Method for manufacturing a substrate for a front side image sensor

By injecting gas ions into the SOI substrate to form a high-density hole layer, the problem of insufficient surface state of the capture layer caused by too thin a buried oxide layer is solved, the electrical performance and adhesion of the image sensor are improved, and the metal atoms are ensured. Efficient capture and image sensor stability.

CN113228248BActive Publication Date: 2024-10-01SOITEC SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980085606.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-24
Filing Date
2019-12-23
Publication Date
2024-10-01
Estimated Expiration
2039-12-23

AI Technical Summary

Technical Problem

In the prior art, when manufacturing SOI substrates for front-side image sensors, the buried oxide layer is too thin, resulting in insufficient surface quality of the capture layer, which affects the electrical performance of the image sensor, especially in near-infrared image sensors.

Method used

The donor substrate providing the semiconductor layer to be transferred is combined with the carrier substrate to form an electrical insulating layer, and gas ions are injected into the carrier substrate through the transferred semiconductor layer and the electrical insulating layer, and heat treatment is performed to form a high-density air The hole layer is used to trap metal atoms and ensure good adhesion between the active layer and the carrier substrate.

Benefits of technology

It achieves the formation of an efficient capture layer in the image sensor, effectively reduces the diffusion and interference of metal atoms, improves the electrical performance of the image sensor, and ensures good bonding and stable performance, especially in the case of thin oxide layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113228248B_ABST
    Figure CN113228248B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a substrate for a front image sensor, the method comprising: providing a donor substrate (30) comprising a semiconductor layer (3a) to be transferred, providing a semiconductor carrier substrate (1), bonding the donor substrate (30) to the carrier substrate (1), an electrical insulating layer (2) being located at the bonding interface, transferring the semiconductor layer (3a) to the carrier substrate (1), implanting gas ions (40) into the carrier substrate (1) via the transferred semiconductor layer (3a) and the electrical insulating layer (2), and after the implantation, epitaxially growing an additional semiconductor layer (3b) on the transferred semiconductor layer (3a).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method of manufacturing a substrate for a front side image sensor. Background Art

[0002] Semiconductor-on-insulator structures, particularly silicon-on-insulator (SOI) substrates, are advantageous substrates for fabricating front-side image sensors.

[0003] The SOI substrate has, from its back side to its front side, a carrier substrate made of silicon doped to a certain degree, a silicon oxide layer called a "buried oxide layer" (commonly referred to by the acronym "BOX"), and a layer called an active silicon layer (having a doping that may be different from that of the carrier substrate). A matrix array of photodiodes (each photodiode defining a pixel of the image sensor) is arranged in the active layer.

[0004] In some applications, the buried oxide layer is chosen to be relatively thin (i.e., less than 100 nm thick, in particular between 20 nm and 50 nm), so as to play the role of a capacitor dielectric by biasing the pixel via the back side. The portion of the carrier substrate beneath the buried oxide layer is biased to a voltage different from the voltage of the active layer, which allows the interface between the dielectric layer and the active layer to be passivated. The voltage applied to the portion of the carrier substrate beneath the buried oxide layer depends on the thickness of the layer. The applied potential difference is proportional to the thickness of the buried oxide layer: the thinner the buried oxide layer, the smaller the applied potential difference.

[0005] Another function of the buried oxide layer is to prevent the collection of parasitic signals (preventing crosstalk) generated by the recombination of unabsorbed photons in the carrier substrate during the passage through each pixel. It should be understood that depending on the selected thickness, the buried oxide layer may only partially reflect and / or absorb incident photons.

[0006] One disadvantage of the method for manufacturing image sensors is that it is very sensitive to metal contamination. In particular, both the SOI substrate itself and the pixels may be exposed to metal during the manufacturing process. This exposure results in the presence of metal atoms in the active layer in particular. However, even at low concentrations, metal atoms (especially copper atoms) may lead to unacceptable image sensor performance losses. In particular, metal atoms can interact with the charge generated by the photons captured in the pixel and negatively affect its collection performance.

[0007] In order to overcome this disadvantage, it is known to form a layer for trapping metal atoms within the SOI substrate.

[0008] Thus, document US 6,083,324 describes the formation of a trapping layer in the active layer of an SOI substrate by ion implantation of gas species followed by a heat treatment suitable for forming microbubbles or precipitates from the implanted ions. These microbubbles or precipitates form trapping sites for metal atoms. However, since the trapping layer forms holes and interfaces in the pixel, it may interfere with the trajectory of photons through the pixel and have a negative impact on the electrical performance of the image sensor.

[0009] Document US 2010 / 0090303 describes forming a capture layer in a carrier substrate. More specifically, when using SmartCut TM When the SOI substrate is formed by the layer transfer technology, the method for manufacturing the SOI substrate includes the following steps:

[0010] - providing a silicon donor substrate covered with a silicon oxide layer intended to form the BOX and comprising weakened areas defining a thin silicon layer;

[0011] - providing a carrier substrate, in which a trapping layer has been formed by ion implantation;

[0012] - bonding the donor substrate and the carrier substrate via an oxide layer;

[0013] - separating the donor substrate along the weakened area, thereby transferring the thin silicon layer and the oxide layer to the carrier substrate;

[0014] - Epitaxially growing additional silicon layers on top of the transferred thin layer until the desired thickness of the active layer of the image sensor is obtained.

[0015] However, if the buried oxide layer is very thin, the surface state of the carrier substrate that is ion implanted to form the capture layer is not of sufficient quality to provide good bonding retention, which is a significant disadvantage of this method, especially when bonding thin oxides (such as those for near-infrared front-side image sensors). Summary of the invention

[0016] Therefore, there remains a need to form a trapping region in a carrier substrate for forming a semiconductor-on-insulator structure of a front side image sensor while ensuring good adhesion between the active layer and the carrier substrate.

[0017] To this end, the present invention proposes a method for manufacturing a substrate for a front image sensor, the method comprising:

[0018] providing a donor substrate including a semiconductor layer to be transferred;

[0019] providing a semiconductor carrier substrate;

[0020] bonding a donor substrate to a carrier substrate, with the electrically insulating layer being located at the bonding interface;

[0021] transferring the semiconductor layer to a carrier substrate;

[0022] implanting gas ions through the transferred semiconductor layer and the electrically insulating layer into the carrier substrate;

[0023] After the implantation, an additional semiconductor layer is epitaxially grown on top of the transferred semiconductor layer.

[0024] Advantageously, the method comprises a thermal treatment carried out at a temperature suitable for forming vacancies from the implanted gas ions, said vacancies forming a layer for trapping metal atoms in the carrier substrate.

[0025] According to one embodiment, the heat treatment is performed during epitaxial growth of the additional semiconductor layer.

[0026] Preferably, the density of holes in the capture layer is greater than or equal to 10 15 holes / cm 3 .

[0027] According to one embodiment, each semiconductor layer is a silicon layer.

[0028] According to one embodiment, the electrically insulating layer is a silicon oxide layer.

[0029] Alternatively, the electrically insulating layer consists of a stack of dielectric materials and / or metallic materials.

[0030] Preferably, the thickness of the electrically insulating layer is between 5 nm and 400 nm, preferably between 30 nm and 150 nm.

[0031] Preferably, the gas ions include helium ions.

[0032] According to one embodiment, the transferring of the semiconductor layer comprises:

[0033] - forming a weakened area in the donor substrate, thereby defining said semiconductor layer to be transferred;

[0034] - After bonding, the donor substrate is separated along the weakened area.

[0035] The present invention also relates to a method for manufacturing a front image sensor, which includes using the above method to manufacture a substrate, the transferred semiconductor layer and the additional semiconductor layer together forming an active layer of the image sensor, and forming a plurality of electrically isolated grooves in the active layer to define a plurality of pixels. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Other features and advantages of the present invention emerge from the following detailed description with reference to the accompanying drawings, in which:

[0037] - Figure 1Ais a cross-sectional view of an SOI substrate of an image sensor according to an embodiment of the present invention;

[0038] - Figure 1B Based on Figure 1A A cross-sectional view of a substrate of a variation of ;

[0039] - Figure 2 schematically illustrates the implantation of atomic species into a donor substrate, thereby forming a weakened region defining therein a semiconductor layer to be transferred;

[0040] - Figure 3 Schematically shows Figure 2 The weakened donor substrate is bonded to the carrier substrate;

[0041] - Figure 4 schematically illustrates transferring a semiconductor layer to a carrier substrate to form an SOI structure;

[0042] - Figure 5 Schematic diagram showing the injection of helium into Figure 4 In the SOI structure;

[0043] - Figure 6 shows the substrate obtained after forming electrical isolation trenches in the substrate of FIG. 1 , so as to individualize each pixel of the image sensor, said substrate having previously been subjected to a re-epitaxial step;

[0044] - Figure 7 The results of transmission electron microscopy show Figure 5 An image of a portion of a substrate (the right image is an enlarged view of the left image);

[0045] - Figure 8 is with Figure 7 Compared to the image produced by transmission electron microscopy after applying additional heat treatment to the substrate Figure 5 an image of a portion of a substrate;

[0046] - Fig. 9 Copper concentration measurements by secondary ion mass spectrometry (SIMS) are shown, which illustrate the Figure 5 diffusion within a substrate of the substrate, the measurement being superimposed on an image of a portion of the substrate produced by a transmission electron microscope;

[0047] - Fig.10 SIMS measurements of copper concentration are shown, which show that copper is Figure 5 Diffusion in a substrate identical to the substrate but without the trapping layer;

[0048] - Fig.11 SIMS measurements of copper concentration are shown, which show that copper Figure 5 diffusion within the substrate.

[0049] In order to make the drawings clearer, the various layers are not drawn to scale. The same reference numerals from one drawing to another are used to denote elements that are the same or have the same function. DETAILED DESCRIPTION

[0050] Figure 1A An SOI substrate of an image sensor according to an embodiment of the present invention is shown.

[0051] The substrate comprises successively, from its rear side to its front side, a carrier substrate 1 , an electrically insulating layer 2 and a semiconductor layer 3 , known as active layer, which is intended for forming pixels of an image sensor.

[0052] The layer 4 for trapping metal atoms is provided at a depth in the carrier substrate 1, which need not be in contact with the electrically insulating layer 2. As will be described in detail below, the layer 4 comprises vacancies formed by gas ions injected into the carrier substrate under the effect of a thermal treatment. The density of the vacancies in the trapping layer 4 is advantageously greater than or equal to 10 15 holes / cm 3 The vacancies are capable of trapping metal atoms present in the SOI substrate, located near the electrically insulating layer 2, which may have a negative impact on the correct operation of the sensor. These atoms may initially be present in the carrier substrate 1 and / or in the active layer 3 and diffuse through the SOI substrate under the effect of the thermal treatment until they reach the trapping layer 4 where they are trapped.

[0053] The carrier substrate is advantageously a silicon substrate, in particular a single-crystalline silicon substrate.

[0054] The electrically insulating layer 2 may be a silicon oxide layer, which is a conventional insulator in the field of silicon-on-insulator substrates.

[0055] Alternatively, the electrically insulating layer may consist of a stack of multiple dielectric materials and / or metallic materials, such as a so-called "ONO" (i.e. oxide-nitride-oxide) stack. The constituent materials of the stack are advantageously chosen so as to increase the reflectivity of the electrically insulating layer in the infrared compared to a silicon oxide layer with the same total thickness. Preferably, the metal layer is encapsulated between two dielectric layers, thereby preventing any metallic contamination of the active layer. This makes it possible to avoid the generation of electrical defects at the interface between the active layer and the electrically insulating layer, and to avoid recombination of the semiconductor material of the active layer with the metallic components of the image sensor (which could dope the active layer).

[0056] according to Figure 1BIn a particular embodiment shown, the electrically insulating layer 2 comprises a silicon nitride layer 22 between two silicon oxide layers 21, 23. The thickness of the layer 21 arranged on the side of the carrier substrate 1 is between 50nm and 500nm, the thickness of the layer 23 arranged on the side of the active layer 3 is between 5nm and 50nm, and the thickness of the layer 22 is between 10nm and 100nm. The advantage of this electrically insulating layer is that it is similar to a layer having the same thickness. Figure 1A Compared with the silicon oxide layer of the substrate, it can better reflect the photons passing through the active layer 3.

[0057] Particularly advantageously, the electrically insulating layer 2, whether it is composed of one material or of a plurality of materials, is relatively thin, i.e. its thickness is between 5 nm and 400 nm, preferably between 30 nm and 150 nm. This layer does not block the diffusion of metal atoms, in particular copper atoms. Therefore, it is not necessary to locally destroy the electrically insulating layer to allow the atoms to pass through, as described in document US 2010 / 0090303.

[0058] The active layer is advantageously a single crystal. As schematically shown in Fig. 1, the active layer 3 is formed by stacking a first layer 3a and an additional layer 3b, which is manufactured by epitaxy on top of the layer 3a and then used as a seed layer. The materials of the layers 3a and 3b advantageously exhibit similar lattice parameters and thermal expansion coefficients, which can reduce the formation of crystal defects in the layer 3b as much as possible when epitaxially growing the layer 3b. According to a preferred embodiment, the layers 3a and 3b are made of the same material (usually silicon or silicon-germanium). The layers 3a and / or 3b may be doped.

[0059] The thickness of layer 3 is generally greater than or equal to 1 μm.

[0060] Now refer to Figures 2 to 5 Description based on Smart Cut TM Method Manufacturing Figure 1A The substrate method.

[0061] refer to Figure 2 , a donor substrate 30 covered with an electrically insulating layer 2 is provided. The electrically insulating layer can be formed by thermal oxidation of the material of the donor substrate and / or by deposition of one or more dielectric layers and / or metal layers. A weakened region defining the semiconductor layer 3a to be transferred is formed by implanting atomic species into the donor substrate 30 (indicated by arrows). The atomic species implanted for this purpose advantageously include hydrogen and / or helium.

[0062] refer to Figure 3 , a donor substrate 30 is bonded to a carrier substrate 1 , and an electrically insulating layer 2 is located at the bonding interface.

[0063] refer to Figure 4, the donor substrate 30 is separated along the weakened area 31 , thereby transferring the semiconductor layer 3 a to the carrier substrate 1 .

[0064] refer to Figure 5 , gas (e.g. helium) ions are implanted into the carrier substrate 1 through the semiconductor layer 3a and the electrically insulating layer 2. A person skilled in the art is able to define the implantation parameters, in particular the dose and the implantation energy, so that the gas ions 40 are concentrated in a layer of the thickness of the carrier substrate 1. As an indication, at 1E16 atoms / cm 2 and 5E17 atoms / cm 2 The dose between 10 and 10E15 holes / cm 3 The injection energy is typically between a few keV and 120 keV. A person skilled in the art will select a suitable energy according to the thickness of the layer through which the ions must pass, so that the ions are concentrated in the carrier substrate below the electrically insulating layer.

[0065] A heat treatment is then carried out to form vacancies from the injected gas ions, thereby forming a layer for trapping metal atoms. Generally speaking, this treatment involves heating the substrate to a temperature between 850° C. and 1200° C. for a duration between 30 minutes and 180 minutes. This heat treatment can be carried out as a specific step of the method. However, the thermal budget of other steps in the method can be advantageously used, such as a step of finishing the SOI substrate (e.g. annealing for smoothing or repairing defects) or an epitaxial step carried out to grow an additional semiconductor layer 3 b on top of the transferred layer 3 a.

[0066] As the above Smart Cut TM Alternatively, the semiconductor layer may be transferred after bonding the donor substrate to the carrier substrate by thinning the donor substrate from the side opposite the bonding interface (eg, by etching) until the desired thickness of the transferred semiconductor layer is obtained. In this case, there is no need to form a weakened region.

[0067] Forming the capture layer after bonding the donor substrate to the carrier substrate, rather than before bonding the donor substrate to the carrier substrate (as described in document US 2010 / 0090303), ensures that the surfaces to be bonded are of optimal quality, thus ensuring good adhesion between the two substrates (even in the case of thin electrically insulating layers). In addition, implanting gas ions before the epitaxy of the additional semiconductor layer makes it possible to reduce the implantation energy as much as possible and avoid damaging the active layer.

[0068] refer to Figure 6, by epitaxially growing an additional semiconductor layer 3b on top of the transferred layer 3a until the desired thickness of the active layer 3 is obtained. As described above, the thermal budget of this epitaxy can be used to form holes intended to form the trapping layer 4. Then, trenches 5 are formed through the active layer 3 and down to the electrically insulating layer 2, said trenches 5 being filled with a dielectric material so as to electrically isolate the pixels of the image sensor.

[0069] Experimental Results

[0070] Production e.g. Figure 5 The SOI substrate shown in FIG. 1 is used to form a trapping layer by heating a portion of the SOI substrate to a temperature of 950° C. for 40 minutes to form holes by the injected gas ions (see FIG. 1 ). Figure 7 ).

[0071] The substrate is then subjected to a thermal treatment to which a SOI substrate comprising a layer for trapping metal atoms may be subjected, in order to check whether the trapping layer is stable and remains functional even after being subjected to a thermal treatment with a high thermal budget (see Figure 8 ). It is assumed that the thermal budget of a 2-hour treatment at 1100°C is the maximum thermal budget that can maintain the trapping properties of the vacancy layer. This thermal budget is compatible with the finishing step and possible epitaxy.

[0072] Figure 7 shows the results of transmission electron microscopy after heat treatment for forming holes. Figure 5 1 (the right image is an enlargement of the left image). Within the carrier substrate 1, cavities arranged in the layer 4 forming the layer for trapping metal atoms can be seen. In the embodiment shown, the thickness of the layer 4 is 179 nm and it is buried at a depth of 205 nm below the interface between the carrier substrate 1 and the electrically insulating layer 2.

[0073] Figure 8 is with Figure 7 Compared to the image produced by transmission electron microscopy after applying additional heat treatment to the substrate Figure 5 Image of a portion of a substrate, the thermal treatment being carried out at a temperature of 1100° C. for a duration less than or equal to 2 hours. In the thickness of the carrier substrate 1 , at the implantation depth of the gas ions, cavities arranged in the layer 4 forming the layer for trapping metal atoms can be seen.

[0074] Fig. 9 The results of secondary ion mass spectrometry (SIMS) are shown. Figure 5Copper concentration measurement in the substrate, superimposed on an image of a portion of said substrate produced by a transmission electron microscope. To perform this measurement, a copper layer was deposited on top of the semiconductor layer 3a and subjected to a heat treatment (800°C, 2 hours) to diffuse the copper atoms into the substrate. This heat treatment was chosen to ensure complete dispersion of the element into the material, taking into account the physical diffusion properties of copper in silicon and silicon oxide. Therefore, this measurement reflects the ability of copper atoms to pass through the electrically insulating layer 2 and be captured by the capture layer 4. Therefore, although the concentration of copper atoms in layer 3a is about 1.1E11 atoms / cm 3 The concentration of copper atoms in the electrical insulating layer is about 1.8E9 atoms / cm 3 , but the curve shows that the concentration of copper atoms in layer 4 is about 2.3E13 atoms / cm 3 The concentration of copper atoms below layer 4 is very low.

[0075] Fig.10 and Fig.11 Shows the Figure 5 SIMS measurements of copper concentration in substrates of the same substrates without and with trapping layer 4 were performed. To carry out the measurements, a copper layer was deposited on the back side of carrier substrate 1 and a heat treatment (800° C., 2 hours) was performed to diffuse copper atoms into the substrate. Fig.10 In the absence of a trapping layer, a high concentration of copper atoms is observed in the carrier substrate 1 below the electrically insulating layer (peak P1), and in the transferred layer near the free surface of said layer (peak P2). Fig.11 In the case where (the trapping layer according to the present invention is present), a copper atom concentration peak P3 concentrated in the trapping layer is observed.

[0076] References

[0077] US 6,083,324

[0078] US 2010 / 0090303

Claims

1. A method for manufacturing a substrate for a front image sensor, the method comprising: - providing a donor substrate (30) comprising a semiconductor layer (3a) to be transferred; - providing a semiconductor carrier substrate (1); - bonding a donor substrate (30) to a carrier substrate (1), with the electrically insulating layer (2) being located at the bonding interface; - transferring the semiconductor layer (3a) to a carrier substrate (1); - implanting gas ions (40) through the transferred semiconductor layer (3a) and the electrically insulating layer (2) into the carrier substrate (1); - after said implantation, epitaxially growing an additional semiconductor layer (3b) on top of the transferred semiconductor layer (3a); as well as - a heat treatment at a temperature suitable for forming vacancies from the implanted gas ions, said vacancies forming a layer (4) for trapping metal atoms in the carrier substrate (1), wherein said heat treatment is carried out during the epitaxial growth of the additional semiconductor layer (3b).

2. The method according to claim 1, wherein: The density of holes in the capture layer (4) is greater than or equal to 10 15 holes / cm 3 .

3. The method according to any one of claims 1 to 2, wherein: Each semiconductor layer (3a, 3b) is a silicon layer.

4. The method according to any one of claims 1 to 2, wherein: The electrical insulating layer (2) is a silicon oxide layer.

5. The method according to any one of claims 1 to 2, wherein: The electrical insulation layer (2) is composed of a stack of layers (21, 22, 23) of dielectric material and / or metallic material.

6. The method according to any one of claims 1 to 2, wherein: The thickness of the electrical insulating layer (2) is between 5 nm and 400 nm.

7. The method according to any one of claims 1 to 2, wherein: The thickness of the electrically insulating layer (2) is between 30 nm and 150 nm.

8. The method according to any one of claims 1 to 2, wherein: The gas ions (40) include helium ions.

9. The method according to any one of claims 1 to 2, wherein: The transfer of the semiconductor layer (3a) comprises: - forming a weakened area (31) in the donor substrate, thereby defining the semiconductor layer to be transferred; - After bonding, the donor substrate (30) is separated along the weakened area (31).

10. A method for manufacturing a front image sensor, the method comprising manufacturing a substrate using the method according to any one of claims 1 to 9, the transferred semiconductor layer (3a) and the additional semiconductor layer (3b) together forming an active layer of the image sensor, and forming a plurality of electrical isolation grooves (5) in the active layer to define a plurality of pixels.