above the backside redistribution structure 206 that is less than the height of the encapsulant 242 above the backside redistribution structure 206. In other words, the thickness T4 may be such that the top surface of the dielectric layer 246 is below the top surface of the encapsulant 242. In some embodiments, the thickness T5 between the upper corner area of ​​the encapsulant 242 and the top surface of the dielectric layer 246 is between about 2 μm and about 10 μm. In some cases, sufficient thickness of dielectric layer 246 near upper corners of encapsulant 242 can reduce thickness variations in subsequently formed conductive features, such as metallization pattern 256. In some cases, dielectric layer 246 over encapsulant 242 can have a roughness of less than about Ra=0.2 μm.

[0062] like Fig.21As shown, a region of dielectric layer 246 extending generally from above encapsulant 242 to above sensor die 100 can have a sloped top surface. In some embodiments, an upper region of the sloped top surface can have an angle A6 between about 5 degrees and about 45 degrees relative to the lateral direction. In some embodiments, a lower portion of the sloped top surface can have an angle A7 between about 105 degrees and about 170 degrees relative to the top surface of dielectric layer 246 located above sensor die 100. In some cases, by forming dielectric layer 246 with a sloped top surface extending above encapsulant 242 and sensor die 100, subsequently formed layers, such as dielectric layer 262, can have a more uniform topography and thickness variations in subsequently formed conductive features (e.g., metallization pattern 256) can be reduced.

[0063] exist Fig. 22 , according to some embodiments, dielectric layer 246 is patterned to form openings 248, 250, and 252. Opening 248 is formed to expose conductive via 216, opening 250 is formed to expose sensor region 110 of sensor die 100, and opening 252 is formed to expose pad 104 of sensor die 100. The patterning may be performed using an acceptable photolithography process, such as by exposing dielectric layer 246 to light and developing dielectric layer 246 when dielectric layer 246 is a photosensitive material.

[0064] exist Figure 23 to Figure 25 In some embodiments, a metallization pattern 256 of a front side redistribution structure 264 is formed. To form the metallization pattern 256, a seed layer (not shown) is first formed over the dielectric layer 246 and in the openings 248, 250, and 252 extending through the dielectric layer 246. Fig.23 According to some embodiments, a photoresist 254 is then formed and patterned over the seed layer. Fig.23 As shown, photoresist 254 may be patterned to expose conductive vias 116 through openings 248 and to expose contact pads 104 through openings 252. Openings 250 may remain at least partially filled with photoresist 254 to protect sensor region 110 of sensor die 100.

[0065] Go to Fig.24, according to some embodiments, a conductive material is then formed in the opening of the photoresist 254 and on the exposed portion of the seed layer. The conductive material can be formed by plating, such as electroplating or chemical plating. The conductive material can be a metal, such as copper, titanium, tungsten, aluminum, etc. or a combination thereof. In some cases, conductive materials with different thicknesses can be formed in different regions. For example, the portion of the conductive material located above the sensor die 100 can have a greater thickness than the portion of the conductive material located above the sealant 242. The combination of the conductive material and the portion of the seed layer below forms a metallization pattern 256. The metallization pattern 256 includes conductive wires located on the main surface of the dielectric layer 246 and extending along the main surface of the dielectric layer 246. The metallization pattern 256 also includes: a conductive via 258 extending through the dielectric layer 246 to be physically and electrically connected to the conductive via 216; and a conductive via 260 extending through the dielectric layer 246 to be physically and electrically connected to the contact pad 104 of the sensor die 100.

[0066] Go to Fig.25 , and then removing the photoresist 254 and the portion of the seed layer on which the conductive material is not formed. The photoresist can be removed by an acceptable ashing or stripping process, such as using an oxygen plasma, etc. Once the photoresist is removed, the exposed portion of the seed layer is removed, such as by using an acceptable etching process, such as by wet or dry etching. Removing the photoresist 254 and the seed layer exposes the sensor region 110 through the opening 250 located in the dielectric layer 246.

[0067] exist Fig.26 In the embodiment of the present invention, a dielectric layer 262 is deposited and patterned on the metallization pattern 256 and the dielectric layer 246 to form a front side redistribution structure 264 according to some embodiments. The dielectric layer 262 can be formed in a manner similar to the dielectric layer 246 and can be formed of the same material as the dielectric layer 246. The dielectric layer 262 can be formed in a manner similar to the dielectric layer 246 and can be formed of the same material as the dielectric layer 246. The dielectric layer 262 is patterned to expose the sensor region 110 of the sensor die 100. In this manner, the opening 250 is extended through the dielectric layer 262. After the dielectric layer 262 is patterned, the opening 250 has a depth D2 extending from the main surface of the dielectric layer 262 to the topmost surface of the sensor die 100. In some embodiments, the depth D2 is in a range between about 2 μm and about 100 μm.

[0068] The opening 250 extends through the dielectric layers 246 and 262 of the front side redistribution structure 264. The metallization pattern 256 is not formed in the opening 250, so that the opening 250 is free of the material of the front side redistribution structure 264 (e.g., the material of the metallization pattern 256 and the dielectric layers 246 and 262). In some embodiments, the dielectric layer 262 is patterned so that the portion of the opening 250 extending through the dielectric 262 has a greater width than the portion of the opening extending through the dielectric layer 246. For example, the sidewalls of the dielectric layer 262 can be offset from the sidewalls of the dielectric layer 246 by a width W3 between about 0 μm and about 50 μm, such as about 20 μm. In some cases, the greater offset can allow greater exposure of the sensor region 110 to the sensed environment, which can increase the sensitivity and responsiveness of the sensing operation.

[0069] exist Fig. 27 2, a carrier substrate peeling process is performed to separate (or "peel") the carrier substrate 202 from the adhesive 228 and the backside redistribution structure 206 (e.g., the dielectric layer 208). Openings are then formed through the dielectric layer 208 to expose portions of the metallization pattern 210 and / or the conductive vias 216. According to some embodiments, conductive connectors 266 are then formed in the openings in the dielectric layer 208 to form the sensor package 400. The conductive connectors 266 can physically and electrically connect the metallization pattern 210 and / or the conductive vias 216.

[0070] In some embodiments, a plurality of sensor packages 400 are formed on a single carrier substrate 202, and a singulation process is performed to form individual sensor packages 400. The singulation process may be, for example, sawing, laser drilling, etc. By forming the sensor package 400 as described herein (e.g., using a sacrificial layer 112 and removing the sacrificial layer 112 using a wet etching process), the thickness of the sensor package 400 may be reduced. In addition, the sensor region 110 may be formed closer to the top of the sensor package 400 (e.g., the top of the dielectric layer 262), which may improve sensing performance.

[0071] exist Fig.28 In some embodiments, the sensor package 400 is mounted to the packaging substrate 302 using the conductive connector 266 to form the sensor device 500. The packaging substrate 302 may include active and passive devices (not shown). As will be appreciated by those of ordinary skill in the art, a variety of devices (such as transistors, capacitors, resistors, combinations thereof, etc.) may be used to generate the structural and functional requirements of the design of the sensor device 500. The device may be formed using any suitable method. The packaging substrate 302 may also include a metallization layer and a through hole (not shown) and a bonding pad 304 located above the metallization layer and the through hole. In some embodiments, the packaging substrate 302 is substantially free of active and passive devices.

[0072] Embodiments can achieve advantages. By forming a sacrificial layer (e.g., sacrificial layer 112) above a sensor die (e.g., sensor die 100), which is removable using a wet etching process or a dry etching process, a redistribution structure can be formed to electrically connect the sensor die without using wiring bonding. In this way, the sensor die can be used as part of an integrated fan-out (InFO) package (e.g., sensor package 200). Packaging the sensor die in an InFO package can allow the form factor of the final sensor package to be reduced. For example, some InFO sensor packages can be thinner than wire-bonded sensor packages. This can allow the sensor area of ​​the sensor die (e.g., sensor area 110) to be closer to the outside of the sensor package, which can improve the sensitivity or responsiveness of the sensing operation. In addition, a wiring loop located above the sensor area of ​​the sensor die can be avoided, and the distance between the sensing area and the target or environment to be sensed is reduced, thereby increasing the sensitivity of the sensor die. The mechanical reliability of the sensor package can also be improved, which is better than other (e.g., wire bonding) packaging schemes. The manufacturing yield of the InFO package can also be greater than that of the wire bond package. Because the InFO package exposes less surface area of ​​the sensor die than other packaging solutions, the sensing area of ​​the sensor die may be easier to keep clean, thereby improving sensing accuracy. In addition, by using a removable sacrificial film, the manufacturing cost or total processing time of the sensor package can be reduced.

[0073] In an embodiment, a device comprises: a sensor die having a sensing region at a top surface of the sensor die; an encapsulant at least laterally encapsulating the sensor die; a conductive via extending through the encapsulant; and a front side redistribution structure on the encapsulant and on the top surface of the sensor die, wherein the front side redistribution structure is connected to the conductive via and the sensor die, wherein an opening in the front side redistribution structure exposes the sensing region of the sensor die, and wherein the front side redistribution structure comprises: a first dielectric layer extending over the encapsulant and the top surface of the sensor die; a metallization pattern on the first dielectric layer; and a second dielectric layer extending over the metallization pattern and the first dielectric layer. In an embodiment, a device comprises: a back side redistribution structure, wherein a bottom surface of the sensor die is attached to the back side redistribution structure, and wherein the conductive via is connected to the back side redistribution structure. In an embodiment, the portion of the first dielectric layer extending over the top surface of the sensor die has a thickness greater than a thickness of the portion of the first dielectric layer extending over the encapsulant. In an embodiment, the front side redistribution structure is connected to the conductive via by a first via extending through the first dielectric layer, and is connected to the sensor die by a second via extending through the first dielectric layer. In an embodiment, the conductive via protrudes from the encapsulant. In an embodiment, the second dielectric layer extends over the sensor die, and wherein a vertical distance between a top surface of the sensor die and a top surface of the second dielectric layer is between 5 μm and 50 μm. In an embodiment, the first dielectric layer extending over the top surface of the sensor die has a lower top surface than the first dielectric layer extending over the encapsulant. In an embodiment, the opening is defined by sidewalls of the second dielectric layer and sidewalls of the first dielectric layer, wherein the sidewalls of the second dielectric layer are laterally recessed from the sidewalls of the first dielectric layer.

[0074] In an embodiment, a package includes: a semiconductor die including a contact pad located on a top surface of the semiconductor die and a sensing region located on the top surface of the semiconductor die; an encapsulant surrounding the semiconductor die, wherein the top surface of the semiconductor die is free of the encapsulant; a conductive via extending through the encapsulant, the conductive via being separated from the semiconductor die by the encapsulant. A first dielectric layer extending above the top surface of the encapsulant, along the sidewalls of the encapsulant, and above the top surface of the semiconductor die, wherein the first dielectric layer has a first opening exposing the sensing region of the semiconductor die; a conductive layer located above the top surface of the first dielectric layer, the conductive layer extending through the first dielectric layer to contact the conductive via, and extending through the first dielectric layer to contact the contact pad; and a second dielectric layer located above the conductive layer, wherein the second dielectric layer has a second opening exposing the sensing region of the semiconductor die through the first opening located in the first dielectric layer. In an embodiment, the sidewalls of the encapsulant extend above the semiconductor die. In an embodiment, the second opening has a width greater than the first opening. In an embodiment, the portion of the first dielectric layer extending above the semiconductor die has a top surface that is lower than a top surface of the encapsulant. In an embodiment, the thickness of the first dielectric layer located on the encapsulant is between 2 μm and 10 μm. In an embodiment, the sidewalls of the encapsulant are inclined away from the semiconductor die. In an embodiment, the first opening located in the first dielectric layer has a width between 5 μm and 50 μm. In an embodiment, the bottom surface of the semiconductor die is attached to the redistribution structure.

[0075] In an embodiment, a method includes: forming a sacrificial layer on a semiconductor die, the semiconductor die including a sensor; forming a conductive via on a first redistribution structure; placing the semiconductor die on the first redistribution structure adjacent to the conductive via; sealing the semiconductor die, the sacrificial layer, and the conductive via with an encapsulant; planarizing the encapsulant to expose the conductive via and the sacrificial layer; removing the sacrificial layer using an etching process; and forming a second redistribution structure over the encapsulant and over the semiconductor die, wherein the second redistribution structure is electrically connected to the conductive via and to the semiconductor die, and wherein the second redistribution structure includes an opening that exposes the sensor of the semiconductor die. In an embodiment, the etching process includes a wet chemical etching process. In an embodiment, the etching process includes a dry plasma etching process. In an embodiment, the method includes: after forming the sacrificial layer on the semiconductor die, using a laser process to remove the sacrificial layer located over a scribe area, and using a sawing process on the scribe area to separate the semiconductor die.

[0076] The features of several embodiments are summarized above so that those skilled in the art can better understand aspects of the present invention. Those skilled in the art should understand that they can easily use the present invention as a basis to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced herein. Those skilled in the art should also appreciate that such equivalent constructions do not deviate from the spirit and scope of the present invention, and that they can make various changes, substitutions and modifications herein without departing from the spirit and scope of the present invention.

Claims

1. A sensor device, comprising: a sensor die having a sensing region at a top surface of the sensor die; an encapsulant that at least laterally encapsulates the sensor die, wherein the encapsulant physically contacts sidewall surfaces of the sensor die; a conductive via extending through the encapsulant; and A front-side redistribution structure is located on the encapsulant and on the top surface of the sensor die, wherein the front-side redistribution structure is connected to the conductive via and the sensor die, wherein an opening located in the front-side redistribution structure exposes a sensing area of ​​the sensor die, and wherein the front-side redistribution structure includes: a first dielectric layer extending above the encapsulant and the top surface of the sensor die, wherein sidewalls of the first dielectric layer form sidewalls of the opening, a metallization pattern located on the first dielectric layer, and a second dielectric layer extending above the metallization pattern and the first dielectric layer, wherein a top surface of the first dielectric layer adjacent to the sidewall of the first dielectric layer is exposed from the second dielectric layer.

2. The sensor device according to claim 1, further comprising: A backside redistribution structure, wherein a bottom surface of the sensor die is attached to the backside redistribution structure, and wherein the conductive via is connected to the backside redistribution structure.

3. The sensor device according to claim 1, wherein: The portion of the first dielectric layer extending over the top surface of the sensor die has a thickness greater than a thickness of the portion of the first dielectric layer extending over the encapsulant.

4. The sensor device according to claim 1, wherein: The front side redistribution structure is connected to the conductive vias through first vias extending through the first dielectric layer and is connected to the sensor die through second vias extending through the first dielectric layer.

5. The sensor device according to claim 1, wherein: The conductive via protrudes from the encapsulant.

6. The sensor device according to claim 1, wherein: The second dielectric layer extends over the sensor die, and wherein a vertical distance between a top surface of the sensor die and a top surface of the second dielectric layer is between 5 μm and 50 μm.

7. The sensor device according to claim 1, wherein: The first dielectric layer extending over the top surface of the sensor die has a lower top surface than the first dielectric layer extending over the encapsulant.

8. The sensor device according to claim 1, wherein: The opening is formed by sidewalls of the second dielectric layer, wherein the sidewalls of the second dielectric layer are laterally recessed from the sidewalls of the first dielectric layer.

9. A sensor package, comprising: a semiconductor die including contact pads on a top surface of the semiconductor die and a sensing region on the top surface of the semiconductor die; an encapsulant surrounding the semiconductor die and physically contacting the semiconductor die, wherein a top surface of the semiconductor die and a bottom surface of the semiconductor die are free of encapsulant; a conductive via extending through the encapsulant, the conductive via being separated from the semiconductor die by the encapsulant; a first dielectric layer extending over a top surface of the encapsulant, along sidewalls of the encapsulant, and over a top surface of the semiconductor die, wherein the first dielectric layer has a first opening exposing a sensing region of the semiconductor die; a conductive layer over a top surface of the first dielectric layer, the conductive layer extending through the first dielectric layer to contact the conductive via, and extending through the first dielectric layer to contact the contact pad; and A second dielectric layer is located on the conductive layer, wherein the second dielectric layer has a second opening exposing a sensing region of the semiconductor die through the first opening in the first dielectric layer.

10. The sensor package according to claim 9, wherein: Sidewalls of the encapsulant extend over the semiconductor die.

11. The sensor package according to claim 9, wherein: The second opening has a width greater than that of the first opening.

12. The sensor package according to claim 9, wherein: The portion of the first dielectric layer extending over the semiconductor die has an exposed top surface.

13. The sensor package according to claim 9, wherein: The thickness of the first dielectric layer on the sealant is between 2 μm and 10 μm.

14. The sensor package according to claim 9, wherein: Sidewalls of the encapsulant slope away from the semiconductor die.

15. The sensor package according to claim 9, wherein: The first opening in the first dielectric layer has a width between 5 μm and 50 μm.

16. The sensor package according to claim 9, wherein: A bottom surface of the semiconductor die is attached to a redistribution structure.

17. A method of forming a sensor package, comprising: forming a sacrificial layer on a semiconductor die, the semiconductor die including a sensor; forming a conductive via on the first redistribution structure; placing the semiconductor die on the first redistribution structure adjacent to the conductive via; sealing the semiconductor die, the sacrificial layer and the conductive via with a sealant; planarizing the encapsulant to expose the conductive vias and the sacrificial layer; removing the sacrificial layer using an etching process; as well as A second redistribution structure is formed over the encapsulant and over the semiconductor die, wherein the second redistribution structure is electrically connected to the conductive vias and to the semiconductor die, and wherein the second redistribution structure includes an opening that exposes a sensor of the semiconductor die.

18. The method according to claim 17, wherein: The etching process includes a wet chemical etching process.

19. The method according to claim 17, wherein: The etching process includes a dry plasma etching process.

20. The method of claim 17, further comprising: After forming the sacrificial layer on the semiconductor die, a laser process is used to remove the sacrificial layer located above a scribe line region, and a sawing process is used on the scribe line region to separate the semiconductor die.