A method and equipment for preparing ultra-thin lithium metal foil
Through the specific formula of complex lithium salt and the continuous integrated process of vacuum thermal reduction-vacuum distillation-vacuum evaporation, the problems of low purity and low recovery rate in the preparation of metallic lithium are solved, and high-efficiency, low-cost ultra-thin metallic lithium is achieved Foil preparation.
Patent Information
- Application Number
- CN202011376686.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-11-30
AI Technical Summary
Existing metal lithium preparation methods have problems such as high lithium production reaction temperature, low lithium recovery rate, low purity of collected lithium foil, and cumbersome process operations.
The composite lithium salt preparation method is used to generate metal vapor through vacuum thermal reduction and vacuum distillation steps, and is deposited through a vacuum evaporation process to form an ultra-thin metal lithium foil. A specific proportion of composite lithium salt and reducing agent are used to perform a thermal reduction reaction, combined with Continuous integrated process of vacuum evaporation equipment.
It improves the purity and recovery rate of metallic lithium, simplifies the process flow, reduces energy consumption and costs, and achieves efficient preparation of ultra-thin metallic lithium foil.
Smart Images

Figure CN113528859B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and a preparation device for a metal lithium foil, and in particular to a continuous preparation method and a continuous preparation device for an ultra-thin metal lithium foil. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, no memory effect, high operating voltage and excellent cycle stability. They are widely used in small mobile devices, energy storage power stations and other fields. With the rise and development of electric vehicles (EV), hybrid electric vehicles (HEV), drones and the popularization and application of other large-scale energy storage equipment, people's requirements for energy storage devices are becoming increasingly diverse. The development and application of EV or HEV depends to a large extent on the improvement of its power energy storage system, which requires that the energy storage device should have high specific energy and high specific power. The specific energy of traditional lithium-ion batteries is 100 to 200Whkg -1 , can no longer meet the needs of these devices.
[0003] Lithium metal has a high theoretical specific capacity, close to 3860 mAh g -1 , and has a very low redox potential (-3.04Vvs.SHE), which is used as a negative electrode material for batteries It is one of the best choices and can be combined with oxygen or sulfur to form lithium-oxygen (Li-O2) batteries and lithium-sulfur (Li-S) batteries. Both Li-O2 batteries and Li-S batteries have extremely high theoretical specific energy, with Li-S batteries reaching up to 2600Whkg. -1 , Li-O battery up to 11140Whkg -1 These batteries all use metallic lithium as the negative electrode of the battery and are collectively referred to as lithium metal batteries.
[0004] At present, the main methods for preparing metallic lithium are molten salt electrolysis, metal thermal reduction and vacuum distillation. The molten salt electrolysis method is a method for converting lithium salt into metallic lithium, which has the advantages of high current efficiency and continuous production. However, this method has high energy consumption, pollutes the environment, and the purity of the obtained metallic lithium is low. The metal thermal reduction method is a method for converting lithium oxide into metallic lithium through metal co-heating. It has the advantages of simple operation, no pollution and short process, but the purity of the obtained metallic lithium ingot is not high; secondly, the fluidity of lithium oxide alone is poor, and the reaction with the reducing agent is not sufficient, resulting in a low lithium recovery rate. The vacuum distillation method can effectively reduce the content of impurity elements in metallic lithium and is a common method for obtaining high-purity metallic lithium. The preparation method of metallic lithium foil is mainly mechanical rolling method. Since this method mainly involves mechanical rolling of metallic lithium ingots, it is very easy to cause the metallic lithium to adhere to the roller press. In addition, the preparation of ultra-thin metallic lithium foil with a thickness of less than 20 microns is a difficult problem for the roller press equipment, with large mechanical loss and high energy consumption.
[0005] Chinese patent publication number CN1299884A discloses a process and equipment for the preparation and purification of metallic lithium by thermal reduction, which includes the following steps: S1. Using Li2CO3 as a raw material and Al2O3 as an auxiliary agent for briquetting and calcining to obtain clinker; S2. Mixing the clinker with a reducing agent and pressing it into a briquette for vacuum thermal reduction; S3. Distilling lithium vapor once in a reduction furnace; S4. Distilling lithium vapor after the first distillation twice to obtain metallic lithium ingots. The disadvantages of this process are that the yield of producing Li2O using Li2CO3 as a raw material is low, and the decomposition conditions of Li2CO3 are more stringent. There is no steam filtration process after the first distillation, which will result in the formation of a metallic lithium ingot containing more dust impurities.
[0006] Chinese patent announcement number CN1213158C discloses a method for preparing lithium from lithium carbonate, wherein lithium carbonate, quicklime and alumina are mixed and granulated, and then calcined; the calcined particles are crushed to obtain powder; the powder is mixed with ferrosilicon and granulated uniformly, and vacuum thermal reduction is performed, and the obtained lithium vapor is condensed to obtain solid lithium. The disadvantage of this process is that the decomposition rate of lithium carbonate is not high, and secondly, there is no secondary distillation process, and the purity of the obtained product is not high.
[0007] Chinese patent publication number CN109182758A discloses a method and system for preparing ultra-thin metal lithium strips from low-grade lithium sources, which first evaporates and removes low-boiling impurities in low-grade lithium sources, such as metal lithium slag with a metal lithium content of 20%-99%, in a vacuum environment to obtain liquid metal lithium, and then uses a vacuum evaporation method to deposit the obtained liquid metal lithium on a substrate to form an ultra-thin metal lithium strip. This process uses a solid low-grade metal lithium source for heating and evaporation to remove impurities, and the distillation effect achieved is average. The impurities remaining in the evaporation boat are lithium carbonate, lithium hydroxide, lithium chloride, etc. These lithium impurities are not utilized, resulting in relatively high raw material costs, and the purity of the prepared metal lithium foil may not be high. Summary of the invention
[0008] In view of the problems in the prior art of lithium production process, such as high lithium production reaction temperature, low lithium recovery rate, low purity of collected lithium foil and complicated process operation, the present invention provides a method and equipment for preparing ultra-thin metal lithium foil.
[0009] The technical solution adopted by the present invention is as follows:
[0010] [1] A method for preparing an ultra-thin lithium metal foil comprises the following steps:
[0011] (1) A composite lithium salt preparation step, wherein the lithium raw material is heated and then cooled, and ball milled to obtain a composite lithium salt with a chemical formula of xLiOH·yLi2CO3·zLi2O, wherein x, y, and z are mass fractions and satisfy 0 <x<0.5、0<y<0.5、0.5≤z<1、x+y+z=1;
[0012] (2) a vacuum thermal reduction step, wherein the composite lithium salt and the reducing agent are mixed uniformly and pressed, and vacuum thermal reduction is performed in a vacuum reduction furnace to generate metal vapor;
[0013] (3) a vacuum distillation step, wherein the metal vapor is passed through a heat exchange tube into a distillation tank for vacuum distillation, so that lithium vapor in the metal vapor is condensed into metallic lithium liquid, and the metallic lithium liquid is stored in a lithium storage tank through a connecting tube;
[0014] (4) A vacuum evaporation step, wherein the metallic lithium liquid in the lithium storage tank is introduced into a crucible of a vacuum evaporation device and heated so that the metallic lithium liquid is converted into lithium vapor, which is deposited on the substrate to form a uniform lithium foil.
[0015] [2] The method for preparing ultrathin metal lithium foil as described in [1], in step (1), at room temperature, the lithium raw material is heated to 600-800°C at a vacuum degree of 1-20Pa at a heating rate of 1-10°C / min, and the temperature is kept for 60-300min. After natural cooling, the composite lithium salt xLiOH·yLi2CO3·zLi2O is obtained by ball milling, wherein x, y, and z are mass fractions and satisfy 0 <x<0.5、0<y<0.5、0.5≤z<1、x+y+z=1;
[0016] The lithium raw material is one or more of lithium hydroxide-lithium carbonate, lithium hydroxide-lithium carbonate-lithium oxalate and lithium hydroxide-lithium oxalate. The particle size of the composite lithium salt after ball milling is 20μm≤D50≤70μm, and the mass ratio of ball to material is (10-15):1.
[0017] [3] A method for preparing an ultra-thin lithium metal foil as described in [1],
[0018] In step (2), the composite lithium salt and the reducing agent are mixed uniformly in a mass ratio of 1:(0.5-1.0), pressed into agglomerates at 10-60 MPa, and subjected to vacuum thermal reduction in a vacuum reduction furnace with a vacuum degree of 1-20 Pa and a thermal reduction temperature of 800-1000° C. to generate metal vapor;
[0019] The reducing agent is selected from one or more of silicon powder, aluminum powder, iron powder and carbon powder.
[0020] [4] The method for preparing ultra-thin lithium metal foil as described in [1], wherein in step (3), the metal vapor is passed through a heat exchange tube into a distillation tank for distillation, and the temperature in the distillation tank is controlled at 300-400°C and the vacuum degree is controlled at 10 -2 -10 -4 Pa, so that the lithium vapor in the metal vapor is condensed into metallic lithium liquid, and the metallic lithium liquid is stored in the lithium storage tank through the connecting pipe, wherein the temperature of the metal vapor passing through the heat exchange tube is reduced from 800-1000°C to 400-500°C, and the heat exchange liquid in the heat exchange tube is heated at the same time, the heat exchange tube is connected to the heat exchange jacket around the distillation tank, and the distillation tank is heated to 300-400°C by using the heat exchange liquid and the heating device, and a ceramic filter with a pore size of 1-10 μm is arranged in the heat exchange tube;
[0021] The sodium vapor and potassium vapor in the metal vapor are secondary distilled by using a distillation pipe connected to a distillation tank, so that the sodium vapor and potassium vapor are condensed in a sodium-potassium condensation tank. An insulation jacket and a heating device are arranged outside the distillation pipe, and the internal temperature is 320-420°C.
[0022] [5] The method for preparing an ultra-thin metal lithium foil as described in [1], wherein in step (4), the metal lithium liquid in the lithium storage tank is passed into a crucible of a vacuum evaporation device, the crucible is heated to convert the metal lithium liquid into lithium vapor, which is deposited on a substrate to form a uniform lithium foil, the lithium foil is collected using a substrate winding collection device, and the collected lithium foil is taken out under an inert atmosphere;
[0023] The vacuum degree in the vacuum evaporation equipment is 10 -2 -10 -4 Pa, the crucible heating temperature is 500-700°C, the distance between the crucible and the substrate is 20-50mm, the winding speed of the winding collection device is 1-5m / min, the substrate is aluminum foil or copper foil, and the inert atmosphere is nitrogen atmosphere or argon atmosphere.
[0024] [6] The method for preparing ultrathin metal lithium foil as described in [1], wherein in step (4), the thickness of the prepared lithium foil is 1-20 μm, the lithium purity in the lithium foil is 99.96wt%-99.99wt%, and the metal lithium recovery rate is 81.7%-85.0%.
[0025] [7] A device for preparing ultra-thin metal lithium foil, which is used to implement the method for preparing ultra-thin metal lithium foil described in [1] to [6], the device comprising a vacuum reduction furnace (2), a heat exchange tube (5), a distillation tank (8), a distillation pipeline (10), a sodium-potassium condensation tank (12), a lithium storage tank (14), and a vapor deposition chamber (16);
[0026] The vacuum reduction furnace (2) is connected to a distillation tank (8) via a heat exchange pipe (5), the distillation tank (8) is connected to a sodium-potassium condensation tank (12) via a distillation pipeline (10), and the distillation tank (8) is connected to a vapor deposition chamber (16) via a lithium storage tank (14).
[0027] [8] The device for preparing ultra-thin lithium metal foil as described in [7], wherein the vacuum reduction furnace (2), the heat exchange tube (5), the distillation tank (8), and the distillation pipeline (10) are all provided with temperature sensors to display the temperature in real time;
[0028] A first vacuum pump (21) is arranged at the upper end of the vacuum reduction furnace (2), a feed port (1) is arranged at the lower end of the vacuum reduction furnace (2), and a slag storage tank (3) is arranged below the vacuum reduction furnace (2);
[0029] The upper end of the distillation tank (8) is connected to a distillation pipeline (10), and the lower end of the distillation tank (8) is connected to a connecting pipe (9), the distillation tank (8) is connected to a lithium storage tank (14) through the connecting pipe (9), and the lithium storage tank (14) is connected to a vacuum evaporation chamber (16) through the connecting pipe (9);
[0030] A sodium-potassium collecting tank (13) is arranged below the sodium-potassium condensing tank (12), and a second vacuum pump (22) is arranged at the upper end of the sodium-potassium condensing tank (12);
[0031] A third vacuum pump (23) is provided at the lower end of the vacuum evaporation chamber (16).
[0032] [9] The device for preparing ultra-thin lithium metal foil as described in [7] or [8] is provided with a pelletizing press (4) in the vacuum reduction furnace (2), a heat exchange jacket and a heating unit are provided outside the distillation tank (8), and a refrigeration jacket is provided around the sodium-potassium condensation tank (12).
[0033]
[10] The device for preparing ultra-thin lithium metal foil as described in [7] or [8], wherein a winding collection device (17), a crucible (18) and a steam hood (19) are arranged in the vacuum evaporation chamber (16), and the crucible (18) and the steam hood (19) are integrated with each other, and the crucible (18) is located below the steam hood (19).
[0034] Compared with the prior art, the lithium raw material in the present invention is processed into a composite lithium salt with a specific component ratio, the lithium raw material has a wide source, the raw material utilization rate is high, and the thermal reduction reaction effect is good; by adopting a continuous integrated process of vacuum thermal reduction-vacuum distillation-vacuum evaporation to produce metal lithium foil, the purity of metal lithium can be improved, the production efficiency can be greatly improved, and it is conducive to industrial production; the lithium in the evaporation process comes from the lithium liquid in the distillation tank, which eliminates the pretreatment process of solid lithium and saves the storage cost of metal lithium ingots; the unique formula of the composite lithium salt of the present invention can promote thermal reduction reaction, so that the recovery rate of metal lithium is higher. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is the XRD diagram of the composite lithium salt of Example 1 of the present invention;
[0036] Figure 2 is the XRD pattern of the composite lithium salt of Example 2 of the present invention;
[0037] Figure 3 is the XRD diagram of the composite lithium salt of Example 3 of the present invention;
[0038] Figure 4 is the XRD pattern of the composite lithium salt of Example 4 of the present invention;
[0039] Figure 5 is the XRD pattern of the composite lithium salt of Example 5 of the present invention;
[0040] Figure 6 is the XRD pattern of the composite lithium salt of Example 6 of the present invention;
[0041] Figure 7 It is a schematic diagram of the device of the present invention. DETAILED DESCRIPTION
[0042] In this specification, when - is used to indicate a numerical range, both endpoints are included and the units are common. For example, 1-20Pa indicates that the vacuum degree is 1Pa or more and 20Pa or less.
[0043] The raw materials, equipment, test conditions and detection methods used in the examples are as follows:
[0044] The vacuum reduction furnace, distillation tank, vacuum pump, and ball mill were purchased from Shanghai Jujing Precision Instrument Manufacturing Co., Ltd., and the vacuum evaporation equipment and film thickness detector were purchased from Guangdong Huicheng Vacuum Technology Co., Ltd.
[0045] The XRD equipment manufacturer is BRUKER of Germany, the model is Bruker D8, and the XRD test conditions are: voltage
[0046] 40KV, current 40Ma, Cu target, scanning range 10-90°, step size 0.02, scanning speed 10° / min.
[0047] The laser particle size analyzer was purchased from Zhuhai Zhenli Optical Instrument Co., Ltd., model: LT3600.
[0048] The ICP detector was purchased from Jiangsu Tianrui Instrument Co., Ltd., and the chemical composition of the metal lithium foil obtained after evaporation was detected according to the conventional method, that is, the ICP test was performed to determine the purity of lithium in the lithium foil.
[0049] The film thickness detector can detect the film thickness during the evaporation process.
[0050] The calculation steps of metal lithium recovery rate are as follows:
[0051] The composite lithium salt is xLiOH·yLi2CO3·zLi2O, and the mass fraction of metallic lithium is:
[0052] W=[6.94×(x / 23.95+y / 36.94+z / 14.94)]×100%
[0053] Weigh a composite lithium salt of mass M, where the mass of metallic lithium (N) is N=MW, and the mass of the substrate before evaporation is n.
[0054] The mass of the substrate after evaporation is m, and the metal lithium recovery rate is R = (mn) / N.
[0055] The present invention is further described in detail below with reference to the accompanying drawings and embodiments.
[0056] The present invention provides a method for preparing an ultra-thin metal lithium foil, which comprises the following steps:
[0057] Step 1: Preparation of composite lithium salt
[0058] The lithium raw material is one or more of a lithium hydroxide-lithium carbonate complex, a lithium hydroxide-lithium carbonate-lithium oxalate complex, and a lithium hydroxide-lithium oxalate complex, and the mass purity is >99%.
[0059] The lithium raw material in the embodiment of the present invention adopts the battery-grade lithium raw material of Jiangxi Ganfeng Lithium Industry Co., Ltd.
[0060] At room temperature, lithium raw materials (lithium hydroxide, lithium carbonate, lithium oxalate) are mixed in a certain ratio and heated to 600 - 800 °C at a heating rate of 1 - 10 °C / min under a vacuum of 1 - 20 Pa for a holding time of 60 - 300 min. After natural cooling, the sample taken out is a块状 solid, which is crushed using zirconium balls with a diameter of 5 mm. The mass ratio of balls to materials is (10 - 15):1, the rotation speed is 500 - 700 rpm, and the ball milling time is 1 - 3 h to obtain composite lithium salt xLiOH·yLi2CO3·zLi2O particles, where x, y, and z are mass fractions. The particle size D50 of the composite lithium salt xLiOH·yLi2CO3·zLi2O is measured using a laser particle size analyzer, and the phase quantitative analysis of the composite lithium salt is carried out by XRD test and GSAS software to determine the values of x, y, and z. By regulating the ratio of lithium raw materials, heating rate, holding time, and ball milling conditions as above, the values of x, y, and z may vary, but as long as x, y, and z satisfy 0 < x < 0.5, 0 < y < 0.5, 0.5 ≤ z < 1, and x + y + z = 1, the thermal reduction reaction effect of the composite lithium salt of the present invention can be achieved; x, y, and z preferably satisfy 0 < x < 0.11, 0 < y < 0.11, 0.8 < z < 1, and x + y + z = 1; more preferably satisfy 0.058 ≤ x < 0.102, 0.024 ≤ y ≤ 0.102, 0.815 ≤ z ≤ 0.912, and x + y + z = 1.
[0061] Since the lithium salts sold on the market are obtained by processing and purifying lithium-containing ores and lithium-containing salt lake brines, trace amounts of sodium salts, potassium salts, magnesium salts, calcium salts, etc. are inevitably contained in the lithium raw materials.
[0062] Step two, vacuum thermal reduction
[0063] The composite lithium salt particles and the reducing agent are mixed evenly at a mass ratio of 1:(0.5 - 1.0), preferably mixed evenly at a mass ratio of 1:(0.6 - 0.72), pressed into pellets at 10 - 60 MPa, and subjected to vacuum thermal reduction in a vacuum reduction furnace with a vacuum of 1 - 20 Pa. The thermal reduction temperature is 800 - 1000 °C, and the thermal reduction time is 4 - 10 h to generate metal vapor. The reducing agent is selected from one or more of silicon powder, aluminum powder, iron powder, and carbon powder.
[0064] Since the holding temperature and time are regulated in step 1, the lithium raw material is decomposed and transformed into a composite lithium salt (lithium source) containing lithium oxide, lithium hydroxide, and lithium carbonate in a specific ratio of the present invention, which makes it easier to achieve a metal thermal reduction reaction with a reducing agent. When the temperature is greater than 450°C, lithium hydroxide will dissolve into a liquid, bringing a certain fluidity between the composite lithium salt and the reducing agent, driving the diffusion of the composite lithium salt, increasing the contact between the composite lithium salt and the reducing agent, and making the thermal reduction reaction more fully carried out. The presence of a small amount of lithium carbonate is conducive to the coordinated diffusion of lithium hydroxide and lithium oxide.
[0065] Step 3: Vacuum distillation
[0066] The metal vapor in step 2 first passes through a ceramic filter with a pore size of 1-10 μm to remove dust, and then the metal vapor passes into the heat exchange tube. The metal vapor and the heat exchange liquid transfer heat, which not only cools the metal vapor, but also heats the heat exchange liquid and then heats the distillation tank. The metal vapor passes through the heat exchange tube into the distillation tank for distillation, and the temperature in the distillation tank is controlled at 300-400℃ and the vacuum degree is controlled at 10 -2 -10 -4 Pa, the lithium vapor in the metal vapor condenses into metallic lithium liquid, which is stored in the lithium storage tank through the connecting pipe, and a heat preservation jacket is set around the lithium storage tank; the sodium vapor and potassium vapor in the metal vapor are passed into the distillation pipeline to condense in the sodium potassium condensation tank, and after the condensation is complete, kerosene is added to the condensation tank and collected in the sodium potassium collection tank. The role of kerosene is to isolate sodium and potassium from air and moisture. Among them, the distillation pipeline plays a role in condensing and recycling the lithium vapor "escaping" in the sodium vapor and potassium vapor. The temperature of the distillation pipeline is maintained at 320-420℃. The material of the distillation pipeline is nickel-chromium alloy, and the material of the heat preservation jacket is phenolic resin; the temperature of the metal vapor after passing through the heat exchange tube is reduced from 800-1000℃ to 400-500℃, and the heat exchange liquid in the heat exchange tube is heated. The heat exchange tube is connected to the heat exchange jacket around the distillation tank to heat the distillation tank to 300-400℃. In addition, the distillation pipeline is provided with a heating device. A condensation jacket is set around the sodium potassium condensation tank, and the cooling temperature is -10℃.
[0067] Since lithium raw materials inevitably contain a small amount of impurities of metal compounds other than lithium, the obtained metallic lithium will also contain some corresponding metal impurities. Since the vapor pressures of different metals are different at the same temperature, their behaviors during condensation are also different. Therefore, in the vacuum distillation step, the relationship between metal vapor pressure and temperature is used to precisely control the temperature, so that metallic lithium can be easily separated from the impurities of metallic sodium and metallic potassium.
[0068] Step 4: Vacuum evaporation
[0069] The metal lithium liquid in the lithium storage tank is passed into the crucible of the vacuum evaporation equipment, and the crucible is heated to turn the metal lithium liquid into lithium vapor, which is then deposited on the substrate to form a uniform lithium foil. The lithium foil is collected by a winding collection device and the collected lithium foil is taken out under an inert atmosphere. The temperature of the wound collected substrate is maintained at 50-80°C, and the vacuum degree of the vacuum evaporation equipment is 10 -2 -10 -4 Pa, the crucible heating temperature is 500-700°C, the distance between the crucible and the substrate is 20-50mm, the winding speed of the winding collection device is 1-5m / min, the substrate is aluminum foil or copper foil, the inert atmosphere is nitrogen atmosphere or argon atmosphere, the thickness of the prepared lithium foil is 1-20μm, preferably 1-15μm, more preferably 5-13μm, the lithium purity in the lithium foil is 99.96wt%-99.99wt%, and the recovery rate of metallic lithium is 80.0%-90.0%, preferably 81.7%-85.0%.
[0070] The metallic lithium liquid in the lithium storage tank can be introduced into the crucible of the vacuum evaporation equipment by means of a liquid feeding paddle, and the liquid feeding paddle is rotated at a uniform speed by electricity to uniformly feed the metallic lithium liquid into the crucible.
[0071] Vacuum evaporation is an effective method for preparing nano-scale and ultra-thin lithium metal foil of more than ten microns. By controlling the heating temperature of the crucible, the winding rate of the winding collection device, and the distance between the substrate and the crucible, the thickness of the lithium metal foil can be controlled to 1-20μm, preferably 1-15μm, and more preferably 5-13μm. This is a thickness that is difficult to achieve by the current calendering method, and it is also a huge challenge for the calendering equipment. See the structural diagram of the vacuum evaporation equipment for details. Figure 7 The evaporation chamber (16) shown in FIG.
[0072] In addition, the present invention provides a device for preparing an ultra-thin metal lithium foil, which is used to implement the method for preparing the ultra-thin metal lithium foil, and the device comprises the following components:
[0073] A feed port (1), a vacuum reduction furnace (2), a slag storage tank (3), a pelletizing pressure device (4), a heat exchange tube (5), a ceramic filter (6), a valve (7), a distillation tank (8), a connecting pipe (9), a distillation pipeline (10), a kerosene feed port (11), a sodium potassium condensation tank (12), a sodium potassium collection tank (13), a lithium storage tank (14), a liquid delivery paddle (15), a vapor deposition chamber (16), a winding collection device (17), a crucible (18), a vapor cover (19), a chamber door (20), a first vacuum pump (21), a second vacuum pump (22), a third vacuum pump (23), etc.
[0074] The vacuum reduction furnace (2) is connected to a distillation tank (8) via a heat exchange pipe (5), the distillation tank (8) is connected to a sodium-potassium condensation tank (12) via a distillation pipeline (10), and the distillation tank (8) is connected to a vapor deposition chamber (16) via a lithium storage tank (14).
[0075] The invention is also applicable to the preparation of metal magnesium foil, aluminum foil, nickel foil, tin foil, copper foil and zinc foil.
[0076] Example 1
[0077] Step 1: Preparation of composite lithium salt
[0078] The lithium raw materials 0.85LiOH-0.15Li2CO3 (by mass fraction) were uniformly mixed, and the temperature was raised to 600℃ at a heating rate of 5℃ / min under a vacuum degree of 1Pa, and the holding time was 150min. The sample was taken out after natural cooling. The taken out sample was a block solid, which was crushed by a ball mill containing zirconium balls with a diameter of 5mm, the ball-to-material mass ratio was 10:1, the rotation speed was 500rpm, and the ball milling time was 1h. The composite lithium salt was obtained by ball milling. The particle size of the composite lithium salt was determined by a laser particle size analyzer. The particle size D50 of the composite lithium salt was 30μm. The composite lithium salt was qualitatively and quantitatively analyzed by XRD test and GSAS software, as shown in FIG. Figure 1 As shown, after XRD testing, the diffraction pattern of the composite lithium salt of LiOH, Li2O and Li2CO3 appeared. The qualitative analysis of the chemical composition was carried out by measuring the diffraction angle (peak position), and the quantitative analysis was carried out by measuring the integral intensity (peak intensity) of the spectrum line. The chemical formula of the composite lithium salt was determined to be 0.092LiOH·0.048Li2CO3·0.86Li2O.
[0079] Step 2: Vacuum thermal reduction to generate metal vapor
[0080] The composite lithium salt and the reducing agent aluminum powder are mixed in a mass ratio of 1:0.7. 3.214 kg of the composite lithium salt (equivalent to 102.19 mol of 0.092LiOH·0.048Li2CO3·0.86Li2O) and 2.25 kg of aluminum powder (equivalent to 83.40 mol of Al atoms) are weighed and mixed evenly, pressed into agglomerates at 30 MPa, and vacuum thermal reduction is carried out in a vacuum reduction furnace with a vacuum degree of 1 Pa. The thermal reduction temperature is 800°C and the thermal reduction time is 6 hours to generate metal vapor.
[0081] Step 3: Vacuum distill the metal vapor
[0082] The metal vapor in step 2 first passes through a ceramic filter with a pore size of 1 μm to remove dust. The metal vapor passes through a heat exchange tube, the temperature is reduced from 800°C to 400°C, and then passes into a distillation tank for distillation. The temperature in the distillation tank is controlled at 400°C and the vacuum degree is controlled at 5×10 -3 Pa, the lithium vapor in the metal vapor condenses into metallic lithium liquid and is stored in a lithium storage tank through a connecting pipe; the sodium vapor and potassium vapor in the metal vapor are passed into a distillation pipe and condensed in a sodium-potassium condensation tank, and the temperature of the distillation pipe is maintained at 320°C. Among them, the distillation pipe plays a role in condensing and recovering the lithium vapor that "escaped" in the sodium vapor and potassium vapor; the temperature of the metal vapor after passing through the heat exchange pipe is reduced from 800°C to 400°C, the heat exchange liquid in the heat exchange pipe is heated, and the heat exchange pipe is connected to the heat exchange jacket around the distillation tank to transfer the exchange heat to the distillation tank, and then the distillation tank is heated to 400°C through the heating unit. A condensation jacket is set around the sodium-potassium condensation tank, and the cooling temperature is -10°C to condense the sodium vapor and potassium vapor.
[0083] Step 4: Preparation of ultra-thin lithium metal foil by vacuum evaporation
[0084] The metallic lithium liquid in the lithium storage tank is passed into the crucible of the vacuum evaporation equipment through the liquid feeding paddle. The liquid feeding paddle has three blades, which rotate at a uniform speed through electricity to uniformly transfer the metallic lithium liquid to the crucible, heat the crucible, and raise the crucible temperature to 600°C. The metallic lithium liquid turns into lithium vapor, which is then deposited on the substrate to form a uniform lithium foil. The substrate is wound by a winding collection device, and the lithium foil is collected at the same time. After the evaporation is completed, argon gas is introduced to take out the lithium foil. The vacuum degree of the vacuum evaporation equipment is 5×10 -3 Pa, the distance between the crucible and the substrate is 20 mm, the winding speed of the winding collection device is 1 m / min, the temperature of the winding substrate is 70°C, and the substrate is copper foil.
[0085] The schematic diagram of the equipment used in the embodiment is as follows Figure 7 As shown, the schematic diagrams show the devices of the present application in a schematic manner and not in actual size and proportion.
[0086] The thickness of the obtained lithium foil is measured by a film thickness detector. The chemical composition of the metal lithium foil obtained after evaporation is detected by an ICP detector to determine the purity of lithium in the lithium foil. The metal lithium recovery rate is calculated according to the above calculation steps of the metal lithium recovery rate.
[0087] The thickness of the lithium foil prepared in Example 1 was 13 μm, the lithium purity in the lithium foil was 99.99 wt %, and the recovery rate of metallic lithium was 85.0%.
[0088] Embodiments 2 to 6
[0089] The steps of the preparation method are basically the same as those of Example 1, except for the related components and parameters, etc., as shown in Tables 1 to 5.
[0090] Comparative Examples 1 to 4
[0091] The steps of the preparation method are basically the same as those of Example 1, except for the related components and parameters, etc., as shown in Tables 1 to 5.
[0092] Table 1
[0093]
[0094] Table 2
[0095]
[0096] Table 3
[0097]
[0098] Table 4
[0099]
[0100] Table 5
[0101]
[0102] As shown in Table 5, the test results of Examples 1 to 6 and Comparative Examples 1 to 4 are analyzed to show that, compared with the composite lithium salt xLiOH·yLi2CO3·zLi2O of Examples 1 to 6, the lithium raw material of Comparative Examples 1 to 4 is lithium carbonate or lithium hydroxide. After thermal decomposition, the composite lithium salts obtained are respectively a composite of lithium carbonate and lithium oxide, or a composite of lithium hydroxide and lithium oxide. The recovery rates of the obtained metal lithium are 65.4%, 74.8%, 73.4%, and 77.3%, respectively, which are significantly lower than those of Examples 1 to 6. The principle may be that the composite lithium salts of Examples 1 to 6 contain lithium hydroxide, lithium carbonate, and lithium oxide in a specific ratio range. When the temperature is greater than 450°C, lithium hydroxide will dissolve into liquid, bring a certain fluidity between the composite lithium salt and the reducing agent, drive the diffusion of the composite lithium salt, increase the contact between the composite lithium salt and the reducing agent, and make the thermal reduction reaction more sufficient. At the same time, the presence of a small amount of lithium carbonate is conducive to the coordinated diffusion of lithium hydroxide and lithium oxide, so that the recovery rate of metal lithium is higher.
[0103] As shown in Table 5, analysis of the test results of Comparative Examples 1, 3 and Comparative Examples 2, 4 shows that the thermal decomposition temperature of Comparative Examples 1 and 3 is 600°C, and the thermal decomposition temperature of Comparative Examples 2 and 4 is increased to 800°C, which significantly improves the decomposition rate of the raw material components. Compared with Comparative Examples 1 and 3, the lithium recovery rate is significantly improved, but it is still lower than that of Examples 1 to 6. This once again shows that the synergistic effect of lithium hydroxide and lithium carbonate in the composite lithium salt improves the efficiency of vacuum thermal reduction.
[0104] As shown in Table 5, the test results of Examples 1 to 6 and Comparative Examples 1 to 4 show that the purity of lithium in Examples 1 to 6 is above 99.96%, and the metal recovery rate is above 81.7%, both higher than Comparative Examples 1 to 4. The principle may be that the lithium raw material uses a composite lithium salt, the thermal reduction temperature is low, and the raw material utilization rate is higher. In addition, by adopting a continuous integrated process of vacuum reduction-vacuum distillation-vacuum evaporation, the lithium in the evaporation process comes from the lithium liquid in the distillation tank, eliminating the pretreatment of solid lithium, saving the storage cost of metal lithium ingots, and greatly improving production efficiency. Therefore, the purity of metal lithium is improved, which is conducive to improving the recovery rate of metal lithium. The recovery rate of metal lithium of the present invention will be affected by the raw materials, reaction process and industrial reaction equipment of the thermal reduction reaction, and has made substantial progress compared with the prior art.
[0105] The beneficial effects of the present invention are summarized as follows:
[0106] 1. The present invention can continuously perform vacuum reduction, vacuum distillation and vacuum evaporation by precisely controlling the formula of the composite lithium salt, the temperature of the thermal reduction reaction, the temperature of the distillation equipment, the degree of vacuum, the materials and the reducing agent, so as to continuously prepare, purify and evaporate lithium, thereby improving the production efficiency of the ultra-thin metal lithium foil, saving the preparation cost and achieving the desired effect.
[0107] The metal lithium foil with a thickness of 5-13 μm and a purity of more than 99.96 wt% was successfully obtained.
[0108] 2. The present invention integrates a vacuum reduction furnace, a distillation tank and an evaporation device to continuously prepare and evaporate lithium, and adopts a heat exchange tube as a connecting pipe. Heat exchange devices are arranged around a plurality of equipment components to recycle "waste heat". The integrated equipment can simplify the preparation process, improve the production efficiency of ultra-thin metal lithium foil, improve the purity of metal lithium, reduce the mixing of external impurities, eliminate material losses caused by material transfer between discontinuous equipment, and reduce energy consumption and storage costs.
[0109] 3. The composite lithium salt used in the present invention promotes the full progress of the thermal reduction reaction. When the temperature is greater than 450°C, lithium hydroxide will dissolve into liquid, bringing a certain fluidity between the composite lithium salt and the reducing agent, thereby driving the composite lithium salt to diffuse more evenly, improving the contact degree between the composite lithium salt and the reducing agent, and making the thermal reduction reaction more fully carried out. The presence of a small amount of lithium carbonate is conducive to the coordinated diffusion of lithium hydroxide and lithium oxide, so that the recovery rate of metal lithium is higher.
[0110] 4. The lithium source required for evaporation flows directly into the crucible in the form of high-temperature liquid. Compared with the solid lithium ingots used in the traditional evaporation process, there is no need to treat and package the lithium source with surface oxides, which saves the storage cost of the lithium ingots, reduces energy consumption, and simplifies the complex process steps.
[0111] The above description of all disclosed embodiments is only the best embodiment of the present invention and the technical principles used, and is not intended to limit the present invention. Those skilled in the art will understand that various modifications to these embodiments are obvious to those skilled in the art. Obviously, various changes and modifications made by those skilled in the art to the embodiments do not depart from the spirit and scope of the present invention, and these changes and modifications should be included in the protection scope of the present invention.
[0112] Description of Reference Numerals
[0113] 1. Feed inlet; 2. Vacuum reduction furnace; 3. Slag storage tank; 4. Briquetting pressure device; 5. Heat exchange tube; 6. Micron ceramic filter; 7. Valve; 8. Distillation tank; 9. Connecting pipe; 10. Distillation pipeline; 11. Kerosene feed inlet; 12. Sodium-potassium condensation tank; 13. Sodium-potassium collection tank; 14. Lithium storage tank; 15. Liquid feeding paddle; 16. Vacuum evaporation chamber; 17. Winding collection device; 18. Crucible; 19. Steam hood; 20. Chamber door; 21. First vacuum pump; 22. Second vacuum pump; 23. Third vacuum pump.
Claims
1. A method for preparing an ultra-thin lithium metal foil, characterized in that: The following steps are involved: (1) A composite lithium salt preparation step, wherein the lithium raw material is heated and then cooled, and ball milled to obtain a composite lithium salt with a chemical formula of xLiOH·yLi2CO3·zLi2O, wherein x, y, and z are mass fractions and satisfy 0 <x<0.5、0<y<0.5、0.5≤z<1、x+y+z=1; (2) a vacuum thermal reduction step, wherein the composite lithium salt and the reducing agent are mixed uniformly and pressed, and vacuum thermal reduction is performed in a vacuum reduction furnace to generate metal vapor; (3) a vacuum distillation step, wherein the metal vapor is passed through a heat exchange tube into a distillation tank for vacuum distillation, so that lithium vapor in the metal vapor is condensed into metallic lithium liquid, and the metallic lithium liquid is stored in a lithium storage tank through a connecting tube; (4) a vacuum evaporation step, wherein the metallic lithium liquid in the lithium storage tank is introduced into a crucible of a vacuum evaporation device by a liquid feeding paddle, and heated so that the metallic lithium liquid is converted into lithium vapor, which is deposited on the substrate to form a uniform lithium foil; The lithium raw material in step (1) is one or more of lithium hydroxide-lithium carbonate, lithium hydroxide-lithium carbonate-lithium oxalate or lithium hydroxide-lithium oxalate; The temperature of the vacuum thermal reduction in step (2) is 800-900° C. and the vacuum degree is 1-20 Pa; The vacuum degree of the vacuum distillation in step (3) is 10 -2 -6×10 -3 Pa; The vacuum degree in the vacuum evaporation equipment in step (4) is 10 -3 -10 -4 Pa.
2. The method for preparing the ultra-thin metal lithium foil according to claim 1, characterized in that: In step (1), at room temperature, the lithium raw material is heated to 600-800°C at a rate of 1-10°C / min under a vacuum degree of 1-20 Pa, and the temperature is kept at this temperature for 60-300 min. After natural cooling, the composite lithium salt xLiOH·yLi2CO3·zLi2O is obtained by ball milling, wherein x, y, and z are mass fractions and satisfy 0 <x<0.5、0<y<0.5、0.5≤z<1、x+y+z=1; The particle size of the composite lithium salt after ball milling is 20 μm≤D50≤70 μm, and the mass ratio of the ball to the material is (10-15):
1.
3. The method for preparing the ultra-thin metal lithium foil according to claim 1, characterized in that: In step (2), the composite lithium salt and the reducing agent are mixed uniformly in a mass ratio of 1: (0.5-1.0), pressed into agglomerates at 10-60 MPa, and vacuum thermally reduced in a vacuum reduction furnace with a vacuum degree of 1-20 Pa and a thermal reduction temperature of 800-900° C. to generate metal vapor; The reducing agent is selected from one or more of silicon powder, aluminum powder, iron powder or carbon powder.
4. The method for preparing the ultra-thin metal lithium foil according to claim 1, characterized in that: In step (3), the metal vapor is passed through a heat exchange tube into a distillation tank for vacuum distillation, and the temperature in the distillation tank is controlled at 300-400°C and the vacuum degree is controlled at 10 -2 -6×10 -3 Pa, so that the lithium vapor in the metal vapor is condensed into metallic lithium liquid, and the metallic lithium liquid is stored in the lithium storage tank through the connecting pipe, wherein the temperature of the metal vapor passing through the heat exchange tube is reduced from 800-900°C to 400-500°C, and the heat exchange liquid in the heat exchange tube is heated at the same time, the heat exchange tube is connected to the heat exchange jacket around the distillation tank, and the distillation tank is heated to 300-400°C by using the heat exchange liquid and the heating device, and a ceramic filter with a pore size of 1-10 μm is arranged in the heat exchange tube; The sodium vapor and potassium vapor in the metal vapor are secondary distilled by using a distillation pipe connected to a distillation tank, so that the sodium vapor and potassium vapor are condensed in a sodium-potassium condensation tank. An insulation jacket and a heating device are arranged outside the distillation pipe, and the internal temperature is 320-420°C.
5. The method for preparing the ultra-thin metal lithium foil according to claim 1, characterized in that: In step (4), the metallic lithium liquid in the lithium storage tank is passed into the crucible of the vacuum evaporation equipment through a liquid feeding paddle, the crucible is heated to convert the metallic lithium liquid into lithium vapor, and the lithium vapor is deposited on the substrate to form a uniform lithium foil, the lithium foil is collected by a substrate winding collection device, and the collected lithium foil is taken out under an inert atmosphere; The vacuum degree in the vacuum evaporation equipment is 10 -3 -10 -4 Pa, the heating temperature of the crucible is 500-700°C, the distance between the crucible and the substrate is 20-50mm, the winding speed of the winding collection device is 1-5m / min, the substrate is aluminum foil or copper foil, and the inert atmosphere is nitrogen atmosphere or argon atmosphere.
6. The method for preparing the ultra-thin lithium metal foil according to claim 1, characterized in that: In step (4), the thickness of the prepared lithium foil is 1-20 μm, the lithium purity in the lithium foil is 99.96 wt%-99.99 wt%, and the recovery rate of metallic lithium is 81.7%-85.0%.
7. A device for preparing ultra-thin lithium metal foil, which is used to implement the method for preparing ultra-thin lithium metal foil according to any one of claims 1 to 6, characterized in that: The equipment comprises a vacuum reduction furnace (2), a heat exchange tube (5), a distillation tank (8), a distillation pipeline (10), a sodium-potassium condensation tank (12), a lithium storage tank (14), a liquid delivery paddle (15), and a vacuum evaporation chamber (16); The vacuum reduction furnace (2) is connected to a distillation tank (8) via a heat exchange pipe (5), the distillation tank (8) is connected to a sodium-potassium condensation tank (12) via a distillation pipeline (10), and the distillation tank (8) is connected to a vacuum evaporation chamber (16) via a lithium storage tank (14).
8. The device for preparing ultra-thin lithium metal foil according to claim 7, characterized in that: The vacuum reduction furnace (2), the heat exchange tube (5), the distillation tank (8), and the distillation pipeline (10) are all provided with temperature sensors to display the temperature in real time; A first vacuum pump (21) is arranged at the upper end of the vacuum reduction furnace (2), a feed port (1) is arranged at the lower end of the vacuum reduction furnace (2), and a slag storage tank (3) is arranged below the vacuum reduction furnace (2); The upper end of the distillation tank (8) is connected to a distillation pipeline (10), and the lower end of the distillation tank (8) is connected to a connecting pipe (9), the distillation tank (8) is connected to a lithium storage tank (14) through the connecting pipe (9), and the lithium storage tank (14) is connected to a vacuum evaporation chamber (16) through the connecting pipe (9); A sodium-potassium collecting tank (13) is arranged below the sodium-potassium condensing tank (12), and a second vacuum pump (22) is arranged at the upper end of the sodium-potassium condensing tank (12); A third vacuum pump (23) is provided at the lower end of the vacuum evaporation chamber (16).
9. The device for preparing ultra-thin lithium metal foil according to claim 7 or 8, characterized in that: A briquetting pressure device (4) is arranged in the vacuum reduction furnace (2), a heat exchange jacket and a heating unit are arranged outside the distillation tank (8), and a refrigeration jacket is arranged around the sodium-potassium condensation tank (12).
10. The device for preparing ultra-thin lithium metal foil according to claim 7 or 8, characterized in that: A winding collection device (17), a crucible (18) and a steam cover (19) are arranged in the vacuum evaporation chamber (16); the crucible (18) and the steam cover (19) are arranged in an integrated manner, and the crucible (18) is located below the steam cover (19).
Citation Information
Patent Citations
Lithium preparing process with lithium carbonate
CN1213158C
Method and system for preparing ultra-thin metal lithium strip by using low-grade lithium source
CN109182758A
Heat reduction preparation and purification process and equipment of metal lithium
CN1299884A
Method for producing lithium and device therefor
CN1377425A