Semi-transparent EMI shielding based on ultra-thin conductors

The broadband electromagnetic interference shielding device, fabricated using a flexible laminated structure and co-sputtering process, solves the balance problem between transparency and shielding effect in traditional electromagnetic shielding devices, achieving highly efficient electromagnetic interference shielding and high visible light transmission, and is suitable for a variety of electronic and optical applications.

CN113544795BActive Publication Date: 2024-11-22THE RGT UNIV OF MICHIGAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080017952.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-02-28
Publication Date
2024-11-22
Estimated Expiration
2040-02-28

AI Technical Summary

Technical Problem

Existing electromagnetic shielding devices struggle to achieve a balance between transparency and broadband electromagnetic interference shielding effectiveness, especially in applications requiring high visibility. The narrow-band performance and mechanical flexibility of traditional metamaterials are insufficient, limiting their use in flexible electronics.

Method used

A flexible laminated structure, including an ultrathin metal film and conductive dielectric material, combined with a graphene layer and a spacer layer, is used to form a broadband electromagnetic interference shield. A continuous silver-copper alloy film is prepared by co-sputtering process to achieve high shielding efficiency in the frequency range of 600MHz to 90GHz, while maintaining high transmission efficiency in the visible light range of 390nm to 740nm.

Benefits of technology

It achieves effective shielding against electromagnetic interference over a wide frequency band while maintaining high visible light transmittance, and possesses good mechanical flexibility and ease of manufacturing, making it suitable for various electronic devices and optical instruments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113544795B_ABST
    Figure CN113544795B_ABST
Patent Text Reader

Abstract

An electromagnetic interference shield and method for broadband electromagnetic interference (EMI) shielding are provided. An EMI shield disposed in an electromagnetic radiation path blocks a wide frequency range (> about 800 MHz to < about 90 GHz) to achieve a shielding efficiency of > to 20 dB, while wavelengths in the visible range are transmitted through the electromagnetic shield to achieve an average transmission efficiency of > about 85%. The shield includes a flexible stack comprising a continuous ultra-thin metal film and two anti-reflective dielectric layers, the continuous ultra-thin metal film comprising silver (Ag) and copper (Cu), and the two anti-reflective dielectric layers are disposed on either side of the ultra-thin metal film. The shield may also include multiple stacks or optional graphene layers, which may be spaced apart from the flexible stack to achieve radio frequency (RE) absorption, which provides an additional form of EMI shielding. The EMI shielding may be made via roll-to-roll sputtering.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Provisional Application No. 62 / 812,706, filed on March 1, 2019. The entire disclosure of the above application is incorporated herein by reference. Technical Field

[0003] The present disclosure relates to a method for broadband electromagnetic interference (EMI) shielding with transmission of visible light by using an electromagnetic shielding member including a flexible laminate having a continuous ultra-thin metal film including silver (Ag) and copper (Cu) and at least two layers including a conductive dielectric material. Background Art

[0004] This section provides background information related to the present disclosure which is not necessarily prior art.

[0005] Remarkable advances in information technology, especially the rapid rise of modern electronics using microwave wireless communications and highly integrated circuits, have generated significant electromagnetic energy pollution, also known as electromagnetic interference (EMI). EMI can cause unacceptable malfunctions in electronic systems used in a wide range of industrial, civil, commercial, and scientific research applications (e.g., aerospace, aircraft, automobiles, and satellite communication instruments). In addition, it has been reported that long-term exposure to intense electromagnetic radiation may cause health hazards, including cancer and insomnia. Therefore, it is advantageous to minimize or eliminate exposure to adverse electromagnetic waves to protect electronic system operations (including sensitive circuits) and maintain a healthy living environment.

[0006] Similarly, there is an increased demand for high-performance electromagnetic interference (EMI) shielding, such as microwave frequency absorbers (microwave absorbers (MA)) that can reduce unwanted radiation. Microwave absorbers (MA) can also enhance energy collection efficiency and improve detector sensitivity, etc. In view of the widespread use of various optoelectronic devices, including wearable sensors and smartphones and the associated complex electromagnetic environment, EMI shielding technology has become more important. However, many traditional electromagnetic shielding devices are opaque, which limits their use in optical applications that require high visible transparency. Therefore, in many applications, such as aircraft windows and displays, aerospace detection facilities, liquid crystal displays (LCDs), mobile communication devices, and optical detection devices used in medical and electronic safety fields, electromagnetic shielding / microwave absorbers are required to provide high visible light transmittance and simultaneously attenuate microwave transmission.

[0007] Recently, so-called meta-materials have been realized through engineering material structures, which can manipulate the effective dielectric constant and magnetic permeability to control microwave responses, such as transmission and reflection. It has been shown that semi-transparent microwave meta-material absorbers can be obtained by minimizing reflection by impedance matching. Although meta-materials offer great potential for perfect microwave absorption, their application is largely limited by undesirable narrow-band performance, which means that they can only block or attenuate a narrow selected wavelength range. However, reducing electromagnetic interference (EMI) across a wide radio frequency band of wavelengths rather than reducing electromagnetic interference (EMI) over a narrow frequency band is more conducive to eliminating the adverse effects of an increasingly complex electromagnetic environment. In addition, poor mechanical flexibility and manufacturing complexity significantly limit the use of meta-material absorbers and other similar absorbers in flexible electronics. It would be desirable to develop EMI shielding devices with high optical transparency and strong electromagnetic wave attenuation. Further, good mechanical flexibility is highly desirable so that EMI shielding devices can be manufactured in a scalable and low-cost manner. Summary of the invention

[0008] This section provides a general summary of the disclosure, and is not a comprehensive disclosure of its full scope or all of its features.

[0009] In certain aspects, the present disclosure relates to a method for broadband electromagnetic interference (EMI) shielding, the method comprising providing an electromagnetic shield in a transmission path of electromagnetic radiation. The method comprises using the electromagnetic shield to block a frequency range of greater than or equal to about 600 MHz to less than or equal to about 90 GHz to achieve a shielding efficiency greater than or equal to 20 dB, while transmitting a wavelength range in the visible range of greater than or equal to about 390 nm to less than or equal to about 740 nm through the electromagnetic shield to achieve an average visible transmission efficiency greater than or equal to about 65%. The electromagnetic shield comprises a flexible laminate, the flexible laminate comprising a continuous metal film, the continuous metal film defining a first side and an opposite second side, and the continuous metal film comprising greater than or equal to about 80 atomic % of silver (Ag) and less than or equal to about 20 atomic % of copper (Cu), having a thickness less than or equal to about 10 nm, having a sheet resistance less than or equal to about 20 Ohm / square, and the continuous metal film is substantially transparent to the wavelength range. The flexible stack also includes a first conductive layer disposed adjacent to the first side of the continuous metal film. The first conductive layer includes a conductive dielectric material selected from the group consisting of: indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine doped tin oxide, poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. A second conductive layer is disposed adjacent to the second side of the continuous metal film. The second conductive layer includes a conductive dielectric material selected from the group consisting of: indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine doped tin oxide, poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof.

[0010] In one aspect, the electromagnetic shield further comprises a graphene layer.

[0011] In one aspect, the graphene layer includes at least one dopant.

[0012] In one aspect, the electromagnetic shield further comprises at least one spacer layer comprising a dielectric material disposed between the graphene layer and the second conductive layer of the flexible stack.

[0013] In one aspect, at least one spacer layer has a thickness corresponding to one quarter of a peak wavelength of electromagnetic radiation in a frequency range of greater than or equal to about 800 MHz to less than or equal to about 90 GHz.

[0014] In one aspect, the blocking is for a frequency range of greater than or equal to about 8 GHz to less than or equal to about 40 GHz to achieve a shielding effectiveness greater than or equal to 26 dB.

[0015] In one aspect, the electromagnetic shield further comprises a graphene layer which together with the flexible stack defines a resonator cavity such that the blocking comprises absorption within the resonator cavity in the frequency range of greater than or equal to about 800 MHz to less than or equal to about 90 GHz such that the reflectivity of the electromagnetic shield is less than or equal to about 1%.

[0016] In one aspect, the shielding efficiency is greater than or equal to 20 dB, and the average visible transmission efficiency is greater than or equal to about 85%.

[0017] In one aspect, the shielding efficiency is greater than or equal to 30 dB, and the average visible transmission efficiency is greater than or equal to about 80%.

[0018] In one aspect, the shielding efficiency is greater than or equal to 50 dB, and the average visible transmission efficiency is greater than or equal to about 65%.

[0019] In one aspect, the first conductive layer has a thickness less than or equal to about 45 nm, and the second conductive layer has a thickness less than or equal to about 45 nm.

[0020] In one aspect, the flexible stack further comprises a substrate that is transmissive to these wavelength ranges.

[0021] In one aspect, the flexible laminate has a sheet resistance (R) of less than or equal to 20 Ohm / square after greater than or equal to about 250 bending cycles. s ).

[0022] The present disclosure also relates to a method for broadband electromagnetic shielding, which includes arranging an electromagnetic shield in the transmission path of electromagnetic radiation. The electromagnetic shield blocks a frequency range of greater than or equal to about 800 MHz to less than or equal to about 90 GHz to achieve a shielding efficiency greater than or equal to 20 dB, and transmits a wavelength range in the visible range of greater than or equal to about 390 nm to less than or equal to about 740 nm through the electromagnetic shield to achieve an average visible transmission efficiency greater than or equal to about 65%. The electromagnetic shield includes a first flexible laminate and a second flexible laminate. The first flexible laminate includes a first continuous metal film, the first continuous metal film defines a first side and an opposite second side, and the first continuous metal film contains greater than or equal to about 80 atomic % of silver (Ag) and less than or equal to about 20 atomic % of copper (Cu), has a thickness less than or equal to about 10 nm, has a sheet resistance less than or equal to about 20 Ohm / square, and the first continuous metal film is substantially transparent to the wavelength range. The first flexible laminate also includes a first conductive layer, which is disposed on the first side of the first continuous metal film. The first conductive layer comprises a conductive dielectric material selected from the group consisting of: indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine doped tin oxide, poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. The second conductive layer is disposed on the second side of the first continuous metal film. The second conductive layer comprises a conductive dielectric material from the group consisting of: indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine doped tin oxide, poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. The second flexible stack comprises a second continuous metal film, the second continuous metal film defining a first side and an opposite second side, and the second continuous metal film comprises greater than or equal to about 80 atomic % silver (Ag) and less than or equal to about 20 atomic % copper (Cu), has a thickness less than or equal to about 10 nm, has a sheet resistance less than or equal to about 20 Ohm / square, and the second continuous metal film is substantially transparent to the wavelength range. The second flexible stack also includes a third layer, the third layer is disposed on the first side of the second continuous metal film. The third layer includes a conductive dielectric material selected from the group consisting of: indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine doped tin oxide, poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. The second flexible stack also includes a fourth layer, which is disposed on the second side of the second continuous metal film. The fourth layer includes a conductive dielectric material selected from the group consisting of: indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine doped tin oxide, poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. A spacer layer including a dielectric material is also disposed between the first flexible stack and the second flexible stack.

[0023] In one aspect, the spacer layer has a thickness corresponding to one quarter of the peak wavelength of electromagnetic radiation in the frequency range of greater than or equal to about 800 MHz to less than or equal to about 90 GHz.

[0024] In one aspect, the shielding efficiency is greater than or equal to 30 dB, and the average visible transmission efficiency is greater than or equal to about 80%.

[0025] In one aspect, the shielding efficiency is greater than or equal to 50 dB, and the average visible transmission efficiency is greater than or equal to about 65%.

[0026] The present disclosure also relates to an electromagnetic interference (EMI) shield, the electromagnetic interference shield comprising a first flexible laminate, the first flexible laminate comprising a first continuous metal film, the first continuous metal film defining a first side and an opposite second side, and the first continuous metal film comprises greater than or equal to about 80 atomic % silver (Ag) and less than or equal to about 20 atomic % copper (Cu), has a thickness less than or equal to about 10 nm, has a sheet resistance less than or equal to about 20 Ohm / square, and the first continuous metal film is substantially transparent to a wavelength range within the visible range of greater than or equal to about 390 nm to less than or equal to about 740 nm. The first flexible laminate also includes a first conductive layer disposed on the first side of the first continuous metal film. The first conductive layer includes a conductive dielectric material selected from the group consisting of: indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. The first flexible laminate also includes a second conductive layer disposed on the second side of the first continuous metal film. The second conductive layer includes a conductive dielectric material selected from the group consisting of: indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. Also included is a second flexible stack, the second flexible stack including a second continuous metal film, the second continuous metal film defining a first side and an opposite second side, and the second continuous metal film contains greater than or equal to about 80 atomic % silver (Ag) and less than or equal to about 20 atomic % copper (Cu), has a thickness of less than or equal to about 10 nm, has a sheet resistance of less than or equal to about 20 Ohm / square, and the second continuous metal film is substantially transparent to a wavelength range within the visible range of greater than or equal to about 390 nm to less than or equal to about 740 nm. The second flexible stack also includes a third layer, the third layer is disposed on the first side of the second continuous metal film. The third layer includes a conductive dielectric material selected from the group consisting of: indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine doped tin oxide, poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. The fourth layer is disposed on the second side of the second continuous metal film. The fourth layer includes a conductive dielectric material selected from the group consisting of: indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine doped tin oxide, poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. A spacer layer including a dielectric material is disposed between the first flexible stack and the second flexible stack.

[0027] In other aspects, the present disclosure relates to an electromagnetic interference (EMI) shield, the electromagnetic interference shield comprising a continuous metal film, the continuous metal film defining a first side and an opposite second side, and the continuous metal film contains greater than or equal to about 80 atomic % silver (Ag) and less than or equal to about 20 atomic % copper (Cu), has a thickness of less than or equal to about 10 nm, and has a sheet resistance of less than or equal to about 20 Ohm / square. A first conductive layer is disposed in contact with the first side of the continuous metal film. The first conductive layer includes a conductive dielectric material selected from the group consisting of: indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine doped tin oxide, poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. A second conductive layer is disposed in contact with the second side of the continuous metal film, wherein the second conductive layer includes a conductive dielectric material selected from the group consisting of: indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine doped tin oxide, poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. A spacer layer includes a dielectric material adjacent to the second conductive layer. The graphene layer is adjacent to the spacer layer.

[0028] In one aspect, the electromagnetic interference (EMI) shield further includes an electrical gating system including a first terminal electrically connected to the graphene layer, a second terminal electrically connected to the continuous metal film, and a voltage source electrically connected to the first terminal and the second terminal.

[0029] In one aspect, the graphene layer includes at least one dopant.

[0030] In one aspect, the graphene layer is a first graphene layer and the electromagnetic interference (EMI) shield further includes a second graphene layer.

[0031] In one aspect, the spacer layer has a thickness corresponding to one quarter of the peak wavelength of electromagnetic radiation in the frequency range of greater than or equal to about 800 MHz to less than or equal to about 90 GHz.

[0032] In one aspect, the continuous metal film has a thickness less than or equal to about 10 nm, the first conductive layer has a thickness less than or equal to about 45 nm, and the second conductive layer has a thickness less than or equal to about 45 nm.

[0033] In one aspect, the electromagnetic interference (EMI) shield has a shielding effectiveness greater than or equal to 30 dB, and an average transmission efficiency through the electromagnetic interference (EMI) shield in the visible wavelength range of greater than or equal to about 390 nm to less than or equal to about 740 nm is greater than or equal to about 80%.

[0034] The present disclosure also relates to a method for broadband electromagnetic shielding, the method comprising arranging an electromagnetic shielding member in a transmission path of electromagnetic radiation to block a frequency range of greater than or equal to about 800 MHz to less than or equal to about 90 GHz to achieve a shielding efficiency greater than or equal to 30 dB, and transmitting a wavelength range in a visible range of greater than or equal to about 390 nm to less than or equal to about 740 nm through the electromagnetic shielding member to achieve an average transmission efficiency greater than or equal to about 80%. The electromagnetic shielding member comprises a continuous metal film, the continuous metal film defining a first side and an opposite second side, and the continuous metal film comprises greater than or equal to about 80 atomic % of silver (Ag) and less than or equal to about 20 atomic % of copper (Cu), has a thickness less than or equal to about 10 nm, and has a sheet resistance less than or equal to about 20 Ohm / square. A first conductive layer is arranged in contact with the first side of the continuous metal film. The first conductive layer includes a conductive material selected from the group consisting of: indium tin oxide, aluminum zinc oxide (AZO), indium zinc oxide (IZO), fluorine-doped tin oxide (FTO), poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. The second conductive layer is arranged to contact the second side of the continuous metal film. The second conductive layer includes a conductive material selected from the group consisting of: indium tin oxide, aluminum zinc oxide (AZO), indium zinc oxide (IZO), fluorine-doped tin oxide (FTO), poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. The electromagnetic shield also includes a spacer layer, which includes a dielectric material adjacent to the second conductive layer, and a graphene layer adjacent to the spacer layer.

[0035] Further areas of applicability will become apparent from the description provided herein.The description and specific examples in this summary are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The drawings described herein are for illustrative purposes only of selected embodiments and not all possible implementations, and are not intended to limit the scope of the present disclosure.

[0037] Figure 1 A schematic diagram of a transparent electromagnetic interference (EMI) shielding device having a stack including an ultra-thin conductive silver alloy flanked by a first conductive transparent anti-reflective layer and a second conductive transparent anti-reflective layer according to certain aspects of the present disclosure is shown.

[0038] Figure 2 A schematic diagram of a transparent electromagnetic interference (EMI) shielding device prepared according to certain aspects of the present disclosure is shown, wherein the transparent electromagnetic interference (EMI) shielding device has a stacked component defining a resonant cavity, wherein the stacked component includes: Figure 1 The stack also includes a spacer layer and a second conductive lossy layer.

[0039] Figure 3 A schematic diagram of a transparent electromagnetic interference (EMI) shielding device prepared according to certain aspects of the present disclosure is shown, wherein the transparent electromagnetic interference (EMI) shielding device has a Figure 2 The stacked assembly of the resonant cavity in the embodiment of the present invention also includes an electrical gating system electrically connected to the ultra-thin conductive silver alloy and the second conductive layer.

[0040] Figure 4 A schematic diagram of a transparent electromagnetic interference (EMI) shielding device having dual stacks according to certain aspects of the present disclosure is shown, each stack comprising an ultra-thin conductive silver alloy flanked by a first conductive transparent anti-reflective layer and a second conductive transparent anti-reflective layer.

[0041] Figure 5 An apparatus for co-sputtering silver and a conductive metal (eg, copper) to form a continuous ultra-thin conductive silver alloy for use with certain variations of the electromagnetic interference shielding devices of the present disclosure is shown.

[0042] Figures 6A-6E FIG. 6A shows an ultra-thin silver alloy film used for various aspects of the present disclosure as a sheet resistor (R s ) as a function of ). FIG. 6B shows a schematic diagram of a stack on a PET substrate comprising two ITO layers surrounding a Cu-doped Ag layer. FIG. 6C shows the calculated average visible transmittance of an electromagnetic interference shielding device (EMAGS) film for various thicknesses of the top and bottom ITO layers with 8 nm thick Cu-doped Ag. FIG. 6D and FIG. 6E show SEM images of a stack of 8 nm Cu-doped Ag films and EMAGS films prepared according to certain aspects of the present disclosure.

[0043] Figures 7A(1)-7D. Figure 7A(1) shows an EMAGS laminate film with good transparency prepared according to certain aspects of the present disclosure. Figure 7A(2) is an EMAGS film in a folded state, showing excellent flexibility. Figure 7B shows a large-area (200cm×50cm) transparent EMAGS laminate film on PET manufactured by a roll-to-roll process according to certain aspects of the present disclosure. Figure 7C shows the transmittance of the EMAGS laminate, Cu-doped Ag (8nm), ITO (40nm) and PET substrate from 300nm to 1000nm, and Figure 7D shows the reflectance spectrum of the EMAGS laminate, Cu-doped Ag (8nm), ITO (40nm) and PET substrate from 300nm to 1000nm.

[0044] Figures 8A-8DThe measured EMI SE results for EMAGS stack, dual stack EMAGS assembly, dual stack EMAGS separated by a quarter wavelength spacer layer, Cu doped Ag (8nm), ITO (40nm), and PET film are shown. Figure 8A shows the X-band (8-12GHz) results, and Figure 8B shows the K u FIG8C shows the results for the K band (18-26.5 GHz), and FIG8D shows the results for the K band (12-18 GHz). a Band results (26.5-40GHz).

[0045] 9A-9G (4) show the measured microwave reflection (R) and absorption (A) as a function of incident frequency for an EMI shielding EMAGS laminate film prepared according to certain aspects of the present disclosure. More specifically, in the X-band (8-12 GHz) ( FIG. 9A ), K u band (12-18 GHz) (Figure 9B), K band (18-26.5 GHz) (Figure 9C), K a The microwave reflection (R) and absorption (A) of the electromagnetic interference shielding EMAGS laminate film measured in the band (26.5-40GHz) (Figure 9D). Figure 9E shows the power loss density in each layer of the ITO / Cu doped Ag / ITO structure calculated using CST Microwave Studio at 12GHz. Figure 9F shows the shielding contribution calculated from R and A for 1) Cu doped Ag, 2) ITO / Cu doped Ag and 3) ITO / Cu doped Ag / ITO structures. The power flow within the structures of Figure 9G (1) air, Figure 9G (2) ITO, Figure 9G (3) ITO / Cu doped Ag and Figure 9G (4) ITO / Cu doped Ag / ITO structures simulated at 12GHz using CST Microwave Studio.

[0046] Figures 10A-10D FIG. 10A is a graph showing the measured sheet resistance (R) of an electromagnetic interference shielding EMAGS stack and ITO (40 nm) on a PET substrate prepared according to certain aspects of the present disclosure as a function of bending cycles at a 6 mm bending radius. s ). The inset is a schematic diagram of the bending system. FIG. 10B is a graph showing the EMI SE at 12 GHz for the EMI shielding EMAGS stack and ITO film as a function of bending cycles at the same bending radius. The inset shows an SEM image of the corresponding film after 250 bends. EMI SE at 12 GHz for the EMI shielding EMAGS and ITO films as a function of bending radius for transverse magnetic (TM) waves ( FIG. 10C ) and transverse electric (TE) waves ( FIG. 10D ). The inset shows the orientation of the electric and magnetic fields of the two polarizations relative to the crack line.

[0047] Figures 11A-11B11A and 11B show cracks in an electromagnetic interference shielding laminate film (EMAGS film) (FIG. 11A) and an ITO film (thickness 40 nm) (FIG. 11B) prepared according to certain aspects of the present disclosure after 250 bending cycles at a bending radius of 3 mm. The white arrows in FIG. 11A and FIG. 11B indicate crack lines on the film.

[0048] Fig.12 A comparison of the electromagnetic interference (EMI) average shielding effectiveness (SE) and average light transmittance in the visible light range is shown for an electromagnetic interference shielding single stack design (EMAGS) and an electromagnetic interference shielding dual stack design (D-EMAGS) compared to the performance of previously reported transparent shielding materials.

[0049] Figures 13A-13E . Figure 13A shows a schematic diagram of a transparent electromagnetic interference (EMI) shielding device used as a microwave absorber (MA). Figure 13B shows a conceptual diagram illustrating multiple reflections of incident microwaves. Figures 13C(1)-13C(3) show SEM (Figure 13C(1)) and AFM (Figure 13C(2)) images of graphene grown by CVD on a silica substrate. Figure 13C(3) shows the Raman spectrum of graphene on a silica substrate (532nm laser wavelength). Figure 13D shows SEM and AFM images of ITO / Cu doped Ag / ITO on a PET substrate. Figure 13E shows photographs of centimeter-scale silica, graphene on a silica substrate, and a transparent electromagnetic interference (EMI) shielding stack formed according to certain aspects of the present disclosure, all of which show good transparency. The scale bars in the figures are all 1 μm.

[0050] Fig.14 Flowchart showing the process of graphene film synthesis and transfer.

[0051] Figures 15A-15D . FIG15A shows a schematic diagram of a computational model of a transparent electromagnetic interference (EMI) microwave absorber on a PET substrate including graphene, a transparent dielectric spacer layer, and a metal film. FIG15B shows the complex refractive index (n and k) of graphene in the microwave region and the perfect absorption point calculated using Equation 4. Microwave absorption spectra calculated from 1 GHz to 30 GHz as a function of graphene Fermi level ( FIG15C ) and transparent dielectric thickness ( FIG15D ).

[0052] Figures 16A-16F . Figures 16A-16F The electromagnetic interference shielding GDS cavity prepared according to certain aspects of the present disclosure is shown as an X-band and K-band u Figures 16A-16B show the microwave absorption spectra of silicon dioxide as a function of thickness in the band. c=0.3 eV, Γ = 20 ps). Figures 16C-16D show the CST simulation (μ c =0.3 eV, Γ=20 ps). Figures 16E-16F show the experimental results.

[0053] Figures 17A-17B FIG. 17A is a calculated electric field distribution and FIG. 17B is a calculated absorbed power distribution at a predetermined frequency within a whole transparent electromagnetic interference (EMI) stack cavity (a GDS cavity having a top graphene layer and a bottom Ag layer separated by a silicon dioxide layer).

[0054] Figures 18A-18B Figure 18A shows the optical transmission spectra of 0.5 mm and 1 mm silica layers, ITO / CU-Ag / ITO on PET substrate, and single-layer graphene. Figure 18B shows the optical transmission spectra of transparent electromagnetic interference (EMI) GDS resonant cavities with different silica thicknesses formed according to certain aspects of the present disclosure.

[0055] Corresponding reference numerals indicate corresponding parts throughout the several views of the drawings. DETAILED DESCRIPTION

[0056] Exemplary embodiments are provided so that the present disclosure will be thorough, and the scope of the present disclosure will be fully conveyed to those skilled in the art. Many specific details (such as embodiments of specific compositions, parts, equipment and methods) are set forth to provide a thorough understanding of the embodiments of the present disclosure. It will be apparent to those skilled in the art that there is no need for the specific details to be adopted, the exemplary embodiments can be implemented in many different forms, and the specific details and exemplary embodiments should not be construed as limiting the scope of the present disclosure. In some exemplary embodiments, known processes, known equipment structures and known technologies are not described in detail.

[0057] The terms used herein are only used for the purpose of describing specific exemplary embodiments and are not intended to be limiting. As used herein, the singular forms "a", "an", and "the" may also be intended to include plural forms unless the context clearly indicates otherwise. The terms "comprises", "comprising", "including", and "having" are inclusive and therefore specifically refer to the presence of the features, elements, compositions, steps, integers, operations, and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts, and / or combinations thereof. Although the open term "comprising" should be understood as a non-limiting term for describing and claiming the various embodiments set forth herein, in some aspects, the term may alternatively be understood as a more restrictive and constraining term, such as "consisting of" or "consisting essentially of". Thus, for any given embodiment describing compositions, materials, parts, elements, features, integers, operations, and / or process steps, the present disclosure also specifically includes embodiments consisting of or consisting essentially of these described compositions, materials, parts, elements, features, integers, operations, and / or process steps. In the case of "consisting of," alternative embodiments do not include any additional compositions, materials, parts, elements, features, integers, operations, and / or process steps, while in the case of "consisting essentially of," any additional compositions, materials, parts, elements, features, integers, operations, and / or process steps that materially affect the basic and novel characteristics are not included in such embodiments, but any compositions, materials, parts, elements, features, integers, operations, and / or process steps that do not materially affect the basic and novel characteristics may be included in such embodiments.

[0058] Any method steps, processes, and operations described herein should not be construed as necessarily being performed in the particular order discussed or illustrated, unless an order of performance is expressly specified. It should also be understood that additional or alternative steps may be employed unless otherwise specified.

[0059] When a component, element or layer is referred to as being "on another component or layer", "engaged to another component or layer", "connected to another component or layer" or "coupled to another component or layer", the component, element or layer may be directly on, engaged to, connected to or coupled to another component, element or layer, or there may be intermediate elements or layers. Conversely, when an element is referred to as being "directly on another component or layer", "directly engaged to another component or layer", "directly connected to another component or layer" or "directly coupled to another component or layer", there may be no intermediate elements or layers. Other words used to describe the relationship between elements should be interpreted in a similar manner (e.g., "between" versus "directly between", "adjacent" versus "directly adjacent", etc.). As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.

[0060] Although the term first, second, third etc. can be used to describe various steps, elements, components, regions, layers and / or sections in this article, unless otherwise specified, these steps, elements, components, regions, layers and / or sections should not be limited by these terms. These terms can only be used to distinguish a step, element, component, region, layer and / or section from another step, element, component, region, layer and / or section. When used in this article, unless the context clearly indicates, terms such as "first", "second" and other digital representations do not imply order or sequence. Therefore, without departing from the teaching of exemplary embodiments, the first step, the first element, the first component, the first area, the first layer or the first section discussed below can be referred to as the second step, the second element, the second component, the second area, the second layer or the second section.

[0061] For ease of description, spatial or temporal relative terms (e.g., "before," "after," "inside," "outside," "below," "lower," "above," and "upper," etc.) may be used herein to describe the relationship of one element or feature to another element or feature illustrated in the drawings. Spatial or temporal relative terms may be intended to encompass different orientations of a device or system in use or operation in addition to the orientation shown in the drawings.

[0062] Throughout this disclosure, numerical values ​​represent approximate measures or limits of ranges to encompass minor deviations from given values ​​and embodiments having approximately the values ​​mentioned as well as those having exactly the values ​​mentioned. Except in the working examples provided at the end of the detailed description, all numerical values ​​(e.g., quantities or conditions) of parameters in this specification (including the appended claims) should be understood in all cases as modified by the term "about", regardless of whether "about" actually appears before the numerical value. "About" means that the numerical value allows some slight imprecision (close to exact in value; approximately or reasonably close to the value; almost). If the imprecision provided by "about" is not understood in the art to have this ordinary meaning, then "about" as used herein means at least the variation that can be produced by the ordinary methods of measuring and using such parameters. For example, "about" may include the following variations: less than or equal to 5%, optionally less than or equal to 4%, optionally less than or equal to 3%, optionally less than or equal to 2%, optionally less than or equal to 1%, optionally less than or equal to 0.5%, and optionally less than or equal to 0.1% in some aspects.

[0063] Furthermore, disclosure of ranges includes disclosure of all values ​​within the entire range and further divided ranges, including endpoints and sub-ranges given for the ranges.

[0064] As used herein, the terms "composition" and "material" are used interchangeably to refer generally to a substance that includes at least a preferred chemical compound, but which may also include additional substances or compounds, including impurities.

[0065] The disclosures of all patents, patent applications, articles, and references referenced or cited in this disclosure are hereby incorporated by reference.

[0066] Example embodiments will now be described more fully with reference to the accompanying drawings.

[0067] In various aspects, the present disclosure provides a method for broadband electromagnetic interference (EMI) shielding. The method may include setting an electromagnetic shield according to various aspects of the present disclosure in a transmission path of electromagnetic radiation. In some aspects, the method provides broadband blocking or attenuation of electromagnetic radiation in the microwave range. For example, the method can block electromagnetic radiation having a frequency greater than or equal to about 600 MHz to less than or equal to about 90 GHz. For example, the method can block electromagnetic radiation in the microwave range (e.g., having a frequency greater than or equal to about 8 GHz to less than or equal to about 40 GHz). Electromagnetic radiation with such a frequency may have a first wavelength range of greater than or equal to about 7.5 mm (40 GHz) to less than or equal to about 3.75 cm (8 GHz). Such electromagnetic radiation includes frequencies in the radio frequency band of the microwave range, including the entire X-band (frequencies of about 7 GHz to about 12 GHz) specified by IEEE, K-band (frequencies of about 7 GHz to about 12 GHz), and the like. uBand (frequency from about 12 GHz to about 18 GHz), K a Band (frequency from about 26.5 GHz to about 40 GHz) and K-band (frequency from about 18 GHz to about 27 GHz). As will be further described below, an electromagnetic shield prepared according to certain aspects of the present disclosure blocks or attenuates electromagnetic radiation having such a frequency / first wavelength range to achieve an average shielding efficiency or shielding effectiveness (SE) greater than or equal to 20 dB. The shielding effectiveness of a material is defined as the logarithmic ratio of incident power to transmitted power and is typically expressed in decibels.

[0068] In addition, the passband of the electromagnetic interference shield corresponds to a second wavelength range in the visible light range, and the second wavelength range is simultaneously transmitted through the electromagnetic shield, while the first wavelength range is blocked or attenuated. Typically, visible light has a wavelength range of greater than or equal to about 390nm to less than or equal to about 740nm. As will be understood by those skilled in the art, the amount of electromagnetic radiation blocked in the microwave range is inversely proportional to the transparency of the material in the visible light range. Therefore, in the case of high transmittance of visible light, the amount of electromagnetic radiation blocked in the microwave range will be relatively small. Conversely, in the case of relatively high blocking of microwave radiation, the visible light transmission level will be relatively low. In certain variations, as will be further described below, when the average shielding efficiency of microwave radiation from greater than or equal to about 600MHz to less than or equal to about 90GHz is greater than or equal to 20dB, the average transmission efficiency of visible light having a second wavelength range through the electromagnetic shield can be greater than or equal to about 65%. In certain other variations, when the average shielding efficiency for microwave radiation from about 600 MHz or more to about 90 GHz or less is greater than or equal to 20 dB, the average transmission efficiency of visible light having a second wavelength range through the electromagnetic shield may be greater than or equal to about 70%, optionally greater than or equal to about 75%, optionally greater than or equal to about 80%, and in certain aspects, when the average shielding efficiency for microwave radiation from about 600 MHz or more to about 90 GHz or less is greater than or equal to 20 dB, optionally greater than or equal to about 85%. In certain variations, the average shielding efficiency for microwave radiation is greater than or equal to 30 dB, and the average visible transmission efficiency for visible light is greater than or equal to about 80%, optionally, the average shielding efficiency is greater than or equal to 50 dB, and the average visible transmission efficiency is greater than or equal to about 65%. In one variation, as further described below, when the average shielding efficiency of microwave radiation from about 600 MHz or more to about 90 GHz or less is greater than or equal to 20 dB, the average transmission efficiency of visible light having a second wavelength range through the electromagnetic shield may be greater than or equal to about 85%. In another variation, as further described below, when the average shielding efficiency of microwave radiation from about 8 GHz or more to about 40 GHz or less is greater than or equal to 26 dB, the average transmission efficiency of visible light having a second wavelength range through the electromagnetic shield may be greater than or equal to about 85%.

[0069] In various aspects, the electromagnetic shield is a laminate 20, such as Figure 1The stack 20 shown. The stack 20 includes a substrate 30. The stack 20 includes an ultra-thin metal layer 40 defining a first side 42 and a second side 44 opposite the first side. A first layer 50 is disposed on the first side 42 of the ultra-thin metal layer 40. The first layer can be formed by a conductive layer transparent to a desired wavelength range of electromagnetic radiation (e.g., visible light). The first layer 50 can be in direct contact with the first side 42 of the ultra-thin metal layer 40. The second layer 52 is disposed on the second side 44 of the ultra-thin metal layer 40. The second layer 52 can be formed by a conductive layer transparent to a desired wavelength range of electromagnetic radiation (e.g., visible light). The second layer 52 can also be in direct contact with the second side 44 of the ultra-thin metal layer 40. In some variations, the first layer 50 has a thickness of less than or equal to about 45 nm, and the second layer 52 has a thickness of less than or equal to about 45 nm. The thickness of the first layer 50 can be greater than or equal to about 3 nm to less than or equal to about 45 nm, optionally greater than or equal to about 35 nm to less than or equal to about 45 nm, and in some variations, the thickness of the first layer 50 can be about 40 nm. Similarly, the thickness of the second layer 52 can be greater than or equal to about 3 nm to less than or equal to about 45 nm, optionally greater than or equal to about 35 nm to less than or equal to about 45 nm, and in some variations, the thickness of the second layer 52 can be about 40 nm.

[0070] In certain aspects, the stacks provided by the present disclosure are flexible and thus capable of significant elongation, flexing, bending, or other deformation along one or more axes. The term "flexible" can refer to the ability of a material, structure, or component to deform (e.g., deform into a curved shape) without undergoing a permanent change that introduces significant strain (e.g., strain that indicates a point of failure of the material, structure, or component). Notably, it was surprisingly found that despite the inclusion of one or more layers of potentially brittle materials (e.g., indium tin oxide) as the first layer 50 and the second layer 52 in a shielding device prepared according to certain aspects of the present technology, the stack having multiple materials still unexpectedly exhibits flexibility.

[0071] Those skilled in the art may select any known substrate 30 having high transmittance to visible light. Suitable examples of substrates include glass-based substrates or polymer substrates. In some aspects, the substrate may be flexible. For example, suitable polymer substrates may optionally include polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate, or poly(ethylene 2,6-naphthalate) (PEN); polycarbonates; polyacrylates and polymethacrylates, including polymethyl methacrylate (PMMA), polymethacrylate, polyethyl acrylate; and siloxanes such as polydimethylsiloxane (PDMS), etc. In other variations, as non-limiting examples, the substrate may include silicon dioxide, silicon, etc.

[0072] The ultra-thin metal layer 40 is a continuous film containing silver (Ag). Silver (Ag) is widely used due to its excellent electrical conductivity and low optical loss in the visible band; however, continuous thin silver films are difficult to achieve and mostly form discontinuous films during or after deposition. The continuous metal film may also contain another conductive metal (e.g., copper (Cu)) that helps to form a continuous and smooth silver alloy layer. The ultra-thin metal layer 40 is desirably smooth and continuous, exhibits low optical loss and low resistance with high temperature stability. Such films can be easily manufactured without applying any seed layer or requiring specific limited manufacturing conditions.

[0073] In certain aspects, the ultra-thin metal layer 40 according to certain aspects of the present disclosure provides a conductive film comprising greater than or equal to about 80 atomic % of silver (Ag) of the total film composition. The film composition also includes a conductive metal different from silver (Ag). In certain variations, the different conductive metals may include copper (Cu). In alternative variations, the conductive metal may be selected from the group consisting of aluminum (Al), gold (Au), platinum (Pt), palladium (Pd), titanium (Ti), nickel (Ni), chromium (Cr), gold (Au), magnesium (Mg), tantalum (Ta), germanium (Ge), or a combination thereof.

[0074] In certain variations, the conductive ultra-thin metal layer 40 may include greater than or equal to about 80 atomic % silver, and the conductive metal (e.g., copper) may be present at greater than 0 atomic % to less than or equal to about 20 atomic % of the total film composition, based on the total composition of the ultra-thin metal layer 40. In certain variations, the silver may be present at greater than or equal to about 90 atomic % of the total film composition, and the conductive metal (e.g., copper) may be present at greater than or equal to 0 atomic % to less than or equal to about 10 atomic % of the total film composition.

[0075] In certain variations, the conductive metal (e.g., copper) is optionally present at greater than or equal to about 1 atomic % to less than or equal to about 20 atomic % of the total film composition, and is optionally present at greater than or equal to about 1 atomic % to less than or equal to about 10 atomic %. Silver may be present at greater than or equal to about 80 atomic % to less than or equal to about 99 atomic % of the total film composition. In certain variations, the conductive metal (e.g., copper) is optionally present at greater than or equal to about 1 atomic % to less than or equal to about 15 atomic % of the total film composition, and silver may be present at greater than or equal to about 85 atomic % to less than or equal to about 99 atomic % of the total film composition. In certain variations, the conductive metal (e.g., copper) is optionally present at greater than or equal to about 2 atomic % to less than or equal to about 10 atomic % of the total film composition, and silver may be present at greater than or equal to about 90 atomic % to less than or equal to about 98 atomic % of the total film composition. Such an ultra-thin metal layer 40 can be prepared by techniques such as those described in U.S. Patent Publication No. 2017 / 0200526 to Guo et al., entitled “Ultra-thin Doped Noble Metal Films for Optoelectronics and Photonics Applications,” the relevant portions of which are incorporated herein by reference.

[0076] As discussed in U.S. Patent Publication No. 2017 / 0200526, small amounts of conductive metals (e.g., aluminum) render doped Ag films smooth and with sub-nanometer RMS roughness. Where U.S. Patent Publication No. 2017 / 0200526 describes the use of aluminum or other conductive metals, copper doping of silver appears to similarly provide a smooth surface with reduced roughness. The ultra-smooth surface morphology of the doped Ag films is very stable at both room and elevated temperatures. However, the inclusion of large amounts of conductive metals (e.g., copper) in excess of 20 atomic % may adversely reduce the optical loss, conductivity, and / or transparency of the silver-based films. Copper-doped silver films prepared according to certain aspects of the present disclosure provide ultra-thin layers of high conductivity, even when compared to other doped silver films (e.g., aluminum-doped films).

[0077] In some aspects, an "ultra-thin" layer or film may have a thickness of less than or equal to about 25 nm. In some variations, the thickness of the ultra-thin metal layer is greater than or equal to about 2 nm and less than or equal to about 20 nm; optionally greater than or equal to about 3 nm to less than or equal to about 20 nm, optionally greater than or equal to about 3 nm to less than or equal to about 15 nm, optionally greater than or equal to about 3 nm to less than or equal to about 10 nm, and optionally greater than or equal to about 5 nm to less than or equal to about 10 nm.

[0078] In addition, in various aspects, the film comprising Ag and a conductive metal (e.g., copper) has a smooth surface. A "smooth" surface refers to a surface roughness (e.g., from peak to valley) measured with a root mean square (RMS) of less than or equal to about 25% of the total film thickness, optionally less than or equal to about 20% of the total film thickness, optionally less than or equal to about 15% of the total film thickness, optionally less than or equal to about 14% of the total film thickness, optionally less than or equal to about 13% of the total film thickness, optionally less than or equal to about 12% of the total film thickness, optionally less than or equal to about 11% of the total film thickness, optionally less than or equal to about 10% of the total film thickness, optionally less than or equal to about 9% of the total film thickness, optionally less than or equal to about 8% of the total film thickness, optionally less than or equal to about 7% of the total film thickness, optionally less than or equal to about 6% of the total film thickness, and in certain variations, optionally less than or equal to about 5% of the total film thickness.

[0079] As will be appreciated by those skilled in the art, determining the smoothness of a film is relative and depends on the overall thickness of the film, and if the film is thicker, it can still be considered smooth with a greater amount of root mean square (RMS) surface roughness. In certain variations, a smooth surface of a film comprising silver and a conductive metal (e.g., copper) has a surface roughness of less than or equal to about 1 nm root mean square (RMS) with an overall thickness of at least about 10 nm of the film. In other variations, a smooth surface has a surface roughness of less than or equal to about 0.5 nm root mean square (RMS) with an overall thickness of at least about 10 nm of the film.

[0080] The sheet resistance (R s ) may be less than or equal to about 25Ohm / square, optionally less than or equal to about 20Ohm / square, optionally less than or equal to about 15Ohm / square, optionally less than or equal to about 13Ohm / square, optionally less than or equal to about 10Ohm / square, optionally less than or equal to about 5Ohm / square, optionally less than or equal to about 4Ohm / square, optionally less than or equal to about 3Ohm / square, optionally less than or equal to about 2Ohm / square, and optionally less than or equal to about 1Ohm / square.

[0081] As described above, the conductive ultra-thin metal layer of the present disclosure is capable of transmitting a selected portion of the electromagnetic spectrum (e.g., visible light) and is therefore considered transparent or translucent. Transparency can generally encompass translucency and can generally be understood to mean that greater than or equal to about 50% of the light / energy of a predetermined target wavelength or wavelength range (which can be polarized or unpolarized) passes through the conductive ultra-thin metal layer. In some variations, greater than or equal to about 60% of the target wavelength range passes through the film, optionally greater than or equal to about 65%, optionally greater than or equal to about 70%, optionally greater than or equal to about 75%, optionally greater than or equal to about 80%, optionally greater than or equal to about 85%, optionally greater than or equal to about 90%, optionally greater than or equal to about 95%, and in some variations, optionally greater than or equal to about 97% of the target wavelength range passes through the conductive ultra-thin metal layer. For certain applications, such as displays on mobile phones and mobile devices, advanced optical components in vehicle windshields and aerospace instruments, optical transmittance levels of more than 80% or even more than 90% are generally required.

[0082] In some aspects, the conductive ultra-thin metal layer can reflect certain selected portions of the electromagnetic spectrum and is therefore reflective or semi-reflective. Reflectivity can generally encompass semi-reflectivity and can generally be understood to mean that greater than or equal to about 50% of the light / energy of a predetermined target wavelength or wavelength range (which can be polarized or unpolarized) is reflected from the surface and therefore does not pass through the conductive ultra-thin metal layer. In some variations, greater than or equal to about 60% of the target wavelength (or wavelength range) reflected from the ultra-thin metal layer, optionally greater than or equal to about 70% of the target wavelength, optionally greater than or equal to about 75% of the target wavelength, optionally greater than or equal to about 80% of the target wavelength, optionally greater than or equal to about 85% of the target wavelength, optionally greater than or equal to about 90% of the target wavelength, optionally greater than or equal to about 95% of the target wavelength, and in some variations, optionally greater than or equal to about 97% of the target wavelength is reflected by the conductive ultra-thin metal layer of the present disclosure.

[0083] In certain variations, the conductive ultra-thin metal layer is transparent to electromagnetic waves in the visible light range and reflective to electromagnetic waves in the microwave radiation range. Transparent means that the conductive ultra-thin metal layer is transmissive to a target wavelength range of electromagnetic energy (e.g., in the visible wavelength range). Reflective means that the conductive ultra-thin metal layer reflects a significant portion of a predetermined wavelength range of electromagnetic energy (e.g., in the microwave range).

[0084] The conductive ultra-thin metal layer comprising silver and a conductive metal such as copper can be flexible (e.g., able to bend without mechanical breakage). As described above, the flexible material can be bent, flexed, or deformed along one or more axes without experiencing permanent changes that introduce significant strain (e.g., strain that indicates a failure point of the material, structure, or component). Further, after greater than or equal to about 100 bending cycles, optionally after greater than or equal to about 250 bending cycles, optionally after greater than or equal to about 500 bending cycles, optionally after greater than or equal to about 1,000 bending cycles, optionally after greater than or equal to about 2,500 bending cycles, optionally after greater than or equal to about 5,000 bending cycles, and in certain variations optionally after greater than or equal to about 10,000 bending cycles, the electromagnetic interference (EMI) shield of the present disclosure can exhibit a sheet resistance (R) of less than or equal to 20 Ohm / square. s In certain variations, the sheet resistance (R) is 0.0407 W after about 100 or more bending cycles, optionally about 250 or more bending cycles, optionally about 500 or more bending cycles, optionally about 1,000 or more bending cycles, optionally about 2,500 or more bending cycles, optionally about 5,000 or more bending cycles, and in certain variations, optionally about 10,000 or more bending cycles. s ) is less than or equal to 15 Ohm / square. In other variations, after greater than or equal to about 100 flex cycles of the electromagnetic interference (EMI) shield, optionally after greater than or equal to about 250 flex cycles, optionally after greater than or equal to about 500 flex cycles, optionally after greater than or equal to about 1,000 flex cycles, optionally after greater than or equal to about 2,500 flex cycles, optionally after greater than or equal to about 5,000 flex cycles, and in some variations optionally after greater than or equal to about 10,000 flex cycles, the sheet resistance (R s ) is less than or equal to 10Ohm / square.

[0085] In various aspects, the present disclosure provides a method for broadband electromagnetic interference (EMI) shielding. The method may include providing an electromagnetic shield in the transmission path of a beam of electromagnetic radiation. In this way, the electromagnetic shield blocks a frequency range of greater than or equal to about 8 GHz to less than or equal to about 40 GHz to achieve a shielding efficiency greater than or equal to 26 dB. Further, the electromagnetic shield transmits a second wavelength range in the visible range of greater than or equal to about 390 nm to less than or equal to about 740 nm to achieve an average transmission efficiency of greater than or equal to about 85% through the electromagnetic shield.

[0086] As described above, the electromagnetic shield can be a flexible stack comprising a plurality of layers. In some variations, the electromagnetic shield comprises a continuous conductive metal film or layer defining a first side and a second opposite side, and the continuous conductive metal film or layer comprises greater than or equal to about 80 atomic % of silver (Ag) and less than or equal to about 20 atomic % of copper (Cu). In some variations, the continuous metal film is an ultra-thin metal layer having any thickness specified above (e.g., less than or equal to about 10 nm). In some other variations, the continuous ultra-thin metal layer has a thickness less than or equal to about 8 nm. The continuous ultra-thin metal layer is also conductive and may have a sheet resistance less than or equal to about 20 Ohm / square or any value specified above.

[0087] By using an ultra-thin metal layer in a stack with an adjacent conductive dielectric anti-reflective material layer, light transmittance can be increased without increasing the thickness of the metal layer. Similarly, the stack can include a first layer 50 disposed on the first side 42 of the continuous ultra-thin metal film. The first layer 50 can be formed of a material that is transparent to the desired wavelength range of electromagnetic radiation (e.g., visible light). Such a first layer 50 can serve as an optical anti-reflective layer. Further, the first layer 50 can be formed of a material that is conductive and can be a dielectric material. In some aspects, the first layer 50 includes a transparent conductive oxide, such as a material selected from the group consisting of: indium tin oxide (ITO); doped zinc oxide, such as aluminum zinc oxide (AZO), indium zinc oxide (IZO); doped tin oxide, such as fluorine-doped tin oxide (FTO); and mixtures thereof. In other aspects, the first layer 50 includes a conductive dielectric polymer material, such as poly (3,4-ethylenedioxythiophene) (PEDOT) that can be combined with polystyrene sulfonate. In a selected variation, the first layer 50 includes a conductive material selected from the group consisting of: indium tin oxide, aluminum zinc oxide (AZO), indium zinc oxide (IZO), fluorine doped tin oxide (FTO), poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. In a further selected variation, the first layer 50 includes indium tin oxide (ITO). With respect to indium doped tin oxide, ITO provides high conductivity with a particularly desirable refractive index for copper doped Ag films in a desired optical range compared to other conductive dielectric materials (e.g., aluminum doped zinc oxide, indium doped zinc oxide, and poly (3,4-ethylenedioxythiophene): polystyrene sulfonate).

[0088] Further, the second layer 52 is disposed on the second side 44 of the continuous ultra-thin metal layer 40. The second layer 52 can be formed of the same material suitable for use in the first layer 50, for example, the second layer 52 can be formed of a material that is a dielectric material that is transparent to the desired wavelength range of electromagnetic radiation (e.g., visible light), which can also serve as an optical anti-reflection layer, which can also be conductive. The first layer 50 and the second layer 52 can have the same composition as each other or different compositions from each other. The second layer 52 optionally includes a transparent conductive oxide, for example, a material selected from the group consisting of: indium tin oxide (ITO); doped zinc oxide, such as aluminum zinc oxide (AZO), indium zinc oxide (IZO); doped tin oxide, such as fluorine doped tin oxide (FTO); and mixtures thereof. In other aspects, the second layer 52 includes a conductive dielectric polymer material, such as poly (3,4-ethylenedioxythiophene) (PEDOT) that can be combined with polystyrene sulfonate. In a selected variation, the second layer 52 includes a conductive material selected from the group consisting of: indium tin oxide, aluminum zinc oxide (AZO), indium zinc oxide (IZO), fluorine-doped tin oxide (FTO), poly (3,4-ethylenedioxythiophene) (PEDOT), and mixtures thereof. In a further selected variation, the second layer 52 includes indium tin oxide (ITO).

[0089] In certain variations, the flexible stack further includes at least one second conductive lossy graphene layer such that the EMI shielding device is based on an asymmetric Fabry-Perot resonant cavity. A Fabry-Perot resonant cavity or etalon is an interference filter whose operation is generally described in U.S. Pat. No. 9,261,753 to Guo et al., entitled “Spectrum Filtering for Visual Displays and Imaging Having Minimal Angle Dependence,” relevant portions of which are incorporated herein by reference.

[0090] Figure 2 The general operating principle of a Fabry-Perot filter-based electromagnetic interference shield 100 prepared according to certain aspects of the present disclosure is shown. A source of electromagnetic radiation is directed toward the shield 100 such that the shield is placed in the transmission path of the electromagnetic radiation. More specifically, an electromagnetic wave 110 having a visible light component (having a wavelength within a first range corresponding to the visible light range) and a second component (having a wavelength / frequency corresponding to the microwave range) approaches the shield 100.

[0091] The shield 100 includes components of a laminate assembly 120 having a plurality of layers. Figure 2 As can be seen in FIG. 1 , the stack assembly 120 includes a Figure 1 Components of the stack 20 shown in . To the extent that components are shared between the stack assembly 120 and the stack 20, for the sake of brevity, the discussion of these components and their characteristics will not be repeated herein. Adjacent to the second layer 52 is a spacer layer 122, which may include a dielectric material, such as fused silica or an insulating polymer layer. In some aspects, the dielectric material has a relatively high refractive index, which is preferably greater than about 1.5, optionally greater than or equal to 2, optionally greater than or equal to about 3, and in some variations greater than or equal to about 4. In some aspects, the spacer layer 122 can be a quarter wavelength (λ / 4) thickness of the peak wavelength of the second range to be reflected or absorbed (e.g., ranging from mm to cm). The spacer can be an inorganic dielectric, an organic dielectric, or a composite material made of both. In some variations, suitable transparent organic materials may optionally include, for example: polyethylene terephthalate (PET); polyethylene naphthalate or poly (ethylene 2,6-naphthalate) (PEN); polycarbonate; polyacrylates and polymethyl acrylates, including polymethyl methacrylate (PMMA), polymethyl acrylate, polyethyl acrylate; and siloxanes, such as polydimethylsiloxane (PDMS), etc. The transparent organic material may be lossless or have a certain amount of absorption in the microwave range. For example, the peak absorption frequency of the stack assembly 120 operating as a resonant cavity can be adjusted by changing the thickness of the dielectric spacer. In some aspects, the thickness of the spacer or spacer layer 122 may be greater than or equal to about 1 mm to less than or equal to about 10 mm.

[0092] The stacked assembly 120 also includes a conductive lossy layer 124, which includes a material such as graphene. Graphene includes carbon atoms having a honeycomb lattice organization. In some variations, the conductive lossy layer 124 can be a single layer of graphene, which can have a thickness of about 0.35nm, or the conductive lossy layer 124 can be a double layer of graphene, or a graphene having multiple layers. The overall conductivity of the conductive lossy layer 124 can increase with the increase in the number of layers, which improves microwave shielding, but there will be some compromise in terms of visible range transmission. It should be noted that the electromagnetic interference (EMI) shielding assembly with a resonant cavity according to some variations of the present disclosure is different from a traditional Fabry-Perot cavity. Traditional Fabry-Perot resonators exhibit high frequency selectivity characteristics (high Q) in their reflection or transmission spectra, and in this case, the transmission process does not involve any energy conversion or absorption. In contrast, certain variations of electromagnetic interference (EMI) shielding devices that incorporate lossy graphene layers in Fabry-Perot cavities provide substantial power absorption.

[0093] Graphene may include at least one dopant known in the art. The presence of one or more dopants may be used to modulate the peak resonance of the resonant cavity. For example, typical chemicals used for graphene doping may be n-type dopants or p-type dopants. Non-limiting examples of n-type graphene dopants include ethanol and / or ammonia, while p-type dopants may be NO2 gas.

[0094] Although not shown, the stack assembly may include multiple conductive lossy layers including materials such as graphene in addition to the conductive lossy layer 124. These additional lossy layers may be strategically located away from the stack 20 to extend broadband absorption of energy over a wider range of wavelengths. For example, a first conductive lossy layer may be spaced apart from the stack 20 by a first spacer layer having a thickness corresponding to a first distance of one quarter wavelength of a first target wavelength of energy, while a second conductive lossy layer may be spaced apart from the stack 20 by a second distance of one quarter wavelength of a second target wavelength of energy. Multiple conductive lossy layers may be incorporated into the stack assembly 120 to target multiple target wavelengths, thereby enhancing and broadening the range of energy absorption.

[0095] In this manner, the stack assembly 120 defines an asymmetric resonant cavity, wherein the ultra-thin metal layer 40 is flanked by the first layer 50 and the second layer 52, and the second conductive layer 124 creates a reflective surface parallel to the second component (having a wavelength / frequency corresponding to the microwave range). Such a shield 100 has an asymmetric structure, wherein the reflective second conductive layer 124 that interfaces with the air 132 has a much higher transmittance than the reflective bottom stack including the ultra-thin metal layer 40, the first layer 50 and the second layer 52. Notably, the ultra-thin metal layer 40 acts as a reflector within the shield 100.

[0096] A portion of the electromagnetic energy corresponding to the first component enters the stack assembly 120 and resonates between a pair of parallel reflective surfaces (e.g., Fabry-Perot based etalon interference filters). The first component / portion of the electromagnetic energy (e.g., visible light) is transmitted through the second conductive layer 124 and then through the stack 20 to produce a filtered output 130 having a predetermined wavelength range that exits the stack assembly 120. The second component / portion of the electromagnetic energy is reflected at various points within the stack assembly 120 such that it is reflected at the second conductive layer 124, at the second layer 52, or at the first layer 50 to produce a reflected output 134 having a predetermined wavelength range. In certain aspects, the second conductive layer 124 formed of graphene can absorb the reflected output 134. Likewise, in the presence of the graphene layer, blocking by the shield 100 can include absorbing the second wavelength range within the resonant cavity such that the reflectivity of the electromagnetic shield is less than or equal to about 5%, optionally less than or equal to about 1%, and in certain variations optionally less than or equal to about 0.1%.

[0097] In an embodiment of the electromagnetic shield 100, Figure 1 Compared to the embodiments shown in , for example, in the frequency range of 600 MHz to less than or equal to about 90 GHz, or alternatively in the frequency range of greater than or equal to about 8 GHz to less than or equal to about 40 GHz, the absorption of the second component of electromagnetic radiation is enhanced. In some variations, the average shielding efficiency of the second component (e.g., microwave radiation) is greater than or equal to 30 dB, while the average transmission efficiency of the first component of electromagnetic radiation (e.g., visible light) is greater than or equal to about 80%. In another variation, the average shielding efficiency of the second component (e.g., microwave radiation) is greater than or equal to 50 dB, while the average transmission efficiency of the first component (e.g., visible light) is greater than or equal to about 65%. In contrast, most commercial products demonstrate shielding performance at relatively low frequencies (typically below 3 GHz) that is much narrower and lower than the broadband shielding effectiveness provided by electromagnetic interference shields prepared according to various aspects of the present technology.

[0098] In certain other variations, electrical gating may be used to shift the wavelength of the peak resonance within a modified Fabry-Perot cavity, as desired. Figure 3 , one such example of an EMI shield 100' is shown. The EMI shield 100' is similar to Figure 2 EMI shield 100 in the present invention, and therefore, to the extent that they are not discussed again, the components or their functions are similar to those in Figure 2 The stack assembly 120' includes a spacer layer 122, which may include a dielectric material, such as fused silica as described above. The stack assembly 120' also includes a second conductive layer 124', which includes a material such as graphene. The stack 20 includes a conductive ultra-thin metal layer 40 flanked by a first layer 50 and a second layer 52.

[0099] The peak absorption frequency of the stacked assembly 120' operating as a resonant cavity can be adjusted by gating the second conductive layer 124' to the conductive ultra-thin metal layer 40 via the electrical gating system 150. Therefore, the first conductive terminal 160 is electrically connected to the second conductive layer 124'. The second conductive terminal 162 is electrically connected to the conductive ultra-thin metal layer 40. The first conductive terminal 160 and the second conductive terminal 162 are connected to each other and to the voltage source 164. Each first conductive terminal 160 and the second conductive terminal 162 can be formed of a conductive material known in the art (e.g., copper, aluminum, silver, gold, etc.). In this way, a voltage can be applied and changed in the electrical gating system to change the properties of the graphene in the second conductive layer 124', thereby modulating and changing the wavelength of the reflected and / or absorbed electromagnetic radiation. Gating refers to field effect modulation of the conductivity of materials such as graphene by applying an external electric field. So by applying different bias voltages between 160 and 162, the charge density and conductivity of the graphene layer can be adjusted. Therefore, the corresponding dielectric constant of graphene can be adjusted, resulting in a change in the microwave absorption of the graphene layer. As the internal loss in the cavity changes, the associated absorption peak position and intensity will move accordingly.

[0100] In certain variations, the EMI shield acts as a microwave absorber that can exhibit high transparency (greater than about 65% average transmittance) in the visible range and u The shielding device is based on the following: Figure 2 The asymmetric modified Fabry-Perot cavity shown, the shielding device incorporates a single layer of graphene and an ultrathin (e.g., 8nm thick) copper-doped silver layer as an absorber and reflector, and a fused silica intermediate dielectric layer. In one aspect, the peak absorption frequency of the resonant cavity can be adjusted by changing the thickness of the dielectric spacer layer. Using electrical gating, the microwave absorption range of the assembly 100' can be further adjusted even when the dielectric layer thickness is fixed. Therefore, the present disclosure contemplates a viable solution for a new type of microwave absorber with high visible transmittance, which has a wide range of applicability, including for use in various optical devices.

[0101] The ultra-thin metal layer having a thickness of about 8 nm includes a continuously doped silver (Ag) film formed by introducing a small amount of copper in a co-sputtering deposition process with Ag, as more fully described in U.S. Patent Publication No. 2017 / 0200526.

[0102] In such a process, for example, Figure 5In the magnetron sputtering device 170 shown, precursor material targets (e.g., a first metal target 172 (e.g., an Ag target) and a second metal target 174 (e.g., a Cu target)) are respectively sputtered in a vacuum chamber 180 by gas ions (e.g., argon ions, Ar) from a first sputtering gun 176 and a second sputtering gun 178. + ) bombardment. The first sputtering gun 176 and the second sputtering gun 178 are connected to a power source 184, such as a DC power source, via a conduit 182. Ions remove (sputter) material from the first metal target 172 and the second metal target 174 to form a first material stream 186 and a second material stream 188 in the high vacuum chamber 180. The sputtered first material stream 186 and the second material stream 188 are focused and condensed onto a receiving substrate 192 using a magnetron 190 to form an alloy film or coating 194. Figure 5 As shown, the substrate 192 is rotatable to provide uniform coverage of the first metal (e.g., Ag) and the second metal (e.g., Cu) during co-deposition. Further, as shown, the first sputtering gun 176 bombarding the first metal target 172 can have a fixed amount of power or a stable amount of power so that the flow rate of sputtering remains relatively constant, while the second sputtering gun 178 can have a variable power to adjust the sputtering rate of the second metal from the second metal target 174 during the process to allow adjustment of the amount of the second metal present in the deposited film or coating 194. Therefore, in one example, the first sputtering gun 176 can have a fixed power level of 300W, while the second sputtering gun 178 has a variable power. The vacuum chamber 180 also has an observation window 196 and a meter 198 for monitoring the deposition process. It should be noted that dielectric and thin doped metal layers can be sequentially deposited on a flexible plastic web in a continuous manner in a roll-to-roll sputtering tool, thereby providing high throughput for mass production.

[0103] In alternative processes such as CVD or thermal CVD processes, the precursors react within a predetermined temperature range and are directed toward the substrate. CVD deposition can also be plasma assisted. The deposited silver-based thin film can have any of the above-described compositions or characteristics. In certain aspects, the methods of the present disclosure involve the co-deposition of a small amount of Cu or other conductive metals during Ag deposition to form a film. These methods achieve a simple process that is highly scalable to industrial and commercial manufacturing.

[0104] In other variations, the method may also include annealing the deposited film after the co-deposition process or heating the substrate during deposition. Annealing may include exposing the deposited film to a heat source to increase the temperature of the film. In some aspects, for the annealing process, the film may be exposed to a temperature below the melting point of silver or the conductive metal. Silver has a melting point of about 961°C, while copper has a melting point of about 1,085°C. In some aspects, the material may be exposed to less than or equal to about 600°C, and optionally less than or equal to about 500°C, optionally less than or equal to about 400°C, optionally less than or equal to about 300°C, optionally less than or equal to about 200°C, and for certain substrates (such as plastics or polymers) with conductive metal films thereon, optionally less than or equal to about 100°C. Annealing may be performed in an inert atmosphere, such as in nitrogen (N2) gas or in air. The amount of time used to perform the annealing process depends on the temperature, with higher temperatures requiring less time.

[0105] In certain aspects, the annealing time can range from greater than or equal to about 5 minutes to less than or equal to about 30 minutes, and optionally greater than or equal to about 10 minutes to less than or equal to about 20 minutes. Annealing improves the optical loss of the deposited film, especially for wavelengths in the visible range, thereby making the silver-based film containing conductive materials more like pure silver while maintaining the desired conductivity, smoothness, transparency and other desired properties. Experimental results show that high temperature annealing makes the doped film itself more conductive, and such annealed films are robust to exposure to high temperatures, thereby providing greater stability. In certain variations, annealing can be performed at about 150°C for 15 minutes in a nitrogen (N2) environment, which results in an observed decrease in sheet resistance, as described below.

[0106] The method may also include applying an additional material to the substrate, such as the first layer or the second layer, before the co-deposition of the silver and the conductive metal. In other variations, one or more additional material layers or films may be formed on the conductive film comprising silver and a conductive metal (such as copper) after deposition.

[0107] The ultra-thin doped silver layer is incorporated into a transparent EMI shielding device. Electromagnetic silver shielding (EMAGS) film components or stacks may include a conductive dielectric layer-ultra-thin metal-conductive dielectric layer to minimize electro-optical tradeoffs, for example, transmitting about 96-97% of visible light relative to the underlying substrate material while covering the entire X, K u , K aThe EMAGS film exhibits an excellent average EMI shielding effectiveness (SE) of about 26 dB over a wide bandwidth of 32 GHz in the EMAGS and K bands (from greater than or equal to about 8 GHz to less than or equal to about 40 GHz). By replicating the stack within the shielding device (simply stacking two EMAGS film assemblies together), an EMI shielding efficiency of greater than or equal to about 30 dB can be achieved. By separating the two layers with a quarter-wavelength spacer layer, such an embodiment can have even greater shielding effectiveness of up to 50 dB.

[0108] Figure 4 An example of such an EMI shield 200 is shown. Figure 2 The electromagnetic interference shield 100 of FIG. 1 is similar to that of FIG. 1 , and therefore, to the extent that no further description is given, components or their functions share the same reference numerals and may be considered to be the same as Figure 2 The stack assembly 210 includes a plurality of layers, including a first stack 20A and a second stack 20B. The first stack 20A includes a substrate 30. The first stack 20A also has an ultra-thin metal layer 40 surrounded by a first layer 50 and a second layer 52. The second stack 20B also includes an ultra-thin metal layer 40 surrounded by a first layer 50 and a second layer 52. A capping layer 220 is disposed above the second layer 52 to define the second stack 20B. The capping layer 220 may be formed of a material that is transparent to visible light. The capping layer 220 may also function as an anti-reflection layer for incident electromagnetic waves, and simultaneously function as a protective and barrier layer for gas and water vapor. The capping layer 220 may be made of an organic material, an organic material, or a combination of the two. A spacer or spacer layer 222 is disposed between the first stack 20A and the second stack 20B. The spacer layer 222 may be similar to Figure 2 The spacer layer 122 in the EMI shield 200 may therefore be selected to have a thickness of one quarter wavelength (λ / 4) of the peak wavelength of the second range to be reflected or to be absorbed. For example, the spacer layer 222 may be formed of the same material as the spacer layer 122 (e.g., fused silica). As will be appreciated by those skilled in the art, although not shown, additional layers or stacks may be present within the stack assembly 210 of the EMI shield 200. For example, the presence of one or more additional stacks may improve the shielding effectiveness of the EMI shield 200, albeit with a potentially slightly reduced transmittance of visible light in such a configuration.

[0109] In addition, the electromagnetic interference shielding device incorporating the stack containing the EMAGS film can be flexible, thereby demonstrating stable EMI shielding performance under mechanical deformation. In addition, large-area EMAGS films can be formed via a roll-to-roll sputtering system suitable for mass production. The electromagnetic interference shielding device provided by various aspects of the present disclosure provides excellent optical, broadband EMI shielding and mechanical properties, making it particularly advantageous in various applications including healthcare, electronic security, roll-up displays, and wearable devices.

[0110] Example

[0111] Various embodiments of the present technology can be further understood through the specific examples included herein.The specific examples are provided for the purpose of illustrating how to make and use compositions, devices and methods according to the present teachings.

[0112] Example 1

[0113] Film deposition. In general, the percolation threshold of pure Ag is usually between 10-20nm, which is the critical thickness for forming a continuous conductive film. However, the conductivity of thin Ag films is largely affected by their high surface roughness (for example, the root mean square (RMS) roughness of a 15nm Ag film is about 6nm), which will limit its EMI shielding function. In addition, due to the inherent properties of metals, thick Ag films block a large amount of visible light. Therefore, in order to be used in electromagnetic interference shielding, silver metal films must be continuous and smooth at a thin thickness. Figure 5 A simple co-sputtering process is shown to produce a smooth and ultrathin Cu-doped Ag film. Ag atoms are fixed by Cu atoms instead of agglomerating into islands, thus forming an ultrathin (thickness of about 8 nm) and smooth Ag film. In addition, at the same thickness, the Cu-doped Ag film exhibits a much lower sheet resistance (R) than aluminum (Al)-doped Ag. s ). For example, 8nm Cu doped Ag film exhibits much lower sheet resistance (12.5ohm / square) compared to aluminum (Al) doped Ag film (22ohm / square). Also, 9nm pure Ag is completely non-conductive in comparison.

[0114] ITO / Cu doped Ag / ITO flexible films were prepared on PET (polyethylene terephthalate) substrates using a roll-to-roll (R2R) magnetron sputtering tool at room temperature. The PET substrate was approximately 50 μm thick, coated on both sides with an acrylate hard coating, and pretreated inline with oxygen and argon plasma exposure, which cleaned the substrate and simultaneously enhanced the adhesion between the substrate and the coated film. Both the bottom ITO layer and the top ITO layer were deposited at a rate of 50 nm·m / min, with the source power maintained at 6 kW. The intermediate Cu-doped Ag ultra-thin layer was deposited via co-sputtering of a Cu target and an Ag target, with the source power maintained at 0.5 kW and 4 kW (as more extensively described in U.S. Patent Publication No. 2017 / 0200526 to Guo et al., and as Figure 5 The source power is converted into deposition rates of 8 nm·m / min and 29 nm·m / min, respectively. The overall rolling speed is controlled at 2.5 m / min.

[0115] Membrane characterization

[0116] The thickness of the Cu-doped Ag film was calculated from the calibrated deposition rate and further confirmed by spectral ellipsometer measurement (JAWoollam M-2000). The refractive index of Cu-doped Ag was measured by spectral ellipsometer (ESI). The morphology of the film was studied by SEM (FEI HELIOS Nanolab 600i) and tapping mode AFM (Bruker DimensionFastScan). The crack images of the film were taken using a stereo microscope (Nikon SMZ1500).

[0117] Measurement

[0118] EMI shielding measurements were performed using a waveguide method system. Four different waveguides (Xibao Co., China) were used to measure X, K u , K and K a The shielding performance of the waveguide band. The scattering parameters are measured using a rectangular waveguide, two waveguide coaxials (waveguide-to-coaxials) adapters and a vector network analyzer (KEYSIGHT N5234A). The EMI SE, microwave reflection (R) and absorption (A) of the film can be calculated directly from the scattering parameters. Two waveguides are coaxially connected to the ends of the rectangular waveguide, and the film is inserted into the waveguide. The film is cut into different sizes so that the waveguide can be accurately adapted to different bands (X-22.7×10×0.05mm 3 , K u -15.6×7.7×0.05mm 3 , K-10.5×4.2×0.05mm3 , K a -7.0×3.4×0.05mm 3 ) measurement. The incoming electromagnetic wave was incident vertically on the test sample. The optical transmittance and reflection of the film were measured in the range from 300nm to 1000nm by a UV-Vis-IR spectrophotometer (PerkinElmer Lambda 950) at vertical incidence. The sheet resistance (R s ) were measured using a four-point probe system and are the average results of at least six fields for each sample.

[0119] Ultrathin (e.g., about 8 nm thick) copper (Cu) doped Ag film is formed by introducing a small amount of Cu into the Ag film via a co-sputtering process and extending it into a dielectric-metal-dielectric (DMD) stacking configuration to solve the trade-off between transparency and microwave shielding of traditional EMI shielding materials. The interlayer ultrathin metal film maintains the high conductivity of the Ag material itself, as well as ultra-smoothness (e.g., surface roughness <1 nm) and low optical loss, thereby providing high transparency and shielding capabilities. A transparent conductive dielectric that acts as an effective anti-reflection (AR) layer is added adjacent to each side of the metal layer, which further improves the visible transmittance and EMI SE simultaneously, wherein the improvement of EMI SE is achieved due to the enhanced conductivity of the entire stack. The experimental results of this electromagnetic Ag shielding film (EMAGS) stacking show that the average EMI SE over a wide RF bandwidth is 26 dB and the average visible transmittance is 96.5% (referenced to a PET substrate), which is considered to be one of the best shielding results reported. This electromagnetic interference shielding device also exhibits significantly improved EMI shielding stability under mechanical deformation. Furthermore, the EMI shielding device with two stacks or double-layer EMAGS (D-EMAGS) exhibits an average EMI SE of more than 30 dB, and the SE in each band can be improved to more than 50 dB by two stacks separated by a quarter-wavelength spacer layer. In addition, large-area EMAGS film stacks are demonstrated using roll-to-roll (R2R) sputtering, which shows that the proposed EMI shielding device is more conducive to mass production than traditional patterned metal structures.

[0120] EMI Shielding Device Stackup Design

[0121] FIG6B shows an electromagnetic interference shielding conductive stack configuration of a Cu-doped Ag layer sandwiched between two ITO layers on a PET substrate. As previously mentioned, in order to obtain maximum light transmission, the thickness of the ITO as an optical AR layer is optimized so that the reflected light beam is offset as much as possible in the visible band by destructive interference. For this purpose, the transfer matrix method is used to calculate the average transmittance (400-700nm) of the three-layer structure by changing the thickness of the top ITO layer and the bottom ITO layer from 0 to 100nm when the Cu-doped Ag center layer is fixed at a thickness of 8nm. As can be seen in FIG6C, the average transmittance depends on the thickness of the dielectric layer adjacent to the ultra-thin metal layer. The maximum transmittance is achieved when both the top ITO layer and the bottom ITO layer have a thickness of about 40nm. In a variant, the electromagnetic interference shielding EMAGS film has a design of ITO (40nm thickness) / Cu-doped Ag (8nm thickness) / ITO (40nm thickness). It should be noted that other transparent conductive dielectric materials with similar refractive indices to ITO (e.g., zinc oxide (ZnO) and fluorine-doped tin oxide (FTO)) can also be used as alternative variants of the AR layer in the laminate structure. However, ITO was chosen because of its stability and relatively high conductivity, which can promote the shielding performance of the electromagnetic interference shielding EMAGS film. Figures 6D and 6E show scanning electron microscope (SEM) images of the Cu-doped Ag center layer and the electromagnetic interference shielding EMAGS laminate. Compared with the rough thin pure Ag film, the 8nm copper-doped Ag film is smooth and has no 3D islands (RMS roughness is about 0.42nm). After coating the ITO layer, the RMS roughness of the electromagnetic interference shielding EMAGS film increased slightly to about 1.21nm, but the overall smoothness was guaranteed.

[0122] Optical properties of electromagnetic interference shielding (EMAGS) stacks

[0123] The electromagnetic interference shielding (EMAGS) stack of the film was then sputtered onto a PET substrate using a roll-to-roll (R2R) sputtering system at room temperature, which demonstrated significant advantages for mass production compared to conventional metal patterned structures. Figures 7A(1)-7A(2) and Figure 7B are photographs of the fabricated samples. Figure 7A(1) demonstrates a highly transparent 2cm×2cm electromagnetic interference shielding EMAGS film stack, through which the underlying logo can be clearly observed. Figure 7A(2) is the bent state of the same electromagnetic interference shielding EMAGS film stack, showing great flexibility. A large-area (200cm×50cm) electromagnetic interference shielding transparent EMAGS film stack manufactured by a roll-to-roll method is shown in Figure 7B.

[0124] The optical transmittance of the EMI shielding EMAGS film stack measured in the range of 300-1,000nm is shown in Figure 7C. For comparison, the transmittance of ITO (about 40nm thick, the same as the ITO layer used in the EMI shielding EMAGS stack film), PET substrate and 8nm Cu-doped Ag layer are plotted. It should be noted that the transmittance of the EMAGS stack film, ITO and Cu-doped Ag film is a relative value relative to the PET substrate, which has an average visible transmittance (400-700nm) of 88.1%, as shown in Figure 7C. The average transmittance of the EMAGS stack film in the visible range exceeds 96% (the peak transmittance at 600nm is 98.5%), which is much higher than that of the pure copper-doped Ag layer and ITO layer. This is due to the optimized stack configuration and the suppressed reflection via the AR dielectric layer, as shown in Figure 7D. The optical reflectance of the EMAGS film in the wavelength range of 400-700nm is much lower than that of the Cu-doped Ag film, and even lower than that of the PET substrate.

[0125] EMI Shielding and Electrical Characteristics of EMAGS Stackup

[0126] The electromagnetic interference (EMI) shielding effectiveness (SE) of a material is defined as the logarithmic ratio of the incident power to the transmitted power and is usually expressed in decibels. Higher EMI SE values ​​mean stronger power attenuation and negligible electromagnetic waves pass through the shielding material. For commercial shielding applications (such as mobile phones and laptops), an EMI SE of 20dB is required, which corresponds to only 1% transmission of the incoming electromagnetic waves. To investigate the EMI shielding performance, EMAGS laminate films deposited on PET were measured using a waveguide configuration.

[0127] The measured RF band is as wide as 32 GHz, covering X (8-12 GHz), K u (12-18GHz), K (18-26.5GHz) and K a (26.5-40GHz) band. For different microwave bands, the EMAGS stack samples are adapted to specific waveguides. Before the measurement, the system is calibrated using a two port thru-reflect-line calibration, which introduces 12 error corrections at each frequency.

[0128] Figures 8A-8DThe EMI SE of the EMAGS laminate film prepared according to certain aspects of the present disclosure in different frequency bands across the range of 8-40 GHz is shown. For comparison, an ITO film and a PET substrate were also measured. The pure PET film without other layers is completely transparent to electromagnetic waves and has an EMI SE close to 0 dB in the entire measured frequency band. The small peak in the higher frequency band (Figure 8D) is attributed to the interference between the reflections from the top and bottom interfaces of PET. Despite the entire frequency range of 8-40 GHz, the EMAGS laminate prepared according to the present disclosure also exhibits excellent shielding performance, with an average EMI SE close to 26 dB ( Figures 8A-8D ), which blocks about 99.7% of radio frequency (RF) power. More importantly, the SE has no roll-off behavior as the frequency increases, which results in effective and indiscriminate shielding performance across a wide range. This wide (32GHz bandwidth) and highly effective (>20dB) EMI SE of the electromagnetic interference shielding EMAGS laminate film according to certain aspects of the present disclosure outperforms most previously reported EMI shielding materials based on patterned metal structures. For example, the EMI SE of the square metal mesh shielding structure drops rapidly in a narrow band, even at K u A 5 dB drop is also shown within the band. The same EMI shielding roll-off behavior at high frequencies is also found in conventional loop-based and crack-based metal meshes due to the high transmission of shorter wavelength electromagnetic waves through the patterned openings.

[0129] As a comparison, Figures 8A-8D The SE of 8nm Cu doped Ag (about 23dB) and 40nm ITO (about 19dB) films are also shown, both of which are lower than the SE of the electromagnetic interference shielding EMAGS stack structure. The shielding performance of the double-layer electromagnetic interference shielding EMAGS (D-EMAGS) stack was studied by merging two EMAGS film stacks together. The double-layer electromagnetic interference shielding EMAGS (D-EMAGS) stack exhibited an EMI SE of more than 30dB in the frequency range of 8GHz to 40GHz, with a peak efficiency of 39dB at 29GHz. The fluctuations in the measured curves of the D-EMAGS film are attributed to multiple reflections between the two EMAGS stacks. The average transmittance of D-EMAGS in the visible range is about 93%. In order to utilize the shielding potential of the D-EMAGS electromagnetic interference shielding structure, the two EMAGS stacks are further separated by a spacing equal to one-quarter of the center wavelength in each band. Ultra-high SE is achieved by these configurations, with an average SE greater than about 50dB.

[0130] When an electromagnetic wave is incident on a shielding material, the incident power can be divided into reflected power (R), absorbed power (A) and transmitted power (T), and the relationship is A+R+T = 1. Using the scattering parameters of the electromagnetic interference shielding EMAGS film measured by the waveguide method, the microwave reflection and absorption in the range of 8-40 GHz are calculated accordingly.

[0131] 9A-9D show the measured microwave reflection and absorption of the EMAGS film as a function of the incident frequency. More specifically, the electromagnetic interference shielding EMAGS film prepared according to certain aspects of the present disclosure has a good performance in the X-band (8-12 GHz) (FIG. 9A), K u band (12-18 GHz) (Figure 9B), K band (18-26.5 GHz) (Figure 9C) and K a Measured microwave reflection and absorption of the band (26.5-40GHz) (Figure 9D). Figure 9E shows the power loss density in each layer of the ITO / Cu doped Ag / ITO structure at 12GHz calculated using CST Microwave Studio. Figure 9F shows the calculated shielding contribution of R and A of 1) Cu doped Ag, 2) ITO / Cu doped Ag and 3) ITO / Cu doped Ag / ITO structure. Shown is the power flow in the structure of Figure 9G (1) air, Figure 9G (2) ITO, Figure 9G (3) ITO / Cu doped Ag and Figure 9G (4) ITO / Cu doped Ag / ITO structure at 12GHz simulated using CST Microwave Studio. The white arrows in Figure 9G (1)-Figure 9G (4) indicate the direction of the incident electromagnetic wave.

[0132] In summary, the average reflection and absorption are 88.5% and 11.2% of the incident power, respectively. Taking the frequency of 12 GHz as an example, the shielding contribution of reflection and absorption of different structures was investigated: 1) Cu doped Ag, 2) ITO / Cu doped Ag, and 3) ITO / Cu doped Ag / ITO. The results are summarized in Figure 9E. As can be seen from the bar graph, the shielding is mainly caused by the strong reflection of all structures. In addition, from 1) to 3), the reflection has an upward trend, from 86.2% to 90.2%, while the absorption undergoes a decline, suggesting that the shielding enhancement comes from increased reflection. At microwave frequencies, the real part (n) and imaginary part (k) of the refractive index of conductors (e.g., Cu doped Ag and ITO) are both on the order of 104, so the reflection at the first air-conductor interface is close to unity. Subsequent reflections from the back conductor-air interface will reduce the total reflection to a certain extent by generating destructive interference. However, when the thickness of the conductor increases (e.g., adding more ITO layers in this case), fewer microwaves can reach the back conductor-air interface and the effect of this secondary reflection on the total reflection intensity is greatly weakened, which is consistent with the observations in Figure 9E.

[0133] In addition to the main reflection, a portion of the microwaves are shielded by absorption inside the conductor. The microwave absorption contributed by the conductive dielectric and metal layers in the EMAGS structure was further examined. In Figure 9F, the contour map of the simulated power loss density shows that the metal layer contributes more to microwave absorption because of its larger attenuation coefficient (higher n and k). In essence, when an electromagnetic wave is incident on the EMAGS structure, the ITO and Cu-doped Ag layers behave like three parallel resistors at the same potential. Therefore, the conductive element characterized by lower resistance (i.e., the Cu-doped Ag layer) will result in relatively stronger ohmic losses and higher microwave absorption. Figures 9G (1)-9G (4) illustrate the power flow distribution within different structures at 12 GHz simulated using CST Microwave Studio. By subsequently adding 40nm ITO and 8nm Cu-doped Ag layers (Figures 9G (2)-9G (4)), the entire incident EM field is gradually blocked due to the reflection and absorption of these conductors, and the minimum power transmission through the ITO / Cu-doped Ag / ITO structure is shown.

[0134] The reflection-dominant mechanism and broadband EMI shielding performance can be explained more intuitively by considering the ITO / Cu-doped Ag / ITO stack as an effective single layer with high conductivity. Compared with the impedance of free space (377Ω), the highly conductive layer has a much lower impedance across a wide microwave range due to the higher density of charge carriers per unit area. As a result, most of the incident electromagnetic waves are reflected back to free space due to the large impedance mismatch at the air / EMAGS interface. In fact, the theoretical shielding bandwidth of the EMI-shielding EMAGS film is much wider than the measured range without any reduction in SE, which was verified by CST simulations in ESI.

[0135] Mechanical properties of EMAGS

[0136] In order to evaluate the mechanical flexibility of the electromagnetic interference shielding EMAGS film prepared according to certain aspects of the present disclosure, the change of EMI SE of the electromagnetic interference shielding EMAGS laminate film was measured as a function of bending cycles and bending radius under repeated bending. The inset in Figure 10A shows a schematic diagram of the bending setting. By adjusting the distance (ΔL) from the initial state (L) to the two ends, different bending radii (r) can be controlled. As shown in Figure 10A, the sheet resistance (R) of the EMAGS film is 6 mm when the bending radius is 6 mm. s ), remained almost unchanged after 250 bending cycles, and slightly increased from 11.0Ω / sq to 12.1Ω / sq after 1,000 bending cycles. In contrast, the R sIt increases sharply from 29.5Ω / sq to 123.0Ω / sq after only 250 bends. Figure 10B shows the variation of EMI SE at 12GHz as a function of bending cycles with a bending radius of 6mm. In contrast, the same bending test was performed on the ITO film. Interestingly, after 250 bending cycles, the EMI SE of the EMAGS film maintained its initial high performance, while the EMI shielding of the ITO film dropped significantly after only 50 bending cycles due to large cracks on the surface (as shown in the embedded SEM image in the figure). As the bending cycles increased from 50 to 250, the EMI SE of the ITO film continued to decrease, showing almost no shielding effect (<1dB) after 250 repeated bends. The inset in Figure 10B provides an SEM image of the EMAGS film after the bending test, without any visible cracks. This is consistent with the stable R of the proposed EMAGS film after a large number of bendings. s And the shielding performance is consistent. At the same time, it is worth noting that the measured R s and EMI SE match well with the predicted relationships presented in Figure 6A.

[0137] Then, as shown in Figures 10C and 10D, the changes in shielding performance for different polarizations were studied when the bending radius varied from 12 mm to 2 mm. It is noteworthy that when the bending radius was greater than 3 mm, the EMI SE of the EMAGS film did not decrease after 1,000 bends. When the radius (r) was reduced to 2 mm, the SE of the transverse magnetic polarization (TM) wave (i.e., the electric field perpendicular to the crack line as shown in the inset of Figure 10C) tended to decrease with the increase in bending cycles. As shown in the graph for r = 2 mm, the EMI SE decreased to 23 dB and 6 dB after 100 and 1,000 bending cycles, respectively. On the other hand, for transverse electric (TE) polarization (i.e., the electric field parallel to the crack line as shown in the inset of Figure 10D), high SE was maintained after 1,000 bends. The dependence of EMI SE on polarization is because the thin conductive film with crack lines after bending is essentially a wire grid polarizer (WGPs) for RF waves, considering the subwavelength distance between the crack lines. Therefore, TM waves can pass easily, while TE polarization is effectively reflected. The same phenomenon can be observed when the ITO film is bent. Regardless of the bending radius, after 250 bending cycles, the EMI SE of ITO to TM waves decreases significantly (SE < 5dB), which contrasts with the good flexibility of the electromagnetic interference shielding EMAGS film prepared according to certain aspects of the present disclosure. Even after bending 250 times at a radius of 2 mm, the TE polarization shows only a small decrease, which is consistent with the WGP model proposed for conductive films with curved crack lines.

[0138] The SEM images in Figures 11A and 11B directly compare the surface morphology of the EMI shielding EMAGS laminate and the ITO film after a bending test at r = 3 mm. Under the same 250 bending cycles, the crack lines on the ITO film in Figure 11B are much more obvious than the crack lines on the EMAGS film of the present invention shown in Figure 11A. The shallow and narrow crack lines on the surface of the EMAGS film show no effect on the shielding as verified in Figures 10A-10D. The results show that the mechanical flexibility of the EMI shielding laminate structure is significantly improved, which is due to the high ductility of the thin Cu-doped Ag sandwiched therein and the enhanced cohesive strength of the ITO after the addition of the metal interlayer. The flexible EMAGS films show excellent EMI shielding stability under mechanical deformation, which makes them potentially useful as high-performance EMI shielding materials in flexible electronics. As shown in Fig.12 As summarized in the report, when considering optical transmittance and microwave shielding performance, electromagnetic interference shielding (EMAGS) films outperform various traditional transparent shielding structures and materials, including metal mesh, graphene-based materials, graphene hybrid structures, silver nanowires, multilayer Ag / acrylate stacks, and commercial transparent foils. Although the EMI SE of the graphene / metal mesh structure can reach 29dB at 12GHz, the shielding is only applicable to a narrow frequency range and drops rapidly to only 13dB at 40GHz.

[0139] According to certain aspects of the present disclosure, a large-area flexible film based on ultra-thin Cu-doped Ag is provided, which has excellent optical transmittance, broadband shielding performance and excellent mechanical flexibility. The electromagnetic interference shielding EMAGS laminated film in these variants shows an average relative transmittance of 96.5% in the visible range, with a peak of 98.5% at 600nm. The average EMI SE is 26dB, which is considered to be one of the best shielding results reported at this level of transparency for visible light. More importantly, it exhibits broadband shielding covering a bandwidth of 32GHz. EMI SE of more than 30dB can also be expected by stacking multiple EMAGS films. Compared with ITO film, no obvious degradation of the EMAGS film was observed under repeated bending cycles with a radius of about 3mm, confirming the mechanical flexibility of the film. The proposed transparent EMAGS film has great potential to become a star material in future RF shielding applications.

[0140] Example 2

[0141] In this embodiment, a transparent microwave absorber (MA) based on an asymmetric Fabry-Perot resonant cavity is formed by adopting a stack including a graphene layer-dielectric layer-ultra-thin doped silver alloy layer (GDS) configuration.

[0142] Fig.14Graphene synthesis is shown in: A graphene film is grown on a 25 μm thick Cu foil (Alfa Aesar, 99.8% purity) using a CVD method at the center of a tube furnace. The foil is then heated to 1,000°C under H2, 60 Pa for half an hour. A carbon source (CH4) is then introduced into the quartz tube for 2 hours. After the subsequent gas mixture, the sample is quickly cooled to room temperature (25°C). The fast cooling rate suppresses the formation of multilayer graphene.

[0143] Graphene transfer: Fig.14 As shown in , the graphene so grown on the Cu foil is transferred by spin coating 5 μm thick polymethyl methacrylate (PMMA) on the graphene. After PMMA dries, the sample is immersed in Marble's etchant (HCl:H2SO4:CuSO4=50ml:50ml:10g) solvent to etch the Cu foil. After removal, the graphene sample is washed in distilled water and transferred to a 1 mm silica substrate to be used.

[0144] Film deposition: ITO / Cu-doped Ag / ITO flexible films were prepared on PET (polyethylene terephthalate) substrates at room temperature using a homemade magnetron sputtering (MS) tool. The PET substrate was about 50 μm thick, coated with an acrylate hard coating on both sides, and pretreated in-line with oxygen and argon plasma exposure, which can clean the substrate and simultaneously enhance the adhesion between the substrate and the coated film. Both the bottom and top ITO layers were deposited at a rate of 50 nm·m / min, with the source power maintained at 6 kW. The middle Cu-doped Ag ultra-thin layer was deposited via co-sputtering of Cu and Ag targets, with the source powers maintained at 0.5 kW and 4 kW, which translated into deposition rates of 8 nm·m / min and 29 nm·m / min, respectively. The overall rolling speed for the roll-to-roll process was controlled at 2.5 m / min.

[0145] Characterization and measurements: The thickness of the ITO / Cu doped Ag / ITO films of each layer was calculated from the calibrated deposition rate and confirmed by spectroscopic ellipsometer measurements (JA Woollam M-2000). The morphology of graphene and ITO / Cu doped Ag / ITO films was studied by SEM (FEI HELIOS Nanolab 600i) and tapping mode AFM (Bruker Dimension FastScan) on fused silica and PET substrates, respectively. The optical transmittance of the films and GDS cavities was measured by UV-Vis-IR spectrophotometer (PerkinElmer Lambda950) at normal incident radiation from 300 nm to 1000 nm. The microwave transmission and reflection of the samples were measured using a waveguide method in the X-band and K-band. u The band is calculated from the measured S parameters.

[0146] The electromagnetic interference shielding (EMI) device stack assembly in this variant includes graphene, an ultrathin doped silver (Ag) film as a transparent microwave absorber and reflector, and fused silica as a dielectric spacer. In addition, by using a single layer of graphene as a building block and adjusting the thickness of the dielectric spacer to achieve critical coupling in the cavity, this device experimentally obtains near-consistent (about 99.5%) absorbance and remains highly transparent (about 65%) in the visible range. In addition, due to the inherent loss of the graphene layer, a wide absorption bandwidth is achieved, with a bandwidth measured at 13.75 GHz being 72.7% of the center resonant frequency.

[0147] Design and fabrication of transparent microwave absorbers

[0148] Materials with high losses need to be incorporated in the resonant cavity design for energy harvesting / absorption. Graphene has partial microwave absorption and reflection properties and can be an effective candidate material for the top absorbing medium of the Fabry-Perot cavity. In addition, silver (Ag) is selected as the back reflector because Ag has high conductivity for strong power reflection in the microwave range and has the lowest absorption loss among metals in the optical range. The schematic diagram of the proposed visible transparent MA utilizing the cavity resonant behavior is shown in Figure 2 13A-13B. The device structure includes a single layer of graphene, an ultra-thin silver alloy containing copper surrounded by two indium tin oxide layers, and a fused silica layer (disposed between the graphene and one indium tin oxide layer). Figure 5 A small amount of copper (Cu) is introduced into Ag during the co-deposition process shown, forming a continuous ultra-thin (8 nm) and ultra-smooth conductive alloy film by suppressing the Volmer-Weber growth mode of Ag.

[0149] One strategy to increase the optical transmittance of ultrathin doped Ag films is to employ antireflection coatings; thus, an ultrathin doped Ag layer is sandwiched between two indium tin oxide (ITO) layers while simultaneously maintaining excellent electrical conductivity. This provides ultralow microwave transmission from the cavity. Finally, the microwave reflector is implemented in the form of an ITO (thickness 40nm) / Cu-doped Ag (thickness 8nm) / ITO (thickness 40nm) stack. By using calculation results using the transfer matrix method (TMM), the thickness of the ITO layer is optimized to maximize the overall transparency.

[0150] Figures 13C(1)-13C(2) show scanning electron microscopy (SEM) and atomic force microscopy (AFM) images of the graphene film on the silicon dioxide substrate after transfer from the Cu foil, respectively, confirming the excellent continuity without macroscopic defects. The small white dots in Figure 13C(2) are PMMA residues after the removal process. In order to verify the quantity and quality of the prepared graphene, the Raman spectrum was measured using a laser wavelength of 532nm as shown in Figure 13C(3). The Raman spectrum exhibits typical peak characteristics of monolayer graphene, including G and 2D bands. The 2D band exhibits a single Lorentzian feature with a peak at about 2686cm -1 At about 26cm -1 The full width at half maximum (FWHM) of the G band is larger than that of the G band. -1 The intensity of the D band at is below the Raman detection limit, confirming the absence of significant defects. The Fermi level of graphene is then determined by comparing the positions of the measured G and 2D peaks, with a characteristic correlation (f) estimated to be f = -0.3 eV.

[0151] Next, for ease of experimental implementation, doped Ag and ITO layers were deposited on a PET substrate. SEM and AFM images of the ITO / Cu doped Ag / ITO deposited in this way are shown in FIG. 13D , both showing a continuous and smooth surface morphology. Finally, FIG. 13E shows optical micrographs of silica, a graphene film on silica, and a final GDS cavity sample prepared according to certain aspects of the present disclosure. Compared to pure silica (left), a single-layer graphene film on silica (middle) is highly transparent with little transmittance loss. The GDS cavity (right) with a size of 2.2 cm×1.1 cm also shows good transparency.

[0152] Theoretical conditions and experimental verification of perfect microwave absorption

[0153] As shown in FIG15A , considering that the thickness of the metal layer is fixed to ensure transparency, the transparent EMI shield / microwave absorber (MA) designed in this configuration involves eight parameters (n1, n2, k2, n3, n4, k4, d2, d3). It is effective to describe the properties of graphene using its surface conductivity (σ) because this quantity can be directly modeled or measured over a wide range from RF frequencies to optical frequencies, and the corresponding refractive index (n) and extinction coefficient (k) can be derived from the conductivity. For theoretical analysis, the conductivity of graphene can be calculated using the Kubo formula for inter-band and intra-band contributions, and estimated using the following expression,

[0154]

[0155]

[0156] Where e is the electron charge, k B is the Boltzmann constant, T is the temperature, is the reduced Planck constant, ω is the frequency of the incident electromagnetic wave, and Γ is the relaxation time, which is assumed to be independent of energy. It is worth noting that the conductivity of graphene depends strongly on its Fermi level μ c The value of the Fermi level can be controlled by chemical doping or electrostatic gating (e.g. Figure 3 On the other hand, the ITO / Cu-doped Ag / ITO stack (mirror) can be modeled as an effective single layer with high conductivity, since most of the contribution comes from Ag, the most conductive element.

[0157] Theoretical conditions for perfect microwave absorption considered in a planar graphene layer through the entire GDS cavity. For simplicity, it is assumed that only the top graphene is lossy and the bottom reflective layer can be considered as a perfect electrical conductor, providing 100% reflectivity. An analytical method is introduced for absorption structures used in optical applications, where the absorptivity per unit length normalized to the incident microwave can be expressed as:

[0158]

[0159] Where E(z) is the electric field in the ultrathin graphene film, E0 is the incident electric field, c is the speed of light in a vacuum, and f is the frequency of the incident electromagnetic wave. Therefore, the total absorption in the graphene film is:

[0160]

[0161] Typically, the ideal thickness d2 of a single-layer graphene is about 0.34nm, in sharp contrast to the incident wavelength in the microwave range, which is in the order of millimeters, indicating that d2<<λ. Therefore, the graphene sheet minimally changes the electric field profile inside the structure, and the electric field can maintain its intensity, which can also be verified by calculating the electric field distribution inside the graphene layer at different frequencies. Given the zero reflection under critical coupling conditions, it can be assumed that

[0162] E(z)=E(z=0)=E0, 0≤z≤d2 (5).

[0163] Substituting equation (5) into equation (4) gives the perfect microwave absorption condition (A total =100%), provided as

[0164]

[0165] Therefore, for uniform absorption in the graphene layer, the parameters should satisfy the above relationship. The dashed line in Figure 15B plots the calculated value of 4πn2k2d2f / cn1 for normal incidence, revealing that c Under the conditions of =0.3eV and Γ=20ps, theoretically, the graphene film can achieve perfect absorption in the GDS cavity at around 15GHz.

[0166] In addition, by adopting TMM, the reflection (R) and absorption (A=1-R) of the GDS cavity are calculated at a predetermined frequency. Considering the symmetry of the cavity in the XY plane, the device is considered to be independent of the polarization under vertical incidence. In the following numerical calculations, only TE-polarized incident microwaves are considered. Figure 15C shows the absorption diagram calculated as a function of different graphene Fermi levels and frequency at a dielectric thickness d3 of 3 mm. The absorption diagram illustrates that the nearly uniform absorption of the GDS cavity can be achieved in region A (black dashed circle) using different Fermi levels, which also shows that the conditions for achieving strong absorption are not very strict. In addition, the ideal perfect absorption is μ near 15 GHz. c = about 0.3eV, which is consistent with the predicted results. Figure 15D shows the absorption calculated by changing the dielectric thickness (ranging from 0mm to 15mm) at different excitation frequencies. As shown in Figure 15D, the absorption peak appears periodically with the increase of frequency and with the growth of dielectric thickness at a specific frequency under a fixed dielectric thickness. Specifically, when the dielectric thickness d3 changes from 1mm to 15mm, the absorption peak moves continuously from ≈40GHz to ≈2GHz. At the same time, in the case of thicker cavities and higher frequencies, some higher modes begin to appear, showing ripples on the absorption graph. Therefore, it is obvious that the peak absorption frequency can be easily adjusted by changing the dielectric thickness of the cavity. Note that at a fixed dielectric thickness (e.g., d3=6mm), the bandwidth of the low-order resonance is slightly wider than the bandwidth of the high-order mode (black dashed line in Figure 15D), which increases the working bandwidth and provides better tolerance for experimental verification.

[0167] To confirm the experimental microwave absorption performance of the GDS cavity, microwave transmission (T) and reflection (R) were measured at normal incidence using a waveguide configuration and then used to calculate absorption, which is defined as A = 1-TR, where R = |S 11 | 2 and T=|S 21 | 2 The microwave responses of the GDS cavity layers were analyzed separately to study the effects of each layer. The X-band and K-band performance of single-layer graphene on SiO2 substrate and ITO / Cu-doped Ag / ITO on PET substrate were plotted. uMicrowave transmission and reflection in the band. As predicted, the single-layer graphene is partially reflective and absorptive to microwaves, with an average of about 25% reflection and about 45% transmission. On the other hand, the ITO / Cu-doped Ag / ITO layer supports broadband high reflection, corresponding to a transmittance of only about 0.3%, which is almost perfect as a microwave reflector.

[0168] Then, the absorption performance of the GDS cavity prepared according to certain aspects of the present disclosure is explored. From model calculations using TMM, numerical CST simulations, and experimental measurements, the absorption performance of the GDS cavity in the X-band and K band is plotted as the silica thickness d3 ranges from 1 mm to 4 mm. u The absorption spectrum in the band, such as Figures 16A-16F As shown. As the dielectric thickness increases, the position of the absorption peak gradually red-shifts to low frequencies and can be adjusted across the entire measured spectrum from 8 GHz to 18 GHz. The calculated and simulated vertical incidence spectra for four different thicknesses of silicon dioxide (d3 = 2.5 mm, 3 mm, 3.5 mm, 4 mm) show near-consistent absorption at resonances where the maximum absorption values ​​all exceed 99.5%. The overall shape, trend, and position of the experimental features in Figures 16E and 16F match the calculated and simulated results very well. As represented by the purple curve (d3 = 3 mm) in Figures 16E and 16F, the measured absorption reaches a maximum value of 99.5% at 13.75 GHz, showing that near-consistent absorption is achieved. At the same time, in the case of d3 = 3 mm, covering the entire X and K u Broadband absorption is obtained with absorption > 50% measured from 8 GHz to 18 GHz, all while maintaining ultra-low microwave transmission through the cavity. For the other cases of d3 = 2.5 mm, 3.5 mm and 4 mm, the maximum absorption values ​​are all over 98% at their resonant frequencies.

[0169] Asymmetric Fabry-Perot Cavity

[0170] To better understand the extraordinary microwave absorption, numerical calculations of the TMM using the electromagnetic response, including the electric field and absorbed power distribution throughout the cavity (d3 = 3 mm) at the wavelength of interest, are shown in Figures 17A-17B. It is noteworthy that the resonant modes in the top graphene layer appear at about 13 GHz (designated as #1) and about 40 GHz (designated as #2), as shown in Figure 17A, which matches well with the perfect absorption frequency when the dielectric thickness is 3 mm in Figure 15D. The enhanced electric field distribution at resonance further reveals the reason for the strong absorption in the graphene layer of the cavity, because the power absorption is proportional to the electric field strength. Although the electric field strength at 25 GHz (designated as #3) is shown to be the highest in the GDS cavity of this thickness, it is located in the middle silica layer, and since the silica layer is lossless in the microwave range, the absorption performance may still be poor.

[0171] Subsequently, the absorbed power distribution was calculated as a function of frequency for the same GDS cavity thickness. In Figure 17B, the strong absorption locations (#1 and #2) correspond well to the areas in Figure 17A, where the electric field is highly concentrated. In addition, it is obvious that almost all the microwave power is absorbed by the top graphene layer. As for the bottom Ag layer, even though the electric field is very weak, the power absorbed by Ag is still very small due to the large attenuation coefficient of Ag in the microwave range. It should be noted that the thickness of the layers in the contour plots are not drawn to scale (for example, the single layer thickness is greatly exaggerated), so the number of sampling points in each layer was adjusted to give a rough estimate of the power absorbed by the Ag layer. Figures 16A-16F The same color distribution as the original image is used to give a more intuitive comparison.

[0172] In fact, the GDS cavity is similar to an asymmetric Fabry-Perot (FP) cavity, which includes a lossless dielectric core with a partially reflective top layer and a back reflector. At resonance, the microwave beams reflected from the air / graphene and silica / metal interfaces form destructive interference, resulting in zero reflection. The interference condition is related to the single or multiple round-trip phase shifts of the electromagnetic waves inside the resonant cavity, which explains the periodic absorption peaks at a fixed dielectric thickness in Figure 15D. Nevertheless, the electromagnetic interference (EMI) shielding component is different from the traditional symmetric FP cavity. Traditional FP resonators exhibit high frequency selectivity (high Q) in their reflection or transmission spectra, in which case the transmission process does not involve any energy conversion or absorption. Note that by incorporating a lossy graphene layer in the FP cavity, the structure can produce a large amount of power absorption.

[0173] Optical performance

[0174] To characterize the optical properties of the electromagnetic interference (EMI) shielding GDS resonant cavity, the optical transmission spectra were measured in the range of 300nm-1000nm for various layers and GDS components / cavities with different dielectric thicknesses, such as Figures 18A-18BAs shown. The graphene and silica substrates (0.5 mm and 1 mm) thus prepared show almost flat transmission spectra in the visible and near-infrared regions, with visible transmittances of 96.7%, 93% and 92% at 550 nm, respectively. For the silica substrate, the thicker substrate has a slightly lower transmittance because of the reduced absorption in the material. The overall average transmittance of ITO / Cu-doped Ag / ITO on PET substrate in the visible band is 88.1%, and the improved transparency is due to the anti-reflection coating on the Cu-doped Ag layer. In addition, at longer wavelengths, it approaches the overall average transmittance of a perfect conductor, and its reflection increases toward the infrared region. Therefore, as depicted by the red curve in Figure 18A, the film transmittance gradually decreases, but still maintains a relatively high value (e.g., 65% at 900 nm).

[0175] Similar to the ITO / Cu doped Ag / ITO layer, the transmission spectrum of the electromagnetic interference (EMI) shielding component GDS resonant cavity shows a downward trend with the increase of wavelength at different dielectric thicknesses in the near-infrared range. On the other hand, as depicted in Figure 18B, when the thickness of the silica layer increases, the transmittance decreases, which is attributed to the reflection loss at the interface and the very small absorption loss in the substrate. In fact, in these experiments, the various dielectric thicknesses (1mm to 4mm) of the cavity are just stacks of different combinations of 0.5mm and 1mm silica substrates, and the air gap between the slides is inevitable. As a result, the step optical losses in the transmission spectrum (e.g., from 1.0mm to 1.5mm / from 2.0mm to 2.5mm / from 3.0mm to 3.5mm) are mainly caused by the reflection loss on the air / silicon dioxide interface in the cavity. The thicker cavity is composed of more silica substrates, so more reflection losses are introduced at the interface. The slight transmittance drop from the adjacent solid to the dotted line is attributed to the absorption loss in the substrate. For the case of d3 = 3 mm, near uniform absorption in the microwave range is achieved, and an average visible transmittance of 65% can still be maintained. It is important to note that the transparency of the GDS cavity formed according to certain aspects of the present disclosure can be further improved by removing the PET substrate (~88.1%) and using a complete stack of dielectric spacers in between (reducing reflection losses at the air / silicon dioxide interface), and the theoretical maximum visible transmittance of the GDS cavity is close to 87%.

[0176] In various aspects, the present disclosure provides a method for broadband electromagnetic interference (EMI) shielding by using a stack with an ultra-thin and smooth doped silver film. Further, a transparent conductive dielectric layer is used as an optical anti-reflection layer in combination with an ultra-thin and smooth doped silver film to improve the shielding performance while avoiding sacrificing light transmittance. Moreover, the manufacture of the structure only involves a material deposition process, which greatly reduces the complexity and cost of making such a structure, so that large-area devices can be manufactured with high yields.

[0177] In summary, the present disclosure provides an electromagnetic interference (EMI) shielding (EMAGS) film stack structure in the form of a dielectric-conductive metal-dielectric layer assembly that can transmit more than 96% of visible light relative to an underlying substrate in certain variations and has a high performance in covering the entire X-band, K-band, and u Band, K-Band and K a The EMAGS film has an excellent EMI shielding effectiveness of at least about 6 dB within a wide bandwidth of 32 GHz in the band. Other embodiments provide an EMI shielding effectiveness of greater than or equal to about 30 dB by assembling two EMAGS film stacks together. By separating the two stacks with a quarter-wavelength spacer layer, the EMI shielding effectiveness can be further improved to 50 dB. This electromagnetic interference (EMI) shielding (EMAGS) film stack structure is also flexible and demonstrates stable EMI shielding performance under mechanical deformation. In addition, a large area electromagnetic interference (EMI) shielding (EMAGS) film stack structure can be formed on a roll-to-roll sputtering system for mass production. A graphene layer or other ultra-thin conductive layer can be placed above the silver alloy layer to achieve RF absorption, which provides an additional form of EMI shielding.

[0178] The present disclosure also contemplates a transparent electromagnetic interference (EMI) shielding device that can provide near-uniform absorption when used as a microwave absorber. A transparent electromagnetic interference (EMI) shielding assembly based on an asymmetric Fabry-Perot cavity can include a stack including graphene, a transparent spacer layer, and ultrathin doped Ag. The experimental results are in good agreement with theoretical predictions. The physical origins of these phenomenal features can be understood through rigorous studies of the critical coupling modes supported by the asymmetric Fabry-Perot cavity. Experimental results show that in selected embodiments, the maximum absorption at 13.75 GHz is as high as about 99.5%, with an average visible transmittance of 65%. In addition, the GDS resonant cavity can be electrically gated (at Figure 3 The transparent electromagnetic interference (EMI) shielding device can be used for transparent microwave absorption applications and thus has broad applicability to new microwave optical components.

[0179] The foregoing description of the embodiments has been provided for the purpose of illustration and description. It is not intended to be exhaustive or to limit the present disclosure. Individual elements or features of a particular embodiment are generally not limited to that particular embodiment, but are interchangeable where applicable and can be used in selected embodiments, even if not specifically shown or described. The same may also be varied in a variety of ways. These variations should not be considered as departing from the present disclosure, and all such modifications are intended to be included within the scope of the present disclosure.

Claims

1. A method for broadband electromagnetic interference shielding, the method comprising: An electromagnetic shielding member is arranged in a transmission path of electromagnetic radiation to block a frequency range of greater than or equal to 600 MHz to less than or equal to 90 GHz to achieve a shielding efficiency greater than or equal to 20 dB, and a wavelength range within a visible range of greater than or equal to 390 nm to less than or equal to 740 nm is transmitted through the electromagnetic shielding member to achieve an average visible transmission efficiency greater than or equal to 65%, wherein the electromagnetic shielding member includes a flexible laminate, and the flexible laminate includes: a continuous metal film defining a first side and an opposite second side, and comprising greater than or equal to 80 atomic % silver and less than or equal to 20 atomic % copper, having a thickness less than or equal to 10 nm, having a sheet resistance less than or equal to 20 Ohm / square, the continuous metal film being substantially transparent to the wavelength range; a first conductive layer disposed adjacent to the first side of the continuous metal film, wherein the first conductive layer comprises a conductive dielectric material selected from the group consisting of indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly(3,4-ethylenedioxythiophene), and mixtures thereof; and A second conductive layer is disposed adjacent to the opposite second side of the continuous metal film, wherein the second conductive layer comprises a conductive dielectric material selected from the group consisting of indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly (3,4-ethylenedioxythiophene), and mixtures thereof.

2. The method according to claim 1, wherein: The electromagnetic shielding element further comprises a graphene layer.

3. The method according to claim 2, wherein: The graphene layer includes at least one dopant.

4. The method according to claim 2, wherein: The electromagnetic shield also includes at least one spacer layer including a dielectric material disposed between the graphene layer and the second conductive layer of the flexible stack.

5. The method according to claim 4, wherein: The at least one spacer layer has a thickness corresponding to one quarter of a peak wavelength of electromagnetic radiation in a frequency range of greater than or equal to 800 MHz to less than or equal to 90 GHz.

6. The method according to claim 1, wherein: The blocking is for a frequency range of greater than or equal to 8 GHz to less than or equal to 40 GHz to achieve a shielding efficiency greater than or equal to 26 dB.

7. The method according to claim 1, wherein: The electromagnetic shielding device also includes a graphene layer, which together with the flexible stack defines a resonant cavity, so that the blocking includes absorbing a frequency range greater than or equal to 800 MHz and less than or equal to 90 GHz in the resonant cavity, so that the reflectivity of the electromagnetic shielding device is less than or equal to 1%.

8. The method according to claim 1, wherein: The shielding efficiency is greater than or equal to 20 dB, and the average visible transmission efficiency is greater than or equal to 85%.

9. The method according to claim 1, wherein: The shielding efficiency is greater than or equal to 30 dB, and the average visible transmission efficiency is greater than or equal to 80%.

10. The method according to claim 1, wherein: The shielding efficiency is greater than or equal to 50 dB, and the average visible transmission efficiency is greater than or equal to 65%.

11. The method according to claim 1, wherein: The first conductive layer has a thickness less than or equal to 45 nm, and the second conductive layer has a thickness less than or equal to 45 nm.

12. The method according to claim 1, wherein: The flexible stack also includes a substrate that is transmissive to the wavelength range.

13. The method according to claim 1, wherein: After greater than or equal to 250 bending cycles, the flexible laminate has a sheet resistance (R s ).

14. A method for broadband electromagnetic shielding, the method comprising: An electromagnetic shielding device is arranged in the transmission path of electromagnetic radiation to block the frequency range of greater than or equal to 800Mhz to less than or equal to 90GHz to achieve a shielding efficiency greater than or equal to 20dB, and a wavelength range within the visible range of greater than or equal to 390nm to less than or equal to 740nm is transmitted through the electromagnetic shielding device to achieve an average visible transmission efficiency greater than or equal to 65%, wherein the electromagnetic shielding device comprises: A first flexible stack, the first flexible stack comprising: a first continuous metal film, the first continuous metal film defining a first side and an opposite second side, and the first continuous metal film comprising greater than or equal to 80 atomic % silver and less than or equal to 20 atomic % copper, having a thickness less than or equal to 10 nm, having a sheet resistance less than or equal to 20 Ohm / square, the first continuous metal film being substantially transparent to the wavelength range; a first conductive layer disposed on the first side of the first continuous metal film, wherein the first conductive layer comprises a conductive dielectric material selected from the group consisting of indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly(3,4-ethylenedioxythiophene), and mixtures thereof; a second conductive layer disposed on the opposite second side of the first continuous metal film, wherein the second conductive layer comprises a conductive dielectric material selected from the group consisting of indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly(3,4-ethylenedioxythiophene), and mixtures thereof; A second flexible stack, the second flexible stack comprising: a second continuous metal film, the second continuous metal film defining a first side and an opposite second side, and the second continuous metal film comprises greater than or equal to 80 atomic % silver and less than or equal to 20 atomic % copper, has a thickness less than or equal to 10 nm, has a sheet resistance less than or equal to 20 Ohm / square, the second continuous metal film being substantially transparent to the wavelength range; a third layer disposed on the first side of the second continuous metal film, wherein the third layer comprises a conductive dielectric material selected from the group consisting of indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly(3,4-ethylenedioxythiophene), and mixtures thereof; a fourth layer disposed on the opposite second side of the second continuous metal film, wherein the fourth layer comprises a conductive dielectric material selected from the group consisting of indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly(3,4-ethylenedioxythiophene), and mixtures thereof; and A spacer layer includes a dielectric material disposed between the first flexible stack and the second flexible stack.

15. The method according to claim 14, wherein: The spacer layer has a thickness corresponding to a quarter of a peak wavelength of electromagnetic radiation in a frequency range of greater than or equal to 800 MHz to less than or equal to 90 GHz.

16. The method according to claim 14, wherein: The shielding efficiency is greater than or equal to 30 dB, and the average visible transmission efficiency is greater than or equal to 80%.

17. The method according to claim 14, wherein: The shielding efficiency is greater than or equal to 50 dB, and the average visible transmission efficiency is greater than or equal to 65%.

18. An electromagnetic interference shielding component, comprising: A first flexible stack, the first flexible stack comprising: a first continuous metal film, the first continuous metal film defining a first side and an opposite second side, and the first continuous metal film comprising greater than or equal to 80 atomic % silver and less than or equal to 20 atomic % copper, having a thickness less than or equal to 10 nm, having a sheet resistance less than or equal to 20 Ohm / square, the first continuous metal film being substantially transparent to a wavelength range within the visible range of greater than or equal to 390 nm to less than or equal to 740 nm; a first conductive layer disposed on the first side of the first continuous metal film, wherein the first conductive layer comprises a conductive dielectric material selected from the group consisting of indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly(3,4-ethylenedioxythiophene), and mixtures thereof; a second conductive layer disposed on the opposite second side of the first continuous metal film, wherein the second conductive layer comprises a conductive dielectric material selected from the group consisting of indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly(3,4-ethylenedioxythiophene), and mixtures thereof; A second flexible stack, the second flexible stack comprising: a second continuous metal film, the second continuous metal film defining a first side and an opposite second side, and the second continuous metal film comprising greater than or equal to 80 atomic % silver and less than or equal to 20 atomic % copper, having a thickness less than or equal to 10 nm, having a sheet resistance less than or equal to 20 Ohm / square, the second continuous metal film being substantially transparent to a wavelength range within the visible range of greater than or equal to 390 nm to less than or equal to 740 nm; a third layer disposed on the first side of the second continuous metal film, wherein the third layer comprises a conductive dielectric material selected from the group consisting of indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly(3,4-ethylenedioxythiophene), and mixtures thereof; a fourth layer disposed on the opposite second side of the second continuous metal film, wherein the fourth layer comprises a conductive dielectric material selected from the group consisting of indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly(3,4-ethylenedioxythiophene), and mixtures thereof; and A spacer layer includes a dielectric material disposed between the first flexible stack and the second flexible stack.

19. An electromagnetic interference shielding component, comprising: a continuous metal film defining a first side and an opposite second side, and comprising greater than or equal to 80 atomic % silver and less than or equal to 20 atomic % copper, having a thickness less than or equal to 10 nm, having a sheet resistance less than or equal to 20 Ohm / square; a first conductive layer disposed in contact with the first side of the continuous metal film, wherein the first conductive layer comprises a conductive dielectric material selected from the group consisting of indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly(3,4-ethylenedioxythiophene), and mixtures thereof; and a second conductive layer disposed in contact with the opposite second side of the continuous metal film, wherein the second conductive layer comprises a conductive dielectric material selected from the group consisting of indium tin oxide, aluminum tin oxide, indium zinc oxide, fluorine-doped tin oxide, poly(3,4-ethylenedioxythiophene), and mixtures thereof; and a spacer layer comprising a dielectric material adjacent to the second conductive layer; and A graphene layer is adjacent to the spacer layer.

20. The electromagnetic interference shielding component according to claim 19 further comprises an electrical gating system, the electrical gating system comprising a first terminal, a second terminal and a voltage source, the first terminal being electrically connected to the graphene layer, the second terminal being electrically connected to the continuous metal film, and the voltage source being electrically connected to the first terminal and the second terminal.

21. The electromagnetic interference shield of claim 19, wherein: The graphene layer includes at least one dopant.

22. The electromagnetic interference shield of claim 19, wherein: The spacer layer has a thickness corresponding to a quarter of a peak wavelength of electromagnetic radiation in a frequency range of greater than or equal to 800 MHz to less than or equal to 90 GHz.

23. The electromagnetic interference shield of claim 19, wherein: The continuous metal film has a thickness less than or equal to 10 nm, the first conductive layer has a thickness less than or equal to 45 nm, and the second conductive layer has a thickness less than or equal to 45 nm.

24. The electromagnetic interference shield of claim 19, wherein: The shielding efficiency of the electromagnetic interference shielding device is greater than or equal to 30dB. The electromagnetic interference shielding device is used to block the frequency range greater than or equal to 800MHz to less than or equal to 90GHz to achieve a shielding efficiency greater than or equal to 20dB, and the average transmission efficiency of the electromagnetic interference shielding device for the wavelength range in the visible range greater than or equal to 390nm to less than or equal to 740nm is greater than or equal to 80%.

25. The electromagnetic interference shield of claim 19, wherein: The graphene layer is a first graphene layer, and the electromagnetic interference shield further includes a second graphene layer.

26. A method for broadband electromagnetic shielding, the method comprising: An electromagnetic shielding component is arranged in the transmission path of electromagnetic radiation to block the frequency range of greater than or equal to 800Mhz to less than or equal to 90GHz to achieve a shielding efficiency greater than or equal to 30dB, and a wavelength range within the visible range of greater than or equal to 390nm to less than or equal to 740nm is transmitted through the electromagnetic shielding component to achieve an average transmission efficiency greater than or equal to 80%, wherein the electromagnetic shielding component comprises: a continuous metal film, the continuous metal film defining a first side and an opposite second side, and the continuous metal film comprising greater than or equal to 80 atomic % of silver Ag and less than or equal to 20 atomic % of copper Cu, having a thickness less than or equal to 10 nm, and having a sheet resistance less than or equal to 20 Ohm / square; a first conductive layer disposed in contact with the first side of the continuous metal film, wherein the first conductive layer comprises a conductive material selected from the group consisting of: indium tin oxide, aluminum zinc oxide AZO, indium zinc oxide IZO, fluorine-doped tin oxide FTO, poly (3,4-ethylenedioxythiophene) PEDOT, and mixtures thereof; and a second conductive layer disposed in contact with the opposite second side of the continuous metal film, wherein the second conductive layer comprises a conductive material selected from the group consisting of: indium tin oxide, aluminum zinc oxide AZO, indium zinc oxide IZO, fluorine-doped tin oxide FTO, poly (3,4-ethylenedioxythiophene) PEDOT, and mixtures thereof; and a spacer layer comprising a dielectric material adjacent to the second conductive layer; and A graphene layer is adjacent to the spacer layer.