Negative electrode for non-aqueous electrolyte secondary battery
By using aromatic organic acids with hydroxyl groups and formaldehyde condensates as additives in the negative electrode mixture layer of the nonaqueous electrolyte secondary battery, the problem of reducing conductivity caused by the combination of carbon materials and Si-containing materials is solved, and the initial charge is significantly improved Discharge efficiency and cycle capacity maintenance.
Patent Information
- Application Number
- CN202080018545.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-28
- Filing Date
- 2020-02-17
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-02-17
AI Technical Summary
In a nonaqueous electrolyte secondary battery, the combination of carbon material and Si-containing material leads to large volume changes during charging and discharging, a decrease in conductive paths, resulting in a decrease in conductivity of the negative electrode mixture layer and a decrease in the initial charge and discharge efficiency.
The negative electrode mixture layer is added with aromatic organic acids with hydroxyl groups and/or formaldehyde condensate as additives, and a stable conductive path is formed with a carbon material and a Si-containing material to suppress the reduction of conductivity and improve the charge and discharge efficiency.
The reduction of the initial charge and discharge efficiency is effectively suppressed, and high efficiency is maintained during the charge and discharge cycle, thereby improving the capacity maintenance rate.
Smart Images

Figure CN113557615B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode for a non-aqueous electrolyte secondary battery comprising a carbon material and a Si-containing material. Background Art
[0002] Non-aqueous electrolyte secondary batteries, especially lithium-ion secondary batteries, have high voltage and high energy density, and therefore are expected to be used as power sources for small civilian applications, power storage devices, and electric vehicles. In the process of requiring high energy density of batteries, materials containing silicon (silicon (Si)) alloyed with lithium are expected to be used as negative electrode active materials with high theoretical capacity density.
[0003] On the other hand, Patent Document 1 proposes an active material for a negative electrode of a non-aqueous secondary battery, which contains: an active material (A) capable of inserting / extracting lithium ions, and an organic compound (B), wherein the organic compound (B) is poorly soluble in a non-aqueous electrolyte, has a π-conjugated structure, and has an electrical conductivity of 0.1 S / cm or less at 25° C. It is said that the organic compound (B) inhibits the reaction between the active material (A) and the non-aqueous electrolyte, and can effectively inhibit the generation of gas.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2013-122115 Pamphlet Summary of the invention
[0007] Problem that the invention aims to solve
[0008] When a carbon material and a Si-containing material are used in combination, the volume change of the Si-containing material accompanying charge and discharge is large, so the conductive path between the carbon material and the Si-containing material is reduced, and there is a tendency for the conductivity of the negative electrode mixture layer to decrease. If the content of the Si-containing material in the negative electrode mixture layer becomes 1% by mass or more, the conductive path is significantly reduced, and the initial charge and discharge efficiency is likely to decrease.
[0009] Solutions for solving problems
[0010] In view of the above, one aspect of the present invention relates to a negative electrode for a non-aqueous electrolyte secondary battery, which comprises a negative electrode mixture layer, wherein the negative electrode mixture layer comprises a negative electrode active material and a negative electrode additive, the negative electrode active material comprises a carbon material and a Si-containing material, the content of the Si-containing material in the negative electrode mixture layer is greater than 1% by mass, and the negative electrode additive comprises a formaldehyde condensate of an aromatic organic acid having a hydroxyl group and / or an aromatic organic acid salt having a hydroxyl group.
[0011] Effects of the Invention
[0012] A decrease in the initial charge and discharge efficiency of the nonaqueous electrolyte secondary battery is suppressed.
[0013] The novel features of the present invention are described in the appended claims, but the present invention, both as to the configuration and content, together with other objects and features of the present invention, will be better understood from the following detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a partially cutaway schematic perspective view of a nonaqueous electrolyte secondary battery according to one embodiment of the present invention. DETAILED DESCRIPTION
[0015] The non-aqueous electrolyte secondary battery negative electrode of the embodiment of the present invention is provided with a negative electrode mixture layer, wherein the negative electrode mixture layer comprises a negative electrode active material and a negative electrode additive. The negative electrode active material comprises a carbon material and a Si-containing material. The content of the Si-containing material in the negative electrode mixture layer is 1% by mass or more. By making the content of the Si-containing material 1% by mass or more, a significant improvement in the theoretical capacity of the negative electrode can be expected.
[0016] The content of the Si-containing material in the negative electrode mixture layer can be 1% by mass or more. From the perspective of improving the theoretical capacity of the negative electrode, the higher the content of the Si-containing material, the more ideal it is. It can be set to 5% by mass or more, or 10% by mass or more, and further 15% by mass or more. However, the volume change of the Si-containing material accompanying charge and discharge is large, so it is difficult to use it alone as a negative electrode active material.
[0017] By using a carbon material and a Si-containing material in combination, the volume change of the entire negative electrode mixture layer can be greatly alleviated. The content of the Si-containing material in the negative electrode mixture layer is, for example, preferably 15% by mass or less. That is, the content of the Si-containing material contained in the negative electrode mixture layer is preferably 1% by mass or more and 15% by mass or less, and more preferably 5% by mass or more and 10% by mass or less.
[0018] When a carbon material and a Si-containing material are used in combination in the negative electrode mixture layer, the initial charge and discharge efficiency tends to decrease when the Si-containing material increases. This is believed to be because when the Si-containing material that expands by charging shrinks by discharging, pores are formed around the Si-containing material. By forming pores, sometimes the contact points between the Si-containing material and the surrounding carbon material (that is, the conductive path between the carbon material and the Si-containing material) are reduced, and a part of the Si-containing material is isolated. Isolated Si-containing materials are difficult to discharge.
[0019] (Formaldehyde condensation product)
[0020] When the negative electrode mixture layer contains a formaldehyde condensate (hereinafter, also referred to as formaldehyde condensate) of an aromatic organic acid having a hydroxyl group and / or an aromatic organic acid salt having a hydroxyl group (hereinafter, also referred to as an aromatic organic acid (salt) having a hydroxyl group), the reduction of the conductive path between the carbon material and the Si-containing material is suppressed. The formaldehyde condensate generally has a structure in which the aromatic rings of an aromatic compound are cross-linked with methylene groups. Here, the formaldehyde condensate has a structure in which an aromatic organic acid (salt) having a hydroxyl group is cross-linked with methylene groups. The hydroxyl group is preferably a phenolic hydroxyl group bonded to the aromatic ring. The number of hydroxyl groups bonded to the aromatic ring is not limited, and is preferably 1 or 2.
[0021] The formaldehyde condensate may be a condensate containing either an aromatic organic acid having a hydroxyl group or an aromatic organic acid salt having a hydroxyl group, or may be a condensate containing both an aromatic organic acid having a hydroxyl group and an aromatic organic acid salt having a hydroxyl group.
[0022] In the formaldehyde condensate, the organic acid group and / or the organic acid salt group are beneficial to the improvement of the solubility of the formaldehyde condensate in the negative electrode slurry and the improvement of the electrochemical stability. In addition, the aromatic ring has a π-conjugated structure, and therefore has a high affinity with the carbon material, and can be firmly bonded to the carbon material such as graphite used as the negative electrode active material and the carbon material used as the conductive auxiliary agent. In addition, the hydroxyl group bonded to the aromatic ring can form a hydrogen bond with the hydroxyl group (such as a silanol group) present on the surface of the Si-containing material, and therefore has a high affinity with the Si-containing material and can be firmly bonded to the Si-containing material. As mentioned above, the formaldehyde condensate has the function of connecting the carbon material and the Si-containing material and assisting the adhesion of the two. As a result, after the initial charge and discharge, it is also easy to maintain the conductive path between the carbon material and the Si-containing material, and the reduction in charge and discharge efficiency is suppressed. In addition, not only the initial charge and discharge efficiency is greatly improved, but also the capacity retention rate is greatly improved at the beginning of the charge and discharge cycle.
[0023] It should be noted that the organic acid group and / or organic acid salt group has a strong electron-withdrawing O=S=O group, C=O group, etc., and therefore is considered to be basically unfavorable for hydrogen bonding with the surface hydroxyl group of the Si-containing material.
[0024] Organic acid refers to an organic compound with an ionic group that releases protons in water and can generate anions. Examples of ionic groups include sulfonic acid groups, carboxylic acid groups, phosphoric acid groups, phosphonic acid groups, etc. In addition, organic acid salts refer to salts with a structure obtained by replacing the protons of the ionic groups of the above-mentioned organic acids with metal cations, and examples include lithium salts, sodium salts, potassium salts, ammonium salts, calcium salts, magnesium salts, etc. Among them, the ionic group can exist in the form of anions in the battery. Among organic acids, sulfonic acids are preferred in terms of excellent solubility, stability, etc., and organic acid salts are preferably sulfonic acids, and organic acid salts are preferably sulfonates, etc.
[0025] Specific examples of the aromatic ring possessed by the aromatic organic acid include aromatic rings having skeletons such as furan, pyrrole, imidazole, thiophene, phosphotrimethylene, pyrazole, oxazole, isoxazole, thiazole, benzene, pyridine, pyrazine, pyrimidine, pyridazine, triazine, benzofuran, isobenzofuran, indole, isoindole, benzothiophene, benzophosphotrimethylene, benzimidazole, purine, indazole, benzoxazole, benzisoxazole, benzothiazole, naphthalene, quinoline, isoquinoline, quinoxaline, quinazoline, cinnoline, anthracene, and pyrene. Among these, aromatic rings having skeletons such as benzene and naphthalene are preferred in view of the ease of availability.
[0026] As specific examples of aromatic organic acids and salts thereof (hereinafter, also referred to as organic acids (salts), etc.) having a hydroxyl group, phenolsulfonic acid (salt), salicylic acid (salt), phthalic acid (salt), cresolsulfonic acid (salt), naphtholsulfonic acid (salt), catecholsulfonic acid (salt), benzyl alcoholsulfonic acid (salt), aminonaphtholsulfonic acid (salt), ligninsulfonic acid (salt), etc. can be cited. In addition, salts can include sodium salts, lithium salts, potassium salts, ammonium salts, calcium salts, magnesium salts, etc. Among them, phenolsulfonates (such as Na phenolsulfonic acid, Li phenolsulfonic acid, etc.) are preferred in terms of easy and cheap acquisition, and preferably 10 mol% or more, and further 30 mol% or more (such as 50 mol% or more) of the units of the aromatic compound constituting the formaldehyde condensate are at least one selected from the group consisting of sodium phenolsulfonate and lithium phenolsulfonate. The formaldehyde condensate can be used alone or in combination of two or more.
[0027] The formaldehyde condensate may contain an aromatic compound other than an aromatic organic acid (salt) having a hydroxyl group as an aromatic compound unit. That is, the formaldehyde condensate may be a copolymer of an aromatic organic acid (salt) having a hydroxyl group and an aromatic compound not having at least one of the above-mentioned ionic group and hydroxyl group. It is desirable that 20 mol% or more, and further 50 mol% or more (e.g. 80 mol% or more) of the aromatic compounds constituting the formaldehyde condensate be an aromatic organic acid (salt) having a hydroxyl group.
[0028] Examples of the aromatic compound having no at least one of an ionic group and a hydroxyl group include aniline, anilinesulfonic acid, benzoic acid, naphthalene, anthracene, phenanthrene, toluene, ethylbenzene, xylene, styrene, and cumene.
[0029] The weight average molecular weight of the formaldehyde condensate can be, for example, 1000 or more and 1,000,000 or less, 2000 or more and 500,000 or less, or 2500 or more and 300,000 or less (e.g., 200,000 or less). It should be noted that the weight average molecular weight refers to the weight average molecular weight measured by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent and calculated as standard polystyrene, or the weight average molecular weight measured by GPC using water, dimethylformamide (DMF) or dimethyl sulfoxide (DMSO) as a solvent and calculated as standard polyethylene glycol.
[0030] In addition, the structural formula of the formaldehyde condensate of sodium phenolsulfonate is shown below as a suitable example of the formaldehyde condensate.
[0031]
[0032] The content of the formaldehyde condensate in the negative electrode mixture layer may be, for example, 0.01 mass % to 10 mass % in consideration of the balance between the high capacity of the negative electrode and the initial charge and discharge efficiency, and may be 5 mass % to 7 mass %.
[0033] (Negative electrode active material)
[0034] The negative electrode active material refers to a material contained in the negative electrode and capable of electrochemically storing and releasing lithium ions. Here, the negative electrode active material includes a carbon material and a Si-containing material, each of which can electrochemically store and release lithium ions.
[0035] As the Si-containing material, for example, a lithium ion conductive phase and Si particles dispersed in the lithium ion conductive phase are included. The lithium ion conductive phase can be at least one selected from the group consisting of a silicon oxide phase, a silicate phase, and a carbon phase. Specifically, as the Si-containing material, for example, at least one selected from the group consisting of the following first composite material, second composite material, and third composite material can be used.
[0036] <First composite material>
[0037] The first composite material includes a silicon oxide phase and first Si particles dispersed in the silicon oxide phase. The first composite material is excellent in terms of high stability and small volume change in the Si-containing material. It is believed that the high stability is due to the small particle size of the first Si particles dispersed in the silicon oxide phase, and deep charging is not easy to carry out. In addition, the silicon oxide phase has a tendency to capture more sites of lithium ions irreversibly, and the irreversible capacity in the Si-containing material becomes larger. In other words, the first composite material can have a large irreversible capacity compared to the second composite material. It is believed that the capture of lithium ions based on the silicon oxide phase is also beneficial to improve the structural stability of the first composite material and suppress volume changes.
[0038] The first composite material can be obtained, for example, by heating silicon oxide in a non-oxidizing atmosphere with an inert gas such as argon to carry out a disproportionation reaction. In the disproportionation reaction, Si microcrystals can be uniformly formed in the silicon oxide phase. The size of the Si particles formed by the disproportionation reaction is small. For example, the average particle size can be less than 100 nm, or can be in the range of 5 nm to 50 nm. The main component of the silicon oxide phase (e.g., 95 to 100% by mass) can be silica. That is, the first composite material can contain an SiO2 phase and first Si particles dispersed in the SiO2 phase. In this case, the first composite material as a whole can be represented by the general formula SiO x It is sufficient that the range of the x value is 0 < x < 2, preferably 0.9 ≤ x ≤ 1.1, or x = 1.
[0039] The average particle size of the first composite material is sufficient to be 1 to 20 μm, preferably 5 to 12 μm. Within the above particle size range, it is easy to relieve the stress generated by the volume change of the Si-containing material accompanied by charge and discharge, and it becomes easy to obtain good cycle characteristics.
[0040] <The second composite material>
[0041] The second composite material contains a silicate phase and second Si particles dispersed in the silicate phase.
[0042] The silicate phase only needs to contain, for example, at least one selected from the group consisting of Group 1 elements and Group 2 elements of the long-period form of the periodic table. As the Group 1 elements and Group 2 elements of the long-period form of the periodic table, for example, lithium (Li), potassium (K), sodium (Na), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), etc. can be used. As other elements, aluminum (Al), boron (B), lanthanum (La), phosphorus (P), zirconium (Zr), titanium (Ti), etc. can also be contained. Among them, from the aspect of small irreversible capacity and high initial charge-discharge efficiency, a silicate phase containing lithium (hereinafter also referred to as a lithium silicate phase) is preferred. That is, the second composite material can contain a lithium silicate phase and second Si particles dispersed in the lithium silicate phase. The second composite material containing a lithium silicate phase and second Si particles dispersed in the lithium silicate phase is also hereinafter referred to as LSX.
[0043] The lithium silicate phase may be simply an oxide phase containing lithium (Li), silicon (Si), and oxygen (O), and may also contain other elements. The atomic ratio of O to Si in the lithium silicate phase: O / Si is, for example, greater than 2 and less than 4. In this case, it is advantageous in terms of stability and lithium ion conductivity. Preferably, O / Si is greater than 2 and less than 3. The atomic ratio of Li to Si in the lithium silicate phase: Li / Si is, for example, greater than 0 and less than 4. Examples of elements other than Li, Si, and O that can be contained in the lithium silicate phase include iron (Fe), chromium (Cr), nickel (Ni), manganese (Mn), copper (Cu), molybdenum (Mo), zinc (Zn), aluminum (Al), etc.
[0044] The lithium silicate phase may have a composition represented by the formula: Li 2z SiO 2+z (0 < z < 2). From the viewpoints of stability, ease of production, lithium ion conductivity, etc., z preferably satisfies the relationship 0 < z < 1, and more preferably z = 1 / 2.
[0045] <The Third Composite Material>
[0046] The third composite material contains a carbon phase and third Si particles dispersed in the carbon phase (hereinafter, the third composite material is also referred to as an Si-C material).
[0047] The carbon phase can be constituted by, for example, low-crystallinity amorphous carbon (i.e., non-crystalline carbon). The amorphous carbon can be, for example, hard carbon, soft carbon, or others. The amorphous carbon can be obtained, for example, by sintering a carbon source in an inert atmosphere and pulverizing the obtained sintered body. The Si-C material can be obtained, for example, by mixing a carbon source and Si particles, crushing the mixture while stirring in a mixer such as a ball mill, and then roasting the mixture in an inert atmosphere. As the carbon source, for example, carboxymethyl cellulose (CMC), polyvinylpyrrolidone, cellulose, sugars such as sucrose, water-soluble resins, etc. can be used. When mixing the carbon source and Si particles, for example, the carbon source and Si particles can be dispersed in a dispersion medium such as alcohol.
[0048] The content of the second Si particles contained in the second composite material and the content of the third Si particles contained in the third composite material can each independently be, for example, 40% by weight or more and 80% by weight or less. Thereby, it becomes easy to balance the high-capacity of the battery and the improvement of the cycle characteristics. Different from the first composite material whose manufacturing method is limited, in the second and third composite materials, the content of the second Si particles and the third Si particles can be arbitrarily changed, so the design of the high-capacity negative electrode is easy. By using the first composite material in combination with the second and / or third composite materials and controlling the distribution in these negative electrode binder layers, when improving the utilization rate of Si, it also becomes possible to balance good cycle characteristics and high capacity.
[0049] The second and third composite materials are excellent in that the irreversible capacity is small. This is because the silicate phase and the carbon phase have few sites for irreversibly capturing lithium ions. By using the second and / or third composite materials, it is possible to obtain excellent charge and discharge efficiency. In particular, the effect is significant at the beginning of charge and discharge.
[0050] The average particle size of the second and third Si particles is independently, for example, less than 500nm, less than 400nm, or less than 200nm. The second Si particles have such a large average particle size, so that it becomes easy to increase the capacity of the second and third composite materials. On the other hand, if it is less than 500nm, the volume change of the second and third Si particles during charge and discharge becomes smaller, and the structural stability of the second and third composite materials is improved. Here, the average particle size of the second and third Si particles is at least the value after the initial charge.
[0051] The Si particles dispersed in the silicate phase and / or the carbon phase are usually composed of a plurality of crystallites. The crystallite size of the Si particles is preferably, for example, less than 30 nm. In this case, the volume change caused by the expansion and contraction of the Si particles accompanying charge and discharge can be minimized, and therefore, the cycle characteristics can be further improved. For example, when the Si particles shrink, pores are formed around the Si particles, the isolation of the Si particles caused by the reduction of the contact points between the Si particles and their surroundings is suppressed, and the reduction in charge and discharge efficiency is suppressed. The lower limit of the crystallite size of the Si particles is not particularly limited, for example, it is greater than 5 nm. The crystallite size can be greater than 10 nm and less than 30 nm, or it can be greater than 15 nm and less than 25 nm.
[0052] The average particle size of the second and third composite materials may be independently 1 to 20 μm, and may be 5 to 12 μm. Within the above particle size range, stress generated by volume change of the Si-containing material accompanying charge and discharge is easily alleviated, and good cycle characteristics are easily obtained.
[0053] The content of Si particles contained in each Si-containing material (each composite material) can be measured by Si-NMR. Desirable measurement conditions of Si-NMR are shown below.
[0054] Measuring device: Varian, solid-state nuclear magnetic resonance spectrometer (INOVA-400)
[0055] Probe: Varian 7mm CPMAS-2
[0056] MAS: 4.2kHz
[0057] MAS speed: 4kHz
[0058] Pulse: DD (45° pulse + signal collection time 1H decoupling)
[0059] Repeat time: 1200 seconds
[0060] Observation amplitude: 100kHz
[0061] Observation center: around -100ppm
[0062] Signal collection time: 0.05 seconds
[0063] Cumulative number of times: 560
[0064] Sample volume: 207.6 mg
[0065] The average particle size of Si particles contained in each Si-containing material (each composite material) can be measured from a cross-sectional SEM (scanning electron microscope) photograph of the Si-containing material. Specifically, the average particle size of Si particles is obtained by averaging the maximum diameters of any 100 Si particles.
[0066] The crystallite size of each Si particle was calculated based on the Scherrer equation from the half-value width of the diffraction peak attributed to the Si (111) plane in the X-ray diffraction (XRD) spectrum of the Si particles.
[0067] The average particle size of each Si-containing material (each composite material) refers to the particle size (volume average particle size) at which the volume cumulative value is 50% in the particle size distribution measured by laser diffraction scattering. For example, the measuring device used can be "LA-750" manufactured by HORIBA.
[0068] It should be noted that the composition of the second composite material can be analyzed by, for example, the following method.
[0069] The battery is disassembled, the negative electrode is taken out, and after cleaning and drying with a non-aqueous solvent such as ethylene carbonate, the cross-section of the negative electrode mixture layer is processed using a cross-section polisher (CP) to obtain a sample. A field emission scanning electron microscope (FE-SEM) is used to obtain a reflected electron image of the sample cross section and observe the cross section of the second composite material. The observed second composite material can be qualitatively and quantitatively analyzed using an AES analysis device (accelerating voltage 10 kV, beam current 10 nA).
[0070] For example, if Li 2z SiO 2+z The LSX shown in FIG. 1 can be used to determine the ratio of 2z to (2+z) from the obtained lithium (Li) content and oxygen (O) content.
[0071] It should be noted that in the cross-sectional observation and analysis of the sample, a carbon sample stand may be used to fix the sample in order to prevent the diffusion of Li. In order to prevent the cross-sectional quality of the sample from being deteriorated, a transfer container may be used to hold the sample without exposing it to the atmosphere.
[0072] The Si-containing material may include a conductive material covering at least a portion of its surface. Among them, the LSX material, which is a silicate phase that is a lithium ion conductive phase and lacks electron conductivity, is preferably coated with a conductive material on the surface of the LSX material to improve conductivity.
[0073] <Carbon materials>
[0074] Compared with Si-containing materials, carbon materials have a smaller degree of expansion and contraction during charge and discharge, so by using them in combination with Si-containing materials, it is easy to improve the cycle characteristics of the battery. The content of carbon material (excluding the carbon phase as a lithium ion conductive phase) in the negative electrode active material can be, for example, 85% by mass or more and 99% by mass or less. That is, the content of Si-containing material in the negative electrode active material can be 1% by mass or more and 15% by mass or less. As a result, it becomes easy to take into account both high capacity and improved cycle characteristics.
[0075] As carbon materials, for example, graphite, easily graphitized carbon (soft carbon), and difficultly graphitized carbon (hard carbon) can be exemplified. Among them, graphite with excellent charge and discharge stability and small irreversible capacity is preferred. Graphite refers to a material having a graphite-type crystal structure, such as natural graphite, artificial graphite, and graphitized mesophase carbon particles. One carbon material can be used alone or in combination of two or more.
[0076] The ratio of the mass Wc of the carbon material contained in the negative electrode mixture layer to the mass Ws of the Si-containing material contained in the negative electrode mixture layer: Wc / Ws may be, for example, 9.5 to 99, and may be 6.3 to 99. The carbon phase of the third composite material is not included in the mass Wc of the carbon material.
[0077] Next, the secondary battery according to the embodiment of the present invention is described in detail. The secondary battery includes, for example, the following negative electrode, positive electrode, and non-aqueous electrolyte.
[0078] [negative electrode]
[0079] The negative electrode contains a negative electrode active material that can electrochemically absorb and release lithium ions. The negative electrode includes a negative electrode collector and a negative electrode mixture layer. The negative electrode mixture layer can be formed, for example, as follows: a negative electrode slurry in which a negative electrode mixture containing a negative electrode active material is dispersed in a dispersion medium is applied to the surface of the negative electrode collector and dried. The dried coating can be rolled as needed. The negative electrode mixture layer can be formed on one surface of the negative electrode collector or on both surfaces.
[0080] The negative electrode mixture contains a negative electrode active material as an essential component, and may contain a binder, a conductive aid, a thickener, etc. as optional components.
[0081] As the negative electrode current collector, a non-porous conductive substrate (metal foil, etc.) or a porous conductive substrate (sieve, mesh, punching sheet, etc.) is used. As the material of the negative electrode current collector, stainless steel, nickel, nickel alloy, copper, copper alloy, etc. can be exemplified. The thickness of the negative electrode current collector is not particularly limited, and is, for example, 1 to 50 μm, and can be 5 to 20 μm.
[0082] As the binder, there can be exemplified resin materials, for example, fluororesins such as polytetrafluoroethylene and polyvinylidene fluoride (PVDF); polyolefin resins such as polyethylene and polypropylene; polyamide resins such as aramid resins; polyimide resins such as polyimide and polyamideimide; acrylic resins such as polyacrylic acid, polymethyl acrylate, and ethylene-acrylic acid copolymer; vinyl resins such as polyacrylonitrile and polyvinyl acetate; polyvinyl pyrrolidone; polyether sulfone; rubber-like materials such as styrene-butadiene copolymer rubber (SBR), etc. These can be used alone or in combination of two or more.
[0083] As the conductive auxiliary agent, for example, carbon black such as acetylene black, carbon nanotubes (hereinafter, also referred to as CNT), metal fibers, carbon fluoride, metal powder, zinc oxide, conductive whiskers such as potassium titanate, conductive metal oxides such as titanium oxide, organic conductive materials such as phenylene derivatives, etc. can be exemplified. These can be used alone or in combination of two or more.
[0084] Among the conductive aids, CNT is suitable as a conductive aid used in combination with a Si-containing material. CNT is fibrous, so when the Si-containing material expanded by charging shrinks due to discharge, when pores are formed around the Si-containing material, it is also effective to ensure the contact between the Si-containing material and the carbon material. In addition, the formaldehyde condensate has a high affinity with both CNT and the negative electrode active material. Therefore, by using CNT, the effect of suppressing the reduction of the conductive path in the negative electrode mixture layer is particularly significantly improved. It is believed that the formaldehyde condensate not only ensures the contact between the Si-containing material and the carbon material, but also plays a role in strengthening the conductive path between CNT and the negative electrode active material.
[0085] From the viewpoint of ensuring a better conductive path, the average length of CNTs may be, for example, 1 μm to 100 μm, preferably 3 μm to 10 μm. Similarly, the average diameter of CNTs may be, for example, 1 nm to 30 nm, preferably 1 nm to 5 nm.
[0086] The average length and average diameter of CNTs were obtained by image analysis using a scanning electron microscope (SEM). Specifically, 50 CNTs were randomly selected, and their lengths and diameters were measured and averaged. It should be noted that the length of CNTs refers to the length when the CNTs are deformed into a straight line.
[0087] The content of CNT in the negative electrode mixture can be, for example, 0.01 mass % to 1.0 mass %, or 0.1 mass % to 0.4 mass %. In this case, not only the effect of suppressing the reduction of the initial charge and discharge efficiency can be improved, but also the charge and discharge cycle characteristics can be significantly improved.
[0088] [positive electrode]
[0089] The positive electrode contains a positive electrode active material that can electrochemically absorb and release lithium ions. The positive electrode, for example, has a positive electrode collector and a positive electrode mixture layer formed on the surface of the positive electrode collector. The positive electrode mixture layer can be formed as follows: a positive electrode slurry in which a positive electrode mixture is dispersed in a dispersion medium is applied to the surface of the positive electrode collector and dried. The dried coating can be rolled as needed. The positive electrode mixture layer can be formed on one surface of the positive electrode collector or on both surfaces. The positive electrode mixture contains a positive electrode active material as an essential component and can contain a binder, a conductive agent, etc. as arbitrary components.
[0090] As the positive electrode active material, for example, a lithium-containing composite oxide can be used. For example, Li a CoO2、Li a NiO2、Li a MnO2、Li a Co b Ni 1-b O2、Li a Co b M 1-b O c , Li a Ni 1-b M b O c , Li a Mn2O4、Li a Mn 2-b M b O4, LiMPO4, Li2MPO4F (M is at least one selected from the group consisting of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B). Here, a=0 to 1.2, b=0 to 0.9, and c=2.0 to 2.3. It should be noted that the value a representing the molar ratio of lithium increases or decreases according to charge and discharge.
[0091] Among them, Li is preferred a Ni b M 1-b O2 (M is at least one selected from the group consisting of Mn, Co, and Al, 0 < a ≤ 1.2, 0.3 ≤ b ≤ 1), a lithium nickel composite oxide. From the viewpoint of high capacity, it is more preferable to satisfy 0.85 ≤ b ≤ 1. From the viewpoint of the stability of the crystal structure, it is further preferable to include Co and Al as M in Li a Ni b Co c Al d O2 (0 < a ≤ 1.2, 0.85 ≤ b < 1, 0 < c < 0.15, 0 < d ≤ 0.1, b + c + d = 1).
[0092] As the binder and the conductive agent, the same substances as those exemplified for the negative electrode can be used. As the conductive agent, graphite such as natural graphite and artificial graphite can be used.
[0093] The shape and thickness of the positive electrode current collector can be selected respectively from the shapes and ranges based on the negative electrode current collector. As the material of the positive electrode current collector, for example, stainless steel, aluminum, aluminum alloy, titanium, etc. can be exemplified.
[0094] [Electrolyte solution]
[0095] The electrolyte solution contains a solvent and an electrolyte salt. As the solvent, a non-aqueous solvent can be used, or water can also be used. The electrolyte salt contains at least a lithium salt.
[0096] The concentration of the lithium salt in the electrolyte solution is preferably, for example, 0.5 mol / L or more and 2 mol / L or less. By controlling the lithium salt concentration within the above range, an electrolyte solution with excellent ionic conductivity and moderate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.
[0097] As the non-aqueous solvent, for example, cyclic carbonates (excluding the unsaturated cyclic carbonates described later), chain carbonates, cyclic carboxylates, chain carboxylates, etc. can be used. As the cyclic carbonate, propylene carbonate (PC), ethylene carbonate (EC), etc. can be cited. As the chain carbonate, diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), etc. can be cited. As the cyclic carboxylate, γ-butyrolactone (GBL), γ-valerolactone (GVL), etc. can be cited. As the chain carboxylate, methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, etc. can be cited. The non-aqueous solvent can be used alone or in combination of two or more.
[0098] Examples of lithium salts include LiClO4, LiBF4, LiPF6, LiAlCl4, LiSbF6, LiSCN, LiCF3SO3, LiCF3CO2, LiAsF6, LiB 10 Cl 10 , lithium lower aliphatic carboxylates, LiCl, LiBr, LiI, borates, imino salts, etc. Examples of borates include lithium bis(1,2-benzenediolate (2-)-O,O')borate, lithium bis(2,3-naphthalenediolate (2-)-O,O')borate, lithium bis(2,2'-biphenylediolate (2-)-O,O')borate, and lithium bis(5-fluoro-2-olate-1-benzenesulfonic acid-O,O')borate. As imino salts, there can be mentioned lithium bis(fluorosulfonyl)imide (LiN(FSO2)2: hereinafter also referred to as LFSI), lithium bis(trifluoromethanesulfonate)imide (LiN(CF3SO2)2), lithium bis(trifluoromethanesulfonate)imide (LiN(CF3SO2)(C4F9SO2)), lithium bis(pentafluoroethanesulfonate)imide (LiN(C2F5SO2)2), etc. Among them, at least one of LiPF6 and LFSI is preferred. The lithium salt can be used alone or in combination of two or more.
[0099] The electrolyte may include additives. As additives, succinic anhydride, maleic anhydride, vinyl sulfite, fluorobenzene, hexafluorobenzene, cyclohexylbenzene (CHB), 4-fluoroethylene carbonate (FEC), lithium bis (oxalate) borate (LiBOB), adiponitrile, pivalonitrile etc. may be used. In addition, the cyclic carbonate (hereinafter referred to as unsaturated cyclic carbonate) having at least one carbon-carbon unsaturated bond in the molecule may also be included.
[0100] As unsaturated cyclic carbonate, for example, vinylene carbonate, 4-methyl vinylene carbonate, 4,5-dimethyl vinylene carbonate, 4-ethyl vinylene carbonate, 4,5-diethyl vinylene carbonate, 4-propyl vinylene carbonate, 4,5-dipropyl vinylene carbonate, 4-phenyl vinylene carbonate, 4,5-diphenyl vinylene carbonate, vinyl ethylene carbonate, divinyl ethylene carbonate etc. can be enumerated. Unsaturated cyclic carbonate can be used alone or in combination of two or more. A part of the hydrogen atom of the unsaturated cyclic carbonate can be substituted by fluorine atoms.
[0101] [Separator]
[0102] Generally, it is desirable to sandwich a separator between the positive electrode and the negative electrode. The separator has high ion permeability and has appropriate mechanical strength and insulation. As the separator, a microporous film, a woven fabric, a non-woven fabric, etc. can be used. As the material of the separator, polyolefins such as polypropylene and polyethylene are preferred.
[0103] As an example of the structure of a secondary battery, the following structure can be cited: an electrode group formed by winding a positive electrode and a negative electrode with a separator interposed therebetween and an electrolyte solution housed in an outer body. Other forms of electrode groups such as a stacked electrode group formed by stacking a positive electrode and a negative electrode with a separator interposed therebetween can also be used. The secondary battery can be in any form, for example, cylindrical, square, coin-shaped, button-shaped, laminated, or the like.
[0104] Below, refer to Figure 1 The structure of a square nonaqueous electrolyte secondary battery as an example of the secondary battery of the present invention will be described. Figure 1 This is a schematic perspective view with a portion of the secondary battery according to one embodiment of the present invention cut away.
[0105] The battery comprises: a battery case 4 having a bottom and a square shape, an electrode group 1 and an electrolyte (not shown) contained in the battery case 4. The electrode group 1 comprises: a long strip-shaped negative electrode; a long strip-shaped positive electrode; and a separator sandwiched between them to prevent direct contact. The electrode group 1 is formed by winding the negative electrode, the positive electrode, and the separator around a flat winding core and pulling out the winding core.
[0106] One end of the negative lead 3 is mounted on the negative electrode collector of the negative electrode by welding or the like. The other end of the negative lead 3 is electrically connected to the negative terminal 6 provided on the sealing plate 5 via a resin insulating plate (not shown). The negative terminal 6 is insulated from the sealing plate 5 by a resin gasket 7. One end of the positive lead 2 is mounted on the positive electrode collector of the positive electrode by welding or the like. The other end of the positive lead 2 is connected to the back of the sealing plate 5 via an insulating plate. That is, the positive lead 2 is electrically connected to the battery case 4 which also serves as the positive terminal. The insulating plate is used to isolate the electrode group 1 from the sealing plate 5 and to isolate the negative lead 3 from the battery case 4. The periphery of the sealing plate 5 is fitted into the opening end of the battery case 4, and the fitting portion is laser welded. The opening of the battery case 4 is sealed by the sealing plate 5. The injection hole for the electrolyte provided in the sealing plate 5 is blocked by the sealing plug 8.
[0107] Hereinafter, the present invention will be specifically described based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0108] (Comparative Example 1)
[0109] [Production of negative electrode]
[0110] As a Si-containing material, SiO with an average particle size of 5 μm was prepared. x (x=1)SiO x The first Si-containing material (SiO2) comprises a SiO2 phase and first Si particles dispersed in the SiO2 phase. x) contained in the first Si particles was 50% by mass. The average particle size of the first Si particles was 20 nm.
[0111] In SiO x The amount of the conductive layer is set to 5% by mass relative to the total mass of the Si-containing material and the conductive layer. Specifically, SiO x Mixed with coal pitch, the mixture was calcined at 800°C in an inert atmosphere to cover the SiO with conductive carbon. x Then, the SiO x The resulting product was pulverized and sieved to adjust the average particle size to 5 μm.
[0112] Preparation of SiO2 containing graphite and having a conductive layer in a mass ratio of 93:7:0.9:0.5:1 x , carboxymethyl cellulose (CMC), polyacrylate lithium (PAAL), styrene butadiene rubber (SBR) negative electrode slurry, then the negative electrode slurry is applied to the surface of the copper foil as the negative electrode collector so that every 1m 2 The mass of the negative electrode mixture was 200 g. After that, the coating was dried and rolled to form a copper foil with a density of 1.5 g / cm 3 A negative electrode mixture layer is formed to obtain a negative electrode.
[0113] [Production of positive electrode]
[0114] Lithium nickel composite oxide (LiNi 0.8 Co 0.18 Al 0.02 O2) was mixed with acetylene black and polyvinylidene fluoride in a mass ratio of 95:2.5:2.5, and N-methyl-2-pyrrolidone (NMP) was added and stirred with a mixer to prepare a positive electrode slurry. Next, the positive electrode slurry was applied to the surface of the aluminum foil, and after the coating was dried, it was rolled to form a film with a density of 3.6 g / cm on both sides of the aluminum foil. 3 The positive electrode of the positive electrode mixture layer.
[0115] [Preparation of electrolyte]
[0116] The electrolyte solution was prepared by dissolving a lithium salt in a non-aqueous solvent. The non-aqueous solvent used was a mixed solvent containing ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and ethylene fluorocarbonate (FEC) in a volume ratio of 20:70:5:5. The lithium salt used was LiPF6. The LiPF6 concentration in the electrolyte solution was set to 1.35 mol / L.
[0117] [Fabrication of non-aqueous electrolyte secondary battery]
[0118] Tabs were attached to each electrode, and the positive electrode and the negative electrode were wound in a spiral shape with the tabs located at the outermost periphery, thereby producing an electrode group. The electrode group was embedded in an outer body made of an aluminum laminate film, vacuum dried at 105° C. for 2 hours, and then injected with an electrolyte solution, and the opening of the outer body was sealed to obtain a battery B1 of Comparative Example 1.
[0119] (Example 1)
[0120] In the negative electrode slurry, graphite, SiO x , CMC, PAAL, SBR and PhSO3Na in a total amount of 0.5% by mass, and further a formaldehyde condensate of sodium phenolsulfonate represented by the following general formula (PhSO3Na: weight average molecular weight 8000) was added as an additive,
[0121]
[0122] Except for the above, a negative electrode was prepared in the same manner as in Comparative Example 1, and a battery A1 was prepared using the negative electrode and evaluated in the same manner.
[0123] (Example 2)
[0124] In the negative electrode slurry, graphite, SiO x , CMC, PAAL, SBR, PhSO3Na and CNT in a total ratio of 0.3 mass % and further adding carbon nanotubes (CNT: average length 10 μm, average diameter 7 nm) as a conductive aid. Apart from this, a negative electrode was prepared in the same manner as in Example 1, and battery A2 was prepared using it and evaluated in the same manner.
[0125] (Comparative Example 2)
[0126] A negative electrode was prepared in the same manner as in Example 1 except that a copolymer of sodium maleate and styrene (RCOONa: weight average molecular weight 8000) as an aliphatic polycarboxylate was added to the negative electrode slurry instead of PhSO3Na. A battery B2 was prepared using the negative electrode and evaluated in the same manner.
[0127] (Comparative Example 3)
[0128] A negative electrode was prepared in the same manner as in Example 1 except that sodium tetradecylsulfonate (TDSO3Na: weight average molecular weight 300) was added to the negative electrode slurry instead of PhSO3Na. A battery B3 was prepared using the negative electrode and evaluated in the same manner.
[0129] (Comparative Example 4)
[0130] A negative electrode was prepared in the same manner as in Example 1 except that a formaldehyde condensate of sodium naphthalenesulfonate (NpSO3Na: weight average molecular weight 23000) was added to the negative electrode slurry instead of PhSO3Na. A battery B4 was prepared using the negative electrode and evaluated in the same manner.
[0131] Each of the batteries produced above was evaluated by the following methods.
[0132] [Evaluation 1: Initial charge and discharge efficiency]
[0133] For each battery after production, a constant current charge is performed at a current of 0.2 It until the voltage reaches 4.2 V in an environment of 25°C, and then a constant voltage charge is performed at a constant voltage of 4.2 V until the current reaches 0.015 It. After that, a constant current discharge is performed at a current of 0.2 It until the voltage reaches 2.75 V. The rest period between charging and discharging is set to 10 minutes. Charging and discharging are performed in an environment of 25°C. The ratio of the initial discharge capacity at this time to the initial charge capacity is calculated as the initial charge and discharge efficiency. Taking the results of battery B1 as the benchmark, the increase rate of each other battery from the benchmark value is shown in Table 1.
[0134] It should be noted that (1 / X)It represents current, (1 / X)It(A) = rated capacity (Ah) / X(h), and X represents the time used to charge or discharge the rated capacity. For example, 0.5It means that X=2, and the current value is the rated capacity (Ah) / 2(h).
[0135] [Evaluation 2: Cycle capacity maintenance rate]
[0136] The charge and discharge conditions were repeated in the same manner as in Evaluation 1, and the ratio (percentage) of the discharge capacity at the 10th cycle to the discharge capacity at the 1st cycle was determined as the 10-cycle capacity retention rate. The increase rates of the other batteries are shown in Table 1, using the results of Battery B1 as a reference.
[0137] [Table 1]
[0138]
[0139] From Table 1, it can be understood that the initial charge and discharge efficiency can be improved specifically by using sodium phenolsulfonate, which is an aromatic organic acid having a hydroxyl group, and the capacity retention rate in the initial cycle can be improved. It can also be understood that the initial cycle characteristics are further improved dramatically by using CNT.
[0140] Industrial Applicability
[0141] The nonaqueous electrolyte secondary battery of the present invention is useful as a main power source for mobile communication equipment, portable electronic equipment, and the like.
[0142] The present invention is described with respect to the present preferred embodiments, but such disclosure is not to be construed in a limiting sense. Various modifications and changes will be apparent to those skilled in the art in the art of the present invention upon reading the above disclosure. Therefore, the appended claims should be construed as including all modifications and changes without departing from the spirit and scope of the present invention.
[0143] Description of Reference Numerals
[0144] 1: electrode group, 2: positive lead, 3: negative lead, 4: battery case, 5: sealing plate, 6: negative terminal, 7: gasket, 8: sealing plug
Claims
1. A negative electrode for a non-aqueous electrolyte secondary battery, comprising a negative electrode mixture layer, wherein the negative electrode mixture layer comprises a negative electrode active material and a negative electrode additive, The negative electrode active material includes a carbon material and a Si-containing material as negative electrode active materials, The Si-containing material comprises a lithium ion conductive phase and Si particles dispersed in the lithium ion conductive phase. The lithium ion conductive phase is at least one selected from the group consisting of a silicon oxide phase, a silicate phase and a carbon phase, In the negative electrode active material, the content of the carbon material as the negative electrode active material is 85 mass % or more and 99 mass % or less, the content of the Si-containing material is 1 mass % or more and 15 mass % or less, and the carbon material as the negative electrode active material excludes the carbon phase as the lithium ion conductive phase, The content of the Si-containing material in the negative electrode mixture layer is 1 mass % or more, The negative electrode additive comprises a formaldehyde condensate of an aromatic organic acid having a hydroxyl group and / or a formaldehyde condensate of an aromatic organic acid salt having a hydroxyl group. The content of the formaldehyde condensate in the negative electrode mixture layer is 0.01 mass % or more and 10 mass % or less.
2. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein The formaldehyde condensate has a weight average molecular weight of 1,000 to 1,000,000.
3. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein The aromatic organic acid having a hydroxyl group is hydroxysulfonic acid.
4. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein The aromatic organic acid salt having a hydroxyl group is a hydroxy sulfonate.
5. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 4, wherein The hydroxysulfonate is at least one selected from the group consisting of sodium hydroxysulfonate and lithium hydroxysulfonate.
6. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein: The content of the Si-containing material contained in the negative electrode mixture layer is 1 mass % to 30 mass %.
7. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein: The silicate phase includes at least one selected from the group consisting of Group 1 elements and Group 2 elements of the long-period periodic table.
8. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein: The negative electrode mixture layer contains carbon nanotubes in a content of 0.01 mass % to 1.0 mass % both inclusive.
Citation Information
Patent Citations
Negative-electrode active material for non-aqueous secondary battery, and negative electrode and non-aqueous secondary battery using said active material
WO2013122115A1
Method for preparing negative electrode plate lead plaster for power type lead acid storage battery
CN103035908A
Active carbon composite anode material for lithium ion battery, preparation method and lithium ion battery
CN106229479A
Manufacturing method of negative plate of safety lithium-ion battery
CN106450169A
Three-dimensional spherical silicon-carbon composite negative electrode material and preparation method therefor
CN107230781A