Carbon having a redox functional group-containing polymer layer formed thereon, sulfur-carbon composite including the carbon, and lithium secondary battery
By using carbon or sulfur-carbon composite with a polymer layer containing redox functional groups in the cathode material of lithium secondary batteries, the dissolution and shuttling problems of lithium polysulfides are solved, and the capacity and life characteristics of lithium secondary batteries are improved.
Patent Information
- Application Number
- CN202080007118.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-28
- Filing Date
- 2020-05-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-05-29
AI Technical Summary
The dissolution and shuttling phenomena of lithium polysulfide in lithium-sulfur secondary batteries lead to reduced capacity and shortened battery life. It is difficult to significantly solve this problem through physical membranes using existing technology.
In the cathode material of lithium secondary batteries, carbon or sulfur-carbon composite with a polymer layer containing redox functional groups is used to catalytically reduce lithium polysulfide to prevent its dissolution and shuttling.
By catalytically reducing lithium polysulfide, the capacity and life characteristics of lithium secondary batteries are improved, and the kinetics and reactivity of the battery are significantly improved.
Smart Images

Figure CN113228352B_ABST
Abstract
Description
Technical Field
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2019-0064308, filed on May 31, 2019, and Korean Patent Application No. 10-2020-0064552, filed on May 28, 2020, which are hereby incorporated by reference in their entirety.
[0002] One aspect of the present disclosure relates to carbon having a redox functional group-containing polymer layer formed thereon, and a sulfur-carbon composite and a lithium secondary battery including the carbon. Background Art
[0003] With the growing interest in energy storage technology, research and development of electrochemical devices is gradually increasing as its applications are extending from energy for mobile phones, tablets, laptops and camcorders to energy for electric vehicles (EV) and hybrid electric vehicles (HEV). In this regard, the field of electrochemical devices is the field of greatest concern. Among them, the development of secondary batteries such as lithium-sulfur secondary batteries that can be charged / discharged has become a focus of attention. In recent years, in the development of these batteries, in order to improve capacity density and specific energy, research and development of new electrode and battery designs have been led.
[0004] Among these electrochemical devices, lithium-sulfur secondary batteries (Li-S batteries) have high energy density (theoretical capacity), and therefore have attracted much attention as next-generation secondary batteries that can replace lithium-ion batteries. In such lithium-sulfur secondary batteries, a reduction reaction of sulfur and an oxidation reaction of lithium metal occur during discharge. At this time, sulfur forms lithium polysulfide (LiPS) having a linear structure from S8 having a ring structure. This lithium-sulfur secondary battery is characterized by showing a step-by-step discharge voltage until the polysulfide is completely reduced to Li2S.
[0005] However, the biggest obstacle to the commercialization of lithium-sulfur secondary batteries is the dissolution and shuttling of lithium polysulfide, which causes a big problem of reduced capacity of lithium-sulfur secondary batteries. That is, since the polysulfide dissolved from the positive electrode has a high solubility in the organic electrolyte, undesired migration of polysulfide through the electrolyte to the negative electrode (polysulfide (PS) shuttling) may occur. As a result, capacity reduction due to irreversible loss of positive electrode active materials and shortened battery life due to precipitation of sulfur particles on the lithium metal surface due to side reactions may occur.
[0006] Therefore, in Korean Patent Publication No. 2018-0048309, it is disclosed that by applying a sulfur-carbon composite containing sulfur and carbon nanotubes having a surface coated with an ion conductive polymer to a lithium-sulfur secondary battery, problems related to the dissolution and shuttling phenomenon of polysulfides can be solved.
[0007] As described above, technologies for preventing the dissolution of lithium polysulfide by coating the outside of a sulfur-carbon composite used as a cathode material for a lithium-sulfur secondary battery, treating the surface of a separator, or using an anode protective film have been developed, but their effects are not significant.
[0008] Therefore, there is a need to develop a technology capable of solving the dissolution and shuttling problems of lithium polysulfide by a means other than the means of solving the dissolution problem of lithium polysulfide by simply using a physical membrane.
[0009] [Prior art literature]
[0010] [Patent Document]
[0011] (Patent Document 1) Korean Patent Publication No. 2018-0048309 Summary of the invention
[0012]
Technical issues
[0013] As a result of various studies conducted to solve the above-mentioned problems, the present inventors have confirmed that the capacity and life characteristics of lithium secondary batteries can be improved by using carbon containing a polymer layer containing redox functional groups that can be used as a catalyst to promote the reduction reaction of lithium polysulfide, or a sulfur-carbon composite prepared by using carbon containing a polymer layer containing redox functional groups as a positive electrode material for lithium secondary batteries.
[0014] Therefore, an object of one aspect of the present disclosure is to provide a method for preparing a sulfur-carbon composite capable of improving the capacity and life characteristics of a lithium secondary battery by being used as a positive electrode material for a lithium secondary battery.
[0015]
Technical solution
[0016] In order to achieve the above-mentioned object, one aspect of the present disclosure provides carbon having a redox functional group-containing polymer layer formed on the surface.
[0017] Another aspect of the present disclosure also provides a sulfur-carbon composite including carbon having a polymer layer containing redox functional groups formed on the surface thereof.
[0018] Another aspect of the present disclosure also provides a method for preparing carbon having a redox functional group-containing polymer layer formed on the surface, the method comprising the step of forming the redox functional group-containing polymer layer by coating the redox functional group-containing polymer on the surface of the carbon.
[0019] Another aspect of the present disclosure also provides a lithium secondary battery including a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode contains carbon or a sulfur-carbon composite formed with a polymer layer containing redox functional groups.
[0020]
Beneficial Effects
[0021] In the case of carbon having a polymer layer containing redox functional groups according to one aspect of the present disclosure, since the polymer containing redox functional groups can be used as a catalyst for reducing lithium polysulfide, when used as a positive electrode material for a lithium secondary battery, the kinetics can be improved to quickly reduce lithium polysulfide, thereby increasing reactivity while preventing the phenomenon of lithium polysulfide escaping from the positive electrode.
[0022] Furthermore, when carbon formed with a redox functional group-containing polymer layer is used alone or in the form of a sulfur-carbon composite as a positive electrode material for a lithium secondary battery, dissolution and shuttling of lithium polysulfide are prevented, thereby improving the capacity and life characteristics of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1a , Figure 1b and Figure 1c It is a graph showing the discharge capacity of lithium secondary batteries manufactured in Examples and Comparative Examples.
[0024] Figure 2a and Figure 2b It is a graph showing the results of evaluation of the life characteristics of the lithium secondary batteries manufactured in Examples and Comparative Examples by cyclic voltammetry.
[0025] Figure 3a and Figure 3b Graphs showing the activities of lithium secondary batteries manufactured in Examples and Comparative Examples to lithium polysulfide measured by cyclic voltammetry. DETAILED DESCRIPTION
[0026] Hereinafter, the present invention will be described in more detail to help understanding of the present invention.
[0027] The terms and words used in this specification and claims should not be interpreted as limited to common terms or dictionary terms, but should be interpreted as meanings and concepts consistent with the technical concept of the present invention based on the principle that the inventor can appropriately define the concept of the terms to describe his invention in the best possible way.
[0028] Carbon having a polymer layer containing redox functional groups and sulfur-carbon composite containing the carbon
[0029] One aspect of the present disclosure relates to carbon having a polymer layer containing redox functional groups formed on the surface, wherein the polymer layer containing redox functional groups can be used as a positive electrode material for a lithium secondary battery. In addition, the carbon having a polymer layer containing redox functional groups formed thereon can be used as a positive electrode material for a lithium secondary battery in the form of a sulfur-carbon composite.
[0030] In one aspect of the present disclosure, the polymer containing redox functional groups can be a component that promotes the reduction of lithium polysulfide (LiPS) dissolved from the positive electrode through a redox reaction, that is, a lithium conductive compound that forms a redox band by accepting electrons and thus exhibits conductivity. Specifically, when the polymer containing redox functional groups is applied to a positive electrode material for a lithium secondary battery, it can play a role in increasing kinetics and quickly reduce lithium polysulfide, thereby increasing reactivity and preventing the phenomenon of lithium polysulfide dissolving from the positive electrode.
[0031] The redox functional group-containing polymer is not particularly limited as long as it is a compound in which a =0 functional group is bonded to a benzene ring, and may be, for example, a compound such as quinones, imides, or naphthalene.
[0032] Specifically, as the redox functional group-containing polymer, quinone compounds such as polyanthraquinone such as poly-1,4-anthraquinone (P14AQ) or poly-1,5-anthraquinone (P15AQ), polynaphthoquinone, polybenzoquinone, etc. represented by the following formula 1 can be exemplified:
[0033] [Formula 1]
[0034]
[0035] Wherein n is a natural number from 1 to 1000.
[0036] In addition, as the polymer containing a redox functional group, a material that forms a redox band when accepting electrons and shows conductivity can be used without particular limitation, and examples thereof can include π-conjugated compounds such as polyaniline, polythiophene, polypyrrole, polyacetylene, polyparaphenylene, polyphenylene vinylene, polyperinaphthalene, polyfuran, polyfluorene, polythiophene, polypyridinediyl, polyisothianaphthene, polyquinoxaline, polypyridine, polypyrimidine, polyindole, polyaminoanthraquinone, polyimidazole and derivatives thereof.
[0037] In one aspect of the present disclosure, based on the total weight of the carbon on which the polymer layer containing redox functional groups is formed, the content of the polymer containing redox functional groups may be 0.1 wt % to 5 wt %, specifically 0.1 wt % or more, 0.15 wt % or more, or 0.25 wt % or more, and may be 1 wt % or less, 3 wt % or less, or 5 wt % or less. If the content of the polymer containing redox functional groups is less than 0.1 wt %, the effect obtained by using the polymer containing redox functional groups and carbon may not be significant. If the content of the polymer containing redox functional groups is greater than 5 wt %, overvoltage may occur in the polymer layer containing redox functional groups, and in this case, the energy density is reduced, which may impair battery performance. In addition, the number average molecular weight (Mn) of the polymer containing redox functional groups may be 500 to 200,000, specifically 500 or more or 1,000 or more, and may be 100,000 or less or 200,000 or less.
[0038] In order to prevent the occurrence of overvoltage, the redox functional group-containing polymer layer according to one aspect of the present disclosure may preferably be formed thinly and uniformly in about several nanometers to several tens of nanometers.
[0039] In one aspect of the present disclosure, carbon can be applied without particular limitation as long as it is a conductive carbon material that can show the effect of improving the reduction efficiency of lithium polysulfide by having conductivity and thus transferring electrons to a redox functional group-containing polymer. Among them, carbon nanotubes (CNTs), graphene, and reduced graphene oxide (rGO) can be exemplified. Among these, reduced graphene oxide is preferably used, and thermally exfoliated reduced graphene oxide (TErGO) is more preferably used, which is advantageous in exfoliation due to thermal expansion and can therefore be applied thinly and over a large area, thereby showing excellent performance.
[0040] In addition, the carbon has pores, and the porosity may be 40% to 90%, specifically 40% or more, 50% or more, or 60% or more, and may be 80% or less, 85% or less, or 90% or less. If the porosity is less than 40%, lithium ions cannot be transported normally, which may cause problems due to acting as a resistance component. If the porosity exceeds 90%, there may be a problem of reduced mechanical strength. In addition, the pore size of the conductive carbon may be 10nm to 5μm, specifically 10nm or more, 20nm or more, 30nm or more, 40nm or more, or 50nm or more, and may be 4μm or less, 4.5μm or less, or 5μm or less. If the size of the pore is less than 10nm, there may be a problem that lithium ions cannot penetrate. If the size of the pore exceeds 5μm, there may be problems with battery short circuits and safety due to contact between electrodes.
[0041] Based on the total weight of the sulfur-carbon composite, the carbon having a polymer layer containing a redox functional group formed on the surface may be contained in an amount of 10 wt % to 40 wt %, specifically 10 wt % or more, 15 wt % or more, or 20 wt % or more, and may be 30 wt % or less, 35 wt % or less, or 45 wt % or less. If the content of the carbon having a polymer layer containing a redox functional group formed thereon is less than 10 wt %, the electrolyte cannot smoothly flow into and out of the positive electrode, so the lithium ion conductivity is reduced and the voltage drops accordingly, so that sufficient capacity of the battery may not be achieved and the reduction effect of lithium polysulfide may be reduced. In addition, if the content of the carbon having a polymer layer containing a redox functional group formed thereon exceeds 40 wt %, the discharge capacity and life characteristics of the battery may be reduced.
[0042] In one aspect of the present disclosure, sulfur can be used without particular limitation as long as it is sulfur commonly used in lithium secondary batteries. Specifically, sulfur can be selected from sulfur (S8), Li2S n (n≥1), organic sulfur compounds and carbon-sulfur polymers [(C2S x ) n , x is an integer from 2.5 to 50, and n≥2] is at least one of the group consisting of.
[0043] Sulfur may be contained in an amount of 60 wt % to 90 wt %, specifically 60 wt % or more, 65 wt % or more, or 70 wt % or more, and 80 wt % or less, 85 wt % or less, or 90 wt % or less, based on the total weight of the sulfur-carbon composite. If the sulfur content is less than 60 wt %, the sulfur content in the battery decreases, and thus the capacity of the battery decreases excessively. If the sulfur content exceeds 90 wt %, the conductivity in the electrode may decrease excessively, and thus the resistance may increase.
[0044] Carbon having a redox functional group-containing polymer layer formed thereon and method for producing a sulfur-carbon composite containing the carbon
[0045] Another aspect of the present disclosure also relates to a method for manufacturing carbon having a redox functional group-containing polymer layer formed thereon, the method comprising the step (S1) of forming the redox functional group-containing polymer layer on a surface of the carbon.
[0046] Furthermore, the sulfur-carbon composite may be prepared by including the following step (S2) after the step (S1): mixing carbon having the redox functional group-containing polymer layer formed thereon and sulfur, and then subjecting them to heat treatment.
[0047] In another aspect of the present disclosure, in step (S1), the polymer layer containing redox functional groups can be formed by a coating method, and the coating method is not particularly limited as long as it is a coating method for forming a layer in the art. For example, the polymer layer containing redox functional groups can be formed by wet coating, drop casting, dip coating, blade coating, spray coating, Meyer bar coating or vacuum filter coating.
[0048] When a solvent is required for coating, as the solvent that can be used, water or an organic solvent such as ethanol, acetone, isopropyl acetate (IPA), tetrahydrofuran (THF), dichloromethane (MC), dimethylformamide (DMF), dimethyl sulfoxide (DMSO) and dimethylacetamide (DMAc) can be exemplified. Among them, THF or a compound having a similar property can be expected to be used as a solvent.
[0049] In addition, when a polymer layer containing redox functional groups is formed on the surface of carbon, bonding at the interface between carbon and the polymer layer containing redox functional groups is achieved by the reaction between the polymer containing redox functional groups and the carbon (bonding by π-π interaction). At this time, the reaction can be carried out at room temperature to 100°C, specifically 20°C or more, 25°C or more, 30°C or more, 35°C or more, or 40°C or more, or 70°C or less, 75°C or less, 80°C or less, 85°C or less, 90°C or less, 95°C or less, or 100°C or less, for 1 hour or more, 2 hours or more, 3 hours or more, or 4 hours or more, or 10 hours or less, 12 hours or less, 14 hours or less, 16 hours or less, 18 hours or less, 20 hours or less, 22 hours or less, or 24 hours or less.
[0050] In another aspect of the present disclosure, in step (S2), sulfur is supported on the carbon having the redox functional group-containing polymer layer formed thereon by mixing the carbon having the redox functional group-containing polymer layer formed thereon and sulfur and heat-treating them.
[0051] The heat treatment temperature is a temperature at which sulfur is melted and infiltrated and supported on carbon, and may be equal to or higher than the melting point of sulfur.
[0052] Specifically, the temperature during the heat treatment may be 100°C or more, 110°C or more, or 120°C or more, and may be 180°C or less, 190°C or less, or 200°C or less, and may be heat treated by a melt diffusion method. If the heat treatment temperature is lower than the above range, the sulfur may not be able to be prepared because the sulfur melts and penetrates into the carbon. If the heat treatment temperature is higher than the above range, the sulfur-carbon composite itself may not be prepared because the loss rate of sulfur increases due to gasification and the sulfur-carbon composite is denatured, so when used as a positive electrode material for a lithium secondary battery, the effect of improving battery performance may be insufficient.
[0053] Lithium secondary battery
[0054] Another aspect of the present disclosure also relates to a lithium secondary battery comprising a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode comprises a carbon or sulfur-carbon composite having a polymer layer containing redox functional groups as described above formed thereon as a positive electrode active material.
[0055] positive electrode
[0056] The positive electrode used in another aspect of the present disclosure will be described below. After preparing a positive electrode composition containing a positive electrode active material, a conductive material and a binder, a slurry prepared by diluting such a composition in a predetermined solvent (dispersion medium) can be directly coated on a positive electrode collector and dried to form a positive electrode layer. Alternatively, after the slurry is cast on a separate support, the film obtained by peeling off the support can be laminated on a positive electrode collector to manufacture a positive electrode layer. In addition, the positive electrode can be manufactured in a variety of ways using methods well known to those skilled in the art.
[0057] The conductive material not only serves as a path for electrons to move from the positive electrode current collector to the positive electrode active material, thereby imparting electronic conductivity, but also electrically connects the electrolyte and the positive electrode active material, thereby simultaneously serving as a lithium ion (Li ion) in the electrolyte. +) moves to sulfur and reacts with sulfur. Therefore, if the amount of conductive material is insufficient or the conductive material does not function properly, the unreacted portion of sulfur in the electrode will increase and eventually lead to a decrease in capacity. In addition, high-rate discharge characteristics and charge / discharge cycle life will be adversely affected. Therefore, it is necessary to add an appropriate amount of conductive material. Based on the total weight of the positive electrode composition, it is preferred to add a conductive material in an amount of 0.01 wt % to 30 wt %.
[0058] The conductive material is not particularly limited as long as it has conductivity without causing chemical changes in the corresponding battery, and for example, graphite can be used; carbon blacks such as DENKA black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum powder and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc. Specific examples of commercially available conductive materials may include acetylene black series products or DENKA black (Denka Singapore Private Limited) from Chevron Chemical Company, products from Gulf Oil Company, Ketjen black EC series products from Armak Company, Vulcan XC-72 products from Cabot Company, and Super P (a product from Timcal Company).
[0059] The binder is used to adhere the positive electrode active material well to the collector. The binder needs to be well dissolved in the solvent, and can not only construct a conductive network between the positive electrode active material and the conductive material, but also have appropriate electrolyte impregnation performance. The binder can be any binder known in the art, and specifically can be but not limited to any one selected from the group consisting of: a fluororesin binder containing polyvinylidene fluoride (PVdF) or polytetrafluoroethylene (PTFE); a rubber binder containing styrene-butadiene rubber, acrylonitrile-butadiene rubber and styrene-isoprene rubber; a cellulose binder containing carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose and regenerated cellulose; a polyol binder; a polyolefin binder containing polyethylene and polypropylene; a polyimide binder; a polyester binder; a silane binder; or a mixture or copolymer of two or more thereof.
[0060] The content of the binder may be, but is not limited to, 0.5 wt % to 30 wt % based on the total weight of the positive electrode composition. If the content of the binder resin is less than 0.5 wt %, the physical properties of the positive electrode may deteriorate, and thus the positive electrode active material and the conductive material may fall off. If the content exceeds 30 wt %, the proportion of the active material and the conductive material in the positive electrode may be relatively reduced, and thus the battery capacity may be reduced, and such a content results in the function of a resistance element and reduces efficiency.
[0061] The positive electrode composition containing a positive electrode active material, a conductive material and a binder can be diluted in a predetermined solvent and coated on a positive electrode collector using conventional methods known in the art. First, a positive electrode collector is prepared. The positive electrode collector generally has a thickness of 3 μm to 500 μm. The positive electrode collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, it can be stainless steel, aluminum, nickel, titanium, sintered carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The collector can also increase the adhesion of the positive electrode active material by forming fine concave-convex on its surface and can be in various forms, such as films, sheets, foils, nets, porous bodies, foams, and non-woven fabrics.
[0062] Next, a slurry obtained by diluting a positive electrode composition containing a positive electrode active material, a conductive material and a binder in a solvent is applied to the positive electrode collector. The positive electrode composition containing the above-mentioned positive electrode active material, conductive material and binder can be mixed with a predetermined solvent to prepare the slurry. At this time, the solvent can be easily dried, and it is most preferred that the binder can be well dissolved but the positive electrode active material and the conductive material are kept in a dispersed state without dissolving them. If the solvent dissolves the positive electrode active material, there is a tendency for sulfur to sink in the slurry due to the high specific gravity of sulfur in the slurry (D=2.07), which in turn causes sulfur to accumulate on the collector during coating and causes problems in the conductive network, thereby causing problems in battery operation. The solvent (dispersion medium) may be water or an organic solvent. The organic solvent may be at least one selected from the group consisting of dimethylformamide, isopropanol, acetonitrile, methanol, ethanol and tetrahydrofuran.
[0063] Subsequently, there is no particular restriction on the coating method of the positive electrode composition in a slurry state. For example, the coating can be prepared by a blade coating method, a dip coating method, a gravure coating method, a slot die coating method, a spin coating method, a comma-type blade coating method, a rod coating method, a reverse roll coating method, a screen printing coating method, and a cap coating method. Afterwards, in the positive electrode composition that has passed through such a coating process, the evaporation of the solvent (dispersion medium), the densification of the coating film, and the adhesion between the coating film and the current collector are realized by a drying process. At this point, drying is carried out according to a conventional method and is not particularly limited.
[0064] negative electrode
[0065] As the negative electrode, any one capable of inserting and extracting lithium ions can be used. For example, metal materials such as lithium metal and lithium alloys; and carbon materials such as low-crystalline carbon and high-crystalline carbon can be exemplified. As low-crystalline carbon, soft carbon and hard carbon are typical. As high-crystalline carbon, natural graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, mesophase carbon microbeads, mesophase pitch, and high-temperature sintered carbon such as coke derived from petroleum or coal tar pitch are typical. In addition, alloy series containing silicon, such as Li4Ti5O 12 Oxides of are also well-known negative electrodes.
[0066] In this case, the negative electrode may include a binder, and the binder may be various kinds of binder polymers such as polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP copolymer), polyacrylonitrile, polymethyl methacrylate, and styrene-butadiene rubber (SBR).
[0067] The negative electrode may optionally further comprise a negative electrode current collector for supporting a negative electrode active layer containing a negative electrode active material and a binder. The negative electrode current collector may be specifically selected from the group consisting of copper, stainless steel, titanium, silver, palladium, nickel, their alloys and combinations thereof. Stainless steel may be surface treated with carbon, nickel, titanium or silver, and aluminum-cadmium alloy may be used as an alloy. In addition, sintered carbon, a non-conductive polymer or a conductive polymer surface treated with a conductive material may be used.
[0068] The binder is used to adhere the negative electrode active material, to bond the active materials to each other, to bond the active material to the current collector, to buffer the expansion and contraction of the active material, etc. Specifically, the binder is the same as that described above for the binder of the positive electrode. In addition, the negative electrode can be lithium metal or a lithium alloy. A non-limiting example of the negative electrode can be a thin film of lithium metal, and can be an alloy of lithium and at least one metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba, Ra, Al and Sn.
[0069] Diaphragm
[0070] The separator may be composed of a porous substrate. Any porous substrate may be used as long as it is a porous substrate generally used in electrochemical devices, and for example, a polyolefin-based porous film or a polyolefin-based nonwoven fabric may be used, but is not particularly limited thereto.
[0071] Examples of polyolefin porous films may be films formed from any one polymer selected from polyethylene, such as high-density polyethylene, linear low-density polyethylene, low-density polyethylene and ultra-high molecular weight polyethylene; and polyolefin polymers, such as polypropylene, polybutene and polypentene, alone or by mixing them.
[0072] In addition to the above-mentioned polyolefin nonwoven fabrics, the nonwoven fabric may be formed of any one polymer selected from polyesters such as polyethylene terephthalate, polybutylene terephthalate and polyethylene naphthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene ether, polyphenylene sulfide, etc., alone or in combination. The structure of the nonwoven fabric may be a spunbond nonwoven fabric or a meltblown nonwoven fabric composed of long fibers.
[0073] The thickness of the porous substrate is not particularly limited, but may be 1 μm or more or 5 μm or more, and may be 50 μm or less or 100 μm or less.
[0074] The size and porosity of the pores present in the porous substrate are also not particularly limited, but may be 0.001 μm to 50 μm and 10% to 95%, respectively.
[0075] Electrolyte
[0076] The electrolyte comprises a solvent and a lithium salt, and may further contain an additive if necessary. The solvent may be used without particular limitation as long as it is a conventional non-aqueous solvent used as a medium through which ions participating in the electrochemical reaction of the battery can move. Examples of the non-aqueous solvent may include carbonate solvents, ester solvents, ether solvents, ketone solvents, alcohol solvents, aprotic solvents, and the like.
[0077] More specifically, examples of carbonate solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), or butylene carbonate (BC), etc. Examples of ester solvents may specifically include methyl acetate, ethyl acetate, n-propyl acetate, 1,1-dimethylethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, decalactone, valerolactone, mevalonolactone, and caprolactone, etc. Examples of ether solvents may specifically include ethyl ether, dipropyl ether, dibutyl ether, dimethoxymethane, trimethoxymethane, dimethoxyethane, diethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, tetrahydrofuran, 2-methyltetrahydrofuran, and polyethylene glycol dimethyl ether, etc. In addition, examples of ketone solvents may include cyclohexanone and the like. Examples of alcohol solvents may include ethanol and isopropanol and the like. Examples of aprotic solvents may include nitriles such as acetonitrile; amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane (DOL); and cyclopentane sulfone and the like. The non-aqueous organic solvent may be used alone or in combination of two or more. The mixing ratio when two or more are used in combination can be appropriately adjusted according to the desired performance of the battery, and a solvent in which 1,3-dioxolane and dimethoxyethane are mixed in a volume ratio of 1:1 can be exemplified.
[0078] Hereinafter, preferred embodiments are provided to help understand the present invention, but the following embodiments only illustrate the present invention, and it is obvious to those skilled in the art that various changes and modifications can be made within the scope and technical spirit of the present invention, and naturally, these changes and modifications belong to the appended claims.
[0079] Example 1
[0080] (1) Preparation of sulfur-carbon composites
[0081] (1-1) Formation of carbon having a redox functional group-containing polymer layer formed thereon
[0082] Using a solution in which poly-1,4-anthraquinone as a redox functional group-containing polymer was dissolved in dichloromethane (MC) at a concentration of 23%, a redox functional group-containing polymer layer having a nanometer unit thickness was formed on the surface of CNT as carbon in a mortar by a wet coating method. At this time, the content of poly-1,4-anthraquinone was set to 0.25 wt % based on the total weight of the carbon on which the redox functional group-containing polymer layer was formed.
[0083] (1-2) Formation of sulfur-carbon complex
[0084] A mixture was obtained by mixing 25 wt % of the carbon powder on which the redox functional group-containing polymer layer obtained in (1-1) above was formed and 75 wt % of the sulfur powder.
[0085] The mixture was heat-treated at 155° C., thereby supporting sulfur on carbon by a melt diffusion method to prepare a sulfur-carbon composite.
[0086] (2) Manufacturing of positive electrode
[0087] The sulfur-carbon composite obtained in (1) as a positive electrode active material, vapor grown carbon fiber (VGCF) as a conductive material, and polyvinylidene fluoride (PVDF) as a binder were mixed at a weight ratio of 8:1:1 and dispersed in water at a concentration of 22.5% to prepare a positive electrode slurry.
[0088] The positive electrode slurry was coated on an Al foil to a thickness of 225 μm and dried at 50° C. to manufacture a positive electrode.
[0089] (3) Manufacturing of lithium secondary batteries
[0090] A lithium secondary battery in the form of a coin cell was manufactured using a lithium foil having a thickness of 50 μm as a negative electrode, the positive electrode manufactured in (2) above, an electrolyte prepared by combining 1 M LiTFSI and 3 wt % LiNO3 with DOL / DME (1:1, v / v) as a solvent, and a polyolefin separator. At this time, DOL refers to dioxolane and DME refers to dimethoxyethane.
[0091] Example 2
[0092] A sulfur-carbon composite including carbon having a redox functional group-containing polymer layer formed thereon and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the content of poly-1,4-anthraquinone was set to 0.5 wt % based on the total weight of the carbon having the redox functional group-containing polymer layer formed thereon.
[0093] Example 3
[0094] A sulfur-carbon composite including carbon having a redox functional group-containing polymer layer formed thereon and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the content of poly-1,4-anthraquinone was set to 1.0 wt % based on the total weight of the carbon having the redox functional group-containing polymer layer formed thereon.
[0095] Example 4
[0096] (1) Formation of carbon having a redox functional group-containing polymer layer formed thereon
[0097] A redox functional group-containing polymer layer was formed on the surface of CNT as carbon in a mortar by a wet coating method using a solution in which poly-1,4-anthraquinone as a redox functional group-containing polymer was dissolved in dichloromethane (MC). At this time, the content of poly-1,4-anthraquinone was set to 0.25 wt % based on the total weight of the carbon on which the redox functional group-containing polymer layer was formed.
[0098] (2) Manufacturing of positive electrode
[0099] The carbon obtained in (1) as a positive electrode active material having a redox functional group-containing polymer layer formed thereon, vapor grown carbon fiber (VGCF) as a conductive material, and polyvinylidene fluoride (PVDF) as a binder were mixed in a weight ratio of 8:1:1 and dispersed in water to prepare a positive electrode slurry.
[0100] The positive electrode slurry was coated on an Al foil and dried to manufacture a positive electrode.
[0101] (3) Manufacturing of lithium secondary batteries
[0102] A lithium secondary battery in the form of a coin cell was manufactured using a lithium foil having a thickness of 50 μm as a negative electrode, the positive electrode manufactured in (2) above, an electrolyte prepared by combining 1 M LiTFSI and 3 wt % LiNO3 with DOL / DME (1:1, v / v) as a solvent, and a polyolefin separator. At this time, DOL refers to dioxolane and DME refers to dimethoxyethane.
[0103] Example 5
[0104] A carbon and lithium secondary battery having a redox functional group-containing polymer layer formed thereon were manufactured in the same manner as in Example 4, except that the content of poly-1,4-anthraquinone was set to 0.5 wt % based on the total weight of the carbon having the redox functional group-containing polymer layer formed thereon.
[0105] Example 6
[0106] A carbon and lithium secondary battery having a redox functional group-containing polymer layer formed thereon were manufactured in the same manner as in Example 4, except that the content of poly-1,4-anthraquinone was set to 1.0 wt % based on the total weight of the carbon having the redox functional group-containing polymer layer formed thereon.
[0107] Comparative Example 1
[0108] A sulfur-carbon composite and a lithium secondary battery were manufactured in the same manner as in Example 1, except that carbon on which the redox functional group-containing polymer layer was not formed was used.
[0109] Comparative Example 2
[0110] A sulfur-carbon composite and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the surface of carbon was not coated with poly-1,4-anthraquinone as a redox functional group-containing polymer but poly-1,4-anthraquinone was simply added.
[0111] Comparative Example 3
[0112] A carbon and lithium secondary battery having a redox functional group-containing polymer layer formed thereon was manufactured in the same manner as in Example 4, except that an electrolyte to which lithium polysulfide (LiPS) was added was used.
[0113] Comparative Example 4
[0114] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode was manufactured by forming a CNT layer on one side of the Al foil and forming a redox functional group-containing polymer layer on the CNT layer.
[0115] At this time, the CNT layer was formed by mixing CNT, VGCF (vapor grown carbon fiber) as a conductive material, and polyvinylidene fluoride (PVDF) as a binder in a weight ratio of 8:1:1, and then dispersing the resulting mixture in water at a concentration of 22.5 wt % to prepare a slurry, coating the slurry on an Al foil and drying it.
[0116] Furthermore, a solution prepared by dissolving poly-1,4-anthraquinone as a redox functional group-containing polymer in MC (dichloromethane) at a concentration of 1 wt % was applied to the CNT layer to a thickness of 225 μm by a wet coating method and dried at 50° C. to form a redox functional group-containing polymer layer.
[0117] Experimental Example 1
[0118] After performing 3 cycles at a discharge current rate of 0.1C and 3 cycles at 0.2C and then setting the discharge current rate to 0.5C, the discharge capacities of the lithium secondary batteries manufactured in Examples 1, 2, 3 and Comparative Examples 1 and 2 were observed.
[0119] Figure 1a , Figure 1b and Figure 1c It is a graph showing the discharge capacity of lithium secondary batteries manufactured in Examples and Comparative Examples.
[0120] Reference Figure 1aIt can be seen that the lithium secondary batteries of Examples 1 to 3 using sulfur-carbon composites containing carbon having a polymer layer containing redox functional groups formed thereon show excellent initial discharge capacity and average specific capacity compared to the lithium secondary battery of Comparative Example 1 using a sulfur-carbon composite containing carbon without a polymer layer containing redox functional groups formed thereon.
[0121] Reference Figure 1b It can be seen that compared with Example 1 in which a sulfur-carbon composite containing carbon on which a polymer layer containing a redox functional group is formed is applied, Comparative Example 4 in which the collector, the CNT layer and the polymer layer containing a redox functional group are stacked in sequence has poor life characteristics.
[0122] Reference Figure 1c , it can be seen that Comparative Example 2 in which the redox functional group-containing polymer was simply added had inferior life characteristics compared to Comparative Example 1 in which the redox functional group-containing polymer was not present.
[0123] Experimental Example 2
[0124] For the lithium secondary batteries manufactured in Example 4, Example 5, Example 6, and Comparative Example 2, life characteristics were evaluated by applying cyclic voltammetry.
[0125] Figure 2a and Figure 2b It is a graph showing the results of evaluation of the life characteristics of the lithium secondary batteries manufactured in Examples and Comparative Examples by cyclic voltammetry. Figure 2a The evaluation results of cyclic voltammetry at a rate of 0.1 mV / s are shown, and for the lithium secondary battery of Example 4, Figure 2b Evaluation results of cyclic voltammetry performed at rates of 0.1 mV / s, 0.2 mV / s, 0.3 mV / s, 0.4 mV / s, and 0.5 mV / s are shown.
[0126] Reference Figure 2a It can be seen that Examples 4, 5, 6, which contain poly-1,4-anthraquinone as a polymer containing redox functional groups in the form of a polymer layer, and Comparative Example 2, in which poly-1,4-anthraquinone is simply added, all have electrochemical reactivity and reversibility, because they include the polymer containing redox functional groups.
[0127] Reference Figure 2b It can be seen that the reactivity of poly-1,4-anthraquinone itself as a polymer containing a redox functional group is rapid, and when applied to a battery it will also be effective in high rate operation.
[0128] Experimental Example 3
[0129] For the lithium secondary batteries manufactured in Example 4 and Comparative Example 3, the activity to lithium polysulfide was evaluated by applying cyclic voltammetry at a rate of 0.1 mV / s.
[0130] Figure 3a and Figure 3b Graphs showing the activities of lithium secondary batteries manufactured in Examples and Comparative Examples to lithium polysulfide measured by cyclic voltammetry.
[0131] Reference Figure 3a , it can be seen that Example 4 has higher activity for lithium polysulfide than Comparative Example 3 in which lithium polysulfide is added to the electrolyte.
[0132] Reference Figure 3b It can be seen that even after 20 cycles, Example 4 has a higher activity towards lithium polysulfide than Comparative Example 3.
[0133] Although the present invention has been described above by means of limited embodiments and drawings, the present invention is not limited thereto, and of course, a person skilled in the art to which the present invention pertains may make various modifications and changes within the technical spirit of the present invention and the scope of equivalents of the appended claims.
Claims
1. A carbon having a polymer layer containing redox functional groups formed on the surface, wherein: The polymer containing redox functional groups is a quinone compound selected from the group consisting of polyanthraquinone, polynaphthoquinone and polybenzoquinone, The content of the polymer containing redox functional groups is 0.1 wt % to 5 wt % based on the total weight of the carbon having the redox functional group-containing polymer layer formed on the surface. 2 . The carbon having a redox functional group-containing polymer layer formed on the surface according to claim 1 , wherein the redox functional group-containing polymer is polyanthraquinone, and the polyanthraquinone is poly-1,4-anthraquinone or poly-1,5-anthraquinone. 3 . The carbon having a redox functional group-containing polymer layer formed on the surface according to claim 1 , wherein the carbon comprises at least one selected from the group consisting of carbon nanotubes, graphene, and reduced graphene oxide. 4 . A sulfur-carbon composite comprising the carbon according to claim 1 having a redox functional group-containing polymer layer formed on the surface thereof.
5. The sulfur-carbon composite according to claim 4, wherein The sulfur-carbon composite contains the carbon having the redox functional group-containing polymer layer formed on the surface in an amount of 10 to 40 weight % and contains sulfur in an amount of 60 to 90 weight %.
6. A method for preparing carbon having a polymer layer containing redox functional groups as claimed in claim 1, comprising the step of coating a polymer containing redox functional groups on the surface of carbon to form the polymer layer containing redox functional groups.
7. The method for preparing carbon having a polymer layer containing redox functional groups according to claim 6, wherein the coating is performed by droplet casting, wet coating, dip coating, blade coating, spray coating, Meyer rod coating or vacuum filter coating. 8 . The method for preparing carbon having a redox functional group-containing polymer layer formed thereon according to claim 6 , wherein when the redox functional group-containing polymer layer is formed, the redox functional group-containing polymer and the carbon are bonded to each other through π-π interaction.
9. A lithium secondary battery comprising a positive electrode; a negative electrode; a separator disposed between the positive electrode and the negative electrode; and an electrolyte, wherein the positive electrode comprises the carbon having a polymer layer containing redox functional groups formed on the surface according to claim 1 or the sulfur-carbon composite according to claim 4. 10 . The lithium secondary battery according to claim 9 , wherein the lithium secondary battery is a lithium-sulfur secondary battery.