Solid polymer electrolyte membrane, membrane electrode assembly and solid polymer fuel cell
By using a polymer electrolyte membrane optimized with hydrogen permeability coefficient and film thickness, combining acid-type sulfonic acid perfluoropolymer and perfluoromonomer units, the insufficient hydrogen utilization efficiency and power generation characteristics in solid polymer fuel cells are solved. The problem has achieved more efficient hydrogen utilization and battery performance improvement.
Patent Information
- Application Number
- CN202080017047.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-02-28
- Filing Date
- 2020-02-28
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-02-28
AI Technical Summary
There is room for improvement in the power generation characteristics and hydrogen utilization efficiency of existing solid polymer fuel cells, especially the low cross-efficiency of hydrogen permeable membranes, which affects the overall performance.
A polymer electrolyte membrane with a hydrogen permeability coefficient of less than a prescribed value is used, with a film thickness of within a range of 7 to 20 μm. A perfluoropolymer having an acid-type sulfonic acid group is used as an electrolyte material, including a perfluoromonomer unit and ion exchange. groups to reduce the resistance of the electrolyte membrane and improve hydrogen utilization efficiency.
The power generation characteristics and hydrogen utilization efficiency have been significantly improved, and the overall performance of solid polymer fuel cells has been improved by reducing hydrogen crossover and reducing electrolyte membrane resistance.
Smart Images

Figure BDA0003231504910000061 
Figure BDA0003231504910000062 
Figure BDA0003231504910000091
Abstract
Description
Technical Field
[0001] The present invention relates to a solid polymer electrolyte membrane, a membrane electrode assembly and a solid polymer fuel cell. Background Art
[0002] A solid polymer fuel cell has, for example, a structure in which a membrane electrode assembly is sandwiched between two separators to form a battery unit and a plurality of battery units are stacked. The membrane electrode assembly includes: an anode and a cathode having a catalyst layer, and a solid polymer electrolyte membrane disposed between the anode and the cathode. The solid polymer electrolyte membrane is obtained by, for example, forming a polymer having an acidic sulfonic acid group into a membrane.
[0003] In the examples of Patent Document 1, as a polymer having an acidic sulfonic acid group, a perfluoropolymer obtained by acidifying the group represented by -SO2F of a polymer obtained by copolymerizing CF2=CFOCF2CF(CF3)OCF2CF2SO2F with tetrafluoroethylene is disclosed.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2002-216804 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] In recent years, there has been a demand for further improvement in the performance of polymer electrolyte fuel cells. Specifically, there has been a demand for polymer electrolyte fuel cells that are excellent in power generation characteristics and in the utilization efficiency of hydrogen gas used as fuel.
[0009] The present inventors evaluated a solid polymer electrolyte membrane containing the perfluoropolymer described in Patent Document 1 as an electrolyte and found that there is room for improvement in at least one of the power generation characteristics and hydrogen utilization efficiency of a solid polymer fuel cell.
[0010] In view of the above-mentioned actual situation, an object of the present invention is to provide a polymer electrolyte membrane capable of producing a polymer electrolyte fuel cell having excellent power generation characteristics and hydrogen utilization efficiency, and a membrane electrode assembly and a polymer electrolyte fuel cell obtained using the same.
[0011] Solutions for solving problems
[0012] The present inventors have conducted intensive research on the above-mentioned issues and have found that by using a solid polymer electrolyte membrane containing a polymer electrolyte having a hydrogen permeability coefficient below a specified value and a membrane thickness within a specified range, a solid polymer fuel cell having excellent power generation characteristics and hydrogen utilization efficiency can be manufactured, thereby completing the present invention.
[0013] That is, the present inventors have found that the above-mentioned problems can be solved by the following configuration.
[0014] [1] A solid polymer electrolyte membrane, characterized in that it contains a polymer electrolyte, wherein the polymer electrolyte has a hydrogen permeability coefficient of 2.4×10 -9 cm 3 cm / (s cm 2 cmHg) or less,
[0015] The solid polymer electrolyte membrane has a thickness of 7 to 20 μm.
[0016] [2] The solid polymer electrolyte membrane according to [1], wherein the polymer electrolyte is a perfluoropolymer having an acidic sulfonic acid group.
[0017] [3] The polymer electrolyte membrane according to [2], wherein the perfluoropolymer comprises a perfluoromonomer unit, and the perfluoromonomer unit comprises at least one unit selected from the group consisting of a perfluorovinyl ether unit and a perfluoroallyl ether unit.
[0018] [4] A solid polymer electrolyte membrane according to [2] or [3], wherein the perfluoropolymer does not substantially contain at least one unit selected from the group consisting of a unit having a halogen atom other than a fluorine atom, a unit having a ring structure, and a unit having a cross-linked structure formed by a covalent bond.
[0019] [5] The solid polymer electrolyte membrane according to [3] or [4], wherein the perfluoroallyl ether unit is a unit represented by the formula A-1 described below. In the formula A-1 described below, R F1 and R F2 Each is independently a perfluoroalkylene group having 1 to 3 carbon atoms.
[0020] [6] The polymer electrolyte membrane according to any one of [3] to [5], wherein the perfluoromonomer unit further includes a tetrafluoroethylene unit.
[0021] [7] The solid polymer electrolyte membrane according to any one of [1] to [6], wherein the ion exchange capacity of the polymer electrolyte is 1.4 to 2.5 milliequivalents / g dry resin.
[0022] [8] A membrane electrode assembly, characterized in that it comprises: an anode having a catalyst layer, a cathode having a catalyst layer, and a solid polymer electrolyte membrane according to any one of [1] to [7] arranged between the anode and the cathode.
[0023] [9] The membrane electrode assembly according to [8], wherein the catalyst layer of the cathode comprises a catalyst and a polymer having ion exchange groups,
[0024] The value obtained by subtracting the hydrogen permeability coefficient of the polymer electrolyte from the hydrogen permeability coefficient of the polymer having an ion exchange group is 1.0×10 -8 cm 3 cm / (s cm 2 ·cmHg) or above.
[0025]
[10] A polymer electrolyte fuel cell comprising the membrane electrode assembly of [8] or [9].
[0026] Effects of the Invention
[0027] According to the present invention, there can be provided a polymer electrolyte membrane capable of producing a polymer electrolyte fuel cell having excellent power generation characteristics and hydrogen utilization efficiency, and a membrane electrode assembly and a polymer electrolyte fuel cell obtained using the membrane electrolyte membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic cross-sectional view showing an example of the membrane electrode assembly of the present invention. DETAILED DESCRIPTION
[0029] The following definitions of terms apply throughout the specification and claims unless otherwise specified.
[0030] The "ion exchange group" refers to a group that can exchange at least a part of ions contained in the group for other ions, and examples thereof include the following sulfonic acid type functional group and carboxylic acid type functional group.
[0031] "Sulfonic acid functional groups" are acidic sulfonic acid groups (-SO3H) and salt-type sulfonic acid groups (-SO3M 2 Among them, M 2 A general term for alkali metal or quaternary ammonium cations.
[0032] "Carboxylic acid functional groups" are acidic carboxylic acid groups (-COOH) and salt-type carboxylic acid groups (-COOM 1 Among them, M 1 A general term for alkali metal or quaternary ammonium cations.
[0033] "Precursor membrane" refers to a membrane comprising a polymer having groups that can be converted into ion exchange groups.
[0034] The "group that can be converted into an ion exchange group" refers to a group that can be converted into an ion exchange group by a treatment such as a hydrolysis treatment or an acidification treatment, and is sometimes referred to as a "precursor group".
[0035] The "group convertible into a sulfonic acid type functional group" refers to a group convertible into a sulfonic acid type functional group by a treatment such as a hydrolysis treatment or an acidification treatment.
[0036] The "group convertible into a carboxylic acid type functional group" refers to a group convertible into a carboxylic acid type functional group by a known treatment such as a hydrolysis treatment or an acidification treatment.
[0037] “Substantially containing no unit” means that the content of the unit is 1 mol% or less based on all units of the polymer containing the unit.
[0038] The "unit" in a polymer refers to an atomic group derived from one molecule of a monomer and formed by polymerization of the monomer. The unit may be an atomic group directly formed by a polymerization reaction, or may be an atomic group of another structure converted by treating the polymer obtained by the polymerization reaction. It should be noted that the structural unit derived from each monomer is sometimes recorded by a name in which the monomer name is annotated with "unit".
[0039] The unit represented by the formula A-1 is referred to as unit A-1. The units represented by other formulae are described similarly.
[0040] The compound represented by formula 1-1 is referred to as compound 1-1. The compounds represented by other formulae are described in the same manner.
[0041] [Solid polymer electrolyte membrane]
[0042] The solid polymer electrolyte membrane of the present invention (hereinafter also referred to as "electrolyte membrane") comprises a hydrogen permeability coefficient of 2.4×10 -9 cm 3 cm / (s cm 2 ·cmHg) or less, and the film thickness of the solid polymer electrolyte membrane is 7 to 20 μm.
[0043] The electrolyte membrane of the present invention can produce a solid polymer fuel cell having excellent power generation characteristics and hydrogen utilization efficiency. The detailed reason for this is not clear, but it is presumed to be due to the following reasons.
[0044] A polymer electrolyte fuel cell generates electricity by supplying an oxygen-containing gas to the cathode and a hydrogen-containing gas to the anode. If the hydrogen-containing gas supplied to the anode permeates the electrolyte membrane and moves toward the cathode (so-called hydrogen crossover), the hydrogen utilization efficiency of the polymer electrolyte fuel cell decreases.
[0045] In view of this problem, the present inventors have found that when an electrolyte membrane including a polymer electrolyte having a hydrogen permeability coefficient of a predetermined value or less is used, hydrogen crossover can be suppressed, and as a result, a fuel cell having excellent hydrogen utilization efficiency can be obtained.
[0046] On the other hand, the present inventors have found that although the power generation characteristics of a polymer electrolyte fuel cell are slightly improved by setting the hydrogen permeability coefficient to a predetermined value or less, there is still room for improvement.
[0047] In response to this problem, the inventors found that if the thickness of the electrolyte membrane is set within a specified range, the resistance of the electrolyte membrane will be sufficiently reduced, and as a result, a solid polymer fuel cell with excellent power generation characteristics can be obtained. That is, it can be inferred that the effect of setting the hydrogen permeability coefficient of the polymer electrolyte to below a specified value and the effect of setting the thickness of the electrolyte membrane to within a specified range work synergistically, so that a solid polymer fuel cell with excellent power generation characteristics can be obtained.
[0048] <Polymer Electrolyte>
[0049] The polymer electrolyte is not particularly limited as long as it is an electrolyte formed by a polymer whose hydrogen permeability coefficient satisfies the range described below. From the viewpoint of better power generation characteristics of solid polymer fuel cells, a perfluoropolymer having an acidic sulfonic acid group (hereinafter also referred to as "polymer H") is preferred.
[0050] From the viewpoint of excellent durability of the electrolyte membrane, the polymer H preferably contains a perfluoromonomer unit.
[0051] From the viewpoint of achieving more excellent power generation characteristics of a polymer electrolyte fuel cell, the perfluoromonomer unit preferably contains at least one unit selected from the group consisting of perfluorovinyl ether units and perfluoroallyl ether units (hereinafter also referred to as "unit A").
[0052] The unit A may contain one or both of a perfluorovinyl ether unit and a perfluoroallyl ether unit, but preferably contains a perfluoroallyl ether unit, and particularly preferably a perfluoroallyl ether unit, from the viewpoint of easy synthesis.
[0053] From the viewpoint of lowering the resistance of the electrolyte membrane and improving the power generation characteristics of the polymer electrolyte fuel cell, the unit contained in unit A preferably has an ion exchange group, more preferably a sulfonic acid functional group, and particularly preferably an acidic sulfonic acid functional group.
[0054] When each unit contained in unit A has an ion exchange group, from the viewpoint of lowering the resistance of the electrolyte membrane and improving the power generation characteristics of the solid polymer fuel cell, the number of ion exchange groups in each unit is preferably 2 or more, and from the viewpoint of easy synthesis, 2 is particularly preferred.
[0055] The perfluoroallyl ether unit is preferably unit A-1 from the viewpoint of easily obtaining a polymer electrolyte having a hydrogen gas permeability coefficient within the range described below.
[0056]
[0057] The perfluorovinyl ether unit is preferably the unit A-2 or the unit A-3 from the viewpoint of easily obtaining a polymer electrolyte having a hydrogen gas permeability coefficient in the range described below.
[0058]
[0059] In Formula A-1 to Formula A-3, R F1 and R F2 Each is independently a perfluoroalkylene group having 1 to 3 carbon atoms.
[0060] As R F1 and R F2 Specific examples include -CF2-, -CF2CF2-, -CF(CF3)-, -CF2CF2CF2-, -CF(CF2CF3)-, -CF(CF3)CF2-, -CF2CF(CF3)-, and -C(CF3)(CF3)-.
[0061] From the viewpoint of low raw material cost, easy production, and the ability to further increase the ion exchange capacity of polymer H, R F1 and R F2 Each independently is preferably a perfluoroalkylene group having 1 or 2 carbon atoms. In the case of 2 carbon atoms, a straight chain is preferred. Specifically, -CF2-, -CF2CF2- or -CF(CF3)- is preferred, -CF2- or -CF2CF2- is more preferred, and -CF2- is particularly preferred.
[0062] In formula A-2, R F3 It is a perfluoroalkylene group having 1 to 6 carbon atoms.
[0063] As R F3Specific examples include -CF2-, -CF2CF2-, -CF(CF3)-, -CF2CF2CF2-, -CF(CF2CF3)-, -CF(CF3)CF2-, -CF2CF(CF3)-, -C(CF3)(CF3)-, and -CF2CF(CF3)OCF2CF(CF3)-.
[0064] From the viewpoint of low raw material cost, easy production, and the ability to further increase the ion exchange capacity of polymer H, R F3 It is preferably a perfluoroalkylene group having 1 to 3 carbon atoms. Specifically, it is preferably -CF2-, -CF2CF2- or -CF2CF(CF3)-, and particularly preferably -CF2CF(CF3)-.
[0065] In formula A-2, m is 0 or 1.
[0066] The perfluoro monomer unit may contain units other than the unit A. As the units other than the unit A, there can be mentioned perfluoro monomer units having no ion exchange group and its precursor group.
[0067] Specific examples of the perfluoromonomer unit having no ion exchange group and its precursor group include tetrafluoroethylene (hereinafter also referred to as "TFE") unit and hexafluoropropylene unit. From the viewpoint of excellent strength of the electrolyte membrane, the TFE unit is preferred.
[0068] From the viewpoint of easily setting the ion exchange capacity of the electrolyte membrane within the range described below and easily obtaining a polymer electrolyte within the range described below in terms of hydrogen permeability, the lower limit of the content of unit A is preferably 7 mol %, more preferably 8 mol %, and particularly preferably 9 mol % relative to all units in polymer H.
[0069] From the viewpoint of excellent strength of the electrolyte membrane, the upper limit of the content of the units A is preferably 45 mol % based on all units in the polymer H, more preferably 36 mol %, and particularly preferably 22 mol %.
[0070] When a perfluoromonomer unit having no ion exchange group and its precursor group is contained, its content is preferably 55 to 93 mol%, more preferably 65 to 92 mol%, and particularly preferably 78 to 91 mol% based on all units in the polymer H. These contents are particularly suitable when the perfluoromonomer unit is a TFE unit.
[0071] The polymer H preferably does not substantially contain a unit having a halogen atom other than a fluorine atom (hereinafter also referred to as "unit X1"). Thus, a chain transfer reaction is less likely to occur when polymerizing the monomer to produce the polymer H, and the amount of oligomers produced during production is small.
[0072] Specific examples of the unit X1 include a chlorotrifluoroethylene unit, a bromotrifluoroethylene unit, an iodotrifluoroethylene unit, and a dichlorodifluoroethylene unit.
[0073] The polymer H substantially does not contain the unit X1 means that the content of the unit X1 is 1 mol% or less relative to all units in the polymer H, and preferably does not contain the unit X1 (0 mol%).
[0074] The polymer H preferably does not substantially contain a unit having a ring structure (hereinafter also referred to as "unit X2"), thereby preventing the polymer H from becoming brittle and increasing the toughness of the polymer H. Therefore, the electrolyte membrane obtained using the polymer H has excellent mechanical strength.
[0075] Examples of the ring structure include an aliphatic hydrocarbon ring, an aliphatic heterocyclic ring, an aromatic hydrocarbon ring, and an aromatic heterocyclic ring. The ring structure may be present in the main chain or in the side chain.
[0076] Specific examples of the unit X2 include units having a cyclic ether structure described in Japanese Patent Nos. 4,997,968 and 5,454,592.
[0077] The polymer H substantially does not contain the unit X2, which means the same as the unit X1, and preferably does not contain it (0 mol%).
[0078] The polymer H preferably does not substantially contain a unit having a cross-linked structure formed by a covalent bond (hereinafter also referred to as "unit X3"). As a result, the polymer H is easily dissolved or dispersed in a liquid medium, and therefore, when an electrolyte membrane is formed using a liquid composition containing the polymer H and the liquid medium, the electrolyte membrane can be made into a thin film.
[0079] The cross-linked structure formed by covalent bonds refers to: a structure obtained by polymerizing a monomer having a cross-linking group (such as vinyl, perfluorovinyl, etc.) that can be cross-linked by covalent bonds, and then causing the cross-linking groups to cross-link by covalent bonds; or a structure obtained by causing a monomer having a cross-linking group that can be cross-linked by covalent bonds to cross-link simultaneously with the polymerization reaction.
[0080] Specific examples of the unit X3 include units having a structure obtained by polymerizing compounds of formulae 8 to 15 described in JP-A-2001-176524 (compounds having two crosslinking groups) and then crosslinking the crosslinking groups not used in the polymerization via covalent bonds.
[0081] The polymer H substantially does not contain the unit X3, which means the same as the unit X1, and preferably does not contain it (0 mol%).
[0082] (Method for producing polymer electrolyte)
[0083] As an example of a method for producing a polymer electrolyte, a method for producing the above-mentioned polymer H will be described as an example.
[0084] An example of a method for producing polymer H is as follows: a precursor polymer (hereinafter also referred to as "polymer F") in which the acidic sulfonic acid group in polymer H becomes a precursor group (specifically, a group represented by -SO2F) is converted into an acidic sulfonic acid group (-SO3 - H + ) method.
[0085] As a specific example of the method of converting the group represented by -SO2F belonging to the precursor group into an acid-type sulfonic acid group, there is listed a method of hydrolyzing the group represented by -SO2F of polymer F to form a salt-type sulfonic acid group, and converting the salt-type sulfonic acid group into an acid-type sulfonic acid group.
[0086] The polymer F is preferably a perfluoropolymer containing a perfluoro monomer unit and having a group represented by -SO2F.
[0087] The perfluoromonomer unit in the polymer F preferably contains at least one unit selected from the group consisting of a perfluorovinyl ether unit and a perfluoroallyl ether unit (hereinafter also referred to as "unit a").
[0088] The unit a may contain one or both of a perfluorovinyl ether unit and a perfluoroallyl ether unit, but preferably contains a perfluoroallyl ether unit, and particularly preferably a perfluoroallyl ether unit, from the viewpoint of easy synthesis.
[0089] The unit contained in unit a may or may not have a precursor group having an ion exchange group. It is preferably a precursor group having an ion exchange group, and particularly preferably a precursor group having a sulfonic acid type functional group (specifically a group represented by -SO2F).
[0090] Specific examples of the perfluorovinyl ether unit in the unit a include units obtained by converting the acidic sulfonic acid group of the perfluorovinyl ether unit in the above-mentioned unit A into a group represented by -SO2F.
[0091] The perfluoroallyl ether unit in the unit a is preferably the unit a-1.
[0092]
[0093] R in formula a-1 F1 and R F2 Respectively with R in formula A-1 F1 and R F2 have the same meaning.
[0094] The perfluoromonomer unit in the unit a may contain units other than the unit a. Specific examples of the units other than the unit a include perfluoromonomer units having no ion exchange group and its precursor group.
[0095] Specific examples of the perfluoromonomer unit having no ion exchange group and its precursor group are the same as those of the polymer H.
[0096] The content of each unit in the polymer F is preferably the same as the content of each unit in the polymer H.
[0097] The polymer F preferably contains substantially no at least one unit selected from the group consisting of a unit having a halogen atom other than a fluorine atom, a unit having a ring structure, and a unit having a crosslinked structure formed by a covalent bond, and particularly preferably contains substantially no all of these units.
[0098] Specific examples of the unit having a halogen atom other than a fluorine atom, the unit having a ring structure, and the unit having a crosslinked structure formed by a covalent bond are the same as those for the polymer H.
[0099] In addition, the phrase “substantially free” has the same meaning as that of the case of the polymer H.
[0100] The capacity flow rate value (hereinafter also referred to as "TQ value") of polymer F is preferably 220°C or more, more preferably 225 to 360°C, and further preferably 230 to 350°C. If the TQ value is above the lower limit, a polymer H having a sufficient molecular weight can be obtained, and therefore, the strength of the electrolyte membrane is excellent. If the TQ value is below the upper limit, the solubility or dispersibility of polymer H relative to the liquid medium is improved, and therefore, it is easy to prepare a liquid composition. The TQ value is an indicator of the molecular weight of polymer F.
[0101] The "TQ value" of the polymer F can be determined by the method described in the Examples section below.
[0102] <Physical properties>
[0103] The hydrogen permeability coefficient of the polymer electrolyte at 80°C and 10% relative humidity is 2.4×10 -9 cm 3 cm / (s cm 2 cmHg) or less, preferably 2.2×10 -9 cm 3 cm / (s cm 2 cmHg) or less, more preferably 2.0×10 -9 cm 3 cm / (s cm 2 cmHg) or less, particularly preferably 1.8×10 -9 cm3 cm / (s cm 2 When the hydrogen permeability coefficient is below the upper limit value, the occurrence of hydrogen crossover can be suppressed.
[0104] From the viewpoint of reducing the resistance value of the electrolyte membrane and further improving the power generation characteristics of the solid polymer fuel cell, the hydrogen permeability coefficient of the polymer electrolyte under the conditions of a temperature of 80°C and a relative humidity of 10% is preferably 1.0×10 -12 cm 3 cm / (s cm 2 cmHg) or more, particularly preferably 1.0×10 -11 cm 3 cm / (s cm 2 ·cmHg) or above.
[0105] The “hydrogen gas permeability coefficient” of the polymer electrolyte was determined by using a 25 μm-thick membrane formed of the polymer electrolyte and by the method described in the section of Examples described later.
[0106] The ion exchange capacity of the polymer electrolyte is preferably 1.4 to 2.5 milliequivalents / gram of dry resin, more preferably 1.6 to 2.4 milliequivalents / gram of dry resin, and particularly preferably 1.8 to 2.3 milliequivalents / gram of dry resin. If the ion exchange capacity of the polymer electrolyte is above the lower limit, the resistance of the electrolyte membrane obtained using it can be reduced, and as a result, the power generation characteristics of the solid polymer fuel cell can be further improved. If the ion exchange capacity of the polymer electrolyte is below the upper limit, the strength when made into an electrolyte membrane is excellent.
[0107] The “ion exchange capacity” of the polymer electrolyte can be determined by the method described in the Examples section below.
[0108] The thickness of the electrolyte membrane is 7 to 20 μm, the lower limit of the above range is preferably 10 μm, particularly preferably 13 μm, and the upper limit of the above range is preferably 18 μm. If the thickness of the electrolyte membrane is above the lower limit of the above range, the crossover of hydrogen can be further suppressed, and the mechanical strength is excellent. In addition, if it is below the upper limit of the above range, the resistance value of the electrolyte membrane can be reduced, and the power generation characteristics of the solid polymer fuel cell can be further improved.
[0109] The film thickness of the electrolyte membrane refers to the average film thickness determined by the method described in the Examples section below.
[0110] <Other Materials>
[0111] The electrolyte membrane may be reinforced with a reinforcing material. Specific examples of the reinforcing material include porous bodies, fibers, woven fabrics, and nonwoven fabrics.
[0112] The reinforcing material is preferably composed of a material selected from the group consisting of polytetrafluoroethylene (hereinafter also referred to as "PTFE"), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (hereinafter also referred to as "PFA"), polyetheretherketone (hereinafter also referred to as "PEEK") and polyphenylene sulfide (hereinafter also referred to as "PPS").
[0113] In order to further improve durability, the electrolyte membrane may contain one or more metals, metal compounds or metal ions selected from the group consisting of cerium and manganese. Cerium and manganese decompose hydrogen peroxide, which is a causative substance that causes degradation of the electrolyte membrane.
[0114] The electrolyte membrane may contain silicon dioxide or a heteropoly acid (eg, zirconium phosphate, phosphomolybdic acid, phosphotungstic acid) as a moisture retaining agent for preventing drying.
[0115] <Purpose>
[0116] The electrolyte membrane can be suitably used as a solid polymer electrolyte membrane of a solid polymer fuel cell.
[0117] <Method for producing electrolyte membrane>
[0118] As an example of a method for producing an electrolyte membrane, there is mentioned a method (casting method) in which a liquid composition described later is applied to the surface of a substrate film or a catalyst layer and then dried.
[0119] As an example of a production method when the electrolyte membrane includes a reinforcing material, there is a method of impregnating the reinforcing material with a liquid composition described later and drying the reinforcing material.
[0120] In order to stabilize the electrolyte membrane, it is preferred to perform heat treatment. The heat treatment temperature also varies depending on the type of polymer electrolyte, and is preferably 130 to 200°C. If the heat treatment temperature is 130°C or higher, the water content of the polymer electrolyte becomes appropriate. If the heat treatment temperature is 200°C or lower, the thermal decomposition of the sulfonic acid group can be suppressed, and the excellent conductivity of the electrolyte membrane can be maintained.
[0121] The electrolyte membrane may be treated with an aqueous hydrogen peroxide solution as necessary.
[0122] (Liquid composition)
[0123] The liquid composition preferably contains a polymer electrolyte and a liquid medium. The polymer electrolyte in the liquid composition may be dispersed in the liquid medium or may be dissolved in the liquid medium.
[0124] Specific examples of the liquid medium include water and organic solvents. The liquid medium may be water alone, an organic solvent alone, or a mixed solvent of water and an organic solvent. A mixed solvent of water and an organic solvent is preferably used.
[0125] When water is included as the liquid medium, the dispersibility or solubility of the polymer electrolyte in the liquid medium is likely to be improved. When an organic solvent is included as the liquid medium, an electrolyte membrane that is not easily broken is likely to be obtained.
[0126] As the organic solvent, alcohols having 1 to 4 carbon atoms are preferred from the viewpoint of easily obtaining an electrolyte membrane that is less prone to rupture.
[0127] Examples of the alcohol having 1 to 4 carbon atoms include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2,2,2-trifluoroethanol, 2,2,3,3,3-pentafluoro-1-propanol, 2,2,3,3-tetrafluoro-1-propanol, 1,1,1,3,3,3-hexafluoro-2-propanol and 3,3,3-trifluoro-1-propanol.
[0128] The organic solvent may be used alone or in combination of two or more.
[0129] When the liquid medium is a mixed solvent of water and an organic solvent, the content of water is preferably 10 to 99% by mass, particularly preferably 20 to 99% by mass, based on the total mass of the liquid medium.
[0130] When the liquid medium is a mixed solvent of water and an organic solvent, the content of the organic solvent is preferably 1 to 90% by mass, particularly preferably 1 to 80% by mass.
[0131] When the contents of water and the organic solvent are within the above ranges, an electrolyte membrane which is excellent in dispersibility or solubility of the polymer electrolyte in the liquid medium and is not easily broken can be easily obtained.
[0132] The content of the polymer electrolyte is preferably 1 to 50% by mass, particularly preferably 3 to 30% by mass, relative to the total mass of the liquid composition. If it is above the lower limit of the above range, a film with a thickness can be stably obtained during film formation. If it is below the upper limit of the above range, the viscosity of the liquid composition becomes appropriate.
[0133] In order to further improve the durability of the electrolyte membrane produced from the liquid composition, the liquid composition may contain one or more metals, metal compounds or metal ions selected from the group consisting of cerium and manganese.
[0134] [Membrane Electrode Assembly]
[0135] The membrane electrode assembly of the present invention includes an anode having a catalyst layer, a cathode having a catalyst layer, and the electrolyte membrane disposed between the anode and the cathode.
[0136] Since the membrane electrode assembly of the present invention includes the above-mentioned electrolyte membrane, a polymer electrolyte fuel cell obtained using the membrane electrode assembly is excellent in power generation characteristics and hydrogen utilization efficiency.
[0137] Hereinafter, an example of the membrane electrode assembly of the present invention will be described with reference to the drawings.
[0138] Figure 1 1 is a schematic cross-sectional view showing an example of a membrane electrode assembly of the present invention. The membrane electrode assembly 10 includes: an anode 13 having a catalyst layer 11 and a gas diffusion layer 12, a cathode 14 having a catalyst layer 11 and a gas diffusion layer 12, and an electrolyte membrane 15 arranged between the anode 13 and the cathode 14 in a state of contacting the catalyst layer 11.
[0139] Specific examples of the catalyst layer 11 include a layer containing a catalyst and a polymer having an ion exchange group.
[0140] Specific examples of the catalyst include: a supported catalyst in which a catalyst containing platinum, a platinum alloy, or platinum having a core-shell structure is supported on a carbon support; an iridium oxide catalyst; and a catalyst containing an alloy containing iridium oxide or iridium oxide having a core-shell structure. As a carbon support, carbon black powder can be cited.
[0141] Specific examples of the polymer having an ion exchange group include polymer H and a perfluoropolymer that is a polymer other than polymer H and has an ion exchange group (hereinafter also referred to as "polymer H'").
[0142] The polymer H' preferably contains a unit based on a fluorine-containing olefin and a unit having a sulfonic acid type functional group and a fluorine atom. It should be noted that the polymer H' may contain units other than these.
[0143] Examples of the fluorinated olefin include TFE, chlorotrifluoroethylene, vinylidene fluoride, vinyl fluoride, and hexafluoropropylene, with TFE being particularly preferred. The fluorinated olefin may be used alone or in combination of two or more.
[0144] The unit having a sulfonic acid type functional group and a fluorine atom is preferably a unit represented by formula (1-1), a unit represented by formula (1-2), or a unit represented by formula (1-3).
[0145] The unit having a sulfonic acid type functional group and a fluorine atom may be used alone or in combination of two or more.
[0146] Formula (1-1) -[CF2-CF(-OR f1 -SO3M)]-
[0147] Formula (1-2) -[CF2-CF(-R f1-SO3M)]-
[0148]
[0149] R f1 The perfluoroalkylene group is a perfluoroalkylene group which may contain an oxygen atom between carbon atoms. The number of carbon atoms in the perfluoroalkylene group is preferably 1 or more, particularly preferably 2 or more, and is preferably 20 or less, particularly preferably 10 or less.
[0150] R f2 The perfluoroalkylene group is a single bond or optionally contains an oxygen atom between carbon atoms. The number of carbon atoms in the perfluoroalkylene group is preferably 1 or more, particularly preferably 2 or more, and is preferably 20 or less, particularly preferably 10 or less.
[0151] r is 0 or 1.
[0152] M is a hydrogen atom, an alkali metal or a quaternary ammonium cation.
[0153] Specific examples of the unit (1-1) include the following units 1-1-1 to 1-1-3. In the formula, w is an integer of 1 to 8, and x is an integer of 1 to 5. M in the formula has the same meaning as described above.
[0154] -[CF2-CF(-O-(CF2) w -SO3M)]- Formula (1-1-1)
[0155] -[CF2-CF(-O-CF2CF(CF3)-O-(CF2) w -SO3M)]- Formula (1-1-2)
[0156] -[CF2-CF(-(O-CF2CF(CF3)) x -SO3M)]- Formula (1-1-3)
[0157] Specific examples of the unit (1-2) include the following units: w in the formula is an integer of 1 to 8. M in the formula has the same meaning as described above.
[0158] -[CF2-CF(-(CF2) w -SO3M)]- Formula (1-2-1)
[0159] -[CF2-CF(-CF2-O-(CF2) w -SO3M)]- Formula (1-2-2)
[0160] The unit (1-3) is preferably a unit represented by the following formula (1-3-1): M in the formula has the same meaning as described above.
[0161] In formula (1-3-1), R f4 is a linear perfluoroalkylene group having 1 to 6 carbon atoms, R f5 It is a single bond or a linear perfluoroalkylene group having 1 to 6 carbon atoms which may contain an oxygen atom between carbon atoms. r and M are as defined above.
[0162]
[0163] The value (Hc-Hk) obtained by subtracting the hydrogen permeability coefficient (hereinafter also referred to as "Hk") of the polymer electrolyte contained in the electrolyte membrane from the hydrogen permeability coefficient (hereinafter also referred to as "Hc") of the polymer having ion exchange groups in the cathode catalyst layer is preferably 1.0×10 -8 cm 3 cm / (s cm 2 cmHg) or more, more preferably 1.3×10 -8 cm 3 cm / (s cm 2 cmHg) or more, more preferably 1.5×10 -8 cm 3 cm / (s cm 2 cmHg) or more, particularly preferably 1.7×10 -8 cm 3 cm / (s cm 2 ·cmHg) or above.
[0164] The upper limit of the value of Hc-Hk is preferably as high as possible, and is not particularly limited, but is, for example, 2.5×10 -8 cm 3 cm / (s cm 2 ·cmHg).
[0165] When the value of Hc-Hk is within the above range, the power generation characteristics of the polymer electrolyte fuel cell are further improved. The reason for this is not completely clear, but it is presumed to be due to the following reasons.
[0166] If the hydrogen permeability coefficient decreases, the amount of hydrogen permeation decreases, but there is a tendency for the amount of oxygen permeation to decrease as well. Therefore, if the Hc in the cathode supplied with the oxygen-containing gas is low, the supply of oxygen to the catalyst surface as the reaction site is hindered.
[0167] To address this problem, if the Hc-Hk value is within the above range, the hydrogen crossover from the anode to the cathode can be suppressed, and for the cathode side catalyst layer, the supply of oxygen to the catalyst surface can be promoted. Therefore, it can be inferred that through their synergistic effect, a solid polymer fuel cell with better power generation characteristics can be obtained.
[0168] It should be noted that the hydrogen permeability coefficient of the polymer having ion exchange groups in the cathode catalyst layer was determined by the method described in the Examples section below.
[0169] The gas diffusion layer 12 has the function of uniformly diffusing the gas in the catalyst layer and the function of serving as a current collector. Specific examples of the gas diffusion layer include carbon paper, carbon cloth, carbon felt, and a titanium porous body (specifically, a sintered body of titanium particles or fibers, etc.).
[0170] In order to prevent the generated gas from adhering, the gas diffusion layer may be subjected to water-repellent or hydrophilic treatment using PTFE or the like, or may be hydrophilicized using a polymer having an ion exchange group or the like.
[0171] Figure 1 The membrane electrode assembly includes the gas diffusion layer 12, but the gas diffusion layer is an optional component and may not be included in the membrane electrode assembly.
[0172] The electrolyte membrane 15 is an electrolyte membrane (solid polymer electrolyte membrane) containing the above-mentioned polymer electrolyte.
[0173] The anode 13 and the cathode 14 may have other components than those described above.
[0174] A specific example of other members is a carbon layer (not shown) provided between the catalyst layer 11 and the gas diffusion layer 12. If the carbon layer is provided, the gas diffusivity on the surface of the catalyst layer 11 is improved, and the power generation performance of the fuel cell can be further improved.
[0175] The carbon layer contains, for example, carbon and a nonionic fluorine-containing polymer. As a specific example of carbon, carbon nanofibers having a fiber diameter of 1 to 1000 nm and a fiber length of 1000 μm or less are preferred. As a specific example of the nonionic fluorine-containing polymer, PTFE can be cited.
[0176] Specific examples of methods for manufacturing membrane electrode assemblies include: a method in which a catalyst layer is formed on an electrolyte membrane and the resulting assembly is further clamped by a gas diffusion layer; and a method in which a catalyst layer is formed on a gas diffusion layer to form an electrode (anode, cathode), and the electrolyte membrane is clamped by the electrodes.
[0177] The catalyst layer can be produced by applying a catalyst layer-forming coating liquid to a predetermined position and drying it as needed. The catalyst layer-forming coating liquid is a liquid obtained by dispersing a polymer having an ion exchange group and a catalyst in a dispersion medium.
[0178] [Solid polymer fuel cell]
[0179] The polymer electrolyte fuel cell of the present invention includes the above-mentioned membrane electrode assembly.
[0180] The polymer electrolyte fuel cell of the present invention includes the membrane electrode assembly described above and therefore has excellent power generation characteristics and hydrogen utilization efficiency.
[0181] The polymer electrolyte fuel cell of the present invention may include separators having grooves serving as gas flow paths formed on both surfaces of the membrane electrode assembly.
[0182] Specific examples of the separator include a metal separator, a carbon separator, a separator formed of a material in which graphite and a resin are mixed, and a separator formed of various conductive materials.
[0183] In a solid polymer fuel cell, an oxygen-containing gas is supplied to a cathode and a hydrogen-containing gas is supplied to an anode to generate electric power.
[0184] Example
[0185] Hereinafter, the present invention will be described in detail by giving examples. Examples 6-1 to 6-8 and 7-1 to 7-10 are embodiments of the present invention, and Examples 6-9 to 6-16 and 7-11 to 7-18 are comparative examples. However, the present invention is not limited to these examples. It should be noted that the compounding amount of each component in the table described below represents a mass basis.
[0186] [ 1 H-NMR]
[0187] 1 H-NMR was measured at a frequency of 300.4 MHz and a chemical shift standard of tetramethylsilane. As a solvent, CD3CN was used unless otherwise specified. The product was quantitatively determined according to 1 The analysis was performed based on the results of H-NMR analysis and the amount of the internal standard sample (1,3-bis(trifluoromethyl)benzene) added.
[0188] [ 19 F-NMR]
[0189] 19 F-NMR was measured under the conditions of frequency: 282.7 MHz, solvent: CD3CN, chemical shift standard: CFCl3. The product was quantitatively determined according to 19 The analysis was performed based on the results of F-NMR analysis and the amount of the internal standard sample (1,3-bis(trifluoromethyl)benzene) added.
[0190] [ 13 C-NMR]
[0191] 13C-NMR was measured under the conditions of frequency: 75.5 MHz, chemical shift standard: tetramethylsilane. Unless otherwise specified, CD3CN was used as the solvent.
[0192] [Ion exchange capacity]
[0193] The film of polymer F or polymer F' is vacuum dried at 120°C for 12 hours. After measuring the mass of the dried polymer film, the polymer film is immersed in a 0.85 mol / g sodium hydroxide solution (solvent: water / methanol = 10 / 90 (mass ratio)) at 60°C for more than 72 hours to hydrolyze the group represented by -SO2F. The ion exchange capacity of polymer F or polymer F' is determined by back titrating the hydrolyzed sodium hydroxide solution with 0.1 mol / L hydrochloric acid. In this specification, the ion exchange capacity of polymer H or polymer H' as a polymer electrolyte is recorded as the same as the ion exchange capacity measured using polymer F or polymer F' as a precursor.
[0194] [Proportion of each unit]
[0195] The ratio of each unit in the polymer F or the polymer F' is calculated from the ion exchange capacity of the polymer F or the polymer F'.
[0196] The ratio of each unit in polymer H or polymer H' is the same as the ratio of the corresponding unit in polymer F or polymer F'.
[0197] [Hydrogen permeability coefficient]
[0198] The hydrogen permeability coefficient of a film (film thickness 25 μm) formed of polymer H or polymer H′ as a polymer electrolyte was measured in accordance with JIS K7126-2: 2006. A gas permeability measuring device (GTR-100XFAG manufactured by GTR TEC Co., Ltd.) was used as a measuring device.
[0199] The effective penetration area is 9.62cm 2 The film formed of polymer H or polymer H' is maintained at 80°C, and hydrogen gas adjusted to 10% relative humidity is circulated to the first surface at 30 mL / min, and argon gas adjusted to 10% relative humidity is circulated to the second surface at 30 mL / min. The hydrogen gas gradually permeating into the argon gas is detected by gas chromatography, and the hydrogen permeation amount converted to a volume at 25°C and 1 atmosphere is calculated. Using the obtained hydrogen permeation amount, the hydrogen permeation amount per 1 cm 2 The hydrogen permeability coefficient is the value obtained by converting the membrane area and the gas permeability per second per 1 cmHg of the pressure difference of the permeating gas into a membrane thickness of 1 cm. It should be noted that the reference size and thickness of the membrane used in the calculation were measured under the conditions of temperature: 23°C and relative humidity: 50%RH.
[0200] [Initial power generation characteristics]
[0201] The membrane electrode assembly was assembled into a power generation battery cell, and the temperature of the membrane electrode assembly was maintained at 95°C. Hydrogen (utilization rate of 70%) was pressurized to 151 kPa (absolute pressure) and supplied to the anode, and air (utilization rate of 50%) was pressurized to 151 kPa (absolute pressure) and supplied to the cathode. Regarding the humidification of the gas, the relative humidity of hydrogen and air was set to 20% RH, and the current density was recorded at 2 A / cm 2 The cell voltage at the time of , is evaluated according to the following criteria. The higher the cell voltage, the better the power generation characteristics of the solid polymer fuel cell.
[0202] ◎◎: Battery cell voltage is 0.43V or above.
[0203] ◎: The battery cell voltage is 0.40V or more and less than 0.43V.
[0204] ○: The battery cell voltage is 0.37V or more and less than 0.40V.
[0205] ×: The battery cell voltage is less than 0.37V.
[0206] [Hydrogen leakage]
[0207] The amount of hydrogen leakage from the anode side to the cathode side through the electrolyte membrane of the membrane electrode assembly was quantified in the form of the oxidation current value of hydrogen on the cathode side by linear sweep voltammetry. The test was carried out as follows: Hydrogen (0.05 mL / min) and nitrogen (0.2 mL / min) were supplied to the anode and cathode respectively at normal pressure, and the potential on the cathode side was scanned from 0.05 V to 0.5 V at a scan rate of 0.5 mV / sec with the anode side as the reference electrode under the conditions of the cell temperature: 80°C and the relative humidity of hydrogen and nitrogen: 100% RH. In the obtained relationship between the current density and the potential, the intercept value of the linear approximation in the range of 0.4 to 0.5 V was used as the hydrogen leakage current value, and the evaluation was performed according to the following criteria. The smaller the hydrogen leakage current value, the better the hydrogen utilization efficiency of the solid polymer fuel cell.
[0208] ◎: Hydrogen leakage current value is 2.5mA / cm 2 the following.
[0209] ○: Hydrogen leakage current value exceeds 2.5mA / cm 2 And 4.0mA / cm 2 the following.
[0210] ×: Hydrogen leakage current value exceeds 4.0 mA / cm2 .
[0211] [film thickness]
[0212] The solid polymer electrolyte membrane was measured using a Digimatic Indicator (ID-C112XB manufactured by MITUTOYO Corporation), and the average membrane thickness was calculated by taking the arithmetic average of the membrane thickness at any six points. The membrane thickness was measured at a temperature of 23° C. and a relative humidity of 50% RH.
[0213] [TQ value]
[0214] Using a flow tester (Shimadzu Corporation, CFT-500A) equipped with a nozzle of 1 mm in length and 1 mm in inner diameter, polymer F or F' was melt-extruded at an extrusion pressure of 2.94 MPa (gauge pressure) while changing the temperature. The extrusion volume of polymer F or F' reaching 100 mm 3 / second temperature (TQ value). The higher the TQ value, the larger the molecular weight of the polymer.
[0215] [Glass transition temperature]
[0216] For the film of polymer F or F', a dynamic viscoelasticity measurement was performed using a dynamic viscoelasticity measuring device (manufactured by IT Measurement and Control Co., Ltd., DVA-225) under the conditions of sample width: 5.0 mm, length between clamps: 15 mm, measurement frequency: 1 Hz, heating rate: 2°C / min, and tensile mode. Tanδ (loss tangent) was calculated from the ratio of loss elastic modulus E" and storage modulus E' (E" / E'), and a tanδ-temperature curve was prepared. The value obtained by reading the peak temperature between -100 and 200°C from the tanδ-temperature curve was taken as the glass transition temperature (Tg) of polymer F or F'.
[0217] [Abbreviation]
[0218] TFE: tetrafluoroethylene,
[0219] PSVE: CF2=CFOCF2CF(CF3)OCF2CF2SO2F,
[0220] PFtBPO: (CF3)3COOC(CF3)3,
[0221] AIBN: (CH3)2C(CN)N=NC(CH3)2(CN)、
[0222] HFC-52-13p: CF3(CF2)5H,
[0223] HFE-347pc-f: CF3CH2OCF2CF2H,
[0224] HCFC-225cb:CClF2CF2CHClF,
[0225] HCFC-141b: CH3CCl2F.
[0226] [Example 1]
[0227] <Example 1-1>
[0228] In a 2L four-necked flask equipped with a stirrer, a condenser, a thermometer, and a dropping funnel, 560 g of chlorosulfonic acid was placed under nitrogen sealing. The flask was cooled in an ice bath, and a mixture of 139.5 g of compound 1-1 and 478.7 g of dichloromethane was added dropwise over 20 minutes while maintaining the internal temperature below 20°C. Heat release and gas generation were observed during the dropwise addition. After the dropwise addition was completed, the flask was placed in an oil bath, and the reaction was carried out for 7 hours while maintaining the internal temperature at 30-40°C. The reaction was carried out while gas was generated, and a white solid was precipitated. After the reaction, the pressure in the flask was reduced to distill off the dichloromethane. A pale yellow white solid remained in the flask. By 1 As a result of H-NMR analysis of the solid, it was confirmed that compound 2-1 was generated.
[0229]
[0230] NMR spectrum of compound 2-1;
[0231] 1 H-NMR (solvent: D2O): 4.27 ppm (-CH2-, 4H, s).
[0232] 13 C-NMR (solvent: D2O): 62.6 ppm (-CH2-), 195.3 ppm (C=O).
[0233] <Example 1-2>
[0234] The compound 2-1 obtained in Example 1-1 was not isolated and was directly used in the next reaction. 2049 g of thionyl chloride was added to the flask of Example 1-1. The flask was heated to 80°C and refluxed for 15 hours. As the reaction proceeded, the reflux temperature rose from 52°C to 72°C. Gas generation was confirmed during the reaction. The point where compound 2-1 was completely dissolved and gas generation ended was set as the reaction endpoint. The reaction solution was transferred to a 2L detachable flask, the gas phase was sealed with nitrogen and naturally cooled for 9 hours. As a result, a dark brown solid was precipitated in the detachable flask. Unreacted thionyl chloride was removed by decantation. Toluene was added to wash the precipitated solid, and the toluene was removed again by decantation. Toluene washing was carried out a total of 3 times, and the total amount of toluene used was 1207 g. The precipitated solid was dried at 25°C for 71 hours under a nitrogen flow. The dried solid was recovered and passed through 1 As a result of H-NMR analysis, it was confirmed that 356.5 g of compound 3-1 with a purity of 96.2% was obtained. The yield based on compound 1-1 was 56.0%.
[0235]
[0236] NMR spectrum of compound 3-1;
[0237] 1 H-NMR: 5.20ppm (-CH2-, 4H, s).
[0238] 13 C-NMR: 72.3ppm (-CH2-), 184.6ppm (C=O).
[0239] <Example 1-3>
[0240] In a 1L four-necked flask equipped with a stirrer, a condenser, and a thermometer, 90.0g of compound 3-1 and 750mL of acetonitrile were placed under nitrogen sealing. The flask was cooled in an ice bath, and 110.3g of potassium bifluoride was added while stirring. A slight exotherm occurred with the addition. The ice bath was changed to a water bath, and the reaction was carried out for 62 hours while maintaining the internal temperature at 15-25°C. As the reaction proceeded, a fine white solid was generated. The reaction solution was transferred to a pressure filter to filter out the unreacted potassium bifluoride and the product. Acetonitrile was added to the filter, and the filtered solid was washed until the filtrate became transparent, and the washing liquid was recovered. The acetonitrile was distilled off the filtrate and the washing liquid using an evaporator. 950mL of toluene was added to the dried and remaining solid, and the solid was dissolved in toluene by heating to 100°C. The dissolved solution was naturally filtered to remove the undissolved components. The filtrate was transferred to a 1L separable flask, the gas phase was sealed with nitrogen and cooled naturally for 14 hours. As a result, light brown needle-shaped crystals were precipitated in the separable flask. The crystals were washed with toluene and dried at 25°C for 30 hours under a nitrogen stream. The dried solid was recovered and 1 H-NMR and 19 As a result of F-NMR analysis, it was confirmed that 58.1 g of compound 4-1 with a purity of 97.6% was obtained. The yield based on compound 3-1 was 72.3%.
[0241]
[0242] NMR spectrum of compound 4-1;
[0243] 1 H-NMR: 4.97ppm (-CH2-, 4H, d, J=3.1Hz).
[0244] 19 F-NMR: 62.4ppm (-SO2F, 2F, t, J=3.1Hz).
[0245] 13 C-NMR: 60.7ppm (-CH2-), 184.9ppm (C=O).
[0246] <Example 1-4>
[0247] In a 200mL nickel autoclave, 9.93g of compound 4-1 and 89.7g of acetonitrile were placed. The autoclave was cooled, and nitrogen was supplied at a flow rate of 6.7L / hr while the internal temperature was maintained at 0-5°C, and the reaction solution was bubbled for 1 hour. While the temperature of the reaction solution was maintained at 0-5°C, a mixed gas of fluorine gas and nitrogen (mixing ratio = 10.3 mol% / 89.7 mol%) was introduced at a flow rate of 6.7L / hr for 6 hours. Nitrogen was supplied again at a flow rate of 6.7L / hr, and the reaction solution was bubbled for 1 hour. 103.2g of the reaction solution was recovered from the autoclave. By 19 The reaction solution was quantitatively analyzed by F-NMR, and as a result, it was confirmed that the solution contained 8.4% by mass of compound 5-1. The reaction yield based on compound 4-1 was 66%.
[0248]
[0249] NMR spectrum of compound 5-1;
[0250] 19 F-NMR: -104.1ppm (-CF2-, 4F, s), 45.8ppm (-SO2F, 2F, s).
[0251] <Example 1-5>
[0252] In a 200mL nickel autoclave, 19.9g of compound 4-1 and 85.6g of acetonitrile were added. The autoclave was cooled, and nitrogen was supplied at a flow rate of 6.7L / hr while the internal temperature was maintained at 0-5°C, and the reaction solution was bubbled for 1 hour. While the temperature of the reaction solution was maintained at 0-5°C, a mixed gas of fluorine gas and nitrogen (mixing ratio = 10.3 mol% / 89.7 mol%) was introduced at a flow rate of 16.4L / hr for 6.5 hours. Nitrogen was supplied again at a flow rate of 6.7L / hr, and the reaction solution was bubbled for 1 hour. 109.6g of the reaction solution containing compound 5-1 was recovered from the autoclave.
[0253] <Example 1-6>
[0254] In a 200mL nickel autoclave, 20.1g of compound 4-1 and 80.1g of acetonitrile were added. The autoclave was cooled, and nitrogen was supplied at a flow rate of 6.7L / hr while the internal temperature was maintained at 0-5°C, and the reaction solution was bubbled for 1 hour. While the temperature of the reaction solution was maintained at 0-5°C, a mixed gas of fluorine gas and nitrogen (mixing ratio = 20.0 mol% / 80.0 mol%) was introduced at a flow rate of 8.4L / hr for 6 hours. Nitrogen was supplied again at a flow rate of 6.7L / hr, and the reaction solution was bubbled for 1 hour. 107.1g of the reaction solution containing compound 5-1 was recovered from the autoclave.
[0255] <Example 1-7>
[0256] In a 50 mL four-necked flask equipped with a stirrer, a condenser, a thermometer, and a dropping funnel, 1.65 g of potassium fluoride and 7.8 mL of diethylene glycol dimethyl ether (diglyme) were placed. While the flask was cooled and stirred in an ice bath to keep the internal temperature at 0-10°C, 8.43 g of the reaction solution obtained in Example 1-4 was added dropwise using a plastic syringe. Strong heat release was confirmed, and the addition required 15 minutes. After the addition was completed, the ice bath was replaced with a water bath, and the reaction was carried out at 15-20°C for 1 hour. After cooling in an ice bath again, 6.56 g of compound 6-1 was added dropwise from a dropping funnel while keeping the temperature of the reaction solution at 0-10°C. After the addition was completed, the ice bath was replaced with a water bath, and the reaction was carried out at 20-25°C for 3.5 hours. The by-product solids were removed from the reaction solution by suction filtration, and the filtrate was recovered. The filtered residual solids were washed with an appropriate amount of acetonitrile, and the washing liquid was mixed with the filtrate. By 19 37.1 g of the filtrate was quantitatively analyzed by F-NMR, and it was confirmed that the filtrate contained 2.04% by mass of compound 7-1. The reaction yield based on compound 4-1 was 46.6%.
[0257]
[0258] NMR spectrum of compound 7-1;
[0259] 19 F-NMR: -191.5ppm (CF2=CF-, 1F, ddt, J=116, 38, 14Hz), -133.8ppm (-O-CF-, 1F, tt, J=21.3, 6.1Hz), -103.1ppm (-CF2-SO2F, 4F, m), -101. 5ppm (CF2=CF-, 1F, ddt, J=116, 49, 27Hz), -87.6ppm (CF2=CF-, 1F, ddt, J=49, 38, 7Hz), -67.5ppm (-CF2-O-, 2F, m), 46.8ppm (-SO2F, 2F, s).
[0260] <Example 1-8>
[0261] Into a 500mL four-necked flask equipped with a stirrer, a condenser, a thermometer, and a dropping funnel, 36.6g of potassium fluoride and 125.6g of acetonitrile were placed. While the flask was cooled in an ice bath and stirred to maintain the internal temperature at 0-10°C, 79.8g of the reaction solution obtained in Example 1-5 was added dropwise using a plastic dropping funnel. Strong heat release was confirmed, and the addition required 23 minutes. After the addition was completed, the ice bath was replaced with a water bath, and the reaction was carried out at 20-30°C for 5.5 hours. The flask was cooled in an ice bath again, and 146.0g of compound 6-1 was added dropwise from the dropping funnel while maintaining the temperature of the reaction solution at 0-10°C. After the addition was completed, the ice bath was replaced with a water bath, and the reaction was carried out at 15-25°C for 16 hours. Suction filtration was performed in the same manner as in Example 1-7, and the reaction mixture was filtered through 19 The obtained filtrate 412.3 g was quantitatively analyzed by F-NMR, and the result confirmed that it contained 3.93% by mass of compound 7-1. The reaction yield based on compound 4-1 was 55.9%. The filtrate was subjected to reduced pressure distillation, thereby isolating compound 7-1 in the form of a boiling point 97.2°C / 10kPa fraction. The gas chromatography purity was 98.0%.
[0262] <Example 1-9>
[0263] Into a 50 mL four-necked flask equipped with a stirrer, a condenser, a thermometer, and a dropping funnel, 3.70 g of potassium fluoride and 10.9 g of acetonitrile were placed. While cooling the flask in an ice bath and stirring to maintain the internal temperature at 0-10°C, 10.2 g of the reaction solution obtained in Example 1-6 was added dropwise using a plastic syringe. Strong heat release was observed, and the addition required 8 minutes. After the addition was completed, the ice bath was replaced with a water bath, and the reaction was carried out at 20-30°C for 3 hours. Cooling was performed again in an ice bath, and 14.6 g of compound 6-1 was added dropwise from the dropping funnel while maintaining the temperature of the reaction solution at 0-10°C. After the addition was completed, the ice bath was replaced with a water bath, and the reaction was carried out at 15-25°C for 17 hours. Suction filtration was performed in the same manner as in Example 1-7, and the reaction mixture was filtered through 19 F-NMR quantitative analysis of 55.9 g of the obtained filtrate confirmed that it contained 4.77% by mass of compound 7-1. The reaction yield based on compound 4-1 was 69.6%. In addition, the reaction yield based on compound 1-1 (the reaction yield in the entire monomer synthesis step) was 28.2%.
[0264] [Example 2]
[0265] (Example 2-1)
[0266] 70.0 g of compound 7-1 was added to an autoclave (internal volume 100 mL, made of stainless steel), cooled with liquid nitrogen and degassed. 2.53 g of TFE was introduced into the autoclave, and the internal temperature was heated in an oil bath until the internal temperature reached 100°C. The pressure at this time was 0.29 MPaG (gauge pressure). A mixed solution of 36.3 mg of PFtBPO and 2.58 g of HFC-52-13p as a polymerization initiator was pressed into the autoclave. Nitrogen was then introduced from the injection line to completely squeeze the injection liquid into the injection line. Through this operation, the TFE in the gas phase was diluted, resulting in an increase in pressure to 0.56 MPaG. TFE was continuously added while maintaining the pressure at 0.56 MPaG to carry out polymerization. After 9.5 hours and when the amount of TFE added was 4.03 g, the autoclave was cooled to stop the polymerization and the gas in the system was purged. After the reaction solution was diluted with HFC-52-13p, HFE-347pc-f was added to aggregate the polymer and filtered. Thereafter, the operation of stirring the polymer in HFC-52-13p and reaggregating it in HFE-347pc-f was repeated twice. Vacuum drying was performed at 120°C to obtain a copolymer of TFE and compound 7-1, namely polymer F-1. The various physical properties of the obtained polymer F-1 were measured. The results are shown in Table 1.
[0267] (Example 2-2)
[0268] The conditions of Example 2-1 were changed as shown in Table 1. In Example 2-2, the initial charging of TFE was not performed. Instead, after heating to the polymerization temperature, TFE was blown in until the pressure before nitrogen dilution recorded in Table 1 was reached. Other than that, the same operation as in Example 2-1 was performed to obtain polymer F-2. The above-mentioned various physical properties were measured using the obtained polymer F-2. The results are shown in Table 1.
[0269] [Table 1]
[0270]
[0271] [Example 3]
[0272] <Example 3-1>
[0273] Using polymer F-1, a film of polymer H-1 was obtained by the following method.
[0274] The polymer F-1 was press-formed at a temperature 10°C higher than the TQ value and 4MPa (gauge pressure) to obtain a film of the polymer F-1. The film of the polymer F-1 was immersed in an alkaline aqueous solution A (potassium hydroxide / water = 20 / 80 (mass ratio)) at 80°C for 16 hours to hydrolyze -SO2F of the polymer F-1 and convert it into -SO3K. The polymer film was then immersed in a 3 mol / L hydrochloric acid aqueous solution at 50°C for 30 minutes, and then immersed in ultrapure water at 80°C for 30 minutes. A total of 5 cycles of immersion in an aqueous hydrochloric acid solution and immersion in ultrapure water were performed to convert -SO3K of the polymer into -SO3H. Washing with ultrapure water was repeated until the pH of the water in which the polymer film was immersed became 7. The polymer film was clamped with filter paper and air-dried to obtain a film of polymer H-1.
[0275] <Example 3-2>
[0276] A film of polymer H-2 was obtained in the same manner as in Example 3-1 except that polymer F-2 was used instead of polymer F-1 and alkali aqueous solution C (potassium hydroxide / methanol / water=15 / 20 / 65 (mass ratio)) was used instead of alkali aqueous solution A.
[0277] [Example 4]
[0278] <Example 4-1>
[0279] Into a Hastelloy alloy autoclave with an internal volume of 230 mL, 123.8 g of PSVE, 35.2 g of HCFC-225cb, and 63.6 mg of AIBN were added, and the mixture was cooled with liquid nitrogen and degassed. The temperature was raised to 70°C, TFE was introduced into the system, and the pressure was maintained at 1.14 MPa (gauge pressure). TFE was continuously added to keep the pressure constant at 1.14 MPa (gauge pressure). After 7.9 hours, when the amount of TFE added was 12.4 g, the autoclave was cooled, and the gas in the system was purged to terminate the reaction. After diluting the polymer solution with HCFC-225cb, HCFC-141b was added and aggregated. After washing with HCFC-225cb and HCFC-141b, the mixture was dried to obtain 25.1 g of polymer F'-1, which is a copolymer of TFE and PSVE. The results are shown in Table 2.
[0280] [Table 2]
[0281]
[0282] [Example 5]
[0283] <Example 5-1>
[0284] A film of polymer H'-1 was obtained in the same manner as in Example 3-1 except that polymer F'-1 was used instead of polymer F-1.
[0285] [Example 6]
[0286] <Example 6-1>
[0287] 4.3 g of a thinly cut polymer H-1 film and 75 g of ultrapure water were added to a 100 mL polytetrafluoroethylene (PTFE) container and heated at 200° C. for 24 hours. The contents were transferred to a PTFE cylinder and air-dried for 64 hours at 30° C. under a nitrogen atmosphere. The dried polymer H-1 was transferred to a 200 mL glass autoclave and 21.4 g of a mixed solvent of ultrapure water / ethanol (50 / 50 (mass ratio)) was added. After stirring at 110° C. for 25 hours, 3.87 g of ultrapure water was added for dilution. After stirring at 90° C. for 5 hours, the mixture was cooled naturally and filtered using a pressure filter (filter paper: ADVANTEC TOYO, PF040) to obtain 31.9 g of a liquid composition S-1 in which polymer H-1 was dispersed in a mixed solvent.
[0288] The liquid composition S-1 was coated on a 100 μm ethylene-tetrafluoroethylene copolymer (ETFE) sheet by a die coater to form a film, which was dried at 80° C. for 15 minutes and then heat-treated at 185° C. for 30 minutes to obtain a solid polymer electrolyte membrane 1 formed of a film of polymer H as an electrolyte. It should be noted that the coating amount of the liquid composition was adjusted so that the film thickness of the solid polymer electrolyte membrane would be the value described in Tables 3-1 to 3-2. The results are shown in Table 3-1.
[0289] <Example 6-2~Example 6-16>
[0290] The same operation as in Example 6-1 was performed except that the polymer H or polymer H' described in Table 3-1 to Table 3-2 was used instead of the polymer H-1 to prepare the liquid composition, and the coating amount of the liquid composition was adjusted so that the film thickness of the solid polymer electrolyte membrane became the value described in Table 3-1 to Table 3-2, thereby obtaining solid polymer electrolyte membranes 2 to 16 formed of a film of polymer H or H'. The results are shown in Table 3-1 to Table 3-2.
[0291] [Table 3-1]
[0292]
[0293] [Table 3-2]
[0294]
[0295] In Tables 3-1 and 3-2, “2.10E-09” and the like are abbreviations of exponential notation. As a specific example, “2.10E-09” means “2.10×10 -9 ” The same applies to Table 4-1 and Table 4-2 described later.
[0296] [Example 7]
[0297] <Example 7-1>
[0298] The polymer H'-1 was mixed with a mixed solvent of ethanol / water (60 / 40 (mass ratio)) to obtain a polymer H'-1 dispersion having a solid content concentration of 25.8% by mass.
[0299] To 44g of a catalyst (manufactured by Tanaka Precious Metals Industry Co., Ltd.) loaded with 46% by mass of platinum in carbon powder, 221.76g of water and 174.24g of ethanol were added, and the mixture was pulverized using an ultrasonic homogenizer to obtain a dispersion of the catalyst. To the dispersion of the catalyst, 102.06g of a mixed solution obtained by pre-mixing and kneading 80.16g of a polymer H'-1 dispersion, 44.4g of ethanol, and 25.32g of ZEORORA-H (manufactured by ZEON Co., Ltd., Japan) was added, and further 26.77g of water and 12g of ethanol were added, and the mixture was mixed using an ultrasonic homogenizer, and the solid content concentration was set to 10% by mass to obtain a coating liquid for forming a catalyst layer. The liquid was applied to an ETFE sheet using a die coater, dried at 80°C, and then heat treated at 160°C for 30 minutes to form a platinum content of 0.4mg / cm 2 of the catalyst layer.
[0300] 81.6 g of ethanol and 154.4 g of distilled water were added to 50 g of vapor-grown carbon fiber (manufactured by Showa Denko K.K., trade name: VGCF-H, fiber diameter of about 150 nm, fiber length of 10 to 20 μm), and stirred thoroughly. 89 g of a polymer H'-1 dispersion obtained by mixing polymer H'-1 with a mixed solvent of ethanol / water (60 / 40 (mass ratio)) at a solid content concentration of 28.1% was added thereto, stirred thoroughly, and then mixed and pulverized using an ultrasonic homogenizer to prepare a coating liquid for forming an intermediate layer.
[0301] The intermediate layer forming coating liquid was coated with a die coater to a solid content of 3 mg / cm 2 The carbon nonwoven fabric was coated on the surface of a gas diffusion substrate (manufactured by NOK Co., Ltd., trade name: X0086 T10X13) in a manner and dried at 80° C. to prepare a gas diffusion substrate with an intermediate layer having an intermediate layer formed on the surface of the carbon nonwoven fabric.
[0302] The solid polymer electrolyte membrane 1 was sandwiched from both sides by two ETFE sheets with catalyst layers, and heated and pressed under the conditions of a pressing temperature of 160°C, a pressing time of 2 minutes, and a pressure of 3 MPa. The catalyst layers were bonded to both sides of the solid polymer electrolyte membrane 1, and the ETFE film was peeled off from the catalyst layer, thereby obtaining an electrode with an area of 25 cm 2 A membrane catalyst layer assembly.
[0303] In the above membrane catalyst layer assembly, a gas diffusion substrate with a carbon layer (manufactured by NOK, trade name: X0086 IX92 CX320) was arranged on the anode side in such a manner that the carbon layer and the intermediate layer were in contact with the catalyst layer side, and the gas diffusion substrate with the intermediate layer was arranged on the cathode side. Heating and pressing were performed under the conditions of a pressing temperature of 160°C, a pressing time of 2 minutes, and a pressure of 3MPa to produce a membrane electrode assembly for initial power generation characteristics evaluation and hydrogen leakage evaluation. The results are shown in Table 4-1.
[0304] <Examples 7-2 to 7-8, Examples 7-11 to 7-18>
[0305] The membrane electrode assembly for initial power generation characteristic evaluation and hydrogen gas leakage evaluation was prepared in the same manner as in Example 7-1 except that the solid polymer electrolyte membranes 2 to 16 listed in Tables 3-1 and 3-2 were used instead of the solid polymer electrolyte membrane 1 obtained in Example 6-1. The results are shown in Tables 4-1 and 4-2.
[0306] <Example 7-9>
[0307] The solid polymer electrolyte membrane 8 described in Table 3-1 was used instead of the solid polymer electrolyte membrane 1 obtained in Example 6-1, and the polymer H'-2 dispersion liquid shown below was used instead of the polymer H'-1 dispersion liquid used to prepare the catalyst layer forming coating liquid, and the addition amount was adjusted in such a way that the mass ratio of the polymer in the catalyst layer forming coating liquid to the catalyst carrier remained unchanged. Except for this, the membrane electrode assembly for initial power generation characteristic evaluation and hydrogen leakage evaluation was prepared in the same manner as in Example 7-1. The results are shown in Table 4-1.
[0308] The polymer H'-2 dispersion was prepared as follows.
[0309] 459.97 g of the monomer shown in formula m32-1 and 79.28 g of the monomer shown in formula m22-1 were added to a stainless steel autoclave with an internal volume of 230 mL, and the mixture was fully degassed under cooling with liquid nitrogen. 22.38 g of TFE was added and the temperature was raised to 22° C. 161.5 mg of a free radical polymerization initiator ((C3F7COO)2) dissolved in a solvent (AGC, trade name: AC-2000) at a concentration of 2.91% by mass was added, and the feed line was cleaned with 2 g of AC-2000 to start the reaction. After stirring for 24 hours, the autoclave was cooled to stop the reaction.
[0310] The product was diluted with AC-2000 and then mixed with a mixture of AC-2000:methanol = 8:2 (mass ratio), and the polymer was aggregated and filtered. The polymer was washed in a mixture of AC-2000:methanol = 7:3 (mass ratio), separated by filtration, and the solid content was dried under reduced pressure at 80°C overnight to obtain a polymer (F'-2).
[0311] The obtained polymer (F'-2) was immersed in a 50°C aqueous solution containing 20% by mass of methanol and 15% by mass of potassium hydroxide for 40 hours, thereby hydrolyzing the -SO2F group in the polymer (F'-2) and converting it into a -SO3K group. Next, the polymer was immersed in a 3 mol / L hydrochloric acid aqueous solution at room temperature for 2 hours. The hydrochloric acid aqueous solution was replaced and the same treatment was repeated 4 times to obtain a polymer H'-2 in which the -SO3K group in the polymer was converted into a sulfonic acid group.
[0312] use 19 The results of F-NMR analysis on the composition of the structural units constituting polymer H'-2 showed that in polymer H'-2, relative to all the units contained in polymer H'-2, the content of the monomer unit represented by formula m22-1 was 50 mol%, the content of the monomer unit represented by formula m32-1 was 21.3 mol%, and the content of the TFE unit was 28.7 mol%.
[0313]
[0314] The obtained polymer H'-2 was mixed with a mixed solvent of ethanol / water (60 / 40 (mass ratio)) to obtain a polymer H'-2 dispersion having a solid content concentration of 10% by mass.
[0315] <Example 7-10>
[0316] The following polymer H'-3 dispersion was used instead of the polymer H'-2 dispersion used to prepare the catalyst layer-forming coating solution, and the addition amount was adjusted so that the mass ratio of the polymer to the catalyst support in the catalyst layer-forming coating solution remained unchanged. The same operation as in Example 7-9 was performed to prepare a membrane electrode assembly for initial power generation characteristic evaluation and hydrogen leakage evaluation. The results are shown in Table 4-1.
[0317] Polymer H'-3 was obtained in the same manner as the synthesis method of Polymer H'-2 except that the amount of each monomer used in the synthesis of Polymer H'-2 was adjusted.
[0318] use 19 The results of F-NMR analysis of the composition of the structural units constituting polymer H'-3 showed that in polymer H'-3, relative to all the units contained in polymer H'-3, the content of the monomer unit represented by formula m22-1 was 65 mol%, the content of the monomer unit represented by formula m32-1 was 17 mol%, and the content of the TFE unit was 18 mol%.
[0319] A polymer H'-3 dispersion was obtained in the same manner as in the preparation of the polymer H'-2 dispersion except that the polymer H'-3 was used instead of the polymer H'-2.
[0320] [Table 4-1]
[0321]
[0322] [Table 4-2]
[0323]
[0324] In the above Tables 4-1 to 4-2, the difference in hydrogen permeability coefficient refers to the value (Hc-Hk) obtained by subtracting the hydrogen permeability coefficient of the above-mentioned polymer electrolyte contained in the electrolyte membrane (hereinafter also referred to as "Hk") from the hydrogen permeability coefficient of the polymer having ion exchange groups in the catalyst layer of the cathode.
[0325] As shown in Tables 3-1 to 3-2 and Tables 4-1 to 4-2, if the hydrogen permeability coefficient under the conditions of temperature 80°C and relative humidity 10% is 2.4×10 -9 cm 3 cm / (s cm 2 ·cmHg) or less and a solid polymer electrolyte membrane with a membrane thickness of 7 to 20 μm can obtain a solid polymer fuel cell with excellent power generation characteristics and hydrogen utilization efficiency (Examples 6-1 to 6-8 and Examples 7-1 to 7-10).
[0326] In contrast, when using a solid polymer electrolyte membrane in which at least one of the hydrogen permeability coefficient and membrane thickness is outside the above range, the solid polymer fuel cell obtained using it has poor at least one of the power generation characteristics and hydrogen utilization efficiency (Examples 6-9 to 6-16, Examples 7-11 to 7-18).
[0327] It should be noted that the entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2019-036477 filed on February 28, 2019 are cited herein and incorporated as the disclosed contents of the present specification.
[0328] Industrial Applicability
[0329] 10 Membrane Electrode Assembly
[0330] 11 Catalyst layer
[0331] 12 Gas Diffusion Layer
[0332] 13 Anode
[0333] 14 Cathode
[0334] 15 Electrolyte membrane
Claims
1. A solid polymer electrolyte membrane, characterized in that: The polymer electrolyte has a hydrogen permeability of 2.4×10 -9 cm 3 cm / (s cm 2 cmHg) or less, The solid polymer electrolyte membrane has a thickness greater than 10 μm and less than 20 μm. The polymer electrolyte is a perfluoropolymer having an acidic sulfonic acid group.
2. The solid polymer electrolyte membrane according to claim 1, wherein The perfluoropolymer comprises perfluoro monomer units, The perfluoromonomer unit includes at least one unit selected from the group consisting of a perfluorovinyl ether unit and a perfluoroallyl ether unit.
3. The solid polymer electrolyte membrane according to claim 1 or 2, wherein: The perfluoropolymer does not substantially contain at least one unit selected from the group consisting of a unit having a halogen atom other than a fluorine atom, a unit having a ring structure, and a unit having a crosslinked structure formed by a covalent bond.
4. The solid polymer electrolyte membrane according to claim 2, wherein: The perfluoroallyl ether unit is a unit represented by formula A-1, In formula A-1, R F1 and R F2 Each is independently a perfluoroalkylene group having 1 to 3 carbon atoms.
5. The solid polymer electrolyte membrane according to claim 2, wherein: The perfluoromonomer units further include tetrafluoroethylene units.
6. The solid polymer electrolyte membrane according to claim 1 or 2, wherein: The ion exchange capacity of the polymer electrolyte is 1.4 to 2.5 milliequivalents per gram of dry resin.
7. A membrane electrode assembly, characterized in that: The invention comprises: an anode having a catalyst layer, a cathode having a catalyst layer, and the solid polymer electrolyte membrane according to any one of claims 1 to 6 arranged between the anode and the cathode.
8. The membrane electrode assembly according to claim 7, wherein: The catalyst layer of the cathode comprises a catalyst and a polymer having ion exchange groups, The value obtained by subtracting the hydrogen permeability coefficient of the polymer electrolyte from the hydrogen permeability coefficient of the polymer having an ion exchange group is 1.0×10 -8 cm 3 cm / (s cm 2 ·cmHg) or above.
9. A solid polymer fuel cell, characterized in that: It comprises the membrane electrode assembly according to claim 7 or 8.