Anodic oxide film structure
By forming a multi-layer structure and filling air holes on the anodic film sheet, the problems of corrosion and insufficient strength of the anodic film in high temperature environments and MEMS processes are solved, and higher durability and wear resistance are achieved.
Patent Information
- Application Number
- CN202110143944.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-06
- Filing Date
- 2021-02-02
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-02-02
AI Technical Summary
The anodized film is prone to corrosion and not resistant to etching solutions in high temperature environments and MEMS processes, and the film structure is insufficient, resulting in easy damage and degradation of performance under severe environments.
By forming multiple single-atom layer thin film layers on the anodized film sheet, including a non-porous barrier layer and a porous layer, and placing metallic substances on the surface, it enhances its drug resistance and corrosion resistance while filling air holes and cracks. to increase strength.
It improves the durability, drug resistance and wear resistance of the anodic oxide film, prevents crack exposure and gas ejaculation caused by corrosion, and enhances its performance stability in high temperature environments.
Smart Images

Figure CN113215632B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an anodized film structure comprising an anodized film sheet. Background Art
[0002] The anodized film can be advantageously used in the semiconductor or display fields requiring a high-temperature process atmosphere.
[0003] Anodized films can be manufactured into thin sheet forms and constitute various parts used in the semiconductor or display fields.
[0004] However, the anodized film having a thin thickness has a disadvantage in that the strength is weak due to its thickness.
[0005] The anodized film may constitute a wiring substrate for electrically connecting probes of a probe card to a printed circuit board (PCB) substrate.
[0006] The wiring substrate may be provided with connection pads electrically connected to the probes on at least one side. In this case, the wiring substrate may be provided with the probes by performing a micro-electromechanical system (MEMS) process on the side provided with the connection pads.
[0007] The MEMS process can be roughly performed through the following process.
[0008] First, in order to configure the probe, a shielding material layer may be configured on the upper part of the connection pad, and patterned by a photolithography process to expose the upper surface of the connection pad. Then, the following process may be repeated: a metal substance is configured at the patterned position, a seed layer is deposited and a shielding material layer is configured on the upper part thereof, and then patterned, and a metal substance is filled at the patterned position. Then, the rest except the metal substance is removed by using an etching solution, so that a probe can be formed on the upper part of the connection pad.
[0009] However, in the case where the wiring substrate is formed of an anodized film, there may be a problem that it is not resistant to an etching solution used in the MEMS process.
[0010] In other words, since the anodized film may be damaged by the etching solution, the process of directly forming the probe needle on the upper portion of the connection pad of the wiring substrate may be relatively poor.
[0011] As described above, anodized films can be advantageously used in high temperature atmospheres, but may have the following problems: relatively weak strength due to thin thickness, easily corroded in harsh atmospheres due to exposure to harsh use environments, and not resistant to specific chemical solutions (e.g., alkaline solutions).
[0012] [Prior art literature]
[0013] [Patent Document]
[0014] [Patent Document 1] Korean registered patent No. 10-0664900 Summary of the invention
[0015] [Problems to be solved by the invention]
[0016] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide an anodic oxide film structure having improved strength and high chemical resistance and corrosion resistance.
[0017] [Technical means to solve the problem]
[0018] According to one feature of the present invention, an anodized film structure comprises: an anodized film sheet; and a first thin film layer, arranged on at least one side of the anodized film sheet, the first thin film layer comprising a first monatomic layer formed by repeatedly executing the following cycle, wherein the cycle is: adsorbing a 1-1 precursor, supplying a 1-2 reactant of a different type from the 1-1 precursor, and generating the first monatomic layer by chemical substitution of the 1-1 precursor and the 1-2 reactant.
[0019] In addition, the thickness of the first thin film layer is between 20 nm and 3 μm.
[0020] In addition, the anodized film sheet includes a non-porous barrier layer having no pores formed therein, and the thickness of the barrier layer is between 100 nm and 1 μm.
[0021] In addition, the anodized film sheet includes a non-porous barrier layer having no pores formed therein, and a porous layer located on the barrier layer and having pores formed therein, and a portion of the first thin film layer is located inside the pores of the porous layer.
[0022] In addition, a second thin film layer is formed including a plurality of second monoatomic layers formed by repeatedly performing the following cycle: a 2-1 precursor is adsorbed on the upper portion of the first thin film layer, a 2-2 reactant of a different type from the 2-1 precursor is supplied, and a second monoatomic layer is generated by chemical substitution of the 2-1 precursor and the 2-2 reactant, wherein the first thin film layer and the second thin film layer have different constituent components from each other.
[0023] Furthermore, a through hole is arranged in the anodized film sheet, and the first thin film layer is arranged on the inner side surface of the through hole.
[0024] In addition, the anodized film sheets are stacked up and down and bonded to each other via a bonding layer, and a metal substance is arranged in the through hole.
[0025] [Effects of the Invention]
[0026] The anodized film structure of the present invention can have the characteristics of durability, chemical resistance and wear resistance. At the same time, the anodized film structure of the present invention has the effect of preventing the re-exposure of the cracked part caused by the corrosion of the film layer and the outgassing problem. Therefore, the anodized film structure of the present invention can improve the overall performance efficiency of the product when it is configured as a structure that performs a specific function in a specific field. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 (a) to Figure 1 (d) is a diagram showing various embodiments of the anodized film structure of the present invention.
[0028] Figure 2 (a) to Figure 2 (d) is a diagram showing various embodiments of modified examples of the anodized film structure of the present invention.
[0029] Figure 3 This is a diagram schematically and enlargedly showing a state in which a conventional thin film layer is formed on a barrier layer.
[0030] Figure 4 This is a diagram schematically and enlargedly showing a state in which a first thin film layer is formed on the barrier layer of the present invention.
[0031] Figure 5 (a) to Figure 5 (c) is a diagram showing a conventional process of forming a thin film layer on a porous layer.
[0032] Figure 6 (a) to Figure 6 (c) is a diagram showing a process of forming a first thin film layer on the porous layer of the present invention.
[0033] Figure 7 and Figure 8 This is a diagram schematically showing an example in which the anodized film structure of the present invention is arranged in a specific configuration. DETAILED DESCRIPTION
[0034] The following content is only an example of the principle of the invention. Therefore, even if it is not clearly described or shown in this specification, a person skilled in the art can implement the principle of the invention and invent various devices included in the concept and scope of the invention. In addition, all conditional terms and embodiments listed in this specification should be understood in principle as the purpose of clearly understanding the concept of the invention, and are not limited to the embodiments and states specifically listed as described above.
[0035] The above-mentioned objects, features and advantages will become more apparent from the following detailed description in conjunction with the accompanying drawings, so that a person having ordinary knowledge in the technical field to which the invention belongs can easily implement the technical concept of the invention.
[0036] The embodiments described in this specification will be described with reference to the cross-sectional views and / or stereograms as ideal illustrations of the present invention. In order to effectively illustrate the technical content, the thickness of the membrane and the region shown in these drawings and the diameter of the holes are exaggerated. The morphology of the illustrations may be deformed due to manufacturing technology and / or tolerances. Therefore, the embodiments of the present invention are not limited to the specific morphology shown, but also include changes in the morphology generated according to the manufacturing process.
[0037] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings as follows.
[0038] Figure 1 (a) to Figure 1 (d) is a diagram showing various embodiments of the anodized film structure AS of the present invention, Figure 2 (a) to Figure 2 (d) is a diagram showing various embodiments of modified examples of the anodized film structure AS of the present invention, Figure 3 1 is a diagram schematically and enlargedly showing a state in which a conventional thin film layer 11 ′ is formed on a barrier layer BL. Figure 4 1 is a diagram schematically showing an enlarged state in which a first thin film layer is formed on the barrier layer BL of the present invention. Figure 5 (a) to Figure 5 (c) is a diagram showing a process of forming a conventional thin film layer 11' on the porous layer PL. Figure 6 (a) to Figure 6 (c) is a diagram showing a process of forming the first thin film layer 11 on the porous layer PL of the present invention.
[0039] like Figure 1 (a) to Figure 1 As shown in (d), the anodized film structure AS of the present invention may include the following: an anodized film sheet 10; and a first thin film layer 11 disposed on at least one side of the anodized film sheet 10.
[0040] The anodized film sheet 10 can be manufactured by the following process.
[0041] First, an aluminum base material may be configured and an anodized process may be performed. Through the above process, an anodized film A made of aluminum oxide (Al2O3) is formed on the surface of the base material. The anodized film A includes a barrier layer BL having no pores P formed therein and a porous layer PL having pores P formed therein.
[0042] The barrier layer BL is located on the base material, and the porous layer PL is located on the barrier layer BL. Specifically, when the base material is anodized, the barrier layer BL is first generated, and the porous layer PL is formed when the barrier layer BL has a predetermined thickness.
[0043] The barrier layer BL is formed to have a thickness of tens of nanometers or more and several micrometers or less, preferably, 100 nm or more and 1 μm or less.
[0044] The porous layer PL is formed to have a thickness of tens of nm or more and hundreds of μm or less.
[0045] The diameter of the pores P included in the porous layer PL is formed in a range from several nm to several hundred nm.
[0046] Then, a process of removing the base material from the base material formed on the surface of the anodized film A having the barrier layer BL and the porous layer PL can be performed. Through the above-mentioned process, the anodized film A made of aluminum oxide (Al2O3) remains.
[0047] The anodized film sheet 10 may be configured in a structure in which the barrier layer BL is located below the porous layer PL, or in a structure in which the barrier layer BL is located above the porous layer PL.
[0048] The anodized film sheet 10 may be configured in a structure in which the porous layer PL is located above or below the barrier layer BL, and the upper surface and the lower surface are asymmetrical.
[0049] The porous layer PL and the barrier layer BL may have a density difference depending on whether or not they include pores P. The barrier layer BL is a region that does not include pores P, and may have a relatively higher density than the porous layer PL.
[0050] The anodized film sheet 10 is configured in a structure where the barrier layer BL is located on the upper part of the porous layer PL or located on the lower part of the porous layer PL, so that the first film layer 11 can be configured on at least one side. Figure 1 (a) to Figure 1 As shown in (d), it can be implemented in various embodiments.
[0051] like Figure 1 As shown in (a), the anodized film sheet 10 may be arranged such that the barrier layer BL is located on the upper portion of the porous layer PL.
[0052] Such anodized film sheet 10 may be provided with a first film layer 11 on at least one side.
[0053] like Figure 1 As shown in (a), as an example, the anodized film sheet 10 may have a first thin film layer 11 disposed on the upper surface. Figure 1The anodized film sheet 10 shown in (a) has a structure in which the barrier layer BL is located on the upper part of the porous layer PL, and therefore the first thin film layer 11 can be arranged on the upper surface of the barrier layer BL.
[0054] The first thin film layer 11 can be formed by repeatedly performing the following cycle: adsorbing a 1-1 precursor on at least one side of the anodized film sheet 10, supplying a 1-2 reactant of a different type from the 1-1 precursor, and generating a first monoatomic layer 11a by chemical substitution of the 1-1 precursor and the 1-2 reactant.
[0055] Specifically, the first thin film layer 11 may be formed through the process described below.
[0056] First, the 1-1 precursor adsorption layer can be configured by supplying and adsorbing the 1-1 precursor on at least one side of the anodized film sheet 10. In this case, the 1-1 precursor adsorption layer can be formed into only one layer by a self-limiting reaction.
[0057] An inert gas supplying step may then be performed.
[0058] In the inert gas supplying step, the excess 1-1 precursor remaining in the 1-1 precursor adsorption layer may be removed. As described above, the 1-1 precursor forms only one layer by a self-limiting reaction. Therefore, the 1-1 precursor remaining in the 1-1 precursor adsorption layer may be an element to be removed.
[0059] In the inert gas supplying step, a process of supplying the inert gas to the anodized film sheet 10 having the 1-1 precursor may be performed to remove an excess of the 1-1 precursor.
[0060] Then, the adsorption and substitution steps of the 1-2 reactants may be performed.
[0061] In the 1-2 reactant adsorption and substitution step, a process of supplying the 1-2 reactant to the surface of the 1-1 precursor adsorption layer may be performed. Therefore, the 1-2 reactant may be adsorbed on the surface of the 1-1 precursor adsorption layer. The 1-1 precursor adsorption layer and the 1-2 reactant may be chemically substituted. Therefore, the first monoatomic layer 11a may be generated.
[0062] The 1-1 precursor and the 1-2 reactant have different constituent components from each other.
[0063] Since the first monatomic layer 11 a is generated by chemical substitution of the 1-1 precursor and the 1-2 reactant, the constituent components of the first monatomic layer 11 a may be different from those of the 1-1 precursor and the 1-2 reactant.
[0064] In the 1-1 precursor and the 1-2 reactant, the remaining components among the components thereof may be exhausted as gas during the process of generating the first monoatomic layer 11 a .
[0065] By repeatedly performing the above-described process, the first thin film layer 11 can be formed of a plurality of first monoatomic layers 11a. The anodized film structure AS can have the first thin film layer 11 by repeatedly performing the process of generating the first monoatomic layer 11a on at least one side.
[0066] The thickness of the first thin film layer 11 can be formed in the range of several nm to several μm, and preferably formed in the range of 20 nm to 3 μm. Therefore, the process of generating the first monoatomic layer 11a can be repeatedly performed so that the thickness of the first thin film layer 11 is preferably formed in the range of 20 nm to 3 μm.
[0067] The plurality of first monoatomic layers 11 a have crystalline characteristics.
[0068] The first thin film layer 11 may be formed of at least any one of aluminum oxide (Al2O3), yttrium oxide (Y2O3), aluminum nitride (AlN), silicon dioxide (SiO2), silicon nitride (Si3N4), and silicon carbide (SiC).
[0069] The first thin film layer 11 may be formed of at least any one of the above materials to have chemical resistance to specific chemicals used in a specific process (eg, an etching process).
[0070] In addition, the first thin film layer 11 may be formed of a plurality of first monoatomic layers 11 a having crystalline properties, and thus may have high rigidity and strength properties.
[0071] The present invention configures the first film layer 11 on at least one side of the anodized film sheet 10, so that the anodized film sheet 10 is not damaged by the chemical even when used in a specific field and exposed to a specific chemical. In addition, the present invention can eliminate the weakening of the strength of the anodized film sheet 10 caused by thinning due to the first film layer 11.
[0072] like Figure 3 and Figure 4 As shown, since the anodized film sheet 10 is manufactured in the form of a thin plate, it may be partially damaged during the manufacturing process and cracks C may exist in the barrier layer BL.
[0073] Figure 3 The figure schematically and enlarges a state where a thin film layer 11 ′ (hereinafter referred to as “conventional thin film layer”) is formed on an anodized film sheet 10 having cracks C by a conventional chemical vapor deposition process or physical vapor deposition process apparatus.
[0074] like Figure 3As shown, the anodized film sheet 10 may have a small gap formed in the barrier layer BL due to the crack C. In such anodized film sheet 10, the barrier layer BL may be deposited by a conventional chemical vapor deposition process or physical vapor deposition process device.
[0075] The crack C is formed with a small gap, but may exist in an irregular shape. Therefore, the conventional deposition layer may be formed relatively thickly in the upper portion C1 of the crack C having a wide gap width, but may be formed thinly or may not be formed in the inner side surface C2 of the crack C and the lower portion of the crack C.
[0076] Therefore, the conventional deposited layer can be formed thickest on the upper surface of the barrier layer BL and in the upper portion C1 of the crack C, and the thin film layer 11 ′ can be formed in a form of sealing the upper portion C1 of the crack C.
[0077] In other words, the conventional thin film layer may form the thin film layer 11' in a form that mainly covers only the upper surface of the barrier layer BL and the exposed partial surface (specifically, the upper portion C1) of the crack C. Therefore, even if the anodized film sheet 10 is provided with the thin film layer 11', it may be provided in a state where there is a gap at the inner side surface C2 of the crack C and the lower portion C3.
[0078] When the anodized film structure equipped with the conventional thin film layer 11' is used for a long time, the thin film layer 11' may be removed or corroded by chemical reaction with the process gas. Therefore, the anodized film structure equipped with the thin film layer 11' may expose the gap existing at the inner side surface C2 and the lower part C3 of the crack C. Therefore, the anodized film structure equipped with the conventional thin film layer 11' may be damaged due to the exposed part of the crack C.
[0079] However, in the present invention, a plurality of first monoatomic layers 11a may be deposited with a fixed thickness to form the first thin film layer 11. One first monoatomic layer 11a may be formed on the upper surface of the barrier layer BL by chemical substitution of the 1-1 precursor and the 1-2 reactant. Therefore, a plurality of first monoatomic layers 11a may be formed by repeatedly performing a cycle of forming one first monoatomic layer 11a.
[0080] Figure 4 This is a diagram schematically and enlargedly showing a state in which the first thin film layer 11 of the present invention is formed on the barrier layer BL of the anodized film sheet 10 having the crack C.
[0081] like Figure 4 As shown, the first thin film layer 11 of the present invention can be configured by forming the first monoatomic layer 11a with the same thickness.
[0082] The anodized film sheet 10 performs the process of forming the first monoatomic layer 11a on the upper surface of the barrier layer BL multiple times, so that the first thin film layer 11 formed of multiple first monoatomic layers 11a can be configured. Therefore, even if the anodized film sheet 10 generates irregular cracks C, the cracks C can be filled by the first thin film layer 11 as a whole.
[0083] In other words, the first thin film layer 11 can perform the function of filling the crack C with a fixed thickness while repairing the minute gap of the anodized film sheet 10. The barrier layer BL can have a structure of repairing and removing the crack C generated portion by the first thin film layer 11.
[0084] The anodized film structure AS of the present invention does not have a tiny gap caused by the crack C due to the first film layer 11. Therefore, even if the first film layer 11 is removed or corroded due to long-term use of the present invention, the problem of being damaged again due to the exposure of the crack C can be fundamentally blocked.
[0085] In this way, the anodized film structure AS of the present invention can ensure high rigidity and strength through the first thin film layer 11 while maintaining the thinning property of the anodized film sheet 10 .
[0086] In addition, even if minute cracks C exist due to the thin thickness of the anodized film sheet 10 of the present invention, the cracks C can be removed by the first thin film layer 11, thereby improving durability.
[0087] like Figure 1 As shown in (b), the anodized film sheet 10 may have a structure in which a porous layer PL having pores P formed therein is positioned on the non-porous barrier layer BL. Therefore, the surface of the anodized film sheet 10 may be formed of the porous layer PL.
[0088] As an example, the anodized film structure AS may include a first thin film layer 11 disposed on the upper surface of an anodized film sheet 10 formed of a porous layer PL.
[0089] The first film layer 11 can be Figure 1 The configuration is the same as the configuration and process described in (a).
[0090] like Figure 1 As shown in (b), the anodized film structure AS can be formed with a structure in which a part of the first thin film layer 11 is located inside the pores P by disposing the first thin film layer 11 on the upper surface of the porous layer PL.
[0091] The inside of the pore P may be filled so that no empty space exists when a plurality of first monoatomic layers 11a are sequentially generated. The first monoatomic layer 11a may be formed on the upper surface of the porous layer PL with a fixed thickness. The first monoatomic layer 11a may be formed with a fixed thickness even inside the pore P. Therefore, the first monoatomic layer 11a may fill the inside of the pore P so that no empty space exists.
[0092] Will refer to Figure 5 (a) to Figure 5 (c) and Figure 6 (a) to Figure 6 (c) The process of forming the first thin film layer 11 on the porous layer PL of the present invention will be described in detail.
[0093] Figure 5 (a) to Figure 5 (c) is a diagram showing a process of forming a conventional thin film layer 11 ′ on the porous layer PL.
[0094] like Figure 5 As shown in (a), in the past, a chemical vapor deposition process device or a physical vapor deposition process device can be used to perform a deposition process on the porous layer PL. Figure 5 As shown in (b), a deposited layer 13 is formed on the upper portion of the porous layer PL.
[0095] In this case, in the deposition layer 13, the thickness T1' formed on the upper part of the upper surface of the porous layer PL, the thickness T2' formed on the bottom surface of the pore P, and the thickness T3' formed on the inner wall PW of the pore P satisfy the relationship "(T1'>T2'>T3')".
[0096] like Figure 5 As shown in (c), conventionally, the thin film layer 11 ′ is formed by increasing the thickness of the deposited layer 13 .
[0097] Specifically, the thickness (T1', T2', T3') of the deposited layer 13 increases differently at each location where it is formed. Figure 5 As shown in (c), the thickness T1' of the deposition layer 13 on the upper surface of the porous layer PL, the thickness T3' on the inner wall PW of the pore P, and the thickness T2' on the bottom surface of the pore P may be increased at non-constant thicknesses.
[0098] The upper surface of the porous layer PL is a region formed around the openings of the pores P and can be formed as a relatively flat surface. Therefore, the deposition layer 13 can be relatively easily deposited on the upper surface of the porous layer PL and formed thickly to have a thickness T1 ′.
[0099] On the other hand, since the inner wall PW of the pore P is formed of a vertical surface formed along the depth, the thickness T3 ′ of the deposition layer 13 can be formed relatively thin.
[0100] The deposition layer 13 is more easily deposited on the bottom surface of the pore P than on the inner wall PW of the pore P, but the deposition layer 13 may be formed to have a thickness T2 ′ thinner than that of the upper surface of the porous layer PL.
[0101] Therefore, the deposition layer 13 can be formed thickest on the upper surface of the porous layer PL and around the openings of the pores P, so that the thin film layer 11 ′ can be formed in a form of sealing the openings of the pores P.
[0102] However, since the deposition layer 13 is formed in a relatively thin thickness T3' in the inner wall PW of the pore P, it may be difficult to entirely fill the inside of the pore P. Therefore, there is a space PS in the pore P due to the thin film layer 11' not being formed inside.
[0103] In the case of using the conventional thin film layer 11' for a long time, the thin film layer 11' formed on the upper surface may be removed or corroded by a chemical reaction with the process gas. Therefore, the space PS inside the pore P is exposed to the outside. Therefore, foreign matter may flow into and remain in the space PS inside the pore P, causing performance errors.
[0104] In addition, in the anodized film sheet 10 whose surface is formed by a porous layer PL, when a conventional thin film layer 11' is arranged on the surface, out-gassing problem may occur. Specifically, the thin film layer 11' may be removed or corroded in the surface of the anodized film sheet 10 due to long-term use. Therefore, the space PS inside the pore P may be exposed. Such space PS inside the pore P may flow into external particles. During the semiconductor or display process, particles may fall on the surface of the chip W or the substrate and bring negative effects. This phenomenon is the out-gassing phenomenon of particles. In the case where the anodized film sheet 10 is provided with a conventional thin film layer 11' on the surface of the porous layer PL, the out-gassing phenomenon as described above may easily occur.
[0105] However, in the present invention, the first thin film layer 11 is formed by forming a plurality of first monoatomic layers 11 a with a constant thickness, thereby more effectively preventing the problem of particle inflow and the problem of outgassing.
[0106] Figure 6 (a) to Figure 6 (c) is a diagram showing a process of forming the first thin film layer 11 on the porous layer PL of the present invention.
[0107] like Figure 6 As shown in (a), the pore P may be in a state where the inside is exposed. Figure 6As shown in (b), a first monoatomic layer 11a can be formed on the upper surface of the porous layer PL by chemical substitution of the 1-1 precursor and the 1-2 reactant.
[0108] At this time, the thickness T1 of the first monoatomic layer 11a on the upper surface of the porous layer PL, the thickness T2 on the bottom surface of the pore P, and the thickness T3 on the inner wall PW of the pore P can satisfy the relationship of "(T1=T2=T3)". In other words, the first monoatomic layer 11a can be formed in the porous layer PL with the same thickness.
[0109] The first thin film layer 11 may be formed on the porous layer PL by repeatedly performing a cycle of forming the first monoatomic layer 11a. Figure 6 As shown in (c), the first monoatomic layer 11a may be formed to have a fixed thickness to form the first thin film layer 11. Therefore, the pores P may be entirely filled with the first thin film layer 11 without leaving any empty space.
[0110] With the above-described structure, the anodized film structure AS can ensure rigidity even if its surface is constituted by the porous layer PL having a relatively low density.
[0111] As described above, even if the first film layer 11 of the anodized film structure AS of the present invention is corroded due to long-term use, no empty space is generated inside the pores P. The inside of the pores P can be a structure filled with the first film layer 11 without an empty space. Therefore, in the case where the anodized film structure AS is configured with the first film layer 11 on the upper surface of the porous layer PL, the internal rigidity can be maintained even if the first film layer 11 on the upper surface is corroded.
[0112] Thus, the present invention can configure the first thin film layer 11 on at least one side of the anodized film sheet 10, that is, the porous layer PL constituting the upper surface. Therefore, the anodized film structure AS is formed into a sealed structure at the upper surface, thereby preventing the problem of particles flowing into the interior in advance.
[0113] In addition, the anodized film structure AS may have a structure in which the interior of the pores P is completely filled with the first film layer 11. Therefore, the anodized film structure AS may have a structure in which there is no empty space inside due to the first film layer 11. Therefore, even if a part of the first film layer 11 is removed or corroded due to long-term use of the anodized film structure AS, the problem of particles flowing into the interior of the pores P can be prevented.
[0114] In addition, the anodized film structure AS has no empty space inside due to the first thin film layer 11, thereby fundamentally preventing the problem of particles generated inside. Therefore, the anodized film structure AS of the present invention does not cause the problem of outgassing of particles generated inside.
[0115] Figure 1 (c) is a diagram showing a structure in which the first thin film layer 11 is arranged on the upper surface and the lower surface of the anodized film sheet 10. Figure 1 As shown in (c), the anodized film structure AS can be configured such that the anodized film sheet 10 is arranged so that the barrier layer BL is located on the porous layer PL.
[0116] In the anodized film structure AS, a process of forming the first thin film layer 11 on the upper surface formed of the barrier layer BL and a process of forming the first thin film layer 11 on the lower surface may be performed.
[0117] Therefore, the anodized film structure AS of the present invention may have a structure in which the first thin film layer 11 is disposed on the upper surface and the lower surface of the anodized film sheet 10 .
[0118] With the above-described structure, the anodized film structure AS can increase the density of the lower surface where the density is relatively low due to the porous layer PL.
[0119] The barrier layer BL has a relatively high density and has a first thin film layer 11 disposed on the upper surface, so that it can have a higher strength. In addition, the porous layer PL has a higher density due to the first thin film layer 11, so that its strength can be improved.
[0120] Therefore, the density of the upper surface and the lower surface of the anodized film structure AS can be made uniform to a certain extent, and the durability and strength of the structure itself can be further improved.
[0121] Figure 1 (d) is a diagram showing an embodiment of a structure in which a second thin film layer 12 is additionally arranged on the upper part of the first thin film layer 11. In this case, as an example, the anodized film sheet 10 can be arranged in a structure in which the barrier layer BL is positioned on the upper part of the porous layer PL. The structure of the anodized film sheet 10 is not limited to this, and can also be arranged in a structure in which the porous layer PL is located on the upper part of the barrier layer BL.
[0122] The upper surface of the anodized film sheet 10 is formed of the barrier layer BL, and the first thin film layer 11 may be disposed on the upper surface of the barrier layer BL. The second thin film layer 12 may be disposed on the upper portion of the first thin film layer 11.
[0123] The second thin film layer 12 may include multiple second monoatomic layers formed by repeatedly performing the following cycle: adsorbing a 2-1 precursor on the upper part of the first thin film layer 11, supplying a 2-2 reactant of a different type from the 2-1 precursor, and generating a second monoatomic layer by chemical substitution of the 2-1 precursor and the 2-2 reactant.
[0124] The second thin film layer 12 may be configured by repeatedly performing a cycle of generating a second monoatomic layer after performing a process of forming the first thin film layer 11 on the upper surface of the barrier layer BL.
[0125] Specifically, a process of supplying the 2-1st precursor to the upper portion of the first thin film layer 11 may be performed. Therefore, the 2-1st precursor may be adsorbed on the surface of the first thin film layer 11 and form a 2-1st precursor adsorption layer on the surface of the first thin film layer 11. The 2-1st precursor adsorption layer may form only one layer through a self-limiting reaction.
[0126] After the 2-1st precursor adsorption layer is formed on the surface of the anodized film sheet 10 provided with the first thin film layer 11, an inert gas supply step may be performed.
[0127] The inert gas can remove the excess 2-1 precursor remaining in the 2-1 precursor adsorption layer. Since the 2-1 precursor adsorption layer is formed by a self-limiting reaction, the excess 2-1 precursor remaining is removed by the inert gas.
[0128] Then, the anodized film sheet 10 may perform a process of supplying the 2-2 reactant to the surface of the 2-1 precursor adsorption layer. The 2-2 reactant may be adsorbed on the surface of the 2-1 precursor, and the 2-1 precursor adsorption layer and the 2-2 reactant may be chemically substituted. Thus, a second monoatomic layer may be generated.
[0129] The 2-2 reactant and the 2-1 precursor have different constituent components from each other.
[0130] The second monatomic layer may be formed by chemical substitution of the 2-1 precursor adsorption layer including the 2-1 precursor and the 2-2 reactant. Therefore, the constituent components of the second monatomic layer may be different from the constituent components of the 2-1 precursor and the 2-2 reactant.
[0131] During the process of generating the second monoatomic layer, the remaining components of the 2-1 precursor and the 2-2 reactant may be exhausted as a gas.
[0132] The second thin film layer 12 may be formed in a range of several nm to several μm, and preferably formed to a thickness of 20 nm to 3 μm. Therefore, the second thin film layer 12 may be repeatedly performed until a plurality of second monoatomic layers are formed to a thickness of 20 nm to 3 μm.
[0133] The second thin film layer 12 may have a different constituent component from that of the first thin film layer 11 .
[0134] For example, in the case where the constituent component of the second monatomic layer constituting the second thin film layer 12 is aluminum oxide (Al 2 O 3 ), the constituent component of the first monatomic layer 11 a constituting the first thin film layer 11 may be silicon dioxide (SiO 2 ).
[0135] Thus, the present invention can form the first thin film layer 11 and the second thin film layer 12 with different components. Therefore, the 1-1 precursor and the 2-1 precursor can have different components. Alternatively, the 1-2 reactant and the 2-2 reactant can have different components.
[0136] For example, even if the 1-1 precursor and the 2-1 precursor have the same constituent components, the 1-1 reactant and the 2-2 reactant may have different constituent components. Therefore, the constituent components of the first thin film layer 11 and the constituent components of the second thin film layer 12 may have different constituent components.
[0137] In other words, the present invention can be configured such that at least any pair of the 1-1 precursor and the 2-1 precursor or the 1-2 reactant and the 2-2 reactant have different constituents from each other, so that the first thin film layer 11 and the second thin film layer 12 have different constituents from each other.
[0138] In the present invention, since the first thin film layer 11 and the second thin film layer 12 have different constituent components, various properties can be obtained.
[0139] For example, the first thin film layer 11 is formed of a component having heat resistance, and the second thin film layer 12 is formed of a component having corrosion resistance. In this case, the anodized film structure AS can have both high heat resistance and high corrosion resistance.
[0140] In addition, the first film layer 11 is formed of a component having voltage resistance, and the second film layer 12 is formed of a component having plasma resistance. In this case, the anodized film structure AS can have both high voltage resistance and high plasma resistance.
[0141] The anodized film structure AS of the present invention may further include a plurality of thin film layers formed of a single atomic layer on the upper portion of the second thin film layer 12 .
[0142] The plurality of thin film layers can be formed by the same method as the formation method of the first thin film layer 11 and the second thin film layer 12, and can be formed by the same configuration. In other words, there is no restriction on the number of thin film layers configured in the anodized film structure AS. However, the plurality of thin film layers can preferably have different constituent components from the first thin film layer 11 and the second thin film layer 12. Therefore, different characteristics can be given to each other in the present invention.
[0143] The anodized film structure AS can ensure not only various characteristics but also further improved rigidity in terms of surface strength by configuring a plurality of thin film layers (for example, the first thin film layer 11 and the second thin film layer 12).
[0144] As an example, when the anodized film structure AS of the present invention is configured as a component of a specific device, the surface of the component may be formed of a plurality of thin film layers 11 and 12 .
[0145] As a more specific example, the anodized film structure AS may be configured in plurality to form a multilayer wiring substrate of the probe card 20. In this case, the anodized film structure AS may be configured with a first thin film layer 11 and a second thin film layer 12 on the upper surface of the barrier layer BL. The first thin film layer 11 and the second thin film layer 12 may be structures sequentially formed on the upper surface of the barrier layer BL.
[0146] Such anodized film structure AS can be arranged so that the first thin film layer 11 and the second thin film layer 12 form the upper surface and the lower surface of the multilayer wiring substrate.
[0147] When the anodic oxide film structure AS of the present invention constitutes a multilayer wiring substrate, the surface density of the multilayer wiring substrate can be made uniform by the first thin film layer 11 and the second thin film layer 12. Therefore, the multilayer wiring substrate formed by the present invention will not produce warping deformation, and the durability of the product itself can be improved.
[0148] In the present invention, as an example, the first thin film layer 11 and the second thin film layer 12 may be formed of a plurality of monoatomic layers (specifically, the first thin film layer 11 is the first monoatomic layer 11a, and the second thin film layer 12 is the second monoatomic layer).
[0149] Different from this, the first thin film layer 11 and the second thin film layer 12 may also be formed of a single monatomic layer instead of a plurality of monatomic layers.
[0150] Specifically, the first thin film layer 11 may be formed of only one first monoatomic layer 11 a , and the second thin film layer 12 may be formed of only one second monoatomic layer.
[0151] Different from this, any one of the first thin film layer 11 and the second thin film layer 12 may be formed of a single monoatomic layer, and any one of them may also be configured by a combination including a plurality of monoatomic layers.
[0152] Specifically, the first thin film layer 11 may be formed of a single monoatomic layer, and the second thin film layer 12 may be formed of multiple monoatomic layers. Alternatively, the first thin film layer 11 may be formed of multiple monoatomic layers, and the second thin film layer 12 may be formed of a single monoatomic layer.
[0153] The anodized film structure AS can selectively form the first thin film layer 11 and / or the second thin film layer 12 by a single monatomic layer or multiple monatomic layers. Therefore, the present invention has the advantage that the thickness of the first thin film layer 11 and / or the second thin film layer 12 can be easily configured to a desired thickness.
[0154] The anodized film structure AS of the present invention can have high rigidity by configuring the first thin film layer 11 on at least one side. Even if the first thin film layer 11 is formed on the surface of any one of the porous layer PL and the barrier layer BL of the anodized film sheet 10, the surface strength of the structure can be improved by forming it with a thickness within a specific range (preferably from 20 nm to 2 μm).
[0155] Since the first thin film layer 11 is formed with a fixed thickness, it can perform a function of filling an empty space as a whole according to a configuration position.
[0156] For example, when the first film layer 11 is disposed on the upper surface of the porous layer PL when the porous layer PL constitutes the upper surface of the anodized film sheet 10, a portion of the first film layer 11 may be located inside the pores P of the porous layer PL. Therefore, the pores P may be filled with the first film layer 11. Therefore, the rigidity of the anodized film structure AS can be improved by eliminating the empty space inside.
[0157] In contrast, the first film layer 11 can fill the cracks C present on the barrier layer BL. Therefore, even if the anodized film structure AS is provided with the anodized film sheet 10 having micro cracks C, the cracks C can be repaired and removed by the first film layer 11. Therefore, even if the anodized film structure AS is used for a long time, there is no problem of exposing the cracks C, and thus further improved durability can be ensured.
[0158] Therefore, the anodized film structure AS of the present invention can have both high strength and high durability by disposing the first thin film layer 11 on at least one surface of the anodized film sheet 10 .
[0159] Figure 2 (a) to Figure 2 (d) is a diagram showing various embodiments of modified examples of the anodized film structure AS of the present invention. The anodized film structure AS of the modified example is different from the anodized film structure AS of the embodiment in that a through hole H is provided in the anodized film sheet 10 .
[0160] like Figure 2 (a) to Figure 2 As shown in (c) of the modification example, the anodized film sheet 10 is provided with a through hole H, and the first thin film layer 11 can be disposed on the inner side surface H′ of the through hole H.
[0161] like Figure 2 As shown in (a), in a modified example, the anodized film sheet 10 having the through holes H may be arranged so that the barrier layer BL is located on the porous layer PL. Then, the first thin film layer 11 may be arranged on the barrier layer BL.
[0162] In this case, the first thin film layer 11 may also be formed on the inner side surface H' of the through hole H. As described above, the first thin film layer 11 may be formed of a plurality of first monoatomic layers 11a having a constant thickness formed by chemical substitution of the 1-1 precursor and the 1-2 reactant.
[0163] Therefore, the first thin film layer 11 may be configured to coat the inner side surface H′ of the through hole H with a constant thickness.
[0164] Thus, variations may have wear resistance and / or corrosion resistance to specific configurations within.
[0165] For example, the anodized film structure AS' can be configured in a probe card (vertical type) with the probe 60 arranged in the through hole H. The through holes H of the anodized film structure AS' can be arranged with a narrow pitch according to the probe 60 that requires a narrow pitch. Therefore, the thickness of the partition wall between the through holes H can be thin.
[0166] Sliding friction with the probe 60 may occur on the inner side surface H' of the through hole H. The sliding friction increases the risk of wearing the inner side surface H' of the through hole H and damaging the product.
[0167] However, in the modified example of the present invention, the first thin film layer 11 disposed on the inner side surface H′ of the through hole H can ensure the wear resistance against sliding friction.
[0168] In addition, in the modified example, since the first thin film layer 11 compensates for the thin thickness of the partition wall between the through holes H with a narrow pitch, the wear resistance against the thin thickness can be improved.
[0169] On the other hand, the modification example can also be configured to eject a specific fluid in a semiconductor or display device. In this case, the modification example can perform the function of ejecting the specific fluid through the through hole H.
[0170] The inner side surface H' of the through hole H may cause a chemical reaction or corrosion due to the specific fluid passing through the through hole H. Therefore, the inner side surface H' of the through hole H may be damaged or particles may be generated. In this case, the conventional structure for performing the fluid ejection function may cause a problem of ejecting particles together with the function of ejecting the specific fluid.
[0171] However, the anodized film structure AS' of the present invention can ensure chemical resistance to the fluid passing through the through hole H by configuring the first thin film layer 11 on the inner side surface H' of the through hole H. Specifically, in the case where the modification is configured to perform the function of ejecting a specific fluid, the first thin film layer 11 can be formed of a component having chemical resistance to the specific fluid. Therefore, the modification can prevent the problem of corrosion or chemical reaction caused by the fluid passing through the through hole H. Therefore, the modification can have the characteristics of corrosion resistance and chemical resistance.
[0172] Figure 2 (b) is a diagram showing a structure in which the anodized film sheet 10 is arranged so that the porous layer PL is located on the upper part of the barrier layer BL and the first thin film layer 11 is arranged on the upper surface of the porous layer PL. In this case, the anodized film sheet 10 may be provided with through holes H.
[0173] Figure 2 The modification shown in (b) is Figure 1 The structure of (b) is different in that a through hole H is provided in the anodized film sheet 10, and the rest of the structure may be the same.
[0174] in addition, Figure 2 The method of configuring the first thin film layer 11 on the inner side surface H' of the through hole H in (b) can be similar to Figure 1 Embodiments of (b) and Figure 2 The method for forming the first thin film layer 11 of the modification example (a) is the same. Figure 2 The structure and configuration of the modified example shown in (b) will be described with reference to Figure 1 (b) and Figure 2 (a) is omitted.
[0175] Figure 2 (c) is a diagram showing a structure in which the first thin film layer 11 is arranged on the upper and lower surfaces of the anodized film sheet 10 having the through hole H. In this case, the first thin film layer 11 may be arranged on the inner side surface H' of the through hole H with a constant thickness.
[0176] Figure 2 An embodiment of (c) with Figure 1 The difference of the embodiment (c) is that a through hole H is provided. Therefore, the description of the same structure will refer to Figure 1 (c) is omitted.
[0177] Figure 2 A variation of (c) can be obtained by Figure 1 Embodiments of (c) and Figure 2 The first thin film layer 11 is arranged in the through hole H in the same manner as the method for forming the first thin film layer 11 of the modified example (a). Figure 2 (a) is omitted for reference only.
[0178] Figure 2 (d) is a diagram showing an anodized film structure AS' in which the anodized film sheet 10 provided with the through-holes H is arranged so that the barrier layer BL is located on the upper part of the porous layer PL.
[0179] The anodized film structure AS' may be formed by forming the first thin film layer 11 on the barrier layer BL on the upper surface and then forming the second thin film layer 12. In this case, Figure 1 The first thin film layer 11 and the second thin film layer 12 are formed by the same method as the method for forming the first thin film layer 11 and the second thin film layer 12 in (d).
[0180] The first thin film layer 11 and the second thin film layer 12 may be disposed on the upper surface of the anodized film structure AS′, and the first thin film layer 11 and the second thin film layer 12 may be disposed on the inner side surface H′ of the through hole H.
[0181] Through Figure 1 Embodiments of (d) and Figure 2 The first thin film layer 11 is disposed on the inner side surface H′ of the through hole H in the same manner as the method for forming the first thin film layer 11 of the modified example (a).
[0182] Then, the anodized film structure AS' may perform the method of forming the second thin film layer 12. As described above, the second thin film layer 12 may be formed of a plurality of second monoatomic layers formed to a fixed thickness by chemical substitution of the 2-1st precursor and the 2-2nd reactant.
[0183] The second film layer 12 may be formed to cover the upper surface of the first film layer 11 formed on the inner side surface H′ of the through hole H. In this case, the second film layer 12 may be formed to a thickness not enough to fill the through hole H so as to maintain the function of the through hole H.
[0184] In such Figure 2 In the modification shown in (d), the wear resistance of the inner side surface H' of the through hole H can be further improved when the probe 60 is configured. In addition, the thin thickness of the partition wall between the through holes H is formed thicker by the first film layer 11 and the second film layer 12, thereby improving the wear resistance and the durability of the product itself.
[0185] on the other hand, Figure 2 The modified example (d) is a structure that performs a fluid ejection function and can be configured in a semiconductor or display device. In this case, the anodized film structure AS' can be configured with a first thin film layer 11 and a second thin film layer 12 on the upper surface of the barrier layer BL and the inner side surface H' of the through hole H.
[0186] The first thin film layer 11 and the second thin film layer 12 may be formed on the upper surface of the barrier layer BL with a fixed thickness, thereby improving the surface strength of the anodized film structure AS'.
[0187] In addition, the first film layer 11 and the second film layer 12 may be formed with a fixed thickness on the inner side surface H' of the through hole H. The first film layer 11 and the second film layer 12 may be configured from constituent components having chemical resistance to the fluid passing through the through hole H, thereby imparting chemical resistance to the anodized film structure AS'.
[0188] In addition, the first film layer 11 and the second film layer 12 have chemical resistance and can prevent the inner side surface H' of the through hole H from being corroded due to chemical reaction. Therefore, the first film layer 11 and the second film layer 12 can impart corrosion resistance to the anodized film structure AS'.
[0189] The first thin film layer 11 and the second thin film layer 12 may be formed of different components and have different properties.
[0190] Specifically, the first film layer 11 may be directly formed on the inner side surface H′ of the through hole H. The second film layer 12 may be formed on the upper surface of the first film layer 11 . Therefore, the fluid passing through the through hole H may directly contact the second film layer 12 .
[0191] In the above case, the first film layer 11 may be formed of a component having excellent rigidity that can increase the strength of the thickness of the partition wall between the through holes H on the inner side surface H' of the through holes H. In this case, the second film layer 12 may be formed of a component having chemical resistance to the fluid.
[0192] Therefore, the anodized film structure AS' can ensure high rigidity and chemical resistance through the first film layer 11 and the second film layer 12. In addition, since the anodized film structure AS' has chemical resistance through the second film layer 12, corrosion caused by the fluid may not occur. Therefore, the anodized film structure AS' can have high rigidity, chemical resistance and corrosion resistance at the same time.
[0193] The anodized film structure AS of the present invention can be used in the field of semiconductors or displays. In this case, the anodized film structure AS can be configured in a deformed structure according to the function, and can be configured with additional configurations.
[0194] As an example, the anodized film structure AS may include an anodized film sheet 10 having a through hole H and a first thin film layer 11 disposed on at least one side of the anodized film sheet 10 and an inner side surface H' of the through hole H. The structure of the anodized film structure AS is not limited thereto and may refer to Figure 1 (a) to Figure 1 (d) Figure 2 (a) to Figure 2 The structures and configurations of the various embodiments and modifications described in (d) are used in the semiconductor or display fields.
[0195] Figure 7 The figure schematically shows a probe card 20 having a structure in which the anodic oxide film structure AS of the present invention is arranged as a multilayer wiring substrate. The multilayer wiring substrate of the probe card 20 may be provided with probe connection pads 61 electrically connected to the probes 60 .
[0196] The probe card 20 can perform a function of applying an electrical signal to chips constituting the semiconductor wafer W to determine whether there is a defect.
[0197] According to the structure of placing the probe 60 on the wiring substrate and the structure of the probe 60 , the probe card can be divided into a vertical type probe card 30 , a cantilever type probe card and a MEMS probe card 20 .
[0198] like Figure 7 As shown, as an example, the anodized film structure AS′ may be disposed in the MEMS probe card 20 .
[0199] The anodized film structure AS' can be formed by stacking a plurality of anodized film sheets 10. In this case, the anodized film sheets 10 are stacked up and down and bonded to each other via the bonding layer 70, and the metal substance M can be arranged in the through hole H to be used as a multilayer wiring board.
[0200] The anodized film structure AS' can be provided with the anodized film sheet 10 constituting the layer on the surface so that the surface thereof can be formed of the barrier layer BL.
[0201] Specifically, if Figure 7 As shown, the anodic oxide film structure AS' can be configured with a barrier layer BL on the porous layer PL to form an anodic oxide film sheet 10 on the upper surface. Here, the upper surface of the anodic oxide film structure AS' can be a surface configured with an interposer connection pad 22 electrically connected to the interposer 21.
[0202] The anodic oxide film structure AS' may have a structure in which a barrier layer BL is disposed below the porous layer PL, and the anodic oxide film sheet 10 may constitute the lower surface. Here, the lower surface of the anodic oxide film structure AS' may be the surface on which the probe connection pad 61 is disposed.
[0203] With the above-described structure, the upper surface and the lower surface of the anodized film structure AS' can be formed by the barrier layer BL.
[0204] The anodized film sheet 10 may have a structure including a porous layer PL with pores P formed therein and a barrier layer BL without pores P, and the upper and lower surfaces are asymmetrical. Due to the structure described above, the anodized film sheet 10 may have density differences between the upper and lower surfaces.
[0205] Therefore, when the anodized film sheet 10 constitutes an anodized film structure AS′ that functions as a multilayer wiring board as a single piece, warping and deformation may occur in a high temperature environment.
[0206] The anodized film structure AS' of the present invention may include a plurality of anodized film sheets 10, and is formed in a structure in which the surfaces thereof are symmetrical with respect to the barrier layer BL.
[0207] The above structure can make the density of the upper and lower surfaces of the anodized film structure AS' uniform, so that warping and deformation will not occur even in a high temperature environment. Due to the above structure, the durability of the anodized film structure AS' can be improved first.
[0208] In addition, the present invention can form the upper surface and the lower surface by the barrier layer BL, and configure the first film layer 11 on the upper surface of the barrier layer BL. The first film layer 11 can have high rigidity and strength characteristics, as shown in FIG. Figure 1 described.
[0209] The present invention can configure the first film layer 11 as described above on the surface of the barrier layer BL constituting the upper surface and the lower surface. Since the first film layer 11 is formed with a fixed thickness, the strength of the product itself can be further improved while maintaining the uniform density of the anodized film structure AS'. Through the above-mentioned structure, the present invention can further improve durability. Therefore, the anodized film structure AS' of the present invention can have the characteristics of high durability.
[0210] like Figure 7 As shown in the enlarged portion of FIG. 1 , the anodized film sheets 10 may be bonded to each other via a bonding layer 70 .
[0211] The bonding layer 70 can be configured by a photolithography process. Therefore, the bonding layer 70 can be formed by a photosensitive material that retains photosensitivity characteristics. As an example, the bonding layer 70 can be a dry film photoresist (DFR). In addition, since the bonding layer 70 performs a bonding function of bonding the anodized film sheets 10, it can be a structure that retains bonding characteristics. Therefore, the bonding layer 70 can be configured by a structure that retains both photosensitivity characteristics and bonding characteristics.
[0212] On the other hand, the bonding layer 70 may be a thermosetting resin, such as polyimide resin, polyquinoline resin, polyamide-imide resin, epoxy resin, polyphenylene ether resin, fluororesin, etc.
[0213] The MEMS probe card 20 can be configured by performing a process of bonding the separately manufactured probes 60 to the probe connection pads 61. Therefore, the anodized film structure AS' can perform a process of bonding the probes 60 to the surface where the probe connection pads 61 are configured.
[0214] The probe 60 may be separately fabricated in the temporary substrate and removed from the temporary substrate at one time after being bonded to the probe connection pad 61. In the process described above, the probe 60 may be removed from the temporary substrate by a specific chemical.
[0215] The anodized film sheet 10 may be damaged by certain chemicals used in the process of removing the probe 60 .
[0216] However, the anodized film structure AS' of the present invention can ensure chemical resistance by configuring the first thin film layer 11 on the surface of the anodized film sheet 10. Therefore, the anodized film structure AS' of the present invention is a structure that performs the function of a multilayer wiring substrate and is not damaged by specific chemicals when configured in the probe card 20.
[0217] In addition, the present invention can also have corrosion resistance characteristics by the components constituting the first film layer 11. Therefore, the present invention protects the surface by the first film layer 11, so even if exposed to a process using specific chemicals, the corrosion resistance characteristics can minimize surface corrosion.
[0218] In addition, the present invention can be formed with a structure in which the surface is sealed by the first thin film layer 11. The MEMS probe card 20 can be configured with the present invention in the form of a multilayer wiring substrate electrically connected to the probe 60. In the conventional multilayer wiring substrate, when particles flow into the inside, the characteristics of the probe 60 may be degraded.
[0219] However, the present invention can prevent the problem of particles flowing into the interior by the first thin film layer 11. Therefore, when the present invention is configured in the MEMS probe card 20, the degradation of characteristics due to the flow of particles can be prevented in advance.
[0220] Figure 8 This is a diagram schematically showing a vertical probe card 30 in which the anodized film structure AS' of the present invention is arranged.
[0221] The vertical probe card 30 may be provided with a guide plate for supporting the probes 60 to accurately position the insertion of the probes 60. The anodized film structure AS of the present invention may be provided on the vertical probe card 30 and function as a guide plate.
[0222] like Figure 8 As shown, the anodized film structure AS′ can be disposed at the lower portion of the wiring substrate 31 , and the probe 60 can be disposed in the through hole H and supported.
[0223] The anodic oxide film structure AS′ may include an upper anodic oxide film structure AS and a lower anodic oxide film structure AS, and is disposed in the vertical probe card 30 .
[0224] In this case, the anodized film structure AS′ may be arranged by being supported by a plate composed of the first plate 32 and the second plate 34 .
[0225] The first plate 32 and the second plate 34 may be configured in a corresponding structure and combined in an inverted form. Specifically, the second plate 34 may be combined to the lower portion of the first plate 32 in an inverted form with the first plate 32. Such plates 32 and 34 may be configured with an anodic oxide film structure AS'.
[0226] like Figure 8 As shown, the first plate 32 may include an upper mounting region 40 for disposing an upper anodized film structure AS. The second plate 34 may include a lower mounting region 50 for disposing a lower anodized film structure AS.
[0227] The first plate 32 and the second plate 34 may be coupled to each other in an inverted manner. Therefore, the upper mounting area 40 and the lower mounting area 50 may be arranged in the same shape at the inverted positions.
[0228] In the first plate 32 , the first through hole 33 is disposed at a lower portion of the upper mounting region 40 , and in the second plate 34 , the second through hole 35 may be disposed at an upper portion of the lower mounting region 50 .
[0229] The first through hole 33 and the second through hole 35 may be configured to position a plurality of probes 60 inserted through the upper through hole H1 and the lower through hole H2 described later. Therefore, the first through hole 33 and the second through hole 35 may be formed with an inner diameter capable of accommodating the plurality of probes 60 in consideration of elastic deformation of the plurality of probes 60.
[0230] The board may be provided with an anodic oxide film structure AS in each mounting area 40 , 50 .
[0231] The upper anodized film structure AS may be provided with an upper through hole H1, and the lower anodized film structure AS may be provided with a lower through hole H2. Therefore, the through hole H of the anodized film structure AS' may be composed of the upper through hole H1 and the lower through hole H2.
[0232] The anodized film structure AS' can be configured by bonding multiple anodized film sheets 10 together vertically through a bonding layer 70. In this case, multiple anodized film sheets 10 can be stacked and bonded so that the through holes H correspond to each other. The present invention can improve rigidity by stacking the anodized film sheets 10.
[0233] The anodized film structure AS' may be configured such that a plurality of anodized film sheets 10 are arranged such that the surface thereof is formed by the barrier layer BL.
[0234] As an example, Figure 8 As shown in the enlarged part of FIG. 1 , the lower anodized film structure AS may include a first anodized film sheet 10a and a second anodized film sheet 10b. Figure 8 In the figure, two anodized film sheets 10 are shown, but the number of the anodized film sheets 10 may be more than two.
[0235] In this case, the first anodized film sheet 10a may be configured with a barrier layer BL disposed on the upper portion of the porous layer PL, thereby constituting the upper surface of the lower anodized film structure AS.
[0236] The second anodized film sheet 10 b may be disposed below the first anodized film sheet 10 a . In this case, the first anodized film sheet 10 a and the second anodized film sheet 10 b may be bonded together via the bonding layer 70 .
[0237] The second anodized film sheet 10b may have a structure in which a barrier layer BL is disposed below the porous layer PL, and constitutes the lower surface of the lower anodized film structure AS.
[0238] Therefore, the lower anodized film structure AS can have a structure in which the upper surface and the lower surface are formed symmetrically with respect to the barrier layer BL. Due to the structure as described above, the density of the upper surface and the lower surface of the lower anodized film structure AS can be made uniform. Therefore, the effect of the anodized film structure AS' in preventing warping deformation can be improved.
[0239] The upper anodized film structure UAS and the lower anodized film structure LAS can have the same structure and configuration. Therefore, the upper anodized film structure UAS can have the same structure and configuration as the lower anodized film structure LAS, thereby playing an effect in preventing warping deformation.
[0240] In addition, the anodized film structure AS′ can minimize damage caused by wear during the insertion of the probe 60 by making the density of the upper surface and the lower surface uniform by using the barrier layer BL.
[0241] Specifically, when the anodized film structure AS is configured as a guide plate, the probe 60 insertion process can be performed. At this time, the inner wall of the opening of the through hole H in the anodized film structure AS' of the present invention can be formed by the high-density barrier layer BL.
[0242] Therefore, in the present invention, the durability against wear generated in the inner wall of the upper opening of the through hole H where the front end of the probe 60 is first inserted can be relatively high. Therefore, the present invention can prevent the particle problem generated by wear of the opening of the through hole H when the probe 60 is inserted.
[0243] In addition, if Figure 8 As shown in the enlarged part of FIG. 1 , the present invention can configure the first thin film layer 11 on the surface of the anodized film structure AS. The first thin film layer 11 can be configured by forming it on the surface of the anodized film sheet 10 after bonding the anodized film sheet 10 up and down.
[0244] As an example, the first film layer 11 may be disposed on the entire upper and lower surfaces of the anodized film structure AS′, and on the inner side surface H′ of the through hole H. In this case, the first film layer 11 may ensure further improved wear resistance.
[0245] Specifically, one end of the probe 60 can be first inserted into the upper through hole H1 and then inserted into the lower through hole H2. Therefore, the probe 60 can be configured as follows: the other end 60c is located in the upper through hole H1, the middle part 60b is located in the first through hole 33 and the second through hole 35, and the first inserted end 60a is inserted into the lower through hole H2 of the lower anodized film structure LAS and protrudes.
[0246] In the present invention, since the first film layer 11 is disposed on the inner side surface H′ of the through hole H, during the insertion of the probe 60 as described above, the inner side surface H′ including the inner wall of the opening of the through hole H can be a structure with improved wear resistance as a whole.
[0247] With the above-described structure, the present invention can prevent the inner side surface H′ of the through hole H from being damaged by the probe 60 during the process of inserting the probe 60 into the through hole H.
[0248] In addition, the present invention can improve the wear resistance to the sliding friction between the through hole H and the probe 60 by the first thin film layer 11. In the anodized film sheet 10, since the through holes H are arranged at a narrow pitch, the thickness of the partition wall between the through holes H can be formed thin. Therefore, in the anodized film sheet 10, the problem of the inner side surface H' of the through hole H being easily worn due to the sliding friction between the through hole H and the probe 60 may occur.
[0249] However, the present invention can compensate for the thickness of the thin partition wall between the through holes H by disposing the first film layer 11 on the inner side surface H' of the through hole H. Therefore, the present invention can improve the wear resistance to the sliding friction between the through hole H and the probe 60. Therefore, even if the present invention is used for a long time, the risk of damage due to wear can be minimized, thereby improving durability.
[0250] In addition, the present invention may be a structure in which the surface is sealed by the first film layer 11. Therefore, the present invention can prevent the problem of particles flowing into the interior.
[0251] Thus, when the present invention is configured as a guide plate of a vertical probe card 30, the durability can be improved. In addition, the present invention can ensure the wear resistance to sliding friction. Therefore, the present invention can function as a guide plate as a structure having both durability and wear resistance.
[0252] Since the anodized film structure AS of the present invention is formed of the anodized film A material, thermal deformation can be small in a high temperature environment. Therefore, the present invention can be effectively used in the semiconductor or display field that requires a process to be performed in a high temperature atmosphere.
[0253] As an example, the probe cards 20 and 30 of the present invention can be used to perform a burn-in test for ensuring chip reliability. The burn-in test can be performed at a high temperature of 85° C. or 100° C. Therefore, the anodized film structure AS can be exposed to high temperatures.
[0254] However, the present invention can reduce thermal deformation caused by high temperature due to the low thermal expansion coefficient. Therefore, even if the present invention is provided with a through hole H, the problem of a difference between the position of the through hole H and the inspection position of the inspection object can be prevented. Therefore, the present invention can prevent the problem of a decrease in the positional accuracy of the additional structure provided in the through hole H.
[0255] In addition, the present invention can have the characteristics of durability, chemical resistance and wear resistance by including the first thin film layer 11. At the same time, the present invention can solve the problem of re-exposure of the crack C portion caused by corrosion of the conventional thin film layer 11' and the problem of outgassing caused by the pores P. Therefore, when the present invention is configured as a structure that performs a specific function in a specific field, the efficiency of the overall performance of the product can be improved.
[0256] As described above, although the present invention has been described with reference to the preferred embodiments, a person skilled in the art may make various modifications or variations to the present invention without departing from the scope of the invention and the scope of the invention described in the above claims.
Claims
1. An anodic oxide film structure, include: An anodic oxide film sheet, comprising a non-porous barrier layer having no pores formed therein and a porous layer located below the barrier layer and having pores formed therein; as well as a first film layer disposed on the upper surface of the non-porous barrier layer, The first thin film layer includes a plurality of first monoatomic layers formed by repeatedly performing the following cycle: adsorbing a 1-1 precursor, supplying a 1-2 reactant of a different type from the 1-1 precursor, and generating the first monoatomic layer by chemical substitution of the 1-1 precursor and the 1-2 reactant.
2. The anodic oxide film structure according to claim 1, wherein The thickness of the first thin film layer is between 20 nm and 3 μm.
3. The anodic oxide film structure according to claim 1, wherein The thickness of the barrier layer is between 100 nm and 1 μm.
4. The anodic oxide film structure according to claim 1, wherein A second thin film layer including a plurality of second monoatomic layers formed by repeatedly performing the following cycle is formed, wherein a 2-1st precursor is adsorbed on an upper portion of the first thin film layer, a 2-2nd reactant of a different type from the 2-1st precursor is supplied, and the second monoatomic layer is generated by chemical substitution between the 2-1st precursor and the 2-2nd reactant, The first film layer and the second film layer have different constituent components.
5. An anodic oxide film structure, include: An anodized film sheet includes a non-porous barrier layer having no pores formed therein and a porous layer located below the barrier layer and having pores formed therein. A first film layer is disposed on the upper surface of the non-porous barrier layer and inside the pores of the porous layer, The first thin film layer includes a plurality of first monoatomic layers formed by repeatedly performing the following cycle: adsorbing a 1-1 precursor, supplying a 1-2 reactant of a different type from the 1-1 precursor, and generating the first monoatomic layer by chemical substitution of the 1-1 precursor and the 1-2 reactant.
6. An anodic oxide film structure, include: An anodized film sheet includes a non-porous barrier layer having no pores formed therein, a porous layer located below the barrier layer and having pores formed therein, and through holes arranged to penetrate the non-porous barrier layer and the porous layer. a first film layer disposed on the upper surface of the non-porous barrier layer and on the inner side surface of the through hole, The first thin film layer includes a plurality of first monoatomic layers formed by repeatedly performing the following cycle: adsorbing a 1-1 precursor, supplying a 1-2 reactant of a different type from the 1-1 precursor, and generating the first monoatomic layer by chemical substitution of the 1-1 precursor and the 1-2 reactant.
7. The anodic oxide film structure according to claim 6, wherein The anodized film sheets are stacked up and down and bonded to each other through a bonding layer. A metal substance is disposed in the through hole.