Polycarbonate resin compositions and their manufacturing methods, masterbatch granules and molded articles
By adding ingredients such as olefin polymers and fatty acid metal salts to polycarbonate resin, an island structure is formed to avoid hydrolysis, solve the processability and appearance problems caused by glass fiber, and realize efficient mixing and molding of polycarbonate resin. Obtain excellent mechanical properties and appearance.
Patent Information
- Application Number
- CN201980084903.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-27
- Filing Date
- 2019-12-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2039-12-25
AI Technical Summary
Polycarbonate resin compositions containing glass fibers have problems with workability and the impact strength of molded articles, and the appearance is damaged by the glass fibers. At the same time, fibrous alkaline magnesium sulfate can cause damage to polycarbonate resins that are not resistant to alkali. Causes hydrolysis and affects mixing and molding.
Ingredients such as olefin polymers, fatty acid metal salts and fatty acids are added to the polycarbonate resin to form an island structure to avoid direct contact between alkaline magnesium sulfate and the polycarbonate resin, thereby avoiding hydrolysis and improving processability through melting and mixing.
It realizes hydrolysis-free mixing and molding of polycarbonate resin, and obtains a molded body with excellent processability, mechanical properties and good appearance.
Smart Images

Figure CN113227219B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polycarbonate resin composition and a method for producing the same, a masterbatch pellet and a molded body. Background Art
[0002] Polycarbonate resin has excellent mechanical properties and thermal properties, and is therefore widely used in various fields such as OA equipment, electronic and electrical equipment, and the automotive field. However, polycarbonate resin has poor processability due to its high melt viscosity, and has poor chemical resistance due to its amorphous resin. Therefore, in order to improve the chemical resistance of polycarbonate resin, it is known to add polyolefin resin to polycarbonate resin. In order to improve the compatibility of the two different properties and to impart practical mechanical properties, many resin compositions with elastomers or fillers added thereto have been proposed.
[0003] For example, Patent Document 1 discloses a technique in which a styrene-based thermoplastic elastomer is added as a compatibilizer to a resin comprising a polycarbonate-based resin and a polypropylene-based resin, and a fibrous filler such as glass fiber or carbon fiber is further added to impart mechanical properties including rigidity to a polycarbonate resin composition.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-204480 Summary of the invention
[0007] Problems to be solved by the invention
[0008] However, polycarbonate resin compositions containing glass fibers have problems in processability. In addition, molded articles obtained by curing polycarbonate resin compositions containing glass fibers not only have insufficient impact strength, but also may have an appearance impaired by the glass fibers.
[0009] Therefore, as a filler material having a fiber diameter smaller than that of glass fiber and having an excellent appearance while having a reinforcing effect, fibrous basic magnesium sulfate has attracted attention. Fibrous basic magnesium sulfate is a safe filler material with biosolubility. However, fibrous basic magnesium sulfate is weakly alkaline, so if it is added to an alkali-intolerant polycarbonate resin, the polycarbonate resin will be hydrolyzed. In this case, there will be a problem that mixing itself cannot be carried out.
[0010] Therefore, an object of the present invention is to provide a polycarbonate resin composition and a method for producing the same, a masterbatch pellet and a molded product, wherein the polycarbonate resin composition does not undergo hydrolysis, can be kneaded / molded, and can obtain a molded product having excellent processability, good mechanical properties and good appearance.
[0011] Means for solving problems
[0012] The present inventors have conducted intensive studies to achieve the above-mentioned purpose and have found that even when fibrous basic magnesium sulfate is added to a polycarbonate resin, if it contains an olefin polymer, at least one selected from a fatty acid metal salt and a fatty acid, and an elastomer, the polycarbonate resin can be kneaded without hydrolysis and the processability is improved, thereby completing the present invention.
[0013] That is, the present invention relates to a polycarbonate resin composition, characterized in that it contains 50% to 90% by mass of a polycarbonate resin (A), 2.0% to 20% by mass of an olefin polymer (B), 5% to 40% by mass of a basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), 0.1% to 8% by mass of at least one (D) selected from fatty acid metal salts and fatty acids, and 1% to 20% by mass of an elastomer (E).
[0014] In addition, the present invention relates to a method for producing a polycarbonate resin composition, characterized in that it comprises the following steps: a first step of melt-kneading 2% to 50% by mass of an olefin polymer (B), 40% to 70% by mass of basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), 0.1% to 5% by mass of at least one (D) selected from fatty acid metal salts and fatty acids, and 1% to 50% by mass of an elastomer (E) to obtain a masterbatch pellet; and a second step of melt-kneading 10% to 60% by mass of the masterbatch pellet and 40% to 90% by mass of a polycarbonate resin (A) to produce a polycarbonate resin composition.
[0015] In addition, the present invention relates to a method for producing a polycarbonate resin composition, characterized in that it comprises the following steps: a first step of melt-kneading 28% to 50% by mass of an olefin polymer (B), 40% to 70% by mass of basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), and 0.1% to 5% by mass of at least one (D) selected from fatty acid metal salts and fatty acids to obtain a masterbatch pellet; and a second step of melt-kneading 10% to 59% by mass of the masterbatch pellets, 40% to 89% by mass of a polycarbonate resin (A), and 1% to 20% by mass of an elastomer (E) to produce a polycarbonate resin composition.
[0016] In addition, the present invention relates to a method for producing a polycarbonate resin composition, characterized in that 50% to 90% by mass of a polycarbonate resin (A), 2.0% to 20% by mass of an olefin polymer (B), 5% to 40% by mass of basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), 0.1% to 8% by mass of at least one (D) selected from fatty acid metal salts and fatty acids, and 1% to 20% by mass of an elastomer (E) are melt-kneaded.
[0017] In addition, the present invention relates to a method for producing a polycarbonate resin composition, characterized in that 2.0% to 20% by mass of an olefin polymer (B), 5% to 40% by mass of basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), 0.1% to 8% by mass of at least one (D) selected from fatty acid metal salts and fatty acids, and 1% to 20% by mass of an elastomer (E) are melt-kneaded, and then 50% to 90% by mass of a polycarbonate resin (A) is added and melt-kneaded.
[0018] The present invention also relates to a masterbatch pellet, characterized in that it is a masterbatch pellet for kneading with a diluent material containing a polycarbonate resin (A) to produce a polycarbonate resin composition, and comprises 2% to 50% by mass of an olefin polymer (B), 40% to 70% by mass of basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), 0.1% to 5% by mass of at least one (D) selected from fatty acid metal salts and fatty acids, and 1% to 50% by mass of an elastomer (E).
[0019] Furthermore, the present invention relates to a molded product, characterized in that it is a molded product of the above-mentioned polycarbonate resin composition.
[0020] Effects of the Invention
[0021] According to the present invention, a polycarbonate resin composition and a method for producing the same, a masterbatch pellet and a molded product can be provided. The polycarbonate resin composition does not undergo hydrolysis, can be kneaded / molded, and can obtain a molded product having excellent processability, mechanical properties and good appearance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a scanning electron microscope photograph of fan-shaped basic magnesium sulfate.
[0023] Figure 2 This is a transmission electron microscope (TEM) photograph of the polycarbonate resin composition of Example 2. DETAILED DESCRIPTION
[0024] 1. Polycarbonate resin composition
[0025] The polycarbonate resin composition of the present invention comprises 50% to 90% by mass of a polycarbonate resin (A), 2.0% to 20% by mass of an olefin polymer (B), 5% to 40% by mass of a basic magnesium sulfate (C) selected from a fibrous basic magnesium sulfate (C-1) and a fan-shaped basic magnesium sulfate (C-2), 0.1% to 8% by mass of at least one (D) selected from a fatty acid metal salt and a fatty acid, and 1% to 20% by mass of an elastomer (E). The polycarbonate resin composition of the present invention comprises the components in the above ratios to form a sea-island structure in which an island portion containing the remaining components is dispersed in a sea portion containing the polycarbonate resin.
[0026] The periphery of the island portion is composed of an elastomer. In the interior of the island portion, basic magnesium sulfate and residual components such as olefin polymers are mixed and exist. Thus, direct contact between basic magnesium sulfate and the polycarbonate resin in the sea portion can be avoided. As a result, it is believed that the polycarbonate resin can be mixed / molded into a polycarbonate resin composition without hydrolysis. Below, each component is explained.
[0027] (A) Polycarbonate resin
[0028] The polycarbonate resin is not particularly limited, and for example, aliphatic polycarbonate, aromatic polycarbonate, etc. can be used. Among these, aromatic polycarbonate is preferred. The polycarbonate resin can be a commercially available product or a synthesized product as appropriate.
[0029] As the method for synthesizing polycarbonate resin, there is no particular restriction, and can be suitably selected according to purpose. For example, the method for synthesizing dihydric phenol and carbonate precursors such as solution method or melting method etc. can be enumerated. In addition, as required, molecular weight regulator, branching agent, catalyst etc. can also be suitably used.
[0030] Examples of the dihydric phenol include bisphenol A [2,2-bis(4-hydroxyphenyl)propane], hydroquinone, 2,2-bis(4-hydroxyphenyl)pentane, 2,4'-dihydroxydiphenylmethane, bis(2-hydroxyphenyl)methane, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-5-nitrophenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 3,3-bis(4-hydroxydiphenyl)pentane, 2,2'-dihydroxybiphenyl, 4,4'-dihydroxybiphenyl, 2,6-dihydroxynaphthalene, bis(4-hydroxyphenyl)sulfone, bis(3,5-diethyl-4-hydroxyphenyl)sulfone, 2,2-bis(3,5-dimethyl-4 -hydroxyphenyl) propane, 2,4'-dihydroxydiphenyl sulfone, 5'-chloro-2,4'-dihydroxydiphenyl sulfone, bis(4-hydroxyphenyl) diphenyl ether, 4,4'-dihydroxy-3,3'-dichlorophenyl ether, 4,4'-dihydroxy-2,5-dichlorodiphenyl ether, bis(4-dihydroxy-5-propylphenyl) methane, bis(4-dihydroxy-2,6-dimethyl-3-methoxyphenyl) methane, 1,1-bis(4-hydroxy-2-ethylphenyl) ethane, 2,2-bis(3-phenyl-4-hydroxyphenyl) propane, bis(4-hydroxyphenyl) cyclohexylmethane, 2,2-bis(4-hydroxyphenyl)-1-phenylpropane, etc. These can be used alone or in combination of two or more. Among these, bis(4-hydroxyphenyl) alkane compounds are preferred from the perspective of ease of market availability, and bisphenol A is particularly preferred.
[0031] The carbonate precursor is not particularly limited and may be appropriately selected depending on the intended purpose, and examples thereof include acid halides, carbonates, and halogen formats, and specifically, phosgene, diphenyl carbonate, dihalogen formats of dihydric phenols, and mixtures thereof.
[0032] The melt flow rate (MFR) of the polycarbonate resin can be appropriately selected according to the purpose, preferably 2g / 10min to 25g / 10min, more preferably 2g / 10min to 10g / 10min. If the melt flow rate of the polycarbonate resin is 2g / 10min or more, a polycarbonate resin composition with good molding processability can be obtained. In addition, if the above-mentioned melt flow rate is 25g / 10min or less, sufficient impact strength can be given to the molded body.
[0033] The content of the polycarbonate resin is in the range of 50% to 90% by mass, preferably in the range of 55% to 75% by mass, relative to the total amount of the polycarbonate resin composition. If the content of the polycarbonate resin is 50% by mass or more, a molded body having high impact strength due to the polycarbonate resin can be obtained. On the other hand, if the content of the polycarbonate resin is 90% by mass or less, the reinforcing effect of the filler is fully exerted, and the desired bending modulus can be given to the molded body.
[0034] (B) Olefin polymer
[0035] As the olefin polymer, ethylene polymer, propylene polymer, ethylene-propylene random copolymer, ethylene-propylene block copolymer, etc. can be mentioned, and propylene polymer is particularly preferred, and propylene homopolymer (propylene homopolymer) is more preferred. The olefin polymer can be used alone or in combination of two or more. The melt flow rate (MFR) of the olefin polymer is usually in the range of 3g / 10min to 300g / 10min, preferably in the range of 6g / 10min to 100g / 10min.
[0036] The content of the olefin polymer is in the range of 2.5% to 20% by mass, preferably in the range of 8% to 15% by mass, relative to the total amount of the polycarbonate resin composition. If the content of the olefin polymer is 2.5% by mass or more, hydrolysis of the polycarbonate resin caused by basic magnesium sulfate can be suppressed. On the other hand, if the content of the olefin polymer is 20% by mass or less, a molded body having a desired impact strength can be obtained.
[0037] (C) Basic magnesium sulfate
[0038] As the basic magnesium sulfate, at least one selected from the group consisting of fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2) described below is used.
[0039] (C-1) Fibrous basic magnesium sulfate
[0040] Fibrous basic magnesium sulfate can be obtained, for example, by hydrothermal synthesis using magnesium hydroxide and magnesium sulfate produced from seawater as raw materials. The average major diameter of the fibrous basic magnesium sulfate is usually in the range of 5 μm to 100 μm, preferably in the range of 10 μm to 60 μm. In addition, the average minor diameter of the fibrous basic magnesium sulfate is usually in the range of 0.1 μm to 5.0 μm, preferably in the range of 0.2 μm to 2.0 μm, and particularly preferably in the range of 0.2 μm to 1.0 μm.
[0041] Conventionally, the average fiber diameter (average minor diameter) of glass fibers used as fillers is at least about 10 μm. Since the average fiber diameter (average minor diameter) of fibrous basic magnesium sulfate is smaller than that of glass fibers, it is more difficult to identify than glass fibers.
[0042] The average aspect ratio (average major diameter / average minor diameter) of the fibrous basic magnesium sulfate is usually 2 or more, preferably 5 or more, and particularly preferably in the range of 5 to 80. It should be noted that the average major diameter and average minor diameter of the fibrous basic magnesium sulfate can be calculated from the average values of the major diameter and minor diameter of 100 particles measured by an enlarged image obtained by a scanning electron microscope (SEM). In addition, the fibrous basic magnesium sulfate may also be an aggregate or a combination of two or more fibrous particles.
[0043] (C-2) Fan-shaped basic magnesium sulfate
[0044] The fan-shaped basic magnesium sulfate is a particle in which a part of two or more fibrous basic magnesium sulfates are joined to form a fan-shaped particle, for example, the average particle length is 2 μm to 100 μm, the average particle width is 1 μm to 40 μm, and the average aspect ratio is about 1 to 100. Here, the average particle length refers to the size of the particle in the length direction, and the average particle width refers to the maximum size of the particle in the width direction. The length direction of the particle refers to the direction in which the particle length is the largest, and the width direction of the particle refers to the direction orthogonal to the length direction. In addition, the average aspect ratio refers to (average particle length / average particle width).
[0045] Figure 1 1 shows a scanning microscope photograph of an example of fan-shaped basic magnesium sulfate that can be used in the present invention. The fan-shaped basic magnesium sulfate shown here is a fan-shaped bundle formed by two or more fibrous basic magnesium sulfates (average particle length 33.0 μm, average particle width 6.0 μm, average aspect ratio 5.5). The average fiber length of each fibrous basic magnesium sulfate is 33.0 μm, the average fiber diameter is 1.3 μm, and the average aspect ratio is 26.
[0046] The average fiber length of each fibrous basic magnesium sulfate constituting the fan-shaped basic magnesium sulfate is 2 μm to 100 μm, the average fiber diameter is 0.1 μm to 5 μm, and the average aspect ratio is 1 to 1000. For example, two or more fibrous basic magnesium sulfates are bundled at one end and dispersed at the other end. In addition, two or more fibrous basic magnesium sulfates can also be bundled at any position in the length direction and dispersed at both ends. This fan-shaped basic magnesium sulfate can be manufactured and confirmed by the method described in Japanese Patent Publication No. 4-36092 and Japanese Patent Publication No. 6-99147, etc.
[0047] In addition, the fan-shaped basic magnesium sulfate need not be in a state where each fibrous basic magnesium sulfate is confirmed, and a part of the fibrous basic magnesium sulfate may be in a state where the fibrous basic magnesium sulfate is joined to each other in the length direction. If it is confirmed that the fibrous basic magnesium sulfate has the above-mentioned shape and further has an average fiber length, an average fiber diameter, and an average aspect ratio within a specified range, it can be regarded as the fan-shaped basic magnesium sulfate used in the present invention.
[0048] The content of basic magnesium sulfate is in the range of 5% to 40% by mass, preferably in the range of 5% to 30% by mass, and more preferably in the range of 10% to 30% by mass, relative to the total amount of the polycarbonate resin composition. If the content of basic magnesium sulfate is 5% by mass or more, the effect of basic magnesium sulfate can be exerted, and the desired bending elastic modulus can be given to the molded body. On the other hand, if the content of basic magnesium sulfate is 40% by mass or less, a polycarbonate resin composition with good processability can be obtained.
[0049] (D) Fatty acid metal salts and fatty acids
[0050] The polycarbonate resin composition of the present invention contains at least one selected from fatty acid metal salts and fatty acids, so that basic magnesium sulfate is preferentially distributed in the olefin polymer. At least one of fatty acid metal salts and fatty acids can be contained in the polycarbonate resin composition, and fatty acid metal salts are particularly preferred.
[0051] The number of carbon atoms of the fatty acid is preferably in the range of 12 to 22, and it can be a saturated fatty acid or an unsaturated fatty acid. Examples of saturated fatty acids include lauric acid, tridecanoic acid, tetradecanoic acid, pentadecanoic acid, palmitic acid, heptadecanoic acid, stearic acid, nonadecanoic acid, arachidic acid, behenic acid, etc. Examples of unsaturated fatty acids include myristic acid, palmitoleic acid, oleic acid, elaidic acid, vaccenic acid, gadoleic acid, erucic acid, etc. Examples of metal salts include magnesium salts, calcium salts, aluminum salts, lithium salts, zinc salts, etc. It is particularly preferred to be selected from at least one of the group consisting of magnesium stearate, calcium stearate, and aluminum stearate.
[0052] The content of the fatty acid metal salt and the fatty acid is in the range of 0.1% to 8% by mass, preferably in the range of 0.1% to 7% by mass, and more preferably in the range of 0.5% to 6% by mass, relative to the total amount of the polycarbonate resin composition. If the content of the fatty acid metal salt and the fatty acid is 0.1% by mass or more, the effect of adding these compounds can be exerted. On the other hand, if the content of the fatty acid metal salt and the fatty acid is 8% by mass or less, a polycarbonate resin composition with good thermal stability can be obtained.
[0053] (E) Elastomer
[0054] As the elastomer, a styrene-based thermoplastic elastomer is preferably used. The styrene-based thermoplastic elastomer is preferably a block copolymer represented by the following formula (e1) or (e2).
[0055] Xk-Ym-Xn…(e1)
[0056] Xm-Yn…(e2)
[0057] In the above formula, X represents an aromatic vinyl polymer block. In formula (e1), the polymerization degrees at both ends of the molecular chain may be the same or different. In addition, Y is selected from a butadiene polymer block, an isoprene polymer block, a butadiene / isoprene copolymer block, a hydrogenated butadiene polymer block, a hydrogenated isoprene polymer block, a hydrogenated butadiene / isoprene copolymer block, a partially hydrogenated butadiene polymer block, a partially hydrogenated isoprene polymer block, and a partially hydrogenated butadiene / isoprene copolymer block. k, m, and n are integers greater than 1.
[0058] Specific examples include styrene-ethylene / butylene-styrene copolymers, styrene-ethylene / propylene-styrene copolymers, styrene-ethylene / ethylene / propylene-styrene copolymers, styrene-butadiene-butylene-styrene copolymers, styrene-butadiene-styrene copolymers, styrene-isoprene-styrene copolymers, styrene-hydrogenated butadiene diblock copolymers, styrene-hydrogenated isoprene diblock copolymers, styrene-butadiene diblock copolymers, styrene-isoprene diblock copolymers, etc. Among them, styrene-ethylene / butylene-styrene copolymers, styrene-ethylene / propylene-styrene copolymers, styrene-ethylene / ethylene / propylene-styrene copolymers, and styrene-butadiene-butylene-styrene copolymers are most preferred.
[0059] The content of the component X in the block copolymer is 20% to 80% by mass, preferably 30% to 75% by mass, and more preferably 40% to 70% by mass. If the amount of the component X is 20% by mass or more, appropriate rigidity and impact strength can be imparted to the molded product. On the other hand, if the component X is 80% by mass or less, a molded product having a desired impact strength can be obtained.
[0060] The weight average molecular weight of the styrene-based thermoplastic elastomer is preferably 250,000 or less, more preferably 200,000 or less, and further preferably 150,000 or less. If the weight average molecular weight is 250,000 or less, the molding processability is reduced, or the dispersibility in the polycarbonate resin composition is likely to deteriorate. In addition, the lower limit of the weight average molecular weight is not particularly limited, but is preferably 40,000 or more, and more preferably 50,000 or more.
[0061] It should be noted that the weight average molecular weight is a value measured by the following method. That is, the molecular weight is measured in terms of polystyrene by gel permeation chromatography, and the weight average molecular weight is calculated. The melt flow rate (230°C, 2.16kg) of the styrene-based thermoplastic elastomer is preferably 0.1g / 10min to 10g / 10min, more preferably 0.15g / 10min to 9g / 10min, and particularly preferably 0.2g / 10min to 8g / 10min. If the melt flow rate of the styrene-based thermoplastic elastomer is within the range of 0.1 to 10g / 10min, a molded body with sufficient toughness can be obtained.
[0062] The content of the elastomer is in the range of 1% to 20% by mass, preferably in the range of 1% to 15% by mass, and more preferably in the range of 1% to 12% by mass, relative to the total amount of the polycarbonate resin composition. If the content of the elastomer is 1.0% by mass or more, the effect of adding the elastomer can be obtained. On the other hand, if the content of the elastomer is 20% by mass or less, appropriate rigidity and long-term anti-creep properties can be imparted to the molded body.
[0063] In addition, other components may be mixed into the polycarbonate resin composition of the present invention within the range that does not hinder the effect of the present invention. Examples of other components include antioxidants, ultraviolet absorbers, pigments, antistatic agents, copper inhibitors, flame retardants, neutralizers, foaming agents, plasticizers, nucleating agents, anti-bubble agents, crosslinking agents, etc. The content of other components is preferably less than 1% by mass of the entire polycarbonate resin composition, and more preferably less than 0.5% by mass.
[0064] 2. Method for producing polycarbonate resin composition
[0065] Next, the method for producing the polycarbonate resin composition is described. The method for producing the polycarbonate resin composition of the present invention can include: (Production Method I) a method having a first step of melt-kneading an olefin polymer (B), a basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), at least one (D) selected from fatty acid metal salts and fatty acids, and an elastomer (E) to obtain a master batch pellet; and a second step of melt-kneading the master batch pellet and a polycarbonate resin (A) to produce a polycarbonate resin composition; (Production Method II) a method having a first step of melt-kneading an olefin polymer (B), a basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), and at least one (D) selected from fatty acid metal salts and fatty acids to obtain a master batch pellet; and a second step of melt-kneading the master batch pellet and a polycarbonate resin (A) to produce a polycarbonate resin composition. A method for preparing a polycarbonate resin composition by melt-kneading a masterbatch pellet, a polycarbonate resin (A), and an elastomer (E); (Production method III) a method for melt-kneading a polycarbonate resin (A), an olefin polymer (B), a basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), at least one (D) selected from fatty acid metal salts and fatty acids, and an elastomer (E); (Production method IV) a method for melt-kneading an olefin polymer (B), a basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), at least one (D) selected from fatty acid metal salts and fatty acids, and an elastomer (E), and then further adding a polycarbonate resin (A) and melt-kneading.
[0066] Any of the above-mentioned (manufacturing method I) to (manufacturing method IV) can obtain a sea-island structure in which an island portion having an elastomer on the periphery is dispersed in a sea portion comprising the polycarbonate resin composition of the present invention, i.e., a polycarbonate resin. Basic magnesium sulfate is present inside the island portion together with residual components such as olefin polymers. As a result, basic magnesium sulfate does not directly contact the polycarbonate resin in the sea portion, thereby avoiding hydrolysis of the polycarbonate resin.
[0067] (Manufacturing method I)
[0068] Production method I is a production method comprising the following steps: a first step of melt-kneading 2% to 50% by mass of an olefin polymer (B), 40% to 70% by mass of basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), 0.1% to 5% by mass of at least one (D) selected from fatty acid metal salts and fatty acids, and 1% to 50% by mass of an elastomer (E) to obtain a masterbatch pellet; and a second step of melt-kneading 10% to 60% by mass of the masterbatch pellet and 40% to 90% by mass of a polycarbonate resin (A) to produce a polycarbonate resin composition.
[0069] In the production method I, as a first step, an olefin polymer (B), basic magnesium sulfate (C), at least one selected from fatty acid metal salts and fatty acids (D), and an elastomer (E) are melt-kneaded to obtain a master batch pellet in which basic magnesium sulfate is introduced into the olefin polymer. By kneading such a master batch pellet with a polycarbonate resin, hydrolysis of the polycarbonate resin can be more effectively suppressed.
[0070] As the melt kneading method in the manufacturing method I, the first step and the second step are not particularly limited, and examples thereof include methods using a single screw extruder, a twin screw extruder, a Banbury mixer, a kneader, an open roll mill, etc. As the melt kneading temperature, the first step is preferably 160° C. to 240° C., more preferably 180° C. to 230° C., and the second step is preferably 230° C. to 280° C., more preferably 240° C. to 260° C.
[0071] The ratios of "2% to 50% by mass of olefin polymer (B), 40% to 70% by mass of basic magnesium sulfate (C), 0.1% to 5% by mass of at least one selected from fatty acid metal salts and fatty acids (D), and 1% to 50% by mass of elastomer (E)" in the first step are ratios in the production of masterbatch pellets. By adjusting the ratios of the masterbatch pellets produced in the above ratios and the polycarbonate resin (A) in the second step, the ratios of the olefin polymer (B), basic magnesium sulfate (C), at least one selected from fatty acid metal salts and fatty acids (D), and elastomer (E) in the polycarbonate resin composition can be adjusted.
[0072] In the first step, the method for obtaining the master batch pellets is not particularly limited, and the master batch pellets can be obtained by molding into a pellet shape by a known method after melt kneading.
[0073] In addition, in the second step, the shape of the polycarbonate resin composition obtained by melt kneading is not limited, and can be formed into any shape such as strands, sheets, flat plates or pellets. If molding is considered in the subsequent steps, it is preferably made into pellets from the aspect of easy supply to a molding machine.
[0074] (Manufacturing method II)
[0075] Manufacturing method II is a manufacturing method having the following steps: a first step of melt-kneading 28% to 50% by mass of an olefin polymer (B), 40% to 70% by mass of basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), and 0.1% to 5% by mass of at least one (D) selected from fatty acid metal salts and fatty acids to obtain a master batch pellet; and a second step of melt-kneading 10% to 60% by mass of the master batch pellet, 40% to 90% by mass of a polycarbonate resin (A), and 1% to 20% by mass of an elastomer (E) to produce a polycarbonate resin composition.
[0076] The melt kneading method in the manufacturing method II is the same as that in the manufacturing method I. In the manufacturing method II, the elastomer (E) is mixed into the masterbatch pellets together with the polycarbonate resin in the second step. Therefore, it is possible to use a masterbatch composed of commercially available polyolefins, basic magnesium sulfate, fatty acid metal salts, etc., and it is possible to change only the content of the elastomer, which is advantageous from this point of view. As for the melt kneading temperature, from the aspect of preventing thermal decomposition of the polycarbonate resin, it is preferably 230°C to 280°C, more preferably 240°C to 270°C, and further preferably 245°C to 260°C.
[0077] The ratios of "28% to 50% by mass of olefin polymer (B), 40% to 70% by mass of basic magnesium sulfate (C), and 0.1% to 5% by mass of at least one selected from fatty acid metal salts and fatty acids (D)" in the first step are ratios in the production of masterbatch pellets. By adjusting the ratios of the masterbatch pellets, polycarbonate resin (A) and elastomer (E) produced in the above ratios in the second step, the ratios of the olefin polymer (B), basic magnesium sulfate (C), at least one selected from fatty acid metal salts and fatty acids (D), and elastomer (E) in the polycarbonate resin composition can be adjusted.
[0078] The shape of the polycarbonate resin composition obtained by melt kneading in Production Method II is not particularly limited, and similarly to Production Method I, the polycarbonate resin composition can be formed into any shape such as a strand, a sheet, a flat plate, or a pellet.
[0079] (Manufacturing method III)
[0080] Manufacturing method III is the following manufacturing method: 50 mass% to 90 mass% of polycarbonate resin (A), 2.0 mass% to 20 mass% of olefin polymer (B), 5 mass% to 40 mass% of basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), 0.1 mass% to 8 mass% of at least one (D) selected from fatty acid metal salts and fatty acids, and 1 mass% to 20 mass% of elastomer (E) are melt-kneaded.
[0081] The melt kneading method in the production method III is the same as that in the production method I. In the production method III, the polycarbonate resin (A), the olefin polymer (B), the basic magnesium sulfate (C), at least one selected from fatty acid metal salts and fatty acids (D), and the elastomer (E) are melt-kneaded together, which has the advantages of preventing thermal decomposition of the polycarbonate resin and simplifying the production process. The melt kneading temperature is preferably 230° C. to 280° C., more preferably 240° C. to 270° C., and even more preferably 245° C. to 260° C. from the perspective of preventing thermal decomposition of the polycarbonate resin.
[0082] The shape of the polycarbonate resin composition obtained by melt kneading in Production Method III is not particularly limited, and similarly to Production Method I, the polycarbonate resin composition can be formed into any shape such as a strand, a sheet, a flat plate, or a pellet.
[0083] (Manufacturing method IV)
[0084] Production method IV is the following production method: 2.0% to 20% by mass of an olefin polymer (B), 5% to 40% by mass of basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), 0.1% to 8% by mass of at least one (D) selected from fatty acid metal salts and fatty acids, and 1% to 20% by mass of an elastomer (E) are melt-kneaded, and then 50% to 90% by mass of a polycarbonate resin (A) is further added and melt-kneaded.
[0085] The melt kneading method in the production method IV is the same as that in the production method I. In the production method IV, the olefin polymer (B), the basic magnesium sulfate (C), at least one selected from the fatty acid metal salt and the fatty acid (D), and the elastomer (E) are first melt-kneaded, and then the polycarbonate resin (A) is added, thereby simplifying the production process. The temperature of the previous melt kneading is preferably 160°C to 240°C, more preferably 180°C to 230°C, and the temperature of the melt kneading after the addition of the polycarbonate resin (A) is preferably 230°C to 280°C, more preferably 240°C to 260°C.
[0086] The shape of the polycarbonate resin composition obtained by melt kneading in Production Method IV is not particularly limited, and similarly to Production Method I, the composition can be formed into any shape such as a strand, a sheet, a flat plate, or a pellet.
[0087] 3. Masterbatch (MB) pellets
[0088] Next, the master batch pellets will be described. The master batch pellets of the present invention are raw materials for producing a polycarbonate resin composition by kneading with a diluent material containing a polycarbonate resin (A).
[0089] The master batch pellets of the present invention contain 2% to 50% by mass of an olefin polymer (B), 40% to 70% by mass of basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), 0.1% to 5% by mass of at least one (D) selected from fatty acid metal salts and fatty acids, and 1% to 50% by mass of an elastomer (E). Preferably, the master batch pellets contain 2% to 45% by mass of an olefin polymer (B), 55% to 70% by mass of basic magnesium sulfate (C), 0.1% to 4.5% by mass of at least one (D) selected from fatty acid metal salts and fatty acids, and 1% to 45% by mass of an elastomer (E). More preferably, the master batch pellets contain 2% to 40% by mass of an olefin polymer (B), 60% to 70% by mass of basic magnesium sulfate (C), 0.5% to 4% by mass of at least one (D) selected from fatty acid metal salts and fatty acids, and 2% to 40% by mass of an elastomer (E).
[0090] The details of the olefin polymer (B), basic magnesium sulfate (C), at least one selected from fatty acid metal salts and fatty acids (D), and the elastomer (E) are as described above, so the description is omitted. In addition, the method for producing the masterbatch pellets is the same as the first step of the method for producing the polycarbonate resin composition I described above. As a diluent, there is no particular limitation as long as it is a resin containing the above-mentioned polycarbonate resin (A).
[0091] 4. Molding
[0092] Next, the molded body is described. The molded body of the present invention can be manufactured by molding the polycarbonate resin composition of the present invention. As a method for molding the polycarbonate resin composition, there can be mentioned: a method of manufacturing a polycarbonate resin composition by the above method and molding it; a method of mixing master batch pellets with diluted pellets and directly molding the mixture using a molding machine; etc. In addition, as a molding machine used for molding, for example, a calender molding machine (calender molding machine, etc.), a vacuum molding machine, an extrusion molding machine, an injection molding machine, a blow molding machine, a press molding machine, etc. can be mentioned.
[0093] The molded article of the present invention has the excellent property of high Izod impact strength. Izod impact strength is an index indicating strength against impact. The value of Izod impact strength in this specification can be defined as the result measured by the method described in the embodiments described later. Specifically, it is the result measured by using an Izod impact tester according to the method of JIS K 7110.
[0094] In addition, the molded article of the present invention is also excellent in terms of high bending elastic modulus. The bending elastic modulus is an index indicating the difficulty of deformation of the molded article and can be defined as the result of measurement using the method described in the embodiments described below. Specifically, it is the result of measurement using a universal mechanical testing machine using a method in accordance with JIS K 7171.
[0095] The molded article of the present invention is obtained by molding a polycarbonate resin composition using fibrous basic magnesium sulfate having a small average fiber diameter (average minor diameter) or fan-shaped basic magnesium sulfate containing such fibrous basic magnesium sulfate as a filler. Therefore, the molded article of the present invention has an advantage of having a superior appearance and being usable in exterior parts that can be touched by human eyes, compared with the case where glass fibers having a large average fiber diameter (average minor diameter) are used as fillers.
[0096] Hereinafter, the present invention will be specifically described based on Examples, but these Examples do not limit the purpose of the present invention, and the present invention is not limited to these Examples.
[0097] First, the measurement method used in this example is described.
[0098] (Melt Flow Rate (MFR))
[0099] A melt flow rate test was performed using a melt flow indexer (G-01, manufactured by Toyo Seiki Seisaku-sho, Ltd.) in accordance with JIS K 7210 to evaluate the melt flow rate (MFR).
[0100] (Izod impact strength)
[0101] The Izod impact strength was evaluated by testing using an Izod impact tester (manufactured by MYS-TESTER Company Limited) in accordance with JIS K 7110. The hammer was set to 2.75 J.
[0102] (Flexural modulus (FM))
[0103] A three-point bending test was performed using a universal mechanical testing machine (manufactured by Imada Co., Ltd.), and the bending modulus was evaluated from the obtained load-deflection curve by a method in accordance with JIS K 7171. The distance between the fulcrums was 40 mm, and the loading speed was 10 mm / min.
[0104] (Transmission electron microscope (TEM) observation)
[0105] After the obtained polycarbonate resin composition is embedded with a photocurable acrylic resin, it is cut into a cross section in which the fiber direction of the fibrous basic magnesium sulfate in the composition can be observed. In addition, it is fixed to an aluminum sample needle. After trimming and surface polishing, ultrathin sections are made using a freezing microtome (manufactured by LEICA, FCS). The obtained ultrathin sections are used as samples and observed using a transmission electron microscope (TEM) (manufactured by JEOL Ltd., JEM-2100F).
[0106] <Manufacturing of resin composition>
[0107] The components used in Examples and Comparative Examples are shown below.
[0108] Polycarbonate resin (A):
[0109] [MFR (temperature 240°C, load 5.000 kg): 4.5 g / 10 min]
[0110] Olefin polymer (B):
[0111] Polypropylene resin [MFR (temperature 230°C, load 2.160 kg): 8 g / 10 min]
[0112] Fibrous basic magnesium sulfate (C-1):
[0113] (MOS-HIGE A-1, manufactured by Ube Materials Co., Ltd., average major diameter: 15 μm, average minor diameter: 0.5 μm)
[0114] Fan-shaped basic magnesium sulfate (C-2):
[0115] (average particle length 33.0 μm, average particle width 6.0 μm, average aspect ratio 5.5)
[0116] Fatty acid metal salt (D): magnesium stearate
[0117] Elastomer (E): Styrene-ethylene-butylene-styrene (SEBS, Tuftec H1043, manufactured by Asahi Kasei Corporation)
[0118] Glass fiber(F):
[0119] (CS(F)3-PE-960S, manufactured by Nittobo Co., Ltd., fiber length: 3 mm, fiber short diameter: 13 μm)
[0120] (Example 1)
[0121] 29.5 mass % of polypropylene resin (B), 68.6 mass % of fibrous basic magnesium sulfate particles (C-1) and 1.9 mass % of magnesium stearate (D) were mixed, and the resulting mixture was melt-kneaded at 180° C. for 2 minutes. The melt-kneading was performed using a melt-kneading extruder Labo Plastomill Roller Mixer (R60 type, capacity 60cc, manufactured by Toyo Seiki Co., Ltd.), and the shaft speed was set to 120 rpm. The resulting melt-kneaded product was made into a sheet by hot pressing (temperature 200° C.), and then cut to obtain a masterbatch pellet.
[0122] 21% by mass of the masterbatch pellets, 76% by mass of the polycarbonate resin (A) and 3% by mass of the elastomer (E) were mixed and then melt-kneaded at 250° C. and 50 rpm using a twin-screw melt-kneading extruder (L / D=25, manufactured by Imoto Seisakusho Co., Ltd.) to obtain a polycarbonate resin composition of Example 1.
[0123] (Example 2)
[0124] A polycarbonate resin composition of Example 2 was obtained in the same manner as in Example 1 except that the ratio of the polycarbonate resin (A) was changed to 73.9% by mass and the ratio of the elastomer (E) was changed to 5.1% by mass.
[0125] (Example 3)
[0126] A master batch pellet was obtained in the same manner as in Example 1 except that 27.5% by mass of the polypropylene resin (B), 64.2% by mass of the fibrous basic magnesium sulfate particles (C-1), 1.7% by mass of magnesium stearate (D) and 6.6% by mass of the elastomer (E) were used.
[0127] A polycarbonate resin composition of Example 3 was obtained in the same manner as in Example 1 except that 22.9 mass % of the masterbatch pellets and 73.9 mass % of the polycarbonate resin (A) were used.
[0128] (Example 4)
[0129] A masterbatch pellet was prepared using 25.5 mass% of a polypropylene resin (B), 59.1 mass% of fibrous basic magnesium sulfate particles (C-1), 1.6 mass% of magnesium stearate (D) and 13.8 mass% of an elastomer (E), and 24.7 mass% of the obtained masterbatch pellet was mixed with 75.3 mass% of a polycarbonate resin (A). The polycarbonate resin composition of Example 4 was obtained in the same manner as in Example 3 except that
[0130] (Example 5)
[0131] A masterbatch pellet was prepared using 22.6 mass% of a polypropylene resin (B), 53.3 mass% of fibrous basic magnesium sulfate particles (C-1), 1.5 mass% of magnesium stearate (D) and 22.6 mass% of an elastomer (E), and 27.4 mass% of the obtained masterbatch pellet was mixed with 72.6 mass% of a polycarbonate resin (A). The polycarbonate resin composition of Example 5 was obtained in the same manner as in Example 3 except that
[0132] (Example 6)
[0133] A masterbatch pellet was prepared using 19.6 mass % of a polypropylene resin (B), 46.2 mass % of fibrous basic magnesium sulfate particles (C-1), 1.3 mass % of magnesium stearate (D) and 32.9 mass % of an elastomer (E). 31.6 mass % of the obtained masterbatch pellet was mixed with 68.4 mass % of a polycarbonate resin (A). The polycarbonate resin composition of Example 6 was obtained in the same manner as in Example 3 except that
[0134] (Example 7)
[0135] A polycarbonate resin composition of Example 7 was obtained in the same manner as in Example 4 except that the fibrous basic magnesium sulfate particles (C-1) were changed to the same amount of fan-shaped basic magnesium sulfate particles (C-2).
[0136] (Example 8)
[0137] A polycarbonate resin composition of Example 8 was obtained in the same manner as in Example 5 except that the fibrous basic magnesium sulfate particles (C-1) were changed to the same amount of fan-shaped basic magnesium sulfate particles (C-2).
[0138] (Comparative Example 1)
[0139] A polycarbonate resin composition of Comparative Example 1 was obtained in the same manner as in Example 1 except that 28.1% by mass of a polypropylene resin (B), 70.0% by mass of fibrous basic magnesium sulfate particles (C-1) and 1.9% by mass of magnesium stearate (D) were used to prepare a masterbatch pellet. 21% by mass of the obtained masterbatch pellet was mixed with 79% by mass of a polycarbonate resin (A).
[0140] (Comparative Example 2)
[0141] The polycarbonate resin (A) was used alone.
[0142] (Comparative Example 3)
[0143] 80 mass % of polycarbonate resin (A) and 20 mass % of glass fiber (F) were mixed and the obtained mixture was melt-kneaded using a twin-screw melt-kneading extruder to obtain a polycarbonate resin composition of Comparative Example 3. Melt-kneading was performed in the same manner as in Example 1 except that the temperature was changed to 280°C.
[0144] (Comparative Example 4)
[0145] 80 mass % of the polycarbonate resin (A) and 20 mass % of the fibrous basic magnesium sulfate particles (C-1) were mixed. Then, melt kneading was attempted using a twin-screw melt kneading extruder in the same manner as in Example 1, but kneading failed.
[0146] (Comparative Example 5)
[0147] 84.7 mass % of polycarbonate resin (A), 14.9 mass % of fibrous basic magnesium sulfate particles (C-1), and 0.4 mass % of fatty acid metal salt (D) were mixed and then melt kneading was attempted using a twin-screw melt kneading extruder in the same manner as in Example 1, but kneading was unsuccessful.
[0148] (Comparative Example 6)
[0149] 79.0 mass % of polycarbonate resin (A), 6.3 mass % of olefin polymer (B) and 14.7 mass % of fibrous basic magnesium sulfate particles (C-1) were mixed and then melt kneading was attempted using a twin-screw melt kneading extruder in the same manner as in Example 1, but kneading was unsuccessful.
[0150] From the results of Comparative Examples 3 to 6, it is understood that even if the fibrous basic magnesium sulfate particles (C-1) are contained, kneading itself cannot be performed without the olefin polymer (B) and / or the fatty acid metal salt (D).
[0151] (Comparative Example 7)
[0152] A polycarbonate resin composition of Comparative Example 7 was obtained in the same manner as in Example 3 except that the fibrous basic magnesium sulfate particles (C-1) were changed to the same amount of glass fibers (F).
[0153] (Comparative Example 8)
[0154] A polycarbonate resin composition of Comparative Example 8 was obtained in the same manner as in Example 4 except that the fibrous basic magnesium sulfate particles (C-1) were changed to the same amount of glass fibers (F).
[0155] (Comparative Example 9)
[0156] A polycarbonate resin composition of Comparative Example 9 was obtained in the same manner as in Example 5 except that the fibrous basic magnesium sulfate particles (C-1) were changed to the same amount of glass fibers (F).
[0157] (Comparative Example 10)
[0158] A polycarbonate resin composition of Comparative Example 10 was obtained in the same manner as in Example 6 except that the fibrous basic magnesium sulfate particles (C-1) were changed to the same amount of glass fibers (F).
[0159] (Comparative Example 11)
[0160] A polycarbonate resin composition of Comparative Example 11 was obtained in the same manner as in Comparative Example 1, except that the fibrous basic magnesium sulfate (C-1) was changed to the same amount of fan-shaped basic magnesium sulfate particles (C-2).
[0161] The contents (mass %) of the polycarbonate resin (A), olefin polymer (B), basic magnesium sulfate particles (C), fatty acid metal salt (D), elastomer (E) and glass fiber (F) in the polycarbonate resin compositions obtained in Examples 1 to 8 and Comparative Examples 1 to 11 are summarized in the following Table 1.
[0162] [Table 1]
[0163]
[0164] <Evaluation method>
[0165] The polycarbonate resin compositions obtained in Examples and Comparative Examples were extruded into strands and then cut to prepare polycarbonate resin composition pellets. The melt flow rate of the polycarbonate resin composition pellets was measured by the above-mentioned method.
[0166] The polycarbonate resin composition pellets were injection molded using a small injection molding machine (C. Mobile 0813, manufactured by Shinko Sellbic Co., Ltd.) to produce a molded body (length 50 mm, width 5 mm, thickness 2 mm). The obtained molded body was used as a test piece, and the impact strength and flexural modulus were measured by the above method.
[0167] Furthermore, the appearance of each test piece was visually observed to check whether the filler was recognized on the surface. If the filler was not recognized, it was marked as "○", and if the filler was recognized, it was marked as "×".
[0168] The obtained results are summarized in Table 2 below together with the above-mentioned measurement results.
[0169] [Table 2]
[0170]
[0171] As shown in Table 2 above, the polycarbonate resin compositions containing a polycarbonate resin, an olefin polymer, basic magnesium sulfate, a fatty acid metal salt and an elastomer in specified amounts (Examples 1 to 8) have significantly improved melt flow rate values compared to the polycarbonate resin alone (Comparative Example 2) or the polycarbonate resin composition containing glass fiber as a filler (Comparative Example 3).
[0172] In addition, the impact strength (Izod) of the molded bodies produced using the polycarbonate resin compositions of Examples 1 to 8 is significantly greater than that of the molded body produced using the polycarbonate resin composition containing no elastomer (Comparative Example 1). Even though the flexural modulus is about 3.5 GPa, the impact strength is less than 13 kJ / m 2 The molded product of the present invention is sometimes not suitable for practical use. The impact strength of the molded product of the present invention is 13 kJ / m 2 From the above, it can be seen that there is no practical problem.
[0173] In addition, the molded bodies produced using the polycarbonate resin compositions of Examples 1 to 8 have a better bending modulus than the molded body produced using the polycarbonate resin alone (Comparative Example 2). Moreover, the molded body produced using the polycarbonate resin composition containing glass fiber as a filler (Comparative Example 3) does not have a poor appearance.
[0174] The molded bodies produced using the polycarbonate resin compositions of Comparative Examples 7 to 10 were all found to be defective in appearance. The polycarbonate resin compositions of Comparative Examples 7 to 10 were the same compositions as the polycarbonate resin compositions of Examples 3 to 6, except that glass fibers were contained instead of fibrous basic magnesium sulfate. This indicates that, when glass fibers are contained as fillers, it is not possible to obtain a polycarbonate resin composition that does not undergo hydrolysis, can be kneaded / molded, and can obtain a molded body having excellent processability, good mechanical properties, and good appearance.
[0175] Comparison between Examples 7 and 8 and Comparative Example 11 shows that even when a polycarbonate resin composition containing fan-shaped basic magnesium sulfate particles but not containing an elastomer is used, a molded product having a high impact strength (Izod) cannot be obtained.
[0176] Here, a TEM photograph of the polycarbonate resin composition of Example 2 is shown in Figure 2 As shown in the figure, island portions 12 surrounded by an elastic body 15 are dispersed in a sea portion 11 made of a polycarbonate resin. Inside the island portion 12, fibrous basic magnesium sulfate 14 and an olefin polymer 13 are confirmed to exist together.
[0177] Explanation of symbols
[0178] 11…Sea part (polycarbonate resin) 12…Island part 13…Olefin polymer
[0179] 14…Fiber-like basic magnesium sulfate 15…Elastomer
Claims
1. A polycarbonate resin composition, characterized in that It contains 50% to 90% by mass of a polycarbonate resin (A), 2.0% to 20% by mass of a polypropylene as an olefin polymer (B), 5% to 40% by mass of a basic magnesium sulfate (C) selected from a fibrous basic magnesium sulfate (C-1) and a fan-shaped basic magnesium sulfate (C-2), 0.1% to 8% by mass of at least one (D) selected from a fatty acid metal salt and a fatty acid, and 1% to 20% by mass of an elastomer (E).
2. The polycarbonate resin composition according to claim 1, wherein It has a sea-island structure composed of a sea portion containing the polycarbonate resin and an island portion having the elastomer on the periphery.
3. The method for producing a polycarbonate resin composition according to claim 1 or 2, characterized in that: The process has the following steps: In the first step, 2% to 50% by weight of an olefin polymer (B), 40% to 70% by weight of a basic magnesium sulfate (C) selected from a fibrous basic magnesium sulfate (C-1) and a fan-shaped basic magnesium sulfate (C-2), 0.1% to 5% by weight of at least one selected from a fatty acid metal salt and a fatty acid (D), and 1% to 50% by weight of an elastomer (E) are melt-kneaded to obtain a masterbatch pellet; and In the second step, 10 to 60% by mass of the master batch pellets and 40 to 90% by mass of the polycarbonate resin (A) are melt-kneaded to produce a polycarbonate resin composition.
4. The method for producing a polycarbonate resin composition according to claim 1 or 2, characterized in that: The process has the following steps: In the first step, 28% to 50% by weight of an olefin polymer (B), 40% to 70% by weight of a basic magnesium sulfate (C) selected from fibrous basic magnesium sulfate (C-1) and fan-shaped basic magnesium sulfate (C-2), and 0.1% to 5% by weight of at least one (D) selected from fatty acid metal salts and fatty acids are melt-kneaded to obtain a masterbatch pellet; and In the second step, 10 to 59 mass % of the master batch pellets, 40 to 89 mass % of the polycarbonate resin (A), and 1 to 20 mass % of the elastomer (E) are melt-kneaded to produce a polycarbonate resin composition.
5. The method for producing a polycarbonate resin composition according to claim 1 or 2, characterized in that: 50 to 90% by mass of a polycarbonate resin (A), 2.0 to 20% by mass of an olefin polymer (B), 5 to 40% by mass of a basic magnesium sulfate (C) selected from a fibrous basic magnesium sulfate (C-1) and a fan-shaped basic magnesium sulfate (C-2), 0.1 to 8% by mass of at least one (D) selected from a fatty acid metal salt and a fatty acid, and 1 to 20% by mass of an elastomer (E) are melt-kneaded.
6. The method for producing a polycarbonate resin composition according to claim 1 or 2, characterized in that: 2.0 to 20% by mass of an olefin polymer (B), 5 to 40% by mass of a basic magnesium sulfate (C) selected from a fibrous basic magnesium sulfate (C-1) and a fan-shaped basic magnesium sulfate (C-2), 0.1 to 8% by mass of at least one selected from a fatty acid metal salt and a fatty acid (D), and 1 to 20% by mass of an elastomer (E) are melt-kneaded, and then, 50 to 90% by mass of the polycarbonate resin (A) is added and melt-kneaded.
7. A molded body, characterized in that This is a molded product of the polycarbonate resin composition according to claim 1.