Precursor for positive electrode active material of lithium secondary battery, method for producing precursor for positive electrode active material of lithium secondary battery, and method for producing lithium composite metal compound
Through the specific particle size distribution and composition of lithium secondary battery positive electrode active substance precursor, combined with the liquid cyclone separation grading and sintering technology, the problems of uneven particle size distribution of the positive electrode active substance of lithium secondary battery positive electrode active substance and high impurity silicon content are solved, and the problem of uneven particle size distribution of the positive electrode active substance of lithium secondary battery is improved. The cycle characteristics and charge and discharge performance of the battery are provided.
Patent Information
- Application Number
- CN201980079596.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-07
- Filing Date
- 2019-12-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-12-06
AI Technical Summary
The particle size distribution of the positive electrode active substance of the existing lithium secondary batteries is uneven, resulting in a decrease in battery characteristics and a high content of impurity silicon, which affects the charge and discharge performance.
Using a specific particle size distribution and composition of lithium secondary battery positive active material precursor, the particle size distribution is controlled, the impurity silicon content is reduced, and the sintering treatment is carried out in an oxygen atmosphere through laser diffraction particle size distribution determination and liquid cyclone separation grading technology. .
The circulation characteristics and charge and discharge load uniformity of lithium secondary batteries are improved, the content of impurity silicon is reduced, and the performance stability of the battery is enhanced.
Smart Images

Figure CN113169327B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a precursor for a positive electrode active material for a lithium secondary battery, a method for producing a precursor for a positive electrode active material for a lithium secondary battery, and a method for producing a lithium composite metal compound.
[0002] This application claims priority based on Japanese Patent Application No. 2018-230351 filed in Japan on December 7, 2018, the contents of which are incorporated herein by reference. Background Art
[0003] Lithium composite metal compounds are used as positive electrode active materials for lithium secondary batteries. Lithium secondary batteries have been put into practical use not only in small power sources for mobile phones and notebook computers, but also in medium-sized or large power sources for automobiles and power storage.
[0004] As an example of a method for producing a lithium mixed metal compound, there is a method of producing a precursor containing a metal element other than lithium (for example, nickel, cobalt, manganese, etc.), and calcining the obtained precursor and a lithium compound.
[0005] However, it is known that when using a positive electrode active material composed of particles with a narrow particle size distribution, a lithium secondary battery with excellent battery characteristics can be provided due to excellent filling into the electrode and the voltage applied to the particles in the electrode becoming uniform. For example, patent document 1 records a nickel-cobalt composite hydroxide (precursor) with a sharp particle size distribution and a method for manufacturing the same. By adjusting the particle size distribution of the precursor, the particle size distribution of the manufactured positive electrode active material can be controlled.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: International Publication No. 2014 / 051089 Summary of the invention
[0009] Problems to be solved by the invention
[0010] The positive electrode active material for lithium secondary batteries using the precursor described in Patent Document 1 has room for improvement from the viewpoint of improving battery characteristics.
[0011] The present invention has been completed in view of the above situation, and its purpose is to provide a precursor for a positive electrode active material for a lithium secondary battery having a specific particle size distribution and having few impurities in the precursor which are a cause of deterioration in battery characteristics, a method for producing a precursor for a positive electrode active material for a lithium secondary battery, and a method for producing a lithium composite metal compound.
[0012] Means used to solve problems
[0013] That is, the present invention includes the following inventions [1] to
[13] .
[0014] [1] A precursor for a positive electrode active material for a lithium secondary battery, comprising at least nickel and satisfying the following formula (1).
[0015] 0.2≤Dmin / Dmax (1)
[0016] (In formula (1), Dmin is the minimum particle size (μm) in the cumulative particle size distribution curve measured by a laser diffraction particle size distribution measuring device, and Dmax is the maximum particle size (μm) in the cumulative particle size distribution curve measured by a laser diffraction particle size distribution measuring device.)
[0017] [2] The precursor for a positive electrode active material for a lithium secondary battery according to [1], which is represented by the following composition formula (A).
[0018] Ni 1-x-y Co x M y O z (OH) 2-α (A)
[0019] (In the composition formula (A), 0≤x≤0.45, 0≤y≤0.45, 0≤x+y≤0.9, 0≤z≤3, -0.5≤α≤2, and M is one or more metal elements selected from Zr, Al, Ti, Mn, Ga, In and W.)
[0020] [3] The precursor for a lithium secondary battery positive electrode active material according to [1] or [2], which satisfies the following formulas (2) and (3).
[0021] (D50-D10) / D50≤0.35 (2)
[0022] (D90-D50) / D50≤0.50 (3)
[0023] (In equations (2) and (3), D10 is the value (μm) of the particle size at the point where the cumulative volume from the small particle side becomes 10% when the whole is set as 100% in the cumulative particle size distribution curve obtained by measuring the precursor using a laser diffraction particle size distribution measuring device, D50 is the value (μm) of the particle size at the point where the cumulative volume becomes 50%, and D90 is the value (μm) of the particle size at the point where the cumulative volume becomes 90%.)
[0024] [4] The precursor for a lithium secondary battery positive electrode active material according to any one of [1] to [3], which satisfies the following formula (4).
[0025] 10μm≤D50≤30μm (4)
[0026] [5] The precursor for a positive electrode active material for a lithium secondary battery according to any one of [1] to [4], wherein the precursor has a BET specific surface area of 2 m 2 / g~80m 2 / g.
[0027] [6] The precursor for a positive electrode active material for a lithium secondary battery according to any one of [1] to [5], which satisfies the following formula (5).
[0028] 0.65≤α / β≤1.45 (5)
[0029] (In formula (5), α is the half-value width of the diffraction peak at 2θ=52.4±1° obtained by X-ray diffraction using CuKα rays, and β is the half-value width of the diffraction peak at 2θ=73.9±1° obtained by X-ray diffraction using CuKα rays.)
[0030] [7] A method for producing a precursor for a positive electrode active material for a lithium secondary battery, comprising the following steps: a slurry preparation step, in which a metal-containing aqueous solution containing at least nickel and an alkaline aqueous solution are supplied to a reaction tank to obtain a hydroxide-containing slurry; and a classification step, in which the hydroxide-containing slurry is classified using a net.
[0031] [8] The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to [7], further comprising a reflow step of supplying the slurry after passing through the mesh to the reaction tank.
[0032] [9] The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to [7] or [8], wherein the mesh is made of a polymer material.
[0033]
[10] A method for producing a precursor for a positive electrode active material for a lithium secondary battery according to any one of [7] to [9], wherein, in the above-mentioned classification step, the classification device has a rotatable screw on the inner side of a fixed net, and classification is performed by rotating the above-mentioned screw at a circumferential speed of 1.0 m / s to 10.0 m / s.
[0034]
[11] A method for producing a precursor for a positive electrode active material for a lithium secondary battery, comprising the following steps: a slurry preparation step, in which a metal-containing aqueous solution containing at least nickel and an alkaline aqueous solution are supplied to a reaction tank to obtain a hydroxide-containing slurry; and a classification step, in which the hydroxide-containing slurry is classified using a cyclonic separation type classification device, wherein the classification step is carried out under the condition that the inlet pressure of the classification device is 0.01 MPa to 0.07 MPa.
[0035]
[12] The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to any one of [7] to
[11] , further comprising a heating step, in which heating is performed at a temperature range of 300° C. to 900° C. in an oxygen-containing atmosphere.
[0036]
[13] A method for producing a lithium composite metal compound, comprising the following steps: a mixing step, in which a precursor obtained by the method for producing a precursor for a lithium secondary battery positive electrode active material described in any one of [7] to
[12] is mixed with a lithium-containing compound; and a calcining step, in which the obtained mixture is calcined at a temperature of 500°C to 1000°C in an oxygen-containing atmosphere.
[0037] Furthermore, the present invention includes the following (1) to (17).
[0038] (1) A precursor for a positive electrode active material for a lithium secondary battery, comprising at least nickel and satisfying the following formula (1).
[0039] 0.20≤Dmin / Dmax (1)
[0040] (In formula (1), Dmin is the minimum particle size (μm) in the cumulative particle size distribution curve obtained by measuring the precursor of the lithium secondary battery positive electrode active material using a laser diffraction particle size distribution measuring device, and Dmax is the maximum particle size (μm) in the cumulative particle size distribution curve obtained by measuring the precursor of the lithium secondary battery positive electrode active material using a laser diffraction particle size distribution measuring device.)
[0041] (2) The precursor for a positive electrode active material for a lithium secondary battery according to (1), which is represented by the following composition formula (A).
[0042] Ni 1-x-y Co x M y Oz(OH) 2-α (A)
[0043] (In the composition formula (A), 0≤x≤0.45, 0≤y≤0.45, 0≤x+y≤0.9, 0≤z≤3, -0.5≤α≤2, and M is one or more metal elements selected from Zr, Al, Ti, Mn, Ga, In and W.)
[0044] (3) The precursor for a positive electrode active material for a lithium secondary battery according to (1) or (2), which satisfies the following formula (4).
[0045] 10μm≤D50≤30μm (4)
[0046] (In formula (4), D50 is the value (μm) of the particle size at the point where the cumulative volume from the small particle side becomes 50% when the whole is set to 100% in the cumulative particle size distribution curve obtained by measuring the precursor for the positive electrode active material of a lithium secondary battery by a laser diffraction particle size distribution measuring device.)
[0047] (4) The precursor for a positive electrode active material for a lithium secondary battery according to any one of (1) to (3), which satisfies the following formulas (2) and (3).
[0048] (D50-D10) / D50≤0.35 (2)
[0049] (D90-D50) / D50≤0.50 (3)
[0050] (In formula (2), D10 is the value (μm) of the particle size at the point where the cumulative volume from the small particle side becomes 10% when the whole is set to 100% for the cumulative particle size distribution curve obtained by measuring the precursor for the positive electrode active material of a lithium secondary battery by a laser diffraction particle size distribution measuring device, D50 is the value (μm) of the particle size at the point where the cumulative volume becomes 50%, and D90 is the value (μm) of the particle size at the point where the cumulative volume becomes 90%.)
[0051] (5) The precursor for a positive electrode active material for a lithium secondary battery according to any one of (1) to (4), wherein the precursor has a BET specific surface area of 2 m 2 / g~80m 2 / g.
[0052] (6) The precursor for a positive electrode active material for a lithium secondary battery according to any one of (1) to (5), which satisfies the following formula (5).
[0053] 0.65≤α / β≤1.45 (5)
[0054] (In formula (5), α is the half-value width of the diffraction peak at 2θ=52.4±1° obtained by X-ray diffraction using CuKα rays, and β is the half-value width of the diffraction peak at 73.9±1° obtained by X-ray diffraction using CuKα rays.)
[0055] (7) A method for producing a precursor for a positive electrode active material for a lithium secondary battery, comprising the following steps: a slurry preparation step, in which a metal-containing aqueous solution containing at least nickel and an alkaline aqueous solution are supplied to a reaction tank to obtain a hydroxide-containing slurry; and a classification step, in which the hydroxide-containing slurry is classified using a net.
[0056] (8) The method for producing a precursor of a positive electrode active material for a lithium secondary battery according to (7), wherein the precursor of a positive electrode active material for a lithium secondary battery is represented by the following composition formula (A).
[0057] Ni 1-x-y Co x M y O z (OH) 2-α (A)
[0058] (In the composition formula (A), 0≤x≤0.45, 0≤y≤0.45, 0≤x+y≤0.9, 0≤z≤3, -0.5≤α≤2, and M is one or more metal elements selected from Zr, Al, Ti, Mn, Ga, In and W.)
[0059] (9) The method for producing a precursor of a positive electrode active material for a lithium secondary battery according to (7) or (8), wherein the precursor of a positive electrode active material for a lithium secondary battery satisfies the following formula (4).
[0060] 10μm≤D50≤30μm (4)
[0061] (In formula (4), D50 is the value (μm) of the particle size at the point where the cumulative volume from the small particle side becomes 50% when the whole is set to 100% in the cumulative particle size distribution curve obtained by measuring the precursor for the positive electrode active material of a lithium secondary battery by a laser diffraction particle size distribution measuring device.)
[0062] (10) The method for producing a precursor of a positive electrode active material for a lithium secondary battery according to any one of (7) to (9), further comprising a reflow step of supplying the slurry after passing through the mesh to the reaction tank.
[0063] (11) The method for producing a precursor of a positive electrode active material for a lithium secondary battery according to any one of (7) to (10), wherein the mesh is made of a polymer material.
[0064] (12) A method for producing a precursor for a positive electrode active material for a lithium secondary battery according to any one of (7) to (11), wherein, in the above-mentioned classification step, the classification device has a rotatable screw on the inner side of a fixed net, and classification is performed by rotating the above-mentioned screw at a circumferential speed of 1.0 m / sec to 10.0 m / sec.
[0065] (13) A method for producing a precursor for a positive electrode active material for a lithium secondary battery, comprising the following steps: a slurry preparation step, in which a metal-containing aqueous solution containing at least nickel and an alkaline aqueous solution are supplied to a reaction tank to obtain a hydroxide-containing slurry; and a classification step, in which the hydroxide-containing slurry is classified using a cyclonic separation type classification device, wherein the classification step is carried out under the condition that the inlet pressure of the classification device is 0.01 MPa to 0.07 MPa.
[0066] (14) The method for producing a precursor of a positive electrode active material for a lithium secondary battery according to (13), wherein the precursor of a positive electrode active material for a lithium secondary battery is represented by the following composition formula (A).
[0067] Ni 1-x-y Co x M y O z (OH) 2-α (A)
[0068] (In the composition formula (A), 0≤x≤0.45, 0≤y≤0.45, 0≤x+y≤0.9, 0≤z≤3, -0.5≤α≤2, and M is one or more metal elements selected from Zr, Al, Ti, Mn, Ga, In and W.)
[0069] (15) The method for producing a precursor of a positive electrode active material for a lithium secondary battery according to (13) or (14), wherein the precursor of a positive electrode active material for a lithium secondary battery satisfies the following formula (4).
[0070] 10μm≤D50≤30μm (4)
[0071] (In formula (4), D50 is the value (μm) of the particle size at the point where the cumulative volume from the small particle side becomes 50% when the whole is set to 100% in the cumulative particle size distribution curve obtained by measuring the precursor for the positive electrode active material of a lithium secondary battery by a laser diffraction particle size distribution measuring device.)
[0072] (16) The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to any one of (7) to (15), further comprising a heating step in which heating is performed at a temperature range of 300° C. to 900° C. in an oxygen-containing atmosphere.
[0073] (17) A method for producing a lithium composite metal compound, comprising the following steps: a mixing step, in which a precursor obtained by the method for producing a precursor for a lithium secondary battery positive electrode active material as described in any one of (7) to (16) is mixed with a lithium compound; and a calcining step, in which the obtained mixture is calcined at a temperature of 500°C to 1000°C in an oxygen-containing atmosphere.
[0074] Effects of the Invention
[0075] According to the present invention, a positive electrode active material precursor for lithium secondary batteries having a low content of silicon as an impurity, a method for producing the positive electrode active material precursor for lithium secondary batteries, and a method for producing a lithium mixed metal compound can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0076] Figure 1A It is a schematic diagram showing the structure of an example of a lithium ion secondary battery.
[0077] Figure 1B It is a schematic diagram showing the structure of an example of a lithium ion secondary battery. DETAILED DESCRIPTION
[0078] <Precursor for positive electrode active material for lithium secondary battery>
[0079] The present embodiment is a precursor for a positive electrode active material for a lithium secondary battery. Hereinafter, a precursor for a positive electrode active material for a lithium secondary battery is sometimes referred to as a "precursor". The precursor of the present embodiment has a specific particle size distribution, so the content of silicon as an impurity is low. By mixing such a precursor with a lithium compound and calcining it, a lithium composite metal compound useful as a positive electrode active material for a lithium secondary battery can be manufactured.
[0080] Formula (1)
[0081] The precursor of the present embodiment satisfies the following formula (1).
[0082] 0.20≤Dmin / Dmax (1)
[0083] (In formula (1), Dmin is the minimum particle size (μm) in the cumulative particle size distribution curve measured by a laser diffraction particle size distribution analyzer. Dmax is the maximum particle size (μm) in the cumulative particle size distribution curve measured by a laser diffraction particle size distribution analyzer.)
[0084] The cumulative volume particle size distribution of the precursor was determined by laser diffraction scattering.
[0085] 250 μL of a 10 mass % sodium hexametaphosphate aqueous solution as a dispersant was charged into Microtrac MT3300EXII manufactured by Microtrac Biore Co., Ltd. to measure the particle size distribution and obtain a volume-based cumulative particle size distribution curve. The precursor powder was charged so that the transmittance during measurement was 85±5%.
[0086] Then, in the obtained cumulative particle size distribution curve, the value of the particle size at the point where the cumulative volume from the small particle side becomes 10% is D10 (μm), the value of the particle size at the point where the cumulative volume becomes 50% is D50 (μm), and the value of the particle size at the point where the cumulative volume becomes 90% is D90 (μm). Furthermore, the above-mentioned cumulative volume particle size distribution measurement is carried out multiple times, and for the minimum particle size and the maximum particle size, the central value of the data within 10% of the respective fluctuation errors is obtained, and the value of the minimum particle size is set as Dmin (μm) and the value of the maximum particle size is set as Dmax (μm).
[0087] In this embodiment, the lower limit of the formula (1) is preferably 0.20, more preferably 0.21, and particularly preferably 0.22. The upper limit of the formula (1) is preferably 0.30, more preferably 0.29, and particularly preferably 0.28.
[0088] The above upper limit and lower limit may be arbitrarily combined. Examples of the combination are shown in the following (1)-1 to (1)-3.
[0089] Among the following (1)-1 to (1)-3, (1)-1 is more preferable.
[0090] 0.20≤Dmin / Dmax≤0.30 (1)-1
[0091] 0.21≤Dmin / Dmax≤0.29 (1)-2
[0092] 0.22≤Dmin / Dmax≤0.28 (1)-3
[0093] The precursor of the present embodiment satisfying formula (1) is characterized in that: due to having a specific particle size distribution, the content of silicon as an impurity is low. When such a precursor is mixed with a lithium compound and fired, the content of silicon as an impurity is reduced for the manufactured lithium composite metal compound, and the firing reaction is easy to be carried out uniformly. When the lithium composite metal compound with reduced content of silicon as an impurity and firing unevenness is used as a positive electrode active material, the charge and discharge load is not easy to deviate due to the particles, and the battery characteristics such as cycle characteristics become good.
[0094] Formula (2) and Formula (3)
[0095] The precursor of the present embodiment preferably satisfies either or both of the following formulas (2) and (3).
[0096] (D50-D10) / D50≤0.35 (2)
[0097] (D90-D50) / D50≤0.50 (3)
[0098] (In equations (2) and (3), D10 is the value (μm) of the particle size at the point where the cumulative volume from the small particle side becomes 10% when the whole is set as 100% in the cumulative particle size distribution curve obtained by measuring the precursor using a laser diffraction particle size distribution measuring device, D50 is the value (μm) of the particle size at the point where the cumulative volume becomes 50%, and D90 is the value (μm) of the particle size at the point where the cumulative volume becomes 90%.)
[0099] Formula (2)
[0100] In this embodiment, the lower limit of formula (2) is preferably 0.15, more preferably 0.16, particularly preferably 0.17, and even more particularly preferably 0.18. The upper limit of formula (2) is preferably 0.34, more preferably 0.33, and even more preferably 0.32.
[0101] The above upper limit and lower limit may be arbitrarily combined. Examples of the combination are shown in the following (2)-1 to (2)-4.
[0102] 0.15≤(D50-D10) / D50≤0.35 (2)-1
[0103] 0.16≤(D50-D10) / D50≤0.34 (2)-2
[0104] 0.17≤(D50-D10) / D50≤0.33 (2)-3
[0105] 0.18≤(D50-D10) / D50≤0.32 (2)-4
[0106] Formula (3)
[0107] In this embodiment, the lower limit of formula (3) is preferably 0.27, more preferably 0.28, particularly preferably 0.29, and even more particularly preferably 0.30. The upper limit of formula (3) is preferably 0.48, more preferably 0.46, and particularly preferably 0.44.
[0108] The above upper limit and lower limit may be arbitrarily combined. Examples of the combination are shown in the following (3)-1 to (3)-5.
[0109] 0.27<(D90-D50) / D50≤0.50 (3)-1
[0110] 0.28<(D90-D50) / D50≤0.48 (3)-2
[0111] 0.29<(D90-D50) / D50≤0.46 (3)-3
[0112] 0.30<(D90-D50) / D50≤0.44 (3)-4
[0113] 0.30<(D90-D50) / D50≤0.50 (3)-5
[0114] In the precursor of the present embodiment that satisfies either or both of the formulas (2) and (3), the content of silicon as an impurity is low.
[0115] The secondary battery using the positive electrode active material produced using the precursor of this embodiment can have sufficiently improved cycle characteristics.
[0116] Formula (4)
[0117] The precursor of the present embodiment preferably further satisfies the formula (4).
[0118] 10μm≤D50≤30μm (4)
[0119] In this embodiment, the lower limit of formula (4) is preferably 11 μm, more preferably 12 μm, and particularly preferably 13 μm. The upper limit is preferably 27 μm or less, more preferably 25 μm or less, and particularly preferably 23 μm or less.
[0120] The above upper limit and lower limit may be arbitrarily combined. Examples of the combination are shown in the following (4)-1 to (4)-3.
[0121] 11μm≤≤D50≤27μm (4)-1
[0122] 12μm≤≤D50≤25μm(4)-2
[0123] 13μm≤D50≤23μm (4)-3
[0124] The positive electrode active material produced by the precursor of the present embodiment that satisfies the formula (4) reacts efficiently with the lithium raw material, and thus an excellent positive electrode active material can be obtained.
[0125] Formula (5)
[0126] The precursor of the present embodiment preferably further satisfies the formula (5). In addition, the lower limit thereof is preferably 0.75 or more, more preferably 0.85 or more, and particularly preferably 0.95 or more.
[0127] 0.65≤α / β≤1.45 (5)
[0128] (In formula (5), α is the half-value width of the diffraction peak at 2θ=52.4±1° obtained by powder X-ray diffraction measurement using CuKα radiation, and β is the half-value width of the diffraction peak at 73.9±1° obtained by powder X-ray diffraction measurement using CuKα radiation.)
[0129] For powder X-ray diffraction measurement, an X-ray diffraction device (e.g., Ultima IV manufactured by Rigaku Corporation) is used to fill the powder of the precursor into a dedicated substrate, and a Cu-Kα ray source is used to perform measurement under the conditions of a diffraction angle of 2θ=10° to 90°, a sampling width of 0.03°, and a scanning speed of 20° / min, thereby obtaining a powder X-ray diffraction pattern. Next, the powder X-ray diffraction pattern is analyzed using comprehensive powder X-ray analysis software PDXL (Rigaku Corporation), and the half-peak width α of the peak at 2θ=52.4±1° and the half-peak width β of the peak at 2θ=73.9±1° are obtained.
[0130] Composition formula (A)
[0131] The precursor of the present embodiment is preferably represented by the following composition formula (A).
[0132] Ni 1-x-y Co x M y O z (OH) 2-α (A)
[0133] (In the composition formula (A), 0≤x≤0.45, 0≤y≤0.45, 0≤x+y≤0.9, 0≤z≤3, -0.5≤α≤2, and M is one or more metal elements selected from Zr, Al, Ti, Mn, Ga, In and W.)
[0134] ··X
[0135] The lower limit of x is preferably 0.01, more preferably 0.02, and particularly preferably 0.03. The upper limit of x is preferably 0.44, more preferably 0.42, and particularly preferably 0.40. The above upper limit and lower limit may be arbitrarily combined.
[0136] As an example of the combination, x is preferably 0.01≤x≤0.44, more preferably 0.02≤x≤0.42, and particularly preferably 0.03≤x≤0.40.
[0137] ··y
[0138] The lower limit of y is preferably 0.01, more preferably 0.02, and particularly preferably 0.03. The upper limit of y is preferably 0.44, more preferably 0.42, and particularly preferably 0.40. The above upper and lower limits may be arbitrarily combined.
[0139] As an example of the combination, y is preferably 0.01≤y≤0.42, more preferably 0.02≤y≤0.44, and particularly preferably 0.03≤y≤0.40.
[0140] ··z
[0141] The lower limit of z is preferably 0.1, more preferably 0.2, and particularly preferably 0.3. The upper limit of z is preferably 2.9, more preferably 2.8, and particularly preferably 2.7. The above upper and lower limits may be arbitrarily combined.
[0142] As an example of the combination, z is preferably 0.1≤z≤2.9, more preferably 0.2≤z≤2.8, and particularly preferably 0.3≤z≤2.7.
[0143] ··α
[0144] The lower limit of α is preferably -0.45, more preferably -0.4, and particularly preferably -0.35. The upper limit of α is preferably 1.8, more preferably 1.6, and particularly preferably 1.4. The upper limit and lower limit mentioned above may be arbitrarily combined.
[0145] As an example of the combination, α is preferably -0.45≤α≤1.8, more preferably -0.4≤α≤1.6, and particularly preferably -0.35≤α≤1.4.
[0146] ··M
[0147] In formula (A), M is one or more metal elements selected from Zr, Al, Ti, Mn, Ga, In and W. Among them, it is preferably one or more metal elements selected from Zr, Al and Mn. Since Ga and In are elements of the same group as Al, the same effect as Al can be obtained.
[0148] BET specific surface area
[0149] The BET specific surface area of the precursor of this embodiment is preferably 2 m 2 / g or more, more preferably 4m 2 / g or more, particularly preferably 6m 2 / g or more. In addition, the BET specific surface area of the precursor of this embodiment is preferably 80m 2 / g or less, more preferably 65m 2 / g or less, particularly preferably 50m 2 / g or less.
[0150] The above upper limit and lower limit may be combined arbitrarily. As a specific example of the combination, the BET specific surface area of the precursor of this embodiment can be listed as 2m 2 / g~80m 2 / g, 4m 2 / g~65m 2 / g, 6m 2 / g~50m 2 / g. Among this combination, 2m is preferred 2 / g~80m 2 / g.
[0151] The positive electrode active material produced using the precursor of the present embodiment having a BET specific surface area within the above range tends to improve the power characteristics of the secondary battery.
[0152] The "BET specific surface area" is a value measured by the BET (Brunauer, Emmet, Teller) method. The BET specific surface area is measured by drying the precursor powder at 105°C for 30 minutes in a nitrogen atmosphere using a measuring device (e.g., Macsorb (registered trademark) manufactured by Moutech).
[0153] The form of the precursor of this embodiment is exemplified.
[0154] (i) One embodiment of the precursor of the present embodiment satisfies the above formula (1).
[0155] (ii) One embodiment of the precursor of the present embodiment satisfies the above formula (1) and is represented by the composition formula (A).
[0156] (iii) One embodiment of the precursor of the present embodiment satisfies the above formula (1) and the above formula (4).
[0157] (iv) One embodiment of the precursor of the present embodiment satisfies the above formula (1), satisfies the above formula (4), and is represented by the composition formula (A).
[0158] It is preferable that any one of the above aspects (i) to (iv) further satisfies the above formula (3).
[0159] It is preferable that any one of the above aspects (i) to (iv) satisfies the above formula (3) and further satisfies the above formula (2).
[0160] The embodiment of any one of (i) to (iv) above preferably satisfies the above formula (3), satisfies the above formula (2), and has a BET specific surface area of 2 m 2 / g~80m 2 / g.
[0161] The embodiment of any one of (i) to (iv) above preferably satisfies the above formula (3), satisfies the above formula (2), and has a BET specific surface area of 2 m 2 / g~80m 2 / g, and also satisfies the above formula (5).
[0162] <Method for producing a precursor for a positive electrode active material for a lithium secondary battery (1)>
[0163] The manufacturing method (1) of the positive electrode active material precursor for lithium secondary batteries of the present embodiment includes the following steps: a slurry preparation step, in which a metal-containing aqueous solution and an alkaline aqueous solution containing at least nickel are supplied to a reaction tank to obtain a hydroxide-containing slurry; and a classification step, in which a mesh is used to classify the above-mentioned hydroxide-containing slurry. Hereinafter, the "manufacturing method (1) of the positive electrode active material precursor for lithium secondary batteries" is referred to as the "manufacturing method (1) of the precursor". By the manufacturing method (1) of the precursor, a precursor satisfying the above formula (1) can be manufactured.
[0164] Specifically, a compound containing Ni as an essential metal and an optional metal element (one or more metal elements selected from Co, Zr, Al, Ti, Mn, Ga, In, and W) can be obtained.
[0165] The precursor production method (1) preferably includes a slurry preparation step, a classification step, and an optional reflow step in this order. Each step will be described below.
[0166] [Slurry preparation process]
[0167] The slurry preparation step is a step of supplying a metal-containing aqueous solution containing at least nickel and an alkaline aqueous solution to a reaction vessel to obtain a hydroxide-containing slurry.
[0168] In this process, the metal-containing aqueous solution and the alkaline aqueous solution are stirred and continuously supplied to the reaction tank respectively to react them to obtain a hydroxide-containing slurry. At this time, an aqueous solution containing an ammonium ion donor can also be supplied. As the hydroxide-containing slurry, this process is described by taking the hydroxide slurry containing nickel, cobalt, manganese and aluminum as an example.
[0169] First, a nickel salt solution, a cobalt salt solution, a manganese salt solution, an aluminum salt solution and a complexing agent are reacted by a continuous coprecipitation method described in Japanese Patent Application Laid-Open No. 2002-201028 to produce a nickel-containing s Co t Mn u Al v (OH) 2 (wherein s+t+u+v=1) is a metal-containing aqueous solution of a metal composite hydroxide.
[0170] The nickel salt used as the solute of the nickel salt solution is not particularly limited, and for example, any nickel salt of nickel sulfate, nickel nitrate, nickel chloride, and nickel acetate can be used.
[0171] As the cobalt salt that is the solute of the cobalt salt solution, for example, any of cobalt sulfate, cobalt nitrate, cobalt chloride, and cobalt acetate can be used.
[0172] As the manganese salt that is the solute of the manganese salt solution, for example, any of manganese sulfate, manganese nitrate, manganese chloride and manganese acetate can be used.
[0173] As the aluminum salt that is the solute of the aluminum salt solution, for example, aluminum sulfate, sodium aluminate, etc. can be used.
[0174] The above metal salts are used with the above Ni s Co t Mn u Al v (OH) 2 The ratio corresponding to the composition ratio is used.
[0175] That is, the molar ratio of each metal salt is nickel in the solute of the nickel salt solution, cobalt in the solute of the cobalt salt solution, manganese in the solute of the manganese salt solution, and aluminum as the solute of the aluminum salt solution. s Co t Mn u Al v (OH) 2 The composition ratio of s:t:u:v is used accordingly.
[0176] In addition, the solvent of the nickel salt solution, the cobalt salt solution, the manganese salt solution, and the aluminum salt solution is water.
[0177] The complexing agent is a compound that can form a complex with nickel ions, cobalt ions and manganese ions in aqueous solution.
[0178] Examples of the complexing agent include ammonium ion donors (ammonium sulfate, ammonium chloride, ammonium carbonate, ammonium fluoride, etc.), hydrazine, ethylenediaminetetraacetic acid, nitrilotriacetic acid, uracildiacetic acid, and glycine.
[0179] In the slurry preparation process, a complexing agent may be used or not. When a complexing agent is used, the molar ratio of the amount of the complexing agent contained in the mixed solution comprising a nickel salt solution, an optional metal salt solution and a complexing agent to the total number of moles of the metal salt is greater than 0 and less than 2.0. In the present embodiment, the molar ratio of the amount of the complexing agent contained in the mixed solution comprising a nickel salt solution, a cobalt salt solution, a manganese salt solution and a complexing agent to the total number of moles of the metal salt is greater than 0 and less than 2.0.
[0180] In the slurry preparation step, in order to adjust the pH value of the mixed solution containing the nickel salt solution, the optional metal salt solution and the complexing agent, an alkali metal hydroxide is added to the mixed solution before the pH of the mixed solution changes from alkaline to neutral. The alkali metal hydroxide is, for example, sodium hydroxide or potassium hydroxide.
[0181] In addition, the pH value in this specification means the value measured when the temperature of the mixed liquid is 40° C. The pH of the mixed liquid is measured when the temperature of the mixed liquid sampled from the reaction tank reaches 40° C.
[0182] The pH of the mixed solution is preferably 10 to 13, and more preferably 11.5 to 11.9, when measured at a liquid temperature of the aqueous solution of 40°C.
[0183] When the complexing agent is continuously supplied to the reaction tank in addition to the above-mentioned nickel salt solution, cobalt salt solution, manganese salt solution, and aluminum salt solution, nickel, cobalt, manganese, and aluminum react to generate Ni s Co t Mn u Al v (OH) 2 .
[0184] During the reaction, the temperature of the reaction tank is controlled within a range of, for example, 20°C to 80°C, and preferably within a range of 30°C to 70°C.
[0185] The reaction tank may be in an inert atmosphere. When the reaction tank is in an inert atmosphere, metals contained in the mixed solution that are more easily oxidized than nickel are prevented from agglomerating before nickel. Therefore, a uniform precursor can be obtained.
[0186] In addition, the reaction tank may be in a moderate oxidizing atmosphere. The oxidizing atmosphere may be an oxygen-containing atmosphere formed by a mixture of an inert gas and an oxidizing gas, or an oxidant may be present in an inert gas atmosphere. By making the reaction tank in a moderate oxidizing atmosphere, the transition metal contained in the mixed solution is moderately oxidized, making it easy to control the form of the precursor.
[0187] As for the oxygen and oxidizing agent in the oxidizing atmosphere, it is sufficient that there are enough oxygen atoms to oxidize the transition metal.
[0188] When the oxidizing atmosphere is an oxygen-containing atmosphere, the atmosphere in the reaction vessel can be controlled by a method such as introducing an oxidizing gas into the reaction vessel or bubbling the oxidizing gas in the mixed liquid.
[0189] When the oxidation amount of the transition metal increases, the specific surface area increases.
[0190] In addition, in order to improve the uniformity in the reaction tank and promote the crystal growth of the precursor based on the oxidation of the transition metal element, it is preferred to stir the solution by a stirring paddle provided in the reaction tank. By adjusting the stirring speed, the specific surface area, particle shape, particle size distribution, etc. of the precursor can be controlled. For example, although it is also related to the stirring speed and the size of the reaction tank, it is preferred to set the stirring speed to 300 rpm to 2000 rpm.
[0191] [Grading process]
[0192] This process is the following process: using a net to classify the hydroxide-containing slurry generated by the slurry preparation process. The hydroxide-containing slurry is continuously taken out from the reaction tank and classified by a classifier equipped with a net. By the classifier, the particles that have not passed through the net are recovered as target particles, and the slurry containing the particles after the net passes is refluxed to the reaction tank. At this time, the classifier can have an inclination angle relative to the horizontal direction, and the inclination angle is preferably adjusted in order to prevent the particles that do not reach the target particle size from mixing into the particles as the target. In addition, the slurry containing the particles after the net passes can appropriately adjust the concentration and flow back to the reaction tank.
[0193] The particles that have not reached the target particle size and have returned to the reaction tank grow again in the reaction tank, and are then guided from the reaction tank to the classification device, and are discharged out of the reaction tank once they reach the target particle size.
[0194] By repeatedly performing this operation, particles that do not reach the target particle size are generated again in the reaction tank, and the target particles that do not pass through the net are selectively discharged to the outside of the reaction tank. At the same time, particles that do not reach the target particle size can be repeatedly grown until the target particle size is reached. Therefore, the particle size of the precursor finally obtained is easy to become uniform, and its particle size distribution can be adjusted to a desired range.
[0195] In this step, a classifying device equipped with a net is used. As such a classifying device, a slurry classifier equipped with a fixed net and a rotatable screw inside the net is preferred.
[0196] The material of the net is preferably a polymer material. Examples of the polymer material include cellulose acetate polymer, polysulfone, polyethersulfone, polyacrylonitrile, polyether, fluorine-based polymer, polyamide, polyimide, polyethylene, and polypropylene.
[0197] In the classification step, when a slurry classifier including a rotatable screw inside a fixed net is used as the classification device, the screw is preferably rotated at a peripheral speed of 1.0 m / sec to 10.0 m / sec.
[0198] By adjusting the mesh size of the mesh used, the Dmin of the produced precursor can be controlled.
[0199] [Reflow process]
[0200] The reflux process is a process in which the slurry containing particles that have not reached the target particle size after being classified by the classification device is returned (refluxed) to the reaction tank in the classification process. The reflux method is not particularly limited, and a known method can be used. For example, in the case where the slurry containing particles that have not reached the target particle size after being classified is directly returned to the reaction tank, it can be returned to the reaction tank directly or after being concentrated by a pump.
[0201] The reflux rate, that is, the rate at which the slurry including particles that do not reach the target particle size is returned to the reaction tank, may be adjusted according to the supply rate of the aqueous solution containing the raw material, the aqueous solution containing the ammonium ion donor, and the like.
[0202] <Method for producing a precursor for a positive electrode active material for a lithium secondary battery (2)>
[0203] The method (2) for manufacturing a positive electrode active material precursor for a lithium secondary battery of the present embodiment includes the following steps: a slurry preparation step, in which a metal-containing aqueous solution and an alkaline aqueous solution containing at least nickel are supplied to a reaction tank to obtain a hydroxide-containing slurry; and a classification step, in which the hydroxide-containing slurry is classified by a cyclone separation type classification device. The classification step is implemented under the condition that the inlet pressure of the classification device is 0.01MPa to 0.07MPa. Hereinafter, the "method (2) for manufacturing a precursor for a positive electrode active material for a lithium secondary battery" is referred to as the "method (2) for manufacturing a precursor". By the method (2) for manufacturing a precursor, a precursor satisfying the above formula (1) can be manufactured.
[0204] The method for producing a precursor (2) preferably includes a slurry preparation step, a classification step, and an optional reflow step in sequence. The following descriptions of the slurry preparation step and the reflow step are the same as those in the method for producing a precursor (1). The classification step in the method for producing a precursor (2) is described below.
[0205] [Grading process]
[0206] This process uses a hydrocyclone-type classifier. According to the hydrocyclone-type classifier, the classification point can be easily controlled by the shape and size of the cyclone separation section and the introduction pressure of the treated slurry. The hydroxide-containing slurry is continuously taken out from the reaction tank and stored in the slurry storage tank, and is classified into a large particle size portion and a small particle size portion by the hydrocyclone-type classifier. The large particle size portion is recovered as the target particle by the classifier, and the small particle size portion is continuously returned to the reaction tank as the particle that does not reach the target particle size. At this time, the slurry in the slurry storage tank can also be continuously returned to the reaction tank while being appropriately dehydrated.
[0207] The operating conditions of the hydrocyclone-type classifier were adjusted so that the classifier inlet pressure would be 0.01 MPa to 0.07 MPa.
[0208] In the present embodiment, the inlet pressure of the classification device is preferably 0.01 MPa to 0.06 MPa, and more preferably 0.01 MPa to 0.05 MPa.
[0209] When the precursor production method (1) or (2) includes a reflow step, it is possible to produce growth particles using particles that have not reached the target particle size as nuclei. Therefore, the precursor can be produced without wasting the raw material metal.
[0210] The precursor produced by the precursor production method (1) or (2) is characterized in that it contains less impurities such as silicon. The reason for this is considered to be as follows.
[0211] The precursor produced by the precursor production method (1) or (2) has a specific particle size distribution. Therefore, it is considered that impurities such as silicon contained in the washing water used in the dehydration step are less likely to be adsorbed on the precursor.
[0212] The precursor production method (1) or (2) may include a dehydration step and a drying step described below, and may also include a heating step described below.
[0213] [Dehydration process]
[0214] The precursor obtained after the classification step is washed and then dried to separate the precursor hydroxide of the nickel-cobalt-manganese-aluminum composite compound.
[0215] The separation is preferably carried out by dehydrating the slurry (coprecipitate slurry) containing the precursor hydroxide by centrifugal separation, suction filtration or the like.
[0216] The precursor hydroxide obtained by the above dehydration is preferably washed with water or a washing liquid containing an alkali. In the present embodiment, it is preferably washed with a washing liquid containing an alkali, more preferably with a sodium hydroxide solution or a potassium hydroxide solution. In addition, a washing liquid containing sulfur element may also be used for washing.
[0217] [Drying process]
[0218] The precursor hydroxide obtained in the above dehydration step is dried at 105° C. to 200° C. in an air atmosphere for 10 to 20 hours.
[0219] In addition, although the above example is about the production of nickel-cobalt-manganese-aluminum composite hydroxide, nickel-cobalt-manganese-aluminum composite oxide can also be produced.
[0220] [Heating process]
[0221] The precursor obtained in the classification step or the precursor obtained in the drying step is preferably heated at a temperature in the range of 300° C. to 900° C. in an oxygen-containing atmosphere.
[0222] By the heating step, when the precursor and the lithium compound are mixed, the composition ratio of lithium and the metal element in the produced lithium mixed metal compound can be stabilized.
[0223] The heating time is preferably set to a total time of 1 to 30 hours from the start of heating to reaching the temperature and ending the temperature holding. The heating rate of the heating process to reach the maximum holding temperature is preferably 180°C / hour or more, more preferably 200°C / hour or more, and particularly preferably 250°C / hour or more.
[0224] The heating temperature is preferably 350° C. to 800° C., more preferably 400° C. to 700° C. When the heating temperature is above the lower limit, hydroxide can be suppressed from remaining in the precursor. When the heating temperature is below the upper limit, sintering between the precursor particles can be suppressed, and the particle size distribution can be uniformly maintained.
[0225] The maximum holding temperature in this specification is the maximum temperature of the holding temperature of the atmosphere in the firing furnace in the firing process, and refers to the firing temperature in the firing process. In the case of a main firing process including multiple heating processes, the maximum holding temperature refers to the highest temperature in each heating process.
[0226] The temperature increase rate in this specification is calculated from the time from the start of temperature increase to the maximum holding temperature in the sintering device and the temperature difference from the temperature at the start of temperature increase to the maximum holding temperature in the sintering furnace of the sintering device.
[0227] The following are examples of the method (1) for producing a precursor or the method (2) for producing a precursor according to the present embodiment.
[0228] (i) According to one embodiment of the method (1) for producing a precursor or the method (2) for producing a precursor of the present embodiment, a precursor satisfying the above formula (1) can be produced.
[0229] (ii) According to one embodiment of the method (1) or the method (2) for producing a precursor of the present embodiment, a precursor satisfying the above formula (1) and represented by the composition formula (A) can be produced.
[0230] (iii) According to one embodiment of the method (1) or the method (2) for producing a precursor of the present embodiment, a precursor satisfying the above formula (1) and the above formula (4) can be produced.
[0231] (iv) According to one embodiment of the precursor production method (1) or the precursor production method (2) of the present embodiment, a precursor satisfying the above formula (1) and the above formula (4) and represented by the composition formula (A) can be produced.
[0232] <Method for producing lithium mixed metal compound>
[0233] The present embodiment is a method for producing a lithium composite metal compound, which includes the following steps: a mixing step, in which a precursor obtained by the above-mentioned precursor production method (1) or precursor production method (2) is mixed with a lithium compound; and a calcining step, in which the obtained mixture is calcined at a temperature of 500°C to 1000°C in an oxygen-containing atmosphere.
[0234] [Mixing process]
[0235] This step is a step of mixing a precursor and a lithium compound to obtain a mixture.
[0236] Lithium compounds
[0237] The lithium compound used in this embodiment can be any one of lithium carbonate, lithium nitrate, lithium acetate, lithium hydroxide, lithium oxide, lithium chloride, and lithium fluoride, or a mixture of two or more thereof. Among them, any one or both of lithium hydroxide and lithium carbonate are preferred.
[0238] The method of mixing the precursor and the lithium compound according to the present embodiment will be described.
[0239] The precursor and the lithium compound are mixed in consideration of the composition ratio of the final target product. For example, when a nickel-cobalt-manganese-aluminum composite hydroxide is used as a precursor, the lithium compound and the precursor are mixed in an amount of Li[Li r (Ni s Co t Mn u Al v ) 1-r ]O 2 The precursor and the lithium compound are mixed in a ratio corresponding to the composition ratio (where s+t+u+v=1). By firing the mixture of the precursor and the lithium compound in the subsequent firing step, a lithium-nickel-cobalt-manganese-aluminum composite oxide can be obtained.
[0240] [Firing process]
[0241] By calcining a mixture of the precursor of the present embodiment and a lithium compound, a lithium mixed metal compound can be obtained.
[0242] The firing is performed using dry air, oxygen atmosphere, inert atmosphere, or the like depending on the desired composition, and a plurality of heating steps are performed as necessary.
[0243] The holding temperature during firing may be adjusted appropriately.
[0244] Specifically, the holding temperature is in the range of 200°C to 1150°C, preferably 300°C to 1050°C, more preferably 500°C to 1000°C, and particularly preferably 650°C to 950°C.
[0245] By setting the calcination temperature to a range of 650°C to 950°C, a lithium nickel composite oxide having particularly high charge and discharge efficiency and excellent cycle characteristics can be produced. The calcination time is preferably set to a total time of 1 to 30 hours from the start of temperature increase to the temperature reached and the end of temperature maintenance. When the total time is less than 30 hours, the volatilization of Li can be prevented, and the degradation of battery performance can be prevented.
[0246] When the total time is 1 hour or longer, the growth of crystals proceeds well, and the battery performance can be improved.
[0247] In addition, the time of holding at the above-mentioned holding temperature can be listed as 0.1 hour to 20 hours, preferably 0.5 hour to 10 hours. The heating rate to the above-mentioned holding temperature is usually 50°C / hour to 400°C / hour, and the cooling rate from the above-mentioned holding temperature to room temperature is usually 10°C / hour to 400°C / hour. In addition, as the atmosphere for sintering, air, oxygen, nitrogen, argon or a mixed gas thereof can be used.
[0248] The lithium mixed metal compound obtained by calcination is pulverized and then appropriately screened to prepare a positive electrode active material for a lithium secondary battery that can be used in a lithium secondary battery.
[0249] <Lithium Secondary Battery>
[0250] Next, while describing the configuration of a lithium secondary battery, a positive electrode using the lithium mixed metal compound produced in this embodiment as a positive electrode active material for a lithium secondary battery and a lithium secondary battery having the positive electrode are described.
[0251] An example of the lithium secondary battery according to the present embodiment includes a positive electrode and a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte solution disposed between the positive electrode and the negative electrode.
[0252] Figure 1A and Figure 1B 1 is a schematic diagram showing an example of a lithium secondary battery according to the present embodiment. A cylindrical lithium secondary battery 10 according to the present embodiment is manufactured as follows.
[0253] First, if Figure 1AAs shown, a pair of strip-shaped separators 1, a strip-shaped positive electrode 2 having a positive electrode lead 21 at one end, and a strip-shaped negative electrode 3 having a negative electrode lead 31 at one end are stacked and wound in the order of separator 1, positive electrode 2, separator 1, and negative electrode 3, thereby forming an electrode group 4.
[0254] Then, if Figure 1B As shown, after the battery can 5 contains the electrode group 4 and the insulator (not shown), the bottom of the can is sealed, and the electrolyte 6 is impregnated into the electrode group 4, and the electrolyte is arranged between the positive electrode 2 and the negative electrode 3. Furthermore, the upper part of the battery can 5 is sealed with the top insulator 7 and the sealing body 8, thereby manufacturing the lithium secondary battery 10.
[0255] Examples of the shape of the electrode group 4 include a shape such as a columnar shape such as a circle, an ellipse, a rectangle, or a rectangle with rounded corners, in which the cross-sectional shape when the electrode group 4 is cut in a direction perpendicular to the winding axis.
[0256] The shape of the lithium secondary battery having the electrode group 4 may be a shape specified in the battery standard IEC60086 or JIS C 8500 established by the International Electrotechnical Commission (IEC). For example, a cylindrical shape, a square shape, etc. may be used.
[0257] In addition, the lithium secondary battery is not limited to the above-mentioned winding type structure, and can also be a stacked structure formed by repeatedly stacking the positive electrode, separator, negative electrode, and separator. As a stacked lithium secondary battery, so-called coin-type batteries, button-type batteries, and paper-type (or sheet-type) batteries can be exemplified.
[0258] Hereinafter, each configuration will be described in sequence.
[0259] (positive electrode)
[0260] The positive electrode of the present embodiment can be manufactured by first preparing a positive electrode mixture including a positive electrode active material, a conductive material, and a binder, and then supporting the positive electrode mixture on a positive electrode current collector.
[0261] (Conductive materials)
[0262] As the conductive material of the positive electrode of the present embodiment, a carbon material can be used. Carbon materials can include graphite powder, carbon black (e.g., acetylene black), fibrous carbon materials, etc. Since carbon black is a particle and has a large surface area, it is possible to improve the conductivity inside the positive electrode by adding a small amount to the positive electrode mixture, thereby improving the charge and discharge efficiency and power characteristics. When too much is added, the bonding force between the positive electrode mixture and the positive electrode collector brought by the binder and the bonding force inside the positive electrode mixture are reduced, which becomes the cause of the increase in internal resistance.
[0263] The ratio of the conductive material in the positive electrode mixture is preferably 5 to 20 parts by mass relative to 100 parts by mass of the positive electrode active material. When a fibrous carbon material such as graphitized carbon fiber or carbon nanotube is used as the conductive material, the ratio may be lowered.
[0264] (Binder)
[0265] As the binder included in the positive electrode of the present embodiment, a thermoplastic resin can be used.
[0266] Examples of the thermoplastic resin include fluorine-containing resins such as polyvinylidene fluoride (hereinafter sometimes referred to as PVdF), polytetrafluoroethylene (hereinafter sometimes referred to as PTFE), tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymers, hexafluoropropylene-vinylidene fluoride copolymers, and tetrafluoroethylene-perfluorovinyl ether copolymers; and polyolefin resins such as polyethylene and polypropylene.
[0267] These thermoplastic resins can be mixed for use. By using fluorine-containing resin and polyolefin resin as binders and making the ratio of fluorine-containing resin to the positive electrode mixture as a whole 1 mass % to 10 mass %, and the ratio of polyolefin resin to the positive electrode mixture as a whole 0.1 mass % to 2 mass %, a positive electrode mixture with high adhesion to the positive electrode collector and high bonding strength inside the positive electrode mixture can be obtained.
[0268] (Positive electrode collector)
[0269] As the positive electrode collector of the positive electrode of this embodiment, a strip-shaped member formed of a metal material such as Al, Ni, stainless steel, etc. can be used. Among them, from the viewpoint of easy processing and low cost, a positive electrode collector formed of Al and processed into a thin film is preferred.
[0270] As a method for making the positive electrode mixture supported on the positive electrode collector, a method of press-molding the positive electrode mixture on the positive electrode collector can be listed. In addition, the positive electrode mixture can be gelatinized using an organic solvent, the paste of the obtained positive electrode mixture is applied to at least one side of the positive electrode collector and dried, and pressed and fixed, thereby making the positive electrode mixture supported on the positive electrode collector.
[0271] When the positive electrode mixture is pasted, the organic solvents that can be used include: amine solvents such as N,N-dimethylaminopropylamine and diethylenetriamine; ether solvents such as tetrahydrofuran; ketone solvents such as methyl ethyl ketone; ester solvents such as methyl acetate; amide solvents such as dimethylacetamide and N-methyl-2-pyrrolidone (hereinafter sometimes referred to as NMP).
[0272] Examples of a method for applying the positive electrode mixture paste to the positive electrode current collector include slot die coating, screen coating, curtain coating, doctor blade coating, gravure coating, and electrostatic spraying.
[0273] The positive electrode can be manufactured by the methods listed above.
[0274] (negative electrode)
[0275] The negative electrode of the lithium secondary battery of this embodiment only needs to be capable of doping and dedoping lithium ions at a lower potential than the positive electrode, and may include an electrode in which a negative electrode mixture containing a negative electrode active material is carried on a negative electrode collector and an electrode consisting solely of a negative electrode active material.
[0276] (Negative electrode active material)
[0277] Examples of the negative electrode active material of the negative electrode include carbon materials, chalcogenides (oxides, sulfides, etc.), nitrides, metals, or alloys that can be doped and dedoped with lithium ions at a potential lower than that of the positive electrode.
[0278] Examples of carbon materials that can be used as the negative electrode active material include graphites such as natural graphite and artificial graphite, cokes, carbon black, pyrolytic carbons, carbon fibers, and calcined products of organic polymer compounds.
[0279] Examples of oxides that can be used as negative electrode active materials include: SiO 2 , SiO, etc., represented by the formula SiOx (where x is a positive real number); TiO 2 , TiO, etc. are represented by the formula TiO x (here, x is a positive real number) represents a titanium oxide; V 2 O 5 , VO 2 Equivalent to VO x (here, x is a positive real number) represents an oxide of vanadium; Fe 3 O 4 , Fe 2 O 3 , FeO, etc. are represented by the formula FeO x (here, x is a positive real number) represents an iron oxide; SnO 2 , SnO, etc. are represented by the formula SnO x (here, x is a positive real number) represents tin oxide; WO 3 , WO 2 By the general formula WO x (here, x is a positive real number) represents tungsten oxide; Li 4 Ti 5 O 12 、LiVO 2 and other composite metal oxides containing lithium and titanium or vanadium.
[0280] Examples of sulfides that can be used as negative electrode active materials include: Ti 2 S 3 、TiS 2 , TiS, etc. are represented by the formula TiS x (here, x is a positive real number) represents titanium sulfide; V 3 S 4 VS 2 , VS, etc. by the formula VS x (here, x is a positive real number) represents a vanadium sulfide; Fe 3 S 4 , FeS 2 , FeS, etc. are represented by the formula FeS x (here, x is a positive real number) represents an iron sulfide; Mo 2 S 3 、MoS 2 Equivalent MoS x (where x is a positive real number) represents molybdenum sulfide; SnS 2 , SnS, etc. are represented by the formula SnS x (here, x is a positive real number) represents tin sulfide; WS 2 WS x (here, x is a positive real number) represents tungsten sulfide; Sb 2 S 3 SbS x (where x is a positive real number) represents antimony sulfide; Se 5 S 3 , SeS 2 , SeS, etc. are represented by the formula SeS x (here, x is a positive real number) represents selenium sulfide.
[0281] Examples of nitrides that can be used as negative electrode active materials include: Li 3 N.Li 3-x A x N (herein, A is either or both of Ni and Co, 0<x<3) or the like lithium-containing nitride.
[0282] These carbon materials, oxides, sulfides, and nitrides may be used alone or in combination of two or more. In addition, these carbon materials, oxides, sulfides, and nitrides may be crystalline or amorphous.
[0283] Examples of metals that can be used as the negative electrode active material include lithium metal, silicon metal, and tin metal.
[0284] Examples of alloys that can be used as negative electrode active materials include: lithium alloys such as Li-Al, Li-Ni, Li-Si, Li-Sn, and Li-Sn-Ni; silicon alloys such as Si-Zn; tin alloys such as Sn-Mn, Sn-Co, Sn-Ni, Sn-Cu, and Sn-La; Cu 2 Sb、La 3 Ni 2 Sn 7 and other alloys.
[0285] These metals and alloys are mainly used alone as electrodes after being processed into foil forms, for example.
[0286] Among the above-mentioned negative electrode active materials, due to the fact that the potential of the negative electrode from the uncharged state to the fully charged state hardly changes (potential flatness is good), the average discharge potential is low, and the capacity retention rate during repeated charge and discharge is high (cycle characteristics are good), it is preferred to use a carbon material with graphite such as natural graphite and artificial graphite as the main component. As the shape of the carbon material, for example, it can be any shape in a flake such as natural graphite, a spherical shape such as mesophase carbon microbeads, a fibrous shape such as graphitized carbon fiber, or an agglomerate of fine powders, etc.
[0287] The negative electrode mixture described above may contain a binder as required. Examples of the binder include thermoplastic resins, and specific examples thereof include PVdF, thermoplastic polyimide, carboxymethyl cellulose, polyethylene, and polypropylene.
[0288] (Negative electrode current collector)
[0289] As the negative electrode current collector of the negative electrode, a strip-shaped component formed of a metal material such as Cu, Ni, stainless steel, etc. can be cited. Among them, from the viewpoint of not easily forming an alloy with lithium and being easy to process, a negative electrode current collector formed of Cu and processed into a thin film is preferred.
[0290] As a method for supporting the negative electrode mixture on such a negative electrode current collector, similarly to the positive electrode, there can be mentioned a method based on pressure molding, a method of making a paste using a solvent or the like, applying the paste on the negative electrode current collector, and pressing and bonding the paste after drying.
[0291] (Diaphragm)
[0292] As the separator of the lithium secondary battery of this embodiment, for example, a material in the form of a porous film, non-woven fabric, woven fabric, etc. formed of a polyolefin resin such as polyethylene or polypropylene, a fluorine-containing resin, a nitrogen-containing aromatic polymer, etc. can be used. In addition, two or more of these materials can be used to form the separator, and these materials can also be stacked to form the separator.
[0293] In this embodiment, the separator has an air permeation resistance of preferably 50 sec / 100 cc to 300 sec / 100 cc, more preferably 50 sec / 100 cc to 200 sec / 100 cc, based on the Gurley method specified in JIS P 8117, in order to allow the electrolyte to permeate well during battery use (charge and discharge).
[0294] The porosity of the separator is preferably 30% to 80% by volume, and more preferably 40% to 70% by volume. The separator may be a laminate of separators having different porosities.
[0295] (Electrolyte)
[0296] The electrolytic solution included in the lithium secondary battery of the present embodiment contains an electrolyte and an organic solvent.
[0297] Examples of the electrolyte contained in the electrolyte solution include LiClO 4 、LiPF 6 、LiAsF 6 、LiSbF 6 , LiBF 4 、LiCF 3 SO 3 、LiN(SO 2 CF 3 ) 2 、LiN(SO 2 C 2 F 5 ) 2 、LiN(SO 2 CF 3 )(COCF 3 )、Li(C 4 F 9 SO 3 )、LiC(SO 2 CF 3 ) 3 , Li 2 B 10 Cl 10 , LiBOB (herein, BOB is bis(oxalato)borate), LiFSI (herein, FSI is bis(fluorosulfonyl)imide), lower aliphatic carboxylic acid lithium salt, LiAlCl 4 The electrolyte preferably uses a lithium salt selected from fluorine-containing LiPF 6 、LiAsF 6 、LiSbF 6 , LiBF 4 、LiCF 3 SO 3 、LiN(SO 2CF 3 ) 2 and LiC(SO 2 CF 3 ) 3 at least one electrolyte.
[0298] In addition, as the organic solvent contained in the above-mentioned electrolyte, for example, the following substances can be used: carbonates such as propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, 4-trifluoromethyl-1,3-dioxolane-2-one, and 1,2-bis(methoxycarbonyloxy)ethane; 1,2-dimethoxyethane, 1,3-dimethoxypropane, pentafluoropropyl methyl ether, 2,2,3,3-tetrafluoropropyl difluoromethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, etc. Ethers such as furan; esters such as methyl formate, methyl acetate, and γ-butyrolactone; nitriles such as acetonitrile and butyronitrile; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; carbamates such as 3-methyl-2-oxazolidinone; sulfur-containing compounds such as cyclopentane, dimethyl sulfoxide, and 1,3-propane sultone; or substances obtained by further introducing fluorine groups into these organic solvents (substances obtained by replacing one or more of the hydrogen atoms possessed by the organic solvent with fluorine atoms).
[0299] As an organic solvent, it is preferred to mix two or more of them for use. Among them, preferably a mixed solvent comprising carbonates, more preferably a mixed solvent of cyclic carbonates and non-cyclic carbonates and a mixed solvent of cyclic carbonates and ethers. As a mixed solvent of cyclic carbonates and non-cyclic carbonates, preferably a mixed solvent comprising ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate. The electrolyte using such a mixed solvent has many characteristics as follows: a wide operating temperature range, even if the charge and discharge at a high current rate is not easy to deteriorate, even if it is used for a long time, it is not easy to degrade, and even if a graphite material such as natural graphite, artificial graphite is used as the active material of the negative electrode, it is difficult to decompose.
[0300] In addition, as the electrolyte, it is preferable to use a liquid electrolyte containing LiPF 6 A mixed solvent containing ethers having fluorine substituents such as pentafluoropropyl methyl ether and 2,2,3,3-tetrafluoropropyl difluoromethyl ether and dimethyl carbonate is more preferred because it has a high capacity retention rate even when charging and discharging at a high current rate.
[0301] Solid electrolytes may be used in place of the above-mentioned electrolytes. As solid electrolytes, for example, organic polymer electrolytes such as polyethylene oxide polymer compounds and polymer compounds containing at least one of polyorganosiloxane chains or polyoxyalkylene chains may be used. In addition, so-called gel-type electrolytes in which a non-aqueous electrolyte is retained in a polymer compound may also be used. In addition, examples of the solid electrolytes include Li 2 S-SiS 2 , Li 2 S-GeS 2 , Li 2 SP 2 S 5 , Li 2 SB 2 S 3 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li 2 SO 4 , Li 2 S-GeS 2 -P 2 S 5 Inorganic solid electrolytes of sulfides such as sulfides may be used as a mixture of two or more of them. By using these solid electrolytes, the safety of lithium secondary batteries can be further improved in some cases.
[0302] In the lithium secondary battery of the present embodiment, when a solid electrolyte is used, the solid electrolyte may also function as a separator. In this case, the separator may not be required.
[0303] Since the positive electrode active material having the above-described structure uses the lithium mixed metal compound produced in the present embodiment described above, the cycle retention rate of the lithium secondary battery using the positive electrode active material can be improved.
[0304] In addition, since the positive electrode having the above-described structure includes the positive electrode active material for a lithium secondary battery having the above-described structure, the cycle retention rate of the lithium secondary battery can be improved.
[0305] Furthermore, since the lithium secondary battery having the above-described structure has the above-described positive electrode, it is a secondary battery having a high cycle retention rate.
[0306] Example
[0307] Next, the present invention will be described in more detail by way of examples.
[0308] <Composition Analysis>
[0309] Regarding the compositional analysis of the obtained precursor powder, the obtained precursor powder was dissolved in hydrochloric acid, and then analyzed using an inductively coupled plasma optical emission spectrometer (manufactured by PerkinElmer, Inc., Optima 7300).
[0310] <Measurement of BET specific surface area>
[0311] The obtained precursor powder was dried at 105 °C for 30 minutes in a nitrogen atmosphere, and then measured using Macsorb (registered trademark) manufactured by Moutech Corporation.
[0312] <Measurement of particle size distribution>
[0313] The cumulative volume particle size distribution of the precursor was measured by the laser diffraction scattering method.
[0314] The particle size distribution measuring device used was Microtrac MT3300EXII manufactured by MicrotracBEL Corporation, and the measurement conditions were carried out according to the conditions shown in Table 1 below. In the obtained cumulative particle size distribution curve, the particle size value at the point where the cumulative volume becomes 10% from the small particle side was set as D10 (μm), the particle size value at the point where it becomes 50% was set as D50 (μm), and the particle size value at the point where it becomes 90% was set as D90 (μm).
[0315] Furthermore, the particle size distribution was measured multiple times, and for the minimum particle size and the maximum particle size, the median values were obtained from the data with a fluctuation error of within 10% for each (n = 5), and the minimum particle size value was set as Dmin (μm) and the maximum particle size value was set as Dmax (μm), respectively.
[0316] The measurement conditions of the particle size distributions of Examples 1 to 4 and Comparative Examples 1 to 3 are shown in Table 1 below.
[0317] Table 1
[0318]
[0319] <Powder X-ray diffraction measurement>
[0320] The powder X-ray diffraction measurement was carried out using an X-ray diffractometer (Ultima IV manufactured by Rigaku Corporation). The precursor powder was filled into a dedicated substrate, and using a Cu-Kα ray source, the measurement was carried out under the conditions of a diffraction angle 2θ = 10° to 90°, a sampling width of 0.03°, and a scanning speed of 20° / minute, and thus a powder X-ray diffraction pattern was obtained.
[0321] The ratio α / β of the half-value width α of the peak at 2θ=52.4±1° and the half-value width β of the peak at 2θ=73.9±1° obtained by analysis using comprehensive powder X-ray analysis software PDXL (manufactured by Rigaku Corporation) was obtained.
[0322] (Example 1)
[0323] First, water was added to a 500 L cylindrical reaction tank equipped with a stirrer having a 220φ propeller type stirring blade and an overflow pipe.
[0324] Next, a 32 mass % sodium hydroxide solution was added until the pH reached 11.8 (when the liquid temperature of the aqueous solution was measured at 40° C.), and the temperature was maintained at 55° C. with a heater.
[0325] Next, nitrogen gas was continuously blown into the reaction tank at a flow rate of 5 L / min to make the atmosphere in the reaction tank an inert atmosphere.
[0326] A nickel sulfate aqueous solution and a cobalt sulfate aqueous solution were mixed so that the atomic ratio of nickel atoms to cobalt atoms was 89:11 to prepare a mixed raw material solution, and the mixed solution was continuously supplied to the reaction tank at a constant rate.
[0327] A 2.8 mol / L ammonium sulfate solution was used as a complexing agent and was continuously supplied to the reaction tank at a fixed rate so that the ammonia concentration in the reaction tank became 0.47 mol / L. Furthermore, 32% by mass sodium hydroxide was intermittently added to maintain the pH of the solution in the reaction tank at 11.8 (measured at a liquid temperature of 40° C. for the aqueous solution).
[0328] The nickel-cobalt composite hydroxide slurry obtained by the above reaction overflows through the overflow pipe.
[0329] The overflowed slurry was introduced into a wet classifier slurry classifier (manufactured by ACO JAPAN Co., Ltd., SS90×250), and the screw of the slurry classifier was rotated at a peripheral speed of 5.8 m / sec to continuously perform classification.
[0330] As the net, a polyamide net having a mesh size of 15 μm was used.
[0331] The particles that did not pass through the mesh of the slurry screener were recovered as the target nickel-cobalt composite hydroxide particles. In addition, the slurry containing the nickel-cobalt composite hydroxide particles that passed through the mesh was appropriately concentrated and continuously refluxed to the reaction tank. In order to make the recovery port side of the target nickel-cobalt composite hydroxide particles higher, the slurry screener was gradually lifted up in an inclined manner of 15°.
[0332] The obtained nickel-cobalt composite hydroxide was washed and dehydrated, dried at 105° C. for 20 hours, sieved, and subjected to particle size distribution measurement, specific surface area measurement, chemical composition analysis, and powder X-ray diffraction measurement.
[0333] (Example 2)
[0334] Water was added to a 500 L cylindrical reaction tank equipped with a stirrer having a 220φ propeller type stirring blade and an overflow pipe.
[0335] Next, a 32 mass % sodium hydroxide solution was added until the pH reached 11.8 (when the liquid temperature of the aqueous solution was measured at 40° C.), and the temperature was maintained at 55° C. with a heater.
[0336] Next, nitrogen gas was continuously blown into the reaction tank at a flow rate of 5 L / min to make the atmosphere in the reaction tank an inert atmosphere.
[0337] A mixed raw material solution was prepared by mixing an aqueous nickel sulfate solution and an aqueous cobalt sulfate solution so that the atomic ratio of nickel atoms to cobalt atoms was 92.5:7.5, and the mixed solution was continuously supplied to a reaction tank at a constant rate.
[0338] A 2.8 mol / L ammonium sulfate solution was used as a complexing agent and was continuously supplied to the reaction tank at a fixed rate so that the ammonia concentration in the reaction tank became 0.47 mol / L. Furthermore, 32% by mass sodium hydroxide was intermittently added to maintain the pH of the solution in the reaction tank at 11.8 (measured at a liquid temperature of 40° C. for the aqueous solution).
[0339] The nickel-cobalt composite hydroxide slurry obtained by the above reaction overflows through the overflow pipe.
[0340] The overflowed slurry was introduced into a wet classifier slurry screener (manufactured by ACO JAPAN Co., Ltd., SS90×250), and the screw of the slurry screener was rotated at a circumferential speed of 5.8 m / s to continuously classify. A polyamide mesh with a mesh size of 15 μm was used. The particles that did not pass through the slurry screener were recovered as the target nickel-cobalt composite hydroxide particles. In addition, the slurry containing the particles of the nickel-cobalt composite hydroxide that passed through the net was appropriately concentrated and continuously refluxed to the reaction tank.
[0341] In order to raise the recovery port side of the target nickel-cobalt composite hydroxide particles, the slurry classifier was gradually raised at an inclination of 15 degrees.
[0342] The obtained nickel-cobalt composite hydroxide was washed and dehydrated, dried at 105° C. for 20 hours, sieved, and subjected to particle size distribution measurement, specific surface area measurement, chemical composition analysis, and powder X-ray diffraction measurement.
[0343] (Example 3)
[0344] Water was added to a 500 L cylindrical reaction tank equipped with a stirrer having a 220φ propeller type stirring blade and an overflow pipe.
[0345] Next, a 32 mass % sodium hydroxide solution was added until the pH reached 11.6 (when measured at a liquid temperature of the aqueous solution of 40° C.), and the temperature was maintained at 45° C. with a heater.
[0346] Next, nitrogen gas was continuously blown into the reaction tank at a flow rate of 5 L / min to make the atmosphere in the reaction tank an inert atmosphere.
[0347] A nickel sulfate aqueous solution and a cobalt sulfate aqueous solution were mixed so that the atomic ratio of nickel atoms to cobalt atoms was 92.5:7.5 to prepare a mixed raw material solution, and the mixed solution was continuously supplied to a reaction tank at a constant rate.
[0348] A 2.8 mol / L ammonium sulfate solution was used as a complexing agent and was continuously supplied to the reaction tank at a fixed rate so that the ammonia concentration in the reaction tank was 0.47 mol / L. The flow rate of the 10.8 mass % aluminum sulfate aqueous solution was adjusted so that the atomic ratio of nickel atoms, cobalt atoms and aluminum atoms was 91.1:7.4:1.5. Furthermore, 32 mass % sodium hydroxide was intermittently added to maintain the pH of the solution in the reaction tank at 11.6 (measured at a liquid temperature of 40° C.).
[0349] The nickel-cobalt-aluminum composite hydroxide slurry obtained by the above reaction overflows through the overflow pipe.
[0350] The overflowed slurry was introduced into a wet classifier slurry screener (manufactured by ACO JAPAN Co., Ltd., SS90×250), and the screw of the slurry screener was rotated at a circumferential speed of 5.8 m / s to continuously classify. The net used was a polyamide net with a mesh size of 15 μm. The particles that did not pass through the net of the slurry screener were recovered as target nickel-cobalt-aluminum composite hydroxide particles. The slurry containing the nickel-cobalt-aluminum composite hydroxide particles that passed through the net was appropriately concentrated and continuously refluxed to the reaction tank.
[0351] In order to raise the recovery port side of the target nickel-cobalt-aluminum composite hydroxide particles, the slurry classifier was gradually raised at an inclination of 15 degrees.
[0352] The obtained nickel-cobalt-aluminum composite hydroxide was washed and dehydrated, dried at 105° C. for 20 hours, sieved, and subjected to particle size distribution measurement, specific surface area measurement, chemical composition analysis, and powder X-ray diffraction measurement. The results are shown in Table 3.
[0353] (Example 4)
[0354] Water was added to a 500 L cylindrical reaction tank equipped with a stirrer having a 220φ propeller type stirring blade and an overflow pipe.
[0355] Next, a 32 mass % sodium hydroxide solution was added until the pH reached 11.2 (when the liquid temperature of the aqueous solution was measured at 40° C.), and the temperature was maintained at 50° C. with a heater.
[0356] Next, nitrogen gas was continuously blown into the reaction tank at a flow rate of 5 L / min to make the atmosphere in the reaction tank an inert atmosphere.
[0357] A mixed raw material solution was prepared by mixing a nickel sulfate aqueous solution and a cobalt sulfate aqueous solution in such a manner that the atomic ratio of nickel atoms to cobalt atoms was 93:7, and the mixed solution was continuously supplied to the reaction tank at a fixed rate. A 2.8 mol / L ammonium sulfate solution was used as a complexing agent, and was continuously supplied to the reaction tank at a fixed rate in such a manner that the ammonia concentration in the reaction tank was 0.29 mol / L. Furthermore, 32% by mass sodium hydroxide was intermittently added to maintain the pH of the solution in the reaction tank at 11.2 (when the liquid temperature of the aqueous solution was 40°C).
[0358] The nickel-cobalt composite hydroxide slurry obtained by the above reaction is stored in a slurry storage tank through an overflow pipe.
[0359] The nickel-cobalt composite hydroxide slurry stored in the slurry storage tank was introduced into a wet classifier hydrocyclone (T-10B-1 model, manufactured by Murata Industries, Ltd.) at a hydrocyclone inlet pressure of 0.04 MPa to classify the nickel-cobalt composite hydroxide into a large particle size fraction and a small particle size fraction.
[0360] The large particle size portion is recovered as particles of the target nickel-cobalt composite hydroxide, and the small particle size portion is continuously returned to the reaction tank as particles of the nickel-cobalt composite hydroxide that do not reach the target particle size.
[0361] Furthermore, the nickel-cobalt composite hydroxide slurry in the slurry storage tank was continuously returned to the reaction tank while being appropriately dehydrated.
[0362] The particles discharged from the bottom of the hydrocyclone were recovered as particles of the target nickel-cobalt composite hydroxide, and the slurry containing the particles of the nickel-cobalt composite hydroxide discharged from the top of the hydrocyclone was continuously refluxed to the reaction tank.
[0363] Furthermore, the nickel-containing cobalt composite hydroxide slurry was appropriately concentrated from the slurry storage tank to the reaction tank, and was continuously refluxed to the reaction tank.
[0364] The obtained nickel-cobalt composite hydroxide was washed and dehydrated, dried at 105° C. for 20 hours, sieved, and subjected to particle size distribution measurement, specific surface area measurement, chemical composition analysis, and powder X-ray diffraction measurement.
[0365] (Comparative Example 1)
[0366] Water was added to a 2000 L cylindrical reaction tank equipped with a stirrer having a 350φ propeller type stirring blade and an overflow pipe.
[0367] Next, 32 mass % sodium hydroxide solution was added until the pH reached 11.9 (measured at a temperature of 40° C. for the aqueous solution), and the temperature was maintained at 45° C. by a heater. Next, nitrogen gas was continuously blown into the reaction tank at a flow rate of 5 L / min to make the atmosphere in the reaction tank an inert atmosphere.
[0368] A nickel sulfate aqueous solution and a cobalt sulfate aqueous solution were mixed so that the atomic ratio of nickel atoms to cobalt atoms was 92.5:7.5 to prepare a mixed raw material solution, and the mixed solution was continuously supplied to a reaction tank at a constant rate.
[0369] A 2.8 mol / L ammonium sulfate solution was used as a complexing agent and was continuously supplied to the reaction tank at a fixed rate so that the ammonia concentration in the reaction tank was 0.47 mol / L. The flow rate of the aluminum sulfate aqueous solution was adjusted so that the atomic ratio of nickel atoms, cobalt atoms, manganese atoms and aluminum atoms was 91.1:7.4:1.5.
[0370] Furthermore, 32% by mass of sodium hydroxide was intermittently added to maintain the pH of the solution in the reaction tank at 11.9 (when measured at a liquid temperature of the aqueous solution of 40° C.).
[0371] The nickel-cobalt composite hydroxide slurry obtained by the above reaction overflows through an overflow pipe, and the overflowed slurry is used as target nickel-cobalt composite hydroxide particles.
[0372] The obtained nickel-cobalt composite hydroxide was washed and dehydrated, dried at 105° C. for 20 hours, sieved, and subjected to particle size distribution measurement, specific surface area measurement, chemical composition analysis, and powder X-ray diffraction measurement.
[0373] (Comparative Example 2)
[0374] Water was added to a 2000 L cylindrical reaction tank equipped with a stirrer having a 350φ propeller type stirring blade and an overflow pipe.
[0375] Next, a 32 mass % sodium hydroxide solution was added until the pH reached 12.3 (when the liquid temperature of the aqueous solution was measured at 40° C.), and the temperature was maintained at 45° C. with a heater.
[0376] Next, nitrogen gas was continuously blown into the reaction tank at a flow rate of 5 L / min to make the atmosphere in the reaction tank an inert atmosphere.
[0377] A nickel sulfate aqueous solution and a cobalt sulfate aqueous solution were mixed so that the atomic ratio of nickel atoms to cobalt atoms was 92.5:7.5 to prepare a mixed raw material solution, and the mixed solution was continuously supplied to a reaction tank at a constant rate.
[0378] A 2.8 mol / L ammonium sulfate solution was used as a complexing agent and was continuously supplied to the reaction tank at a fixed rate so that the ammonia concentration in the reaction tank became 0.41 mol / L.
[0379] The flow rate of the 10.8 mass % aluminum sulfate aqueous solution was adjusted so that the atomic ratio of nickel atoms, cobalt atoms, and aluminum atoms became 91.1:7.4:1.5.
[0380] Furthermore, 32% by mass of sodium hydroxide was intermittently added to maintain the pH of the solution in the reaction tank at 12.3 (when measured at a liquid temperature of the aqueous solution of 40° C.).
[0381] The nickel-cobalt-aluminum composite hydroxide slurry obtained by the above reaction overflowed through an overflow pipe, and the overflowed slurry was recovered as target particles.
[0382] The obtained nickel-cobalt composite hydroxide was washed and dehydrated, dried at 105° C. for 20 hours, sieved, and subjected to particle size distribution measurement, specific surface area measurement, chemical composition analysis, and powder X-ray diffraction measurement.
[0383] (Comparative Example 3)
[0384] Water was added to a 500L cylindrical reaction tank equipped with a stirrer and an overflow pipe. The stirrer had a 220φ propeller type stirring blade. Then, a 32% by mass sodium hydroxide solution was added until the pH reached 11.6 (when the liquid temperature of the aqueous solution was 40°C), and the temperature was maintained at 50°C with a heater. Then, nitrogen gas was continuously blown into the reaction tank at a flow rate of 5L / min to make the atmosphere in the reaction tank an inactive atmosphere.
[0385] A nickel sulfate aqueous solution and a cobalt sulfate aqueous solution were mixed so that the atomic ratio of nickel atoms to cobalt atoms was 93:7 to prepare a mixed raw material solution, and the mixed solution was continuously supplied to a reaction tank at a constant rate.
[0386] A 2.8 mol / L ammonium sulfate solution was used as a complexing agent and was continuously supplied to the reaction tank at a fixed rate so that the ammonia concentration in the reaction tank became 0.41 mol / L.
[0387] Furthermore, 32% by mass of sodium hydroxide was intermittently added to maintain the pH of the solution in the reaction tank at 11.6 (when measured at a liquid temperature of the aqueous solution of 40° C.).
[0388] The nickel-cobalt composite hydroxide slurry obtained by the above reaction is stored in a slurry storage tank through an overflow pipe.
[0389] The nickel-cobalt composite hydroxide slurry stored in the slurry storage tank was introduced into a wet classifier hydrocyclone (T-10B-1 model, manufactured by Murata Industries, Ltd.) at a hydrocyclone inlet pressure of 0.08 MPa to classify the nickel-cobalt composite hydroxide into a large particle size fraction and a small particle size fraction.
[0390] The large particle size fraction was recovered as particles of the target nickel-cobalt composite hydroxide.
[0391] The small particle size fraction continuously flows back to the reaction tank as particles of nickel-cobalt composite hydroxide that do not reach the target particle size. Furthermore, the nickel-cobalt composite hydroxide slurry in the slurry storage tank continuously flows back to the reaction tank while being appropriately dehydrated.
[0392] The obtained nickel-cobalt composite hydroxide was dehydrated, dried at 105° C. for 20 hours, sieved, and subjected to particle size distribution measurement, specific surface area measurement, chemical composition analysis, and powder X-ray diffraction measurement.
[0393] Table 2 shows the production conditions of the precursors of Examples 1 to 4 and Comparative Examples 1 to 3.
[0394] Table 2
[0395]
[0396] The Dmin, D10, D50, D90, Dmax, Dmin / Dmax, (D50-D10) / D50, (D90-D50) / D50, BET value, α, β, α / β, and silicon value as impurity of the precursors of Examples 1 to 4 and Comparative Examples 1 to 3 are recorded in the following Table 3.
[0397]
[0398] As shown in the above results, the content of silicon as an impurity in the precursors of Examples 1 to 4 to which the present invention was applied was as low as less than 130 ppm. In contrast, the content of silicon as an impurity in the precursors of Comparative Examples 1 to 3 to which the present invention was not applied was as high as 130 ppm or more.
[0399] In addition, the precursors of Examples 1 to 3 in which the hydroxide-containing slurry was classified using a net in the classification step had a lower silicon content than the precursors of Comparative Examples 1 to 2 in which such a classification step was not included.
[0400] In addition, regarding the precursor of Example 4 in which a hydrocyclone-type classifier was used in the classification step, the silicon content of the precursor of Example 4 with an inlet pressure of 0.07 MPa or less was lower than that of the precursor of Comparative Example 3. In contrast, the silicon content of the precursor of Comparative Example 3 with an inlet pressure exceeding 0.07 MPa did not decrease.
[0401] Explanation of symbols
[0402] 1 diaphragm, 2 positive electrode, 3 negative electrode, 4 electrode group, 5 battery can, 6 electrolyte, 7 top insulator, 8 sealing body, 10 lithium secondary battery, 21 positive electrode lead, 31 negative electrode lead
Claims
1. A precursor for a positive electrode active material for a lithium secondary battery, comprising at least nickel and satisfying the following formulas (1) and (5), and represented by the following composition formula (A): 0.2≤Dmin / Dmax (1) In formula (1), Dmin is the minimum particle size in μm in the cumulative particle size distribution curve obtained by measuring the precursor of the lithium secondary battery positive electrode active material using a laser diffraction particle size distribution measuring device, and Dmax is the maximum particle size in μm in the cumulative particle size distribution curve obtained by measuring the precursor of the lithium secondary battery positive electrode active material using a laser diffraction particle size distribution measuring device. 0.65≤α / β≤1.45 (5) In formula (5), α is the half-value width of the diffraction peak at 2θ=52.4±1° obtained by X-ray diffraction using CuKα rays, and β is the half-value width of the diffraction peak at 73.9±1° obtained by X-ray diffraction using CuKα rays. Ni 1-x-y Co x M y O z (OH) 2-α (A) In the composition formula (A), 0≤x≤0.45, 0≤y≤0.45, 0≤x+y≤0.9, 0≤z≤3, -0.5≤α≤2, and M is one or more metal elements selected from Zr, Al, Ti, Mn, Ga, In and W. 2 . The precursor for a positive electrode active material for a lithium secondary battery according to claim 1 , wherein in the composition formula (A), 0.01≤x≤0.44, 0.01≤y≤0.44, 0.1≤z≤2.9, and −0.45≤α≤1.
8.
3. The precursor for a positive electrode active material for a lithium secondary battery according to claim 1 or 2, which satisfies the following formula (4): 10μm≤D50≤30μm (4) In formula (4), D50 is the particle size value in μm at the point where the cumulative volume from the small particle side becomes 50% when the whole is set to 100% for the cumulative particle size distribution curve obtained by measuring the precursor for the lithium secondary battery positive electrode active material using a laser diffraction particle size distribution analyzer.
4. The precursor for a positive electrode active material for a lithium secondary battery according to claim 1 or 2, which satisfies the following formulas (2) and (3): (D50-D10) / D50≤0.35 (2) (D90-D50) / D50≤0.50 (3) In formula (2), D10 is the value of the particle size in μm at the point where the cumulative volume from the small particle side becomes 10% when the whole is set to 100% for the cumulative particle size distribution curve obtained by measuring the precursor for the positive active material of a lithium secondary battery by a laser diffraction particle size distribution measuring device, D50 is the value of the particle size in μm at the point where the cumulative volume becomes 50%, and D90 is the value of the particle size in μm at the point where the cumulative volume becomes 90%.
5. The precursor for the positive electrode active material for lithium secondary battery according to claim 4, which satisfies the following formula (3)-5, 0.30<(D90-D50) / D50≤0.50 (3)-5.
6. The precursor for the positive electrode active material for lithium secondary battery according to claim 1 or 2, wherein the BET specific surface area is 2 m 2 / g~80m 2 / g.
7. The precursor for the positive electrode active material for lithium secondary battery according to claim 6, wherein the BET specific surface area is 4 m 2 / g~65m 2 / g.
8. The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to any one of claims 1 to 7, comprising the following steps: a slurry preparation step in which a metal-containing aqueous solution containing at least nickel and an alkaline aqueous solution are supplied to a reaction tank to obtain a hydroxide-containing slurry; and A classification step in which the hydroxide-containing slurry is classified using a net.
9. The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to claim 8, wherein: In the composition formula (A), 0.02≤x≤0.42, 0.02≤y≤0.42, 0.2≤z≤2.8, and -0.4≤α≤1.
6.
10. The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to claim 8 or 9, wherein: The precursor for the positive electrode active material of the lithium secondary battery satisfies the following formula (4)-1: 11μm≤D50≤27μm (4)-1 In formula (4), D50 is the particle size value in μm at the point where the cumulative volume from the small particle side becomes 50% when the whole is set to 100% for the cumulative particle size distribution curve obtained by measuring the precursor for the lithium secondary battery positive electrode active material using a laser diffraction particle size distribution analyzer. 11 . The method for producing a precursor of a positive electrode active material for a lithium secondary battery according to claim 8 , further comprising a reflow step of supplying the slurry after passing through a mesh to the reaction tank.
12. The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to claim 8 or 9, wherein: The material of the net is polymer material.
13. The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to claim 8 or 9, wherein: In the classification step, the classification device includes a rotatable screw inside the fixed net. The classification is performed by rotating the screw at a peripheral speed of 1.0 m / sec to 10.0 m / sec. 14 . The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to claim 8 , further comprising a heating step, wherein heating is performed at a temperature range of 300° C. to 900° C. in an oxygen-containing atmosphere.
15. The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to any one of claims 1 to 7, comprising the following steps: a slurry preparation step in which a metal-containing aqueous solution containing at least nickel and an alkaline aqueous solution are supplied to a reaction tank to obtain a hydroxide-containing slurry; and a classification step, in which the hydroxide-containing slurry is classified by a hydrocyclone classification device, in, The classification step is carried out under the condition that the inlet pressure of the classification device is 0.01 MPa to 0.07 MPa.
16. The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to claim 15, wherein: In the composition formula (A), 0.03≤x≤0.40, 0.03≤y≤0.40, 0.3≤z≤2.7, and -0.35≤α≤1.
4.
17. The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to claim 15 or 16, wherein: The precursor for the positive electrode active material of the lithium secondary battery satisfies the following formula (4)-2: 12μm≤D50≤25μm (4)-2 In formula (4), D50 is the particle size value in μm at the point where the cumulative volume from the small particle side becomes 50% when the whole is set to 100% for the cumulative particle size distribution curve obtained by measuring the precursor for the lithium secondary battery positive electrode active material using a laser diffraction particle size distribution analyzer. 18 . The method for producing a precursor for a positive electrode active material for a lithium secondary battery according to claim 15 , further comprising a heating step, wherein heating is performed at a temperature ranging from 300° C. to 900° C. in an oxygen-containing atmosphere.
19. A method for producing a lithium composite metal compound, comprising the following steps: a mixing step of mixing the precursor obtained by the method for producing a precursor for a positive electrode active material for a lithium secondary battery according to any one of claims 8 to 18 and a lithium compound; and The calcining step is to calcine the obtained mixture at a temperature of 500° C. to 1000° C. in an oxygen-containing atmosphere.