Glass plate and method for manufacturing the same

By controlling the density of Si-OH groups on the first main surface of the glass plate and grinding it with calcium carbonate slurry, the problem of stripping and electrification is solved, ensuring the stability of electronic devices and component quality, and avoiding electrostatic damage.

CN113443830BActive Publication Date: 2024-10-18AGC INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202110324192.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-26
Publication Date
2024-10-18
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

When forming electronic components on a glass plate, the phenomenon of peeling off charging may lead to electrostatic damage, especially in highly integrated electronic devices. The existing roughening treatment method may have adverse effects on the second main surface, affecting the formation and operation of the device. .

Method used

By controlling the density of Si-OH groups on the first main surface of the glass plate, grinding it with a slurry containing calcium carbonate and cleaning it with an alkaline solution, it is ensured that the first main surface is smooth and less likely to be charged, thereby suppressing stripping and charging, and avoiding damage to the second main surface. The electronic components on the second main surface cause electrostatic damage.

Benefits of technology

It is possible to suppress the peeling charge when the glass plate is peeled off from the adsorption table without performing roughening treatment, prevent electrostatic damage, have no adverse effects on the formation and operation of electronic components, and improve the stability of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113443830B_ABST
    Figure CN113443830B_ABST
Patent Text Reader

Abstract

The present invention relates to a glass plate and a method for manufacturing the same. The present invention relates to a glass plate having a first main surface and a second main surface opposite to the first main surface, the second main surface being a side on which an electronic component is formed, wherein the surface Si-OH group density of the first main surface derived using a specific calculation method is 0 (pieces / cm 2 ) and above 8.7×10 14 (pcs / cm 2 ) below, expressed as mass % based on oxides, the glass composition of the glass plate contains SiO2: 35% to 73%, Al2O3: 5% to 35%, B2O3: 0 to 30%, MgO: 0 to 20%, CaO: 0 to 30%, SrO: 0 to 30%, BaO: 0 to 40%, and the total of MgO, CaO, SrO and BaO: 1% to 55%, and substantially does not contain alkali metal oxides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a glass plate and a method for producing the same, and in particular to a glass plate suitable for use as a substrate for an electronic device and a method for producing the same. Background Art

[0002] In electronic devices and semiconductor packages, electronic components (electronic parts) such as metal wiring, transparent electrodes, semiconductor elements, and light-emitting elements, flexible resin substrates such as polyimide, and RDL (redistribution layer) are sometimes formed on a glass plate. Examples of such electronic devices include FPD (flat panel display), flat antennas using liquid crystal technology, etc. FPDs include liquid crystal displays, organic EL (electroluminescent) displays, and micro LED displays. In addition, as semiconductor packages, fan-out semiconductor packages can be listed.

[0003] As a specific example, in a liquid crystal display, a transparent electrode, a TFT (Thin Film Transistor), a color filter, and the like are formed on a glass plate.

[0004] For forming electronic components on glass sheets, for example Figure 1 As shown, the second main surface 1b is subjected to vacuum adsorption while the first main surface 1a of the glass plate 1 is fixed to the adsorption table 2. However, when the glass plate is peeled off from the adsorption table, the glass plate is charged, which may cause electrostatic damage to the wiring due to electrostatic discharge (ESD). In recent years, the integration of electronic devices has increased significantly, so the width and spacing of the wiring have been miniaturized, and the possibility of adverse conditions caused by ESD has become higher. In FPD, in particular, with the high integration of TFTs, problems such as TFT destruction and display quality impairment are likely to become more obvious. In addition, whether TFTs, wiring, etc. are directly formed on the second main surface of the glass plate, or polyimide resin is applied to the second main surface and then TFTs, wiring, etc. are formed, the possibility of electrostatic damage to the wiring caused by the above-mentioned ESD is the same.

[0005] In this regard, a method is adopted in which the first main surface of the glass plate attached to the adsorption platform is roughened to reduce the contact area between the glass plate and the adsorption platform, thereby preventing the glass plate from peeling and charging.

[0006] For example, Patent Document 1 discloses a glass substrate for a display, wherein the first surface has a plurality of openings through a glass etching process, and the average opening area of ​​the holes is 1.70×10 4 (nm 2) or less, the total opening area of ​​the above holes is 6.00×10 6 (nm 2 / 25μm 2 ) or more. In addition, as a glass etching process, an etching method using a gas containing hydrogen fluoride is disclosed.

[0007] Patent Document 2 discloses a glass plate which is polished using cerium oxide as a polishing material and has a maximum valley depth Rv (JIS B 0601: 2013) of 3.0 nm on the first surface. <Rv<5.0nm。

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: International Publication No. 2017 / 065138

[0011] Patent Document 2: Japanese Patent Application Publication No. 2015-131751 Summary of the invention

[0012] Problems to be solved by the invention

[0013] However, when the first main surface is roughened, the second main surface opposite thereto may also be roughened in the same manner. Specifically, since the gas and abrasive grains used for the roughening process go around at least the peripheral portion of the second main surface, the peripheral portion is also roughened.

[0014] The second main surface is the surface on which the electronic component is to be formed. Therefore, since at least a part of the second main surface is roughened, there is a possibility that the formation and operation of the device represented by the electronic component may be adversely affected.

[0015] Therefore, an object of the present invention is to provide a glass plate in which the occurrence of peeling electrification is suppressed without roughening the first main surface, particularly a glass substrate suitable for use as a substrate for electronic devices, and a method for producing the glass plate.

[0016] Means used to solve problems

[0017] That is, the present invention relates to the following [1] to

[12] .

[0018] [1] A glass plate having a first main surface and a second main surface opposite to the first main surface, the second main surface being a side on which an electronic component is formed, wherein:

[0019] The surface Si-OH group density of the first main surface derived by the following calculation method is 0 (groups / cm 2 ) and above 8.7×1014 (pcs / cm 2 )the following,

[0020] Expressed as mass % based on oxides, the glass composition of the glass plate contains: SiO2: 35% to 73%, Al2O3: 5% to 35%, B2O3: 0 to 30%, MgO: 0 to 20%, CaO: 0 to 30%, SrO: 0 to 30%, BaO: 0 to 40%, and the total of MgO, CaO, SrO and BaO: 1% to 55%, and substantially contains no alkali metal oxides.

[0021] <Calculation method>

[0022] (i) For the first main surface of the glass plate as a sample, the atomic concentrations (atomic %) of Si, Mg, Ca, Sr, Ba, Al and B were measured by X-ray photoelectron spectroscopy with the detection angle between the sample and the detector set to 15°, and the surface Si-OR bond number (SiOR) normalized by the atomic concentration of Si was calculated by the following formula (1): surf ). R refers to Mg, Ca, Sr, Ba, Al and B.

[0023] S O surf =2×(S Mg +S Ca +S Sr +S Ba )+3×(S Al +S B )…(1)

[0024] In the formula, S Mg , S Ca , S Sr , S Ba , S Al and S B Each of them means a value obtained by normalizing the atomic concentration of Mg, Ca, Sr, Ba, Al and B by the atomic concentration of Si.

[0025] (ii) Next, for the first major surface, use C 60 The glass plate was cut in the depth direction by ion sputtering to expose the inside of the glass plate. The atomic concentrations (atomic %) of Si, Mg, Ca, Sr, Ba, Al and B were measured for the inside of the glass plate by X-ray photoelectron spectroscopy with a detection angle of 75°. The number of internal Si-OR bonds (SiOR) normalized by the atomic concentration of Si was calculated by the following formula (2): bulk ).

[0026] S O bulk =2×(B Mg+B Ca +B Sr +B Ba )+3×(B Al +B B )…(2)

[0027] In the formula, B Mg , B Ca , B Sr , B Ba , B Al and B B Each of them means a value obtained by normalizing the atomic concentration of Mg, Ca, Sr, Ba, Al and B by the atomic concentration of Si.

[0028] (iii) using the glass density, the Si concentration in the glass plate, and the number of Si-OR bonds on the surface calculated in (i) above (SiOR surf ) and the internal Si-OR bond number (SiOR bulk ), the surface Si-OH group density (SiOH surf )(pcs / cm 2 ).

[0029] D Si =(D×Si mass% ×6.02×10 23 ) / (100×28.09)…(3)

[0030] D Si-surf =(D Si ) 2 / 3 …(4)

[0031] SiOH surf =(SiOR bulk -SiOR surf )×D Si-surf …(5)

[0032] Where D Si Refers to the Si atom density in the glass plate (a / cm 3 ), D refers to the glass density (g / cm 3 ), Si mass% refers to the Si concentration (mass %) in the glass plate, D Si-surf Refers to the surface Si atom density (a / cm 2 ).

[0033] [2] The glass plate according to [1], wherein the surface Si-OH group density is 7.6×10 14 (pcs / cm 2)the following.

[0034] [3] The glass plate according to [1] or [2], wherein the surface Si-OH group density is 6.1×10 14 (pcs / cm 2 )the following.

[0035] [4] The glass plate according to any one of [1] to [3] above, wherein an absolute value of a maximum valley depth Rv of the first main surface is 3.0 nm or less.

[0036] [5] The glass plate according to any one of [1] to [4] above, wherein the glass plate has a thickness of 0.1 mm to 1.0 mm.

[0037] [6] The glass plate according to any one of [1] to [5] above, wherein the glass plate is rectangular in which at least one side has a length of 2500 mm or more.

[0038] [7] The glass plate according to any one of [1] to [6] above, wherein the glass plate is used as a substrate for an electronic device.

[0039] [8] The glass plate according to any one of [1] to [7] above, wherein the glass plate is used as a substrate for a display.

[0040] [9] The glass plate according to any one of [1] to [7] above, wherein the glass plate is used as a carrier substrate for manufacturing a flexible display.

[0041]

[10] The glass plate according to any one of [1] to [7] above, wherein the glass plate is used as a carrier substrate for semiconductor packaging.

[0042]

[11] A method for producing a glass plate, which is a method for producing the glass plate described in any one of [1] to

[10] above, wherein:

[0043] The method for manufacturing a glass plate includes the step of polishing a first main surface opposite to a second main surface on which an electronic component is to be formed by 1 nm or more using a slurry containing calcium carbonate.

[0044]

[12] The method for producing a glass plate according to

[11] above, wherein after the polishing step, the first main surface is cleaned using an alkaline solution.

[0045] Effects of the Invention

[0046] According to the present invention, a glass plate that is not prone to peeling electrification when peeling from an adsorption platform can be obtained without roughening treatment. Therefore, when the glass plate is used as a substrate for electronic devices, electrostatic damage can be suppressed. In addition, it is also expected to prevent adverse effects on the formation and operation of devices represented by electronic components. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is a schematic cross-sectional view showing the positional relationship between a glass plate and an adsorption stage when an electronic component is formed on the glass plate.

[0048] Figure 2 This is a graph showing the relationship between the surface Si-OH group density and the delta charge potential for the glass plates of Examples 1 to 7.

[0049] Description of symbols

[0050] 1 Glass Pane

[0051] 1a First main surface

[0052] 1b Second main surface

[0053] 2 Adsorption table DETAILED DESCRIPTION

[0054] Hereinafter, the present invention will be described in detail, but the present invention is not limited to the following embodiments, and can be arbitrarily deformed and implemented without departing from the scope of the gist of the present invention. In addition, the " to " representing a numerical range is used to include the numerical value recorded before and after it as the meaning of the lower limit and the upper limit.

[0055] Unless otherwise specified, the content of each component representing the glass composition is expressed as mass % based on oxides.

[0056] [glass plate]

[0057] The glass plate of this embodiment has a first main surface and a second main surface opposite to the first main surface. The surface Si-OH group density of the first main surface is 0 (pieces / cm 2 ) and above 8.7×10 14 (pcs / cm 2 )the following.

[0058] When the glass plate is a substrate for electronic devices, the first main surface of the glass plate is brought into contact with the adsorption stage and adsorbed, and electronic components such as wiring are formed on the second main surface. Then, the glass plate is peeled off from the adsorption stage and provided for the next manufacturing process of the electronic device. That is, when the glass plate is used as a substrate for electronic devices, the first main surface is the side in contact with the adsorption stage, and the second main surface is the side where the electronic components are formed. When the electronic device is a liquid crystal display, the first main surface is the polarizer side, and the second main surface is the TFT side.

[0059] The present invention has conducted in-depth research on suppressing the peeling charge when the glass plate is peeled off from the adsorption platform. As a result, it was found that the surface Si-OH group (silanol group) density of the first main surface of the glass plate is related to the charged potential of the second main surface. When the surface Si-OH group density of the first main surface is low, the absolute value of the charged potential of the second main surface is small, which can suppress the electrostatic damage (static damage) of the wiring caused by ESD. Although the details are not clear, it is speculated as follows. It should be noted that the charged potential is an indicator of the ease of charging, and the closer it is to 0, the less likely it is to be charged.

[0060] Due to the structure of the measuring device, the measurement of the charge potential of the first main surface when the glass plate is peeled off from the adsorption table cannot be implemented. However, in the present invention, the second main surface of the glass plate is negatively (minus) charged, so it is inferred that the first main surface is positively (plus) charged. This is based on dielectric polarization. In addition, from the same point of view, it is inferred that the charge potential of the first main surface is related to the charge potential of the second main surface. If the positive (plus) charge potential of the first main surface is large, the negative (minus) charge potential of the second main surface is also large.

[0061] Furthermore, according to the triboelectric charging sequence, the glass plate is a material that is extremely easily charged positively (plus). Therefore, even if the triboelectric charging sequence is considered, it is estimated that the first main surface is charged positively (plus) and the adsorption base made of stainless steel (SUS) is charged negatively (minus).

[0062] When considering the peeling charge of different types of metals, it is speculated that when the metals are brought into contact with each other, the electrons move from the metal with a small work function to the metal with a large work function, which is the cause of the charge. That is, it is believed that the metal with a small work function is positively charged (plus), and the metal with a large work function is negatively charged (minus). The greater the difference between these work functions, the greater the charge potential of each of the two. When studying the glass plate in consideration of the above, it is difficult to define the work function of the insulator. However, it can at least be speculated that if the work function of the first main surface of the glass plate is large, the movement of electrons from the glass plate to the adsorption platform is suppressed, or a force similar to it is exerted, so that the first main surface of the glass plate is not easy to be positively charged (plus).

[0063] In order to increase the work function of the first main surface of the glass plate, the inventors focused on the amount of adsorbed water. This is because it is reported that for TiO2 and Cu(In,Ga)Se2, the work function decreases by increasing the amount of adsorbed water. The higher the surface Si-OH group density of the first main surface of the glass plate, the more it will combine with water molecules in the air, resulting in an increase in the amount of adsorbed water. If it is assumed that the glass plate also has the same tendency as TiO2, etc., the work function decreases by increasing the amount of adsorbed water.

[0064] That is, the lower the surface Si-OH group density of the first main surface of the glass plate, the less the amount of adsorbed water and the greater the work function. As a result, when peeling off from the adsorption platform, the first main surface of the glass plate is not easily positively charged (plus). Moreover, based on the dielectric polarization, it is inferred that the charged potential of the first main surface is associated with the charged potential of the second main surface, and the second main surface is not easily negatively charged (minus).

[0065] If the surface Si-OH group density of the first main surface of the glass plate is 8.7×10 14 (pcs / cm 2 ) or less, the peeling charge during peeling from the adsorption platform can be fully suppressed, and the electrostatic damage of the electronic components formed on the second main surface can be suppressed. The surface Si-OH group density is preferably 7.6×10 14 (pcs / cm 2 ) or less, more preferably 7.1×10 14 (pcs / cm 2 ) or less, and more preferably 6.6×10 14 (pcs / cm 2 ) or less, and more preferably 6.1×10 14 (pcs / cm 2 ) or less, particularly preferably 5.6×10 14 (pcs / cm 2 ) or less. In addition, the surface Si-OH group density is 0 (pieces / cm 2 ) or more, and the lower the value, the better. However, considering the load of the grinding process using a slurry containing calcium carbonate, the lower limit is, for example, 4.0×10 14 (pcs / cm 2 )above.

[0066] In this specification, the surface Si—OH group density of the main surface of the glass plate is a value derived by the following calculation methods (i) to (iii) using the analysis results using X-ray photoelectron spectroscopy (XPS).

[0067] <Calculation method>

[0068] (i) With respect to the first main surface of the glass plate as a sample, the atomic concentrations (atomic %) of Si, Mg, Ca, Sr, Ba, Al and B were measured by X-ray photoelectron spectroscopy with the detection angle between the sample and the detector set to 15°, and the number of Si-OR bonds on the surface normalized by the atomic concentration of Si (SiOR) was calculated by the following formula (1): surf ). R refers to Mg, Ca, Sr, Ba, Al and B.

[0069] S O surf =2×(S Mg +S Ca +S Sr +S Ba )+3×(S Al +S B )…(1)

[0070] In the formula, S Mg , S Ca , S Sr , S Ba , S Al and S B Each of them means a value obtained by normalizing the atomic concentration of Mg, Ca, Sr, Ba, Al and B by the atomic concentration of Si.

[0071] In X-ray photoelectron spectroscopy, the information depth can be adjusted by changing the detection angle. The smaller the detection angle, the shallower the information depth. That is, in the above (i), by setting the detection angle to 15°, the concentration of each atom in the extremely shallow surface layer of the first main surface of the glass plate is measured.

[0072] The atomic concentrations of Si, Mg, Ca, Sr, Ba, Al and B were measured, and then the atomic concentrations of Mg, Ca, Sr, Ba, Al and B were divided by the atomic concentration of Si to obtain the atomic concentrations of S, respectively. Mg , S Ca , S Sr , S Ba , S Al and S B The atomic concentrations shown are values ​​normalized by the atomic concentration of Si.

[0073] In formula (1), the sum of the values ​​obtained by normalizing the atomic concentration of each element by the atomic concentration of Si and multiplying the value by a coefficient of 2 or 3 is taken as the surface Si-OR bond number (SiOR surf ). The coefficient of 2 or 3 is a value corresponding to the valence of each element. The coefficient is explained below.

[0074] Among the above elements, for example, as a divalent Mg, one of the states in which it exists in the glass can be -Si-O-Mg-O-Si-, etc., in which it is bonded to Si via two O atoms. Similarly, Ca, Sr, and Ba are also divalent, and can be bonded to Si via two O atoms. In addition, Al and B are trivalent, and for convenience, they are treated as being bonded to Si via three O atoms. These valence numbers are multiplied by the normalized atomic concentrations, and the sum of their values ​​is the surface Si-OR bond number (SiOR) calculated by formula (1). surf ).

[0075] (ii) Next, for the first major surface, use C 60 The glass plate was cut in the depth direction by ion sputtering to expose the inside of the glass plate. The atomic concentrations (atomic %) of Si, Mg, Ca, Sr, Ba, Al and B were measured for the inside of the glass plate by X-ray photoelectron spectroscopy with a detection angle of 75°. The number of internal Si-OR bonds (SiOR) normalized by the atomic concentration of Si was calculated by the following formula (2): bulk ).

[0076] S O bulk =2×(B Mg +B Ca +B Sr +B Ba )+3×(B Al +B B )…(2)

[0077] In the formula, B Mg , B Ca , B Sr , B Ba , B Al and B B Each of them means a value obtained by normalizing the atomic concentration of Mg, Ca, Sr, Ba, Al and B by the atomic concentration of Si.

[0078] In C 60 In ion sputtering, the main surface of the glass plate is irradiated with C 60 The ions cause a phenomenon of removing atoms on the surface such as sputtering evaporation. As a result, the glass plate is cut in the depth direction to expose the inside of the glass plate, and the concentration of each atom inside the glass plate can be measured.

[0079] Specifically, in C 60 The atomic concentrations of Si, Mg, Ca, Sr, Ba, Al, and B were measured multiple times while ion sputtering. Then, it was confirmed that the values ​​of the measured atomic concentrations were constant in the depth direction.

[0080] Generally, if the composition of aluminosilicate glass does not contain alkali metal oxides substantially, the value of each atomic concentration is constant in the depth direction within a depth region of 300nm or less (SiO2 conversion depth). If the value of each atomic concentration is not constant in the depth direction due to the depth exceeding 300nm, the glass plate may be ground by several μm and C 60 Ion sputtering. It should be noted that the SiO2 conversion depth is based on C 60 The depth of the SiO2 film calculated from the sputtering rate (nm / min) of the ion sputtered SiO2 film is 60 The sputtering rate (nm / min) of the SiO 2 film by ion sputtering was calculated using a thermal oxide film (SiO 2 film) with a known film thickness formed on a silicon wafer.

[0081] By C 60 The main surface of the glass plate was cut by ion sputtering, and the atomic concentrations of Si, Mg, Ca, Sr, Ba, Al and B inside the glass plate were measured. In the above (ii), the detection angle was set to 75° to deepen the information depth, and the C generated in the extremely shallow surface layer was 60 The influence of composition changes due to ion sputtering is suppressed to a minimum, and the concentration of each atom inside the glass plate is obtained with high accuracy.

[0082] After measuring the atomic concentrations of Si, Mg, Ca, Sr, Ba, Al and B, the atomic concentrations of Mg, Ca, Sr, Ba, Al and B were divided by the atomic concentration of Si to obtain the atomic concentrations of B, Mg , B Ca , B Sr , B Ba , B Al and B B The atomic concentrations shown are values ​​normalized by the atomic concentration of Si.

[0083] Then, similarly to the above (i), the valence of each element is multiplied, and the sum of these values ​​is the internal Si-OR bond number (SiOR bulk ).

[0084] (iii) using the glass density, the Si concentration in the glass plate, and the number of Si-OR bonds on the surface calculated in (i) above (SiOR surf ) and the internal Si-OR bond number (SiOR bulk ), the surface Si-OH group density (SiOH surf )(pcs / cm 2 ).

[0085] DSi =(D×Si mass% ×6.02×10 23 ) / (100×28.09)…(3)

[0086] D Si-surf =(D Si ) 2 / 3 …(4)

[0087] SiOH surf =(SiOR bulk -SiOR surf )×D Si-surf …(5)

[0088] Where D Si Refers to the Si atom density in the glass plate (a / cm 3 ), D refers to the glass density (g / cm 3 ), Si mass% refers to the Si concentration (mass %) in the glass plate, D Si-surf Refers to the surface Si atom density (a / cm 2 ) It should be noted that the Si concentration in the glass plate refers to a value expressed in mass % on an atomic basis.

[0089] Glass density (D) (g / cm 3 ) is a value obtained according to JIS Z 8807:2012. In addition, the Si concentration in the glass plate (Si mass% ) (mass %) is a value determined in accordance with JIS R 3105:1995.

[0090] In the above formula (3), the glass density (D) is multiplied by the Si concentration in the glass plate / 100 (Si mass% / 100) and Avogadro's constant, and divided by the atomic weight of Si 28.09 (g / mol), the Si atomic density in the glass plate (D Si )(pcs / cm 3 ).

[0091] In the above formula (4), the Si atom density (D Si )(pcs / cm 3 ) is raised to the power of 2 / 3, reducing the dimension from three dimensions to two dimensions, and is converted into the surface Si atom density of the glass plate (D Si-surf )(pcs / cm 2 ).

[0092] Then, in formula (5), the number of internal Si-OR bonds (SiOR bulk) and the number of Si-OR bonds on the surface (SiOR surf Taking Mg among Mg, Ca, Sr, Ba, Al and B as an example, the following is explained.

[0093] It is equivalent to finding: through a Mg 2+ and two H + An ion exchange reaction occurs, and the state of -Si-O-Mg-O-Si- in the main surface of the glass plate changes to -Si-OH+Mg 2+ The number of surface Si-OH groups generated when +HO-Si- is given as a value relative to the number of Si atoms.

[0094] The sum of the above numbers of each element is multiplied by the surface Si atom density (D Si-surf )(pcs / cm 2 ), and thus the number of Si-OH groups per unit area on the main surface of the glass plate, i.e., the surface Si-OH group density (number / cm 2 ).

[0095] The glass plate of this embodiment can suppress the occurrence of peeling electrification due to the low density of Si-OH groups on the surface. Therefore, roughening treatment is not required, and the first main surface is a smooth surface without irregularities.

[0096] The absolute value of the maximum valley depth Rv of the first main surface is preferably 3.0 nm or less, more preferably less than 2.0 nm. In addition, the lower limit of the absolute value is not particularly limited, but is usually 0.5 nm or more. It should be noted that the maximum valley depth Rv in this specification refers to the value measured according to JIS B 0601:2013.

[0097] There are no open pores in the first main surface, or even if there are open pores, the number of open pores is small. Specifically, if the roughening treatment is not performed by glass etching using gas, the average opening area of ​​the pores is at least greater than 1.70×10 4 (nm 2 ), usually 2.00×10 4 (nm 2 ) or more. In addition, if the roughening treatment is not performed by glass etching using gas, the total opening area is at least less than 6.00×10 6 (nm 2 / 25μm 2 ), usually 4.00×10 6 (nm 2 / 25μm 2 )the following.

[0098] The upper limit of the average opening area of ​​the pores and the lower limit of the total opening area are not particularly limited, but are generally 1.00×10 3 (nm 2 ) or less, 1.00×10 6 (nm 2 / 25μm 2 It should be noted that the average opening area and the total opening area of ​​the holes in this specification refer to the values ​​calculated by obtaining the shape image of the first main surface using an atomic force microscope and then performing slope correction processing, filtering processing and particle / hole analysis using nanoscale three-dimensional image processing software (SPIP manufactured by Image Metrology).

[0099] The shape and properties of the second main surface of the glass plate are not particularly limited, and may be the same as those of the side of a conventional electronic device substrate on which an electronic component is formed.

[0100] In view of the fact that the glass sheet of the present embodiment is preferably used as a substrate for electronic devices, the glass composition of the glass sheet is preferably alkali-free glass, which has a very low possibility of short circuit caused by the migration of alkali ions. Alkali-free glass refers to glass that does not substantially contain alkali metal oxides (Li2O, Na2O, and K2O). Substantially containing no alkali metal oxides means glass in which the total content of Li2O, Na2O, and K2O is 0.1% by mass or less.

[0101] In the case of a glass plate containing an alkali metal oxide, such as soda-lime glass, H + Therefore, in the manufacture of a glass plate containing alkali metal oxides, even if a step of polishing by 1 nm or more using a slurry containing calcium carbonate is included, it is difficult to reduce the surface Si-OH group density.

[0102] Expressed as mass % based on oxides, the glass composition of this embodiment contains: SiO2: 35% to 73%, Al2O3: 5% to 35%, B2O3: 0 to 30%, MgO: 0 to 20%, CaO: 0 to 30%, SrO: 0 to 30%, BaO: 0 to 40%, and the total of MgO, CaO, SrO and BaO: 1% to 55%, and contains substantially no alkali metal oxides.

[0103] When the strain point is high and the solubility is taken into consideration, the glass composition, expressed in mass % based on oxides, more preferably contains: SiO2: 58% to 66%, Al2O3: 15% to 22%, B2O3: 5% to 12%, MgO: 0 to 8%, CaO: 0 to 9%, SrO: 3% to 12.5%, BaO: 0 to 2%, and the total of MgO, CaO, SrO and BaO: 9% to 18%, and contains substantially no alkali metal oxides.

[0104] In the case of such a purpose, it is more preferable to contain SiO2: 56% to 62%, Al2O3: 15% to 20%, B2O3: 6% to 10%, MgO: 2% to 5%, CaO: 3% to 7%, SrO: 4% to 10%, BaO: 0 to 1%, and the total of MgO, CaO, SrO and BaO: 12% to 17%, and substantially no alkali metal oxide is contained. It is more preferable to substantially no BaO is contained.

[0105] Taking the high strain point into consideration, the glass composition, expressed in mass % based on oxides, more preferably contains: SiO2: 54% to 73%, Al2O3: 10.5% to 22.5%, B2O3: 0 to 7%, MgO: 0 to 10%, CaO: 0 to 10%, SrO: 0 to 16%, BaO: 0 to 10%, and the total of MgO, CaO, SrO and BaO: 8% to 26%, and contains essentially no alkali metal oxides.

[0106] Taking higher strain points into consideration, the glass composition, expressed in mass % based on oxides, further preferably contains: SiO2: 54% to 73%, Al2O3: 10.5% to 22.5%, B2O3: 0 to 5.5%, MgO: 0 to 10%, CaO: 0 to 10%, SrO: 0 to 10%, BaO: 0 to 10%, and the total of MgO, CaO, SrO and BaO: 8% to 20%, and contains substantially no alkali metal oxides.

[0107] Taking into account electrical properties such as low dielectric constant and low dielectric loss tangent, the glass composition, expressed in mass % based on oxides, more preferably contains: SiO2: 54% to 73%, Al2O3: 5% to 22.5%, B2O3: 15% to 30%, MgO: 0 to 10%, CaO: 0 to 9%, SrO: 0 to 16%, BaO: 0 to 20%, and the total of MgO, CaO, SrO and BaO: 1% to 26%, and contains substantially no alkali metal oxides.

[0108] When it is desired to improve the controllability of the expansion coefficient, especially when it is desired to obtain a substrate with a high expansion coefficient, the glass composition, expressed in mass % based on oxides, more preferably contains: SiO2: 40% to 73%, Al2O3: 5% to 23%, B2O3: 0 to 15%, MgO: 0 to 20%, CaO: 0 to 20%, SrO: 0 to 20%, BaO: 0 to 40%, and the total of MgO, CaO, SrO and BaO: 10% to 55%, and substantially contains no alkali metal oxides.

[0109] The thickness of the glass plate is preferably 0.1 mm or more, more preferably 0.2 mm or more, and further preferably 0.3 mm or more. On the other hand, the thickness is preferably 2.0 mm or less, more preferably 1.5 mm or less, further preferably 1.0 mm or less, further preferably 0.7 mm or less, and particularly preferably 0.5 mm or less.

[0110] The shape of the glass plate is not particularly limited, but when used as a substrate for a display, a rectangular shape is preferred.

[0111] The size of the glass plate is not particularly limited. When the glass plate is rectangular, the length of at least one side is preferably 1000 mm or more, more preferably 1400 mm or more, and further preferably 2500 mm or more. The upper limit is not particularly limited either, and the length of one side is usually 5000 mm or less.

[0112] In addition, when used as a carrier substrate, the shape of the glass plate is preferably rectangular or circular.

[0113] When the glass plate is circular, it is preferably a shape having positioning parts such as notches. The diameter is preferably 200 mm or more, more preferably 300 mm or more. The upper limit is not particularly limited, and the diameter is usually 450 mm or less.

[0114] When the glass plate is rectangular, the length of at least one side is preferably 500 mm or more, more preferably 1200 mm or more, and further preferably 1400 mm or more. The upper limit is not particularly limited either, and the length of one side is usually 3300 mm or less, preferably 2800 mm or less, and more preferably 2000 mm or less.

[0115] The glass plate of this embodiment can also form electronic components such as wiring on the second main surface when the area is large, and then cut into the desired size according to the size of the product. Originally, the charge increases with the area, so the larger the area, the greater the charge when peeling, and the higher the possibility of electrostatic damage. However, the glass plate of this embodiment has a low surface Si-OH group density, so the charge when peeling from the adsorption platform is also suppressed to a small amount. Therefore, even in the case of a large area of ​​the glass plate, electrostatic damage to electronic components can be suppressed.

[0116] [Method for manufacturing glass plate]

[0117] An example of the method for producing the glass plate of the present embodiment is shown below, and there is no particular limitation as long as the surface Si—OH group density of the first main surface is low.

[0118] The method for producing a glass plate includes the step of polishing a first main surface of the glass plate opposite to a second main surface on which an electronic component is to be formed by 1 nm or more using a slurry containing calcium carbonate.

[0119] In addition, it is preferred that after the first main surface is polished, the first main surface is cleaned with an alkaline solution. This is because when an acidic solution is used, the H + Mg on the first main surface 2+ , Ca 2+ , Sr 2+ , Ba 2+ 、Al 3+ and B 3+ Ion exchange reaction occurs, which increases the density of surface Si-OH groups.

[0120] Hereinafter, each step will be described in detail.

[0121] (Grinding process)

[0122] In the grinding process, the first main surface of the glass plate is ground by more than 1 nm while supplying the slurry (hereinafter, sometimes referred to as calcium carbonate slurry) comprising calcium carbonate. Grinding can be suitably carried out by the method satisfying the above-mentioned conditions, and there is no particular restriction, but from the viewpoint of easily making the thickness sufficient to remove the glass plate surface by grinding, it is preferred to use the grinding of a grinding pad.

[0123] Compared with cerium oxide generally used in glass grinding, calcium carbonate has a much lower hardness. Therefore, unlike conventional grinding, no deep grinding damage is generated on the main surface of the glass plate. Therefore, for example, the absolute value of the maximum valley depth Rv of the first main surface is 3.0 nm or less. The absolute value of the maximum valley depth Rv of the first main surface is preferably 3.0 nm or less, and more preferably less than 2.0 mm.

[0124] In the past, grinding using a slurry containing cerium oxide may increase the surface Si-OH group density due to chemical action in addition to the above-mentioned hardness difference. Therefore, from the viewpoint of the surface Si-OH group density, calcium carbonate is also preferably used.

[0125] In addition, when polishing is performed without using abrasive grains and only pure water is supplied, the polishing speed is extremely slow, and the H +Mg on the glass surface 2+ , Ca 2+ , Sr 2+ , Ba 2+ 、Al 3+ and B 3+ The ion exchange reaction occurs, which increases the density of surface Si-OH groups.

[0126] In contrast, when grinding with slurry containing calcium carbonate, only mechanical action is used, and the grinding speed is faster than that of pure water. + Mg on the glass surface 2+ , Ca 2+ , Sr 2+ , Ba 2+ 、Al 3+ and B 3+ The ion exchange reaction occurs quickly, which is speculated to reduce the surface Si-OH group density.

[0127] As the dispersion medium for dispersing calcium carbonate to form a slurry, for example, pure water, industrial water, etc. can be used.

[0128] The concentration of calcium carbonate in the slurry is preferably 1% by mass or more, more preferably 3% by mass or more. In addition, the concentration of calcium carbonate is preferably 40% by mass or less, more preferably 20% by mass or less.

[0129] The slurry may contain other optional components in addition to calcium carbonate and a dispersion medium within a range that does not impair the effects of the present invention. Examples of other optional components include a dispersant and the like.

[0130] For the surface Si-OH group density of the first main surface, in addition to the concentration of the above-mentioned calcium carbonate, it is also possible to control it by grinding conditions. The grinding conditions can be appropriately adjusted without particular restrictions. For example, when grinding with a grinding pad, the grinding pressure is preferably 0.05MPa to 0.5MPa, the glass delivery speed is preferably 0.1 to 20 (m / minute), and the grinding pad rotation speed (revolution) is preferably 30rpm to 1000rpm. In addition, the grinding times in the embodiments described later are not particularly limited. If the load of the grinding process is considered, it is preferably 1 to 20 times, more preferably 1 to 10 times, and most preferably 1 to 7 times.

[0131] (Cleaning process)

[0132] The first main surface is ground using the above-mentioned slurry containing calcium carbonate, and then the first main surface is cleaned. The cleaning is carried out using at least one selected from the group consisting of high-pressure spray, calcium carbonate slurry, detergent and pure water. In the case of using calcium carbonate slurry, detergent, and pure water for cleaning, it is preferred to use a disc brush or a roller brush to clean the first main surface.

[0133] It is preferred to use an alkaline solution as a detergent for cleaning so that the surface Si-OH group density controlled by the polishing process does not become high. The alkaline solution can have a pH greater than 7, preferably a pH of 9 or more. In addition, there is no particular upper limit, but the pH is preferably 13.5 or less.

[0134] In order to prevent the reattachment of deposits, the alkaline solution used in cleaning preferably contains a surfactant. In addition, in order to prevent the dissolution of metal components, it is preferred that a chelating material is not contained.

[0135] It should be noted that, as described above, cleaning may be performed using a slurry containing calcium carbonate, but slurry cleaning using a disc brush or a roller brush alone cannot effectively reduce the surface Si—OH group density of the first main surface as in the above-mentioned polishing step.

[0136] (Drying process)

[0137] After the cleaning step, it is preferred to rinse with pure water and then dry the filter. The drying step can be performed by a conventionally known method. For example, from the perspective of operability and simplicity of equipment, it is preferred to spray compressed air through the filter, i.e., use an air knife.

[0138] In addition to the drying using compressed air, washing and drying using IPA (isopropyl alcohol), spin drying, and Marangoni drying may also be performed.

[0139] In addition to the above-mentioned steps, an optional step such as chamfering may be further performed within a range not impairing the effects of the present invention.

[0140] When the glass plate obtained by the method for producing a glass plate of this embodiment is used as a substrate for an electronic device, Figure 1 As shown, the first main surface 1a of the glass plate 1 is placed in contact with the adsorption platform 2, and the electronic component is formed on the second main surface 1b. Then, the glass plate 1 is peeled off from the adsorption platform 2, and since the peeling charge is suppressed at this time, the formed electronic component can be prevented from being electrostatically damaged.

[0141] In addition, in the grinding using the slurry and grinding pad containing calcium carbonate, the main surface is not roughened. Therefore, even if the peripheral portion of the second main surface is also ground together when the first main surface is ground, the peripheral portion of the second main surface will not be roughened. Therefore, there is no need to worry about the adverse effects on device formation and operation due to the roughening of the second main surface.

[0142] [Electronic devices]

[0143] The glass plate of this embodiment is preferably used as a substrate for electronic devices, more preferably as a substrate for displays, further preferably as a substrate for liquid crystal displays, and most preferably as a substrate for a-Si (amorphous silicon) TFTs.

[0144] Furthermore, it is more preferably used as a carrier substrate for manufacturing a flexible display or a carrier substrate for semiconductor packaging. Among them, it is more preferably used as a carrier substrate for manufacturing a flexible display.

[0145] In addition, the electronic device of this embodiment has the above-mentioned glass plate, and for example, even in a large-scale electronic device with at least one side being a rectangle of 2500 mm or more, the glass plate can be appropriately used as a substrate. In addition, the glass plate can also be appropriately used in a carrier substrate with at least one side being a rectangle of 1400 mm or more or a circle of 500 mm or more in diameter. In the case of a carrier substrate, it can be particularly suitable for use in the manufacture of flexible displays and semiconductor packaging.

[0146] It should be noted that the preferred embodiment of the glass plate in the electronic device is the same as the preferred embodiment described in the above-mentioned [Glass Plate]. In addition, the configuration other than the glass plate can use a conventionally known configuration.

[0147] Example

[0148] The present invention is specifically described below by way of test examples, but the present invention is not limited thereto. It should be noted that Examples 1 to 5 are embodiments, and Examples 6 and 7 are comparative examples.

[0149] [Example 1]

[0150] Using 520mm×410mm and 0.5mm thick alkali-free glass plate for electronic devices (glass A), a main surface to be the first main surface is supplied with calcium carbonate dispersed in pure water to obtain slurry, and a polyurethane foam system polishing pad is used for grinding. The calcium carbonate concentration in the slurry is set to 8% by mass. The process of grinding about 30 seconds under the conditions of glass conveying speed of 130 (cm / minute), rotating speed of 386rpm, and grinding pressure of 0.204MPa is counted as the number of grindings 1 time, and grinding is performed once.

[0151] Next, an alkaline solution adjusted to pH 12 (PK-LCG213 (product name) manufactured by Parker Corporation) was used to perform chemical solution cleaning using a disk brush as a single-sheet cleaning device at a processing speed of 330 (cm / min) and a rotation speed of 300 rpm. After the chemical solution cleaning, the glass plate was dried using an air knife to obtain the glass plate. The thickness of the surface layer of the glass plate removed was estimated to be about 2 nm by weight measurement before the grinding process and after drying using the air knife.

[0152] In addition, the composition of glass A is shown in Table 1 in terms of mass % based on oxides.

[0153] [Example 2]

[0154] A glass plate was obtained in the same manner as in Example 1 except that the number of polishings was set to 2. The thickness of the surface layer of the glass plate removed was about 4 nm.

[0155] [Example 3]

[0156] A glass plate was obtained in the same manner as in Example 1 except that the number of polishing was set to 5. The thickness of the surface layer of the glass plate removed was about 10 nm.

[0157] [Example 4]

[0158] A glass plate was obtained in the same manner as in Example 3 except that the alkali-free glass plate for electronic components was changed to glass B. The thickness of the surface layer of the glass plate removed was about 10 nm.

[0159] In addition, the composition of glass B is shown in Table 1 in terms of mass % based on oxides.

[0160] [Example 5]

[0161] A glass plate was obtained in the same manner as in Example 1 except that the alkali-free glass plate for electronic components was changed to glass C and the number of polishing was changed to 7. The thickness of the surface layer of the glass plate removed was about 14 nm.

[0162] In addition, the composition of glass C is shown in Table 1 in terms of mass % based on oxides.

[0163] [Example 6]

[0164] A glass plate was obtained in the same manner as in Example 1 except that only chemical solution cleaning using an alkaline solution and drying using an air knife were performed without polishing. The weight was measured before chemical solution cleaning using an alkaline solution and after drying using an air knife, but no significant weight loss was confirmed. That is, the thickness of the surface layer of the glass plate removed only by chemical solution cleaning using an alkaline solution was considered to be 0 nm.

[0165] [Example 7]

[0166] A glass plate was obtained in the same manner as in Example 1 except that the same slurry as in Example 1 was used for slurry cleaning instead of grinding. Slurry cleaning was performed by spraying a slurry obtained by dispersing calcium carbonate in pure water, using a disk brush as a single-sheet cleaning device under the conditions of a rotation speed of 300 rpm and a glass conveying speed of 330 (cm / min). The thickness of the surface layer removed from the glass plate by slurry cleaning was estimated to be about 0.2 nm by weight measurement before slurry cleaning and after drying with an air knife.

[0167] According to Example 6, the thickness removed by chemical solution cleaning using an alkaline solution is considered to be 0 nm. Therefore, the thickness removed from the surface layer of the glass plate in Examples 1 to 5 all depends on the grinding process, and it is confirmed that they are all 1 nm or more. In addition, the thickness removed in Example 7 depends on the slurry cleaning using calcium carbonate, and the thickness removed in Example 7 is less than 1 nm. As shown in the results of Example 7, it is difficult to remove more than 1 nm from the surface layer of the glass plate using a disc brush. In order to make the thickness removed from the surface layer of the glass plate more than 1 nm, it is preferred to use, for example, a grinding pad.

[0168] In addition, two glass plates of Example 1 were produced in total, three glass plates of Example 7 were produced in total, and one glass plate of each of Examples 2 to 6 was produced, and used for each evaluation later.

[0169] Table 1 (mass %)

[0170] Glass A Glass B Glass C <![CDATA[SiO2]]> 60 62 62 <![CDATA[Al2O3]]> 17 20 20 <![CDATA[B2O3]]> 8 1 2 MgO 3 5 6 CaO 4 5 6 SrO 8 7 4 BaO 0 0 0 other <0.1 <0.1 <0.1 total 100 100 100

[0171] [Evaluation method]

[0172] (Surface Si-OH group density)

[0173] For the first major surface of the glass plate, calculation of the surface Si—OH group density was performed by the following method.

[0174] (i) The atomic concentrations of Si, Mg, Ca, Sr, Ba, Al, and B were measured on the first main surface of the glass plate by X-ray photoelectron spectroscopy under the following measurement conditions. The atomic concentrations of Mg, Ca, Sr, Ba, Al, and B were divided by the atomic concentration of Si to calculate the atomic concentration of S. Mg , S Ca , S Sr , S Ba , S Al and S B The atomic concentrations of each element normalized by the atomic concentration of Si are shown in FIG. 1 and FIG. 2 are used to calculate the surface Si-OR bond number normalized by the atomic concentration of Si (SiOR surf ).

[0175] It should be noted that even if Ba is included in the basic composition of the glass plate, it is a trace amount below the detection limit of X-ray photoelectron spectroscopy, so it is not monitored. In addition, the relative sensitivity factor (RSF) of each peak used in the calculation of each atomic concentration uses the default corrected relative sensitivity factor (Corrected RSF) provided by the analysis software. The Corrected RSF of each peak is 19.327 (B1s), 30.796 (Mg2s), 23.675 (Al2p), 34.619 (Si2p), 62.711 (Ca2s), 123.306 (Sr3p 3 / 2 ).

[0176] S O surf =2×(S Mg +S Ca +S Sr +S Ba )+3×(S Al +S B )…(1)

[0177] (Measurement conditions)

[0178] Device: ESCA5500 manufactured by ULVAC-PHI

[0179] X-ray: monochromatized AlKα ray

[0180] Energy: 117.4 (eV)

[0181] Energy step size: 0.5 (eV / step)

[0182] Monitoring peaks: B1s, Mg2s, Al2p, Si2p, Ca2s, Sr3p 3 / 2

[0183] Detection angle (the angle between the sample surface and the detector): 15°

[0184] Analysis software: MultiPak Version9.3.0.3

[0185] Peak bottom removal method: Shirley method

[0186] (ii) Next, for the first major surface, use C 60 Ion sputtering cuts the glass plate in the depth direction to expose the inside of the glass plate. The atomic concentrations of Mg, Ca, Sr, Ba, Al, and B normalized by the atomic concentration of Si were measured in the same manner as in (i) above, except that the detection angle was set to 75°. The internal Si-OR bond number normalized by the atomic concentration of Si (SiOR) was calculated using the following formula (2) using these. bulk). It should be noted that the measured depth inside the glass plate refers to a depth of about 200 nm from the surface of the glass plate in terms of SiO2 conversion depth. It should be noted that the SiO2 conversion depth refers to the C calculated based on the thermal oxide film (SiO2 film) formed on the silicon wafer with a known film thickness. 60 The depth is calculated from the sputtering rate (nm / min) of the SiO2 film by ion sputtering.

[0187] S O bulk =2×(B Mg +B Ca +B Sr +B Ba )+3×(B Al +B B )…(2)

[0188] In the formula, B Mg , B Ca , B Sr , B Ba , B Al and B B Each of them means a value obtained by normalizing the atomic concentration of Mg, Ca, Sr, Ba, Al and B by the atomic concentration of Si.

[0189] (iii) using the glass density, the Si concentration in the glass plate, and the number of Si-OR bonds on the surface calculated in (i) above (SiOR surf ) and the internal Si-OR bond number (SiOR bulk ), the surface Si-OH group density (SiOH surf )(pcs / cm 2 ).

[0190] The glass density was measured in accordance with JIS Z 8807:2012 (measurement method by weighing in liquid). mass% ) (mass %) was measured in accordance with JIS R 3105:1995 (agglutination, weight and absorbance method).

[0191] D Si =(D×Si mass% ×6.02×10 23 ) / (100×28.09)…(3)

[0192] D Si-surf =(D Si ) 2 / 3 …(4)

[0193] SiOHsurf =(SiOR bulk -SiOR surf )×D Si-surf …(5)

[0194] Where D Si Refers to the Si atom density in the glass plate (a / cm 3 ), D refers to the glass density (g / cm 3 ), Si mass% refers to the Si concentration (mass %) in the glass plate, D Si-surf Refers to the surface Si atom density (a / cm 2 ).

[0195] (Charge potential, delta charge potential)

[0196] The glass plate was placed on a stainless steel (SUS) 304 adsorption stage with the first main surface in contact with the adsorption stage and fixed by vacuum adsorption. A surface potentiometer (manufactured by Trek Japan, MODEL 542A (product name)) was set above the second main surface of the glass plate.

[0197] Release from the vacuum state, and use the lifting pins of the adsorption stage to peel the glass plate from the adsorption stage. Use a surface potentiometer to measure the change in surface potential of the glass plate until it is 80 mm above the adsorption stage. In the measurement results, the surface potential with the largest absolute value is taken as the charged potential (V) of the second main surface during peeling.

[0198] The charged potential of all the produced glass plates was measured over three days. The glass plates of Examples 1, 2, 6, and 7 were measured on the first day, the glass plates of Examples 4, 5, and 7 were measured on the second day, and the glass plates of Examples 1, 3, and 7 were measured on the third day. On each measurement day, the difference between the charged potential of the glass plate of Example 7 as a comparative example and the charged potential of each glass plate was calculated and taken as the Δ charged potential (V). The Δ charged potential (V) was calculated to exclude as much as possible the influence of the charged potential fluctuation caused by the environmental differences such as temperature and humidity during the measurement. For any of the glass plates in Examples 1 to 7, the surface potential of the surface potentiometer showed a negative (minus) value, and the second main surface was negatively (minus) charged. Therefore, if the charged potential of each glass plate of Examples 1 to 6 is closer to 0 than Example 7 as a comparative example, the Δ charged potential shows a negative (minus) value. On the other hand, if the charged potential is further away from 0 than Example 7 as a comparative example, the Δ charged potential shows a positive (plus) value. Therefore, it can be judged that the larger the negative value of the delta charging potential (V) is, the more the occurrence of peeling charging of the glass plate can be suppressed.

[0199] (Maximum valley depth Rv)

[0200] The absolute value of the maximum valley depth Rv of the first main surface of the glass plate was measured using a non-contact surface shape measuring device using optical interference (VertScan R5500HML-A150 (product name) manufactured by Mitsubishi Chemical Systems Co., Ltd.) in accordance with JIS B 0601: 2013. This device uses the principle of low-coherence interference to accurately measure the surface roughness of the glass plate in a non-contact manner. Specifically, white light with a wide spectral wavelength emitted from a low-coherence light source is divided into measurement light and reference light, and the measurement light is irradiated onto the surface of the glass plate, and the reflected measurement light is interfered with the reference light, thereby measuring the surface roughness of the glass plate.

[0201] For the first main surface, the maximum valley depth Rv is measured at 5 random positions at least 10 mm apart, and after removing the maximum and minimum values, the average value of the maximum valley depth Rv at the three positions is taken as the maximum valley depth Rv of the first main surface of the glass plate.

[0202] (Average opening area and total opening area of ​​the holes)

[0203] The shape image of the first main surface of the glass plate was obtained using an atomic force microscope (AFM), and then the average opening area and the total opening area of ​​the holes were calculated by particle analysis using nanoscale three-dimensional image processing software (SPIP6.7.8 manufactured by Image Metrology).

[0204] The measurement conditions of the shape image using AFM are as follows.

[0205] Atomic force microscope: Nanoscope III manufactured by Digital Instruments

[0206] Measurement mode: Tapping mode

[0207] Probe: NCH10

[0208] Samples / Line: 256

[0209] Scan rate: 1.0Hz

[0210] Observation field: 5μm×5μm

[0211] The calculation of the average opening area and the total opening area of ​​the pores by particle analysis was performed by the following operation steps (manual) 1 to 4.

[0212] Operation procedure 1: As a slope correction process, perform the following operation.

[0213] "Leveling for each line" and "leveling for the entire surface" are performed. Then, the image is rotated 90 degrees, and "leveling for each line" and "leveling for the entire surface" are performed again.

[0214] Operation step 2: As filtering process 1, perform the following operation.

[0215] In the Filter tool, in the Median window, select or enter Non-directional interference, High and Low values, Ratio for displacement: 2, Window size: 5, enable "Include boundaries" and apply.

[0216] Operation step 3: As filtering process 2, perform the following operation.

[0217] In the Filter Tools, select from the Convolution window or enter Smooth, Gaussian Distribution, Standard Deviation: 1, enable "X=Y" and "Auto Size" and apply.

[0218] Operation step 4: For particle and pore analysis, perform the following operation.

[0219] First, from the Detect window, select or enter the branch line-dispersed shape, hole detection, and the platform range for classification: ±0.50, and the minimum shape width: 2.00 pixels. Next, from the Post-Processing window, enable "Shape Preservation Completely", "Suppress Pixel Noise", and "Include Shapes at Image Ends". Finally, click Detect to find the average surface area and total surface area of ​​the holes.

[0220] The average surface area of ​​the pores (nm 2 ) as the average opening area of ​​the pores (nm 2 In addition, the total surface area of ​​the pores (nm 2 ) relative to the observation field of each AFM, i.e. 25 (μm 2 ) as the total opening area of ​​the pores (nm 2 / 25μm 2 ).

[0221] The type of the obtained glass plate, the number of polishing times, the cleaning process, and each evaluation result are shown in Table 2. In the table, NCW means not measured.

[0222] In addition, for the glass plates of Examples 1 to 7, the relationship between the surface Si-OH group density and the delta charge potential is shown in Figure 2 It should be noted that Figure 2 In the example, Example 1-1 shows the result of the first day of Example 1, and Example 1-2 shows the result of the third day of Example 1. In addition, Examples 7-1 to 7-3 show the results of the first to third days of Example 7, respectively.

[0223]

[0224] According to Table 2 and Figure 2 The results confirmed that the charge potential can be controlled by controlling the surface Si-OH group density in the first main surface. That is, the lower the surface Si-OH group density, the greater the minus value of the delta charge potential, and the closer the charge potential is to 0.

[0225] The results of Examples 1 to 6 show that the surface Si-OH group density can be reduced by grinding with a slurry containing calcium carbonate. On the other hand, the results of Examples 6 and 7 show that the effect of reducing the surface Si-OH group density is extremely low if grinding is not performed but only slurry cleaning is performed with a disc brush using a slurry containing calcium carbonate.

[0226] according to Figure 2 The reason for confirming the correlation between the surface Si-OH group density and the △ charge potential is still uncertain, but, as mentioned above, it is believed that as the work function of the first main surface of the glass plate increases, the charge is suppressed. That is, by controlling the surface Si-OH group density of the first main surface of the glass plate to be low, the amount of adsorbed water is also reduced, and the work function increases. As a result, when peeling off from the adsorption platform, the movement of electrons from the first main surface of the glass plate to the adsorption platform is suppressed, or a force similar to it acts, and the first main surface of the glass plate is not easy to be positively (plus) charged. It is speculated that it is related to the charge potential of the second main surface, and the second main surface is not easy to be negatively (minus) charged.

[0227] According to the results of Examples 1, 6, and 7, even if the number of grinding times is 1, the charge suppression effect brought about by grinding using a slurry containing calcium carbonate and a grinding pad is also obvious. In the case of Example 1, in which the number of grinding times using a grinding pad containing a slurry containing calcium carbonate is 1, compared with Example 7 in which the slurry is cleaned only by a disc brush containing a slurry containing calcium carbonate, the surface Si-OH group density is low, and the charge suppression effect is more than 500 V. It can be seen that compared with the previous cleaning using a slurry containing calcium carbonate, grinding using a slurry containing calcium carbonate is very useful for reducing the surface Si-OH group density and suppressing charge.

[0228] When a glass plate having a low surface Si-OH group density is used as a substrate for an electronic device, peeling electrification during peeling from an adsorption sheet is suppressed, thereby suggesting that electrostatic destruction of electronic components can be prevented.

[0229] In addition, since the maximum valley depth Rv of the first main surface is shallow, even if the slurry used in the grinding is assumed to go around at least the peripheral portion of the second main surface, the smoothness of the second main surface will not be lost. Therefore, with respect to the formation and operation of devices represented by electronic components formed on the second main surface, it is suggested that the adverse effects caused by grinding on the first main surface can be prevented.

[0230] This application is based on Japanese Patent Application No. 2020-058106 filed on March 27, 2020 and Japanese Patent Application No. 2020-208670 filed on December 16, 2020, and the contents thereof are incorporated herein by reference.

Claims

1. A glass plate having a first main surface and a second main surface opposite to the first main surface, the second main surface being a side on which an electronic component is formed, in, The surface Si—OH group density of the first main surface derived by the following calculation method is 0 groups / cm 2 Above and 8.7×10 14 Pieces / cm 2 the following, The glass composition of the glass plate comprises, expressed in mass % based on oxides: Not. 2 :35%~73%、 <h2 style=";text-align:left;direction:ltr">Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> :5%~35%、 B 2 O 3 :0~30%、 MgO: 0-20%, CaO: 0-30%, SrO: 0-30%, BaO: 0-40%, and Total of MgO, CaO, SrO and BaO: 1% to 55%, and substantially no alkali metal oxides, Calculation method: (i) For the first main surface of the glass plate as a sample, the atomic concentrations of Si, Mg, Ca, Sr, Ba, Al and B were measured by X-ray photoelectron spectroscopy with the detection angle between the sample and the detector set to 15°, and the surface Si-OR bond number SiOR normalized by the Si atomic concentration was calculated by the following formula (1): surf , R refers to Mg, Ca, Sr, Ba, Al and B, and the unit of the atomic concentration is atomic %. SiOR surf =2×(S Mg +S Ca +S Sr +S Ba )+3×(S Al +S B )…(1) In the formula, S Mg , S Ca , S Sr , S Ba , S Al and S B Each refers to a value obtained by normalizing the atomic concentration of Mg, Ca, Sr, Ba, Al, and B by the atomic concentration of Si. (ii) Next, for the first major surface, use C 60 The glass plate was cut in the depth direction by ion sputtering to expose the inside of the glass plate. The atomic concentrations of Si, Mg, Ca, Sr, Ba, Al and B were measured for the inside of the glass plate by using X-ray photoelectron spectroscopy with a detection angle of 75°. The internal Si-OR bond number SiOR normalized by the Si atomic concentration was calculated by the following formula (2): bulk The unit of atomic concentration is atomic %. SiOR bulk =2×(B Mg +B Ca +B Sr +B Ba )+3×(B Al +B B )…(2) In the formula, B Mg , B Ca , B Sr , B Ba , B Al and B B Each refers to a value obtained by normalizing the atomic concentration of Mg, Ca, Sr, Ba, Al, and B by the atomic concentration of Si. (iii) Using the glass density, the Si concentration in the glass plate, and the number of Si-OR bonds on the surface calculated in (i), surf and the internal Si-OR bond number SiOR calculated in (ii) bulk The surface Si-OH group density SiOH of the first main surface is calculated by the following formulas (3) to (5): surf , SiOH surf The unit is pieces / cm 2 , D Si =(D×Si mass% ×6.02×10 23 ) / (100×28.09)…(3) D Si-surf =(D Si ) 2 / 3 …(4) SiOH surf =(SiOR bulk -SiOR surf )×D Si-surf …(5) Where D Si Refers to the Si atom density in the glass plate, measured in pieces / cm 3 , D refers to the glass density, the unit is g / cm 3 , Si mass% Refers to the Si concentration in the glass plate, expressed in mass %. Si-surf Refers to the surface Si atom density, unit is / cm 2 .

2. The glass sheet according to claim 1, in, The surface Si-OH group density is 7.6×10 14 Pieces / cm 2 the following.

3. The glass sheet according to claim 1 or 2, in, The surface Si-OH group density is 6.1×10 14 Pieces / cm 2 the following.

4. The glass sheet according to claim 1 or 2, in, An absolute value of a maximum valley depth Rv of the first main surface is 3.0 nm or less.

5. The glass sheet according to claim 1 or 2, in, The glass plate has a thickness of 0.1 mm to 1.0 mm.

6. The glass sheet according to claim 1 or 2, in, The glass plate is rectangular in shape, at least one side of which is greater than or equal to 2500 mm in length.

7. The glass sheet according to claim 1 or 2, in, The glass plate is used as a substrate for electronic devices.

8. The glass sheet according to claim 1 or 2, in, The glass plate is used as a substrate for a display.

9. The glass sheet according to claim 1 or 2, in, The glass sheet is used as a carrier substrate for the manufacture of flexible displays.

10. The glass sheet according to claim 1 or 2, in, The glass plate is used as a carrier substrate for semiconductor packaging.

11. A method for producing a glass plate, the method comprising producing the glass plate according to any one of claims 1 to 10, in, The method for manufacturing the glass sheet comprises: A step of polishing the first main surface opposite to the second main surface on which the electronic member is to be formed by 1 nm or more using a slurry containing calcium carbonate.

12. The method for manufacturing a glass sheet according to claim 11, in, After the polishing step, the first main surface is cleaned using an alkaline solution.

Citation Information

Patent Citations

  • Glass plate, and apparatus and method for manufacturing glass plate

    JP2015131751A

  • Meterless switch gear and meterless switch gear system

    JP2020058106A

  • Glass sheet and manufacturing method thereof

    JP2021155320A

  • Glass substrate for displays and method for producing same

    WO2017065138A1

  • Slurry for polishing magnetic disk glass, method for manufacturing magnetic disk glass substrate using polishing slurry, and magnetic disk glass substrate

    JP2013122795A