Controlling dopant concentration in silicon melt to enhance ingot quality

By controlling the dopant concentration in the silicon melt, the problem of incomplete dislocation elimination during the growth of single crystal silicon ingots is solved, and the growth of single crystal silicon ingots with low dislocation is achieved, improving the quality and manufacturing application of ingots sex.

CN113272479BActive Publication Date: 2024-11-08GLOBALWAFERS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980066785.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-10-12
Filing Date
2019-09-09
Publication Date
2024-11-08
Estimated Expiration
2039-09-09

AI Technical Summary

Technical Problem

The existing single-crystal silicon ingots have problems of incomplete dislocation elimination during the growth process, resulting in poor quality of the ingot, difficult to manufacture and high cost for equipment.

Method used

By controlling the dopant concentration in the silicon melt, n-type dopants are added to the silicon seed during growth, ensuring the resistivity of the neck and outwardly open seed-cone portions is between 5 mohms and 12 mt to 12 mt. Between milliohm-cm, minimize or eliminate dislocations, achieving low or zero dislocation growth.

Benefits of technology

Effectively reduce or eliminate dislocations in single-crystal silicon ingots, improve the quality of the ingots, reduce scrap costs, and is suitable for device manufacturing to achieve efficient growth of single-crystal silicon ingots.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113272479B_ABST
    Figure CN113272479B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for manufacturing a single crystal silicon ingot, wherein the dopant concentration in the silicon melt is controlled. The control of the dopant concentration enhances the ingot quality by reducing or eliminating dislocations in the neck, crown and body of the single crystal silicon ingot.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of priority to U.S. Provisional Application No. 62 / 744,672, filed on October 12, 2018, the disclosure of which is incorporated by reference as if fully set forth. Technical Field

[0003] The field of the present disclosure relates to methods for making single crystal silicon ingots, and more particularly, to a method of making single crystal silicon ingots with enhanced quality by controlling dopant concentration in a silicon melt. Background Art

[0004] Single crystal silicon, which is the starting material for most processes used to make semiconductor electronic components, is typically prepared by the Czochralski ("Cz") method. In this method, polycrystalline silicon ("polysilicon") is loaded into a crucible and melted, a seed crystal is brought into contact with the molten silicon, and a single crystal is grown by slow extraction. After the formation of the neck is complete, the diameter of the crystal is enlarged by, for example, reducing the pull rate and / or melt temperature until the desired or target diameter is reached. Next, a cylindrical body of the crystal with an approximately constant diameter is grown by controlling the pull rate and melt temperature while compensating for the reduced melt level. Towards the end of the growth process but before the crucible is emptied of molten silicon, the crystal diameter is typically gradually reduced to form a tail end in the form of an end cone. The end cone is typically formed by increasing the crystal pull rate and the heat supplied to the crucible. When the diameter becomes sufficiently small, the crystal then separates from the melt.

[0005] At the start of crystal growth, dislocations are generated in the crystal by the thermal shock of bringing the seed crystal into contact with the melt. These dislocations propagate and multiply throughout the growing crystal unless they are eliminated in the neck portion between the seed crystal and the main body of the crystal.

[0006] Conventional methods for eliminating dislocations within silicon single crystals include the so-called "necking method," which involves growing a neck having a small diameter (e.g., 2 to 4 mm) at a high pull rate (e.g., up to 6 mm / minute) to completely eliminate dislocations before starting growth of the main body of the crystal. Generally, dislocations can be eliminated in these small diameter necks after approximately 100 to about 125 mm of necks have been grown. Once the dislocations have been eliminated, the diameter of the crystal is expanded to form an outwardly flaring "cone" or "taper" portion. When the desired diameter of the outwardly flaring seed-cone adjacent the neck portion is reached, a cylindrical main body is then grown to have an approximately constant diameter.

[0007] While conventional methods for eliminating dislocations are mostly successful, such methods can result in some necks containing dislocations that propagate into the constant diameter portion of the ingot. Such ingots are not suitable for device fabrication and have high scrap costs.

[0008] This paragraph is intended to introduce the reader to various aspects of the art that may be related to the various aspects of the present disclosure described and / or claimed below. It is believed that this discussion helps to provide the reader with background information to facilitate a better understanding of the various aspects of the present disclosure. Therefore, it should be understood that these statements should be read in this sense and not as an admission of prior art. Summary of the invention

[0009] One aspect of the present disclosure relates to a method of preparing a single crystal silicon ingot by a Czochralski method. The method includes: contacting a silicon seed crystal with a silicon melt, wherein the silicon melt is contained in a crucible and includes molten silicon and an n-type dopant; withdrawing the silicon seed crystal from the silicon melt to form a neck portion of the single crystal silicon ingot, the neck portion having a resistivity between 5 milliohm-cm and about 12 milliohm-cm; growing an outwardly flared seed-cone adjacent to the neck portion of the single crystal silicon ingot, the outwardly flared seed-cone having a resistivity between 5 milliohm-cm and about 12 milliohm-cm; adding an n-type dopant to the melt at a concentration sufficient to reduce the resistivity of the main body of the single crystal silicon ingot to a resistivity of less than 4 milliohm-cm; and growing a main body of the single crystal silicon ingot adjacent to the outwardly flared seed-cone, the main body of the single crystal silicon ingot having a resistivity of less than 4 milliohm-cm.

[0010] There are various improvements to the features set forth with respect to the above-mentioned aspects of the present disclosure. Likewise, further features may also be incorporated into the above-mentioned aspects of the present disclosure. These improvements and additional features may exist individually or in any combination. For example, the various features discussed below with respect to any of the illustrated embodiments of the present disclosure may be incorporated into any of the above-mentioned aspects of the present disclosure individually or in any combination. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 is a partial elevation view of a single crystal silicon ingot grown by the Czochralski method.

[0012] Figure 2 is a graph depicting zero dislocation or zero dislocation loss growth of a single crystal silicon ingot grown by the Czochralski method as a function of the resistivity of the neck and flared seed-cone portions of the ingot.

[0013] Corresponding reference characters indicate corresponding parts throughout the drawings. DETAILED DESCRIPTION

[0014] The disclosed arrangements relate to methods for manufacturing single crystal silicon ingots with enhanced ingot quality. Growing zero dislocation (ZD) single crystal silicon ingots from highly doped silicon melts according to the Czochralski method presents difficulties. During crystal growth, especially for highly doped silicon melts, the outward flaring seed-cone or crown can lose structure. A common cause for zero dislocation loss (LZD) in the outward flaring seed-cone or crown is incomplete dislocation elimination during growth of the neck portion. If a dislocation survives, it can reach the solid-liquid interface and begin to grow with the growth interface.

[0015] When the crystal diameter is increased to make the crown, thermal stresses increase significantly, and dislocations begin to multiply to relieve stresses through plastic deformation. After some time, the density of dislocations is high enough that the growth lines disappear and the loss of structure becomes apparent. Therefore, a method is needed to address the incomplete dislocation elimination in silicon crystals during the growth of the neck from a highly doped silicon melt.

[0016] The present invention provides a method for maximizing the probability of reducing or eliminating dislocations in one or all of the neck portion, the adjacent outward flaring seed-cone and the main body of a single crystal silicon ingot. Low or zero dislocation growth is obtained by controlling the dopant concentration in the silicon melt during the growth of the single crystal silicon ingot. The method provides for adding a controlled amount of dopant to the melt before starting the neck. The amount of dopant should be such that a resistivity between 5 milliohm-cm and about 12 milliohm-cm (e.g., between 5 milliohm-cm and about 8 milliohm-cm) is obtained at the seed end. This resistivity corresponds to a dopant concentration range in which the vacancy concentration in the crystal is the maximum during neck growth in the case of doping with n-type dopants (e.g., arsenic doping). Therefore, in some embodiments, the neck portion of the single crystal silicon ingot includes vacancies as the dominant intrinsic point defects. In some embodiments, the outward flaring seed-cone of the single crystal silicon ingot includes vacancies as the dominant intrinsic point defects. In the resistivity range between 5 milliohm-cm and about 12 milliohm-cm (e.g., between 5 milliohm-cm and about 8 milliohm-cm), dislocations climb to the crystal / melt surface interface (i.e., the edge of the growing ingot) and are eliminated. This method can be conveniently applied to crystal growth methods in which any target resistivity is achieved by doping during the bulk phase, such as the continuous Czochralski method. In this case, in fact, the process can be started with a melt concentration optimized for dislocation elimination in the neck, and a successful zero dislocation (ZD) crown is achieved, and the bulk is started. When starting the bulk, by doping during growth, much lower resistivities (e.g., less than about 4 milliohm-cm, less than about 2 milliohm-cm, less than about 1.7 milliohm-cm, or even about 1.6 milliohm-cm and less) can be achieved without incurring losses in the structure (zero dislocation losses or LZD).

[0017] Figure 1 A single crystal silicon ingot 10 is shown, produced according to an embodiment of the present disclosure, and in general, by the Czochralski method. The ingot 10 includes a portion of a seed 12 that is initially in contact with a silicon melt, a neck portion 24 adjacent the seed 12, a flared seed-cone portion 16, a shoulder 18, and a constant diameter body 20. The neck 24 is attached to the seed 12, which is in contact with the melt and is withdrawn to form the ingot 10. The neck 24 terminates once the cone portion 16 of the ingot begins to form.

[0018] In general, the melt from which the ingot 10 is extracted is formed by loading polycrystalline silicon into a crucible to form a silicon charge. Various sources of polycrystalline silicon can be used, including, for example, granular polycrystalline silicon produced by thermally decomposing silane or halogenated silane in a fluidized bed reactor, or polycrystalline silicon produced in a Siemens reactor. The solid polycrystalline silicon added to the crucible is usually granular polycrystalline silicon, but block polycrystalline silicon can be used, and it is fed into the crucible using a polycrystalline silicon feeder optimized for use with granular polycrystalline silicon. Block polycrystalline silicon typically has a size between 3 mm and 45 mm (e.g., maximum size), and granular polycrystalline silicon typically has a size between 400 microns and 1400 microns. Granular polycrystalline silicon has several advantages, including easy and precise control of the feeding rate due to its smaller size. However, due to the chemical vapor deposition process or other manufacturing methods used in its manufacture, the cost of granular polycrystalline silicon is usually higher than that of block polycrystalline silicon. Chunk multicrystalline silicon has the advantage of being less expensive and capable of higher feed rates given its larger size. The operation of the heating unit, the location of the cooling jacket, and the power control are adjusted to accommodate the multicrystalline silicon feeder. Depending on the size of the single crystal silicon ingot, particularly for batch processes, the mass of the loaded silicon charge may vary from at least about 25 kg to about 2000 kg, such as at least about 50 kg to about 2000 kg, or at least about 50 kg to about 1800 kg, such as between about 50 kg and about 1500 kg.

[0019] Once polycrystalline silicon is added to the crucible to form a charge, the charge is heated to a temperature above about the melting temperature of silicon (e.g., about 1412° C.) to melt the charge and thereby form a silicon melt including molten silicon. In some embodiments, the crucible including the silicon melt is heated to a temperature of at least about 1425° C., at least about 1450° C., or even at least about 1500° C.

[0020] In some embodiments, the process of the present invention is utilized in an n-type single crystal silicon ingot. As used herein, the term "n-type" refers to silicon containing an element from Group 5 of the periodic table (e.g., arsenic, phosphorus, antimony, or a combination thereof). In some embodiments, the silicon includes arsenic as an n-type dopant. An N-type ingot is obtained by adding an n-type dopant source (e.g., a solid element source of arsenic, phosphorus, and / or antimony of acceptable purity) to a silicon melt during Czochralski growth. In some embodiments, the concentration of the n-type dopant added to the silicon melt is between about 200 grams of n-type dopant / 60 kilograms of silicon and about 400 grams of n-type dopant / 60 kilograms of silicon, such as about 300 grams of n-type dopant / 60 kilograms of silicon. Due to factors such as incomplete incorporation of dopants, segregation coefficients of dopants between solidified silicon in the silicon melt and the ingot, and evaporation of dopants from the melt, the doping efficiency is typically less than 100%. Therefore, the amount of n-type dopant added to the silicon melt is typically about twice the amount effectively incorporated into the melt itself.

[0021] Once the charge is liquefied to form a silicon melt comprising molten silicon and n-type dopants, a silicon seed crystal (a portion of which is Figure 1 The silicon seed is then extracted from the melt, wherein the silicon is attached to the silicon seed (i.e., wherein the neck 24 is formed), thereby forming a melt-solid interface near or at the surface of the melt. In some embodiments, the silicon seed is extracted at a pulling rate between about 1.5 mm / min and about 6 mm / min (e.g., between about 3 mm / min and about 5 mm / min). In some embodiments, the silicon seed is rotated at a rate between about 5 rpm and about 30 rpm (or between about 5 rpm and about 20 rpm, or between about 8 rpm and about 20 rpm, or between about 10 rpm and about 20 rpm). In some embodiments, the silicon seed is rotated at a rate between about 8 rpm and about 15 rpm (e.g., about 11 rpm). In some embodiments, the crucible is rotated at a rate between about 0.5 rpm and about 10 rpm (or between about 1 rpm and about 10 rpm, or between about 4 rpm and about 10 rpm, or between about 5 rpm and about 10 rpm) (e.g., about 8 rpm). In some embodiments, the seed crystal is rotated at a faster rate than the crucible. In some embodiments, the seed crystal is rotated at a rate at least 1 rpm higher (e.g., at least about 3 rpm higher or at least about 5 rpm higher) than the crucible rotation rate. Conventionally, the crystal rotation rate is higher than the crucible rotation rate to facilitate good radial uniformity of dopant concentration in the crystal. In some embodiments, the silicon seed crystal and the crucible are rotated in opposite directions, i.e., counter-rotated.

[0022] In general, the neck portion has a length between about 10 mm and about 700 mm, between about 30 mm and about 700 mm, between about 100 mm and about 700 mm, between about 200 mm and about 700 mm, or between about 300 mm and about 700 mm. In some embodiments, the neck portion has a length between about 10 mm and about 100 mm (e.g., between about 20 mm and about 50 mm). In some embodiments, the neck portion has a length between about 350 mm and about 550 mm. In some embodiments, the neck portion has a length between about 450 mm and about 550 mm. However, the length of the neck portion may vary outside these ranges. In some embodiments, the neck portion has a diameter between about 1 mm and about 10 mm, between about 2.5 mm and about 6.5 mm (e.g., between about 3 mm and about 6 mm). The lower limit of the neck diameter is determined by the need to have sufficient mechanical strength to maintain the weight of the crystal when the size of the main body of the crystal ingot grows. The upper limit is determined by the fact that dislocation elimination becomes more difficult as the diameter increases, i.e., if the diameter is larger, then the distance from the surface that the dislocation must travel is longer plus the risk of dislocation multiplication driven by higher thermal stresses induced by higher thermal gradients between the crystal center and the crystal surface. In some embodiments, the neck portion formed during the growth of the n-type single crystal silicon ingot has a resistivity between 5 milliohm-cm and about 12 milliohm-cm, such as between 5 milliohm-cm and about 8 milliohm-cm. Suitable concentrations of n-type dopants, particularly arsenic, incorporated into the neck portion to achieve these resistivities may be between about 3.5 x 10 18 atoms / cm 3 With about 1.3x10 19 atoms / cm 3 (For example, at about 4x10 18 atoms / cm 3 With 1x10 19 atoms / cm 3 )between.

[0023] After the neck is formed, the outwardly flared seed-cone portion 16 adjacent the neck 24 is grown. Generally, the pull rate is reduced from the neck portion pull rate to a rate suitable for growing the outwardly flared seed-cone portion 16. For example, the seed-cone pull rate during the growth of the outwardly flared seed-cone 16 is between about 0.5 mm / minute and about 2.0 mm / minute, such as about 1.0 mm / minute. In some embodiments, the outwardly flared seed-cone 16 has a length between about 100 mm and about 400 mm, such as between about 150 mm and about 250 mm. The length of the outwardly flared seed-cone 16 may vary outside of these ranges. In some embodiments, the outwardly flared seed-cone 16 is grown to a terminal diameter of about 150 mm, at least about 150 mm, about 200 mm, at least about 200 mm, about 300 mm, at least about 300 mm, about 450 mm, or even at least about 450 mm. The terminal diameter of the flared seed-cone 16 is generally equivalent to the diameter of the constant diameter of the main body of the single crystal silicon ingot. In some embodiments, the flared seed-cone adjacent the neck portion formed during the growth of the n-type single crystal silicon ingot has a resistivity between 5 milliohm-cm and about 12 milliohm-cm (e.g., between 5 milliohm-cm and about 8 milliohm-cm). Suitable concentrations of n-type dopants, particularly arsenic, incorporated into the flared seed-cone to achieve these resistivities may be between about 3.5 x 10 18 atoms / cm 3 With about 1.3x10 19 atoms / cm 3 (For example, at about 4x10 18 atoms / cm 3 With 1x10 19 atoms / cm 3 )between.

[0024] In some embodiments, the concentration of n-type dopants in the neck portion and the flared seed-cone and body exceeds the concentration of p-type dopants (e.g., boron, aluminum, or gallium) in the neck portion and the flared seed-cone. The n-type dopant is the predominant dopant in order to achieve the desired resistivity in the neck and the flared seed-cone and vacancies as the dominant intrinsic point defects. Preferably, the concentration of n-type dopants greatly exceeds the concentration of p-type dopants. The p-type dopant concentration (whether intentionally added to the silicon melt and growing crystal or as a contaminant) is preferably less than about 1×10 16 atoms / cm 3 , preferably less than 1x10 15 atoms / cm 3 , and even more preferably less than 1x10 14 atoms / cm 3 .

[0025] After forming the neck 24 and the outwardly flared seed-cone 16 adjacent the neck portion 24, then the ingot body 20 having a constant diameter adjacent the conical portion 16 is grown. The constant diameter portion of the body 20 has a circumferential edge 50, a central axis X parallel to the circumferential edge, and a radius R extending from the central axis to the circumferential edge. The central axis X also passes through the conical portion 16 and the neck 24. The diameter of the ingot body 20 can vary and in some embodiments, the diameter can be about 150 mm, about 200 mm, about 300 mm, greater than about 300 mm, about 450 mm, or even greater than about 450 mm. In some embodiments, the body of the single crystal silicon ingot is ultimately grown to be at least about 1000 mm long, such as at least 1100 mm long, such as at least 1200 mm long, such as at least 1400 mm long, such as at least 1500 mm long, such as at least 1700 mm long or at least 1900 mm long, or at least 2000 mm long, or at least 2200 mm long, or at least about 3000 mm long or at least about 4000 mm long.

[0026] According to the methods of the present invention, the resistivity of the body of the single crystal silicon ingot can be lower than the resistivity of the neck portion and / or the outward flaring seed-cone adjacent to the neck portion. This can be achieved by adding additional n-type dopants (e.g., arsenic) to the silicon melt after the outward flaring seed-cone adjacent to the neck portion is formed. In some embodiments, the body of the single crystal silicon ingot is an n-type ingot doped, for example, with arsenic, having a resistivity of less than 4 milliohm-cm, such as less than 2 milliohm-cm, less than 1.7 milliohm-cm, or even less than about 1.6 milliohm-cm. At these resistivities, the body of the ingot can shift from vacancy-dominated material (such as in the neck and outward flaring seed-cone) to interstitials as the dominant intrinsic point defects. However, once dislocations are removed in the neck and crown, the bulk phase does not need to be rich in vacancies to maintain the dislocation-free characteristics of the growing single crystal silicon ingot.

[0027] In addition, according to the process of the present invention, a magnetic field can be applied to the crucible including the silicon melt. A sharp magnetic field or a horizontal magnetic field can be applied to set a suitable crystal / melt interface, that is, the shape and height of the meniscus. The magnetic field is mainly used to fix the desired crystal / melt interface shape and height, and the control of the oxygen content Qi is a secondary purpose.

[0028] Control of melt flow and the shape of the melt / solid interface and thus the quality of the ingot can be enhanced by applying a magnetic field to the silicon melt during the growth of the main body of the single crystal silicon ingot. In some embodiments, the magnetic field is applied to maintain a substantially constant melt / solid interface profile during at least about 70% of the growth of the main body of the single crystal silicon ingot or between about 70% and about 90% of the growth of the main body of the single crystal silicon ingot. The magnetic field applies an electromagnetic force that affects the flow of the silicon melt and thus the heat transfer in the melt. It changes the profile of the crystal / melt interface and the temperature of the growing crystal, which are key control parameters for perfect silicon.

[0029] The magnetic field affects the oxygen content and uniformity in the ingot. The oxygen source in the ingot comes from the dissolution of the quartz crucible wall, SiO x (g) Evaporation at the melt-free surface (controlled by melt flow dynamics) and incorporation into the growing crystal front. The magnetic field affects the convective melt flow during growth, which can affect oxygen evaporation and incorporation. The variation of oxygen incorporation into the single crystal silicon ingot with time increments is controlled by diffusion and convection of oxygen in the melt according to the following equation:

[0030]

[0031] C is the oxygen concentration in the solidified silicon, t is the time, v is the convection velocity (melt flow velocity) rho, ρ is the density of the silicon melt, The applied magnetic field affects the melt velocity (v) and the gradient of oxygen concentration in the melt. Since the magnetic field induces a steady-state melt flow, the incorporation of oxygen Oi into the ingot is time-constant, which enhances the radial and axial oxygen concentration uniformity. The SOURCE term is derived from the following two parameters: the dissolution of the quartz (SiO2) crucible, which is the generation of oxygen (Si(l) + SiO2(s) → SiO x (g)); and evaporation, which is oxygen (SiO x (g)) is removed (disappeared) from the melt. In a batch Cz process, this SOURCE term is non-constant. Instead, it depends on the crystal length, because the melt mass decreases as the crystal grows. When the ingot has grown a substantial portion of its body length, the remaining melt volume is low, so that the amount of silicon melt in contact with the crucible is reduced, which therefore leads to a lower concentration of oxygen incorporated into the melt from the crucible. Therefore, if the other terms (diffusion, convection, evaporation) are constant, the oxygen incorporated into the solidified silicon crystal is reduced. The area without melt surface (contact surface between melt and gas) affects the SiO x (g) evaporation rate. Figure 1 The crucible shape shown in the figure shows that small melt masses in batch Cz processes have relatively small surface areas. SiOx Less evaporation of (g) means more oxygen is incorporated into the solidifying silicon crystal. According to the method of the present invention, the melt quality is maintained constant because polysilicon is added as the crystal ingot grows. Therefore, all source terms (the generation of oxygen dissolved into the melt by the SiO2 crucible and the SiO2 x (g) gas permeation without evaporation of the melt surface) is constant. Therefore, diffusion and convection terms affect the oxygen of the solidified silicon crystal. The melt flow is made more stable by applying a magnetic field (that is, the melt flow is constant, as if it is a stable condition regardless of time), so during the growth of the entire length of the ingot, the incorporation of oxygen is uniform and stable in the axial and radial directions. In some embodiments, interstitial oxygen can be incorporated into the ingot at a concentration between about 4PPMA and about 18PPMA. In some embodiments, interstitial oxygen can be incorporated into the ingot at a concentration between about 10PPMA and about 35PPMA. In some embodiments, the ingot includes oxygen at a concentration of not more than about 15PPMA or not more than about 10PPMA. Interstitial oxygen can be measured according to SEMI MF 1188-1105.

[0032] In some embodiments, during the growth of the main body of the single crystal silicon ingot, a horizontal magnetic field is applied to the silicon melt. Crystal growth is achieved in the presence of a horizontal magnetic field by placing a crucible holding the silicon melt between the poles of a conventional electromagnet. In some embodiments, the horizontal magnetic field may have a magnetic flux density between about 0.2 Tesla and about 0.4 Tesla in the melt region. The magnetic field variation in the melt is less than + / - about 0.03 Tesla in a given intensity. The application of the horizontal magnetic field causes a Lorentz force opposite to the force driving the melt convection in the axial direction, in the direction opposite to the fluid motion. Therefore, convection in the melt is suppressed, and the axial temperature gradient in the crystal near the interface increases. The melt-crystal interface then moves upward to the crystal side to accommodate the increased axial temperature gradient in the crystal near the interface and the contribution of the melt convection from the crucible is reduced.

[0033] In some embodiments, a cusp magnetic field is applied to the silicon melt during the growth of the main body of the single crystal silicon ingot. The cusp magnetic field has two control parameters, namely, the magnetic flux density and the magnetic field shape. The cusp magnetic field combines with a vertical (axial) magnetic field deeper in the melt near the axis of the ingot to apply a horizontal (radial) magnetic field component at the closest surface of the melt. The cusp magnetic field is generated using a pair of Helmholtz coils carrying current in opposite directions. Therefore, at a position midway between the two magnetic fields, vertically along the ingot axis, the magnetic fields cancel each other out so that the vertical magnetic field component is equal to or close to zero. For example, in the axial direction, the cusp magnetic flux density is typically about zero to about 0.2 Tesla. The magnetic flux density in the radial direction is typically higher than the magnetic flux density in the vertical direction. For example, in radial positions, depending on the radial position, the cusp magnetic flux density is typically between about 0 T and about 0.6 T, such as between about 0.2 T and about 0.5 T. The radial cusp magnetic field constrains the flow of the melt to thereby stabilize the melt. In other words, the application of a radial cusp magnetic field induces convection at a portion of the solid-liquid interface adjacent to where crystal growth occurs, and suppresses convection at the remainder of the melt to thereby serve as an effective method for achieving uniform oxygen distribution. Hot melt convection can be controlled locally and independently at the melt-free surface and at the melt-crucible interface by the cusp magnetic field at the same time. This implementation controls the oxygen concentration in the growing crystal only by the magnetic flux density regardless of the crystal rotation speed. In the presence of an axial or radial magnetic field, control of the oxygen concentration is achieved via control of the crystal rotation speed. The application of a cusp magnetic field can achieve growth on an ingot that includes less oxygen content (e.g., not more than about 15 PPMA or not more than about 10 PPMA) than an ingot grown without an applied magnetic field. Interstitial oxygen can be measured according to SEMI MF1188-1105.

[0034] After the first single crystal silicon ingot is completed, the crystal puller may undergo a stabilization period to allow the chuck and seed to be sufficiently preheated prior to the growth of the second neck. Thus, in some embodiments, the growth of the first single crystal silicon ingot is completed, followed by replenishing the silicon melt by adding silicon and n-type dopants. Next, the second neck is contacted with the replenished silicon melt; and a second silicon seed is withdrawn to form a second neck portion of a second single crystal silicon ingot. In some embodiments, the second neck portion has a resistivity between 5 milliohm-cm and about 12 milliohm-cm, such as between 5 milliohm-cm and about 8 milliohm-cm. Additionally, a second outwardly flared seed-cone is grown, the seed-cone having a resistivity between 5 milliohm-cm and about 12 milliohm-cm, such as between 5 milliohm-cm and about 8 milliohm-cm. Thereafter, additional n-type dopants are added to the melt to achieve a lower resistivity of the body of the second crystal. Thus, the bulk of the second single crystal silicon ingot has a resistivity of less than 4 milliohm-cm, such as less than 2 milliohm-cm, less than 1.7 milliohm-cm, or even less than about 1.6 milliohm-cm.

[0035] The process can be repeated multiple times to grow additional ingots having these resistivity properties.

[0036] According to the method of the present invention, n-type dopants are added in a concentration sufficient to achieve a resistivity between 5 milliohm-cm and about 12 milliohm-cm (e.g., between 5 milliohm-cm and about 8 milliohm-cm) in the neck portion and the outwardly flared seed-cone adjacent to the neck portion to promote a very high vacancy concentration in the grown single crystal silicon ingot. In some embodiments, the vacancies are the dominant intrinsic point defects in the neck portion. In some embodiments, the vacancies are the dominant intrinsic point defects in the outwardly flared seed-cone adjacent to the neck portion. In some embodiments, the vacancies are the dominant intrinsic point defects in the neck portion and in the outwardly flared seed-cone adjacent to the neck portion. Vacancies as dominant intrinsic point defects facilitate the elimination of existing dislocations by climbing toward the crystal surface even when high pull rates are not used. In lightly doped materials, a combination of high pull rates and small diameter necks are typically used. A thin neck helps minimize thermal stresses and the distance that existing dislocations travel to the crystal surface where the dislocations disappear. High pull rates help to incorporate many vacancies and favor dislocation movement towards the crystal surface. However, in the case of heavily doped crystals, this approach is useless for two reasons. First, the vacancy concentration becomes a function of the dopant concentration and does not significantly depend on the pull rate (or more precisely, on the V / G ratio between the pull rate and the axial thermal gradient). Second, in the case of heavily doped melts, high pull rates favor the onset of constitutional supercooling problems, and therefore, for heavily doped melts, the pull rate cannot be selected in a wide range of values ​​as for lightly doped melts. The present solution allows the selection of a pull rate value that is optimized to avoid constitutional supercooling conditions during the neck while controlling the vacancy concentration through the dopant concentration. In this way, the two problems are decoupled.

[0037] The method of the present invention achieves the formation of a single crystal silicon ingot having reduced or eliminated dislocations. In some embodiments, a strip of the body of the single crystal silicon ingot includes less than about 400 dislocations / cm 2 , for example less than about 100 dislocations / cm 2 , or less than about 10 dislocations / cm 2 , or even less than 1 dislocation / cm 2 In some embodiments, a strip of the bulk of the single crystal ingot is a zero dislocation wafer. Dislocations may be determined by means conventional in the art, such as by removing the strip from the ingot and performing a preferential etch to delimit the dislocations.

[0038] Examples

[0039] The process of the present disclosure is further illustrated by the following examples. These examples should not be considered in a limiting sense.

[0040] A plurality of single crystal silicon ingots were grown. The ingots were n-type and doped with arsenic. The crystals were grown to have a neck diameter of 5.5 mm and a neck length of 40 mm. The crystal rotation rate was 11 rpm and the crucible rotation rate was 8 rpm. The melt mass was 60 kg. The resistivity of the neck portion and the crown was varied to values ​​below and above 5 milliohm-cm. The dislocations in the body portion were then measured. Figure 2 As can be clearly seen, all attempts using resistivity less than 4.5 mΩ·cm resulted in zero dislocation loss (LZD) in the crown and dislocations in the bulk of the ingot, while attempts using resistivity greater than 5.5 mΩ·cm successfully achieved zero dislocation growth in the crown and bulk of the single crystal silicon ingot.

[0041] As used herein, the terms "about," "substantially," "substantially," and "approximately" when used in conjunction with ranges of size, concentration, temperature, or other physical or chemical properties or characteristics, are meant to encompass variations that may exist in the upper and / or lower limits of the range of the property or characteristic, including, for example, those resulting from rounding off, variations in the method of measurement, or other statistical variations.

[0042] When introducing elements of the present disclosure or (several) embodiments of the present disclosure, the articles "a," "an," and "the" are intended to mean that there are one or more elements. The terms "comprising," "including," "containing," and "having" are intended to be inclusive and mean that additional elements may be present in addition to the listed elements. The use of terms indicating a particular orientation (e.g., "top," "bottom," "side," etc.) is for convenience of description and does not require any particular orientation of the items being described.

[0043] As various changes could be made in the above constructions and methods without departing from the scope of the disclosure, it is intended that all matter contained in the above description and shown in the accompanying drawing(s) shall be interpreted as illustrative and not in a limiting sense.

Claims

1. A method for preparing a single crystal silicon ingot by a Czochralski method, the method comprising: contacting a silicon seed crystal with a silicon melt, wherein the silicon melt is contained in a crucible and includes molten silicon and an n-type dopant; extracting the silicon seed crystal from the silicon melt to form a neck portion of the single crystal silicon ingot, the neck portion having a resistivity between 5 milliohm-cm and 12 milliohm-cm; growing an outwardly flared seed-cone adjacent the neck portion of the single crystal silicon ingot, the outwardly flared seed-cone having a resistivity between 5 milliohm-cm and 12 milliohm-cm; adding an n-type dopant to the melt at a concentration sufficient to reduce the resistivity of a bulk of the single crystal silicon ingot to a resistivity of less than 4 milliohm-cm; and A main body of the single crystal silicon ingot is grown adjacent to the outwardly flared seed-cone, the main body of the single crystal silicon ingot having a resistivity of less than 4 milliohm-cm.

2. The method according to claim 1, further comprising: Completing the growth of the single crystal silicon ingot; adding silicon and an n-type dopant to the crucible to form a replenished silicon melt; contacting a second silicon seed crystal with the compensated silicon melt comprising molten silicon and added n-type dopants; and The second silicon seed crystal is extracted from the silicon melt to form a second neck portion of a second single crystal silicon ingot, the second neck portion having a resistivity between 5 milliohm-cm and 12 milliohm-cm.

3. The method of claim 1, wherein the silicon seed crystal is withdrawn at a pull rate between 1.5 mm / min and 6 mm / min.

4. The method of claim 1, wherein the silicon seed crystal is withdrawn at a pull rate between 3 mm / min and 5 mm / min.

5. The method of any one of claims 1 to 3, wherein the silicon seed crystal is rotated at a rate between 8 rpm and 15 rpm.

6. The method of any one of claims 1 to 3, wherein the crucible is rotated at a rate between 5 rpm and 10 rpm.

7. The method of any one of claims 1 to 4, wherein the neck portion has a diameter between 2.5 mm and 6.5 mm.

8. The method of any one of claims 1 to 4, wherein the neck portion has a diameter between 3 mm and 6 mm.

9. The method of any one of claims 1 to 4, wherein the single crystal silicon ingot is an n-type ingot.

10. The method of claim 9, wherein a concentration of the n-type dopant in the neck portion and the flared seed-cone exceeds a concentration of the p-type dopant in the neck portion and the flared seed-cone.

11. The method according to claim 9, wherein the concentration of the n-type dopant in the neck portion is between 3.5×10 18 atoms / cm 3 With 1.3x10 19 atoms / cm 3 between.

12. The method according to claim 11, wherein the concentration of the n-type dopant in the neck portion is between 4×10 18 atoms / cm 3 With 1x10 19 atoms / cm 3 between.

13. The method of claim 9, wherein the concentration of the n-type dopant in the flared seed-cone is between 3.5 x 10 18 atoms / cm 3 With 1.3x10 19 atoms / cm 3 between.

14. The method of claim 13, wherein the concentration of the n-type dopant in the flared seed-cone is between 4×10 18 atoms / cm 3 With 1x10 19 atoms / cm 3 between.

15. The method of claim 9, wherein the neck portion has a resistivity between 5 milliohm-cm and 8 milliohm-cm.

16. The method of claim 9, wherein the flared seed-cone has a resistivity between 5 and 8 milliohm-cm.

17. The method of any one of claims 1-4, wherein the body of the single crystal silicon ingot has a resistivity of less than 2 milliohm-cm.

18. The method of any one of claims 1-4, wherein the body of the single crystal silicon ingot has a resistivity of less than 1.7 milliohm-cm.

19. The method of any one of claims 1-4, wherein the body of the single crystal silicon ingot has a resistivity of less than 1.6 milliohm-cm.

20. The method of any one of claims 1-4, wherein the n-type dopant is selected from the group consisting of arsenic, phosphorus, antimony, and any combination thereof.

21. The method of any one of claims 1-4, wherein the n-type dopant is arsenic.

22. The method of any one of claims 1-4, wherein the concentration of n-type dopant added to the silicon melt is between 200 grams of n-type dopant per 60 kilograms of silicon and 400 grams of n-type dopant per 60 kilograms of silicon.

23. The method of any one of claims 1-4, wherein the concentration of n-type dopant added to the silicon melt is about 300 grams of n-type dopant per 60 kilograms of silicon.

24. The method of any one of claims 1-4, wherein the neck portion of the single crystal silicon ingot includes vacancies as dominant interstitial point defects.

25. The method of any one of claims 1-4, wherein the outwardly flaring seed-cone of the single crystal silicon ingot comprises vacancies as dominant interstitial point defects.

26. The method of any one of claims 1 to 4, wherein a strip of the body of the single crystal silicon ingot comprises less than 400 dislocations / cm 2 .

27. The method of any one of claims 1 to 4, wherein a stripe of the body of the single crystal silicon ingot comprises less than 100 dislocations / cm 2 .

28. The method of any one of claims 1 to 4, wherein a stripe of the body of the single crystal silicon ingot comprises less than 10 dislocations / cm 2 .

29. The method of any one of claims 1 to 4, wherein a stripe of the body of the single crystal silicon ingot comprises less than 1 dislocation / cm 2 .

30. The method of any one of claims 1-4, wherein strips of the body of the single crystal silicon ingot are zero dislocation wafers.

31. A single crystal silicon ingot, comprising: a neck portion of the single crystal silicon ingot, the neck portion having a resistivity between 5 milliohm-cm and 12 milliohm-cm; an outwardly flared seed-cone adjacent the neck portion of the single crystal silicon ingot, the outwardly flared seed-cone having a resistivity between 5 milliohm-cm and 12 milliohm-cm; and A main body of the single crystal silicon ingot, adjacent to the outwardly flared seed-cone, the main body of the single crystal silicon ingot having a resistivity of less than 4 milliohm-cm.

32. The single crystal silicon ingot of claim 31, wherein the stripes of the body of the single crystal silicon ingot comprise less than 400 dislocations / cm 2 .

33. The single crystal silicon ingot of claim 31, wherein the stripes of the body of the single crystal silicon ingot comprise less than 100 dislocations / cm 2 .

34. The single crystal silicon ingot of claim 31, wherein the stripes of the body of the single crystal silicon ingot include less than 10 dislocations / cm 2 .

35. The single crystal silicon ingot of claim 31, wherein a strip of the body of the single crystal silicon ingot comprises less than 1 dislocation / cm 2 .

36. The single crystal silicon ingot of claim 31, wherein the strips of the body of the single crystal silicon ingot are zero dislocation wafers.