Composition for forming protective film having acetal structure and amide structure
By using a protective film composition containing a compound of acetal and amide structure in semiconductor manufacturing, the problem of insufficient resistance of the wet etching liquid is solved, and higher resistance to the resist solvent and stability to the wet etching liquid are achieved.
Patent Information
- Application Number
- CN202080009988.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-01-21
- Filing Date
- 2020-01-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-01-20
Smart Images

Figure BDA0003170531810000021 
Figure BDA0003170531810000031 
Figure BDA0003170531810000041
Abstract
Description
Technical Field
[0001] The present invention relates to a composition for forming a protective film having excellent resistance to a semiconductor wet etching solution, preferably an acidic or alkaline hydrogen peroxide aqueous solution, in a photolithography process in semiconductor manufacturing, and also relates to a method for forming a resist pattern using the protective film and a method for manufacturing a semiconductor device. Background Art
[0002] In semiconductor manufacturing, a photolithography process is well known in which a resist underlayer film is provided between a substrate and a resist film formed thereon to form a resist pattern of a desired shape.
[0003] Patent Document 1 discloses an antireflective coating composition for use with an overcoated photoresist, which contains a polymer having a glycidyl group and a polymer having an aromatic group substituted with a hydroxyl group or the like, and a method for forming a photoresist underlayer film therefrom and performing exposure, development, and patterning.
[0004] Patent Document 2 discloses a method of forming a photoresist relief image by coating a composition containing a resin having an epoxy reactive group such as a hydroxyl group and a crosslinking resin containing an epoxy group on a substrate and forming a photoresist layer thereon.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2017-107185
[0008] Patent Document 2: Japanese Patent Application Publication No. 2017-187764 Summary of the invention
[0009] Problems to be solved by the invention
[0010] When a base substrate is processed by wet etching using the resist underlayer film as an etching mask, the resist underlayer film is required to have a good masking function against a wet etching solution during processing of the base substrate.
[0011] Conventionally, a method of using gallic acid as an additive has been used to develop resistance to SC-1 (ammonia-hydrogen peroxide solution), which is a type of wet etching solution.
[0012] Furthermore, it is known that a catechol structure shows an effect of improving resistance to semiconductor wet etching solutions (Patent Document 1), but resistance to semiconductor wet etching solutions is still not sufficiently satisfactory.
[0013] An object of the present invention is to solve such problems.
[0014] Methods for solving problems
[0015] The present invention includes the following aspects. [1]
[0017] A composition for forming a protective film for a semiconductor wet etching solution, comprising: a compound or polymer comprising at least one acetal structure and at least one amide structure, and a solvent. [2]
[0019] The protective film-forming composition according to [1], wherein the polymer is a copolymer of a compound (a) containing at least one acetal structure in a molecule and a compound (b) containing at least one amide structure in a molecule. [3]
[0021] The protective film-forming composition according to [1] or [2], wherein the acetal structure is a structure in which adjacent hydroxyl groups of an aromatic group are protected. [4]
[0023] The protective film-forming composition according to any one of [1] to [3], wherein the acetal structure or compound (a) includes a structure represented by formula (1).
[0024]
[0025] (In formula (1),
[0026] R 1 and R 2 are the same or different and are a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted with a monovalent organic group (A), or an aryl group having 6 to 40 carbon atoms which may be substituted with a monovalent organic group (A),
[0027] n1 is 0, 1, or 2,
[0028] n2 is 1 or 2,
[0029] A 1 represents a hydrogen atom or a hydroxyl group,
[0030] A 2 Represents -CH(R 0 )-A 4 base,
[0031] R 0 represents a hydrogen atom, a phenyl group which may be substituted with 1 to 3 hydroxyl groups, or a benzodioxolyl group,
[0032] A 3 and A 4 Each represents the same or different monovalent organic group (A-1). [5]
[0034] The protective film-forming composition according to [1] or [2], wherein the amide structure or compound (b) includes a structure represented by -CO-NH- or -CO-N=. [6]
[0036] The protective film-forming composition according to [2], wherein the compound (b) is represented by formula (2).
[0037]
[0038] (In formula (2), R 20 represents a hydrogen atom or a methyl group, R 21 and R 22 Each is the same or different and is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted by a monovalent organic group (B) and may be interrupted by an oxygen atom or a quaternary ammonium cation, or an aryl group having 6 to 40 carbon atoms which may be substituted by a monovalent organic group (B) and may be interrupted by an oxygen atom or a quaternary ammonium cation). [7]
[0040] The protective film forming composition according to [6], wherein the monovalent organic group (B) is selected from a hydroxyl group, a cyano group, a sulfo group, a carboxylate group, a boron atom which may be substituted with one or two hydroxyl groups, an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom, and -NR a1 R b1 Base (R a1 and R b1 are the same or different and represent a hydrogen atom or an alkyl group having 1 to 3 carbon atoms). [8]
[0042] The protective film-forming composition according to [2], wherein the compound (b) is represented by formula (2-1).
[0043]
[0044] (In formula (2-1), R 20 represents a hydrogen atom or a methyl group, R 23 represents an alkylene group having 1 to 5 carbon atoms, R 24 Indicates blocked isocyanate groups. ) [9]
[0046] The protective film-forming composition according to any one of [1] to [8], further comprising a crosslinking catalyst.
[10]
[0048] The protective film-forming composition according to any one of [1] to [9], further comprising a crosslinking agent.
[11]
[0050] The protective film-forming composition according to any one of [1] to
[10] , further comprising a surfactant.
[12]
[0052] A protective film characterized by being a fired product of a coating film formed from the protective film-forming composition according to any one of [1] to
[11] .
[13]
[0054] A method for producing a substrate with a resist pattern, characterized in that it comprises the steps of applying the protective film composition described in any one of [1] to
[11] on a semiconductor substrate and firing the composition to form a protective film as a resist underlayer film, and is used for the production of the above-mentioned semiconductor.
[14]
[0056] A method for manufacturing a semiconductor device, comprising the following steps: forming a protective film on a semiconductor substrate on which an inorganic film can be formed using a protective film forming composition for a semiconductor wet etching solution as described in any one of [1] to
[11] , forming a resist pattern on the protective film, dry-etching the protective film using the resist pattern as a mask to expose the surface of the inorganic film or the semiconductor substrate, and wet-etching and washing the inorganic film or the semiconductor substrate using a semiconductor wet etching solution using the dry-etched protective film as a mask.
[0057] Effects of the Invention
[0058] In the present invention, the protective film-forming composition contains a compound or polymer having at least one acetal structure and at least one amide structure, so that high resistance to a semiconductor wet etching solution can be exhibited. DETAILED DESCRIPTION
[0059] [Protective film forming composition]
[0060] The protective film forming composition for semiconductor wet etching liquid according to the present invention is a protective film forming composition for semiconductor wet etching liquid containing a compound or polymer having at least one acetal structure and at least one amide structure, and a solvent.
[0061] Among the compounds or polymers containing at least one acetal structure and at least one amide structure, a polymer containing at least one acetal structure and at least one amide structure is preferred.
[0062] The compound including at least one acetal structure and at least one amide structure includes at least one acetal structure and at least one amide structure in one molecule.
[0063] The above compound is preferably represented by the following formula (a1).
[0064]
[0065] (In formula (a1), R 20 represents a hydrogen atom or a methyl group, R 1 and R 2 Each is the same or different and is a hydrogen atom, or an alkyl group having 1 to 10 carbon atoms which may be substituted by a monovalent organic group (A), or an aryl group having 6 to 40 carbon atoms which may be substituted by a monovalent organic group (A), n1 is 0, 1 or 2, and n2 is 1 or 2. ) As a specific example of the compound, it is represented by the following structural formula.
[0066]
[0067] The polymer including at least one acetal structure and at least one amide structure may include one or more acetal structures and one or more amide structures in a repeating unit of the polymer.
[0068] The repeating unit of the polymer is preferably represented by the following structural formula (a2).
[0069]
[0070] (In formula (a2), R 20 , R 1 , R 2 , n1 and n2 are the same as those described in the above formula (a1).
[0071] Specific examples of the repeating unit of the polymer are represented by the following structural formula.
[0072]
[0073] The polymer is preferably a copolymer comprising repeating units having an acetal structure and repeating units having an amide structure. The polymer is preferably a copolymer comprising a compound (a) having at least one acetal structure in the molecule and a compound (b) having at least one amide structure in the molecule. The following is described in order.
[0074] [Compound (a) containing at least one acetal structure in the molecule]
[0075] The acetal structure is preferably a structure in which adjacent hydroxyl groups of an aromatic group are protected. In this case, the compound contains at least one aromatic group in which adjacent hydroxyl groups are protected by acetal in the molecule.
[0076] Such an acetal structure preferably includes a structure represented by formula (1).
[0077]
[0078] (In formula (1),
[0079] R 1 and R 2 are the same or different and are a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted with a monovalent organic group (A), or an aryl group having 6 to 40 carbon atoms which may be substituted with a monovalent organic group (A),
[0080] n1 is 0, 1, or 2,
[0081] n2 is 1 or 2,
[0082] A 1 represents a hydrogen atom or a hydroxyl group,
[0083] A 2 Represents -CH(R 0 )-A 4 base,
[0084] R 0 represents a hydrogen atom, a phenyl group which may be substituted with 1 to 3 hydroxyl groups, or a benzodioxolyl group,
[0085] A 3 and A 4 Each represents the same or different monovalent organic group (A-1).
[0086] Examples of the alkyl group having 1 to 10 carbon atoms which may be substituted with the monovalent organic group (A) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, a cyclopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a cyclobutyl group, a 1-methyl-cyclopropyl group, a 2-methyl-cyclopropyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, a cyclopentyl group, a 1-methyl- Cyclobutyl, 2-methyl-cyclobutyl, 3-methyl-cyclobutyl, 1,2-dimethyl-cyclopropyl, 2,3-dimethyl-cyclopropyl, 1-ethyl-cyclopropyl, 2-ethyl-cyclopropyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl Butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, cyclohexyl, 1-methyl-cyclopentyl, 2-methyl-cyclopentyl, 3-methyl-cyclopentyl, 1-ethyl-cyclobutyl, 2-ethyl-cyclobutyl, 3-ethyl-cyclobutyl, 1,2-dimethyl-cyclobutyl, 1,3-dimethyl-cyclobutyl, 2,2-dimethyl-cyclobutyl, 2, 3-dimethyl-cyclobutyl, 2,4-dimethyl-cyclobutyl, 3,3-dimethyl-cyclobutyl, 1-n-propyl-cyclopropyl, 2-n-propyl-cyclopropyl, 1-isopropyl-cyclopropyl, 2-isopropyl-cyclopropyl, 1,2,2-trimethyl-cyclopropyl, 1,2,3-trimethyl-cyclopropyl, 2,2,3-trimethyl-cyclopropyl, 1-ethyl-2-methyl-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl and 2-ethyl-3-methyl-cyclopropyl, etc.
[0087] Examples of the aryl group having 6 to 40 carbon atoms which may be substituted with the monovalent organic group (A) include phenyl, o-methylphenyl, m-methylphenyl, p-methylphenyl, o-chlorophenyl, m-chlorophenyl, p-chlorophenyl, o-fluorophenyl, p-fluorophenyl, o-methoxyphenyl, p-methoxyphenyl, p-nitrophenyl, p-cyanophenyl, α-naphthyl, β-naphthyl, o-biphenyl, m-biphenyl, p-biphenyl, 1-anthryl, 2-anthryl, 9-anthryl, 1-phenanthryl, 2-phenanthryl, 3-phenanthryl, 4-phenanthryl and 9-phenanthryl.
[0088] Examples of the monovalent organic group (A) as a substituent of the alkyl group and the aryl group include, but are not limited to, a halogen atom (fluorine, chlorine, bromine, iodine), a nitro group, a cyano group, an amino group, a hydroxyl group, a carbonyl group, and a carbonyloxy group.
[0089] In formula (1), preferably n1 is 0 and n2 is 1.
[0090] In formula (1), preferably R 1 and R 2 are the same or different and are hydrogen atoms or methyl groups. 1 and R 2 All are hydrogen atoms.
[0091] [Monovalent organic group (A-1)]
[0092] The monovalent organic group (A-1) is not particularly limited. It may be a group derived from various polymers or oligomers, or a group derived from a low molecular weight compound. The monovalent organic group may be a group derived from a compound represented by formula (1). 4 In the case of representing a compound represented by formula (1), it means that the same or different compounds represented by formula (1) are separated by -CH(R 0 )- groups connected to form an oligomer or polymer.
[0093] [Monovalent organic group derived from polymer (A-1)]
[0094] By using an organic group derived from a polymer, the dry etching rate (the amount of film thickness reduction per unit time), the extinction coefficient, the refractive index, etc. of the resist underlayer film formed from the protective film-forming composition of the present invention can be adjusted.
[0095] As the polymer, there is no particular limitation, and various organic polymers can be used. For example, addition polymers and condensation polymers of polyester, polystyrene, polyimide, acrylic polymer, methacrylic polymer, polyvinyl ether, phenol novolac, naphthol novolac, polyether, polyamide, polycarbonate, etc., and ring-opening polymerization polymers can be used, but acrylic polymers or methacrylic polymers are preferred.
[0096] Examples of such organic polymers include addition polymers containing addition polymerizable monomers such as benzyl acrylate, benzyl methacrylate, phenyl acrylate, naphthyl acrylate, anthracene methacrylate, anthracene methyl methacrylate, styrene, hydroxystyrene, benzyl vinyl ether and N-phenylmaleimide as structural units; and condensation polymers such as phenol novolac and naphthol novolac.
[0097] When an addition polymer is used as the organic polymer, the polymer may be a homopolymer or a copolymer. Addition polymers are produced using addition polymerizable monomers. Examples of such addition polymerizable monomers include acrylic acid, methacrylic acid, acrylate compounds, methacrylate compounds, acrylamide compounds, methacrylamide compounds, vinyl compounds, styrene compounds, maleimide compounds, maleic anhydride, and acrylonitrile.
[0098] Examples of the acrylate compound include methyl acrylate, ethyl acrylate, n-hexyl acrylate, isopropyl acrylate, cyclohexyl acrylate, benzyl acrylate, phenyl acrylate, anthracenemethyl acrylate, 2-hydroxyethyl acrylate, 3-chloro-2-hydroxypropyl acrylate, 2-hydroxypropyl acrylate, 2,2,2-trifluoroethyl acrylate, 2,2,2-trichloroethyl acrylate, 2-bromoethyl acrylate, 4-hydroxybutyl acrylate, 2-methoxyethyl acrylate, tetrahydrofurfuryl acrylate, 2-methyl-2-adamantyl acrylate, 5-acryloyloxy-6-hydroxynorbornene-2-carboxy-6-lactone, 3-acryloyloxypropyltriethoxysilane, and glycidyl acrylate.
[0099] Examples of the methacrylate compound include methyl methacrylate, ethyl methacrylate, n-hexyl methacrylate, isopropyl methacrylate, cyclohexyl methacrylate, benzyl methacrylate, phenyl methacrylate, anthracene methyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2,2,2-trifluoroethyl methacrylate, 2,2,2-trichloroethyl methacrylate, 2-bromoethyl methacrylate, 4-hydroxybutyl methacrylate, 2-methoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, 2-methyl-2-adamantyl methacrylate, 5-methacryloyloxy-6-hydroxynorbornene-2-carboxy-6-lactone, 3-methacryloyloxypropyltriethoxysilane, glycidyl methacrylate, 2-phenylethyl methacrylate, hydroxyphenyl methacrylate, and bromophenyl methacrylate.
[0100] Examples of the acrylamide compound include acrylamide, N-methylacrylamide, N-ethylacrylamide, N-benzylacrylamide, N-phenylacrylamide, N,N-dimethylacrylamide, and N-anthrylacrylamide.
[0101] Examples of the methacrylamide compound include methacrylamide, N-methyl methacrylamide, N-ethyl methacrylamide, N-benzyl methacrylamide, N-phenyl methacrylamide, N,N-dimethyl methacrylamide, and N-anthryl acrylamide.
[0102] Examples of the vinyl compound include vinyl alcohol, 2-hydroxyethyl vinyl ether, methyl vinyl ether, ethyl vinyl ether, benzyl vinyl ether, vinyl acetic acid, vinyltrimethoxysilane, 2-chloroethyl vinyl ether, 2-methoxyethyl vinyl ether, vinylnaphthalene, and vinylanthracene.
[0103] Examples of the styrene compound include styrene, hydroxystyrene, chlorostyrene, bromostyrene, methoxystyrene, cyanostyrene, and acetylstyrene.
[0104] Examples of the maleimide compound include maleimide, N-methylmaleimide, N-phenylmaleimide, N-cyclohexylmaleimide, N-benzylmaleimide, and N-hydroxyethylmaleimide.
[0105] When a polycondensate is used as the polymer, examples of such a polymer include a polycondensate of a diol compound and a dicarboxylic acid compound.
[0106] Examples of the diol compound include diethylene glycol, 1,6-hexanediol, and butanediol.
[0107] Examples of the dicarboxylic acid compound include aliphatic dicarboxylic acids and aromatic dicarboxylic acids such as succinic acid, 2,2-dimethylsuccinic acid, adipic acid, terephthalic acid, isophthalic acid, phthalic acid, 3,3′-dithiodipropionic acid, tartaric acid, malic acid, and maleic anhydride.
[0108] Other examples include polyesters such as poly(1,2,4,5-pyromellitimide), poly(p-phenylene terephthalamide), polybutylene terephthalate, and polyethylene terephthalate, polyamides, and polyimides.
[0109] When a ring-opening polymer is used as the polymer, examples of such a polymer include condensation products of a diepoxy compound and a dicarboxylic acid compound.
[0110] Examples of the diepoxy compound include sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether, glycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, and compounds such as the compounds shown in the following [3-1] to [3-16].
[0111]
[0112]
[0113] Examples of the dicarboxylic acid compound include the dicarboxylic acid compounds described above.
[0114] It is preferred that the polymer has a structure of formula (10).
[0115]
[0116] (In formula (10), A represents a direct bond or -C(=O)-, and Ar represents a benzene ring, a naphthalene ring, or an anthracene ring which may be substituted with an alkyl group having 1 to 6 carbon atoms, a halogen atom, a hydroxyl group, a carboxyl group, an amino group, an alkoxy group having 1 to 6 carbon atoms, an alkylthio group having 1 to 6 carbon atoms, a cyano group, an acetyl group, an acetoxy group, an alkoxycarbonyl group having 1 to 6 carbon atoms, a nitro group, a nitroso group, an amide group, an imide group, an alkoxysulfonyl group having 1 to 6 carbon atoms, or a sulfonamide group.)
[0117] In addition, examples of the alkyl group in the formula (10) include a methyl group, an ethyl group, a n-butyl group, a tert-butyl group, an isopropyl group, a cyclohexyl group, and the like; examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom; examples of the alkoxy group include a methoxy group, an ethoxy group, a butoxy group, and the like; examples of the alkylthio group include a methylthio group, an ethylthio group, a butylthio group, and the like; examples of the alkoxycarbonyl group include a methoxycarbonyl group, an ethoxycarbonyl group, an isopropoxycarbonyl group, and the like; examples of the alkoxysulfonyl group include a methoxysulfonyl group, an ethoxysulfonyl group, and the like.
[0118] The above copolymer can be produced by the method described in Japanese Patent No. 5041175, for example.
[0119] [Monovalent organic group derived from a low molecular weight compound (A-1)]
[0120] The low molecular weight compound from which the monovalent organic group is derived is not particularly limited, but in consideration of the risk of volatilization during firing, the molecular weight is preferably 300 or more. The upper limit of the molecular weight is, for example, 999. Some preferred specific examples are as follows. * represents a bond.
[0121]
[0122]
[0123] Furthermore, the monovalent organic group may be a group obtained by adding a spacer group to the above-mentioned low molecular weight compound.
[0124] Examples of the spacer group include -CH-, -(CH2) n -(n=1 to 20), -CH=CH-, -CH≡CH-, -N=N-, -NH-, -NHR-, -NHCO-, -NRCO-, -S-, -COO-, -O-, -CO-, -CH=N-, -CH(OH)- and phenylene, or a combination of two or more thereof. Two or more of these spacers may be linked together.
[0125] [Specific examples of preferred compounds having a partial structure represented by formula (1)]
[0126] Preferred examples of compounds having a partial structure represented by formula (1) are as follows.
[0127] Examples of the polymer having a partial structure represented by formula (1) include structural units represented by the following formulae (A-1) to (A-6).
[0128]
[0129] In the polymer having a partial structure represented by formula (1), the molar ratio of the unit structure having the partial structure represented by formula (1) to the whole copolymer is 10 to 85 mol%, or 30 to 70 mol%, or 30 to 45 mol%. The unit structure having the partial structure represented by formula (1) may be one type or two or more types.
[0130] Furthermore, the compound or polymer having the partial structure represented by the above formula (1) can be exemplified by the reaction product (D) obtained by the epoxy compound or resin represented by the following formula (B) and the proton-generating compound having the partial structure represented by the above formula (1) represented by the following formula (C).
[0131] Examples of the epoxy compound (B) include glycidyl ether compounds, glycidyl ester compounds, glycidyl group-containing isocyanurates, epoxycyclohexyl compounds, epoxy-substituted cyclohexyl compounds, and resins thereof. Examples of the epoxy compound (B) used in the present invention are shown below.
[0132]
[0133] Formula (B-1) is available as TEPIC-SS, a product of Nissan Chemical Co., Ltd.
[0134] Formula (B-2) is available as MA-DGIC manufactured by Shikoku Chemical Industry Co., Ltd.
[0135] Formula (B-3) is available as a product of Nagase Chem-Tech Co., Ltd. under the trade name EX-411.
[0136] Formula (B-4) is available as a product of Nagase Chemtech Co., Ltd. under the trade name EX-521.
[0137] Formula (B-7) is available as RE-810NM manufactured by Nippon Kayaku Co., Ltd.
[0138] Formula (B-8) is available as BATG, a product of Showa Denko K.K.
[0139] Formula (B-9) is available as a product of Nagase Chem-Tech Co., Ltd. under the trade name EX-711.
[0140] Formula (B-10) is available as a product of DIC Corporation under the trade name YD-4032D.
[0141] Formula (B-11) is available as HP-4770, a product of DIC Corporation.
[0142] Formula (B-12) is available as Nippon Steel & Sumitomo Metal Chemical Co., Ltd. under the trade name YH-434L.
[0143] Formula (B-13) is available as EPICLON HP-4700, a product of DIC Corporation.
[0144] Formula (B-14) is available as TEP-G, a product of Asahi Organic Materials Industries, Ltd.
[0145] Formula (B-15) is manufactured by Daicel Corporation and is trade name Epilide GT401. a, b, c, and d are each 0 or 1, and a+b+c+d=1.
[0146] Formula (B-16) is available as EHPE-3150, a product of Daicel Corporation.
[0147] Formula (B-17) is available as a product of DIC Corporation under the trade name HP-7200L.
[0148] Formula (B-18) is available as EPPN-201 manufactured by Nippon Kayaku Co., Ltd.
[0149] Formula (B-19) is available as ECN-1229, a product of Asahi Kasei Epochi Corporation.
[0150] Formula (B-20) is available as EPPN-501H manufactured by Nippon Kayaku Co., Ltd.
[0151] Formula (B-21) is available as NC-2000L, manufactured by Nippon Kayaku Co., Ltd.
[0152] Formula (B-22) is available as NC-3000L, manufactured by Nippon Kayaku Co., Ltd.
[0153] Formula (B-23) is available as NC-7000L, manufactured by Nippon Kayaku Co., Ltd.
[0154] Formula (B-24) is available as NC-7300L, manufactured by Nippon Kayaku Co., Ltd.
[0155] Formula (B-25) is available as NC-3500, a product of Nippon Kayaku Co., Ltd.
[0156] Formula (B-26) is available as EPICLON HP-5000, a product of DIC Corporation.
[0157] Formula (B-27) is available as FAE-2500 manufactured by Nippon Kayaku Co., Ltd.
[0158] Formula (B-28) is available as NC-6000, a product of Nippon Kayaku Co., Ltd.
[0159] In addition, examples of the proton-generating compound (C) having a partial structure represented by the above formula (1) are shown below: 5-hydroxy-1,3-benzodioxole (sesamol) or piperic acid is preferred.
[0160]
[0161] Specific examples of the reactant (D) having the partial structure represented by the above formula (1) include the following, but are not limited thereto.
[0162]
[0163] Furthermore, the compound or polymer having the partial structure represented by the above formula (1) can be exemplified by a novolac resin (E) obtained from a compound containing a phenolic hydroxyl group or an aromatic amine and an aldehyde having the partial structure represented by the above formula (1), or from a compound containing a phenolic hydroxyl group having the partial structure represented by the above formula (1) and an aldehyde.
[0164] The aldehyde having the partial structure represented by the above formula (1) is preferably heliotropin (piperonal), and the compound having a phenolic hydroxyl group and having the partial structure represented by the above formula (1) is preferably 5-hydroxy-1,3-benzodioxole (sesamol).
[0165] Specific examples of the reactant (E) having the partial structure represented by the above formula (1) include the following, but are not limited thereto.
[0166]
[0167] [Compound (b) containing at least one amide structure in the molecule]
[0168] The compound containing at least one amide structure in the molecule preferably contains a partial structure represented by -CO-NH- or -CO-N=.
[0169] The above compound (b) is preferably represented by formula (2).
[0170]
[0171] (In formula (2), R 20 represents a hydrogen atom or a methyl group, R 21 and R 22 each being the same or different and being a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted by a monovalent organic group (B) and which may be interrupted by an oxygen atom or a quaternary ammonium cation, or an aryl group having 6 to 40 carbon atoms which may be substituted by a monovalent organic group (B) and which may be interrupted by an oxygen atom or a quaternary ammonium cation)
[0172] The quaternary ammonium cation is preferably substituted with an alkyl group having 1 to 5 carbon atoms.
[0173] Specific examples of the alkyl group having 1 to 10 carbon atoms include the above-mentioned alkyl groups having 1 to 10 carbon atoms.
[0174] Specific examples of the alkyl group having 1 to 5 carbon atoms include groups having 1 to 5 carbon atoms among the above-mentioned alkyl groups having 1 to 10 carbon atoms.
[0175] Specific examples of the aryl group having 6 to 40 carbon atoms include the above-mentioned aryl groups having 6 to 40 carbon atoms.
[0176] The monovalent organic group (B) is preferably selected from a hydroxyl group, a cyano group, a sulfo group, a carboxylate group, a boron atom which may be substituted with one or two hydroxyl groups, an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom, and -NR a1 R b1 Base (R a1 and R b1 are the same or different and represent a hydrogen atom or an alkyl group having 1 to 3 carbon atoms).
[0177] Specific examples of the alkyl group having 1 to 6 carbon atoms include groups having 1 to 6 carbon atoms among the above-mentioned alkyl groups having 1 to 10 carbon atoms.
[0178] Specific examples of the alkyl group having 1 to 3 carbon atoms include groups having 1 to 3 carbon atoms among the above-mentioned alkyl groups having 1 to 10 carbon atoms.
[0179] Specific examples of the compound represented by formula (2) include compounds represented by the following structural formulas, but are not limited thereto.
[0180]
[0181]
[0182] The partial structure of the copolymer derived from the compound represented by formula (2) can be exemplified by the structural unit represented by the following formula.
[0183]
[0184]
[0185]
[0186] The above compound (b) can be represented by formula (2-1).
[0187]
[0188] (In formula (2-1), R 20 represents a hydrogen atom or a methyl group, R 23 represents an alkylene group having 1 to 5 carbon atoms, R 24 Indicates blocked isocyanate groups. )
[0189] The blocked isocyanate group is represented by the following general formula (21).
[0190]
[0191] [In the formula, A represents a residue of an isocyanate-blocking compound selected from alcohols, amines, amides, active methylene compounds, nitrogen-containing heteroaryl compounds, oximes, ketoximes, and hydroxamates.]
[0192] R 25 The term "blocked isocyanate group" refers to a group in which an isocyanate group is blocked by a thermally removable protective group, that is, a group obtained by reacting an isocyanate blocking compound (blocking agent) with an isocyanate group.
[0193] The so-called isocyanate blocking agent generally refers to a substance that reacts with isocyanate groups to prevent reactions with functional groups in other molecules (e.g., acid functional groups, etc.) at room temperature, but dissociates at high temperatures to regenerate the isocyanate groups and enable subsequent reactions (e.g., with acid functional groups).
[0194] Examples of the blocking agent include alcohols such as methanol, ethanol, isopropanol, n-butanol, 2-ethoxyhexanol, 2-N,N-dimethylaminoethanol, 2-ethoxyethanol, and cyclohexanol; phenols such as phenol, o-nitrophenol, p-chlorophenol, o-cresol, m-cresol, and p-cresol; lactams such as ε-caprolactam; oximes such as acetone oxime, methyl ethyl ketone oxime, methyl isobutyl ketone oxime, cyclohexanone oxime, acetophenone oxime, and benzophenone oxime; amines, amides; nitrogen-containing heteroaryl compounds such as pyrazole, 3,5-dimethylpyrazole, and 3-methylpyrazole; thiols such as dodecanethiol and benzenethiol; malonic acid diesters, acetoacetic acid esters, malonic acid dinitrile, acetylacetone, and methylene disulfone. disulfone), dibenzoylmethane, dipivaloylmethane, acetone dicarboxylic acid diester and other active methylene compounds, isohydroxamates, etc.
[0195] It is advantageous for the blocking agent to be volatile, a material which evaporates from the composition after release.
[0196] The blocked isocyanate group is represented by, for example, the following formula.
[0197]
[0198] [In the formula, A represents a residue of an isocyanate-blocking compound selected from alcohols, amines, amides, active methylene compounds, nitrogen-containing heteroaryl compounds, oximes, ketoximes, and hydroxamates.]
[0199] Specific examples of the isocyanate compound represented by the above formula (20) include isocyanate-containing (meth)acrylates such as 2-isocyanateethyl methacrylate and 2-isocyanateethyl acrylate, and compounds obtained by adding blocking agents such as methyl ethyl ketoxime, ε-caprolactam, γ-caprolactam, 3,5-dimethylpyrazole, diethyl malonate, ethanol, isopropanol, n-butanol, and 1-methoxy-2-propanol to these compounds. These compounds may be used alone or in combination of two or more.
[0200] (B) The isocyanate compound can be synthesized by a known method, and the following commercially available products can be used.
[0201] KALENS AOI (2-isocyanateethyl acrylate manufactured by Showa Denko K.K., registered trademark),
[0202] Calenz AOI-BM (2-(0-[1'-methylpropyleneamino]carboxyamino)ethyl acrylate manufactured by Showa Denko K.K., registered trademark)
[0203] KALENS AOI-VM (2-isocyanateethyl acrylate manufactured by Showa Denko K.K., registered trademark),
[0204] KALENS MOI (2-isocyanateethyl methacrylate manufactured by Showa Denko K.K., registered trademark),
[0205] Calence MOI-BM (2-(O-[1'-methylpropyleneamino]carboxyamino)ethyl methacrylate manufactured by Showa Denko K.K., a registered trademark),
[0206] Calenz MOI-BP (2-[(3,5-dimethylpyrazolyl)carbonylamino]ethyl methacrylate manufactured by Showa Denko K.K., a registered trademark),
[0207] Karens MOI-EG (Showa Denko K.K., registered trademark),
[0208] Calends BEI (1,1-(bisacryloyloxymethyl)ethyl isocyanate manufactured by Showa Denko K.K., a registered trademark).
[0209] Among the above, 2-(O-[1′-methylpropyleneamino]carboxyamino)ethyl methacrylate (for example, Calence MOI-BM (manufactured by Showa Denko K.K.)) is preferred.
[0210] Examples of the compound represented by the above formula (2-1) include compounds represented by the following structural formulas, but the compound is not limited thereto.
[0211]
[0212]
[0213] The partial structure of the copolymer derived from the compound represented by the formula (2-1) can be exemplified by the structural unit represented by the following formula.
[0214]
[0215]
[0216] The molar ratio of the compound (b) containing at least one amide structure in the molecule to the whole copolymer is 5 to 80 mol%, preferably 8 to 50 mol%, and preferably 10 to 30 mol%. The unit structure having the partial structure represented by formula (1) may be one or more.
[0217] In the case of a copolymer of a third component comprising a unit structure having a partial structure other than formula (1) and formula (2), its molar ratio is the remainder of the portion occupied by the unit structure having the partial structure shown in formula (1) or formula (2) relative to the whole copolymer, but preferably has a unit structure containing a site that reacts with a crosslinking agent for crosslinking the copolymers. As the site of the above reaction, a hydroxyl group can be cited. The proportion of the unit structure having a site that reacts with the above crosslinking agent in the whole copolymer is 5 to 30 mol%, preferably 8 to 25 mol%, and preferably 10 to 23 mol%. The third component can be one or more.
[0218] As a preferred example of the above copolymer, the unit structure represented by formula (1) accounts for 15 to 85 mol%, the unit structure represented by formula (2) accounts for 5 to 30 mol%, and the unit structure having a site reactive with a crosslinking agent for crosslinking the above copolymer accounts for 10 to 30 mol%. The copolymer of the present application can be obtained by copolymerizing the compound (a) having at least one acetal structure in the molecule, the compound (b) having at least one amide structure in the molecule, and a compound derived from a partial structure other than formula (1) and formula (2) as required by a method known per se.
[0219] As the third component, those having unit structures represented by the following formulae (A-7) to (A-18) are preferred.
[0220]
[0221] As the polymer (copolymer), a polymer having a weight average molecular weight of, for example, 1,000 to 100,000, or 1,500 to 50,000, or 2,000 to 30,000, or 3,000 to 20,000 can be used.
[0222] [Cross-linking catalyst]
[0223] In order to promote the crosslinking reaction, the protective film forming composition of the present invention may contain a crosslinking catalyst as an optional component. As the crosslinking catalyst, in addition to the acidic compound (crosslinking acid catalyst), a compound that generates an acid or a base by heat can be used. As the acidic compound, a sulfonic acid compound or a carboxylic acid compound can be used, and as a compound that generates an acid by heat, a thermal acid generator can be used. Among them, a crosslinking acid catalyst is preferably used.
[0224] Examples of the sulfonic acid compound or carboxylic acid compound include ammonium trifluoroacetate, p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridine Trifluoromethanesulfonate, pyridine - p-Toluenesulfonate, pyridine -4-Hydroxybenzenesulfonate, salicylic acid, camphorsulfonic acid, 5-sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-hydroxybenzenesulfonic acid, pyridine -4-Hydroxybenzenesulfonic acid, benzene disulfonic acid, 1-naphthalenesulfonic acid, 4-nitrobenzenesulfonic acid, citric acid, benzoic acid, hydroxybenzoic acid.
[0225] Examples of the thermal acid generator include K-PURE [registered trademark] CXC-1612, K-PURE CXC-1614, K-PURE TAG-2172, K-PURE TAG-2179, K-PURE TAG-2678, and K-PURE TAG2689 (all manufactured by King Industries), and SI-45, SI-60, SI-80, SI-100, SI-110, and SI-150 (all manufactured by Sanshin Chemical Industry Co., Ltd.).
[0226] These crosslinking catalysts may be used alone or in combination of two or more.
[0227] When the protective film forming composition contains a crosslinking catalyst, the content thereof is 0.0001 to 20% by weight, preferably 0.01 to 15% by weight, and more preferably 0.1 to 10% by weight, based on the total solid content of the protective film forming composition.
[0228] [Crosslinking agent]
[0229] The resist underlayer film forming composition of the present invention may include a crosslinking agent component. As the crosslinking agent, melamine system, substituted urea system, or polymer system thereof, etc. may be cited. Preferably, the crosslinking agent has at least two crosslinking substituents, such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea, or methoxymethylated thiourea. In addition, condensates of these compounds may also be used.
[0230] In addition, as the crosslinking agent, a crosslinking agent with high heat resistance can be used. As the crosslinking agent with high heat resistance, a compound containing a crosslinking-forming substituent having an aromatic ring (for example, a benzene ring or a naphthalene ring) in the molecule can be used.
[0231] Examples of the compound include a compound having a partial structure of the following formula (5-1) and a polymer or oligomer having a repeating unit of the following formula (5-2).
[0232]
[0233] The above R 11 , R12 , R 13 , and R 14 Each of them is the same or different and is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and the alkyl groups exemplified above can be used.
[0234] m1 is 1≤m1≤6-m2, m2 is 1≤m2≤5, m3 is 1≤m3≤4-m2, and m4 is 1≤m4≤3.
[0235] Examples of the compounds, polymers, and oligomers of formula (5-1) and formula (5-2) are shown below.
[0236]
[0237]
[0238] The above compounds can be obtained as products of Asahi Organic Materials Industries, Ltd. and Honshu Chemical Industries, Ltd. For example, the compound of formula (6-22) among the above crosslinking agents can be obtained as TMOM-BP from Asahi Organic Materials Industries, Ltd.
[0239] These cross-linking agents may be used alone or in combination of two or more.
[0240] The amount of the crosslinking agent added varies depending on the coating solvent used, the base substrate used, the required solution viscosity, the required film shape, etc., but is generally 0.001 to 80% by weight, preferably 0.01 to 50% by weight, and more preferably 0.1 to 40% by weight relative to the total solid content of the protective film-forming composition. Although these crosslinking agents sometimes undergo crosslinking reactions by self-condensation, when there are crosslinking substituents in the above-mentioned polymer of the present invention, they can undergo crosslinking reactions with these crosslinking substituents.
[0241] [Surfactant]
[0242] In order to improve the coating property on the semiconductor substrate, the protective film forming composition of the present invention may contain a surfactant as an optional component. Examples of the surfactant include polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, polyoxyethylene oleyl ether and other polyoxyethylene alkyl ethers, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether and other polyoxyethylene alkyl aryl ethers, polyoxyethylene / polyoxypropylene block copolymers, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, Sorbitan fatty acid esters such as sorbitan trioleate and sorbitan tristearate, polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate and polyoxyethylene sorbitan tristearate, etc., nonionic surfactants, EFTOP (registered trademark) EF30 1. EFT EF303, EFT EF352 (Mitsubishi Mitsubishi Electronics Co., Ltd. Co., Ltd.), メガファック [registered trademark] F171, メガファック F173, メガファックR -30、メガファックR-30N、メガファックR-40、メガファックR-40-L M (manufactured by DIC Co., Ltd.), Fluoro FC430, Fluoro FC431 (Sumitomo Solar Fluorine-based surfactants such as SURFLUO® (manufactured by Asahi Glass Co., Ltd.), ASHIGADO (registered trademark) AG710, S-382 (registered trademark), S-101, S-102, S-103, S-104, S-105, and S-106 (manufactured by Asahi Glass Co., Ltd.), and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). These surfactants may be used alone or in combination of two or more. When the protective film-forming composition contains a surfactant, the content thereof is 0.0001 to 10% by weight, preferably 0.01 to 5% by weight, relative to the total solid content of the protective film-forming composition.
[0243] [Other ingredients]
[0244] The protective film forming composition of the present invention may contain a light absorber, a rheology regulator, an adhesion aid, etc. The rheology regulator is effective in improving the fluidity of the protective film forming composition. The adhesion aid is effective in improving the adhesion between the semiconductor substrate or the resist and the underlying film.
[0245] As the light absorber, for example, commercially available light absorbers described in "Industrial Colorant Technology and Market" (published by CMC) and "Dye Handbook" (edited by the Society of Synthetic Organic Chemistry) can be suitably used, such as CI Disperse Yellow 1, 3, 4, 5, 7, 8, 13, 23, 31, 49, 50, 51, 54, 60, 64, 66, 68, 79, 82, 88, 90, 93, 102, 114 and 124; CI Disperse Orange 1, 5, 13, 25, 29, 30, 31, 44, 57, 72 and 73; CI Disperse Red 1, 5, 7, 13, 17, 19, 43, 50, 54, 58, 65, 72, 73, 88, 117, 137, 143, 199 and 210; CI Disperse Violet 43; CI Disperse Blue 96; CI Fluorescent Brightener 112, 135 and 163; CI Solvent Orange 2 and 45; CI Solvent Red 1, 3, 8, 23, 24, 25, 27 and 49; CI Pigment Green 10; CI Pigment Brown 2, etc. The light absorber is usually blended in a ratio of 10% by mass or less, preferably 5% by mass or less, based on the total solid content of the protective film-forming composition.
[0246] The rheology modifier is mainly added to improve the fluidity of the protective film forming composition, especially in the baking process, to improve the uniformity of the film thickness of the resist lower film and to improve the filling property of the protective film forming composition into the hole. As a specific example, phthalic acid derivatives such as dimethyl phthalate, diethyl phthalate, diisobutyl phthalate, dihexyl phthalate, butyl isodecyl phthalate, di-n-butyl adipate, diisobutyl adipate, diisooctyl adipate, octyl decyl adipate, di-n-butyl maleate, diethyl maleate, dinonyl maleate, maleic acid derivatives such as maleic acid, methyl oleate, butyl oleate, tetrahydrofurfuryl oleate, or stearic acid derivatives such as stearic acid n-butyl ester and glyceryl stearate can be cited. These rheology modifiers are usually matched in a ratio of less than 30% by mass relative to the total solid content of the protective film forming composition.
[0247] The adhesion aid is mainly added for the purpose of improving the adhesion between the substrate or the resist and the protective film-forming composition, and particularly for the purpose of preventing the resist from peeling off during development. Specific examples include chlorosilanes such as trimethylchlorosilane, dimethylhydroxymethylchlorosilane, methyldiphenylchlorosilane, and chloromethyldimethylchlorosilane; alkoxysilanes such as trimethylmethoxysilane, dimethyldiethoxysilane, methyldimethoxysilane, dimethylhydroxymethylethoxysilane, diphenyldimethoxysilane, and phenyltriethoxysilane; silazanes such as hexamethyldisilazane, N,N'-bis(trimethylsilyl)urea, dimethyltrimethylsilylamine, and trimethylsilylimidazole; silanes such as hydroxymethyltrichlorosilane, γ-chloropropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and γ-glycidoxypropyltrimethoxysilane; benzotriazole, benzimidazole, indazole, imidazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, and 2-mercaptobenzothiazole. Heterocyclic compounds such as azole, urea, thiouracil, mercaptoimidazole, and mercaptopyrimidine, urea such as 1,1-dimethylurea and 1,3-dimethylurea, or thiourea compounds. These adhesion aids are usually blended in a ratio of less than 5% by mass, preferably less than 2% by mass, relative to the total solid content of the protective film forming composition.
[0248] [Protective film forming composition]
[0249] The solid content of the protective film forming composition of the present invention is usually 0.1 to 70% by mass, preferably 0.1 to 60% by mass. The solid content is the content ratio of all components after removing the solvent from the protective film forming composition. The ratio of the ring-opening polymer in the solid content is preferably in the order of 1 to 100% by mass, 1 to 99.9% by mass, 50 to 99.9% by mass, 50 to 95% by mass, and 50 to 90% by mass.
[0250] [Protective film, method for manufacturing substrate with resist pattern, and method for manufacturing semiconductor device]
[0251] Hereinafter, a protective film produced using the protective film-forming composition according to the present invention, a method for producing a substrate with a resist pattern, and a method for producing a semiconductor device will be described.
[0252] The substrate with a resist pattern according to the present invention can be produced by applying the protective film-forming composition on a semiconductor substrate and firing the coating.
[0253] Examples of the semiconductor substrate to which the protective film-forming composition of the present invention is applied include silicon wafers, germanium wafers, and compound semiconductor wafers such as gallium arsenide, indium phosphide, gallium nitride, indium nitride, and aluminum nitride.
[0254] When a semiconductor substrate having an inorganic film formed on the surface is used, the inorganic film is formed by, for example, ALD (atomic layer deposition) method, CVD (chemical vapor deposition) method, reactive sputtering method, ion plating method, vacuum evaporation method, spin coating method (spin-on glass: SOG). Examples of the inorganic film include polysilicon film, silicon oxide film, silicon nitride film, BPSG (Boro-Phospho Silicate Glass) film, titanium nitride film, titanium oxynitride film, tungsten nitride film, gallium nitride film, and gallium arsenide film.
[0255] On such a semiconductor substrate, the protective film forming composition of the present invention is applied by a suitable coating method such as a spin coater or a coater. Then, a protective film is formed by baking using a heating device such as a hot plate. As baking conditions, it is appropriately selected from a baking temperature of 100°C to 400°C and a baking time of 0.3 minutes to 60 minutes. Preferably, the baking temperature is 120°C to 350°C, the baking time is 0.5 minutes to 30 minutes, and more preferably, the baking temperature is 150°C to 300°C, and the baking time is 0.8 minutes to 10 minutes. As the film thickness of the protective film formed, for example, it is 0.001μm to 10μm, preferably 0.002μm to 1μm, and more preferably 0.005μm to 0.5μm. When the temperature during baking is lower than the above range, crosslinking sometimes becomes insufficient, and it is not easy to obtain the resistance of the formed protective film to the resist solvent or the alkaline hydrogen peroxide aqueous solution. On the other hand, when the temperature during baking is higher than the above range, the protective film is sometimes decomposed by heat.
[0256] Exposure is performed through a mask (intermediate mask) for forming a predetermined pattern, using, for example, i-rays, KrF excimer lasers, ArF excimer lasers, EUV (extreme ultraviolet rays) or EB (electron beams). An alkaline developer is used for development, and is appropriately selected from a development temperature of 5°C to 50°C and a development time of 10 seconds to 300 seconds. As an alkaline developer, an aqueous solution of an alkali such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, ammonia water, etc., a primary amine such as ethylamine, n-propylamine, a secondary amine such as diethylamine, di-n-butylamine, a tertiary amine such as triethylamine, methyldiethylamine, etc., an alcohol amine such as dimethylethanolamine, triethanolamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, quaternary ammonium salts such as choline, cyclic amines such as pyrrole and piperidine, etc. can be used. Furthermore, an appropriate amount of an alcohol such as isopropyl alcohol, a nonionic surfactant, etc. can also be added to the aqueous solution of the above-mentioned alkali and used. Among them, preferred developing solutions are quaternary ammonium salts, and more preferably tetramethylammonium hydroxide and choline. Furthermore, surfactants and the like may be added to these developing solutions. Instead of alkaline developing solutions, a method may be used in which the portion of the photoresist whose alkali dissolution rate is not increased is developed by using an organic solvent such as butyl acetate.
[0257] Next, the protective film is dry-etched using the formed resist pattern as a mask. At this time, if the inorganic film is formed on the surface of the semiconductor substrate used, the surface of the inorganic film is exposed, and if the inorganic film is not formed on the surface of the semiconductor substrate used, the surface of the semiconductor substrate is exposed.
[0258] Furthermore, a desired pattern is formed by performing wet etching using a semiconductor wet etching solution using the protective film after dry etching (when a resist pattern remains on the protective film, the resist pattern is also used) as a mask.
[0259] [Wet etching solution for semiconductors]
[0260] As the semiconductor wet etching solution, a general chemical solution used for etching a semiconductor wafer can be used, and for example, either an acidic substance or an alkaline substance can be used.
[0261] As the acidic substance, for example, hydrogen peroxide, hydrofluoric acid, ammonium fluoride, acidic ammonium fluoride, ammonium bifluoride, buffered hydrofluoric acid, hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid or a mixture thereof can be cited. As a specific example, SC-2 (hydrochloric acid-hydrogen peroxide solution) can be cited.
[0262] As a substance showing alkalinity, an alkaline hydrogen peroxide solution obtained by mixing an organic amine such as ammonia, sodium hydroxide, potassium hydroxide, sodium cyanide, potassium cyanide, triethanolamine, etc. with hydrogen peroxide solution to make the pH alkaline can be cited. As a specific example, SC-1 (ammonia-hydrogen peroxide solution) can be cited. In addition, a substance capable of making the pH alkaline can also be used as a wet etching solution, for example, a substance that makes the pH alkaline by mixing urea with hydrogen peroxide solution and causing thermal decomposition of urea by heating to generate ammonia.
[0263] Among them, acidic hydrogen peroxide water or alkaline hydrogen peroxide water is preferred.
[0264] These liquids may contain additives such as surfactants.
[0265] The use temperature of the semiconductor wet etching solution is preferably 25° C. to 90° C., more preferably 40° C. to 80° C. The wet etching time is preferably 0.5 minute to 30 minutes, more preferably 1 minute to 20 minutes.
[0266] Example
[0267] The present invention will be described in further detail below with reference to Examples etc., but the present invention is not limited to the following Examples etc. at all.
[0268] The apparatus and the like used for measuring the weight average molecular weight of the polymer obtained in the following synthesis example are shown.
[0269] Device: HLC-8320GPC manufactured by Higashikata Co., Ltd.
[0270] GPC column: Shodex〔registered trademark〕Asahipak〔registered trademark〕(Showa Denko K.K.)
[0271] Column temperature: 40°C
[0272] Flow rate: 0.35mL / min
[0273] Eluent: Tetrahydrofuran (THF)
[0274] Standard sample: Polystyrene (Tosoh Corporation)
[0275] <Synthesis example 1>
[0276] A solution of 3.0 g of glycerol monomethacrylate (product name: Brenma GLM, manufactured by NOF Corporation), 4.6 g of 5-vinylbenzo[d][1,3]dioxole (manufactured by Cool Pharm LTD.), 1.4 g of N-isopropylacrylamide (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.7 g of dimethyl 2,2'-azobis(isobutyrate) (manufactured by Wako Pure Chemical Industries, Ltd.), and 31.2 g of propylene glycol monomethyl ether was added to a dropping funnel, and the mixture was added dropwise to a reaction flask containing 7.8 g of propylene glycol monomethyl ether at 100° C. under a nitrogen atmosphere, followed by heating and stirring for 24 hours. To the obtained solution, 9.8 g of anion exchange resin (product name: Dawuex [registered trademark] 550A, Muromachi Technos Co., Ltd.) and 9.8 g of cation exchange resin (product name: Anvalite [registered trademark] 15JWET, Organo Co., Ltd.) were added, and ion exchange treatment was performed at room temperature for 4 hours. The ion exchange resin was separated to obtain a resin solution corresponding to formula (P-1), and the weight average molecular weight (Mw) measured by GPC in terms of polystyrene was 6819.
[0277]
[0278] <Example 1>
[0279] Pyridine was added as a crosslinking acid catalyst to 7.6 g of the resin solution (solid content: 15.0 wt%) obtained in Synthesis Example 1. A solution of a protective film-forming composition was prepared by adding 0.06 g of trifluoromethanesulfonic acid (manufactured by ADEKA Corporation), 0.001 g of a surfactant (manufactured by DIC Corporation, product name: Megafac R-40, a fluorine-based surfactant), 10.4 g of propylene glycol monomethyl ether, and 1.9 g of propylene glycol monomethyl ether acetate.
[0280] <Synthesis example 2>
[0281] A solution of 2.5 g of glycerol monomethacrylate (product name: Brenma GLM, manufactured by NOF Corporation), 3.9 g of 5-vinylbenzo[d][1,3]dioxole (manufactured by Cool Pharm LTD.), 2.5 g of 2-(O-[1'-methylpropyleneamino]carboxyamino)ethyl methacrylate (manufactured by Showa Denko K.K., trade name: Calends [registered trademark] MOI-BM), 0.6 g of dimethyl 2,2'-azobis(isobutyrate) (manufactured by Wako Pure Chemical Industries, Ltd.), and 30.3 g of propylene glycol monomethyl ether was placed in a dropping funnel, and the mixture was added dropwise to a reaction flask containing 7.6 g of propylene glycol monomethyl ether at 100° C. under a nitrogen atmosphere, followed by heating and stirring for 24 hours. To the obtained solution, 9.5 g of anion exchange resin (product name: Dawuex [registered trademark] 550A, Muromachi Technos Co., Ltd.) and 9.5 g of cation exchange resin (product name: Anvalite [registered trademark] 15JWET, Organo Co., Ltd.) were added, and ion exchange treatment was performed at room temperature for 4 hours. The ion exchange resin was separated to obtain a resin solution corresponding to formula (P-2), and the weight average molecular weight (Mw) measured by GPC in terms of polystyrene was 17108.
[0282]
[0283] <Example 2>
[0284] Pyridine was added as a crosslinking acid catalyst to 6.6 g of the resin solution (solid content: 17.3 wt%) obtained in Synthesis Example 2. A solution of a protective film-forming composition was prepared by adding 0.06 g of trifluoromethanesulfonic acid (manufactured by ADEKA Corporation), 0.001 g of a surfactant (manufactured by DIC Corporation, product name: Megafac R-40, a fluorine-based surfactant), 11.4 g of propylene glycol monomethyl ether, and 1.9 g of propylene glycol monomethyl ether acetate.
[0285] <Synthesis example 3>
[0286] A solution of 3.0 g of glycerol monomethacrylate (product name: Brenma GLM, manufactured by NOF Corporation), 4.6 g of 5-vinylbenzo[d][1,3]dioxole (manufactured by Cool Pharm LTD.), 1.6 g of N-(methoxymethyl)methacrylamide (manufactured by Wako Pure Chemical Industries, Ltd.), 0.7 g of dimethyl 2,2'-azobis(isobutyrate) (manufactured by Wako Pure Chemical Industries, Ltd.), and 31.9 g of propylene glycol monomethyl ether was added to a dropping funnel, and the mixture was added dropwise to a reaction flask containing 8.0 g of propylene glycol monomethyl ether at 100° C. under a nitrogen atmosphere, followed by heating and stirring for 24 hours. To the obtained solution, 10.0 g of anion exchange resin (product name: Dawuex [registered trademark] 550A, Muromachi Technos Co., Ltd.) and 10.0 g of cation exchange resin (product name: Anvalite [registered trademark] 15JWET, Organo Co., Ltd.) were added, and ion exchange treatment was performed at room temperature for 4 hours. The ion exchange resin was separated to obtain a resin solution corresponding to formula (P-3), and the weight average molecular weight (Mw) measured by GPC in terms of polystyrene was 6622.
[0287]
[0288] <Example 3>
[0289] Pyridine was added as a crosslinking acid catalyst to 7.4 g of the resin solution (solid content: 15.5 wt%) obtained in Synthesis Example 3. A solution of a protective film-forming composition was prepared by adding 0.06 g of trifluoromethanesulfonic acid (manufactured by ADEKA Corporation), 0.001 g of a surfactant (manufactured by DIC Corporation, product name: Megafac R-40, a fluorine-based surfactant), 10.7 g of propylene glycol monomethyl ether, and 1.9 g of propylene glycol monomethyl ether acetate.
[0290] <Synthesis example 4>
[0291] A solution of 3.0 g of glycerol monomethacrylate (product name: Brenma GLM, manufactured by NOF Corporation), 4.6 g of 5-vinylbenzo[d][1,3]dioxole (manufactured by Cool Pharm LTD.), 1.26 g of N-(hydroxymethyl)acrylamide (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.7 g of dimethyl 2,2'-azobis(isobutyrate) (manufactured by Wako Pure Chemical Industries, Ltd.), and 30.7 g of propylene glycol monomethyl ether was added to a dropping funnel, and the mixture was added dropwise to a reaction flask containing 7.7 g of propylene glycol monomethyl ether at 100° C. under a nitrogen atmosphere, followed by heating and stirring for 24 hours. To the obtained solution, 9.6 g of anion exchange resin (product name: Dawuex [registered trademark] 550A, Muromachi Technos Co., Ltd.) and 9.6 g of cation exchange resin (product name: Anvalite [registered trademark] 15JWET, Organo Co., Ltd.) were added, and ion exchange treatment was performed at room temperature for 4 hours. The ion exchange resin was separated to obtain a resin solution corresponding to formula (P-4), and the weight average molecular weight (Mw) measured by GPC in terms of polystyrene was 5450.
[0292]
[0293] <Example 4>
[0294] Pyridine was added as a crosslinking acid catalyst to 6.9 g of the resin solution (solid content: 16.5 wt%) obtained in Synthesis Example 4. A solution of a protective film-forming composition was prepared by adding 0.06 g of trifluoromethanesulfonic acid (manufactured by ADEKA Corporation), 0.001 g of a surfactant (manufactured by DIC Corporation, product name: Megafac R-40, a fluorine-based surfactant), 11.2 g of propylene glycol monomethyl ether, and 1.9 g of propylene glycol monomethyl ether acetate.
[0295] <Synthesis example 5>
[0296] A solution of 5.50 g of glycerol monomethacrylate (product name: Brenma GLM, manufactured by NOF Corporation), 5.09 g of 5-vinylbenzo[d][1,3]dioxole (manufactured by Cool Pharm LTD.), 0.66 g of 2,2'-azobis(isobutyronitrile) (manufactured by Tokyo Chemical Industry Co., Ltd.), and 35.99 g of propylene glycol monomethyl ether was added to a dropping funnel, and the mixture was added dropwise to a reaction flask containing 9.00 g of propylene glycol monomethyl ether at 100° C. under a nitrogen atmosphere, and heated with stirring for 17 hours. To the obtained solution, 11 g of anion exchange resin (product name: DauEx [registered trademark] 550A, Muromachi Technos Co., Ltd.) and 11 g of cation exchange resin (product name: Anvalite [registered trademark] 15JWET, Organo Co., Ltd.) were added, and ion exchange treatment was performed at room temperature for 4 hours. The ion exchange resin was separated to obtain a resin solution corresponding to formula (X-1), and the weight average molecular weight (Mw) measured by GPC in terms of polystyrene was 10,800.
[0297]
[0298] <Comparative Example 1>
[0299] Pyridine was added as a crosslinking acid catalyst to 6.6 g of the resin solution (solid content: 17.4 wt%) obtained in Synthesis Example 5. A solution of a protective film-forming composition was prepared by adding 0.06 g of trifluoromethanesulfonic acid (manufactured by ADEKA Corporation), 0.001 g of a surfactant (manufactured by DIC Corporation, product name: Megafac R-40, a fluorine-based surfactant), 11.5 g of propylene glycol monomethyl ether, and 1.9 g of propylene glycol monomethyl ether acetate.
[0300] [Resist solvent resistance test]
[0301] The protective film forming composition prepared in Examples 1 to 4 and Comparative Example 1 was applied (spin-coated) on a silicon wafer using a spin coater. The coated silicon wafer was heated on a hot plate at 215°C for 1 minute to form a film (protective film) with a thickness of 100 nm. Next, in order to confirm the resist solvent resistance of the protective film, the silicon wafer after the protective film was formed was immersed in a solvent obtained by mixing propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate in a weight ratio of 7:3 for 1 minute, and then baked at 100°C for 30 seconds after spin drying. The film thickness of the protective film before and after immersion in the mixed solvent was measured by an optical interference film thickness meter.
[0302] Regarding the evaluation of the solvent resistance of the resist, the film thickness reduction rate (%) of the protective film removed by solvent immersion was calculated by the calculation formula of ((film thickness before solvent immersion)-(film thickness after solvent immersion))÷(film thickness before solvent immersion)×100, and the evaluation was performed. In addition, if the film thickness reduction rate is about 1% or less, it can be said to be within the allowable range.
[0303] [Table 1]
[0304] (Table 1)
[0305]
[0306] The above results show that the film thickness change was very small even after immersion in a resist solvent in Examples 1 to 4 and Comparative Example 1, indicating good resist solvent resistance. Therefore, all examples have sufficient resist solvent resistance to function as a protective film.
[0307] [Resistance test to alkaline hydrogen peroxide solution]
[0308] As an evaluation of resistance to alkaline hydrogen peroxide water, the protective film forming compositions prepared in Examples 1 to 4 and Comparative Example 1, which showed good resist solvent resistance in the above-mentioned resist solvent resistance test, were each applied to a TiN vapor-deposited substrate with a film thickness of 50 nm, and heated at 215°C for 1 minute to form a film with a film thickness of 100 nm. Next, 28% ammonia water, 33% hydrogen peroxide, and water were mixed in a weight ratio of 1:1:2 to prepare alkaline hydrogen peroxide water. The TiN vapor-deposited substrate coated with the protective film forming composition was immersed in the alkaline hydrogen peroxide water heated to 50°C, and the time from just after immersion to the protective film peeling off from the substrate was measured. The results are shown in Table 2.
[0309] [Table 2]
[0310] (Table 2)
[0311]
[0312] According to the above results, Examples 3 and 4 show that the coating films are less likely to peel off from the substrate in alkaline hydrogen peroxide water than Comparative Example 1. That is, Examples 3 and 4 show better chemical resistance to alkaline hydrogen peroxide water than Comparative Example 1, and are useful as protective films against alkaline hydrogen peroxide water.
[0313] [Resistance test to acidic hydrogen peroxide water]
[0314] As an evaluation of resistance to acidic hydrogen peroxide water, the protective film forming compositions prepared in Examples 1 to 4 and Comparative Example 1, which showed good resist solvent resistance in the above-mentioned resist solvent resistance test, were each coated on a TiN vapor-deposited substrate with a film thickness of 50 nm, and heated at 215°C for 1 minute to form a film with a film thickness of 100 nm. Next, 85% phosphoric acid and 35% hydrogen peroxide were mixed in a weight ratio of 1:1 to prepare acidic hydrogen peroxide water. The TiN vapor-deposited substrate coated with the protective film forming composition was immersed in the acidic hydrogen peroxide water heated to 60°C, and the time from just after immersion to the protective film peeling off from the substrate was measured. The results are shown in Table 3.
[0315] [Table 3]
[0316] (Table 3)
[0317]
[0318] Industrial Availability
[0319] According to the present invention, a composition for forming a protective film having excellent resistance to a semiconductor wet etching solution in a photolithography process in semiconductor manufacturing can be provided.
Claims
1. A composition for forming a protective film for a semiconductor wet etching solution, comprising: a compound or polymer comprising at least one acetal structure and at least one amide structure, and a solvent, The acetal structure comprises the structure shown in formula (1), In formula (1), R 1 and R 2 are the same or different and are a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted with a monovalent organic group (A), or an aryl group having 6 to 40 carbon atoms which may be substituted with a monovalent organic group (A), n1 is 0, 1, or 2, n2 is 1 or 2, A 1 represents a hydrogen atom or a hydroxyl group, A 2 Represents -CH(R 0 )-A 4 base, R 0 represents a hydrogen atom, a phenyl group which may be substituted with 1 to 3 hydroxyl groups, or a benzodioxolyl group, A 3 and A 4 Each represents the same or different monovalent organic group (A-1). 2 . The protective film-forming composition according to claim 1 , wherein the polymer is a copolymer of a compound (a) containing at least one acetal structure in a molecule and a compound (b) containing at least one amide structure in a molecule. 3 . The protective film-forming composition according to claim 1 , wherein the amide structure or compound (b) includes a structure represented by —CO—NH— or —CO—N═.
4. The protective film-forming composition according to claim 2, wherein the compound (b) is represented by formula (2): In formula (2), R 20 represents a hydrogen atom or a methyl group, R 21 and R 22 Each is the same or different and is a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be substituted by a monovalent organic group (B) and may be interrupted by an oxygen atom or a quaternary ammonium cation, or an aryl group having 6 to 40 carbon atoms which may be substituted by a monovalent organic group (B) and may be interrupted by an oxygen atom or a quaternary ammonium cation.
5. The protective film-forming composition according to claim 4, wherein the monovalent organic group (B) is selected from a hydroxyl group, a cyano group, a sulfo group, a carboxylate group, a boron atom which may be substituted with one or two hydroxyl groups, an alkyl group having 1 to 6 carbon atoms which may be substituted with a halogen atom, and -NR a1 R b1 Base, where R a1 and R b1 Each of them is the same or different and represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.
6. The protective film-forming composition according to claim 2, wherein the compound (b) is represented by formula (2-1): In formula (2-1), R 20 represents a hydrogen atom or a methyl group, R 23 represents an alkylene group having 1 to 5 carbon atoms, R 24 Indicates blocked isocyanate groups.
7. The protective film-forming composition according to claim 6, wherein the blocked isocyanate group is represented by the following general formula (21): In the formula, A represents a residue of an isocyanate-blocking compound selected from alcohols, amines, amides, active methylene compounds, nitrogen-containing heteroaryl compounds, oximes, ketoximes, and hydroxamates.
8. The protective film-forming composition according to claim 6 or 7, wherein the compound represented by formula (2-1) is represented by the following structural formula: 9 . The protective film-forming composition according to claim 2 , wherein the molar ratio of the unit structure derived from the compound (a) containing at least one acetal structure in the molecule is 10 to 85 mol % based on the entire copolymer.
10. The protective film-forming composition according to claim 2, wherein the molar ratio of the unit structure derived from the compound (a) containing at least one acetal structure in the molecule is 30 to 70 mol% based on the entire copolymer.
11. The protective film-forming composition according to claim 2, wherein the molar ratio of the unit structure derived from the compound (a) containing at least one acetal structure in the molecule is 30 to 45 mol% based on the entire copolymer. 12 . The protective film-forming composition according to claim 2 , wherein the molar ratio of the compound (b) containing at least one amide structure in the molecule is 5 to 80 mol % based on the entire copolymer. 13 . The protective film-forming composition according to claim 2 , wherein the molar ratio of the compound (b) containing at least one amide structure in the molecule is 8 to 50 mol % based on the entire copolymer. 14 . The protective film-forming composition according to claim 2 , wherein the molar ratio of the compound (b) containing at least one amide structure in the molecule is 10 to 30 mol % based on the entire copolymer. 15 . The protective film-forming composition according to claim 2 , wherein the copolymer further has a unit structure containing a hydroxyl group.
16. The protective film-forming composition according to claim 15, wherein the unit structure containing a hydroxyl group is represented by the following formulas (A-7) to (A-18): 17 . The protective film-forming composition according to claim 1 , wherein the unit structure represented by the formula (1) accounts for 15 to 85 mol % based on the entire copolymer. 18 . The protective film-forming composition according to claim 4 , wherein the unit structure represented by the formula (2) accounts for 5 to 30 mol % based on the entire copolymer. 19 . The protective film-forming composition according to claim 15 , wherein the unit structure containing a hydroxyl group accounts for 10 to 30 mol % based on the entire copolymer. 20 . The protective film-forming composition according to claim 1 , further comprising a cross-linking catalyst. 21 . The protective film-forming composition according to claim 1 , further comprising a crosslinking agent. 22 . The protective film-forming composition according to claim 1 , further comprising a surfactant.
23. A protective film, characterized in that: A fired product of a coating film formed from the protective film-forming composition according to any one of claims 1 to 22.
24. A method for manufacturing a substrate with a resist pattern, characterized in that: The method comprises the steps of applying the protective film composition according to any one of claims 1 to 22 on a semiconductor substrate and firing the composition to form a protective film as a resist underlayer film, and is used for the production of a semiconductor.
25. A method for manufacturing a semiconductor device, comprising the following steps: forming a protective film on a semiconductor substrate on which an inorganic film can be formed using the protective film forming composition for a semiconductor wet etching solution according to any one of claims 1 to 22, forming a resist pattern on the protective film, dry-etching the protective film using the resist pattern as a mask to expose the surface of the inorganic film or the semiconductor substrate, and wet-etching and washing the inorganic film or the semiconductor substrate using a semiconductor wet etching solution using the dry-etched protective film as a mask.