Semiconductor device and method for separating semiconductor device having PN junction
By setting a high-charge-density passivation layer on the separation surface and combining it with TLS or LIC methods, the problem of electronic quality degradation caused by the recombination effect on the separation surface is solved, thereby improving the performance of semiconductor devices and the efficiency of photovoltaic solar cells.
Patent Information
- Application Number
- CN201980077037.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-09-24
- Filing Date
- 2019-09-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2039-09-24
AI Technical Summary
During the separation process of semiconductor devices, recombination effects on the separation surface lead to a decline in electronic quality. Existing technologies are unable to effectively mitigate this impact, especially in photovoltaic solar cells, where recombination at the separation surface causes power loss and increases recombination rate.
A passivation layer with a fixed charge surface density of 10¹² cm⁻² is applied to the separation surface. This layer reduces the rate at which charge carriers reach the separation surface, and in particular, prevents charge carriers from passing through to a depth of about 20 nm in the silicon layer. Separation is performed using methods such as TLS or LIC, and heat treatment is performed after separation to further improve the passivation quality.
It effectively reduces the adverse effects of separation on electronic quality, improves the overall performance of semiconductor devices, especially in photovoltaic solar cells, reduces the recombination rate and power loss of separation surfaces, and simplifies the manufacturing process.
Smart Images

Figure CN113169242B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a semiconductor device according to claim 1 and a method for separating a semiconductor device having a pn junction according to claim 7. Background Art
[0002] When manufacturing semiconductor components, it is often desirable to separate a plurality of semiconductor components produced on a substrate by separating the substrate at at least one separation plane and thereby separating the semiconductor components. Such separation is necessary when manufacturing computer processors, since a plurality of computer processors are usually manufactured on a silicon wafer. In addition, the separation of photovoltaic solar cells is increasingly being used.
[0003] Today, photovoltaic modules are usually made of silicon solar cells with a side length of about 156 mm. The interconnection is achieved by means of an electrically conductive connection using conductive elements (mostly so-called cell connectors), which are connected alternately to the front and back sides of the solar cells. A disadvantage of this interconnection is that the high currents (up to about 10 A) of the individual solar cells require a very high conductivity of the cell connectors and thus a high conductor cross section.
[0004] One known possibility for avoiding this disadvantage is to arrange two or more solar cells on a silicon wafer so that the current per solar cell is proportionally reduced accordingly. The solar cells are not separated until the end of the process, so that production can be carried out with large starting wafers for as long as possible and thus maintain a high productivity and use existing production equipment.
[0005] If the solar cells are still electrically connected via the cell connectors as described above, spaces remain between the solar cells which are not photovoltaically effective and thus lead to a reduction in the efficiency of the module.
[0006] A known method for avoiding this disadvantage is the so-called shingled arrangement of solar cells, in which the upper side of one end of a solar cell is directly connected to the lower side of the next cell. For this purpose, external contacts are required on the front and rear sides of the solar cells at the edges that lie opposite each other. Since there are no highly conductive contact elements in the solar cells and for such shingled designs based on large conventional solar cells, the path through which the current must flow in the contact fingers to the external contacts located outside becomes very large in order to minimize shading. After processing the solar cells, the silicon wafers are cut into narrow strips, so that a plurality of photovoltaic solar cells with a conventional rectangular shape are thus obtained in order to minimize power losses in the finger-shaped contacts of the solar cells during shingling.
[0007] The singulation of semiconductor components produced on a substrate, in particular a silicon wafer, leads to an increase in the ratio of circumference to area and thus to a normalization of the area due to edge recombination. Power loss increases. Research shows (J.Dicker, "Analyse und Simulation von hocheffizienten Silizium-Solarzellenstrukturen für industrielle Fertigungstechniken", Dissertation, Konstanz, 2003), especially when pn junctions occur in the region of the separating planes where separation takes place. The cause of this is especially in the quasi-neutral region of emitter and base and, as mentioned above, especially in the edge recombination in the space charge region. It also turns out that the separation of separate semiconductor components leads to a significant increase in the recombination rate itself at the edges that are produced. This effect is important if the semiconductor component has a high electronic quality, especially a low recombination rate, on the other surface due to a passivation layer or other passivation mechanisms.
[0008] There is therefore a need to separate semiconductor components without significantly reducing the electronic quality due to the separation planes, in particular due to recombination effects at the separation planes.
[0009] It is known that for silicon solar cells, a native silicon dioxide layer on the separation surface can reduce the adverse effects when the illumination intensity is low (M. Hermle, J. Dicker, W. Warta, SW Glunz and G. Willeke, "Analysis of edge recombination for high-efficiency solar cells at low illumination densities", 2003, pp. 1009-1012.). However, only a slight improvement can be achieved when the silicon solar cell receives normal illumination. Summary of the invention
[0010] Therefore, an object of the present invention is to provide a semiconductor device and a method for separating a semiconductor device, thereby reducing the adverse effect of the separation surface on the electronic quality.
[0011] This object is achieved by a semiconductor component according to claim 1 and a method according to claim 7. Advantageous embodiments are specified in the dependent claims.
[0012] The method according to the invention is preferably designed for producing a semiconductor component according to the invention, in particular a preferred embodiment of the semiconductor component. The semiconductor component according to the invention is preferably formed by the method according to the invention, in particular a preferred embodiment of the method.
[0013] The semiconductor device according to the invention has a front side and an opposite back side and a side surface. In addition, the semiconductor device also has at least one emitter and at least one base, between which a pn junction is formed. The emitter extends parallel to the front side and / or the back side. The semiconductor device can thus be configured, for example, as a photovoltaic solar cell or a transistor. The emitter can be configured in a manner known per se. In particular, emitters produced by diffusion and / or injection, as well as heterogeneous emitters and emitters produced epitaxially are within the scope of the invention.
[0014] It is important that at least one side surface is a passivated separation surface, on which a separation surface passivation layer is arranged. The separation surface passivation layer has a positionally fixed charge, the charge having a value greater than or equal to 10 12 cm -2 The charge surface density can therefore be positive or negative. Importantly, the value of the charge surface density is greater than or equal to 10 12 cm -2 , that is, for positive charges, greater than or equal to 10 12 cm -2 , and for negative charges, less than or equal to -1×10 12 cm -2 .
[0015] The invention is based on the recognition that the adverse effects occurring at the separation surface can be particularly effectively reduced by having a value of ≥ 10 12 cm -2The charge surface density of the separation surface passivation layer is reduced. Although passivation layers that reduce the surface recombination velocity of charge carriers are known in semiconductor devices and especially in photovoltaic solar cells. However, the applicant's research shows that the negative effects on the separation surface can be particularly effectively reduced by the separation surface passivation layer described above. The reason is firstly that the fixed position charges in the separation surface passivation layer prevent the charge carriers in the semiconductor device, especially in the silicon layer of the semiconductor device, from reaching the separation surface. In particular, in the silicon layer, the charge carriers are prevented from reaching the separation surface from the separation surface to a depth of about 20nm. The advantage of this is that the near-surface damage caused by the separation process to the separation surface can be tolerated, and its depth can reach about 20nm. Mechanical separation is usually impossible without damaging multiple atomic layers on the volume surface of the semiconductor. But it can be limited to a depth of less than 20nm by appropriate process selection. Therefore, it is advantageous to implement this method so that separation is carried out by one of the following methods: TLS, LIC or LDC, because these methods have a smaller damage depth.
[0016] Advantageously, the separating surface passivation layer covers at least a region where the pn junction adjoins the separating surface, or, if the pn junction does not adjoin the separating surface, at least a region where the pn junction is extended to adjoin the separating surface.
[0017] A particularly advantageous passivation of the separating surface is achieved in that, in an advantageous embodiment, the separating surface passivation layer extends over the entire separating surface.
[0018] The semiconductor device according to the present invention has the advantage that, due to the passivation of the separation plane by the separation plane passivation layer, the area of the semiconductor device can be effectively utilized and the emitter can extend all the way to the separation plane. In particular, previously known methods for avoiding the negative influence of the separation plane, which are to isolate the pn junction from the separation plane by insulating trenches and / or by forming an emitter window, are no longer necessary or are not necessary. Even by not extending the pn junction directly to the separation plane, this advantageous effect can be increased, but in order to achieve this increase, a smaller spacing is sufficient.
[0019] The pn junction is therefore advantageously spaced apart from the separating plane by a distance of less than 50 μm, in particular less than 20 μm. It is particularly advantageous if the pn junction adjoins the separating plane, thereby enabling a simplified production method.
[0020] The separation surface passivation layer is preferably designed as a dielectric layer, in particular as an aluminum oxide layer, a silicon nitride layer or a silicon oxynitride layer. These layers can be produced in a manner known per se and provided with a high charge surface density. In particular, within the scope of the invention, the separation surface passivation layer is formed using one of the following methods:
[0021] -CVD (see below);
[0022] -ALD (see below);
[0023] - printing technology, in particular printing by screen printing, inkjet, extrusion or dispensing;
[0024] - spraying;
[0025] - Applying the layer material to the separation surface via the medium.
[0026] The semiconductor device can be designed as a transistor. Advantageously, the semiconductor device is designed as a photovoltaic solar cell. Since a long lifetime of minority charge carriers in the emitter and base is necessary for high efficiency, in particular in photovoltaic solar cells, the passivation of the separation plane is of particular importance here.
[0027] The semiconductor component is thus advantageously designed as a photovoltaic solar cell having at least one silicon layer in which at least the base is formed. It is within the scope of the invention that both the emitter and the base are formed in the silicon layer. It is also within the scope of the invention that a separate layer, in particular a separate silicon layer, is provided in order to form the emitter on the base.
[0028] The separation of the semiconductor component at the separation plane is advantageously carried out in such a way that a damage zone with a small depth is formed. It is particularly advantageous if the semiconductor component has a damage zone at the separation plane, in which the current charge carriers have a charge carrier lifetime of <1 μs at least in the base, and the damage zone has a thickness of <20 nm perpendicular to the separation plane. It is particularly advantageous if, at least in the base, in a region adjacent to the damage zone, the charge carriers have a charge carrier lifetime of >10 μs, as is customary in photovoltaic solar cells.
[0029] The method according to the invention for separating semiconductor components having a pn junction comprises the following method steps:
[0030] In method step A, a semiconductor component is provided, which has at least one emitter and at least one base, between which a pn junction is formed.
[0031] In method step B, the semiconductor component is singulated by singulation into at least two individual components at at least one separating plane.
[0032] It is essential that after method step B, a separating surface passivation layer is provided on the separating surface, the separating surface passivation layer being designed to have a localized charge having a value greater than or equal to 10 12 cm -2 This results in the advantages mentioned in the description of the semiconductor component according to the invention.
[0033] The separating surface passivation layer is preferably formed to cover the entire separating surface in order to achieve the most effective reduction possible of the adverse effects of the separating surface on the electronic quality of the semiconductor component.
[0034] It is within the scope of the present invention to separate the semiconductor components in method step B by using methods known per se. The separation of the semiconductor components in method step B can therefore be carried out in a manner known per se, in particular by one or more of the following methods:
[0035] a) separation by chip saw (WP Mulligan, A. Terao, DD Smith, PJ Verlinden, and R. M. Swanson, "Development of chip-size silicon solar cells", in Proceedings of the 28th IEEE Photovoltaic Specialists Conference, Anchorage, USA, 2000, pp. 158-163);
[0036] b) Groove generation using laser combined with subsequent mechanical fracture (M. Oswald, M. Turek, J. Schneider, and S. "Evaluation of silicon solar cell separation techniques for advanced module concepts", in Proceedings of the 28th European PhotovoltaicSolar Energy Conference and Exhibition, Paris, France, 2013, pp.1807-1812);
[0037] c) Thermal laser separation (TLS): M. Oswald, M. Turek, J. Schneider, and S. "Evaluation of silicon solar cell separation techniques for advanced module concepts", in Proceedings of the 28th European Photovoltaic Solar Energy Conference and Exhibition, Paris, France, 2013, pp.1807-1812; S.Eiternick, F.Kaule, H.-U.Zühlke, T.Kieβling, M.Grimm, S.Schoenfelder, and M.Turek, "High quality half-cell processing using thermal laser Separation", Energy Procedia, vol.77, pp.340-345, 2015.
[0038] d) Laser induced cutting (LIC): S.Weinhold, A.Gruner, R.Ebert, J.Schille, andH.Exner, "Study of fast laser induced cutting of silicon materials", inProc.SPIE 8967, Laser Applications in Microelectronic and OptoelectronicManufacturing (LAMOM), San Francisco, USA, 2014, 89671J.
[0039] Studies have shown that separation by TLS or LIC in method step B is particularly advantageous. The basis of the TLS method is the generation of a short laser groove by a first laser beam, which in this case leads to wafer separation along the edge to be produced by thermomechanical stresses introduced in any direction due to simultaneous heating (e.g. by a second laser beam) and cooling (e.g. by an air-water mixture). In this way, in particular the separation plane is achieved independently of the crystal orientation of the wafer to be separated. The LIC method is very similar to the TLS method, wherein in the LIC no effective cooling is supplemented after the heating (e.g. by a laser beam). The LIC method is also known by the name of LDC method (laser direct cutting).
[0040] The method according to the invention has the advantage, in particular, that the separation can be carried out after the production of the semiconductor component has been completed or at least substantially completed. Therefore, a passivation layer is advantageously applied to the front side and / or the back side of the semiconductor component before method step B. It is particularly advantageous if, before method step B, one or more metallic contact structures are applied to the front side and / or the back side of the semiconductor component in order to input and / or discharge charge carriers.
[0041] In order to improve the passivation quality of the separating surface passivation layer, it is advantageous if, after applying the separating surface passivation layer, the separating surface passivation layer is heat treated, in particular heated to a temperature greater than or equal to 150° C. for a period of at least 1 minute.
[0042] Furthermore, in order to improve the passivation quality, it may be advantageous to carry out the heat treatment in a defined atmosphere, in particular in an atmosphere containing hydrogen.
[0043] The heat treatment can be carried out in its entirety, in that the entire semiconductor component is heated. In an advantageous embodiment, the heat treatment of the separation plane passivation layer is carried out by successive local heating, in particular by laser. In this case, the local sub-regions of the separation plane passivation layer are heated successively, and it is particularly preferred that the heating be carried out in a hydrogen-containing atmosphere, as described above.
[0044] As explained above, the method according to the invention can be used particularly advantageously for separating photovoltaic solar cells. The semiconductor component is therefore preferably designed as a photovoltaic solar cell, particularly preferably at least the base is formed in a silicon layer.
[0045] In another advantageous embodiment, the separation surface passivation layer is additionally formed at least on the front side or at least on the back side of the semiconductor device. This has the advantage that the separation surface passivation layer can be used additionally on the front side and / or the back side with another function. In particular, when the semiconductor device is configured as a photovoltaic solar cell, the separation surface passivation layer is applied as an additional optical layer on the side facing the incident light when the solar cell is used, in particular on the front side, so that the light input in the solar module can be increased. Therefore, in the method according to the invention, in particular during the formation of the separation surface passivation layer on the separation surface, the separation surface passivation layer is additionally formed on the front side and / or the back side of the semiconductor device.
[0046] It is particularly advantageous if, as described above, a passivation layer is applied to at least one surface of the semiconductor component and a separation surface passivation layer is applied to the passivation layer and to the separation surface to be passivated. It is particularly advantageous if the passivation layer is additionally configured as a charge carrier blocking layer. This avoids the formation of fixed charges in the separation surface passivation layer on the surface where the separation surface passivation layer covers the charge carrier blocking layer. The reason for this is that the charge carrier blocking layer acts as a tunnel barrier, so that charge carriers from the semiconductor cannot enter the separation surface passivation layer and thus the separation surface passivation layer cannot form fixed charges. The charge carrier blocking layer is advantageously configured as a dielectric layer, in particular as a silicon nitride layer, a silicon oxide layer, a silicon oxynitride layer or an aluminum oxide layer.
[0047] Another advantage of the method is that the separation plane does not necessarily have to be parallel to the preferred direction in which the semiconductor substrate of the semiconductor component has the weakest bond. In the case of crystalline silicon wafers, the breaking is usually carried out in a direction of 45° relative to the edge of the silicon wafer, because there is less bond in this direction due to the crystal orientation. However, the method makes it possible to achieve a separation plane at any angle, in particular a separation plane parallel to the edge of the silicon wafer.
[0048] The separating plane is therefore preferably parallel to an edge of the semiconductor component, in particular parallel to an edge of a silicon wafer of the semiconductor component. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Other advantageous features and embodiments of the present invention are described below with the aid of examples and drawings.
[0050] Figure 1 Two embodiments of semiconductor devices according to the present invention and partial steps of two embodiments of methods according to the present invention are shown;
[0051] Figure 2 : A schematic plan view of a silicon wafer is shown from above in order to illustrate the position of the separation plane.
[0052] In the drawings, schematic diagrams not in accordance with the scale are shown. In particular, for better illustration, the width and thickness of each layer do not correspond to the actual scale.
[0053] Reference numerals list
[0054] 1a, 1b Semiconductor devices
[0055] 2a, 2b Emitter
[0056] 3a, 3b Base
[0057] 4a, 4b pn junction
[0058] 5b Lateral conduction avoidance zone
[0059] 6a, 6b Separation surface passivation layer
[0060] T separation surface DETAILED DESCRIPTION
[0061] Figure 1 Two embodiments A and B are shown, each with partial steps of an embodiment of the method according to the invention. Figure 1 a, iii respectively show the first embodiment of the semiconductor device according to the present invention, and Figure 1 b, iii shows a second embodiment of a semiconductor device according to the present invention.
[0062] As an example, a photovoltaic solar cell is described below as a semiconductor component. The semiconductor component also shown can be designed as a transistor in a modification of this example.
[0063] According to Figure 1 The partial steps shown in a illustrate a first embodiment of the method according to the present invention:
[0064] In method step A, a semiconductor device 1a is provided. In the present case, the semiconductor device has an n-doped emitter 2a formed by diffusion from the gas phase and a corresponding base 3a, which is doped with a p-doped dopant. Accordingly, a pn junction 4a is formed between the emitter 2a and the base 3a. The emitter and the base are formed in a silicon wafer. In addition, additional components of the solar cell known per se have been produced: these include a passivation layer located on the upper front side and on the lower back side, a metallization structure on the front side and the back side for conducting away charge carriers, an anti-reflection layer on the front side and, if necessary, on the back side for increasing the light absorption. In a variant of the embodiment, the emitter is formed by diffusion from a previously applied doping layer or by injection. The doping types of the emitter and the base can also be interchanged.
[0065] Next, in method step B, the separation is performed by cutting at the separation plane T using the TLS method described above. The separation plane T is perpendicular to Figure 1 and thus passes through the base 3a and the emitter 2a.
[0066] The TLS method is performed from the back side, that is, first, an initial groove is formed by laser on the back side located below in the area where the separation line T intersects with the back side. The initial groove starts at one edge of the semiconductor device. However, the initial groove does not extend over the entire width of the semiconductor device. Common initial grooves have a length in the range of 200 μm to 4 mm, usually less than 2 mm. Then, the separation of the semiconductor device is achieved by simultaneous heating and cooling as described above. In a variant of the embodiment, the TLS method is performed from the front side, so that the solar cell does not need to be rotated during the process.
[0067] exist Figure 1 The result is shown in a, ii: two mirror-symmetrical semiconductor components are produced, each of which has a pn junction 4 a which adjoins the separating plane T.
[0068] After method step B, a separating surface passivation layer 6 a is formed on the separating surface T. This formation is carried out by means of the industrially customary chemical vapor deposition (CVD) or, in a variant, by means of atomic layer deposition (ALD).
[0069] The separating surface passivation layer 6a therefore extends over the entire separating surface T. The separating surface passivation layer is formed as an aluminum oxide layer which, at the boundary surface with the separating surface T, has a value of ≥10 12 cm -2 , in the current case -3x10 12 cm -2 The charge surface density is 200 nm, and the separation surface passivation layer has a thickness of a few atomic layers, which is in the range of a few nm to a plurality of 10 nm, in the present case 6 nm.
[0070] exist Figure 1 A second embodiment of the method according to the invention is shown in Fig. b. In order to avoid repetition, only the main differences are described below:
[0071] The semiconductor component 1b also has an emitter 2b and a base 3b, so that a pn junction 4b is formed between the emitter and the base. However, as described above, between method steps A and B, that is, before separation, in method step B0, a lateral conduction avoidance region 5b is formed. Figure 1As shown in FIG. 2 , a lateral conduction avoidance region 5 b in the form of a separation trench is formed by laser ablation, which completely passes through the emitter 2 b and also through the pn junction 4 b. As a result, lateral conduction of charge carriers through the emitter to the separation plane T is avoided, and the adverse effect of the separation plane on the electronic quality of the semiconductor device is additionally reduced.
[0072] As in Figure 1 b, 2ii, similarly to the first embodiment, the semiconductor components are subsequently cut and separated at the separation plane T. In this embodiment, the cutting is performed by the LIC method described above.
[0073] As in Figure 1 b, 3iii, then the separation surface passivation layer 6b is applied. In the present case, the separation surface passivation layer is formed as an aluminum oxide layer, which has a value greater than or equal to 10 at the interface with the base and the emitter. 12 cm -2 , in the current case -3x10 12 cm -2 The charge surface density is 0.1%, and the separation surface passivation layer has a thickness of a few atomic layers, which is in the range of a few nm to a plurality of 10 nm, and is 6 nm in the present case. The separation surface passivation layer 6 b is produced by ALD. Thus, the separation surface passivation layer is formed not only on the separation surface T, but also on the wall of the lateral conduction avoidance region 5 b configured as a separation trench.
[0074] exist Figure 1 In the figures, only one separation surface is shown in each case for better illustration.
[0075] When singulating photovoltaic solar cells, for example in order to form modules according to the above-described shingled technology, a plurality of solar cells is usually singulated starting from a silicon wafer.
[0076] exist Figure 2 2 shows a schematic plan view from above of a silicon wafer in which photovoltaic solar cells have been formed. The method described above is carried out on a plurality of, in the present case four, separation planes T, so that five semiconductor components are present after separation.
Claims
1. A semiconductor device (1a, 1b) having a front side and an opposite back side and side surfaces, and having at least one emitter (2a, 2b) and at least one base (3a, 3b), a pn junction (4a, 4b) being formed between the emitter (2a, 2b) and the base (3a, 3b), and the emitter (2a, 2b) extending parallel to the front side and / or the back side, characterized in that At least one side surface is a passivated separation surface (T), on which a separation surface passivation layer (6a, 6b) is arranged, and the separation surface passivation layer has a positionally fixed charge, and the charge has a value greater than or equal to 10 on the separation surface (T). 12 cm -2 The pn junction (4a, 4b) is adjacent to the separation plane (T) with a charge surface density of .
2. The semiconductor device (1a, 1b) according to claim 1, characterized in that The separating surface passivation layer (6a, 6b) extends over the entire separating surface (T).
3. The semiconductor device (1a, 1b) according to any one of the preceding claims, characterized in that The pn junction (4a, 4b) is spaced apart from the separation plane (T) by a distance of less than 50 μm.
4. The semiconductor device (1a, 1b) according to claim 3, characterized in that The pn junction (4a, 4b) is separated from the separation plane (T) by a distance less than 50 μm, comprising: The pn junction (4a, 4b) is spaced apart from the separation plane (T) by a distance of less than 20 μm.
5. The semiconductor device (1a, 1b) according to claim 1, characterized in that The separation surface passivation layers (6a, 6b) are designed as dielectric layers.
6. The semiconductor device (1a, 1b) according to claim 5, characterized in that The dielectric layer includes one of an aluminum oxide layer, a silicon nitride layer, or a silicon oxynitride layer.
7. The semiconductor device (1a, 1b) according to claim 1, characterized in that The semiconductor component (1a, 1b) is designed as a photovoltaic solar cell.
8. The semiconductor device (1a, 1b) according to claim 7, characterized in that The photovoltaic solar cell has at least one silicon layer in which a base (3a, 3b) is formed.
9. The semiconductor device (1a, 1b) according to claim 1, characterized in that The semiconductor device (1a, 1b) has a damaged region on the separation plane (T), the current carriers in the damaged region have a carrier lifetime of less than 1 μs at least in the base (3a, 3b), and the damaged region has a thickness of less than 20 nm perpendicular to the separation plane (T).
10. The semiconductor device (1a, 1b) according to claim 9, characterized in that At least in the base (3a, 3b), in a region adjacent to the damaged region, the current charge carriers have a charge carrier lifetime of more than 10 μs.
11. A method for separating semiconductor components (1a, 1b) having a pn junction (4a, 4b), the method comprising the following method steps: A. A semiconductor device (1a, 1b) is provided, wherein the semiconductor device has at least one emitter (2a, 2b) and at least one base (3a, 3b), and a pn junction (4a, 4b) is formed between the emitter (2a, 2b) and the base (3a, 3b), B. separating the semiconductor component (1a, 1b) into at least two sub-components at at least one separation plane (T), the pn junction (4a, 4b) being adjacent to the separation plane (T), It is characterized in that Prior to method step B, a passivation layer is applied to the front side and / or the back side of the semiconductor component (1a, 1b), prior to method step B, one or more metallic contact structures are applied to the front side and / or the back side of the semiconductor component (1a, 1b), After method step B, a separating surface passivation layer (6a, 6b) is provided on the separating surface (T), the separating surface passivation layer having a fixed charge with a value greater than or equal to 10 12 cm -2 The surface charge density.
12. The method according to claim 11, characterized in that The separation surface passivation layer (6a, 6b) is configured to cover the entire separation surface (T).
13. The method according to claim 11 or 12, characterized in that: In method step B, separation is carried out by thermal laser separation, laser-induced cutting or laser direct cutting.
14. The method according to claim 11, characterized in that After the separation surface passivation layer (6a, 6b) is applied, the separation surface passivation layer (6a, 6b) is subjected to a heat treatment.
15. The method according to claim 14, characterized in that The heat treatment of the separation surface passivation layer (6a, 6b) comprises: The separation plane passivation layer (6a, 6b) is heated to a temperature greater than or equal to 150°C for a period of at least 1 minute.
16. The method according to claim 14, characterized in that The heat treatment is carried out by continuous local heating.
17. The method according to claim 16, characterized in that The heat treatment is performed by continuous local heating, comprising: The heat treatment is performed using a laser.
18. The method according to claim 17, characterized in that The heat treatment is performed in an atmosphere containing hydrogen.
19. The method according to claim 18, characterized in that The hydrogen-containing atmosphere includes a hydrogen atmosphere or a hydrogen / nitrogen atmosphere.
20. The method according to claim 11, characterized in that The separating plane passivation layer is additionally applied to at least one of the front side or the back side of the semiconductor component.
21. The method according to claim 11, characterized in that The semiconductor component (1a, 1b) is designed as a photovoltaic solar cell.
22. The method according to claim 21, characterized in that The photovoltaic solar cell has at least one silicon layer in which a base (3a, 3b) is formed.