tire

By using the outer rubber layer of high-content isoprene system and styrene butadiene rubber in the tire, combining silica and zinc compounds, the existing tires have low combustion cost, deterioration inhibition and block loss resistance. The lack of performance has achieved better grip performance and service life.

CN113372628BActive Publication Date: 2024-11-01SUMITOMO RUBBER INDUSTRIES LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202110194385.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-09
Filing Date
2021-02-20
Publication Date
2024-11-01
Estimated Expiration
2041-02-20

AI Technical Summary

Technical Problem

The existing multi-layer tread tires have shortcomings in low combustion cost, deterioration suppression and block loss resistance during use, especially it is difficult to effectively suppress deterioration over the years and improve grip performance.

Method used

The tread structure is adopted, and the outer rubber layer contains more than 25% isoprene-based rubber and styrene butadiene rubber, combined with silicon dioxide and zinc-containing compounds with a nitrogen adsorption specific surface area of ​​more than 200m2/g. And by optimizing the rubber composition ratio and additives, low combustion cost and deterioration inhibition are improved.

Benefits of technology

The comprehensive performance of the tire's low combustion cost, deterioration suppression and block loss resistance is significantly improved, extending the service life of the tire and improving the grip performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113372628B_ABST
    Figure CN113372628B_ABST
Patent Text Reader

Abstract

The present invention provides a tire that can improve the comprehensive performance of low fuel consumption, degradation suppression and block resistance. The present invention is a tire, wherein the outer rubber layer on the outer side in the radial direction of the tire in two or more treads adjacent to each other in the radial direction of the tire is formed by a rubber composition for the outer rubber layer, the rubber composition for the outer rubber layer comprising a rubber component containing 25% by mass or more of an isoprene-based rubber and a styrene-butadiene rubber, a nitrogen adsorption specific surface area of ​​200 m 2 / g or more of silica, sulfur and zinc-containing compounds; the inner rubber layer on the inner side of the tire in the radial direction is formed by a rubber composition for the inner rubber layer containing a rubber component and a zinc-containing compound; the tire satisfies the following formula (1). #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to tires. Background Art

[0002] In order to give tires required characteristics such as low fuel consumption and grip performance, tires with multi-layer treads have been proposed. For example, as a tire for reducing rolling resistance, the following tire has been proposed: a tire in which the tread portion that contributes most to this characteristic is made into a two-layer structure consisting of a tread base (base tread) (inner side) with small energy loss and a tread running surface (cap tread) (outer side) with excellent wear resistance.

[0003] Patent document 1 discloses a rubber composition for a tread base containing specified amounts of the following components: natural rubber, butadiene rubber containing 1,2-syndiotactic polybutadiene crystals, butadiene rubber synthesized using a rare earth element catalyst, and a reinforcing agent; however, it is still expected that tires with conventional multi-layer treads can suppress aging degradation.

[0004] [Prior art literature]

[0005] [Patent Document]

[0006] Patent Document 1: Japanese Patent Application Publication No. 2012-111795 Summary of the invention

[0007] [Problems to be solved by the invention]

[0008] The present invention has been made in view of the above-mentioned current situation, and an object of the present invention is to provide a tire having improved comprehensive performance of low fuel consumption, degradation suppression, and chipping resistance.

[0009] [Methods of solving the problem]

[0010] The present invention relates to a tire, wherein among two or more tread layers, an outer rubber layer on the outer side in the radial direction of the tire is formed of a rubber composition for an outer rubber layer, wherein the rubber composition for the outer rubber layer comprises: a rubber component containing 25% by mass or more of an isoprene-based rubber and a styrene-butadiene rubber, respectively, and a nitrogen adsorption specific surface area of ​​200 m 2 / g or more of silica, sulfur, and a zinc-containing compound; the inner rubber layer on the inner side in the radial direction of the tire is formed by a rubber composition for an inner rubber layer containing a rubber component and a zinc-containing compound; the tire satisfies the following formula (1).

[0011]

[0012] The above tire preferably satisfies the following formula.

[0013]

[0014] The above tire preferably satisfies the following formula (2).

[0015]

[0016] The rubber composition for the inner rubber layer of the tire preferably contains a resin having an unsaturated bond.

[0017] The rubber composition for an outer rubber layer of the tire preferably includes a mercapto-based silane coupling agent.

[0018] The rubber composition for the outer rubber layer has a nitrogen adsorption specific surface area of ​​200 m2 relative to 100 parts by mass of the rubber component. 2 The silica content of 1.577777 g / g or more is preferably 5 to 170 parts by mass.

[0019] The above tire preferably satisfies the following formula (3).

[0020]

[0021] The tire is preferably a pneumatic tire for a passenger car.

[0022] The tire outer diameter Dt and the tire cross-sectional width Wt of the above tire preferably satisfy the relationship of the following formula (I).

[0023]

[0024] [Effects of the invention]

[0025] The present invention is a tire in which, among two or more treads, the outer rubber layer on the outer side in the radial direction of the tire is formed of a rubber composition for an outer rubber layer, wherein the rubber composition for the outer rubber layer comprises: a rubber component containing 25% by mass or more of an isoprene-based rubber and a styrene-butadiene rubber, respectively, and a nitrogen adsorption specific surface area of ​​200 m 2 / g or more of silica, sulfur, and a zinc-containing compound; the inner rubber layer on the inner side in the radial direction of the tire is formed by a rubber composition for the inner rubber layer comprising a rubber component and a zinc-containing compound; and the tire satisfies the above formula (1), thereby being able to improve the comprehensive performance of low fuel consumption, degradation inhibition and resistance to block falling. DETAILED DESCRIPTION

[0026] The present invention is a tire in which, among two or more treads, the outer rubber layer on the outer side in the radial direction of the tire is formed of a rubber composition for an outer rubber layer, wherein the rubber composition for the outer rubber layer comprises: a rubber component containing 25% by mass or more of an isoprene-based rubber and a styrene-butadiene rubber, respectively, and a nitrogen adsorption specific surface area of ​​200 m 2 / g or more of silicon dioxide, sulfur, and a zinc-containing compound; the inner rubber layer on the inner side in the radial direction of the tire is formed by a rubber composition for an inner rubber layer containing a rubber component and a zinc-containing compound; and the above formula (1) is satisfied. Thus, the comprehensive performance of low fuel consumption, degradation inhibition, and anti-blocking performance can be improved.

[0027] The mechanism for obtaining this effect is not clear, but the following inference can be made. In order to obtain low fuel consumption, it is considered to use a rubber composition mixed with silica and a rubber component on the tread, wherein the rubber component mainly comprises (more than 50% by mass) isoprene-based rubber and styrene butadiene rubber. In addition, in order to achieve further low fuel consumption, it is considered to micronize silica, but silica is easily mixed into styrene butadiene rubber, and when micronized, it is difficult to disperse. Therefore, in styrene butadiene rubber, silica and the silane coupling agent mixed with silica at the same time may be localized. When this localization occurs, not only is it difficult to obtain the reinforcement of the rubber composition as a whole, but also the sulfur free radical becomes easy to act when it is generated, and the reinforcement may be further reduced. When the reinforcement decreases, it may become the starting point of the block falling. In the above tire, among the two adjacent layers in the radial direction of the tire, the inner rubber layer on the inner side in the radial direction of the tire contains a large amount of zinc-containing compounds such as zinc oxide with the function of capturing free radicals, compared with the outer rubber layer on the outer side in the radial direction of the tire, so it becomes easy to induce free radicals on the inner rubber layer side. The inner rubber layer does not directly contact the road surface, so even if some sulfur free radicals are generated, it is difficult to affect the block falling. Based on the above functions, it can be inferred that by using the above tire, the comprehensive performance of low fuel consumption, degradation inhibition and block falling resistance can be improved.

[0028] The tire has more than two layers of tread, and thus, any of a tread with a two-layer structure and a tread with a three-layer structure or more is also applicable. As the layers constituting the two-layer or more tread, there can be cited: a cap tread (a rubber layer disposed at the outermost side in the tire radial direction and in direct contact with the road surface), a base tread (a rubber layer disposed more radially inward than the cap tread), and rubber layers other than these (a base tread (a rubber layer disposed more radially inward than the base tread), etc.).

[0029] The above tire satisfies the following formula (1).

[0030]

[0031] From the viewpoint of suppressing aging degradation, the content of zinc element contained in the rubber composition for the outer rubber layer relative to 100 parts by mass of the rubber component / the content of zinc element contained in the rubber composition for the inner rubber layer relative to 100 parts by mass of the rubber component is preferably ≦0.90, more preferably ≦0.80, and further preferably ≦0.70. The upper limit is not particularly limited, but the content of zinc element contained in the rubber composition for the outer rubber layer relative to 100 parts by mass of the rubber component / the content of zinc element contained in the rubber composition for the inner rubber layer relative to 100 parts by mass of the rubber component is preferably ≧0.30, more preferably ≧0.40, and further preferably ≧0.50.

[0032] In addition, the above formula (1) can be realized by mixing a zinc-containing compound into both the rubber composition for the outer rubber layer and the rubber composition for the inner rubber layer, and adjusting the zinc element content by adjusting the respective contents.

[0033] In the above tire, among the two or more treads, the two adjacent layers in the radial direction of the tire (the outer rubber layer on the outer side in the radial direction of the tire and the inner rubber layer on the inner side in the radial direction of the tire) are made of a rubber composition for the outer rubber layer with a specified ratio.

[0034] (Rubber composition for outer rubber layer)

[0035] The rubber composition for the outer rubber layer contains isoprene rubber and styrene butadiene rubber (SBR). In the rubber composition for the outer rubber layer, the content of isoprene rubber in 100% by mass of the rubber component is 25% by mass or more, preferably 30% by mass or more, and more preferably 35% by mass or more, from the viewpoint of low fuel consumption and suppression of aging degradation. The upper limit of the content is not particularly limited, but is preferably 80% by mass or less, more preferably 60% by mass or less, and further preferably 50% by mass or less.

[0036] Examples of isoprene-based rubbers include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR. For NR, NR commonly used in the tire industry, such as SIR20, RSS#3, and TSR20, can be used; for IR, IR commonly used in the tire industry, such as IR2200, can be used. Modified NR includes deproteinized natural rubber (DPNR) and high-purity natural rubber (UPNR); modified NR includes epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber; modified IR includes epoxidized isoprene rubber, hydrogenated isoprene rubber, and grafted isoprene rubber. These can be used alone or in combination of two or more.

[0037] In the rubber composition for the outer rubber layer, from the viewpoint of low fuel consumption and suppression of aging degradation, the SBR content in 100% by mass of the rubber component is 25% by mass or more, preferably 35% by mass or more, more preferably 45% by mass or more, and further preferably 50% by mass or more. The upper limit of the content is not particularly limited, but is preferably 90% by mass or less, more preferably 80% by mass or less, and further preferably 70% by mass or less.

[0038] The SBR is not particularly limited, and for example, SBR commonly used in the tire industry, such as emulsion-polymerized SBR (E-SBR) and solution-polymerized SBR (S-SBR), can be used. These can be used alone or in combination of two or more.

[0039] Here, the rubber component is preferably a rubber having a weight average molecular weight (Mw) of 150,000 or more (more preferably 200,000 or more, and further preferably 250,000 or more). The upper limit of Mw is not particularly limited, but is preferably 4 million or less, more preferably 1 million or less, further preferably 700,000 or less, and particularly preferably 500,000 or less. By making Mw within the above range, there is a tendency that good fuel efficiency is obtained while suppressing the decline of aging degradation.

[0040] The styrene content of SBR is preferably 5% by mass or more, more preferably 10% by mass or more, and further preferably 15% by mass or more; and preferably 50% by mass or less, more preferably 40% by mass or less, further preferably 37% by mass or less, and particularly preferably 30% by mass or less. By making the styrene content within the above range, there is a tendency that good low fuel efficiency is obtained while suppressing the decline of deterioration over the years.

[0041] The vinyl content of SBR is preferably 20% by mass or more, more preferably 40% by mass or more, further preferably 45% by mass or more, particularly preferably 55% by mass or more, and preferably 70% by mass or less, more preferably 65% ​​by mass or less, further preferably 62% by mass or less. By making the vinyl content within the above range, there is the following trend: while obtaining good low fuel efficiency, the decline of deterioration over the years can also be suppressed.

[0042] SBR may be non-modified SBR or modified SBR. As modified SBR, it may be an SBR having a functional group that interacts with a filler such as silica, for example, an end-modified SBR obtained by modifying at least one end of SBR with a compound (modifier) ​​having the above functional group (end-modified SBR having the above functional group at the end), a main chain modified SBR having the above functional group in the main chain, a main chain end-modified SBR having the above functional group in the main chain and the end (for example, a main chain end-modified SBR having the above functional group and modified at least one end with the above modifier), or a multifunctional compound having two or more epoxy groups in the molecule (coupling), an end-modified SBR having a hydroxyl group or an epoxy group, etc. may be introduced. These may be used alone or in combination of two or more.

[0043] As the functional group, for example, there can be mentioned: amino, amide, silyl, alkoxysilyl, isocyanate, imino, imidazole, urea, ether, carbonyl, oxycarbonyl, mercapto, sulfide, disulfide, sulfonyl, sulfinyl, thiocarbonyl, ammonium, imido, hydrazine, azo, diazo, carboxyl, cyano, pyridyl, alkoxy, hydroxyl, oxy, and epoxy. In addition, these functional groups may have a substituent. Among them, amino (preferably, an amino group in which the hydrogen atom possessed by the amino group is substituted by an alkyl group having 1 to 6 carbon atoms), alkoxy (preferably, an alkoxy group having 1 to 6 carbon atoms), alkoxysilyl (preferably, an alkoxysilyl group having 1 to 6 carbon atoms) and amide are preferred.

[0044] For example, as the modified SBR, SBR modified with a compound (modifying agent) represented by the following formula can be suitably used.

[0045]

[0046] (Where R 1 , R 2 and R 3 are the same or different and represent an alkyl group, an alkoxy group, a silyloxy group, an acetal group, a carboxyl group (-COOH), a mercapto group (-SH) or a derivative thereof. 4 and R 5 are the same or different and represent a hydrogen atom or an alkyl group. 4 and R 5 It can bond with the nitrogen atom to form a ring structure. n represents an integer.)

[0047] As R 1 , R 2 and R 3, preferably an alkoxy group (preferably an alkoxy group having 1 to 8 carbon atoms, more preferably an alkoxy group having 1 to 4 carbon atoms). 4 and R 5 , preferably an alkyl group (preferably an alkyl group having 1 to 3 carbon atoms). n is preferably 1 to 5, more preferably 2 to 4, and even more preferably 3. 4 and R 5 When the alkoxy group forms a ring structure together with a nitrogen atom, a 4- to 8-membered ring is preferred. In addition, the alkoxy group may also include a cycloalkoxy group (cyclohexyloxy group, etc.) and an aryloxy group (phenoxy group, benzyloxy group, etc.).

[0048] As the specific example of the compound (modifier) ​​represented by the above formula, can enumerate: 2-dimethylaminoethyl trimethoxysilane, 3-dimethylaminopropyl trimethoxysilane, 2-dimethylaminoethyl triethoxysilane, 3-dimethylaminopropyl triethoxysilane, 2-diethylaminoethyl trimethoxysilane, 3-diethylaminopropyl trimethoxysilane, 2-diethylaminoethyl triethoxysilane and 3-diethylaminopropyl triethoxysilane etc.Wherein, preferably 3-dimethylaminopropyl trimethoxysilane, 3-dimethylaminopropyl triethoxysilane and 3-diethylaminopropyl trimethoxysilane.These can be used alone or with 2 or more kinds and use.

[0049] As the modified SBR, modified SBR modified with the following compounds (modifiers) may also be used appropriately. Examples of the modifier include: polyglycidyl ethers of polyols such as ethylene glycol diglycidyl ether, glycerol triglycidyl ether, trimethylolethane triglycidyl ether, and trimethylolpropane triglycidyl ether; polyglycidyl ethers of aromatic compounds having two or more phenolic groups such as diglycidyl bisphenol A; polyepoxy compounds such as 1,4-diglycidylbenzene, 1,3,5-triglycidylbenzene, and polyepoxidized liquid polybutadiene; 4,4'-diglycidyl- Tertiary amines containing epoxy groups, such as diphenylmethylamine and 4,4'-diglycidyl-dibenzylmethylamine; diglycidyl amino compounds, such as diglycidyl aniline, N,N'-diglycidyl-4-glycidyloxyaniline, diglycidyl o-toluidine, tetraglycidyl m-xylenediamine, tetraglycidylaminodiphenylmethane, tetraglycidyl p-phenylenediamine, diglycidylaminomethylcyclohexane and tetraglycidyl-1,3-bisaminomethylcyclohexane;

[0050] Acid chlorides containing amino groups, such as bis-(1-methylpropyl)carbamoyl chloride, 4-morpholinecarbonyl chloride, 1-pyrrolidinecarbonyl chloride, N,N-dimethylcarbamoyl chloride and N,N-diethylcarbamoyl chloride; silane compounds containing epoxy groups, such as 1,3-bis-(glycidyloxypropyl)-tetramethyldisiloxane and (3-glycidyloxypropyl)-pentamethyldisiloxane;

[0051] Silane compounds containing a thioether group such as (trimethylsilyl)[3-(trimethoxysilyl)propyl] sulfide, (trimethylsilyl)[3-(triethoxysilyl)propyl] sulfide, (trimethylsilyl)[3-(tripropoxysilyl)propyl] sulfide, (trimethylsilyl)[3-(tributoxysilyl)propyl] sulfide, (trimethylsilyl)[3-(methyldimethoxysilyl)propyl] sulfide, (trimethylsilyl)[3-(methyldiethoxysilyl)propyl] sulfide, (trimethylsilyl)[3-(methyldipropoxysilyl)propyl] sulfide and (trimethylsilyl)[3-(methyldibutoxysilyl)propyl] sulfide;

[0052] N-substituted aziridine compounds such as ethyleneimine and propyleneimine; alkoxysilanes such as methyltriethoxysilane; (thio)benzophenone compounds having an amino group and / or a substituted amino group such as 4-N,N-dimethylaminobenzophenone, 4-N,N-di-tert-butylaminobenzophenone, 4-N,N-diphenylaminobenzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(diphenylamino)benzophenone and N,N,N',N'-bis-(tetraethylamino)benzophenone; 4-N,N-dimethylaminobenzaldehyde, 4-N,N-diphenylaminobenzaldehyde and 4-N,N-divinylaminobenzophenone Benzaldehyde and other benzaldehyde compounds having an amino group and / or a substituted amino group; N-substituted pyrrolidones such as N-methyl-2-pyrrolidone, N-vinyl-2-pyrrolidone, N-phenyl-2-pyrrolidone, N-tert-butyl-2-pyrrolidone and N-methyl-5-methyl-2-pyrrolidone; N-substituted piperidones such as N-methyl-2-piperidone, N-vinyl-2-piperidone and N-phenyl-2-piperidone; N-substituted lactams such as N-methyl-ε-caprolactam, N-phenyl-ε-caprolactam, N-methyl-ω-laurolactam, N-vinyl-ω-laurolactam, N-methyl-β-propiolactam and N-phenyl-β-propiolactam; and others:

[0053] N,N-bis-(2,3-epoxypropoxy)-aniline, 4,4-methylene-bis-(N,N-glycidylaniline), tris-(2,3-epoxypropyl)-1,3,5-triazine-2,4,6-triones, N,N-diethylacetamide, N-methylmaleimide, N,N-diethylurea, 1,3-dimethylethyleneurea, 1,3-divinylethyleneurea, 1,3-diethyl-2-imidazolidinone, 1-methyl-3-ethyl-2-imidazolidinone, 4-N,N-dimethylaminoacetophenone, 4-N,N-diethylaminoacetophenone, 1,3-bis(diphenylamino)-2-propanone, and 1,7-bis(methylethylamino)-4-heptanone. Among them, modified SBR modified with alkoxysilane is preferred.

[0054] In addition, as the modified SBR modified by the compound (modifier) ​​represented by the above formula, for example, it is suitable to use the modified SBR obtained by modifying the polymerization end (active end) of the solution-polymerized styrene-butadiene rubber by the compound represented by the above formula. The modification by the above compound (modifier) ​​can be implemented by a known method.

[0055] As the SBR, for example, SBR manufactured and sold by Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Co., Ltd., etc. can be used.

[0056] The other rubber components that can be used in the rubber composition for the outer rubber layer are not particularly limited, and rubbers used in the field of tires can be used. For example, diene rubbers such as butadiene rubber (BR), acrylonitrile butadiene rubber (NBR), chloroprene rubber (CR), butyl rubber (IIR), and styrene isoprene butadiene copolymer rubber (SIBR) can be cited. Among them, BR is preferred.

[0057] In the rubber composition for the outer rubber layer, from the viewpoint of low fuel consumption and suppression of aging degradation, the BR content in 100% by mass of the rubber component is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. The upper limit of the content is not particularly limited, but is preferably 45% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less.

[0058] From the viewpoint of on-ice performance, the cis content of BR is preferably 80% by mass or more, more preferably 85% by mass or more, further preferably 90% by mass or more, particularly preferably 95% by mass or more.

[0059] BR is not particularly limited, and examples thereof include BR with a high cis content, BR containing 1,2-syndiotactic polybutadiene crystals (SPB-containing BR), butadiene rubber synthesized using a rare earth element catalyst (rare earth BR), and tin-modified butadiene rubber modified by a tin compound (tin-modified BR), which are commonly used in the tire industry. As for BR, products of Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, and Nippon Zeon Corporation can be used as commercial products. These can be used alone or in combination of two or more.

[0060] BR may be either unmodified BR or modified BR. Examples of modified BR include modified BR into which the above-mentioned functional groups are introduced. Preferred embodiments are the same as those of the modified SBR.

[0061] In this specification, Mw can be calculated based on the measured value obtained by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, chromatographic column: TSKGEL SUPERMULTIPOREHZ-M manufactured by Tosoh Corporation) and converted by standard polystyrene. The amount of styrene can be calculated by 1 The vinyl content (1,2-bonded butadiene unit amount) and the cis content (cis-1,4-bonded butadiene unit amount) can be measured by infrared absorption spectroscopic analysis.

[0062] The rubber composition for the outer rubber layer comprises: a nitrogen adsorption specific surface area (N2SA) of 200 m 2 The nitrogen adsorption specific surface area (N2SA) of silica is preferably 220 m 2 / g or more, more preferably 225m 2 / g or more, more preferably 230m 2 The upper limit of N2SA of silica is not particularly limited, but is preferably 350 m 2 / g or less, more preferably 300m 2 / g or less, more preferably 250m 2 / g or less, particularly preferably 280m 2 / g or less. By making the N2SA of silica below the upper limit, there is a tendency to obtain good dispersibility. By making the N2SA of silica within the above range, there is a tendency that good low fuel efficiency can be obtained while suppressing the decline of degradation over the years. In addition, the N2SA of silica is a value measured by the BET method according to ASTM D3037-93.

[0063] In the rubber composition for the outer rubber layer, N2SA is 200 m / s relative to 100 parts by mass of the rubber component. 2 The silica content of 100 g or more is preferably 5 parts by mass or more, more preferably 60 parts by mass or more, further preferably 70 parts by mass or more, and particularly preferably 90 parts by mass or more. The upper limit of the content is not particularly limited, but is preferably 170 parts by mass or less, more preferably 150 parts by mass or less, further preferably 150 parts by mass or less, and particularly preferably 120 parts by mass or less. By making the content within the above range, there is a tendency that good low fuel consumption can be obtained while suppressing the decline of degradation over the years.

[0064] As silica that can be used in the rubber composition for the outer rubber layer, dry silica (anhydrous silica) and wet silica (hydrous silica) etc. can be cited. Among them, wet silica is preferred because of the large number of silanol groups. As commercially available products, products of Degussa, Rhodia, Tosoh Silica Co., Ltd., Solvay Japan Co., Ltd. and Tokuyama Co., Ltd. etc. can be used. These can be used alone or in combination of two or more.

[0065] In the rubber composition for the outer rubber layer, from the viewpoint of low fuel consumption and suppression of aging degradation, the total vinyl content of the styrene butadiene rubber contained in the rubber composition for the outer rubber layer (the total amount of the vinyl content of the styrene butadiene rubber per 100 parts by mass of the rubber component contained in the rubber composition for the outer rubber layer) and the nitrogen adsorption specific surface area of ​​the rubber contained in the rubber composition for the outer rubber layer relative to 100 parts by mass of the rubber component are 200 m 2 The silica content of 1000 g or more preferably satisfies the following formula (3).

[0066]

[0067] Total vinyl content in the styrene-butadiene rubber contained in the rubber composition for the outer rubber layer / nitrogen adsorption specific surface area per 100 parts by mass of the rubber component contained in the rubber composition for the outer rubber layer is 200 m 2 The silica content of more than 1 g is preferably ≤0.45, more preferably ≤0.40, further preferably ≤0.35, and particularly preferably ≤0.30. The lower limit of this ratio is not particularly limited, but the total vinyl content in the rubber component contained in the rubber composition for the outer rubber layer / the nitrogen adsorption specific surface area contained in the rubber composition for the outer rubber layer relative to 100 parts by mass of the rubber component is 200 m 2 The silica content of 1.3777 W / g or more is preferably ≧0.10, more preferably ≧0.15, and further preferably ≧0.20.

[0068] In addition, the total vinyl content in the styrene butadiene rubber (the total content of the vinyl part contained in the total amount of the styrene butadiene rubber) is Σ(content of each styrene butadiene rubber×vinyl content of each styrene butadiene rubber / 100). For example, when the rubber component is composed of 90 mass% of SBR (A) (vinyl content of 20 mass%), 5 mass% of SBR (B) (vinyl content of 10 mass%) and 5 mass% of BR (vinyl content of 2 mass%), the total vinyl content in the rubber component is 18.6 mass% (= (90×20 / 100+5×10 / 100+5×2 / 100)).

[0069] When the rubber composition for the outer rubber layer contains silica, it is preferred to further contain a silane coupling agent. The silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis( 4-trimethoxysilylbutyl) trisulfide, bis(3-triethoxysilylpropyl) disulfide, bis(2-triethoxysilylethyl) disulfide, bis(4-triethoxysilylbutyl) disulfide, bis(3-trimethoxysilylpropyl) disulfide, bis(2-trimethoxysilylethyl) disulfide, bis(4-trimethoxysilylbutyl) disulfide, 3-trimethoxysilyl Sulfide-based silanes such as alkylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, and 3-triethoxysilylpropyl methacrylate monosulfide; mercapto-based silanes such as 3-mercaptopropyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, and NXT and NXT-Z manufactured by Momentive; vinyl-based silanes such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based silanes such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based silanes such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based silanes such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chlorine-based silanes such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. As commercially available products, products of Degussa, Momentive, Shin-Etsu Silicone Co., Ltd., Tokyo Chemical Industry Co., Ltd., Azmax Co., Ltd., Dow Corning Toray Co., Ltd., etc. can be used. These can be used alone or in combination of two or more.

[0070] Among the silane coupling agents, mercapto-based silane coupling agents are preferably used. In addition, as mercapto-based silane coupling agents, in addition to using compounds having a mercapto group, compounds having a structure in which a mercapto group is protected by a protective group (for example, a compound represented by the following formula (S1)) can also be used.

[0071] Particularly suitable mercapto-based silane coupling agents include silane coupling agents represented by the following formula (S1), or silane coupling agents comprising a bonding unit A represented by the following formula (I) and a bonding unit B represented by the following formula (II).

[0072]

[0073] (Where R 1001 represents a compound selected from -Cl, -Br, -OR 1006 、-O(O=)CR 1006 、-ON=CR 1006 R 1007 、-NR 1006 R 1007 and-(OSiR 1006 R 1007 ) h (OSiR 1006 R 1007 R 1008 ) in the monovalent group (R 1006 , R 1007 and R 1008 may be the same or different, and are respectively a hydrogen atom or a monovalent hydrocarbon group having 1 to 18 carbon atoms, and the average value of h is 1 to 4); R 1002 Represents R 1001 , a hydrogen atom or a monovalent hydrocarbon group having 1 to 18 carbon atoms; R 1003 Indicates -[O(R 1009 O) j ]-group (R 1009 is an alkylene group having 1 to 18 carbon atoms, and j is an integer of 1 to 4. ); R 1004 represents a divalent hydrocarbon group having 1 to 18 carbon atoms; R 1005 represents a monovalent hydrocarbon group having 1 to 18 carbon atoms; x, y and z are values ​​satisfying the following relationship: x+y+2z=3, 0≦x≦3, 0≦y≦2, 0≦z≦1. )

[0074]

[0075]

[0076] (wherein, v represents an integer greater than 0, and w represents an integer greater than 1. 11R represents: hydrogen, halogen, branched or unbranched alkyl group having 1 to 30 carbon atoms, branched or unbranched alkenyl group having 2 to 30 carbon atoms, branched or unbranched alkynyl group having 2 to 30 carbon atoms, or a group in which the terminal hydrogen of the alkyl group is replaced by a hydroxyl group or a carboxyl group. 12 represents: a branched or unbranched alkylene group having 1 to 30 carbon atoms, a branched or unbranched alkenylene group having 2 to 30 carbon atoms, or a branched or unbranched alkynylene group having 2 to 30 carbon atoms. 11 and R 12 Can form a ring structure. )

[0077] In formula (S1), R 1005 , R 1006 , R 1007 and R 1008 Each of them is independently preferably a group selected from a linear, cyclic or branched alkyl group, alkenyl group, aryl group and aralkyl group having 1 to 18 carbon atoms. 1002 When it is a monovalent hydrocarbon group having 1 to 18 carbon atoms, it is preferably a group selected from a linear, cyclic or branched alkyl group, alkenyl group, aryl group and aralkyl group. 1009 A linear, cyclic or branched alkylene group is preferred, and a linear alkylene group is particularly preferred. 1004 For example, there can be mentioned: alkylene groups having 1 to 18 carbon atoms, alkenylene groups having 2 to 18 carbon atoms, cycloalkylene groups having 5 to 18 carbon atoms, cycloalkylalkylene groups having 6 to 18 carbon atoms, arylene groups having 6 to 18 carbon atoms, and aralkylene groups having 7 to 18 carbon atoms. Alkylene groups and alkenylene groups may be straight-chain or branched; cycloalkylene groups, cycloalkylalkylene groups, arylene groups, and aralkylene groups may have a functional group such as a lower alkyl group on the ring. 1004 , preferably an alkylene group having 1 to 6 carbon atoms, particularly preferably a linear alkylene group (eg, a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, and a hexamethylene group).

[0078] As R in formula (S1) 1002 , R 1005 , R 1006 , R 1007 and R 1008 Specific examples of include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, octyl, decyl, dodecyl, cyclopentyl, cyclohexyl, vinyl, propenyl, allyl, hexenyl, octenyl, cyclopentenyl, cyclohexenyl, phenyl, tolyl, xylyl, naphthyl, benzyl, phenethyl and naphthylmethyl. 1009Examples of the linear alkylene group include a methylene group, an ethylene group, a n-propylene group, a n-butylene group, and a hexylene group. Examples of the branched alkylene group include an isopropylene group, an isobutylene group, and a 2-methylpropylene group.

[0079] Specific examples of the silane coupling agent represented by formula (S1) include: 3-hexanoylthiopropyl triethoxysilane, 3-octanoylthiopropyl triethoxysilane, 3-decanoylthiopropyl triethoxysilane, 3-lauroylthiopropyl triethoxysilane, 2-hexanoylthioethyl triethoxysilane, 2-octanoylthioethyl triethoxysilane, 2-decanoylthioethyl triethoxysilane, 2-lauroylthiopropyl triethoxysilane, 2-hexanoylthioethyl triethoxysilane, 2-octanoylthioethyl triethoxysilane, 2-decanoylthioethyl triethoxysilane, 2-lauroylthiopropyl triethoxysilane, 2- 3-capryloylthiopropyl trimethoxysilane, 3-capryloylthiopropyl trimethoxysilane, 3-lauroylthiopropyl trimethoxysilane, 2-caproylthioethyl trimethoxysilane, 2-capryloylthioethyl trimethoxysilane, 2-capryloylthioethyl trimethoxysilane, 2-capryloylthioethyl trimethoxysilane and 2-lauroylthioethyl trimethoxysilane etc. These can be used alone or with two or more kinds in combination. Among them, 3-capryloylthiopropyl triethoxysilane is particularly preferred.

[0080] In the silane coupling agent comprising the binding unit A represented by formula (I) and the binding unit B represented by formula (II), the content of the binding unit A is preferably 30 mol% or more, more preferably 50 mol% or more, preferably 99 mol% or less, and more preferably 90 mol% or less. In addition, the content of the binding unit B is preferably 1 mol% or more, more preferably 5 mol% or more, further preferably 10 mol% or more, preferably 70 mol% or less, more preferably 65 mol% or less, and further preferably 55 mol% or less. In addition, the total content of the binding units A and B is preferably 95 mol% or more, more preferably 98 mol% or more, and particularly preferably 100 mol%. In addition, the content of the binding unit A and the binding unit B is also included when the binding unit A and the binding unit B are located at the end of the silane coupling agent. The form of the binding unit A and the binding unit B when they are located at the end of the silane coupling agent is not particularly limited, as long as the binding unit A and the binding unit B form units corresponding to formulas (I) and (II).

[0081] Regarding R in formula (I) and (II): 11 As halogen, chlorine, bromine and fluorine can be mentioned. As branched or unbranched alkyl groups having 1 to 30 carbon atoms, methyl and ethyl can be mentioned. As branched or unbranched alkenyl groups having 2 to 30 carbon atoms, vinyl and 1-propenyl can be mentioned. As branched or unbranched alkynyl groups having 2 to 30 carbon atoms, ethynyl and propynyl can be mentioned.

[0082] Regarding R in formula (I) and (II): 12 Examples of the branched or unbranched alkylene group having 1 to 30 carbon atoms include ethylene and propylene. Examples of the branched or unbranched alkenylene group having 2 to 30 carbon atoms include vinylene and 1-propenylene. Examples of the branched or unbranched alkynylene group having 2 to 30 carbon atoms include ethynylene and propynylene.

[0083] In the silane coupling agent comprising the linking unit A represented by formula (I) and the linking unit B represented by formula (II), the total repetition number (v+w) of the repetition number (v) of the linking unit A and the repetition number (w) of the linking unit B is preferably in the range of 3 to 300.

[0084] The content of the silane coupling agent is preferably 3 parts by mass or more, more preferably 6 parts by mass or more, and further preferably 8 parts by mass or more relative to 100 parts by mass of silicon dioxide. By making the content above the lower limit, there is a tendency to obtain good breaking strength, etc. In addition, the above content is preferably 20 parts by mass or less, more preferably 15 parts by mass or less. By making the content within the above range, there is the following tendency: while obtaining good low fuel efficiency, the decline of degradation over the years can also be suppressed.

[0085] The rubber composition for the outer rubber layer preferably contains carbon black. In the rubber composition for the outer rubber layer, the content of carbon black is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and further preferably 5 parts by mass or more, relative to 100 parts by mass of the rubber component. The upper limit of the content is not particularly limited, but is preferably 30 parts by mass or less, more preferably 15 parts by mass or less, and further preferably 8 parts by mass or less. By making the content within the above range, there is the following trend: while obtaining good low fuel consumption, the decline of degradation over the years can also be suppressed.

[0086] The nitrogen adsorption specific surface area (N2SA) of carbon black is preferably 50 m 2 / g or more, more preferably 80m 2 / g or more, more preferably 100m 2 / g or more. In addition, the above N2SA is preferably 150m 2 / g or less, more preferably 130m 2 / g or less, more preferably 120m 2 / g or less. By making N2SA within the above range, there is a tendency that good low fuel efficiency can be obtained while suppressing the decline due to aging. In addition, the nitrogen adsorption specific surface area of ​​carbon black is obtained according to JIS K6217-2:2001.

[0087] Carbon black is not particularly limited, and examples thereof include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. Commercially available products include those produced by Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Co., Ltd., Lion Co., Ltd., Shin Nichika Carbon Co., Ltd., and Colombia Carbon Co., Ltd. These can be used alone or in combination of two or more.

[0088] The rubber composition for the outer rubber layer includes: a zinc-containing compound. Examples of the zinc-containing compound include: zinc oxide, basic zinc carbonate, zinc dithiophosphate compounds, fatty acid zinc, zinc hydroxide, and zinc carboxylate (zinc stearate, etc.). In addition, a microparticle zinc carrier having zinc oxide microparticles or basic zinc carbonate microparticles loaded on the surface of silicate particles may also be used. Among them, zinc oxide and zinc stearate may be used appropriately.

[0089] In the rubber composition for the outer rubber layer, the zinc content (the content converted from the zinc contained in the zinc-containing compound) is preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, further preferably 1.2 parts by mass or more, and particularly preferably 1.4 parts by mass or more, relative to 100 parts by mass of the rubber component. The upper limit of the content is preferably 3.0 parts by mass or less, more preferably 2.5 parts by mass or less, further preferably 2.0 parts by mass or less, and particularly preferably 1.8 parts by mass or less. By making the content within the above range, there is the following tendency: while obtaining good low fuel consumption, the decline of degradation over the years can also be suppressed.

[0090] As the zinc-containing compound, a conventionally known zinc-containing compound can be used. For example, zinc oxide products of Mitsui Mining and Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Shodo Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc. can be used.

[0091] The rubber composition for the outer rubber layer preferably contains: a liquid plasticizer (plasticizer that is liquid at 20°C) and a resin, etc. The resin refers to a resin that is solid at room temperature (25°C). In particular, a rubber composition in which a resin is mixed in a rubber component is preferred, wherein the rubber component contains SBR, BR and isoprene-based rubber.

[0092] In the rubber composition for the outer rubber layer, the content of the liquid plasticizer is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and further preferably 8 parts by mass or more, relative to 100 parts by mass of the rubber component. The upper limit of the content is not particularly limited, but is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and further preferably 15 parts by mass or less. By making the content within the above range, there is a tendency that good fuel efficiency is obtained while suppressing the decline of deterioration over time.

[0093] The liquid plasticizer is not particularly limited, and examples thereof include oils, liquid resins, and liquid diene polymers, etc. These may be used alone or in combination of two or more.

[0094] As oil, for example, process oil, vegetable oil or mixture thereof can be mentioned. As process oil, for example, paraffin process oil, aromatic process oil and cycloparaffin process oil etc. can be used. As vegetable oil, castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia oil and tung oil etc. can be mentioned. As commercially available products, products of Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., Japan Energy Co., Ltd., Olisoy Co., Ltd., H&R Co., Ltd., Toyokuni Oil Refining Co., Ltd., Showa Shell Sekiyu Co., Ltd., Fujikosan Co., Ltd. and Nissin OilliO Group Co., Ltd. etc. can be used.

[0095] Examples of liquid resins include terpene resins (including terpene phenol resins and aromatic modified terpene resins) that are liquid at 20°C, rosin resins, styrene resins, C5 resins, C9 resins, C5 / C9 resins, dicyclopentadiene (DCPD) resins, coumarone indene resins (including coumarone and indene monomer resins), phenol resins, olefin resins, polyurethane resins, and acrylic (ester) resins.

[0096] Examples of the liquid diene polymer include liquid styrene butadiene copolymers (liquid SBR), liquid butadiene polymers (liquid BR), liquid isoprene polymers (liquid IR), liquid styrene isoprene copolymers (liquid SIR), liquid styrene butadiene styrene block copolymers (liquid SBS block polymers), liquid styrene isoprene styrene block copolymers (liquid SIS block polymers), liquid farnesene polymers, and liquid farnesene butadiene copolymers, etc. The terminals or main chains thereof may be modified with polar groups.

[0097] In the rubber composition for the outer rubber layer, the content of the resin is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and further preferably 8 parts by mass or more, relative to 100 parts by mass of the rubber component. The upper limit of the content is not particularly limited, but is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and further preferably 15 parts by mass or less. By making the content within the above range, there is a tendency that good fuel efficiency is obtained while suppressing the decline of aging degradation.

[0098] The softening point of the resin is preferably 10°C or higher, more preferably 50°C or higher, further preferably 70°C or higher, and particularly preferably 80°C or higher. In addition, the softening point is preferably 180°C or lower, more preferably 150°C or lower, and further preferably 120°C or lower. By making the softening point within the above range, there is a tendency that good fuel efficiency is obtained while suppressing the decline due to aging. In addition, the softening point of the resin refers to the temperature at which the ball falls when the softening point specified in JIS K 6220-1:2001 is measured by a ring and ball softening point measuring device.

[0099] As resin, for example, it is suitable to use a resin with an unsaturated bond (double bonds and triple bonds in chain compounds, unsaturated bonds in cyclic compounds, etc.). Specifically, it can be cited: aromatic vinyl polymers (aromatic olefin polymers), coumarone-indene resins, coumarone resins, indene resins, phenol resins, rosin resins, petroleum resins, terpene resins and acrylic acid (ester) resins, etc. As commercially available products, products of Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Co., Ltd., Nippon Coating Chemical Co., Ltd., Nippon Catalyst Co., Ltd., JXTG Energy Co., Ltd., Arakawa Chemical Industries, Ltd., Tiangang Chemical Industries, Ltd., Toagosei Co., Ltd., Struktol, Performance Additive, and Mitsui Chemicals, Inc. can be used. These can be used alone or in combination of two or more.

[0100] The aromatic vinyl polymer may be a resin obtained by polymerizing α-methylstyrene and / or styrene, and examples thereof include homopolymers of styrene (styrene resins), homopolymers of α-methylstyrene (α-methylstyrene resins), copolymers of α-methylstyrene and styrene, and copolymers of styrene and other monomers. In addition, the aromatic vinyl polymer is preferably an ethylene-propylene-styrene copolymer. The ethylene-propylene content (EP content) in 100% by mass of the ethylene-propylene-styrene copolymer is preferably 70% by mass or more, more preferably 80% by mass or more, preferably 98% by mass or less, and more preferably 95% by mass or less. Among them, homopolymers of styrene, homopolymers of α-methylstyrene, and copolymers of α-methylstyrene and styrene are preferred.

[0101] Coumarone-indene resin refers to a resin containing coumarone and indene as main monomer components constituting the resin skeleton (main chain); monomer components that may be contained in the skeleton other than coumarone and indene include styrene, α-methylstyrene, methylindene, vinyltoluene, etc.

[0102] The coumarone resin is a resin containing coumarone as a main monomer component constituting the resin skeleton (main chain).

[0103] Indene resin refers to a resin containing indene as a main monomer component constituting the resin skeleton (main chain).

[0104] Examples of the phenol resin include phenol resins obtained by reacting phenol with aldehydes (such as formaldehyde, acetaldehyde, and furfural) under an acid or base catalyst, etc. Among them, phenol resins obtained by reacting under an acid catalyst (such as novolac phenol resins) are preferred.

[0105] Examples of the rosin resin include rosin-based resins represented by natural rosin, polymerized rosin, modified rosin, and ester compounds thereof, and hydrogenated products thereof.

[0106] Examples of the petroleum resin include C5-based resins, C9-based resins, C5 / C9-based resins, and dicyclopentadiene (DCPD) resins.

[0107] As the terpene resin, a polyterpene resin obtained by polymerizing a terpene compound, an aromatic modified terpene resin obtained by polymerizing a terpene compound and an aromatic compound, etc. can be used. In addition, hydrogenated products thereof can also be used.

[0108] Polyterpene resin is a resin obtained by polymerizing terpene compounds. The terpene compounds are (C5H8) n The hydrocarbons and their oxygenated derivatives are classified as monoterpenes (C 10 H 16 ), sesquiterpenes (C 15H 24 ) and diterpenes (C 20 H 32 ) and the like as a basic skeleton, for example, α-pinene, β-pinene, dipentene, limonene, myrcene, alloocimene, ocimene, α-phellandrene, α-terpinene, γ-terpinene, terpinolene, 1,8-cineole, 1,4-cineole, α-terpineol, β-terpineol and γ-terpineol.

[0109] As polyterpene resins, there can be mentioned: pinene resins, limonene resins, dipentene resins, and pinene / limonene resins, etc., which are made of the above-mentioned terpene compounds as raw materials. Among them, pinene resins are preferred from the perspective of easy polymerization reaction and the perspective of low price due to natural rosin as raw material. Pinene resins usually contain both α-pinene and β-pinene, which are isomers. Based on the difference in the components contained, they can be classified into β-pinene resins with β-pinene as the main component and α-pinene resins with α-pinene as the main component.

[0110] As aromatic modified terpene resins, there can be mentioned terpene phenol resins made from the above-mentioned terpene compounds and phenolic compounds, or terpene styrene resins made from the above-mentioned terpene compounds and styrene compounds. In addition, terpene phenol styrene resins made from the above-mentioned terpene compounds, phenolic compounds and styrene compounds can also be used. In addition, as phenolic compounds, for example, phenol, bisphenol A, cresol and xylenol can be mentioned. In addition, as styrene compounds, styrene and α-methylstyrene can be mentioned.

[0111] As the acrylic resin, styrene acrylic resins such as styrene acrylic resins obtained by copolymerizing an aromatic vinyl monomer component and an acrylic monomer component having a carboxyl group can be used. Among them, solvent-free carboxyl-containing styrene acrylic resins can be preferably used.

[0112] Solvent-free carboxyl-containing styrene acrylic (ester) resins refer to the following resins:

[0113] A (meth)acrylic acid (ester) resin (polymer) synthesized by a high temperature continuous polymerization method (high temperature continuous block polymerization method) (methods described in U.S. Patent No. 4,414,370, Japanese Patent Laid-Open No. 59-6207, Japanese Patent Laid-Open No. 5-58005, Japanese Patent Laid-Open No. 1-313522, U.S. Patent No. 5,010,166, East Asia Synthesis Research Annual Report TREND 2000 No. 3, pp. 42-45, etc.) without using a polymerization initiator, chain transfer agent, organic solvent, etc. as auxiliary raw materials as much as possible. In addition, in this specification, (meth)acrylic acid refers to methacrylic acid and acrylic acid.

[0114] Examples of acrylic monomer components constituting acrylic resins include (meth)acrylic acid, (meth)acrylic acid esters (alkyl esters, aryl esters, arylalkyl esters, etc., such as 2-ethylhexyl acrylate), (meth)acrylamide, (meth)acrylic acid derivatives such as (meth)acrylamide derivatives. (Meth)acrylic acid is a general term for acrylic acid and methacrylic acid.

[0115] Examples of the aromatic vinyl monomer component constituting the acrylic resin include aromatic vinyl monomers such as styrene, α-methylstyrene, vinyltoluene, vinylnaphthalene, divinylbenzene, trivinylbenzene, and divinylnaphthalene.

[0116] In addition, as the monomer component constituting the acrylic resin, other monomer components may be used together with (meth)acrylic acid or a (meth)acrylic acid derivative and an aromatic vinyl monomer.

[0117] From the viewpoint of blocking resistance, ozone resistance, and the like, the rubber composition for the outer rubber layer preferably contains an antioxidant.

[0118] The antioxidant is not particularly limited, and examples thereof include: naphthylamine antioxidants such as phenyl-α-naphthylamine; diphenylamine antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; p-phenylenediamine antioxidants such as N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and N,N'-di-2-naphthyl-p-phenylenediamine; quinoline antioxidants such as polymers of 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-tert-butyl-4-methylphenol and styrenated phenol; diphenol antioxidants, triphenol antioxidants, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane. Among them, p-phenylenediamine antioxidants and quinoline antioxidants are preferred, and polymers of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and 2,2,4-trimethyl-1,2-dihydroquinoline are more preferred. As commercially available products, for example, products of Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd. can be used.

[0119] In the rubber composition for the outer rubber layer, the content of the antioxidant is preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the rubber component. By making the content above the lower limit, there is a tendency to obtain sufficient ozone resistance. The content is preferably 7.0 parts by mass or less, more preferably 4.0 parts by mass or less. By making the content below the upper limit, there is a tendency to obtain a good tire appearance.

[0120] The rubber composition for the outer rubber layer preferably contains stearic acid. The content of stearic acid is preferably 0.5 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the rubber component.

[0121] As stearic acid, conventionally known stearic acid can be used. For example, products of NOF Corporation, NOF Corporation, Kao Corporation, Fujifilm Co., Ltd., Wako Pure Chemical Industries, Ltd., Chiba Fatty Acid Co., Ltd., etc. can be used.

[0122] The rubber composition for the outer rubber layer may contain wax, and the wax content is preferably 0.1 to 5.0 parts by mass, more preferably 0.5 to 3.0 parts by mass, based on 100 parts by mass of the rubber component.

[0123] There is no particular limitation on the wax, and examples thereof include: petroleum wax and natural wax; in addition, synthetic waxes obtained by purifying or chemically treating a variety of waxes may also be used. These waxes may be used alone or in combination of two or more. Examples of petroleum wax include paraffin wax and microcrystalline wax. As natural waxes, there is no particular limitation as long as they are waxes from resources other than petroleum; for example, examples thereof include: plant waxes such as candelilla wax, carnauba wax, wood wax, rice wax, and jojoba wax; animal waxes such as beeswax, lanolin, and spermaceti; mineral waxes such as ozokerite, ceresin, and petrolactam; and their purified products. As commercial products, for example, products of Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., etc. may be used. In addition, the wax content may be appropriately set from the perspectives of ozone resistance and cost.

[0124] The rubber composition for the outer rubber layer contains sulfur. In the rubber composition for the outer rubber layer, the sulfur content is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, further preferably 0.7 parts by mass or more, and particularly preferably 0.9 parts by mass or more, relative to 100 parts by mass of the rubber component. The content is preferably 5.0 parts by mass or less, more preferably 3.0 parts by mass or less, further preferably 2.0 parts by mass or less, and particularly preferably 1.8 parts by mass or less. By making the content within the above range, there is a tendency that good fuel efficiency is obtained while suppressing the decline of degradation over time.

[0125] Sulfur includes powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, and soluble sulfur commonly used in the rubber industry. Commercially available products include those of Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Co., Ltd., Nippon Senryu Industry Co., Ltd., and Hosoi Chemical Industry Co., Ltd. These may be used alone or in combination of two or more.

[0126] The rubber composition for the outer rubber layer preferably contains a vulcanization accelerator. In the rubber composition for the outer rubber layer, the content of the vulcanization accelerator is preferably 0.5 parts by mass or more, more preferably 2.0 parts by mass or more, further preferably 3.0 parts by mass or more, and particularly preferably 3.5 parts by mass or more, relative to 100 parts by mass of the rubber component. The content is preferably 10.0 parts by mass or less, more preferably 7.0 parts by mass or less, further preferably 6.0 parts by mass or less, and particularly preferably 5.0 parts by mass or less. By making the content within the above range, there is the following trend: while obtaining good low fuel consumption, the decline of degradation over the years can also be suppressed.

[0127] The type of the vulcanization accelerator is not particularly limited, and a commonly used vulcanization accelerator can be used. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, and N-cyclohexyl-2-benzothiazole sulfenamide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD), tetrabenzylthiuram disulfide (TBzTD), and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, N-tert-butyl-2-benzothiazolyl sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenylguanidine, di-o-tolylguanidine, and o-tolylbiguanide. These may be used alone or in combination of two or more. Among them, sulfenamide-based vulcanization accelerators and guanidine-based vulcanization accelerators are preferred.

[0128] In the rubber composition for the outer rubber layer, the content of sulfur and the vulcanization accelerator contained in the rubber composition for the outer rubber layer per 100 parts by mass of the rubber component preferably satisfies the following formula (2) from the viewpoint of low fuel consumption and suppression of aging degradation.

[0129]

[0130] The sulfur content contained in the rubber composition for the outer rubber layer relative to 100 parts by mass of the rubber component / the vulcanization accelerator content contained in the rubber composition for the outer rubber layer relative to 100 parts by mass of the rubber component is preferably ≤0.9, more preferably ≤0.7, and further preferably ≤0.5. The lower limit of the ratio is not particularly limited, but is preferably ≥0.1, more preferably ≥0.2, and further preferably ≥0.3.

[0131] In addition to the above-mentioned components, materials such as compounding agents commonly used in the tire industry (for example, mold release agents) may be appropriately mixed into the rubber composition for the outer rubber layer.

[0132] The rubber composition for the outer rubber layer is preferably used for the rubber layer (cap tread, etc.) that comes into direct contact with the road surface among two or more tread layers.

[0133] (Rubber composition for inner rubber layer)

[0134] The rubber composition for the inner rubber layer includes a rubber component and a zinc-containing compound. As the rubber component, for example, the rubber component described in the rubber composition for the outer rubber layer can be used. Among them, isoprene-based rubber and BR are preferably used.

[0135] From the viewpoint of low fuel consumption and suppression of aging degradation, the isoprene rubber content in 100% by mass of the rubber component in the rubber composition for the inner rubber layer is preferably 5% by mass or more, more preferably 30% by mass or more, and even more preferably 50% by mass or more. The upper limit of the content is not particularly limited, but is preferably 90% by mass or less, more preferably 75% by mass or less, and even more preferably 65% ​​by mass or less.

[0136] From the viewpoint of low fuel consumption and suppression of aging degradation, the BR content in 100% by mass of the rubber component in the rubber composition for the inner rubber layer is preferably 5% by mass or more, more preferably 25% by mass or more, and even more preferably 35% by mass or more. The upper limit of the content is not particularly limited, but is preferably 90% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less.

[0137] As the zinc-containing compound, for example, the zinc-containing compounds described in the rubber composition for the outer rubber layer can be used. Among them, zinc oxide and basic zinc carbonate can be used appropriately.

[0138] In the rubber composition for the inner rubber layer, the zinc content (the content calculated as zinc contained in the zinc-containing compound) is preferably 1.0 parts by mass or more, more preferably 1.5 parts by mass or more, further preferably 2.0 parts by mass or more, and particularly preferably 2.2 parts by mass or more, relative to 100 parts by mass of the rubber component. The upper limit of the content is preferably 4.0 parts by mass or less, more preferably 3.5 parts by mass or less, further preferably 3.0 parts by mass or less, and particularly preferably 2.8 parts by mass or less. By making the content within the above range, there is a tendency that good fuel efficiency is obtained while suppressing the decline of deterioration over time.

[0139] It is preferred to add silica to the rubber composition for the inner rubber layer. As silica, for example, in addition to the silica described in the rubber composition for the outer rubber layer, silica having an N2SA of less than 200 m 2 / g of silica.

[0140] In the rubber composition for the inner rubber layer, the content of silica is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, and further preferably 25 parts by mass or more, relative to 100 parts by mass of the rubber component. In addition, the content is preferably 150 parts by mass or less, more preferably 100 parts by mass or less, and further preferably 50 parts by mass or less.

[0141] When the rubber composition for the inner rubber layer contains silica, it is preferred to further contain a silane coupling agent. As the silane coupling agent, for example, the silane coupling agent described in the rubber composition for the outer rubber layer can be used, and the same content can be appropriately used.

[0142] The rubber composition for the inner rubber layer preferably contains carbon black. As the carbon black, for example, the carbon black described in the rubber composition for the outer rubber layer can be used.

[0143] In the rubber composition for the inner rubber layer, the content of carbon black is preferably 1 part by mass or more, more preferably 10 parts by mass or more, and further preferably 15 parts by mass or more, relative to 100 parts by mass of the rubber component. In addition, the content is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and further preferably 40 parts by mass or less.

[0144] The rubber composition for the inner rubber layer preferably contains: a liquid plasticizer (plasticizer that is liquid at 20°C) and a resin (resin that is solid at room temperature (25°C)). As the liquid plasticizer and the resin, for example, the liquid plasticizer and the resin described in the rubber composition for the outer rubber layer can be used appropriately. In particular, as the resin, a resin having an unsaturated bond is preferred, an aromatic vinyl polymer is more preferred, and an ethylene-propylene-styrene copolymer is further preferred.

[0145] In the rubber composition for the inner rubber layer, the content of the liquid plasticizer is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and further preferably 8 parts by mass or more, relative to 100 parts by mass of the rubber component. The upper limit of the content is not particularly limited, but is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and further preferably 15 parts by mass or less. By making the content within the above range, there is a tendency that good fuel efficiency is obtained while suppressing the decline of aging degradation.

[0146] In the rubber composition for the inner rubber layer, the content of the resin is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and further preferably 5 parts by mass or more, relative to 100 parts by mass of the rubber component. The upper limit of the content is not particularly limited, but is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and further preferably 15 parts by mass or less. By making the content within the above range, there is a tendency that good fuel efficiency is obtained while suppressing the decline of aging degradation.

[0147] The above-mentioned antioxidant, stearic acid, wax, sulfur, vulcanization accelerator, mold release agent and other materials may be appropriately added to the rubber composition for the inner rubber layer, and the proportions may be appropriately adjusted.

[0148] The rubber composition for the inner rubber layer can be applied to the rubber layer that does not come into direct contact with the road surface among two or more treads, and is preferably used in a base tread or the like.

[0149] The rubber composition for the outer rubber layer and the rubber composition for the inner rubber layer can be produced by a known method. For example, the rubber composition can be produced by kneading the above components using a rubber kneading device such as an open roll mill and a Banbury mixer, and then vulcanizing the components.

[0150] As the mixing conditions, in the basic kneading process of mixing additives other than the vulcanizing agent and the vulcanization accelerator, the mixing temperature is usually 50 to 200°C, preferably 80 to 190°C; the mixing time is usually 30 seconds to 30 minutes, preferably 1 minute to 30 minutes. In the final kneading process of mixing the vulcanizing agent and the vulcanization accelerator, the mixing temperature is usually below 100°C, preferably room temperature to 80°C. In addition, the composition mixed with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. As the vulcanization temperature, it is usually 120 to 200°C, preferably 140 to 180°C.

[0151] The tire can be manufactured by using the rubber composition for the outer rubber layer and the rubber composition for the inner rubber layer according to a conventional method. That is, in the unvulcanized stage, the rubber composition for the outer rubber layer and the rubber composition for the inner rubber layer, which are mixed with various components, are extruded and processed into the shapes of the cap tread, the base tread and other components, and then formed on a tire molding machine according to a conventional method together with other tire components to form an unvulcanized tire. In the vulcanizer, the unvulcanized tire is heated and pressurized to obtain a tire.

[0152] The tire outer diameter Dt and the tire cross-sectional width Wt of the above tire preferably satisfy the relationship of the following formula (I).

[0153]

[0154] In addition, the tire outer diameter (Dt) refers to the outer diameter of the tire when the tire is mounted on the applicable rim and adjusted to a no-load state. The tire cross-sectional width (Wt) refers to the straight-line distance between all sidewalls including patterns or text on the tire side when the tire is mounted on the applicable rim and adjusted to a no-load state, that is, the width obtained by subtracting the patterns and text on the tire side from the total width.

[0155] Specific examples of tire sizes that satisfy the above formula (I) include 145 / 60R18, 145 / 60R19, 155 / 55R18, 155 / 55R19, 155 / 70R17, 155 / 70R19, 165 / 55R20, 165 / 55R21, 165 / 60R19, 165 / 65R19, 165 / 70R18, 175 / 55R19, 175 / 55R20, 175 / 55R22, 175 / 60R18, 185 / 55R19, 185 / 60R20, 195 / 50R20, and 195 / 55R20.

[0156] Examples of tires include pneumatic tires and airless (solid) tires, among which pneumatic tires are preferred. Tires can be used for heavy-duty tires such as passenger car tires, large passenger car tires, large SUV tires, truck tires, and bus tires, light truck tires, two-wheeled vehicle tires, and racing tires (high-performance tires). In addition, winter tires (studless tires, snow tires, and studded tires, etc.)

[0157] Among them, it is particularly preferred to apply it to a pneumatic tire for a passenger car. In addition, the pneumatic tire for a passenger car preferably satisfies the above formula (I). This is because the pneumatic tire for a passenger car that satisfies formula (1) has a tendency to use low fuel consumption and resistance to falling off as a subject.

[0158] [Example]

[0159] The present invention is specifically described based on the examples, but the present invention is not limited to these examples.

[0160] Hereinafter, various chemicals used in Examples and Comparative Examples will be described.

[0161] NR:RSS#3

[0162] SBR1: modified SBR synthesized in the following Production Example 1 (styrene content: 25 mass %; vinyl content: 60 mass %; Mw: 300,000)

[0163] SBR2: modified SBR synthesized in the following Production Example 2 (styrene content: 35% by mass; vinyl content: 50% by mass; Mw: 600,000)

[0164] BR: BR150B manufactured by Ube Industries, Ltd. (cis form: 95% by mass or more)

[0165] Carbon black: SHOBLACK N220 (N2SA: 112m 2 / g)

[0166] Silica 1: 9100GR (N2SA: 235m 2 / g)

[0167] Silica 2: Zeosil 1115MP (N2SA: 115m 2 / g)

[0168] Silane coupling agent 1: Si266 (bis(3-triethoxysilylpropyl) disulfide) manufactured by Evonik Degussa

[0169] Silane coupling agent 2: NXT-Z45 manufactured by Momentive (copolymer of bonding unit A and bonding unit B (bonding unit A: 55 mol %; bonding unit B: 45 mol %)

[0170] Resin 1: Sylvatraxx 4401 manufactured by Arizona Chemical (copolymer of α-methylstyrene and styrene, softening point 85°C)

[0171] Resin 2: 40MS manufactured by Struktol (ethylene propylene styrene copolymer, softening point 78° C., EP content: 82% by mass)

[0172] Oil: Diana process oil NH-70S (aromatic oil) manufactured by Idemitsu Kosan Co., Ltd.

[0173] Wax: Ozoace 0355 manufactured by Nippon Seiwa Co., Ltd.

[0174] Stearic acid: TSUBAKI stearic acid manufactured by NOF Corporation

[0175] Zinc oxide: Silver Ridge R manufactured by Toho Zinc Co., Ltd.

[0176] Basic zinc carbonate: Zinc carbonate ("SEDOAEN") from Shodo Chemical Industry Co., Ltd.

[0177] Antioxidant 1: NOCRAC 6C (N-(1,3-dimethylbutyl) N'-phenyl-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0178] Antioxidant 2: NOCRAC RD (poly(2,2,4-trimethyl-1,2-dihydroquinoline)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0179] Sulfur: HK-200-5 manufactured by Hosoi Chemical Industry Co., Ltd. (powdered sulfur containing 5% oil)

[0180] Vulcanization accelerator 1: NOCCELER CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0181] Vulcanization accelerator 2: NOCCELER D (1,3-diphenylguanidine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0182] (Production Example 1)

[0183] Cyclohexane, tetrahydrofuran, styrene and 1,3-butadiene were placed in an autoclave reactor purged with nitrogen. After adjusting the temperature of the contents of the reactor to 20°C, n-butyl lithium was added to initiate polymerization. The polymerization was carried out under adiabatic conditions, with the maximum temperature reaching 85°C. When the polymerization conversion rate reached 99%, 1,3-butadiene was added, and after further polymerization for 5 minutes, N-(3-dimethylaminopropyl)acrylamide as a modifier was added to react. After the polymerization reaction was completed, 2,6-di-tert-butyl-p-cresol was added. Next, the solvent was removed by steam stripping, and dried by a hot roller adjusted to a temperature of 110°C to obtain SBR1.

[0184] (Production Example 2)

[0185] Cyclohexane, tetrahydrofuran, styrene and 1,3-butadiene were placed in an autoclave reactor purged with nitrogen. After adjusting the temperature of the contents of the reactor to 20°C, n-butyl lithium was added to initiate polymerization. The polymerization was carried out under adiabatic conditions, and the maximum temperature reached 85°C. When the polymerization conversion rate reached 99%, 1,3-butadiene was added, and after further polymerization for 5 minutes, 3-diethylaminopropyltriethoxysilane was added as a modifier to react. After the polymerization reaction was completed, 2,6-di-tert-butyl-p-cresol was added. Next, the solvent was removed by steam stripping, and dried by a hot roller adjusted to a temperature of 110°C to obtain SBR2.

[0186] (SBR Analysis)

[0187] The structure identification of SBR (determination of styrene content and vinyl content) was performed using a JNM-ECA series device manufactured by JEOL Ltd. For the determination, 0.1 g of the polymer was dissolved in 15 ml of toluene, slowly poured into 30 ml of methanol for reprecipitation, and then dried under reduced pressure before the determination.

[0188] <Examples and Comparative Examples>

[0189] The rubber composition for cap tread and the rubber composition for base tread described in Table 1 were kneaded in a Banbury mixer to obtain respective kneaded products. The obtained unvulcanized rubber composition (rubber composition for cap tread) was press-vulcanized at 170° C. for 12 minutes in a 0.5 mm thick mold to obtain a vulcanized rubber composition for cap tread.

[0190] In addition, each of the obtained unvulcanized rubber compositions was formed into a tread surface and a tread base shape, and laminated together with other tire components on a tire forming machine, and press-vulcanized at 150°C for 30 minutes to obtain a test tire (tire size 175 / 60R18).

[0191] The following evaluations were performed using the obtained vulcanized rubber composition for cap tread and the test tire. The results are shown in Table 1.

[0192] <Low fuel efficiency>

[0193] The rolling resistance of the test tire when running under the conditions of rim (18×5JJ), internal pressure (260kPa), load (3.43kN), and speed (80km / h) was measured using a rolling resistance tester, and the rolling resistance was expressed as an index. The larger the index, the better the fuel efficiency. In addition, the index is expressed by the following formula.

[0194] (Fuel efficiency) = (tire rolling resistance of Comparative Example 1) / (tire rolling resistance of each formulation) × 100

[0195] <Destruction Characteristics>

[0196] A No. 3 dumbbell-shaped test piece was prepared from a vulcanized rubber composition for a tread (vulcanized rubber composition), and a tensile test was performed at a tensile speed of 500 mm / min in accordance with JIS K6251 "Vulcanized rubber and thermoplastic rubber - Method for obtaining tensile properties". The initial elongation at break EB (%) at 23°C ± 2°C and the elongation at break EB (%) after the following degradation conditions were measured, and the EB maintenance rate after degradation (%) was calculated (=EB after degradation / EB before degradation × 100).

[0197] (Deteriorated conditions)

[0198] The vulcanized rubber composition for cap tread was thermally degraded in an oven (80°C, 168 hours).

[0199] The EB maintenance rate after degradation of Comparative Example 1 was taken as 100, and the respective formulations were indexed according to the following formula. A larger index indicates better degradation inhibition.

[0200] (EB maintenance rate after degradation (index)) = (EB maintenance rate after degradation of each formulation / EB maintenance rate after degradation of Comparative Example 1) × 100

[0201] <Block drop resistance>

[0202] The test tire was assembled on a rim (18×5JJ), the air pressure was adjusted to 230 kPa, and the tire was installed on the test vehicle. After driving 5,000 km on an unpaved road, the tire was visually observed and the total area of ​​external injuries (defects or groove-shaped scars of 1 square mm or more on the tread surface) was measured. The evaluation results were indexed by the formula of 100×(total area of ​​comparative example 1+1) / (total area of ​​each example+1). The larger the index, the higher the resistance to block falling.

[0203]

Table 1

[0204] Tread and base tread

[0205]

[0206] According to Table 1, for a tire having a rubber composition for an outer rubber layer (rubber composition for a tread surface) comprising a specified formulation, a tread surface layer and a base layer of a rubber composition for an inner rubber layer and satisfying the above formula (1), the comprehensive performance of low fuel consumption, degradation inhibition and chipping resistance (expressed as the sum of the three indexes of low fuel consumption, EB maintenance rate after degradation (deterioration inhibition) and chipping resistance) is significantly improved.

Claims

1. A tire having two or more treads, wherein two adjacent treads in the radial direction of the tire are: The outer rubber layer on the outer side in the radial direction of the tire is formed by a rubber composition for an outer rubber layer, wherein the rubber composition for the outer rubber layer comprises: a rubber component containing 25% by mass or more and 40% by mass or less and 55% by mass of an isoprene-based rubber and styrene-butadiene rubber and butadiene rubber, and a nitrogen adsorption specific surface area of ​​200 m 2 / g or more of silicon dioxide, sulfur, a resin having an unsaturated bond, and a zinc-containing compound selected from zinc oxide and basic zinc carbonate; In the rubber composition for the outer rubber layer, the content of zinc element is 1.4 parts by mass or more and 2.5 parts by mass or less relative to 100 parts by mass of the rubber component; The inner rubber layer on the inner side in the radial direction of the tire is formed of a rubber composition for an inner rubber layer, wherein the rubber composition for the inner rubber layer comprises: a rubber component containing 50 mass % to 65 mass % of isoprene-based rubber and 35 mass % to 50 mass % of butadiene rubber, silica, carbon black, sulfur and zinc oxide; In the rubber composition for the inner rubber layer, the content of silica is 25 parts by mass or more and 50 parts by mass or less relative to 100 parts by mass of the rubber component; The tire meets the following requirements: 0.20≦Total vinyl content of styrene-butadiene rubber contained in the rubber composition for the outer rubber layer / nitrogen adsorption specific surface area per 100 parts by mass of the rubber component contained in the rubber composition for the outer rubber layer is 200 m 2 / g or above with a silica content of ≤0.45, and 0.50≦The content of zinc element contained in the rubber composition for the outer rubber layer relative to 100 parts by mass of the rubber component / the content of zinc element contained in the rubber composition for the inner rubber layer relative to 100 parts by mass of the rubber component≦0.

90.

2. The tire according to claim 1, wherein: The tire satisfies the following formula: 。 3. The tire according to claim 1, wherein: The tire satisfies the following formula (2): 。 4. The tire according to any one of claims 1 to 3, wherein The rubber composition for the inner rubber layer includes a resin having an unsaturated bond.

5. The tire according to any one of claims 1 to 3, wherein The rubber composition for the outer rubber layer includes a mercapto-based silane coupling agent.

6. The tire according to any one of claims 1 to 3, wherein: The rubber composition for the outer rubber layer has a nitrogen adsorption specific surface area of ​​200 m2 relative to 100 parts by mass of the rubber component. 2 The silica content of MgO2 / g or more is 5 to 170 parts by mass.

7. The tire according to any one of claims 1 to 3, wherein The tire meets the following requirements: 0.20≦Total vinyl content of styrene-butadiene rubber contained in the rubber composition for the outer rubber layer / nitrogen adsorption specific surface area per 100 parts by mass of the rubber component contained in the rubber composition for the outer rubber layer is 200 m 2 / g or above silica content ≤0.

30.

8. The tire according to any one of claims 1 to 3, wherein The tire is a pneumatic tire for passenger cars.

9. The tire according to any one of claims 1 to 3, wherein The tire outer diameter Dt and the tire cross-sectional width Wt satisfy the following relationship (I): 。

Citation Information

Patent Citations

  • Catalytic lumpy production of cyclic ester modified acrylic polymer

    JP1989313522A

  • Process for continuous bulk copolymerization of vinyl monomers

    US4414370A

  • Process and apparatus for producing polyol polymers and polyol polymers so produced

    US5010166A

  • Rubber composition for tread, and pneumatic tire

    CN103804731A

  • Tread rubber composition and pneumatic tire

    CN106459514A