Polishing composition, polishing method, and method for producing semiconductor substrate
Patent Information
- Application Number
- CN202110291363.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-19
- Filing Date
- 2021-03-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-03-18
AI Technical Summary
In the polishing process of the semiconductor substrate, the polishing speed of the existing polishing composition has not been sufficiently increased, and it is easy to cause scratches and scratches on the surface of the polishing object.
A polishing composition containing negative zeta potential abrasive grains, alkaline inorganic compounds and anionic water-soluble polymers is used. The aspect ratio of the abrasive grains is less than 1.1 and the particle size distribution is wide. The laser diffraction and scattering method is used to ensure that D90/D50 is greater than 1.3. , the basic inorganic compound is an alkali metal salt, combined with anionic water-soluble polymer and dispersion medium, to improve the grinding speed and surface treatment effect.
It significantly increases the grinding speed, reduces scratches and abrasions on the surface of the grinding object, enhances the grinding efficiency and stability, and ensures the efficiency and quality of the grinding process.
Smart Images

Figure BDA0002982118160000191 
Figure BDA0002982118160000222 
Figure BDA0002982118160000231
Abstract
Description
Technical Field
[0001] The present invention relates to a polishing composition, a polishing method, and a method for producing a semiconductor substrate. Background Art
[0002] In recent years, with the multi-layer wiring on the surface of semiconductor substrates, the semiconductor substrates are physically polished to be flattened during device manufacturing, which is the so-called chemical mechanical polishing (CMP) technology. CMP is a method of flattening the surface of a polishing object (polished object) such as a semiconductor substrate using a polishing composition (slurry) containing abrasives such as silicon dioxide, aluminum oxide, and cerium oxide, an anticorrosive agent, a surfactant, etc. Specifically, it is used in shallow trench isolation (STI), interlayer dielectric film (ILD film) flattening, tungsten plug formation, and formation of multi-layer wiring formed by copper and low dielectric constant films.
[0003] For example, Japanese Patent Publication No. 2001-185516 discloses a kind of grinding composition, and it comprises water-soluble polymer, polyacrylic acid and abrasive grains added with alkylene oxide.Through this technology, can grind with high grinding speed, and can suppress the generation of the scratch of the grinding surface of the grinding object accompanying with grinding. Summary of the invention
[0004] Problem that the invention aims to solve
[0005] However, the technique described in Japanese Patent Application Laid-Open No. 2001-185516 has a problem that the improvement in polishing rate is not sufficient.
[0006] Solutions for solving problems
[0007] Therefore, an object of the present invention is to provide a polishing composition that can polish an object to be polished at a high polishing rate.
[0008] Effects of the Invention
[0009] The present inventors have repeatedly conducted in-depth studies to solve the above problems. As a result, they found that the above problems can be solved by the following polishing composition: the polishing composition comprises abrasive grains, a basic inorganic compound, an anionic water-soluble polymer and a dispersion medium, the zeta potential of the abrasive grains is negative, the aspect ratio of the abrasive grains is 1.1 or less, in the particle size distribution of the abrasive grains obtained by laser diffraction scattering method, the ratio D90 / D50 of the diameter D90 of the grains when the cumulative particle mass from the microparticle side reaches 90% of the total particle mass to the diameter D50 of the grains when the cumulative particle mass from the microparticle side reaches 50% of the total particle mass is greater than 1.3, and the basic inorganic compound is an alkali metal salt. DETAILED DESCRIPTION
[0010] The following describes the embodiments of the present invention, but the present invention is not limited to the following embodiments. It should be noted that, unless otherwise specified, the operation and physical properties are measured under the conditions of room temperature (20-25°C) / relative humidity 40-50%RH. In addition, in this specification, "X-Y" indicating a range means "above X and below Y".
[0011] <Polishing Composition>
[0012] The present invention is a polishing composition for polishing a polishing object, which comprises abrasive grains, an alkaline inorganic compound, anionic water-soluble polymer and a dispersion medium, wherein the zeta potential of the abrasive grains is negative, the aspect ratio of the abrasive grains is less than 1.1, and in the particle size distribution of the abrasive grains obtained by a laser diffraction scattering method, the ratio D90 / D50 of the diameter D90 of the particles when the cumulative particle mass from the particle side reaches 90% of the total particle mass to the diameter D50 of the particles when the cumulative particle mass from the particle side reaches 50% of the total particle mass is greater than 1.3, and the alkaline inorganic compound is an alkali metal salt.
[0013] The reason why the polishing composition of the present invention exhibits the above-mentioned effects is not clear, but is considered to be as follows.
[0014] The polishing composition generally polishes the object to be polished by physical action based on friction with the substrate surface, chemical action of components other than the abrasive on the substrate surface, and a combination thereof. Therefore, the shape and type of the abrasive have a great influence on the polishing rate.
[0015] The grinding composition of the present invention contains abrasive grains having a predetermined shape and a predetermined particle size distribution. That is, the abrasive grains used in the grinding composition are formed by spherical particles having an aspect ratio of less than 1.1 and thus close to a true sphere, and are further formed by particles having a wide particle size distribution because D90 / D50 is greater than 1.3. Since the abrasive grains are spherical particles close to a true sphere, the abrasive grains rotate efficiently in the grinding surface. Thus, the abrasive grains can fully apply mechanical force to the grinding surface while rotating, so that grinding can be performed appropriately. Furthermore, since the particle size distribution of the abrasive grains is wide, there are abrasive grains with relatively small sizes and abrasive grains with relatively large sizes. The abrasive grains with relatively small sizes are contacted with abrasive grains with relatively large sizes, so that the rotation in the grinding surface is suppressed and they are easily retained on the grinding surface. When the particles with relatively small sizes retained on the grinding surface rotate again by contact with other particles, a larger mechanical force is applied to the grinding surface compared to the particle size. As described above, it can be inferred that the abrasive grains having a wide particle size distribution and close to a true sphere can achieve effective grinding at each particle size, thereby further improving the grinding speed of the object to be ground. That is, the present invention has found a balance between the aspect ratio and particle size distribution of the abrasive grains that can effectively act on the grinding surface.
[0016] In addition, the zeta (ζ) potential of the abrasive grains contained in the polishing composition of the present invention is negative. In other words, in the polishing composition, abrasive grains with a negative zeta potential are used. Here, the anionic water-soluble polymer contained in the polishing composition of the present invention is a polymer, so it is easy to adhere to the surface of the polishing pad (for example, polyurethane). By attaching the anionic water-soluble polymer to the surface of the polishing pad, the zeta potential of the polishing pad surface is negative. Specifically, when the zeta potential of the pad surface is positive, the zeta potential of the pad surface becomes negative by the attachment of the anionic water-soluble polymer, and when the zeta potential of the pad surface is negative, the absolute value of its zeta potential increases by the attachment of the anionic water-soluble polymer. It can be inferred that when the polishing composition is used to polish the polishing object, a repulsion based on negative charges is generated between the polishing pad in contact with the polishing composition and the abrasive grains in the polishing composition, and through this repulsion, the abrasive grains become easier to act on the surface of the polishing object, and the polishing speed is further improved.
[0017] Furthermore, the grinding composition of the present invention comprises an alkaline inorganic compound belonging to an alkali metal salt. For example, compared with an alkaline organic compound, an alkaline inorganic compound is more likely to improve the conductivity of the grinding composition. It is thus believed that the grinding speed based on the grinding composition is further improved. In addition, by making the alkaline inorganic compound an alkali metal salt, there is no large steric volume compared with the alkaline organic compound, and thus, the alkaline inorganic compound and the anionic water-soluble polymer are not easy to form aggregates. Therefore, the grinding composition of the present invention is a stable dispersion state of anionic water-soluble polymers, so the anionic water-soluble polymers can be efficiently attached to the polishing pad.
[0018] As described above, it is believed that the polishing composition of the present invention further improves the polishing properties of the abrasive particles by comprising a combination of abrasive particles with high grinding force having a predetermined shape and a predetermined particle size distribution, anionic water-soluble polymers, and a specific basic inorganic compound. However, the mechanism described above is only a speculation and obviously does not limit the technical scope of the present invention.
[0019] [Object to be polished]
[0020] The material contained in the object to be polished by the polishing composition of the present invention is not particularly limited, and examples thereof include silicon oxide, silicon nitride (SiN), silicon carbonitride (SiCN), polycrystalline silicon (polysilicon), amorphous silicon (amorphous silicon), metal, SiGe, and the like.
[0021] The polishing object of the present invention preferably comprises silicon oxide or silicon nitride, more preferably comprises silicon oxide. Therefore, the polishing composition of the present invention is preferably used for polishing a polishing object comprising silicon oxide or silicon nitride, more preferably for polishing a polishing object comprising silicon oxide.
[0022] Examples of films containing silicon oxide include TEOS (Tetraethyl Orthosilicate) type silicon oxide films (hereinafter also referred to as "TEOS films") generated using tetraethyl orthosilicate as a precursor, HDP (High Density Plasma) films, USG (Undoped Silicate Glass) films, PSG (Phosphorus Silicate Glass) films, BPSG (Boron-PhosphoSilicate Glass) films, RTO (Rapid Thermal Oxidation) films, and the like.
[0023] [Abrasive grains]
[0024] The grinding composition of the present invention contains abrasive grains. There is no particular limitation on the type of abrasive grains used in the grinding composition of the present invention, and examples thereof include oxides such as silicon dioxide, aluminum oxide, zirconium oxide, and titanium oxide. The abrasive grains can be used alone or in combination of two or more. The abrasive grains can be commercially available or synthetic. As the type of abrasive grains, aluminum oxide is preferred. That is, the grinding composition of the present invention contains aluminum oxide (preferably aluminum oxide obtained by the later-described deflagration method) as abrasive grains.
[0025] In the polishing composition of the present invention, the abrasive particles show a negative zeta potential, the aspect ratio of the abrasive particles is less than 1.1, and in the particle size distribution of the abrasive particles determined by a laser diffraction scattering method, the ratio D90 / D50 of the particle diameter D90 when the cumulative particle mass from the microparticle side reaches 90% of the total particle mass to the particle diameter D50 when the cumulative particle mass from the microparticle side reaches 50% of the total particle mass is greater than 1.3.
[0026] The abrasive used in the polishing composition of the present invention shows a negative zeta potential. Here, "zeta (ζ) potential" refers to the potential difference generated at the interface of a solid and a liquid in contact with each other when the two are in relative motion. In the polishing composition of the present invention, the abrasive has a negative charge, thereby increasing the polishing speed of the polishing object. The zeta potential of the abrasive is preferably above -80mV and below -5mV, more preferably above -60mV and below -20mV. By making the abrasive (aluminum oxide) have a zeta potential in such a range, the polishing speed of the polishing object can be further increased.
[0027] The zeta potential of the abrasive in the polishing composition is calculated as follows: the polishing composition is supplied to ELS-Z2 manufactured by Otsuka Electronics Co., Ltd., and measured by the laser Doppler method (electrophoretic light scattering measurement method) using a flow cell at a measurement temperature of 25° C., and the obtained data is analyzed by the Smoluchowski equation.
[0028] The aspect ratio of the abrasive used in the grinding composition of the present invention is less than 1.1. By using abrasives with an aspect ratio of less than 1.1, the grinding surface is effectively rotated, thereby improving the grinding speed. In the grinding composition of the present invention, when the aspect ratio of the abrasive is greater than 1.1, a large amount of abrasives will be retained on the grinding surface, and there is a concern that excessive grinding will occur due to a large amount of retained abrasives. The aspect ratio of the abrasive is preferably less than 1.1, more preferably less than 1.09, and further preferably less than 1.08. If it is such a range, the grinding speed can be further improved. It is speculated that the deformation of the particles when stress is applied to spherical particles close to a true sphere, and the destruction caused by the deformation is less likely to occur, and a greater stress can be conducted to the grinding object. The aspect ratio of the abrasive is 1 when it is a true sphere, so its lower limit is more than 1. It should be noted that the aspect ratio of the abrasive is the smallest rectangle circumscribed with the image of the abrasive particles by a scanning electron microscope, and the average of the values obtained by dividing the length of the long side of the rectangle by the length of the short side of the same rectangle, which can be obtained using conventional image analysis software. Specifically, 100 abrasive grains can be randomly selected from an image measured by a scanning electron microscope (SEM) (manufactured by Hitachi High Technology Co., Ltd., product name: SU8000), and their average major diameter and average minor diameter can be measured and calculated, and then calculated by the formula "average major diameter / average minor diameter". The details of the measurement and calculation method of the aspect ratio of the abrasive grains are described in the Examples.
[0029] For the abrasive used in the grinding composition of the present invention, in the particle size distribution obtained by the laser diffraction scattering method, the ratio D90 / D50 of the diameter D90 of the particles when the cumulative particle mass from the particle side reaches 90% of the total mass of the particles and the diameter D50 of the particles when the cumulative particle mass from the particle side reaches 50% of the total mass of the particles is greater than 1.3. Thus, in the grinding composition, there are relatively small abrasives and relatively large abrasives. The relatively small abrasives are suppressed from rotating in the grinding surface by contacting with the relatively large abrasives. As a result, the relatively small abrasives can fully apply mechanical force to the grinding object during grinding, and the grinding speed of the grinding object can be further increased. When the D90 / D50 is below 5.0, the grinding speed decreases.
[0030] D90 / D50 is preferably more than 1.5, more preferably more than 1.8, further preferably more than 2.0, and particularly preferably more than 2.5. If it is such a range, the grinding speed can be further improved. In addition, in the particle size distribution of the abrasive in the grinding composition obtained by the laser diffraction scattering method, the upper limit of the ratio D90 / D50 of the diameter (D90) of the particle when the cumulative particle mass from the particle side reaches 90% of the total mass of the particle and the diameter (D50) of the particle when the cumulative particle mass from the particle side reaches 50% of the total mass of the particle is not particularly limited, preferably less than 4.0, more preferably less than 3.5. If it is such a range, it is possible to suppress the defects such as scratches that may occur on the surface of the grinding object after grinding using the grinding composition.
[0031] The size of abrasive grains is not particularly limited, and the lower limit of the average primary particle size of the abrasive grains obtained by image analysis according to the observation photograph of a scanning electron microscope is preferably more than 10nm, more preferably more than 25nm, and more preferably more than 50nm. In addition, in the grinding composition of the present invention, the upper limit of the average primary particle size of abrasive grains is preferably less than 500nm, more preferably less than 250nm, and more preferably less than 200nm. If it is such a range, it is possible to suppress the defects such as scratches that may be produced on the surface of the grinding object after grinding using the grinding composition. That is, the average primary particle size of abrasive grains is preferably more than 10nm and less than 500nm, more preferably more than 25nm and less than 250nm, and more preferably more than 50nm and less than 200nm. It should be noted that the average primary particle size of abrasive grains can be calculated based on the specific surface area of the abrasive grains measured by the BET method, for example.
[0032] In the grinding composition of the present invention, the lower limit of the average secondary particle size of abrasive particles is preferably more than 30nm, more preferably more than 80nm, more preferably more than 100nm, and more preferably more than 150nm. In addition, in the grinding composition of the present invention, the upper limit of the average secondary particle size of abrasive particles is preferably less than 1000nm, more preferably less than 500nm, more preferably less than 400nm, and particularly preferably less than 350nm. If it is such a range, it is possible to suppress the defects such as scratches that may be produced on the surface of the grinding object after grinding using the grinding composition. That is, the average secondary particle size of abrasive particles is preferably more than 30nm and less than 1000nm, more preferably more than 80nm and less than 500nm, more preferably more than 100nm and less than 400nm, and particularly preferably more than 150nm and less than 350nm. It should be noted that the average secondary particle size of abrasive particles can be measured, for example, by a dynamic light scattering method represented by a laser diffraction scattering method. That is, the average secondary particle size of the abrasive grains corresponds to the diameter D50 of the grains when the cumulative particle mass from the fine particle side accounts for 50% of the total particle mass in the particle size distribution of the abrasive grains determined by the laser diffraction scattering method.
[0033] The average degree of association of the abrasive is preferably 4.0 or less, more preferably 3.0 or less, and further preferably 2.5 or less. As the average degree of association of the abrasive decreases, the occurrence of defects on the surface of the object to be polished can be further reduced. In addition, the average degree of association of the abrasive is preferably 1.5 or more, more preferably 1.8 or more. As the average degree of association of the abrasive increases, there is an advantage of increasing the polishing speed of the polishing composition. It should be noted that the average degree of association of the abrasive is obtained by dividing the value of the average secondary particle size of the abrasive by the value of the average primary particle size.
[0034] The size of the abrasive grains (average grain size, aspect ratio, D90 / D50, etc.) can be appropriately controlled by selecting a method for producing the abrasive grains, etc.
[0035] The destructive strength of the abrasive used in the present invention is preferably 0.5 GPa or more. The destructive strength of the abrasive is not particularly limited as long as it is 0.5 GPa or more, preferably 0.6 GPa or more, more preferably 0.65 GPa or more, further preferably 0.7 GPa or more, further preferably 0.75 GPa or more, and particularly preferably 0.8 Pa or more. When it is in the above range, the grinding speed is further improved. In addition, the destructive strength of aluminum oxide is preferably 2 GPa or less. When it is in the above range, a high grinding speed can be maintained, and production adaptability is further improved.
[0036] The destructive strength of abrasive particles can be calculated with reference to "Rapid test of tensile strength of rocks based on irregular test pieces, Yoshio Hiramatsu, Yukitoshi Oka, Hideo Kiyama, Journal of the Japan Mining Society, Vol. 81, No. 932, pp. 1024-1030, 1965". In detail, when particles (especially spherical particles) are compressed, the compressive stress is distributed near the load point, and the tensile stress is distributed almost on the entire surface. Therefore, for the destructive strength of alumina, the load-indentation displacement line diagram obtained can be recorded, and the point where the displacement increases sharply is the point where the particle undergoes large-scale destruction, and it can be calculated according to the following formula.
[0037] S t =(2.8×P) / (π×d 2 )
[0038] In the formula,
[0039] S t Indicates the breaking strength [GPa],
[0040] P represents the breaking load (kgf),
[0041] d represents the average particle size of the particles (μm)
[0042] Here, the breaking load P can be measured using a micro compression tester MCTW-500 manufactured by Shimadzu Corporation and a diamond flat indenter (φ=50 μm). In addition, the method for measuring the average particle size d is described in the description of the average particle size described later. The details of the measurement and calculation method of the breaking strength of aluminum oxide are described in the Examples.
[0043] It should be noted that the destructive strength of the abrasive calculated based on the above measurement is the same whether it is measured in the state of the raw material of the polishing composition (e.g., powdered aluminum oxide) or the abrasive (e.g., aluminum oxide) is taken out from the prepared polishing composition and measured.
[0044] When alumina is used as an abrasive, it can be appropriately selected from various known aluminas and used. As known alumina, for example, alumina containing at least one selected from α-alumina, γ-alumina, δ-alumina, θ-alumina, η-alumina, and κ-alumina can be cited. In addition, alumina called fumed alumina (Fumed Alumina) based on the classification according to the production method can also be used (typically, alumina particles produced when alumina salt is sintered at high temperature). Furthermore, alumina called colloidal alumina or alumina sol (alumina hydrates such as boehmite) is also included in the above-mentioned examples of known alumina. The alumina used as the abrasive of the polishing composition of the present invention may contain one of such aluminas alone or a combination of two or more. Among these, alumina containing a γ phase as a crystal phase (alumina containing γ-alumina) is preferred, and alumina containing a γ phase as the main crystal phase (alumina containing γ-alumina as the main component) is more preferred.
[0045] In this specification, when the peak of the γ phase appearing at the position of 2θ=46° can be confirmed based on the powder X-ray diffraction spectrum obtained using a powder X-ray diffraction device, the aluminum oxide is judged to "contain the γ phase as a crystal phase". In addition, in this specification, when the gamma conversion rate described later is greater than 50%, the aluminum oxide is judged to "contain the γ phase as the main crystal phase" (upper limit 100%). By using aluminum oxide containing the γ phase as a crystal phase, the grinding speed is further improved, and the effect is further improved when the γ phase is the main crystal phase. It is speculated that this is because the γ phase has a large amount of deformability when stress is applied, which helps to improve the breaking strength. It should be noted that for aluminum oxide produced by the later-described deflagration method, when the peak of the γ phase appearing at the position of 2θ=46° can be confirmed, there is a tendency for the γ phase content ratio to be particularly high.
[0046] In addition, the alpha conversion rate of aluminum oxide is preferably less than 50%, more preferably less than 45%, and further preferably less than 40% (lower limit 0%). When it is within the above range, the grinding speed is further improved. It is speculated that this is because, although the α phase has high hardness, it tends to be brittle, so by setting its content to a certain level or less, it helps to further improve the breaking strength when stress is applied. Here, the alpha conversion rate [%] can be calculated by the following formula based on the peak height (I25.6) of the α phase (012) plane appearing at the position of 2θ = 25.6° and the peak height (I46) of the γ phase appearing at the position of 2θ = 46° from the powder X-ray diffraction spectrum obtained using a powder X-ray diffraction device.
[0047] Alpha conversion rate = I25.6 / (I25.6+I46)×100〔Unit: %〕
[0048] When the γ phase is included as the main crystal phase, it is preferred that the α phase is also included as the crystal phase. In this case, the hardness is further increased and the polishing speed is further increased. In this case, the α conversion rate is preferably greater than 0% and less than 40%.
[0049] In addition, in this specification, the definition of the gamma conversion rate [%] is: the value calculated by the following formula based on the peak height (I25.6) of the α phase (012) plane appearing at the position of 2θ=25.6° and the peak height (I46) of the γ phase appearing at the position of 2θ=46° in the powder X-ray diffraction spectrum obtained using a powder X-ray diffraction device.
[0050] Gamma conversion rate = I25.6 / (I25.6+I46)×100〔Unit: %〕
[0051] The type and content ratio of the crystalline phase in alumina can be controlled by the manufacturing method and manufacturing conditions. For example, the alumina manufactured by the deflagration method described below has a higher γ-transformation rate and a lower α-transformation rate. In addition, in the deflagration method, the α-transformation rate can be reduced by making the heating temperature after the deflagration reaction lower than 1225°C.
[0052] The types of crystal phases in aluminum oxide, and the measurement and calculation methods of the alpha conversion rate and the gamma conversion rate are described in detail in the Examples.
[0053] The α-conversion rate and the γ-conversion rate calculated based on the above measurement have the same values whether the measurement is performed in the state of powdered alumina as a raw material of the polishing composition or when the alumina is taken out from the prepared polishing composition.
[0054] The method for producing the aluminum oxide used in the present invention is not particularly limited, and a known method can be used appropriately. Among these, the method for producing aluminum oxide based on the deflagration method (VMC method: Vaporized Metal Combustion Method) can obtain aluminum oxide with an aspect ratio of less than 1.1, so it is preferred. That is, as aluminum oxide, aluminum oxide produced by the deflagration method is preferred. By adopting the deflagration method, aluminum oxide with an aspect ratio of less than 1.1 can be obtained, and by using the particles, the grinding speed is further improved. In addition, the aluminum oxide obtained by the deflagration method has a high destructive strength (for example, a destructive strength of more than 0.5 GPa). In the present invention, by using abrasive particles with high destructive strength, the improvement of the grinding speed is further exerted, so from the viewpoint of destructive strength, it is also preferred to produce aluminum oxide by the deflagration method.
[0055] The deflagration method refers to "a method of synthesizing oxide ultrafine particles by forming a chemical flame in an atmosphere containing oxygen, throwing into the chemical flame an amount of metal powder that can form a dust cloud and is used to form a part of the target oxide ultrafine particles, and causing it to deflagrate". The details of the deflagration method are recorded in known documents such as Japanese Patent Publication No. 60-255602, and these records can be used as a reference to manufacture alumina. In addition, in the deflagration method, in the deflagration reaction, the heating temperature of the liquid powder of metal alumina as a precursor is higher than 1200°C for pretreatment, thereby increasing the value of the breaking strength. In addition, from the perspective of ease of control, the heating temperature in the deflagration reaction is preferably between 1250 and 1275°C. In the deflagration method, by making the heating temperature after the deflagration reaction lower than 1225°C, the aspect ratio can be made close to 1. A known device / method such as a rotary kiln can be used for the heating treatment.
[0056] The lower limit of the content (concentration) of the abrasive grains in the grinding composition based on one embodiment of the present invention is preferably 0.2 mass % or more relative to the grinding composition, more preferably 0.3 mass % or more, and further preferably 0.5 mass % or more. In addition, in the grinding composition of the present invention, the upper limit of the content of abrasive grains is preferably 20 mass % or less relative to the grinding composition, more preferably 15 mass % or less, further preferably 10 mass % or less, and further preferably 5 mass % or less. When it is such a range, the grinding speed can be further improved. It should be noted that when the grinding composition includes more than two kinds of abrasive grains, the content of abrasive grains is their total amount.
[0057] [Basic Inorganic Compounds]
[0058] The polishing composition of the present invention comprises an alkaline inorganic compound in the form of an alkali metal salt. Here, the alkaline inorganic compound refers to an inorganic compound having a function of increasing the pH of the composition by adding it to the polishing composition. The alkaline inorganic compound has the effect of chemically polishing the surface of the polishing object and improving the dispersion stability of the polishing composition. In addition, the alkaline inorganic compound contained in the polishing composition of the present invention is easier to improve the conductivity of the polishing composition than the alkaline organic compound. It is believed that the polishing speed based on the polishing composition is further improved.
[0059] In addition, the basic inorganic compound in the form of an alkali metal salt does not have a large steric volume compared to the basic organic compound, so the basic inorganic compound and the anionic water-soluble polymer are not likely to form aggregates. Therefore, the polishing composition of the present invention is a stable dispersion state of the anionic water-soluble polymer, so the anionic water-soluble polymer can be efficiently attached to the polishing pad.
[0060] Examples of the basic inorganic compound in the form of an alkali metal salt include lithium hydroxide, lithium carbonate, potassium hydroxide, potassium carbonate, potassium hydrogen carbonate, potassium phosphate, dipotassium hydrogen phosphate, sodium hydroxide, sodium carbonate, sodium hydrogen carbonate, sodium phosphate, disodium hydrogen phosphate, etc. Among these, the basic inorganic compound in the form of an alkali metal salt is preferably potassium hydroxide and sodium hydroxide, and more preferably potassium hydroxide, from the viewpoint of pH and slurry stability.
[0061] In the embodiment of the present invention, the content of the basic inorganic compound in the grinding composition is preferably 0.001 mass % or more relative to the grinding composition, more preferably 0.01 mass % or more, further preferably 0.05 mass % or more, and particularly preferably 0.1 mass % or more. By being such a lower limit, the grinding speed is further improved. The content of the basic inorganic compound in the grinding composition is preferably 10 mass % or less relative to the grinding composition, more preferably 8 mass % or less, and further preferably 5 mass % or less. By being such an upper limit, a stable slurry without aggregation can be obtained.
[0062] [Anionic water-soluble polymer]
[0063] The polishing composition of the present invention contains anionic water-soluble polymers. Anionic water-soluble polymers are water-soluble polymers having anionic groups in the molecule. In this specification, "water-soluble" means that the solubility in water (25° C.) is 1 g / 100 mL or more. Anionic water-soluble polymers can be used alone or in combination of two or more.
[0064] When using the grinding composition of the present invention to grind the grinding object, the anionic water-soluble polymer contained in the grinding composition is attached to the grinding pad. At this time, when the zeta potential of the pad surface is positive, the zeta potential is negatively offset by the attachment of the anionic water-soluble polymer, and when the zeta potential of the pad surface is negative, the absolute value of its zeta potential increases by the attachment of the anionic water-soluble polymer. For example, when the grinding pad is polyurethane, the zeta potential of the surface of the polyurethane is about -45mV, and the zeta potential of the grinding pad surface can be increased to -80mV by the contact of the grinding pad with the grinding composition of the present invention (that is, by attaching the anionic water-soluble polymer). Therefore, by attaching the anionic water-soluble polymer to the grinding pad surface, the surface charge of the grinding pad is negative or the absolute value of the negative surface charge of the grinding pad is increased, so that the grinding pad and the abrasive are more easily repelled, and the grinding speed is improved.
[0065] According to an embodiment of the present invention, as anionic water-soluble polymer, it is suitable to include at least one functional group selected from the group consisting of carboxyl, sulfonic acid, phosphoric acid and phosphonic acid in the molecule. Wherein, the anionic water-soluble polymer preferably includes a carboxyl. By including such a group in the anionic water-soluble polymer, the desired effect of the present invention can be efficiently exerted.
[0066] In addition, according to an embodiment of the present invention, it is suitable that the anionic water-soluble polymer contains a structural unit derived from a monomer having an ethylenically unsaturated bond. For example, for anionic water-soluble polymers, as structural units derived from monomers, it is preferred to contain one or more selected from the group consisting of acrylic acid and methacrylic acid. Therefore, the anionic water-soluble polymer is more preferably selected from at least one of the group consisting of polyacrylic acid polymers and polymethacrylic acid polymers. It is speculated that by the above embodiment, in the polishing composition, the carboxyl group interacts with the alkaline inorganic compound, and the abrasive is in a stably dispersed state.
[0067] The anionic water-soluble polymer can be a copolymer containing a structural unit derived from a monomer having an ethylenically unsaturated bond and a structural unit derived from other monomers in one molecule. As such a copolymer, a copolymer of (meth)acrylic acid and vinyl alcohol, a copolymer of (meth)acrylic acid and 2-hydroxy-2-phosphinoacetic acid (HPAA), a copolymer of (meth)acrylic acid and acryloylmorpholine (ACMO), etc. can be cited. It should be noted that the meaning of (meth)acrylic acid includes acrylic acid and methacrylic acid.
[0068] In addition, the anionic water-soluble polymer may also contain oxyalkylene units. Examples of oxyalkylene units that the anionic water-soluble polymer may contain include polyethylene oxide (PEO), block copolymers of ethylene oxide (EO) and propylene oxide (PO), random copolymers of EO and PO, etc. The block copolymers of EO and PO may be diblocks and triblocks containing polyethylene oxide (PEO) blocks and polypropylene oxide (PPO) blocks. The above-mentioned triblocks include PEO-PPO-PEO triblocks and PPO-PEO-PPO triblocks.
[0069] In the embodiment of the present invention, the lower limit of the molecular weight (mass average molecular weight) of the anionic water-soluble polymer is preferably 1000 or more, 5000 or more, 10000 or more, 50000 or more, 100000 or more, 300000 or more, 500000 or more, 800000 or more. The upper limit of the molecular weight (mass average molecular weight) of the anionic water-soluble polymer is preferably 8500000 or less, 6000000 or less, 4000000 or less, 2000000 or less, 1500000 or less. That is, the molecular weight (mass average molecular weight) of anionic water-soluble polymer is, for example, preferably more than 1000 and less than 8500000, more than 5000 and less than 6000000, more than 10000 and less than 4000000, more than 50000 and less than 4000000, more than 100000 and less than 2000000. If it is such a scope, then the polishing rate can be further improved. The molecular weight (mass average molecular weight) of anionic water-soluble polymer can adopt the value measured by GPC method.
[0070] In the embodiment of the present invention, the content of the anionic water-soluble polymer in the grinding composition is preferably 0.001 mass % or more relative to the grinding composition, more preferably 0.005 mass % or more, further preferably 0.01 mass % or more, further preferably 0.05 mass % or more, and most preferably 0.08 mass % or more. In addition, the content of the anionic water-soluble polymer in the grinding composition is 0.8 mass % or less relative to the grinding composition, more preferably 0.5 mass % or less, and particularly preferably 0.4 mass % or less. If it is such a range, a high polishing rate can be maintained. It should be noted that when the grinding composition includes more than two kinds of anionic water-soluble polymers, the content of the anionic water-soluble polymer is their total amount.
[0071] [Dispersion medium]
[0072] The polishing composition includes a dispersion medium (solvent) for dispersing the components constituting the polishing composition. The dispersion medium has the function of dispersing or dissolving the components. As the dispersion medium, an organic solvent or water can be cited, preferably water, more preferably water.
[0073] From the viewpoint of suppressing the pollution of the grinding object and the effect of suppressing the damage to other components, as a dispersion medium, water free of impurities as much as possible is preferred. As such water, for example, water having a total content of transition metal ions of less than 100 ppb is preferred. Here, the purity of water can be improved by, for example, removing impurity ions using an ion exchange resin, removing foreign matter through a filter, and distillation. Specifically, as water, for example, deionized water (ion exchange water), pure water, ultrapure water, distilled water, etc. are preferably used. Usually, it is preferred that 90% by volume or more of the dispersion medium contained in the grinding composition is water, more preferably 95% by volume or more is water, further preferably 99% by volume or more is water, and particularly preferably 100% by volume is water.
[0074] In addition, for the dispersion or dissolution of each component, the dispersion medium can be a mixed solvent of water and an organic solvent. At this time, as the organic solvent used, acetone, acetonitrile, ethanol, methanol, isopropanol, glycerol, ethylene glycol, propylene glycol, etc., which are organic solvents miscible with water, can be cited. In addition, these organic solvents can also be used without mixing with water, but after each component is dispersed or dissolved, mixed with water. These organic solvents can be used alone or in combination of two or more.
[0075] [Other additives]
[0076] The polishing composition of the present invention may further contain known additives such as pH adjusters, chelating agents, thickeners, oxidants, dispersants, surface protective agents, wetting agents, surfactants, rust inhibitors, preservatives, and mildew inhibitors, without prejudice to the present invention. The content of the above additives may be appropriately set according to the purpose of addition.
[0077] (pH adjuster)
[0078] The polishing composition of the present invention may have its pH adjusted to within a desired range by a basic inorganic compound, and may further contain a pH adjuster other than a basic inorganic compound.
[0079] As the pH adjuster, a known acid, a base other than a basic inorganic compound, or a salt thereof can be used. Specific examples of the acid that can be used as the pH adjuster include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid, and organic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylvaleric acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, lactic acid, diglycolic acid, 2-furancarboxylic acid, 2,5-furandicarboxylic acid, 3-furancarboxylic acid, 2-tetrahydrofurancarboxylic acid, methoxyacetic acid, methoxyphenylacetic acid, and phenoxyacetic acid.
[0080] Examples of bases other than basic inorganic compounds that can be used as pH adjusters include aliphatic amines such as ethanolamine and 2-amino-2-ethyl-1,3-propanediol, aromatic amines, basic organic compounds such as quaternary ammonium hydroxides, etc. Ammonia can also be used as a pH adjuster.
[0081] The above pH adjusters may be used alone or in combination of two or more. The amount of the pH adjuster added is not particularly limited, and may be appropriately adjusted so that the pH of the polishing composition falls within a desired range.
[0082] The lower limit of the pH of the polishing composition is not particularly limited, and is preferably more than 9.5, more preferably more than 10, further preferably more than 10.5, and particularly preferably more than 11. By being set to such a lower limit, the polishing rate of the polished object can be improved. In addition, as the upper limit of pH, there is no particular restriction, and is preferably less than 13, more preferably less than 12.5, and further preferably less than 12. By being set to such an upper limit, the stability of the polishing composition can be improved.
[0083] In addition, the pH of the polishing composition can be measured with, for example, a pH meter.
[0084] <Method for producing polishing composition>
[0085] The method for producing the polishing composition of the present invention is not particularly limited, and can be obtained, for example, by stirring and mixing abrasive grains, a basic inorganic compound, an anionic water-soluble polymer, and other additives as needed in a dispersion medium. The details of each component are as described above. Therefore, the present invention provides a method for producing a polishing composition, which comprises mixing abrasive grains, a basic inorganic compound, an anionic water-soluble polymer, and a dispersion medium.
[0086] The temperature when mixing the components is not particularly limited, but is preferably 10° C. or higher and 40° C. or lower, and heating may be performed to increase the dissolution rate. The mixing time is not particularly limited as long as uniform mixing is possible.
[0087] <Polishing Method and Method for Manufacturing Semiconductor Substrate>
[0088] The present invention provides a polishing method, comprising the step of polishing an object to be polished using the polishing composition according to one embodiment of the present invention. In addition, the present invention provides a method for manufacturing a semiconductor substrate having the polishing method.
[0089] As the polishing device, a general polishing device can be used which is equipped with a holder for holding a substrate having an object to be polished, a motor whose rotation speed can be changed, and a polishing plate to which a polishing pad (polishing cloth) can be attached.
[0090] As the polishing pad, ordinary nonwoven fabric, polyurethane, porous fluororesin, etc. can be used without particular limitation. The polishing pad is preferably provided with grooves for accumulating the polishing liquid.
[0091] Regarding the grinding conditions, for example, the rotation speed of the grinding plate is preferably 10 rpm (0.17 s -1 ) and above 500rpm(8.3s -1 ) or less. The pressure (polishing pressure) applied to the substrate having the polishing object is preferably 0.5 psi (3.4 kPa) or more and 10 psi (68.9 kPa) or less. There is no particular limitation on the method of supplying the polishing composition to the polishing pad, and for example, a method of continuously supplying with a pump or the like can be adopted. There is no limitation on the supply amount, and it is preferred that the surface of the polishing pad is always covered with the polishing composition of the present invention.
[0092] After polishing, the substrate is washed in running water, and water droplets adhering to the substrate are shaken off with a spin dryer or the like to be dried, thereby obtaining a substrate having a layer containing a metal.
[0093] The polishing composition used in the present invention may be a single component type or a multi-component type including a two-component type. In addition, the polishing composition used in the present invention may be prepared by diluting the stock solution of the polishing composition, for example, 10 times or more, with a diluent such as water.
[0094] Although the embodiments of the present invention have been described in detail, these are merely illustrative and exemplary descriptions and are not restrictive. The scope of the present invention should obviously be interpreted by the appended claims.
[0095] The present invention includes the following embodiments and aspects.
[0096] 1. A polishing composition comprising abrasive grains, a basic inorganic compound, an anionic water-soluble polymer and a dispersion medium,
[0097] The zeta potential of the aforementioned abrasive particles is negative.
[0098] The aspect ratio of the abrasive grains is 1.1 or less.
[0099] In the particle size distribution of the abrasive grains obtained by a laser diffraction scattering method, a ratio D90 / D50 of a particle diameter D90 when the cumulative particle mass from the particle side reaches 90% of the total particle mass to a particle diameter D50 when the cumulative particle mass from the particle side reaches 50% of the total particle mass is greater than 1.3,
[0100] The aforementioned basic inorganic compound is an alkali metal salt.
[0101] 2. The polishing composition according to 1. above, wherein the anionic water-soluble polymer is at least one selected from the group consisting of polyacrylic acid polymers and polymethacrylic acid polymers.
[0102] 3. The polishing composition according to 1. or 2. above, wherein the molecular weight of the anionic water-soluble polymer is 5,000 to 6,000,000.
[0103] 4. The polishing composition according to any one of 1. to 3. above, wherein the pH is 9.5 or higher.
[0104] 5. The polishing composition according to any one of 1. to 4. above, wherein the abrasive grains contain aluminum oxide.
[0105] 6. The polishing composition according to 5. above, wherein the aluminum oxide contains a γ phase as a crystal phase.
[0106] 7. The polishing composition according to 5. or 6. above, wherein the alpha conversion rate of the aluminum oxide is less than 50%.
[0107] 8. The polishing composition according to any one of 5. to 7. above, wherein the aluminum oxide has a fracture strength of 0.5 GPa or more.
[0108] 9. A polishing method comprising the step of polishing an object to be polished using the polishing composition according to any one of 1. to 8. above.
[0109] 10. A method for manufacturing a semiconductor substrate, comprising the polishing method described in 9. above.
[0110] Example
[0111] The present invention is further described in detail using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. It should be noted that, unless otherwise specified, "%" and "parts" represent "mass %" and "mass parts", respectively. In addition, in the following examples, unless otherwise specified, the operation is carried out under the conditions of room temperature (20-25°C) / relative humidity 40-50%RH.
[0112] [Adjustment of abrasive grains]
[0113] (Aluminum Oxide by Deflagration Method: Production of Abrasive Grains A)
[0114] With reference to the examples of Japanese Patent Application Laid-Open No. 60-255602, abrasive grains A were prepared by the deflagration method. It should be noted that, hereinafter, abrasive grains A produced by the deflagration method may be referred to as "VMC alumina". The physical properties of abrasive grains A (VMC alumina) were calculated according to the following measurement method and are shown in Table 1 below.
[0115] (Sintered and pulverized α-alumina: Production of abrasive grains B)
[0116] As abrasive B, sintered and crushed α-alumina is prepared. Specifically, as described in paragraph "0013" of Japanese Patent Gazette No. 2006-36864, aluminum hydroxide is calcined under the conditions of a calcination temperature in the range of 1100 to 1500°C and a calcination time in the range of 1 to 5 hours, and then crushed using alumina balls with a diameter of 20,000 μm. Powdered sintered and crushed α-alumina as abrasive B is manufactured by a method for manufacturing alumina (crushing method) based on such calcination and subsequent crushing as needed. In the manufacture of the abrasive B, the crushing time is controlled in such a way as to obtain the value of the average particle size described in Table 1 below. The physical properties of abrasive B (sintered and crushed α-alumina) calculated according to the following measurement method are shown in Table 1 below.
[0117] [Analysis of the types and contents of crystal phases]
[0118] (Types of Crystal Phases Contained in Alumina)
[0119] Regarding the powdered abrasive (aluminum oxide), a powder X-ray diffraction apparatus (SmartLab, a fully automatic multi-purpose X-ray diffractometer manufactured by Rigaku Corporation) is used to obtain a powder X-ray diffraction spectrum, and the type of crystal phase contained in the aluminum oxide is determined based on the peak position of the powder X-ray diffraction spectrum. Here, in the powder X-ray diffraction spectrum, when the peak of the α phase (012) plane appearing at the position of 2θ=25.6° can be confirmed, the aluminum oxide is determined to "contain the α phase as a crystal phase". In addition, when the peak of the γ phase appearing at the position of 2θ=46° can be confirmed, the aluminum oxide is determined to "contain the γ phase as a crystal phase".
[0120] (α-ratio)
[0121] The alpha conversion rate [%] is calculated by the following formula based on the peak height (I25.6) of the α phase (012) plane appearing at 2θ=25.6° and the peak height (I46) of the γ phase appearing at 2θ=46° in the powder X-ray diffraction spectrum obtained using a powder X-ray diffraction apparatus.
[0122] Alpha conversion rate = I25.6 / (I25.6+I46)×100〔Unit: %〕
[0123] (Main crystal phase)
[0124] When the α conversion rate is greater than 50%, the aluminum oxide particles are judged to "contain the α phase as the main crystal phase". In addition, the value calculated by the following formula based on the peak height (I25.6) of the α phase (012) plane appearing at 2θ=25.6° and the peak height (I46) of the γ phase appearing at 2θ=46° in the powder X-ray diffraction spectrum obtained using a powder X-ray diffraction device is defined as the γ conversion rate [%). When the γ conversion rate is greater than 50%, the aluminum oxide particles are judged to "contain the γ phase as the main crystal phase".
[0125] Gamma conversion rate = I46 / (I25.6+I46)×100〔Unit: %〕
[0126] [Aspect Ratio]
[0127] Regarding the powdered abrasive grains (alumina), 100 abrasive grains were randomly selected from an image measured by a scanning electron microscope (SEM) (manufactured by Hitachi HighTechnology Co., Ltd., product name: SU8000), and their average major diameter and average minor diameter were measured and calculated. Then, using the values of the average major diameter and the average minor diameter, the aspect ratio of the abrasive grains was calculated according to the following formula.
[0128] Aspect ratio = average major diameter [μm] / average minor diameter [μm]
[0129] [Average secondary particle size]
[0130] The powdery abrasive grains (alumina) were measured using a particle size distribution measuring device (Microtrac MT3000II manufactured by Microtrac BEL Co., Ltd.) to evaluate the average secondary particle size.
[0131] [Destruction strength]
[0132] The load-indentation displacement graph of the powdered abrasive (alumina) was obtained by the following measuring device and measuring conditions. The point where the displacement increased sharply was the point where the particle was extensively broken, and the breaking strength of the abrasive was calculated by the following formula.
[0133] S t =(2.8×P) / (π×d 2 )
[0134] In the formula,
[0135] S t Indicates the breaking strength [GPa],
[0136] P represents the breaking load (kgf),
[0137] d represents the average particle size of the particles (μm)
[0138] (Measurement equipment and measurement conditions)
[0139] Measurement equipment: Micro compression tester MCTW-500 manufactured by Shimadzu Corporation,
[0140] Indenter used: Diamond flat indenter (φ=50μm),
[0141] Load speed: 7.747mN / s: Load speed fixed mode,
[0142] Measurement atmosphere: room temperature air.
[0143] Table 1 shows the characteristics (material and production method) of each abrasive grain, the alpha conversion rate, the main crystal phase, the average grain size, the aspect ratio, the average major diameter and the average minor diameter, and the evaluation results of the fracture strength.
[0144] It should be noted that in the following Table 1, α conversion rate <40〔%〕means that although the α phase is included as a crystal phase, its α conversion rate value is greater than 0% and less than 40%, and α conversion rate >70〔%〕means that the α phase is included as a crystal phase, and its α conversion rate value is greater than 70%.
[0145] [Table 1]
[0146]
[0147]
[0148] [Preparation of Polishing Composition]
[0149] (Example 1)
[0150] The above-obtained abrasive A (average primary particle size of 100 nm, average secondary particle size of 200 nm, average degree of association of 2) as abrasive is 1.0 mass%, polyacrylic acid (PAA) having a molecular weight (mass average molecular weight) of 1000000 as a water-soluble polymer is 0.1 mass%, and potassium hydroxide as an alkaline compound is 0.2 mass%. The above-mentioned components and ion exchange water are stirred and mixed for 30 minutes at room temperature (25°C) to prepare a polishing composition. The pH of the polishing composition measured by a pH meter (model: LAQUA (registered trademark) manufactured by Horiba, Ltd.) is 12.0. It should be noted that the zeta potential of the abrasive A in the polishing composition obtained by the following method is -30 mV. Regarding the abrasive A in the obtained polishing composition, the results of the average primary particle size, average secondary particle size, D90 / D50 measured by the following method, and the aspect ratio measured by the above method are shown in Table 2.
[0151] The particle size of the abrasive grains A in the polishing composition is the same as the particle size of the powdered aluminum oxide in Table 1. Therefore, although the powdered aluminum oxide was used as a measurement sample, the abrasive grains A in the polishing composition may be taken out and measured in the same manner.
[0152] It should be noted that "Broad" in the particle size distribution column in Table 2 means that D90 / D50 is greater than 1.3, and "Sharp" means that D90 / D50 is less than 1.3. Furthermore, "Spherical" in the particle shape column in Table 2 means that the aspect ratio is less than 1.1, and "Special Shape" means that the aspect ratio is greater than 1.1. In Table 3, "PAA" means polyacrylic acid, and "-" means that the component is not contained.
[0153] (Example 2, Comparative Examples 1 to 3)
[0154] The polishing compositions of Example 2 and Comparative Examples 1 to 3 were prepared in the same manner as in Example 1 except that the abrasives described in Table 2 were used and the types of the water-soluble polymer and the basic compound were changed to those shown in Table 3. The results of the zeta potential, average primary particle size, average secondary particle size, D90 / D50, and aspect ratio measured by the above methods for the abrasive A in the obtained polishing composition are shown in Table 2. It should be noted that the particle size of the abrasive in the polishing composition is the same as the particle size of the powdered aluminum oxide in Table 1 above. The pH of the obtained polishing composition is shown in Table 3 below.
[0155] [evaluate]
[0156] [Zeta potential measurement]
[0157] Each polishing composition prepared below was supplied to ELS-Z2 manufactured by Otsuka Electronics Co., Ltd. and measured by laser Doppler method (electrophoretic light scattering measurement method) using a flow cell at a measurement temperature of 25° C. The obtained data was analyzed using the Smoluchowski equation to calculate the zeta potential of aluminum oxide in the polishing composition.
[0158] [Measurement of average primary particle size]
[0159] The average primary particle size of the abrasive grains was calculated from the specific surface area of the abrasive grains and the density of the abrasive grains measured by the BET method using "FlowSorbII 2300" manufactured by Micromeritics Instrument Corp. The average secondary particle size of the abrasive grains was measured using a dynamic light scattering particle size distribution apparatus UPA-UTI151 manufactured by Nikkiso Co., Ltd.
[0160] [Measurement of average secondary particle size]
[0161] The average secondary particle size of the abrasive grains was measured by a light scattering method using a laser, and a Microtrac MT3000II (manufactured by Microtrac BEL Co., Ltd.) was used as a measuring device. It should be noted that in the particle size distribution of the average secondary particle size of the abrasive grains, the ratio D90 / D50 of the diameter D90 of the grains when the cumulative particle mass from the microparticle side reaches 90% of the total particle mass and the diameter D50 of the grains when the cumulative particle mass from the microparticle side reaches 50% of the total particle mass is calculated.
[0162] [Grinding speed]
[0163] As the object to be polished, a surface having a thickness of A silicon wafer (200 mm, blank wafer, manufactured by Advantec Co., Ltd.) having a TEOS film having a thickness of Silicon wafers (200 mm, blank wafers, manufactured by Advantec Co., Ltd.) with SiN films were prepared. Each silicon wafer was cut into 60 mm × 60 mm pieces as test pieces, and the substrates were polished using the polishing compositions obtained above under the following polishing conditions. The two polishing objects were polished under the following conditions. It should be noted that the polishing rate of the SiN film was measured only in the polishing compositions of Example 1 and Comparative Example 1.
[0164] (Grinding conditions)
[0165] ·TEOS film
[0166] As a grinder, EJ-380IN-CH (Engis Japan Corporation) was used, and as a polishing pad, a hard polyurethane pad IC1000 (Rohm and Haas Company) was used. The polishing was carried out for 60 seconds under the conditions of a polishing pressure of 3.05 psi (21.0 kPa), a plate rotation speed of 60 rpm, a bracket rotation speed of 60 rpm, and a supply rate of 100 ml / min of the polishing composition.
[0167] ·SiN film
[0168] Respectively, as grinder, use EJ-380IN-CH (Engis Japan Corporation system), as polishing pad, use hard polyurethane pad IC1000 (Rohm and Haas Company system).With grinding pressure 4.0psi (27.6kPa), fixed plate speed 113rpm, bracket speed 107rpm, the condition of supply speed 200ml / minute of polishing composition, implement grinding with grinding time 60 seconds.
[0169] (grinding speed)
[0170] The polishing rate (Removal Rate; RR) is calculated by the following formula.
[0171]
[0172] The film thickness was determined using an optical interference film thickness measuring device (manufactured by Dainippon Screen Mfg. Co., Ltd., model: LAMBDA ACE VM-2030), and the polishing rate was evaluated by dividing the difference in film thickness before and after polishing by the polishing time.
[0173] The evaluation results of the polishing rate for the TEOS film are shown in Table 3 below.
[0174] When the polishing composition of Example 1 is used, the polishing rate of the SiN film is When the polishing composition of Comparative Example 1 was used,
[0175] [Number of scratches]
[0176] A polishing object to be evaluated for the number of scratches is prepared. First, a polishing object having a surface formed with a thickness of A silicon wafer (200 mm, blank wafer, manufactured by Advantec Co., Ltd.) having a TEOS film and a surface having a thickness of Silicon wafers (200 mm, blank wafers, manufactured by Advantec Co., Ltd.) having a SiN film were used. The two polishing objects were polished using the polishing compositions of Example 1 and Comparative Example 4 obtained above under the following polishing conditions.
[0177] (Polishing conditions for scratch number evaluation)
[0178] Polishing equipment: Applied Materials 200mm CMP single-side polishing equipment Mirra
[0179] Polishing pad: NITTA HAAS Co., Ltd. hard polyurethane pad IC1010
[0180] Grinding pressure: 2.0psi
[0181] Grinding plate speed: 83rpm
[0182] Bracket speed: 77rpm
[0183] Supply of polishing composition: Overflow
[0184] Polishing composition supply amount: 200 ml / min
[0185] Grinding time: 60 seconds.
[0186] For the number of scratches on the surface of the polished object after polishing, the wafer inspection device "Surfscan (registered trademark) SP2" manufactured by KLA-Tencor was used to measure the coordinates of the entire surface of both sides of the polished object (excluding the outer circumference of 2 mm), and all the measured coordinates were observed with Review-SEM (RS-6000, Hitachi High Technology Co., Ltd.) to measure the number of scratches. It should be noted that the scratches on the surface of the substrate with a depth of more than 10nm and less than 100nm, a width of more than 5nm and less than 500nm, and a length of more than 100μm were counted as scratches, and the scratch evaluation was performed according to the following criteria.
[0187] [Scratch Evaluation Criteria]
[0188] ○…The number of scratches is less than 10, good
[0189] ×…The number of scratches is 10 or more, which is defective.
[0190] The number of scratches was counted. When the polishing composition of Example 1 was used, the number of scratches was evaluated as ○, and when the polishing composition of Comparative Example 3 was used, the number of scratches was evaluated as ×.
[0191] [Table 2]
[0192]
[0193] [Table 3]
[0194]
[0195] As shown in Table 3, when the polishing compositions of Examples 1 and 2 were used, the polishing rate of the TEOS film was greater than Compared with the polishing compositions of Comparative Examples 1 and 2, the TEOS film can be polished at a higher polishing rate.
[0196] The polishing composition of Comparative Example 3 polished the TEOS film at a high rate, but easily scratched it. This is probably because the rotation of the abrasive grains with an aspect ratio greater than 1.3 was suppressed, resulting in easier scratching.
[0197] On the other hand, the polishing composition of Example 1 showed less scratching than the polishing composition of Comparative Example 3. This is considered to be the result of the properties of the abrasive grains A used in the polishing composition of Example 1, such as aspect ratio, particle size, particle size distribution, and hardness, acting on the polishing rate in a well-balanced manner.
[0198] When Example 1 and Comparative Example 3 are compared, when the basic inorganic compound contained in the polishing composition is not an alkali metal salt, the polishing rate by the polishing composition is significantly reduced.
[0199] This shows that the polishing rate of the object to be polished is improved by making the polishing composition contain a basic inorganic compound as an alkali metal salt and an anionic water-soluble polymer.
[0200] This application is based on Japanese Patent Application No. 2020-049621 filed on March 19, 2020, the disclosure of which is incorporated herein by reference in its entirety.
Claims
1. A polishing composition comprising: abrasive grains, a basic inorganic compound, an anionic water-soluble polymer and a dispersion medium, The abrasive grains include aluminum oxide, The zeta potential of the abrasive particles is negative. The aspect ratio of the abrasive grains is less than 1.09, In the particle size distribution of the abrasive grains obtained by a laser diffraction scattering method, a ratio D90 / D50 of a particle diameter D90 when the cumulative particle mass from the particle side reaches 90% of the total particle mass to a particle diameter D50 when the cumulative particle mass from the particle side reaches 50% of the total particle mass is 2.0 or more, The basic inorganic compound is an alkali metal salt.
2. The polishing composition according to claim 1, in, The anionic water-soluble polymer is at least one selected from the group consisting of polyacrylic acid-based polymers and polymethacrylic acid-based polymers.
3. The polishing composition according to claim 1, in, The molecular weight of the anionic water-soluble polymer is 5,000 or more and 6,000,000 or less. The polishing composition according to claim 1 , which has a pH of 9.5 or higher.
5. The polishing composition according to claim 1, in, The aluminum oxide includes a γ phase as a crystal phase.
6. The polishing composition according to claim 1, in, The alpha conversion rate of the aluminum oxide is less than 50%.
7. The polishing composition according to claim 1, in, The breaking strength of the aluminum oxide is greater than 0.5 GPa. 8 . A polishing method comprising the step of polishing an object to be polished using the polishing composition according to claim 1 . 9 . A method for manufacturing a semiconductor substrate, comprising the polishing method according to claim 8 .