Lithium secondary battery positive electrode active material, preparation method thereof and lithium secondary battery containing the same

By using lithium nickel cobalt manganese oxide and nano-sized metal oxide particles in the positive electrode active material of lithium secondary battery, combined with the core-shell concentration gradient structure, the problem of insufficient resistance and capacity at high temperature is solved, and low resistance and high resistance are achieved Capacity performance improvement.

CN113169332BActive Publication Date: 2024-11-29POSCO HLDG INC +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN201980078894.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-09-27
Publication Date
2024-11-29
Estimated Expiration
2039-09-27

AI Technical Summary

Technical Problem

Existing lithium secondary battery positive electrode active materials show problems of high initial resistance and insufficient discharge capacity at high temperatures, especially high-content nickel positive electrode active materials are prone to increased resistance and reduced structural safety in the early stage of discharge.

Method used

Lithium nickel cobalt manganese oxide is used as the positive electrode active material, which contains nano-sized metal oxide particles, and improves resistance and capacity performance through core-shell concentration gradient structure and doping metal oxides. The specific steps include before preparing hydroxide Body particles, calcination, porous oxide precursors are prepared, mixed with metal oxides and secondary calcination is performed to form a positive electrode active material with excellent structure.

Benefits of technology

It realizes low initial resistance and excellent discharge capacity at high temperatures, improves charge and discharge cycle performance and thermal safety, and is suitable for the application of high-content nickel positive electrode active materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113169332B_ABST
    Figure CN113169332B_ABST
Patent Text Reader

Abstract

The present invention relates to a lithium secondary battery positive electrode active material, a preparation method thereof and a lithium secondary battery containing the same, wherein the positive electrode active material comprises: a lithium nickel cobalt manganese oxide, which comprises secondary particles formed by agglomeration of at least one primary particle and is represented by the following chemical formula 1; and metal oxide particles, which are located inside the secondary particles and have an average particle size (D50) of nanometer size. [Chemical formula 1] Li a [Ni x Co y Mn z ] t M 1‑t O 2‑p X p In the above Chemical Formula 1, the definition of each substituent is the same as that in the Summary of the Invention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a lithium secondary battery positive electrode active material, a preparation method thereof and a lithium secondary battery containing the same. Background Art

[0002] In recent years, with the explosive growth in demand for IT mobile devices and small electric drive devices (electric bicycles, small electric vehicles, etc.) and the increasing demand for electric vehicles with a mileage of more than 400 km, research and development of secondary batteries with high capacity and high energy density are actively carried out worldwide. In order to prepare such high-capacity batteries, high-capacity positive electrode active materials are required.

[0003] Among the existing layered positive electrode active materials, the material with the highest capacity is LiNiO2 (275 mAh / g), but it is prone to structural collapse during charging and discharging, and the thermal stability caused by the oxidation number problem is low, so it is actually difficult to commercialize. Therefore, in order to solve such problems, by replacing unstable Ni sites with other stable transition metals (Co, Mn, etc.), a ternary NCM system active material (containing Li, Ni, Co and Mn) substituted with Co and Mn has been developed. However, for this ternary NCM system active material, the more the Ni content increases, the more it is necessary to use various doping additives to ensure structural safety, in which case the capacity may decrease. In addition, the more the Ni content increases, the more resistance increases at the beginning of discharge. Summary of the invention

[0004] Technical issues

[0005] One embodiment is directed to providing a lithium secondary battery positive electrode active material that exhibits low initial resistance at high temperatures and exhibits excellent discharge capacity.

[0006] Another embodiment aims to provide a method for preparing the positive electrode active material of the lithium secondary battery.

[0007] Yet another embodiment is directed to providing a lithium secondary battery including the positive electrode active material.

[0008] Technical Solution

[0009] According to one embodiment, a lithium secondary battery positive electrode active material is provided, which includes: a lithium nickel cobalt manganese oxide, which includes secondary particles in which one or more primary particles are agglomerated and is represented by the following chemical formula 1; and metal oxide particles, which are located inside the secondary particles and have an average particle size (D50) of nanometer size.

[0010] [Chemical formula 1]

[0011] Lia [Ni x Co y Mn z ] t M 1-t O 2-p X p

[0012] In the above chemical formula 1,

[0013] M is any one element selected from the group consisting of Al, Mg, Sn, Ca, Ge, Ga, B, Ti, Mo, Nb and W,

[0014] X is any one element selected from the group consisting of F, N and P,

[0015] a is 0.8≤a≤1.3,

[0016] 0.6≤x≤0.95,0 <y≤0.2,0<z≤0.2,x+y+z=1,0≤t≤1,0≤p≤0.1。

[0017] In one embodiment, 0.8≤x≤0.95, 0 <y≤0.1,0<z≤0.1。

[0018] The metal oxide may be one or more selected from the group consisting of ZrO2, WO3, CeO2, TiO2, HfO2, Co3O4, La2O3, BaO, SrO and combinations thereof.

[0019] The metal oxide may have an average particle size (D50) of 50 nm to 800 nm.

[0020] The metal content of the metal oxide may be 0.1 wt % to 0.7 wt % relative to 100 wt % of the positive electrode active material.

[0021] In one embodiment, the secondary particles may include: an inner core portion, which is a region having a constant molar content of nickel; and an outer shell portion, which surrounds the outer surface of the inner core portion and has a concentration gradient (gradient) in which the molar content of nickel decreases along the direction from the interface with the inner core portion to the outermost portion.

[0022] A coating layer may also be included on the surface of the secondary particles.

[0023] According to another embodiment, a method for preparing a positive electrode active material for a lithium secondary battery is provided, which includes: a step of preparing hydroxide precursor particles containing nickel, cobalt and manganese; a step of calcining the hydroxide precursor particles once to prepare porous oxide precursor particles; a step of mixing the oxide precursor particles and a metal oxide to prepare a primary mixture; a step of mixing the primary mixture and a lithium raw material to prepare a secondary mixture; and a step of calcining the secondary mixture for a second time.

[0024] The primary calcination may be carried out by heating to 400°C to 800°C at a temperature increase of 1.0°C / min to 5.0°C / min and maintaining for 3 to 20 hours. In addition, the primary calcination may be carried out by introducing air or oxygen at a rate of 10 ml / min to 50 liters / min.

[0025] In the step of mixing the oxide precursor and the metal oxide to prepare a primary mixture, a doping raw material substance may be further mixed.

[0026] Yet another embodiment provides a lithium secondary battery including: a positive electrode including the positive electrode active material; a negative electrode; and a nonaqueous electrolyte.

[0027] Effects of the Invention

[0028] According to an embodiment of the present invention, a positive electrode active material for a lithium secondary battery may exhibit low initial resistance at high temperatures and exhibit excellent discharge capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is a schematic structural diagram of a lithium secondary battery according to one embodiment.

[0030] Figure 2 is a surface SEM image of the hydroxide precursor prepared according to Preparation Example 1.

[0031] Figure 3 3 is a surface SEM image of the porous oxide precursor prepared according to Preparation Example 3.

[0032] Figure 4 This is a cross-sectional EDS measurement image of the positive electrode active material prepared according to Example 1.

[0033] Figure 5 This is a cross-sectional EDS measurement image of the positive electrode active material prepared according to Comparative Example 1. DETAILED DESCRIPTION

[0034] Hereinafter, embodiments of the present invention will be described in detail. However, the following embodiments are merely provided as examples, and the present invention is not limited to the following embodiments. The present invention is defined by the scope of the claims.

[0035] The positive electrode active material of a lithium secondary battery according to an embodiment includes: a lithium nickel cobalt manganese-based oxide, which includes secondary particles aggregated from at least one primary particle and is represented by the following Chemical Formula 1; and metal oxide particles, which are located inside the secondary particles and have an average particle size (D50) in the nanometer size range.

[0036] [Chemical Formula 1]

[0037] Li a [Ni x Co y Mn z t M 1-t O 2-p X p

[0038] In the above Chemical Formula 1,

[0039] M is any one element selected from the group consisting of Al, Mg, Sn, Ca, Ge, Ga, B, Ti, Mo, Nb, and W, and X is any one element selected from the group consisting of F, N, and P.

[0040] In addition, a is 0.8 ≤ a ≤ 1.3, 0.6 ≤ x ≤ 0.95, 0 < y ≤ 0.2, 0 < z ≤ 0.2, x + y + z = 1, 0 ≤ t ≤ 1, 0 ≤ p ≤ 0.1. Additionally, it can also be 0.8 ≤ x ≤ 0.95, 0 < y ≤ 0.1, 0 < z ≤ 0.1.

[0041] The metal oxide may be one or more selected from the group consisting of ZrO2, WO3, CeO2, TiO2, HfO2, Co3O4, La2O3, BaO, SrO, and combinations thereof.

[0042] ​The metal oxide may have an average particle size (D50) of 50nm to 800nm, and when the average particle size (D50) of the metal oxide falls within the range, the metal oxide may exhibit the advantage of being able to be embedded in the interior of the secondary particles. If the average particle size (D50) of the metal oxide is less than 50nm, there is a problem of low possibility of embedding in the interior of the secondary particles due to the agglomeration phenomenon of the metal oxide. In addition, if the average particle size (D50) of the metal oxide is greater than 600nm, there is a problem of reduced possibility of embedding in the interior of the secondary particles due to the oxide particles being larger than the pore size of the secondary particles. Unless otherwise defined in this specification, the average particle diameter (D50) refers to the diameter of 50% by volume of the particles.

[0043] As described above, according to the positive electrode active material of one embodiment, it contains metal oxides such as ZrO2 in the form of particles inside the secondary particles, especially metal oxides with an average particle size (D50) of nanometer size, so the initial resistance at high temperature is reduced, and an improved discharge capacity can be exhibited. In particular, this effect brought about by the inclusion of metal oxide particles with an average particle size (D50) of nanometer size can more effectively solve the problems of increased resistance and reduced structural safety when there is a possibility of an initial discharge that is more serious than that of a high-content nickel positive electrode active material, so it is very suitable. At this time, the high-content nickel positive electrode active material refers to a positive electrode active material as represented by the above chemical formula 1, which contains Ni, Co and Mn as main components, and Ni is 60 mol% or more or 80 mol% or more relative to the total 100 mol% of Ni, Co and Mn.

[0044] If the metal does not exist in the form of an oxide but exists in the form of being doped into an active material, that is, exists alone in the form of particles, it will be embedded in the metal site structure of the lithium nickel cobalt manganese oxide represented by the above chemical formula 1, so the charge and discharge capacity will decrease. In addition, the initial resistance at high temperature increases, and there may also be a problem of decreased charge and discharge efficiency.

[0045] The metal content of the metal oxide may be 0.1 wt % to 0.7 wt % relative to 100 wt % of the positive electrode active material. When the metal content of the metal oxide falls within the range, the initial discharge capacity can be more effectively increased and the initial discharge direct current internal resistance (DC-IR) can be more effectively reduced.

[0046] In one embodiment, the secondary particles may include: a core portion, which is a region with a constant molar content of nickel; and a shell portion, which surrounds the outer surface of the core portion, and there is a concentration gradient (gradient) in which the molar content of nickel decreases along the direction from the interface with the core portion to the outermost portion. That is, there is a core-shell concentration gradient (Core-Shell Gradient, "CSG"). As described above, when the primary particle has a core-shell concentration gradient, a higher nickel content is maintained in the core portion, so that a high capacity based on a high content of nickel can be obtained, while the content of nickel in the shell portion decreases. Therefore, in the shell portion, the content of Mn, Co and optionally M other than nickel is increased, so that the structural stability of the positive electrode active material can be further improved.

[0047] As a result, the positive electrode active material comprises secondary particles of agglomerated primary particles, and the secondary particles comprise a core represented by the following chemical formula 1a and an outer shell represented by the following chemical formula 1b. At this time, in the core, the molar content of nickel, i.e., x in the above chemical formula 1, is 0.6 or more, and is constantly maintained at 60 mol% or more relative to the total 100 mol% of nickel, cobalt and manganese in the metal elements constituting the positive electrode active material, while in the outer shell, the molar content of nickel decreases along the direction from the interface with the core to the outermost periphery. Therefore, the positive electrode active material as a whole has the components of the above chemical formula 1, and the core and the outer shell have the components of the following chemical formulas 1a and 1b, respectively, satisfying the conditions that the core has a constant molar content of Ni and the outer shell has a decreasing molar content of nickel.

[0048] [Chemical formula 1a]

[0049] Li a1 [Ni x1 Co y1 Mn z1 ] t1 M 1-t1 O 2-p1 X p1

[0050] In the above chemical formula 1a,

[0051] M is any one element selected from the group consisting of Al, Mg, Sn, Ca, Ge, Ga, B, Ti, Mo, Nb and W, X is any one element selected from the group consisting of F, N and P,

[0052] a1 is 0.8≤a≤1.3, 0.6≤x1≤1.0, 0 <y1≤0.2,0<z1≤0.2,x1+y1+z1=1,0≤t1≤1,0≤p1≤0.1。

[0053] [Chemical formula 1b]

[0054] Li a2 [Ni x2 Co y2 Mn z2 ] t2 M 1-t2 O 2-p2 X p2

[0055] In the above chemical formula 1b,

[0056] M is any one element selected from the group consisting of Al, Mg, Sn, Ca, Ge, Ga, B, Ti, Mo, Nb and W, X is any one element selected from the group consisting of F, N and P,

[0057] a2 is 0.8≤a≤1.3, 0.4≤x2≤0.9, 0 <y2≤0.2,0<z2≤0.2,x2+y2+z2=1,0≤t2≤1,0≤p2≤0.1。

[0058] The positive electrode active material having such a structure has a constant molar content of nickel in the core, especially a high content, so that a high capacity based on a high content of nickel can be achieved. In addition, the content of nickel is reduced in the outer shell, and the content of cobalt, manganese and M other than nickel is increased, so that the structure of the positive electrode active material can be stabilized. At the same time, since the secondary particles contain metal oxides such as ZrO2, the effect of reducing resistance and increasing capacity during initial discharge can be further improved.

[0059] For the concentration gradient, the ratio of the nickel molar content at the outermost periphery to the nickel molar content at the interface with the inner core is preferably 0.6 to 0.95. When the nickel concentration gradient satisfies the conditions, the capacity of the positive electrode active material can be further increased, and the charge-discharge cycle performance and thermal safety can be further improved through the structural stability of the surface portion of the positive electrode active material.

[0060] In the secondary particles of the positive electrode active material, an average particle size (D50) of the inner core may be 60% to 90% relative to 100% of an overall average particle size (D50) of the secondary particles of the positive electrode active material.

[0061] The positive electrode active material comprises secondary particles of agglomerated primary particles (agglomerated primary particles of more than one), and the average particle size (D50) of the secondary particles may be 7 μm to 20 μm. When the average particle size (D50) of the secondary particles falls within the range, the packing density can be further increased, so it is more suitable. The average particle size (D50) of the primary particles is smaller than that of the secondary particles, and can be appropriately adjusted without special restrictions.

[0062] In addition, the positive electrode active material may be composed only of secondary particles having the average particle size (D50), or may be a bimodal form in which large-size particles and small-size particles are mixed. When the positive electrode active material is in a bimodal form, the large-size particles may have an average particle size (D50) of 10 μm to 20 μm, and the small-size particles may have an average particle size (D50) of 3 μm to 7 μm. At this time, for the large-size particles and the small-size particles, of course, they may also be in the form of secondary particles agglomerated by at least one primary particle. In addition, the mixing ratio of large-size particles and small-size particles is based on the overall 100 weight %, and the large-size particles may be 50 to 80 weight %. Due to this bimodal particle distribution, energy density can be improved.

[0063] In one embodiment, a coating layer may be further included on the surface of the secondary particles of the positive electrode active material. The coating layer may include boron, boron oxide, lithium boron oxide, or a combination thereof. However, this is only an example, and various coating materials for positive electrode active materials may be used. The content and thickness of the coating layer may be appropriately adjusted without particular limitation.

[0064] In one embodiment, a method for preparing a positive electrode active material for a lithium secondary battery is provided, which comprises: a step of preparing hydroxide precursor particles containing nickel, cobalt and manganese; a step of calcining the hydroxide precursor particles once to prepare porous oxide precursor particles; a step of mixing the oxide precursor particles and a metal oxide to prepare a primary mixture; a step of mixing the primary mixture and a lithium raw material to prepare a secondary mixture; and a step of calcining the secondary mixture for a second time.

[0065] Hereinafter, the method for preparing the positive electrode active material is described in further detail.

[0066] First, hydroxide precursor particles containing nickel, cobalt, and manganese are prepared.

[0067] The hydroxide precursor particles can be prepared by mixing a nickel raw material, a cobalt raw material, a manganese raw material and a solvent, coprecipitating the mixture, and then drying. The amounts of the nickel raw material, the cobalt raw material and the manganese raw material can be adjusted to a suitable molar ratio according to the compounds of the desired components, and the overall metal concentration of nickel, cobalt and manganese in the mixture can be 1M to 3M.

[0068] The nickel raw material may be nickel hydroxide, nickel carbonate, nickel nitrate, nickel sulfate, hydrates thereof or combinations thereof, and the cobalt raw material may be Co(OH)2, Co3O4, CoO, Co(SO4), hydrates thereof or combinations thereof. In addition, the manganese raw material may be manganese hydroxide, manganese carbonate, manganese nitrate, manganese sulfate, hydrates thereof or combinations thereof.

[0069] The solvent can use water, such as deionized water or distilled water. In the coprecipitation process, a chelating agent and a pH adjusting agent can also be used. As the chelating agent, NH4(OH), NH2CH2CH2NH2 or a combination thereof can be used. In addition, the pH adjusting agent can use a base such as NaOH or ammonia to adjust the pH to 10.0 to 12.0. When the chelating agent and the pH adjusting agent are used, there is no need to particularly limit the supply speed, for example, they can be supplied at a supply speed of 0.05 liters / hour to 0.5 liters / hour, respectively.

[0070] For the coprecipitation process, it can be implemented under the condition of supplying an inert gas such as nitrogen (N2) to remove dissolved oxygen to prevent oxidation of Ni. For nitrogen supply, as long as it is a supply speed suitable for removing dissolved oxygen, there is no need for special restrictions, for example, it can be supplied at a supply speed of 1 liter / minute to 4 liters / minute. In addition, for the coprecipitation process, it can be implemented at 30°C to 60°C, and can be stirred at a speed of 120rpm to 160rpm, but the temperature and stirring speed do not need to be limited thereto.

[0071] In addition, the drying process may be performed at a temperature of 80°C to 120°C.

[0072] For the coprecipitation process, a first metal salt solution and a second metal salt solution are prepared respectively, wherein the first metal salt solution and the second metal salt solution contain a nickel raw material, a cobalt raw material, a manganese raw material and a solvent, and the molar concentration of the nickel raw material is different. Then, a first coprecipitation step is performed, and the first metal salt solution is supplied at a constant concentration to a reactor in which the pH is kept constant and a chelating agent is supplied to form a core portion. After the first coprecipitation step, a second coprecipitation step may also be performed, and the supply rate of the first metal salt aqueous solution is gradually reduced, while the supply rate of the second metal salt aqueous solution is gradually increased to form a shell portion surrounding the outer surface of the core portion. When the coprecipitation process is performed by the first coprecipitation step and the second coprecipitation step, hydroxide precursor particles may be formed, which contain: a core portion, which contains nickel, cobalt and manganese, and the core portion is a region with a constant molar content of nickel; and a shell portion, which surrounds the outer surface of the core portion, and there is a concentration gradient in which the molar content of nickel decreases along the direction from the interface with the core portion to the outermost periphery.

[0073] The supply of the first metal salt aqueous solution can be implemented as follows: start supplying at a rate of 0.5 to 1.0 L / hour and gradually reduce to 0.05 to 0.5 L / hour. The supply of the second metal salt aqueous solution can be implemented at a rate of 0.5 to 1.0 L / hour.

[0074] Next, the hydroxide precursor particles are subjected to a primary calcination to prepare porous oxide precursor particles. The primary calcination process may be carried out by heating to 400° C. to 800° C. at a temperature increase of 1.0° C. / min to 5.0° C. / min and maintaining the temperature for 3 to 20 hours. In addition, the primary calcination may be carried out while introducing air or oxygen at a rate of 10 ml / min to 50 liters / min.

[0075] When the primary calcination process is carried out under the conditions, the hydroxide precursor is converted into an oxide precursor, thereby preparing a porous oxide precursor with pores formed on the surface. The pores are spaces where the metal oxide is embedded in the subsequent mixing process with the metal oxide, and due to the formation of such pores, the metal oxide can remain in the final active material in the form of particles.

[0076] If the temperature rise condition of the primary calcination process is slower or faster than the range, or the temperature is kept lower or higher, or the holding time is shorter than the time, pores may not be formed on the surface. This is because the oxidation reaction of the hydroxide precursor Me(OH)2(s)→MeO(s)+H2O(g) is not completed, that is, the generated H2O is volatilized, so that the process of forming pores does not occur.

[0077] The oxide precursor particles and the metal oxide are mixed to prepare a primary mixture. At this time, the metal oxide is embedded in the pores formed on the surface of the oxide precursor particles. The metal oxide can be ZrO2, WO3, CeO2, TiO2, HfO2, Co3O4, La2O3, BaO, SrO or a combination thereof.

[0078] In the step of mixing the oxide precursor and the metal oxide to prepare a primary mixture, a doping raw material may be further mixed. The doping raw material is a compound containing any one element selected from the group consisting of Al, Mg, Sn, Ca, Ge, Ga, B, Ti, Mo, Nb and W, and may be a hydroxide, carbonate, nitrate, sulfate, a hydrate thereof or a combination thereof.

[0079] The obtained primary mixture is mixed with a lithium raw material to prepare a secondary mixture. The lithium raw material may be lithium hydroxide, lithium carbonate, lithium nitrate, lithium sulfate, hydrates thereof or a combination thereof.

[0080] As described above, before the precursor and the lithium raw material are mixed, a process of mixing the metal oxide is implemented, so that most of the metal oxide can be located in the pores formed on the surface of the oxide precursor particles. After the pores are filled with the metal oxide, they are mixed with the lithium raw material to form a secondary mixture having a structure in which the metal oxide is covered by the lithium raw material.

[0081] Next, the secondary mixture is subjected to secondary calcination to prepare a positive electrode active material for a lithium secondary battery. The secondary calcination process can be implemented by heating to 700°C to 900°C at a temperature increase of 1.0°C / min to 5.0°C / min and maintaining for 10 hours to 24 hours and a cooling process. In addition, the secondary calcination can be implemented by introducing air or oxygen at a rate of 10 ml / min to 50 liters / min.

[0082] After the secondary calcination process is performed, a coating layer may be further formed. For the coating layer formation process, the product of the secondary calcination process and the coating raw material are mixed and then heat treated. The coating raw material may be boron, boron oxide, H3BO3, lithium boron oxide, or a combination thereof. For the heat treatment process, the temperature may be 300°C to 500°C for 5 to 10 hours.

[0083] Despite the secondary calcination process and the selective further coating process, the metal oxide is located in the pores formed on the surface of the oxide precursor particles and is covered with the lithium raw material, so the metal oxide in the final positive electrode active material can maintain the metal oxide particle form.

[0084] Yet another embodiment provides a lithium secondary battery including: a positive electrode; a negative electrode; and a non-aqueous electrolyte, the positive electrode including the aforementioned positive electrode active material according to one embodiment.

[0085] The positive electrode includes a positive electrode active material layer on a positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, and the positive electrode active material may include the aforementioned positive electrode active material for a lithium secondary battery according to one embodiment.

[0086] In the positive electrode active material layer, the positive electrode active material may be included in an amount of 90 wt % to 98 wt % relative to the total weight of the positive electrode active material layer.

[0087] In one embodiment, the positive electrode active material layer may further include a binder and a conductive material, and the contents of the binder and the conductive material may be 1 wt % to 5 wt % respectively relative to the total weight of the positive electrode active material layer.

[0088] The binder plays a role in making the positive electrode active material particles adhere well to each other and to the positive electrode active material adhere well to the collector. Typical examples of the binder may include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylated styrene butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.

[0089] The conductive material is used to impart conductivity to the electrode, and any conductive material can be used as long as it does not cause chemical changes in the composed battery. The conductive material can be, for example, a conductive material including carbon materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal materials such as metal powders or metal fibers such as copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives, etc.; or a mixture thereof.

[0090] As the positive electrode current collector, aluminum foil, nickel foil, or a combination thereof may be used, but is not limited thereto.

[0091] The negative electrode comprises a negative electrode current collector and a negative electrode active material layer located on the current collector. The negative electrode active material layer comprises a negative electrode active material.

[0092] As the negative electrode active material, a material capable of reversibly inserting / deinserting lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide may be used.

[0093] The material capable of reversibly embedding / de-embedding lithium ions may be, for example, a carbon material, i.e., a carbon-based negative electrode active material commonly used in lithium secondary batteries. Typical examples of carbon-based negative electrode active materials may be crystalline carbon, amorphous carbon, or a combination thereof. As examples of the crystalline carbon, graphite such as amorphous, plate-like, flake-like, spherical or fibrous natural graphite or artificial graphite may be cited, and as examples of the amorphous carbon, soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc. may be cited.

[0094] As the alloy of the lithium metal, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn can be used.

[0095] Examples of the material capable of lithium doping and de-doping include Si, SiOx (0 < x < 2), Si-Q alloy (where Q is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Si-carbon composite, Sn, SnO2, Sn-R (where R is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), Sn-carbon composite, etc. At least one of them can also be used in combination with SiO2. As the elements Q and R, elements selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, and their combinations can be used.

[0096] As the transition metal oxide, lithium titanate oxide can be used.

[0097] In the negative electrode active material layer, the content of the negative electrode active material can be 95% to 99% by weight based on the total weight of the negative electrode active material layer.

[0098] The negative electrode active material layer contains a negative electrode active material and a binder, and may also selectively contain a conductive material.

[0099] In the negative electrode active material layer, the content of the negative electrode active material can be 95% to 99% by weight based on the total weight of the negative electrode active material layer. In the negative electrode active material layer, the content of the binder can be 1% to 5% by weight based on the total weight of the negative electrode active material layer. In addition, when a conductive material is further contained, the negative electrode active material can be 90% to 98% by weight, the binder can be 1% to 5% by weight, and the conductive material can be 1% to 5% by weight.

[0100] The binder serves to bond the negative electrode active material particles well to each other and to bond the negative electrode active material well to the current collector. As the binder, a water-insoluble binder, a water-soluble binder, or a combination thereof can be used.

[0101] The water-insoluble binder may be polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, a polymer containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyimide or a combination thereof.

[0102] The water-soluble binder may be styrene-butadiene rubber, acrylated styrene-butadiene rubber, polyvinyl alcohol, sodium polyacrylate, a copolymer of propylene and an olefin having 2 to 8 carbon atoms, a copolymer of (meth)acrylic acid and an alkyl (meth)acrylate, or a combination thereof.

[0103] When a water-soluble binder is used as the negative electrode binder, a cellulose series compound capable of imparting viscosity may also be included as a thickener. As the cellulose series compound, one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose or their alkali metal salts may be mixed and used. As the alkali metal, Na, K or Li may be used. The thickener may be used in an amount of 0.1 to 3 parts by weight relative to 100 parts by weight of the negative electrode active material.

[0104] The conductive material is used to impart conductivity to the electrode, and any conductive material can be used as long as it does not cause chemical changes in the composed battery. The conductive material can be, for example, a conductive material including carbon materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, Denka black, carbon fiber, etc.; metal materials such as metal powders or metal fibers such as copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives, etc.; or a mixture thereof.

[0105] As the negative electrode current collector, a material selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer material coated with a conductive metal, and a combination thereof may be used.

[0106] The nonaqueous electrolyte includes a nonaqueous organic solvent and a lithium salt.

[0107] The non-aqueous organic solvent functions as a medium through which ions participating in the electrochemical reaction of the battery can migrate.

[0108] As the non-aqueous organic solvent, carbonic acid, esters, ethers, ketones, alcohols or aprotic organic solvents can be used. As the carbonic acid solvent, dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) etc. can be used, as the ester solvent, methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, caprolactone etc. can be used. As the ether solvent, dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran etc. can be used, as the ketone solvent, cyclohexanone etc. can be used. In addition, as the alcohol solvent, ethanol, isopropanol, etc. can be used, and as the aprotic solvent, nitriles such as R-CN (R is a linear, branched or cyclic hydrocarbon group with 2 to 20 carbon atoms, which may contain a double-bonded aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, sulfolanes, etc. can be used.

[0109] The non-aqueous organic solvent may be used alone or as a mixture of more than one kind. The mixing ratio when more than one kind is used in a mixture may be appropriately adjusted according to the desired battery performance, which is well known to those skilled in the art.

[0110] In addition, for the carbonic acid solvent, it is preferred to use a mixture of a cyclic carbonate and a chain carbonate. In this case, when the cyclic carbonate and the chain carbonate are used in a volume ratio of 1:1 to 1:9, excellent electrolyte performance can be exhibited.

[0111] The non-aqueous organic solvent may include an aromatic hydrocarbon organic solvent in addition to the carbonic acid solvent. In this case, the carbonic acid solvent and the aromatic hydrocarbon organic solvent may be mixed in a volume ratio of 1:1 to 30:1.

[0112] As the aromatic hydrocarbon organic solvent, an aromatic hydrocarbon compound represented by the following Chemical Formula 2 may be used.

[0113] [Chemical formula 2]

[0114]

[0115] In Chemical Formula 2, R1 to R6 are the same or different and are selected from hydrogen, halogen, an alkyl group having 1 to 10 carbon atoms, a haloalkyl group, and a combination thereof.

[0116] Specific examples of aromatic organic solvents are selected from benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, , 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene and combinations thereof.

[0117] The non-aqueous electrolyte may further include vinylene carbonate or an ethylene carbonate-based compound of the following Chemical Formula 3 to improve battery life.

[0118] [Chemical formula 3]

[0119]

[0120] In Chemical Formula 3, R7 and R8 are the same or different and are selected from hydrogen, a halogen group, a cyano group (CN), a nitro group (NO2) and a fluorinated alkyl group having 1 to 5 carbon atoms, and at least one of R7 and R8 is selected from a halogen group, a cyano group (CN), a nitro group (NO2) and a fluorinated alkyl group having 1 to 5 carbon atoms, but R7 and R8 are not both hydrogen.

[0121] Typical examples of ethylene carbonate compounds include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, and fluoroethylene carbonate, etc. When such a life-improving additive is further used, its usage amount can be appropriately adjusted.

[0122] Lithium salt is a material that plays the following role. It is dissolved in an organic solvent and acts as a lithium ion source in the battery to ensure the basic operation of the lithium secondary battery and promote the migration of lithium ions between the positive electrode and the negative electrode. Typical examples of such lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are natural numbers), one or more of LiCl, LiI and LiB(C2O4)2 (lithium bis(oxalato)borate; LiBOB). The concentration of the lithium salt is preferably in the range of 0.1 to 2.0 M. When the concentration of the lithium salt falls within the range, since the electrolyte has appropriate conductivity and viscosity, excellent electrolyte performance can be exhibited, and lithium ions can be efficiently migrated.

[0123] In addition, the lithium secondary battery may include a separator between the positive electrode and the negative electrode. The positive electrode, the negative electrode and the separator may be immersed in an electrolyte.

[0124] The separator is used to separate the positive electrode and the negative electrode and provide a migration channel for lithium ions, and any separator commonly used in lithium secondary batteries can be used. In other words, a separator with low ion migration resistance to the electrolyte and excellent electrolyte wetting performance can be used.

[0125] The separator can be selected from glass fiber, polyester, polyethylene, polypropylene, polytetrafluoroethylene or a combination thereof, and can be in the form of non-woven fabric or woven fabric. For example, a polyolefin polymer separator such as polyethylene or polypropylene can be mainly used in a lithium secondary battery, and a separator coated with a composition containing a ceramic component or a polymer material can also be used to ensure heat resistance or mechanical strength, and a single layer or multilayer structure can be selectively used.

[0126] In addition, as the diaphragm, for example, polyethylene, polypropylene, polyvinylidene fluoride or two or more multilayer films thereof can be used. Of course, mixed multilayer films such as polyethylene / polypropylene two-layer diaphragm, polyethylene / polypropylene / polyethylene three-layer diaphragm, polypropylene / polyethylene / polypropylene three-layer diaphragm, etc. can be used.

[0127] Figure 1 2 is a schematic diagram of a lithium secondary battery according to an embodiment. The lithium secondary battery according to an embodiment is described by taking a cylindrical shape as an example, but the present invention is not limited thereto and can be applied to batteries of various shapes such as a prismatic shape and a pouch shape.

[0128] See also Figure 1 The lithium secondary battery 100 is cylindrical, and its main parts are a negative electrode 112, a positive electrode 114, a separator 113 arranged between the negative electrode 112 and the positive electrode 114, an electrolyte (not shown in the figure) impregnated in the negative electrode 112, the positive electrode 114 and the separator 113, a battery container 120, and a sealing component 140 for sealing the battery container 120.

[0129] The lithium secondary battery 100 is constructed by stacking a negative electrode 112 , a positive electrode 114 , and a separator 113 in this order, winding the stacked layers into a spiral shape, and housing the stacked layers in a battery container 120 .

[0130] Modes for Carrying Out the Invention

[0131] Hereinafter, examples of the present invention and comparative examples will be described. However, the following examples are merely examples of the present invention, and the present invention is not limited to the following examples.

[0132] Preparation Example 1: Large particle size active material hydroxide precursor

[0133] 1) Preparation of metal salt solution

[0134] NiSO4·6H2O was used as a nickel raw material, CoSO4·7H2O was used as a cobalt raw material, and MnSO4·H2O was used as a manganese raw material. These were added to deionized water and dissolved to prepare two metal salt aqueous solutions having different concentrations of Ni, Co, and Mn.

[0135] For the first metal salt aqueous solution for forming the core portion, the raw materials are mixed in deionized water to satisfy (Ni 0.98 Co 0.01 Mn 0.01 )(OH)2 in a stoichiometric molar ratio and prepared so that the overall molar concentration of the metal salt reaches 2.5M.

[0136] Separately, for the second metal salt aqueous solution for forming the outer shell portion, the raw materials are mixed in deionized water to satisfy (Ni 0.64 Co 0.23 Mn 0.13 )(OH)2 in a stoichiometric molar ratio and prepared so that the overall molar concentration of the metal salt reaches 2.5M.

[0137] 2) Co-precipitation process

[0138] A coprecipitation reactor having two metal salt aqueous solution supply tanks connected in series is prepared, and the first metal salt aqueous solution and the second metal salt aqueous solution are charged into the respective metal salt aqueous solution supply tanks.

[0139] After 3 liters of distilled water were placed in the coprecipitation reactor (capacity 20 L, power of the rotating motor 200 W), nitrogen was supplied at a supply rate of 2 liters / minute to remove dissolved oxygen, and the temperature of the reactor was maintained at 50°C and stirred at a speed of 140 rpm.

[0140] In addition, 14 M NH4(OH) as a chelating agent (0.06 L / h) and 8 M NaOH solution as a pH adjuster (0.1 L / h) were continuously added to the reactor respectively. During the process, the addition amount can be appropriately controlled to keep the pH in the reactor at 12.

[0141] The first metal salt aqueous solution is added to the reactor maintaining the pH and supplying the chelating agent at a rate of 0.4 liters / hour from two metal salt aqueous solution supply tanks connected in series to the reactor, and the impeller speed of the reactor is adjusted to 140 rpm to carry out the coprecipitation reaction until the diameter of the precipitate reaches about 11.1 μm (equivalent to 75% of the diameter of the final product). At this time, by adjusting the flow rate, the average residence time of the solution in the reactor reaches about 10 hours. After the reaction is in a normal state, the reactant is given a normal state duration to obtain a coprecipitated compound with a higher density.

[0142] Next, the mixing ratio of the first metal salt aqueous solution and the second metal salt aqueous solution was changed and the total supply solution was added at a rate of 0.5 liters / hour, while the supply rate of the first metal salt aqueous solution was 0.5 liters / hour at the beginning and gradually decreased to 0.05 liters / hour, and the supply rate of the second metal salt aqueous solution was 0.5 liters / hour. At this time, by adjusting the flow rate, the average residence time of the solution in the reactor was within 20 hours, and the coprecipitation reaction was carried out until the diameter of the final precipitate reached 14.8 μm.

[0143] 3) Post-processing process

[0144] The precipitate obtained by the coprecipitation process was filtered, washed with water, and dried in an oven at 100° C. for 24 hours to prepare particles having a composition of (Ni 0.88 Co 0.095 Mn 0.025 )(OH)2 and large-size particle active material precursor with an average particle size of 15μm.

[0145] Preparation Example 2: Small-particle-size positive electrode active material hydroxide precursor

[0146] 1) Preparation of metal salt solution

[0147] The same first metal salt aqueous solution and second metal salt aqueous solution as those in Preparation Example 1 were prepared.

[0148] 2) Co-precipitation process

[0149] The same reactor as in Preparation Example 1 was used, except that the addition time and amount of each metal salt solution were different, and other conditions were the same.

[0150] Specifically, the first metal salt aqueous solution is added at a rate of 0.3 liters / hour, and the impeller speed of the reactor is adjusted to 140 rpm, so as to carry out the coprecipitation reaction until the diameter of the precipitate reaches about 15.0 μm. At this time, by adjusting the flow rate, the average residence time of the solution in the reactor reaches more than 15 hours. After the reaction is in a normal state, the reactant is given a normal state duration to obtain a coprecipitated compound with a higher density.

[0151] Next, the mixing ratio of the first metal salt aqueous solution and the second metal salt aqueous solution was changed and the total supply solution was added at a rate of 0.5 liters / hour, while the supply rate of the first metal salt aqueous solution was 0.5 liters / hour at the beginning and gradually decreased to 0.05 liters / hour, and the supply rate of the second metal salt aqueous solution was 0.5 liters / hour. At this time, the flow rate was adjusted so that the average residence time of the solution in the reactor was within 15 hours, and the coprecipitation reaction was carried out until the diameter of the final precipitate reached 5.3 μm.

[0152] 3) Post-processing process

[0153] The precipitate obtained by the coprecipitation process was filtered, washed with water, and dried in an oven at 100° C. for 24 hours to prepare particles having a composition of (Ni 0.88 Co 0.095 Mn 0.025 )(OH)2 and a small particle size hydroxide active material precursor with an average particle size of 5μm.

[0154] Preparation Example 3: Preparation of large particle size oxide precursor

[0155] The core-shell concentration gradient large particle size (Ni 0.88 Co 0.095 Mn 0.025 The precursor of the (OH)2 component is loaded into a heat treatment furnace and heat treated in an air atmosphere with air introduced at a rate of 200 ml / min to prepare a porous Ni 0.88 Co 0.095 Mn 0.025 The heat treatment process is performed by heating to 700°C at a heating rate of 2.5°C / min and then maintaining the temperature at 700°C for 5 hours.

[0156] Preparation Example 4: Preparation of small particle size oxide precursor

[0157] The small-sized particles (Ni 0.88 Co 0.095 Mn 0.025The precursor of the (OH)2 component is loaded into a heat treatment furnace and heat treated in an air atmosphere with air introduced at a rate of 200 ml / min to prepare a porous Ni 0.88 Co 0.095 Mn 0.025 The heat treatment process is performed by heating to 700°C at a heating rate of 2.5°C / min and then maintaining the temperature at 700°C for 5 hours.

[0158] Example 1

[0159] 1) Preparation of large particle size active materials

[0160] The large-particle porous Ni 0.88 Co 0.095 Mn 0.025 An O2 oxide precursor, ZrO2 (Aldrich, 4N) having an average particle size (D50) of 50 nm and Al(OH)3 (Aldrich, 4N) were uniformly mixed to prepare a primary mixture. When the mixing was performed, ZrO2 was used in an amount such that Zr in the final product reached 0.34% by weight, and Al(OH)3 was used in an amount such that Al in the final product reached 0.014% by weight.

[0161] The primary mixture was mixed with LiOH·H 2 O (Mita Chemical, battery grade) so that the molar ratio of the total moles of Ni, Co, and Mn to Li in the final product was 1:1.05 to prepare a secondary mixture.

[0162] The secondary mixture was placed in a tube furnace (with an inner diameter of 50 mm and a length of 1000 mm), and oxygen was introduced at a rate of 200 ml / min for secondary calcination. For the secondary calcination process, the temperature was raised to 730°C at a rate of 2.5°C / min, and then maintained at the temperature for 16 hours, and then the calcined product was naturally cooled to 25°C.

[0163] Next, the cooled product was washed with water to remove residual lithium on the surface, H3BO3 was dry mixed, and the mixture was kept at 380°C for 5 hours to prepare a positive electrode active material. The prepared positive electrode active material is a large-particle active material, which is a secondary particle with an average particle size (D50) of 16.0 μm and agglomerated primary particles with an average particle size (D50) of 0.75 μm and an average particle size (D50) of 50 nm. The secondary particles contain ZrO2 particles with an average particle size (D50) of 50 nm. In the prepared active material, the overall component is Li 1.05 (Ni 0.88 Co 0.095 Mn 0.025 ) 0.995Al 0.005 O2, the prepared active material comprises secondary particles, which contain Li 1.05 (Ni 0.92 Co 0.067 Mn 0.013 ) 0.995 Al 0.005 The core of O2 and Li 1.05 (Ni 0.85 Co 0.12 Mn 0.03 ) 0.995 Al 0.005 O2 shell. At this time, the core portion as a whole constantly maintains Ni at 92 mol%, and the molar content of nickel in the shell portion decreases along the direction from the interface with the core portion to the outermost portion, and the ratio of the molar content of nickel at the outermost portion to the molar content of nickel at the interface with the core portion is 0.92. In addition, relative to the average particle size (D50) of the secondary particles of 100%, the average particle size (D50) of the core portion of the secondary particles is 63%.

[0164] In the prepared active material, the content of Zr was 0.34 wt % relative to 100 wt % of the prepared positive electrode active material, and the content of the coated B was 0.1 wt %.

[0165] 2) Preparation of small particle size active materials,

[0166] Instead of the large-particle oxide precursor, a small-particle oxide precursor is used, and the implementation method is the same as 3), thereby preparing a small-particle active material, which is B coated on the surface and the average particle size (D50) of the primary particles agglomerated with an average particle size (D50) of 0.5 μm, and the average particle size (D50) of 5.0 μm is secondary particles, and the secondary particles contain small-particle ZrO2 particles with an average particle size (D50) of 50.0 nm containing ZrO2. In the prepared active material, the overall component is Li 1.05 (Ni 0.88 Co 0.095 Mn 0.025 ) 0.995 Al 0.005 O2, the prepared active material comprises secondary particles, which contain Li 1.05 (Ni 0.92 Co 0.067 Mn 0.013 ) 0.995 Al 0.005 The core of O2 and Li 1.05 (Ni 0.85 Co 0.12 Mn _0.03 ) 0.995 Al 0.005At this time, the core portion as a whole constantly maintains Ni at 92 mol%, and the molar content of nickel in the shell portion decreases along the direction from the interface with the core portion to the outermost portion, and the ratio of the molar content of nickel at the outermost portion to the molar content of nickel at the interface with the core portion is 0.92. In addition, relative to the average particle size (D50) of the secondary particles of 100%, the average particle size (D50) of the core portion of the secondary particles is 70%.

[0167] In the prepared active material, the content of Zr was 0.34 wt % relative to 100 wt % of the prepared positive electrode active material, and the content of the coated B was 0.1 wt %.

[0168] The prepared large particle size active material and small particle size active material were mixed at a weight ratio of 8:2 to prepare a final positive electrode active material. In the final positive electrode active material, the content of Zr was 0.34 weight % relative to 100 weight % of the entire positive electrode active material.

[0169] 3) Preparation of half-cell

[0170] After the prepared final positive electrode active material, polyvinylidene fluoride binder (trade name: KF1100) and Denka black conductive material were mixed in a weight ratio of 92.5:3.5:4, the mixture was added into N-Methyl-2-pyrrolidone solvent to prepare positive electrode active material slurry.

[0171] The slurry was coated on an aluminum foil (Al foil, thickness: 15 μm) collector with a doctor blade and pressed into a positive electrode after drying. The positive electrode loading was 14.6 mg / cm 2 , compacted density is 3.1g / cm 3 .

[0172] A 2032 half-cell was prepared by conventional methods using the positive electrode, a lithium metal negative electrode (thickness of 200 μm, native metal), an electrolyte and a polypropylene separator. As the electrolyte, an electrolyte in which vinylene carbonate was added to a mixed solvent (mixing ratio of 3:4:3 volume %) of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate in which 1M LiPF6 was dissolved was used. At this time, the content of vinylene carbonate reached 1.5 weight % relative to 100 weight % of the mixed solvent in which 1M LiPF6 was dissolved.

[0173] Example 2

[0174] The large-particle or small-particle porous Ni 0.88 Co 0.095 Mn 0.025An O2 oxide precursor, ZrO2 (Aldrich, 4N) with an average particle size (D50) of 50 nm and Al(OH)3 (Aldrich, 4N) are uniformly mixed to prepare a mixture. In the process, the amount of ZrO2 used is changed so that the Zr in the final product reaches 0.1 wt %. Other than that, the implementation method is the same as that of Example 1, thereby preparing large-particle active materials and small-particle active materials, which are mixed in a ratio of 8:2 to prepare active materials.

[0175] Example 3

[0176] The large-particle or small-particle porous Ni 0.88 Co 0.095 Mn 0.025 An O2 oxide precursor, ZrO2 (Aldrich, 4N) with an average particle size (D50) of 50 nm and Al(OH)3 (Aldrich, 4N) are uniformly mixed to prepare a mixture. In the process, the amount of ZrO2 used is changed so that the Zr content in the final product reaches 0.35 wt %. Other than that, the implementation method is the same as that of Example 1, thereby preparing large-particle active materials and small-particle active materials, which are mixed in a ratio of 8:2 to prepare active materials.

[0177] Example 4

[0178] The large-particle or small-particle porous Ni 0.88 Co 0.095 Mn 0.025 An O2 oxide precursor, ZrO2 (Aldrich, 4N) with an average particle size (D50) of 50 nm and Al(OH)3 (Aldrich, 4N) are uniformly mixed to prepare a mixture. In the process, the amount of ZrO2 used is changed so that the Zr content in the final product reaches 0.7 wt %. Other than that, the implementation method is the same as that of Example 1, thereby preparing large-particle active materials and small-particle active materials, which are mixed in a ratio of 8:2 to prepare active materials.

[0179] Example 5

[0180] The large-particle or small-particle porous Ni 0.88 Co 0.095 Mn 0.025O2 oxide precursor, ZrO2 (Aldrich, 4N) with an average particle size (D50) of 50 nm and Al(OH)3 (Aldrich, 4N) are uniformly mixed to prepare a mixture. In the process, the amount of ZrO2 used is changed so that the Zr in the final product reaches 0.34 weight %, and ZrO2 with an average particle size (D50) of 500 nm is used. Except for this, the implementation method is the same as that of Example 5, thereby preparing large-particle active materials and small-particle active materials, which are mixed in a ratio of 8:2 to prepare active materials.

[0181] Example 6

[0182] The large-particle or small-particle porous Ni 0.88 Co 0.095 Mn 0.025 O2 oxide precursor, ZrO2 (Aldrich, 4N) and Al(OH)3 (Aldrich, 4N) are uniformly mixed to prepare a primary mixture. In the process, ZrO2 with an average particle size (D50) of 800nm ​​is used. Except for this, the implementation method is the same as that of Example 5, thereby preparing large-particle active materials and small-particle active materials, which are mixed in a ratio of 8:2 to prepare active materials.

[0183] Comparative Example 1

[0184] 1) Preparation of large particle size active materials

[0185] The (Ni 0.88 Co 0.095 Mn 0.025 The large-particle hydroxide precursor of the (OH)2 component is mixed with LiOH·H2O (Mita Chemical, battery grade) lithium raw material, ZrO2 (Aldrich, 4N) and Al(OH)3 (Aldrich, 4N). In the mixing process, the hydroxide precursor and the lithium raw material are mixed so that the total molar ratio of Ni, Co and Mn to the molar ratio of Li in the final active material is 1:1.05, and in the final active material, the content of Zr and Al (i.e., the doping amount) is such that Zr is 0.34 wt% and Al is 0.014 wt%.

[0186] The mixture was placed in a tube furnace (with an inner diameter of 50 mm and a length of 1000 mm) and oxygen was introduced at a rate of 200 ml / min for secondary calcination. For the secondary calcination process, the temperature was raised to 730°C at a rate of 2.5°C / min, and then maintained at the temperature for 16 hours. Next, the calcined product was naturally cooled to 25°C.

[0187] Next, the cooled product was washed with water to remove residual lithium on the surface, H3BO3 was dry mixed, and the mixture was kept at 380°C for 5 hours to prepare a positive electrode active material. The prepared positive electrode active material has a large particle size and a total component of Li 1.05 (Ni 0.88 Co 0.095 Mn 0.025 ) 0.9985 Zr 0.0037 Al 0.005 O2 active material, which is a secondary particle with an average particle size (D50) of 15.0 μm agglomerated by primary particles with an average particle size (D50) of 0.75 μm and coated on the surface, wherein the prepared active material comprises Li 1.05 (Ni 0.92 Co 0.067 Mn 0.013 ) 0.9985 Zr 0.0037 Al 0.005 The core of O2 and Li 1.05 (Ni 0.85 Co 0.12 Mn 0.03 ) 0.9985 Zr 0.0037 Al 0.005 O2 shell. At this time, the core portion as a whole constantly maintains Ni at 92 mol%, and the molar content of nickel in the shell portion decreases along the direction from the interface with the core portion to the outermost portion, and the ratio of the molar content of nickel at the outermost portion to the molar content of nickel at the interface with the core portion is 0.92. In addition, relative to the average particle size (D50) of the secondary particles of 100%, the average particle size (D50) of the core portion is 63%.

[0188] The B content of the coating was 0.1 wt%.

[0189] 2) Preparation of small particle size active materials

[0190] In addition to using the (Ni 0.88 Co 0.095 Mn 0.025 The method is the same as the process using the large-particle hydroxide precursor except for the small-particle hydroxide precursor of the (OH)2 component, thereby preparing a small-particle active material, which is a secondary particle with an average particle size (D50) of 5.0 μm and agglomerated with primary particles with an average particle size (D50) of 0.5 μm and B coated on the surface. In the prepared active material, the overall component is Li 1.05 (Ni 0.88 Co 0.095 Mn 0.025 ) 0.9985 Zr0.0037 Al 0.005 O2, the prepared active material contains Li 1.05 (Ni 0.92 Co 0.067 Mn 0.013 ) 0.9985 Zr 0.0037 Al 0.005 The core of O2 and Li 1.05 (Ni 0.85 Co 0.12 Mn 0.03 ) 0.9985 Zr 0.0037 Al 0.005 O2 shell. At this time, the core portion as a whole constantly maintains Ni at 92 mol%, and the molar content of nickel in the shell portion decreases along the direction from the interface with the core portion to the outermost portion, and the ratio of the molar content of nickel at the outermost portion to the molar content of nickel at the interface with the core portion is 0.92. In addition, relative to the average particle size (D50) of the secondary particles of 100%, the average particle size (D50) of the core portion is 70%.

[0191] The B content of the coating was 0.1 wt%.

[0192] The prepared large-particle active material and small-particle active material were mixed at a weight ratio of 8:2 to prepare a final positive electrode active material.

[0193] A half-cell was prepared by using the positive electrode active material in the same manner as in Example 1.

[0194] (Comparative Example 2)

[0195] The large-particle or small-particle porous Ni 0.88 Co 0.095 Mn 0.025 O2 oxide precursor, ZrO2 (Aldrich, 4N) and Al(OH)3 (Aldrich, 4N) are uniformly mixed to prepare a mixture. In the process, the amount of ZrO2 used is changed so that the Zr in the final product reaches 0.05 weight %. Other than that, the implementation method is the same as that of Example 1, thereby preparing large-particle active materials and small-particle active materials, which are mixed in a ratio of 8:2 to prepare active materials.

[0196] (Comparative Example 3)

[0197] The large-particle or small-particle porous Ni 0.88 Co 0.095 Mn 0.025O2 oxide precursor, ZrO2 (Aldrich, 4N) and Al(OH)3 (Aldrich, 4N) are uniformly mixed to prepare a mixture. In the process, the amount of ZrO2 used is changed so that the Zr in the final product reaches 1.0 weight %. Other than that, the implementation method is the same as that of Example 1, thereby preparing large-particle active materials and small-particle active materials, which are mixed in a ratio of 8:2 to prepare active materials.

[0198] (Comparative Example 4)

[0199] The large-particle or small-particle porous Ni 0.88 Co 0.095 Mn 0.025 O2 oxide precursor, ZrO2 (Aldrich, 4N) and Al(OH)3 (Aldrich, 4N) are uniformly mixed to prepare a process of a primary mixture, using ZrO2 with an average particle size (D50) of 20 nm. Except for this, the implementation method is the same as that of Example 5, thereby preparing large-particle active materials and small-particle active materials, which are mixed in a ratio of 8:2 to prepare active materials.

[0200] (Comparative Example 5)

[0201] The large-particle or small-particle porous Ni 0.88 Co 0.095 Mn 0.025 In the process of uniformly mixing an O2 oxide precursor, ZrO2 (Aldrich, 4N) and Al(OH)3 (Aldrich, 4N) to prepare a primary mixture, ZrO2 having an average particle size (D50) of 1000 nm is used. Except for this, the implementation method is the same as that of Example 5, thereby preparing large-particle active materials and small-particle active materials, which are mixed in a ratio of 8:2 to prepare active materials.

[0202] *SEM analysis

[0203] In order to understand the Ni 0.88 Co 0.095 Mn 0.025 The surface morphology of the large-particle hydroxide precursor of the OH2 component and the Ni 0.88 Co 0.095 Mn 0.025 The surface morphology of the large-particle oxide precursor of the O2 component is shown in Figure 1. The large-particle hydroxide precursor of Preparation Example 1 and the Ni-containing precursor of Preparation Example 3 0.88 Co 0.095 Mn 0.025 The surface SEM images of the large-particle oxide precursors of the O2 component are shown in Figure 2 and Figure 3 middle.

[0204] like Figure 2 As shown in FIG. 1 , the surface of the hydroxide precursor of Preparation Example 1 is formed very densely, while Figure 3 As shown, the oxide precursor of Preparation Example 3 has a surface with many pores, that is, a porous surface.

[0205] *EDS (Energy Dispersive X-ray Spectroscopy) analysis

[0206] The positive electrode active materials prepared in Example 1 and Comparative Example 1 were cut into cross sections using FIB (focused ion beam) and subjected to energy dispersive x-ray spectroscopy analysis to analyze the cross-sectional shape and the distribution of Ni, Co, Mn and Zr. The results are shown in Figure 4 and Figure 5 middle.

[0207] like Figure 4 As shown, the positive electrode active material prepared according to Example 1 is a ZrO2 particle with a size of 50 nanometers observed in the particle cross section, while Figure 5 As shown, no particle-shaped Zr was observed in the positive electrode active material prepared according to Comparative Example 1.

[0208] *Evaluation of electrochemical characteristics

[0209] The half-cells prepared according to the embodiments 1 to 7 and the comparative examples 1 to 5 were charged at 0.2C and discharged at 0.2C at constant current-constant voltage of 2.5V to 4.25V and 1 / 20C cut-off conditions to determine the initial charge and discharge capacity. The results of the embodiments 1 to 4 and comparative examples 1 to 3 are shown in Table 1 below, and the coulomb efficiency is calculated from the charge and discharge capacity, and the results are also shown in Table 1 below. In addition, the results of the embodiments 5 to 6 and comparative examples 4 to 5 are shown in Table 2 below. At the same time, for comparison, the results of the embodiment 1 are also shown in Table 2 below.

[0210] In addition, the half-cells prepared according to the above-mentioned Examples 1 to 7 and the above-mentioned Comparative Examples 1 to 5 were subjected to a 0.2C charge and a 0.2C discharge at 45°C under constant current-constant voltage conditions of 2.5V to 4.25V and 1 / 20C cut-off conditions. After applying a discharge current when the battery was charged to 100% at 4.25V, the voltage change after 60 seconds was measured, and the direct current internal resistance (DC-IR) was obtained from the results. Among the results, the results of Examples 1 to 4 and Comparative Examples 1 to 3 are shown in the following Table 1, and the results of Examples 5 to 6 and Comparative Examples 4 to 5 are shown in the following Table 2.

[0211]

Table 1

[0212]

[0213]

[0214] As shown in Table 1 above, compared with Comparative Example 1, the half cells of the positive electrode active materials of Examples 1 to 4 having nanosized ZrO2 particles contained inside the secondary particles have high charge and discharge capacities, and exhibit excellent coulombic efficiency and low initial resistance at high temperatures.

[0215] Meanwhile, although nano-sized ZrO2 particles are contained inside the secondary particles, if the content is too small (Comparative Example 2) or too large (Comparative Example 3), the initial resistance increases at high temperature, and thus it is not suitable.

[0216]

Table 2

[0217]

[0218] As shown in Table 2 above, the half-cells of the positive electrode active materials of Examples 1, 5 and 6 in which ZrO2 particles having an average particle size (D50) of 50 nm to 800 nm are contained inside the secondary particles have low high temperature initial resistance compared to the case where the average particle size (D50) is too small (Comparative Example 4) or too large (Comparative Example 5).

[0219] The present invention can be implemented in various different ways and is not limited to the above-mentioned embodiments. It will be appreciated by those skilled in the art that the present invention can be implemented in other specific ways without changing the technical concept or essential features of the present invention. Therefore, the above-mentioned embodiments are exemplary in all aspects and are not restrictive.

Claims

1. A lithium secondary battery positive electrode active material, comprising: A lithium nickel cobalt manganese oxide comprising secondary particles formed by agglomeration of at least one primary particle and represented by the following chemical formula 1; and Metal oxide particles, which are located inside the secondary particles and have an average particle size D50 of nanometer size, wherein the metal oxide has an average particle size D50 of 50 nm to 800 nm, in, The secondary particle comprises: a core portion, which is a region having a constant molar content of nickel; and a shell portion, which surrounds the outer surface of the core portion and has a concentration gradient in which the molar content of nickel decreases along a direction from an interface with the core portion to the outermost periphery, [Chemical formula 1] Li a [Ni x Co y Mr z ] t M 1-t O 2-p X p In the above chemical formula 1, M is any one element selected from the group consisting of Al, Mg, Sn, Ca, Ge, Ga, B, Ti, Mo, Nb and W, X is any one element selected from the group consisting of F, N and P, a is 0.8≤a≤1.3, 0.6≤x≤0.95,0 <y≤0.2,0<z≤0.2,x+y+z=1,0<t≤1,0≤p≤0.1。 2. The positive electrode active material for lithium secondary battery according to claim 1, wherein In the above chemical formula 1, 0.8≤x≤0.95, 0 <y≤0.1,0<z≤0.1。 3. The positive electrode active material for lithium secondary battery according to claim 1, wherein The metal oxide is one or more selected from the group consisting of ZrO2, WO3, CeO2, TiO2, HfO2, Co3O4, La2O3, BaO, SrO and combinations thereof.

4. The positive electrode active material for lithium secondary battery according to claim 1, wherein The metal content of the metal oxide is 0.1 wt % to 0.7 wt % relative to 100 wt % of the positive electrode active material. 5 . The lithium secondary battery positive electrode active material according to claim 1 , further comprising a coating layer located on the surface of the secondary particles.

6. A method for preparing a positive electrode active material for a lithium secondary battery, comprising: a step of preparing hydroxide precursor particles comprising nickel, cobalt and manganese; A step of calcining the hydroxide precursor particles once to prepare porous oxide precursor particles; A step of mixing the oxide precursor particles and the metal oxide to prepare a primary mixture; The step of mixing the primary mixture with a lithium raw material to prepare a secondary mixture; as well as a step of subjecting the secondary mixture to secondary calcination, wherein the metal oxide has an average particle size D50 of 50 nm to 800 nm, The primary calcination is carried out by heating to 400° C. to 800° C. at a temperature increase of 1° C. / min to 5° C. / min and maintaining the temperature for 3 to 20 hours. The primary calcination is carried out by introducing air or oxygen at a rate of 10 ml / min to 50 liters / min.

7. The preparation method according to claim 6, wherein: In the step of mixing the oxide precursor particles and the metal oxide to prepare a primary mixture, a doping raw material material is further mixed.

8. The preparation method according to claim 6, wherein: The step of preparing hydroxide precursor particles containing nickel, cobalt and manganese comprises: the steps of preparing a first metal salt solution and a second metal salt solution respectively, wherein the first metal salt solution and the second metal salt solution contain a nickel raw material, a cobalt raw material, a manganese raw material and a solvent, and the molar concentration of the nickel raw material is different; A first coprecipitation step of supplying the first metal salt solution at a constant concentration into a reactor in which the pH is kept constant and a chelating agent is supplied to form a core portion; a second coprecipitation step, after the first coprecipitation step, gradually reducing the supply rate of the first metal salt aqueous solution and gradually increasing the supply rate of the second metal salt aqueous solution to form a product for forming a shell portion surrounding the outer surface of the core portion; as well as The product is dried.

9. A lithium secondary battery comprising: A positive electrode comprising the positive electrode active material according to any one of claims 1 to 5; a negative electrode; and Non-aqueous electrolytes.

Citation Information

Patent Citations

  • Nickel-based active material for lithium secondary battery, method of preparing the same, and lithium secondary battery including positive electrode including the nickel-based active material

    CN107644981A