Electrochemical battery repair method
Through the mechanical removal and cleaning method of semi-solid electrode materials, the cost and environmental issues in the repair and reuse of electrochemical battery electrodes are solved, and the efficient separation and reconstruction of electrode materials are achieved.
Patent Information
- Application Number
- CN202111046904.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2015-06-19
- Filing Date
- 2016-06-20
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2036-06-20
AI Technical Summary
Existing technologies make it difficult to effectively repair and reuse electrochemical cell electrodes, especially in terms of removing residues and separating electrode materials, which pose high economic and environmental costs.
A repair method using semi-solid electrode materials that separates electrode materials through mechanical removal and cleaning to remove residues and separate into multiple components for reuse, avoiding the high cost and environmental impact of chemical treatments.
It achieves low-cost, low-energy input separation and recycling of electrode materials, ensures clean separation and effective reconstruction of active materials, and improves the reusability of electrodes.
Smart Images

Figure CN113594485B_ABST
Abstract
Description
[0001] This patent application is a divisional application based on the Chinese patent application with application date of June 20, 2016, application number 201680048102.8, and invention name “Electrochemical Battery Repair Method”.
[0002] CROSS-REFERENCE TO RELATED APPLICATIONS
[0003] This application claims priority to and the benefit of U.S. Provisional Patent Application Serial No. 62 / 182,241, filed on June 19, 2015, entitled “Methods for Electrochemical Cell Remediation,” the disclosure of which is incorporated herein by reference in its entirety. background Technical Field
[0005] Embodiments described herein generally relate to the remediation of electrochemical cell electrodes. Background Art
[0007] Batteries are typically composed of solid electrodes, separators, electrolytes, and auxiliary components (e.g., related to packaging, thermal management, cell balancing, consolidation of current carriers into terminals), and / or other such components. Battery electrodes typically contain active materials, conductive materials, binders (e.g., polyvinylidene fluoride ("PVDF") and styrene-butadiene rubber ("SBR")), and other additives, which are calendered onto a metal substrate or current collector as a dry solid matrix coating.
[0008] Some known methods for removing conventional electrode coatings involve immersing the coating in a molten salt bath at very high temperatures (e.g., 450° C. or higher). It has been found that such methods can cause damage / corrosion of the current collector below, and subsequent recovery of the coating components from the molten salt bath has been found to be uneconomical. Other methods involve dissolution / leaching of electrode materials in strong acids. Due to the presence of a large amount of binder material and also due to the hardness and density of the coating after the mechanical calendering process, it is difficult to mechanically separate the electrode components in conventional electrode coatings, so it is necessary to use harsh chemical treatments. Still other methods involve metal recovery based on electrolysis, which requires high power consumption and a large amount of equipment investment, while resulting in a large amount of unrecovered electrode components.
[0009] Improved methods for reconditioning electrochemical cell electrodes are economically and environmentally desirable.
[0010] summary Summary of the invention
[0011] Embodiments described herein generally relate to methods for repairing electrochemical cell electrodes. In some embodiments, a method includes obtaining an electrode material. At least a portion of the electrode material is washed to remove residues therefrom. The electrode material is separated into multiple components for reuse.
[0012] BRIEF DESCRIPTION OF THE DRAWINGS BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1A is a flow chart illustrating a process for repairing / regenerating an electrode material according to one embodiment.
[0014] Figure 1B is a flow chart illustrating a process for repairing / regenerating an electrode material according to one embodiment.
[0015] Figure 2 is a flow chart showing the composition evolution of an electrode material according to one embodiment.
[0016] Figure 3 is a photographic view of a sealed / packaged electrochemical cell according to one embodiment.
[0017] Figure 4A is a schematic diagram of a disassembled electrochemical cell according to one embodiment.
[0018] Figure 4B A mechanical electrode material removal process according to one embodiment is depicted.
[0019] Figure 5A and 5B Photographic partial views of positive (cathode) and negative (anode) current collectors, respectively, with their respective electrode materials physically removed, according to one embodiment.
[0020] Figure 6 is a photographic fragmentary view of a centrifuge tube / vial containing recovered (but not yet centrifuged) cathode material, according to one embodiment.
[0021] Figure 7 is a photographic fragmentary view of a centrifuge tube / vial showing separated / stratified cathode material after centrifugation according to one embodiment.
[0022] Detailed description DETAILED DESCRIPTION
[0023] Rechargeable batteries such as lithium-ion batteries exhibit capacity loss or "capacity fade" during their service life, such as loss of cyclable lithium due to active materials and / or electrical disconnection. In lithium-ion batteries, the entire lithium inventory of the battery is provided by the positive electrode ("cathode") active material. Lithium is lost by consumption in irreversible side reactions within the lithium-ion battery, such as the formation of solid electrolyte interphase ("SEI") materials or layers during the original charging cycle and the continued growth of the SEI layer during aging, storage and / or cycling. Due to the fixed lithium budget of the battery, the lithium lost due to any side reaction in the battery manifests as a non-stoichiometric amount of the cathode active material. Capacity fade manifests as a decrease in the ability of the battery to deliver charge at rated voltage. Conventional methods for recycling conventional solid battery electrodes typically involve high-temperature chemical (e.g., acid)-based dissolution of electrode materials and are complicated by the need to remove binder materials / adhesives. These aggressive chemical recovery methods are necessary due to the difficulty in mechanically separating the components of traditional electrode coatings. Many such methods are time and labor intensive, costly to implement, and have low yields in terms of useful feedstock materials. Nevertheless, given the various valuable components in most battery compositions, and the economic and environmental costs associated with large-scale disposal of electrochemical cells, recycling is an ongoing goal for most battery manufacturers.Due to the challenges described above, improved methods for regenerating electrode materials are needed.
[0024] Embodiments described herein generally relate to methods for remediation (also referred to as "recycling," "reconstituting," "reclamation," "refurbishment," "repurposing," or "remanufacturing") of semisolid electrochemical cell electrodes (as further described herein), and can also be implemented for conventional battery electrodes. In some embodiments, the remediation method includes obtaining an electrode material. For example, the electrode material may include a depleted (i.e., used, substoichiometric, non-stoichiometric, or "wasted") electrode material (e.g., a cathode electrode material or an anode electrode material). In addition, a "depleted" electrode material as described herein may include an electrode material that has been formed into an electrode, an electrode material that has been formed into an electrochemical cell, an electrode material that has been used in an electrochemical cell, and / or an electrode material that has played a role in an electrochemical reaction. In other words, an electrode material that already exists as an electrode can be considered a "depleted" electrode material because it is no longer a pristine electrode material. In some embodiments, the electrode material may include substantially depleted, semi-depleted, partially depleted, and nearly depleted electrode materials.
[0025] After obtaining the electrode material, i.e., the depleted electrode material, optionally, at least a portion of the depleted electrode material is cleaned to remove residues (e.g., electrolyte salts or side reaction products) therefrom. The depleted electrode material is separated into a variety of components (e.g., active materials, conductive additives, etc.) for reuse. In some embodiments, the depleted electrode material is a semisolid anode material or a semisolid cathode material. In some embodiments, the depleted electrode material does not contain a binder. In some embodiments, cleaning and separation are performed simultaneously (e.g., in the same medium). When compared to conventional battery recycling methods, the methods described herein allow separation and recovery of active materials (or "ion storage materials") and other electrode components at reduced cost and energy input.
[0026] Semi-solid electrodes repaired according to the methods described herein are significantly more recyclable than conventional battery electrodes for several reasons. For example, the release / separation of depleted semi-solid electrode materials (i.e., from current collectors) can be performed mechanically rather than chemically, and can require low applied forces for removal (e.g., semi-solid electrode materials can have low adhesive strengths), for example due to their semi-solid physical state and / or the absence of binders. The semi-solid electrode materials can thus be safely and easily removed from the current collectors without causing damage to the current collectors, and have significantly less (or no) contamination of the remediated electrode materials by metals (e.g., copper, aluminum, etc.) from the current collectors. In addition, since there is no binder in the semi-solid electrodes, the steps involving the uptake or dissolution of the binder in strong acids (usually at very high temperatures) are eliminated, and the separation of active materials and conductive carbon can be cleaner and more efficient. Moreover, the spent semi-solid electrode materials generated by the battery manufacturing process are easier to process and reuse.
[0027] The term "semi-solid" as used herein refers to a material that is a mixture of a liquid phase and a solid phase, such as a particle suspension, a colloidal suspension, an emulsion, a gel or a micelle. Examples of battery structures utilizing semi-solid suspensions are described in the following documents: International Patent Publication No. WO 2012 / 024499 entitled "Stationary, Fluid Redox Electrode", International Patent Publication No. WO 2012 / 088442 entitled "Semi-Solid Filled Battery and Method of Manufacture", and International Patent Publication No. WO 2014 / 093876 entitled "Semi-Solid Electrodes Having High Rate Capability", all of which are incorporated herein by reference. See also the section entitled "Semi-Solid Compositions" below.
[0028] As used herein, the terms "about" and "approximately" generally mean plus or minus 10% of the indicated value, for example, about 250 μm would include 225 μm to 275 μm, and about 1,000 μm would include 900 μm to 1,100 μm.
[0029] Figure 1A 1 is a flow chart illustrating a process 100A for repairing / regenerating electrode materials according to one embodiment. According to process 100A, one or more depleted electrode materials are first obtained at 110, optionally by separating (at 120) one or more depleted electrode materials from an electrochemical cell that has reached its "end of service" or exhibited capacity fade. The "depleted" nature of an electrode refers to at least partial degradation or loss or gain of a material such that its active material is compositionally different from its state in the original assembly of the electrochemical device. For example, due to the loss of cyclable lithium in a lithium-ion battery, the stoichiometry of the cathode active material can be significantly different from the stoichiometry of a "fresh" cathode material (i.e., there is a change in the relative amounts of its components), as shown in Tables 1A and 1B below, which compare (respectively) fresh and recycled 111 lithium nickel cobalt manganese oxide (Li 1+x (Ni 0.33 Co 0.33 Mn 0.33 ) 1-x Elemental analysis (by inductively coupled plasma (ICP) mass spectrometry) of the fresh NCM 111 material (also referred to as "NMC") cathode. Table 1A shows the composition of the fresh NCM 111 material with Li 1.17 Ni 0.37 Co 0.38 Mn 0.38 O2 composition and a lithium to transition metal ratio of about 1.04. Table 1B shows the composition of the recycled / depleted NCM (originally NCM 111) material with Li 0.84 Ni 0.63 Co 0.25 Mn 0.38 O2 composition and a lithium to transition metal ratio of about 0.66 (i.e., about 36.5% lithium loss compared to fresh NCM 111). For negative electrode ("anode") active materials such as graphite, silicon, tin, hard carbon, soft carbon, etc., the composition change can be reflected as: lithium (or other working ions) have an increased depth in the recovered anode active material compared to its original state.
[0030]
[0031] Table 1A: Example ICP analysis of fresh NCM (NCM 111) cathode material
[0032]
[0033] Table 1B: Example ICP Analysis of Recycled NCM Cathode Materials
[0034] Separation 120 may involve disassembly of the electrochemical cell. Prior to disassembly, the electrochemical cell includes a positive current collector, a negative current collector, and a separator disposed between the positive current collector and the negative current collector. The positive current collector is spaced apart from the separator and at least partially defines a positive electroactive region. The negative current collector is spaced apart from the separator and at least partially defines a negative electroactive region. The cathode (positive electrode) is disposed in the positive electroactive region, and the anode (negative electrode) is disposed in the negative electroactive region. In some embodiments, the cathode may be a conventional or solid cathode. In some embodiments, the cathode may be a semi-solid cathode. In other words, the cathode may contain a semi-solid electrode composition (also referred to herein as a "semi-solid suspension" and / or "slurry")-see "semi-solid composition" below. In some embodiments, the anode may be a conventional or solid anode, such as a lithium metal anode, a solid graphite electrode, or a rolled anode. In some embodiments, the anode may be a semi-solid anode. In other words, the anode may contain a semi-solid electrode composition (also referred to herein as a "semi-solid suspension" and / or "slurry")-see "semi-solid composition" below. In some embodiments, the electrochemical cell includes both a semisolid cathode and a semisolid anode.
[0035] The positive and negative current collectors can be any current collectors that are electrically conductive and electrochemically inactive under the battery operating conditions. Typical current collectors for lithium batteries include copper, aluminum, or titanium for the negative current collector, and aluminum for the positive current collector, in the form of a sheet or mesh, or any combination thereof. The current collector materials can be selected to be stable at the operating potential of the positive and negative electrodes of the electrochemical cell. For example, in a non-aqueous lithium system, the positive current collector can include aluminum or aluminum coated with a conductive material that is at a relative conductivity to the Li / Li + The negative electrode current collector may include copper or a metal that does not form an alloy or intermetallic compound with lithium or carbon, and / or a coating of such a material disposed on another conductor.
[0036] The anode may comprise an anode active material selected from the group consisting of lithium metal, carbon, lithium intercalated carbon, lithium nitride, lithium alloys, and lithium alloy-forming compounds of silicon, bismuth, boron, gallium, indium, zinc, tin, tin oxide, antimony, aluminum, titanium oxide, molybdenum, germanium, manganese, niobium, vanadium, tantalum, gold, platinum, iron, copper, chromium, nickel, cobalt, zirconium, yttrium, molybdenum oxide, germanium oxide, silicon oxide, silicon carbide, any other material or alloy thereof, and any other combination thereof. The anode may also comprise an intercalated oxide, such as Li4Ti5O 12 (also known as LTO) or TiO2, or a metal salt that undergoes a conversion or substitution reaction. Examples of metal oxides that are converted to Li2O and a metal when reacting with lithium may include CoO, NiO, MnO, and FeO. Examples of metal fluorides that are converted to LiF and a metal when reacting with lithium may include FeF2, FeF3, and BiF3.
[0037] In some embodiments, the anode may be a semisolid stationary anode.In some embodiments, the anode may be a semisolid flowable anode, such as the type used in redox flow batteries.
[0038] The anode may also include a carbonaceous material, such as graphite, carbon powder, pyrolytic carbon, carbon black, carbon fibers, carbon microfibers, carbon nanotubes (CNTs), single-walled CNTs, multi-walled CNTs, fullerene carbons, including "buckyballs", graphene sheets and / or aggregates of graphene sheets, any other carbonaceous material, or a combination thereof. In some embodiments, the anode may also include a non-aqueous liquid electrolyte.
[0039] In some embodiments, the anode may comprise about 35% to about 75% by volume of active material. In some embodiments, the anode may comprise about 40% to about 75% by volume, about 45% to about 75% by volume, about 50% to about 75% by volume, about 55% to about 75% by volume, about 60% to about 75% by volume, or about 65% to about 75% by volume of active material, including all ranges therebetween.
[0040] In some embodiments, the anode may include about 0% to about 10% volume of conductive material. In some embodiments, the anode may include about 0.2% to about 9% volume, about 0.4% to about 8% volume, about 0.6% to about 7% volume, about 0.8% to about 6% volume, about 1% to about 5% volume, or about 2% to about 4% volume of conductive material, including all ranges therebetween. In some embodiments, the anode may include about 1% to about 6% volume of conductive material. In some embodiments, the anode may include about 0.5% to about 2% volume of conductive material, including all ranges therebetween.
[0041] In some embodiments, the anode can comprise about 10% to about 70% electrolyte by volume. In some embodiments, the anode can comprise about 30% to about 50% electrolyte by volume or about 20% to about 40% electrolyte by volume, including all ranges therebetween.
[0042] The cathode can be a semi-solid fixed cathode or a semi-solid flowable cathode of the type used, for example, in a redox flow battery. The cathode can comprise an active material, such as a lithium-containing compound described in further detail below. The cathode can also comprise a conductive material, such as graphite, carbon powder, pyrolytic carbon, carbon black, carbon fibers, carbon microfibers, carbon nanotubes (CNTs), single-walled CNTs, multi-walled CNTs, fullerene carbon, including "buckyballs", graphene sheets and / or aggregates of graphene sheets, any other conductive material, alloys or combinations thereof. The cathode can also comprise a non-aqueous liquid electrolyte as described in further detail below.
[0043] In some embodiments, the cathode and / or anode may comprise an active material and an optional conductive material in the form of particles suspended in a non-aqueous liquid electrolyte. In some embodiments, the conductive particles have a shape, which may include spheres, flakes, or rods to optimize the solid packing ratio, increase the net electronic conductivity of the semi-solid, and improve the rheological behavior of the semi-solid. In some embodiments, low aspect ratio or substantially equiaxed or spherical particles are used to improve the ability of the semi-solid electrode material to flow under stress.
[0044] In some embodiments, the particles have multiple sizes to improve the packing ratio. In particular, the particle size distribution can be bimodal, where the average particle size of the larger particle mode is at least 5 times larger than the average particle size of the smaller particle mode. In some embodiments, the mixture of large particles and small particles improves the flow of materials during battery loading and increases the solid volume ratio and packing density in the loaded battery.
[0045] In some embodiments, the cathode may include about 35% to about 75% volume of active material. In some embodiments, the cathode may include about 40% to about 75% volume, 45% to about 75% volume, about 50% to about 75% volume, about 55% to about 75% volume, about 60% to about 75% volume, or about 65% to about 75% volume of active material, including all ranges therebetween. In some embodiments, the cathode may include about 0.5% to about 8% volume of conductive material. In some embodiments, the cathode may include about 0.6% to about 7.5% volume, about 0.7% to about 7.0% volume, about 0.8% to about 6.5% volume, about 0.9% to about 6% volume, about 1.0% to about 6%, about 1.5% to about 5.0% volume, or about 2% to about 4% volume of conductive material, including all ranges therebetween. In some embodiments, the cathode may include about 25% to about 70% volume of electrolyte. In some embodiments, the cathode can include from about 30% to about 50% or from about 20% to about 40% electrolyte by volume, including all ranges therebetween.
[0046] In some embodiments, the cathode and / or anode may have a thickness of less than 100 μm (the thickness of the final single-sided coating). In some embodiments, the cathode (e.g., a semi-solid cathode) and / or the anode (e.g., a semi-solid anode) may have a thickness in the range of about 250 μm to about 2,000 μm. In some embodiments, the cathode and / or the anode may have a thickness in the range of about 250 μm to about 600 μm, about 300 μm to about 600 μm, about 350 μm to about 600 μm, about 400 μm to about 600 μm, about 450 μm to about 600 μm, or about 500 μm to about 600 μm, including all ranges therebetween.
[0047] The separation of depleted electrode material (e.g., anode or cathode material) from an electrochemical cell may include mechanical removal, such as by scraping, brushing, or wrinkling of a current collector, so that the depleted electrode material peels off, etc. In some embodiments, the separation of depleted electrode material from an electrochemical cell does not involve the use of chemicals (i.e., only mechanical). In some embodiments, the separation of depleted electrode material from an electrochemical cell includes the "clean" removal of electrode material from its corresponding current collector (i.e., so that there is little or no damage to the current collector, and / or substantially no current collector material is present in the separated electrode material). As discussed above, the mechanical separation of depleted semi-solid electrode material (i.e., separation from the current collector) may require only low applied force for removal, for example, due to its semi-solid physical state and / or the absence of a binder. After the depleted electrode material is separated from the current collector, it may optionally be powdered or ground to produce a free-flowing powder for subsequent process steps. Optionally, this powdering or grinding step may be applied at another time in the process, or may be applied multiple times in the process.
[0048] In some embodiments, the depleted active material can be remediated using reagents and / or heat to restore the active material to a "like new" state. Regardless of the separation method, the depleted active material retains the morphology of the original (i.e., "fresh") active material, so remediation does not require significant processing. In other words, since the active material itself is not dissolved, mechanically ground, or otherwise modified, the depleted active material can be restored to a like new state using simple processing techniques.
[0049] In some embodiments, a solvent may be used to dissolve the binder from the recycled electrochemical cell. For example, NMP solvent, acetone, or DMSO may be used to dissolve only the binder from the end-of-life or spent electrodes without damaging the active material. Such recycled active material may then undergo the reconditioning steps described herein to restore the active material to a "like new" state.
[0050] The depleted electrode material is cleaned or washed at 130 to remove one or more residues, such as electrolyte salts, electrolyte solvents, or reaction products, including but not limited to solid-electrolyte-interphase (SEI) formed during cell operation. The cleaning medium can be any polar organic solvent such as dimethyl carbonate ("DMC") or any solvent that is miscible with the electrolyte and in which the electrolyte salt is soluble. For example, the solvent may include, but is not limited to, ethylene carbonate, propylene carbonate, butylene carbonate and their chlorinated or fluorinated derivatives, and the family of acyclic dialkyl carbonates, such as dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, dibutyl carbonate, butyl methyl carbonate, butyl ethyl carbonate and butyl propyl carbonate, γ-butyrolactone, dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, diethyl ether, sulfolane, methyl sulfolane, acetonitrile, propionitrile, ethyl acetate, methyl propionate, ethyl propionate, dimethyl carbonate, tetraglyme, etc. The cleaning can be performed, for example, by immersing the depleted electrode material in the cleaning medium / solvent with or without stirring. In some embodiments, the cleaning medium can be recycled or reused during or after process 100A. In some embodiments, the cleaning medium can be water or an aqueous solution, such as an acidic or alkaline solution. In some embodiments, the cleaning medium can be an acidic solution intended to preferentially dissolve side reaction products (including SEI materials or layers) from the anode active material.
[0051] The cleaned depleted electrode material (with or without a cleaning medium, as discussed below) is loaded into a processing container at 140. The processing container is selected based on the separation technology that will be used later at 150. The material may optionally undergo a powdering or grinding step before or during transfer to the processing container. For example, the processing container may include, for example, a centrifuge vial / tube, a separation chamber of an air classification machine, a beaker, a trough, or any other suitable container. The depleted electrode material is then at least partially separated into component parts at 150 by using one or more separation techniques, such as centrifugation, air classification, or any other suitable separation / classification technology (e.g., filtration, sieving, sedimentation, field flow classification, electrophoresis, and / or similar techniques). In certain embodiments, the component materials may be separated based on other physical properties (e.g., magnetic properties), provided that there are significant differences in the relevant physical properties between the various components. In some embodiments, the separation of the electrode material or the binder-free electrode material may include separation into a first part and a second part. In some embodiments, the separation further includes a third part, a fourth part, a fifth part, and so on. As described herein, the first part, the second part, and the third part may comprise any one component or separate components, such as active electrode materials, including active cathode materials and active anode materials, metals, conductive carbon materials, electrolyte salts, salts, reaction byproducts, SEI materials, etc. In some embodiments, the first part may comprise active electrode materials and the second part comprises conductive carbon materials. In some embodiments, the third part may comprise metals.
[0052] Centrifugation involves rotating one or more samples around a fixed axis so that centrifugal acceleration causes sedimentation of the sample contents. In some embodiments, the depleted electrode material and cleaning medium that form a diluted dispersion together are loaded into a centrifuge vial / tube at 140 and centrifuged at 150 (e.g., 2 minutes at a speed of 1000 rpm) so that the solids (e.g., active materials and conductive carbon) are separated to the bottom of the processing container (centrifuge vial / tube), and the supernatant (e.g., cleaning medium or solvent) is placed on top of the solid. The solid can undergo sedimentation so that the components of the solid are separated into layers based on their particle size and / or density. The supernatant can be decanted / removed from the centrifuge vial / tube. In some embodiments, the decanted supernatant and / or cleaning medium are discarded. In some embodiments, the salts from the decanted supernatant and / or wash medium (i.e., comprising a polar solvent and one or more salts in solution) are regenerated, for example, by adding a non-polar solvent such as hexane to the supernatant or wash medium to precipitate the salts, and optionally, performing one or more purification steps before reusing the salts. Optionally, in some embodiments, the supernatant can be further treated to recover additional materials; for example, a strong base such as ammonium hydroxide is added to precipitate a lithium salt such as lithium hydroxide from the wash solution.
[0053] Air classification involves placing one or more samples into a processing chamber containing a rising column of air that exerts upward aerodynamic air drag on the one or more samples, causing them to separate vertically (i.e., classify) according to size, shape, density, mass, etc. In some embodiments, the depleted electrode material is loaded into a separation chamber of an air classifier at 140 without a cleaning medium and is classified into component parts by air classification.
[0054] Optionally, process 100A forms a loop at 155A (i.e., steps 130, 140, and 150 may be repeated in a loop) such that one or more components (e.g., active materials) resulting from separation 150 are again washed at 130 to remove one or more residues. This subsequent washing may be performed in the same processing vessel used for separation 150, or one or more components may be transferred to a separate washing vessel for washing at 130 and then loaded again into the processing vessel for a second separation step 150 (which may involve the same separation technology used during the first pass, or alternatively, a different technology (centrifugation or air classification)). One or more "wash and separate" loops 155A may be performed as part of process 100A.
[0055] At 160A, at least one component (e.g., active cathode material, active anode material, or conductive carbon material) is recovered or "regenerated" from the processing container for reuse. A post-processing step may be applied to the regenerated component material at 170, for example, to correct its composition, or to repair or reconstruct it in other ways. For example, post-processing may include adding additives by mixing, for example, to compensate for one or more "missing" components. In some embodiments, when the regenerated component material is a cathode material, the additive includes a lithium source, such as lithium carbonate, lithium hydroxide, lithium nitrate, lithium sulfate, or any lithium salt. In some embodiments, when the regenerated component material is an anode material (e.g., to "pre-lithiate" the anode), the additive includes a lithium source, such as lithium carbonate, lithium hydroxide, lithium nitrate, lithium sulfate, or any lithium salt. Additionally or alternatively, the additive may include, for example, any material described herein under the following heading "semi-solid composition". In some embodiments, the at least one regenerated component, optionally in combination with any additive or material described herein, is formed into or incorporated into a fresh, recycled electrode (e.g., a solid electrode or a semi-solid electrode). The reconstructed / recycled cathode and / or anode may be disposed on the respective current collectors using any suitable method, such as by coating, pouring, dripping, pressing, rolling or depositing onto the respective current collectors. The repair atmosphere may be similar to the atmosphere used when the electrode material was originally produced (i.e., before depletion or when it was originally manufactured). For example, metal oxide cathodes such as LiCoO2 (lithium cobalt oxide, "LCO"), Li(Ni,Mn,Co)O2 (lithium nickel manganese cobalt oxide, "NMC", also known as "NCM"), LiNi 0.8 Co 0.15 Al 0.05 The repair of Lithium Nickel Cobalt Aluminum Oxide (NCA), LiMn2O4 (Lithium Manganese Oxide (LMO)), LiCoPO4 (Lithium Cobalt Phosphate (LCP)), and LiNiPO4 (Lithium Nickel Phosphate (LNP)) can be carried out in an oxidizing or inert atmosphere, while other materials such as LiFePO4 (Lithium Iron Phosphate (LFP)), LiMnPO4 (Lithium Manganese Phosphate (LMP)), LiMn 0.85 Fe 0.15 PO4 (lithium manganese iron phosphate, "LMFP") and Li4Ti5O 12 The reconditioning of lithium titanate ("LTO") can be performed in an inert or reducing environment. The regenerated electrode material and / or the recycled electrode can be subjected to one or more thermal treatment steps, for example, to restore crystalline order, collapse or evaporate one or more surface molecules (e.g., surfactants), and / or densify the regenerated material.
[0056] In some embodiments, the repaired electrode comprises a semi-solid suspension, and a redox mediator is used to improve charge transfer within the semi-solid suspension. In some embodiments, the redox mediator is based on Fe 2+ or V 2+ 、V 3+ or V 4+ In some embodiments, the redox mediator is ferrocene. In some embodiments, the cathode may have at least about 10 -3 S / cm or at least about 10 -2 S / cm electronic conductivity. In some embodiments, the semi-solid suspension is a cathode suspension having a mixing index of at least about 0.9, at least about 0.95, or at least about 0.975. In some embodiments, the semi-solid anode suspension may have a mixing index of at least about 0.9, at least about 0.95, or at least about 0.975.
[0057] Semi-solid compositions
[0058] In some embodiments the semisolid cathode and in some embodiments the anode (eg, a semisolid anode) collectively function as an ion storage / source, an electron conductor, and an ion conductor in a single medium that serves as a working electrode.
[0059] When measured in molar concentration (mol / L), the cathode and / or anode semi-solid ion storage redox composition as described herein may have a redox species concentration of at least 10M (mol / L). In some embodiments, the cathode and / or anode semi-solid ion storage redox composition may contain at least 12M, at least 15M, or at least 20M of redox species. The electrochemically active material can be an ion storage material and / or any other compound or ion complex capable of undergoing a Faraday reaction to store energy. The electroactive material can also be a multiphase material, including the above-mentioned redox active solids mixed with non-redox active phases, including solid-liquid suspensions or liquid-liquid multiphase mixtures, including micelles or emulsions having liquid ion storage materials intimately mixed with a supporting liquid phase. Systems utilizing various working ions may include wherein Li + 、Na + or other alkali ions as working ions, even alkaline earth metal working ions such as Ca 2+ Mg 2+ or Al 3+ In each of these cases, a negative electrode storage material and a positive electrode storage material can be used, with the negative electrode storing the working ion of interest at a lower absolute potential than the positive electrode. The cell voltage can be approximately determined by the difference in ion storage potentials of the two ion storage electrode materials.
[0060] Systems that employ negative ion storage materials and / or positive ion storage materials that are insoluble storage hosts for working ions (meaning that the material can absorb or release working ions while all other components of the material remain substantially insoluble in the electrolyte) are particularly advantageous because the electrolyte does not become contaminated with the electrochemical composition products. Additionally, systems that employ negative and / or positive lithium ion storage materials are particularly advantageous when non-aqueous electrochemical compositions are used.
[0061] In some embodiments, the semi-solid ion storage redox composition includes materials that have been demonstrated to function in conventional lithium ion batteries. In some embodiments, the semi-solid cathode electroactive material comprises a lithium positive electroactive material, and the lithium cations shuttle between the anode (e.g., semi-solid anode) and the semi-solid cathode, embedded in solid host particles suspended in a liquid electrolyte.
[0062] In some embodiments, at least one of the semi-solid cathode and / or anode (e.g., semi-solid anode) comprises a concentrated ion storage liquid of the following substances: a redox active compound, which may be organic or inorganic, and includes, but is not limited to, lithium metal, sodium metal, lithium-metal alloys, gallium and indium alloys with or without dissolved lithium, molten transition metal chlorides, thionyl chloride, etc., or redox polymers and organics that may be liquid under the operating conditions of the battery. Such a liquid form may also be diluted or mixed with another non-redox active liquid as a diluent or solvent, including mixing with such diluents to form a lower melting point liquid phase. In some embodiments, the redox active component may constitute at least 10% of the total mass of the electrolyte by mass. In other embodiments, the redox active component will constitute approximately 10% to 25% of the total mass of the electrolyte by mass. In some embodiments, the redox active component will constitute at least 25% or more of the total mass of the electrolyte by mass.
[0063] In some embodiments, the redox-active electrode material (whether used in semi-solid or concentrated liquid form as defined above) comprises an organic redox compound that stores a working ion of interest at a potential useful for the positive or negative electrode of a battery. Such organic redox-active storage materials include "p"-doped conducting polymers such as polyaniline or polyacetylene materials, polynitroxide or organic group electrodes (such as those described in the following literature: H. Nishide et al. Electrochim. Acta, 50, 827-831, (2004), and K. Nakahara et al. Chem. Phys. Lett., 359, 351-354 (2002)), carbonyl-based organics, as well as oxocarbons and carboxylates, including compounds such as Li2C6O6, Li2C8H4O4 and Li2C6H4O4 (see, for example, M. Armand et al. Nature Materials, DOI: 10.1038 / nmat2372) and organic sulfur compounds.
[0064] In some embodiments, an electronically insulating organic redox compound is used. In some cases, the redox compound is in a concentrated liquid phase, such as an electronically insulating liquid or a flowable polymer. In such cases, the redox active slurry may or may not include an additional carrier liquid. Additives may be combined with concentrated phase liquid redox compounds to improve electronic conductivity. In some embodiments, such electronically insulating organic redox compounds are electrochemically active by mixing or blending with microparticles of electronically conductive materials, such as solid inorganic conductive materials, including but not limited to metals, metal carbides, metal nitrides, metal oxides and carbon allotropes, including carbon black, graphite carbon, carbon fibers, carbon microfibers, vapor grown carbon fibers (VGCF), fullerene carbon, including "bucky balls", carbon nanotubes (CNTs), multi-walled carbon nanotubes (MWNTs), single-walled carbon nanotubes (SWNTs), graphene sheets or graphene sheet aggregates, and materials comprising fullerene fragments.
[0065] In some embodiments, such electronically insulating organic redox compounds are rendered electrochemically active by mixing or blending with electronically conductive polymers, including but not limited to polyaniline or polyethynyl conductive polymers or poly(3,4-ethylenedioxythiophene) (PEDOT), polypyrrole, polythiophene, poly(p-phenylene), poly(triphenylene), polyazulene, polyfluorene, polynaphthalene, polyanthracene, polyfuran, polycarbazole, tetrathiafulvalene-substituted polystyrene, ferrocene-substituted polyethylene, carbazole-substituted polyethylene, polyoxyphenazine, polyacene or poly(heteroacene). The conductive additive forms a conductive framework within the insulating liquid redox compound that significantly increases the conductivity of the composition. In some embodiments, the conductive additive forms a percolation path to the current collector. In some embodiments, the redox-active electrode material comprises a sol or gel, including, for example, a metal oxide sol or gel produced by hydrolysis of a metal alkoxide, particularly by other methods commonly referred to as "sol-gel processing". Composition V x O y Vanadium oxide gels belong to such redox-active sol-gel materials.
[0066] Other suitable positive active materials for semi-solid cathodes include solid compounds known to those skilled in the art such as those used in nickel-metal hydride (NiMH) and nickel cadmium (NiCd) batteries. Other positive electrode compounds for Li storage include those used in carbon monofluoride batteries, commonly referred to as CF x, or a metal fluoride compound having an approximate stoichiometry of MF2 or MF3, where M comprises, for example, Fe, Bi, Ni, Co, Ti or V. Examples include those described in H. Li, P. Balaya and J. Maier, Li-Storage via Heterogeneous Reaction in Selected Binary Metal Fluorides and Oxides, Journal of The Electrochemical Society, 151
[11] A1878-A1885 (2004), M. Bervas, AN Mansour, W.-S. Woon, J. F. Al-Sharab, F. Badway, F. Cosandey, L. C. Klein and G. G. Amatucci, "Investigation of the Lithiation and Delithiation Conversion Mechanisms in a Bismuth Fluoride Nanocomposites", J. Electrochem. Soc., 153, A799 (2006), and I. Plitz, F. Badway, J. Al-Sharab, A. Du Pasquier, F. Cosandey and G. G. Amatucci, "Structure and Electrochemistry of Carbon-Metal Fluoride Nanocomposites Fabricated by a Solid State RedoxConversion Reaction", J. Electrochem. Soc., 152, A307 (2005).
[0067] As another example, fullerene carbons including single-walled carbon nanotubes (SWNTs), multi-walled carbon nanotubes (MWNTs), or metal or metalloid nanowires can be used as ion storage materials. An example is silicon nanowires used as high energy density storage materials in the following report: CK Chan, H. Peng, G. Liu, K. McIlwrath, XF Zhang, RA Huggins, and Y. Cui, High-performance lithium battery anodes using silicon nanowires, Nature Nanotechnology, published online on December 16, 2007; DOI: 10.1038 / nnano.2007.411. In some embodiments, the electroactive material for the semi-solid cathode in the lithium system may include the general family of ordered rock salt compounds LiMO2, including those with α-NaFeO2 (so-called "layered compounds") or orthorhombic-LiMnO2 structure types or derivatives thereof with different crystal symmetry, atomic ordering, or metal or oxygen partial substitution. M includes at least one first row transition metal, but may include non-transition metals, including but not limited to Al, Ca, Mg, or Zr. Examples of such compounds include LiCoO2, LiCoO2 doped with Mg, LiNiO2, Li(Ni, Co, Al)O2 (referred to as "NCA"), and Li(Ni, Mn, Co)O2 (referred to as "NMC" or "NCM"). Other families of exemplary cathode 140 electroactive materials include those of spinel structure, such as LiMn2O4 and its derivatives, so-called "layered spinel nanocomposites" where the structure includes nanoscale regions with ordered rock salt and spinel ordering, olivine LiMPO4 and its derivatives where M includes one or more of Mn, Fe, Co, or Ni, partially fluorinated compounds such as LiVPO4F, other "polyanionic" compounds as described below, and compounds including V2O5 and V6O 11 Vanadium oxide V x O y .
[0068] In some embodiments, the semi-solid cathode electroactive material comprises a transition metal polyanion compound, such as described in U.S. Pat. No. 7,338,734. In some embodiments, the active material comprises an alkali metal transition metal oxide or phosphate, and, for example, the compound has the following composition: A x (M′ 1-a M″ a ) y (XD4) z , A x (M′ 1-a M″a ) y (DXD4) z or A x (M′ 1-a M″ a ) y (X2D7) z , and has a value such that x plus y(1-a) times the formal valence of M' or multiple valence plus ya times the formal valence of M" or valence equals z times the formal valence of the XD4, X2D7 or DXD4 group; or comprises the composition (A 1-a M″ a ) x M′ y (XD4) z ,(A 1-a M″ a ) x M′ y (DXD4)z(A 1-a M″ a ) x M′ y (X2D7) z A compound and having a value such that (1-a)x plus the amount ax times the formal valence or multiple valences of M″ plus y times the formal valence or multiple valences of M′ equals z times the formal valence of the XD4, X2D7 or DXD4 group. In the compound, A is at least one of an alkali metal and hydrogen, M′ is a first-row transition metal, X is at least one of phosphorus, sulfur, arsenic, molybdenum and tungsten, M″ is any of Group IIA, IIIA, IVA, VA, VIA, VIIA, VIIIA, IB, IIB, IIIB, IVB, VB and VIB metals, and D is at least one of oxygen, nitrogen, carbon or halogen. The positive electroactive material can be an olivine structure compound LiMPO4, wherein M is one or more of V, Cr, Mn, Fe, Co and Ni, wherein the compound is optionally doped at the Li, M or O-position. The deficiency at the Li-position is compensated by adding a metal or metalloid, and the deficiency at the O-position is compensated by adding a halogen. In some embodiments, the positive active material includes a material having an olivine structure and having the formula (Li 1-x Z x ) A thermally stable, transition metal-doped lithium transition metal phosphate of MPO4, wherein M is one or more of V, Cr, Mn, Fe, Co and Ni, and Z is a non-alkali metal dopant such as one or more of Ti, Zr, Nb, Al or Mg, and x is in the range of 0.005-0.05.
[0069] In other embodiments, the lithium transition metal phosphate material has Li 1-x-z M 1+zThe overall composition of PO4, where M includes at least one first-row transition metal selected from Ti, V, Cr, Mn, Fe, Co, and Ni, where x ranges from 0 to 1, and z can be positive or negative. M includes Fe, and z is between approximately 0.15 - 0.15. The material can exist as a solid solution in the composition range of 0 < x < 0.15, or the material can exist as a stable solid solution in the composition range where x ranges from 0 to at least about 0.05, or the material can exist as a stable solid solution at room temperature (22 - 25 °C) in the composition range where x ranges from 0 to at least about 0.07. The material can also exist as a solid solution in a lithium-depleted state, for example, where x ≥ 0.8, or x ≥ 0.9 or x ≥ 0.95.
[0070] In some embodiments, the redox-active electrode material includes a metal salt that stores alkali ions by undergoing a displacement or conversion reaction. Examples of such compounds include metal oxides such as CoO, Co3O4, NiO, CuO, MnO, which are commonly used as negative electrodes in lithium batteries and undergo a displacement or conversion reaction upon reaction with Li to form a mixture of Li2O and the metal component in the form of a more reduced oxide or the metal form. Other examples include metal fluorides such as CuF2, FeF2, FeF3, BiF3, CoF2, and NiF2, which undergo a displacement or conversion reaction to form LiF and a reduced metal component. Such fluorides can be used as positive electrodes in lithium batteries. In other embodiments, the redox-active electrode material includes single-fluorinated carbon or its derivatives. In some embodiments, the material that undergoes a displacement or conversion reaction is in the form of fine particles with an average size of 100 nanometers or less. In some embodiments, the material that undergoes a displacement or conversion reaction includes a nanocomposite of an active material mixed with an inactive host, where the inactive host includes but is not limited to a conductive and relatively ductile compound such as carbon or a metal or a metal sulfide. FeS2 and FeF3 can also be used as inexpensive and electronically conductive active materials in non-aqueous or aqueous lithium systems. In some embodiments, CF x The CoO electrode, FeS2 electrode, or MnO2 electrode is a positive electrode used with a lithium metal negative electrode to produce a lithium battery. In some embodiments, such a battery is a primary battery. In some embodiments, such a battery is a rechargeable battery.
[0071] In some embodiments, the working ion is selected from Li + 、Na + 、H + 、Mg 2+ 、Al 3+ 或Ca 2+ 。
[0072] In some embodiments, the working ion is selected from Li + 或Na +.
[0073] In some embodiments, a semi-solid ion-storing redox composition comprises a solid comprising an ion-storing compound.
[0074] In some embodiments, the ions are protons or hydroxide ions, and the ion storage compounds include those used in nickel-cadmium or nickel metal hydride batteries.
[0075] In some embodiments, the ion is lithium and the ion storage compound is selected from metal fluorides such as CuF2, FeF2, FeF3, BiF3, CoF2, and NiF2.
[0076] In some embodiments, the ion is lithium and the ion storage compound is selected from metal oxides such as CoO, Co3O4, NiO, CuO, MnO.
[0077] In some embodiments, the ion is lithium and the ion storage compound comprises an intercalation compound selected from the group consisting of 1-x Z x )MPO4 compound, wherein M is one or more of V, Cr, Mn, Fe, Co and Ni, and Z is a non-alkali metal dopant such as one or more of Ti, Zr, Nb, Al or Mg, and x ranges from 0.005 to 0.05.
[0078] In some embodiments, the ion is lithium and the ion storage compound comprises an intercalation compound selected from compounds having the formula LiMPO4, wherein M is one or more of V, Cr, Mn, Fe, Co and Ni, wherein the compound is optionally doped at the Li, M or O-position.
[0079] In some embodiments, the ion is lithium and the ion storage compound comprises an intercalation compound selected from A x (M′ 1-a M″ a ) y (XD4) z , A x (M′ 1-a M″ a ) y (DXD4) z and A x (M′ 1-a M″ a ) y (X2D7) z, wherein x plus y(1-a) times the formal valence of M' or multiple valences plus ya times the formal valence of M" or a valence equal to z times the formal valence of the XD4, X2D7 or DXD4 group; and A is at least one of an alkali metal and hydrogen, M' is a first row transition metal, X is at least one of phosphorus, sulfur, arsenic, molybdenum and tungsten, M" is any of Group IIA, IIIA, IVA, VA, VIA, VIIA, VIIIA, IB, IIB, IIIB, IVB, VB and VIB metals, and D is at least one of oxygen, nitrogen, carbon or halogen.
[0080] In some embodiments, the ion is lithium and the ion storage compound comprises an intercalation compound selected from A 1-a M″ a ) x M′ y (XD4) z ,(A 1-a M″ a ) x M′ y (DXD4)z and A 1-a M″ a ) x M′ y (X2D7) z , wherein (1-a)x plus the amount ax times the formal valence or valences of M″ plus y times the formal valence or valences of M′ is equal to z times the formal valence of the XD4, X2D7 or DXD4 group, and A is at least one of an alkali metal and hydrogen, M′ is a first row transition metal, X is at least one of phosphorus, sulfur, arsenic, molybdenum and tungsten, M″ is any of Group IIA, IIIA, IVA, VA, VIA, VIIA, VIIIA, IB, IIB, IIIB, IVB, VB and VIB metals, and D is at least one of oxygen, nitrogen, carbon or a halogen.
[0081] In some embodiments, the ion is lithium and the ion storage compound comprises an insertion compound selected from the ordered rock salt compound LiMO2, including those having α-NaFeO2 and orthorhombic-LiMnO2 structure types or derivatives thereof of different crystal symmetry, atomic ordering or metal or oxygen partial substitution, wherein M comprises at least one first row transition metal, but may include non-transition metals, including but not limited to Al, Ca, Mg or Zr.
[0082] In some embodiments, the semi-solid ion-storing redox composition comprises a solid comprising amorphous carbon, disordered carbon, graphitic carbon, or metal-coated or metal-modified carbon.
[0083] In some embodiments, the semi-solid ion-storing redox composition may comprise a solid that includes nanostructures such as nanowires, nanorods, and nanotetrapods.
[0084] In some embodiments, the semi-solid ion-storing redox composition comprises a solid including an organic redox compound.
[0085] In some embodiments, the positive electrode may comprise a semi-solid ion storage redox composition comprising a solid selected from the following: ordered rock salt compounds LiMO2, including those with α-NaFeO2 and orthorhombic-LiMnO2 structure types or derivatives thereof with different crystal symmetry, atomic ordering, or metal or oxygen partial substitution, wherein M comprises at least one first row transition metal, but may include non-transition metals, including but not limited to Al, Ca, Mg, or Zr. The anode may comprise a semi-solid ion storage composition comprising a solid selected from the following: amorphous carbon, disordered carbon, graphitic carbon, or metal-coated or metal-modified carbon.
[0086] In some embodiments, the semi-solid cathode 140 may include a semi-solid ion-storing redox composition, such as a solid selected from the group consisting of: A x (M′ 1-a M″ a ) y (XD4) z , A x (M′ 1-a M″ a ) y (DXD4) z and A x (M′ 1-a M″ a ) y (X2D7) z , and wherein x plus y(1-a) times the formal valence of M' or multiple valences plus ya times the formal valence of M" or valence equals z times the formal valence of the XD4, X2D7 or DXD4 group, and A is at least one of an alkali metal and hydrogen, M' is a first row transition metal, X is at least one of phosphorus, sulfur, arsenic, molybdenum and tungsten, M" is any of Group IIA, IIIA, IVA, VA, VIA, VIIA, VIIIA, IB, IIB, IIIB, IVB, VB and VIB metals, and D is at least one of oxygen, nitrogen, carbon or halogen. In some embodiments, the anode can be a semi-solid anode comprising a semi-solid ion storage redox composition, such as a solid selected from the group consisting of amorphous carbon, disordered carbon, graphitic carbon, or metal-coated or metal-modified carbon. In some embodiments, the anode can comprise a semi-solid ion storage redox composition, including a compound having a spinel structure.
[0087] In some embodiments, the semisolid cathode may comprise a semisolid ion-storing redox composition, such as a compound selected from the group consisting of: LiMn2O4 and its derivatives; a layered spinel nanocomposite wherein the structure comprises nanoscale regions having ordered rock salt and spinel ordering; a so-called "high-pressure spinel" having a Li / Li ratio in excess of 4.3 V; + potential, including but not limited to LiNi 0.5 Mn 1.5 O4; olivine LiMPO4 and its derivatives, wherein M includes one or more of Mn, Fe, Co or Ni, partially fluorinated compounds such as LiVPO4F, other "polyanion" compounds, and V2O5 and V6O 11 Vanadium oxide V x O y .
[0088] In some embodiments, the semi-solid battery is a lithium battery and the anode compound includes graphite, graphite or non-graphite carbon, amorphous carbon, mesophase carbon microspheres, boron-carbon alloys, hard carbon or disordered carbon, lithium titanate spinel, or a solid metal or metal alloy or metalloid or metalloid alloy that reacts with lithium to form an intermetallic compound, such as Si, Ge, Sn, Bi, Zn, Ag, Al, any other suitable metal alloy, metalloid alloy or combination thereof, lithiated metal or metal alloy, including compounds such as: LiAl, Li9Al4, Li3Al, LiZn, LiAg, Li 10 Ag3, Li5B4, Li7B6, Li 12 Si7、Li 21 Si8、Li 13 Si4、Li 21 Si5, Li5Sn2, Li 13 Sn5, Li7Sn2, Li 22 Sn5, Li2Sb, Li3Sb, LiBi or Li3Bi, or an amorphous metal alloy of lithiated or non-lithiated composition, any other material or alloy thereof, or any other combination thereof.
[0089] In some embodiments, the electrochemical function of the electrochemical cell can be improved by mixing or blending the semi-solid cathode and / or semi-solid anode particles with microparticles of an electronically conductive material, such as a solid inorganic conductive material, including but not limited to metals, metal carbides, metal nitrides, metal oxides, and allotropes of carbon, including carbon black, graphitic carbon, carbon fibers, carbon microfibers, vapor grown carbon fibers (VGCF), fullerene carbon, including "buckyballs", carbon nanotubes (CNTs), multi-walled carbon nanotubes (MWNTs), single-walled carbon nanotubes (SWNTs), graphene sheets or aggregates of graphene sheets, and materials containing fullerene fragments. In some embodiments, such electronically insulating organic redox compounds are rendered electronically active by mixing or blending with electronically conductive polymers, including but not limited to polyaniline or polyethynyl conductive polymers or poly(3,4-ethylenedioxythiophene) (PEDOT), polypyrrole, polythiophene, poly(p-phenylene), poly(triphenylene), polyazulene, polyfluorene, polynaphthalene, polyanthracene, polyfuran, polycarbazole, tetrathiafulvalene-substituted polystyrene, ferrocene-substituted polyethylene, carbazole-substituted polyethylene, polyoxyphenazine, polyacene or poly(heteroacene). In some embodiments, the resulting semi-solid cathode and / or semi-solid anode mixture has at least about 10 -3 S / cm, at least about 10 -2 S / cm or higher electronic conductivity.
[0090] In some embodiments, particles included in a semisolid cathode and / or a semisolid anode may be configured to have a partial or full conductive coating.
[0091] In some embodiments, the semi-solid ion storage redox composition comprises an ion storage solid coated with a conductive coating material. In some embodiments, the conductive coating material has a higher electronic conductivity than the solid. In some embodiments, the solid is graphite and the conductive coating material is a metal, metal carbide, metal oxide, metal nitride or carbon. In some embodiments, the metal is copper.
[0092] In some embodiments, the solid of the semi-solid ion storage material is coated with a metal that is redox inert under the operating conditions of the redox energy storage device. In some embodiments, the solid of the semi-solid ion storage material is coated with copper to increase the conductivity of the storage material particles, increase the net conductivity of the semi-solid, and / or promote charge transfer between the energy storage particles and the conductive additive. In some embodiments, the storage material particles are coated with about 1.5% by weight of metallic copper. In some embodiments, the storage material particles are coated with about 3.0% by weight of metallic copper. In some embodiments, the storage material particles are coated with about 8.5% by weight of metallic copper. In some embodiments, the storage material particles are coated with about 10.0% by weight of metallic copper. In some embodiments, the storage material particles are coated with about 15.0% by weight of metallic copper. In some embodiments, the storage material particles are coated with about 20.0% by weight of metallic copper.
[0093] In some embodiments, the conductive coating is disposed on the semi-solid cathode and / or anode particles by chemical precipitation of the conductive component and subsequent drying and / or calcination.
[0094] In some embodiments, the conductive coating is placed on the semisolid cathode and / or anode particles by electroplating (eg, in a fluidized bed).
[0095] In some embodiments, the conductive coating is disposed on the semi-solid cathode and / or anode particles by co-sintering with a conductive compound and subsequent comminution.
[0096] In some embodiments, the electrochemically active particles have continuous intra-particle conductive material or are embedded in a conductive matrix.
[0097] In some embodiments, the conductive coating and intra-particle conductive network are produced by multi-component spray drying of semi-solid cathode and / or anode particles and conductive material particles.
[0098] In some embodiments, the semi-solid composition (e.g., a semi-solid cathode composition or a semi-solid anode composition) further comprises a conductive polymer that provides an electronic conductive element. In some embodiments, the conductive polymer may include one or more of the following: polyacetylene, polyaniline, polythiophene, polypyrrole, poly(p-phenylene), poly(triphenylene), polyazulene, polyfluorene, polynaphthalene, polyanthracene, polyfuran, polycarbazole, polybenzone or poly(heterobenzone). In some embodiments, the conductive polymer may be a compound that reacts in situ to form a conductive polymer on the surface of the active material particles. In some embodiments, the compound may be 2-hexylthiophene or 3-hexylthiophene, and is oxidized during battery charging to form a conductive polymer coating on solid particles in the cathode semi-solid suspension. In other embodiments, the redox active material may be embedded in a conductive matrix. The redox active material may coat the external and internal interfaces in the flocculated or agglomerated microparticles of the conductive material. In some embodiments, the redox active material and the conductive material may be two components of the composite microparticles. Without being bound by any theory or mode of operation, such a coating can calm the redox-active particles and can help prevent undesired reactions with the carrier fluid or electrolyte. Thus, it can act as a synthetic solid-electrolyte interphase (SEI) layer.
[0099] In some embodiments, inexpensive iron compounds such as pyrite (FeS2) are used as intrinsically electronically conductive ion storage compounds. In some embodiments, the stored ions are Li + .
[0100] In some embodiments, a redox mediator is added to the semisolid to improve the charge transfer rate within the semisolid electrode. In some embodiments, the redox mediator is ferrocene or a ferrocene-containing polymer. In some embodiments, the redox mediator is one or more of tetrathiafulvalene-substituted polystyrene, ferrocene-substituted polyethylene, and carbazole-substituted polyethylene.
[0101] In some embodiments, the surface conductivity or charge transfer resistance of the positive current collector and / or the negative current collector included in the electrochemical cell is increased by coating the current collector surface with a conductive material. Such a layer may also serve as a synthetic SEI layer. Non-limiting examples of conductive coating materials include carbon, metals, metal carbides, metal nitrides, metal oxides or conductive polymers. In some embodiments, conductive polymers include but are not limited to polyaniline or polyacetylene conductive polymers or poly (3,4-ethylenedioxythiophene) (PEDOT), polypyrrole, polythiophene, poly (p-phenylene), poly (triphenylene), polyazulene, polyfluorene, polynaphthalene, polyanthracene, polyfuran, polycarbazole, tetrathiafulvalene substituted polystyrene, ferrocene substituted polyethylene, carbazole substituted polyethylene, polyoxyphenazine, polyphenylene or poly (heterophenylene). In some embodiments, the conductive polymer is a compound that reacts in situ to form a conductive polymer on the surface of the current collector. In some embodiments, the compound is 2-hexylthiophene and is oxidized at a high potential to form a conductive polymer coating on the current collector. In some embodiments, the current collector is coated with a metal that is redox inert under the operating conditions of the redox energy storage device.
[0102] The semi-solid redox composition may contain various additives to improve the performance of the redox cell. The semi-solid liquid phase in this case will contain a solvent in which an electrolyte salt is dissolved, as well as a binder, a thickener or other additives, which are added to improve stability, reduce gas formation, improve SEI formation on the negative electrode particles, and so on. Examples of such additives include vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC) or alkyl cinnamate to provide a stable passivation layer on the anode or a thin passivation layer on the oxide cathode, propane sultone (PS), propylene sultone (PrS), or thioethylene carbonate as a degassing agent, biphenyl (BP), cyclohexylbenzene, or partially hydrogenated terphenyl as an inflating / safety / cathode polymerization agent, or lithium bis(oxalate)borate as an anode passivator.
[0103] In some embodiments, the semi-solid redox composition is free of a binder.
[0104] In some embodiments, the semi-solid cathode and / or anode may comprise a non-aqueous liquid electrolyte, which may comprise a polar solvent such as an alcohol or an aprotic organic solvent. Numerous organic solvents have been proposed as components of lithium ion battery electrolytes, particularly the family of cyclic carbonates, such as ethylene carbonate, propylene carbonate, butylene carbonate, and their chlorinated or fluorinated derivatives, and the family of acyclic dialkyl carbonates, such as dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, dibutyl carbonate, butyl methyl carbonate, butyl ethyl carbonate, and butyl propyl carbonate. Other solvents proposed as components of lithium-ion battery electrolyte solutions include γ-butyrolactone, dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, diethyl ether, sulfolane, methyl sulfolane, acetonitrile, propionitrile, ethyl acetate, methyl propionate, ethyl propionate, dimethyl carbonate, tetraethylene glycol dimethyl ether, and the like. These non-aqueous solvents are usually used in the form of a multi-component mixture in which a salt is dissolved to provide ionic conductivity. Exemplary salts that provide lithium conductivity include LiClO4, LiPF6, LiBF4, LiTFSI, LiBETI, LiBOB, and the like.
[0105] In some embodiments, the non-aqueous cathode and / or anode semi-solid compositions are prevented from absorbing impure water and producing acid (e.g., HF in the case of LiPF6 salts) by introducing a compound that draws water into the active material suspension or into a storage tank or other conduit of the system (e.g., in the case of a redox flow battery). Optionally, the additive is an alkaline oxide that neutralizes the acid. Such compounds include, but are not limited to, silica gel, calcium sulfate (e.g., a product known as Drierite), aluminum oxide, and aluminum hydroxide.
[0106] In some embodiments, the cathode can be a semi-solid cathode, and the anode can be a conventional anode, for example, a solid anode formed by a calendering process as known in the prior art. In some embodiments, the cathode can be a semi-solid cathode, and the anode can also be a semi-solid anode as described herein. In some embodiments, both the cathode and the anode can be semi-solid flowable electrodes, for example, for use in a redox flow battery.
[0107] In some embodiments, the semi-solid cathode and semi-solid anode can be prepared by combining an amount of active material with an electrolyte and a conductive material and mixing until a substantially stable suspension is formed, the suspension having a mixing index of at least about 0.9, at least about 0.95, or at least about 0.975, including all ranges therebetween. In some embodiments, the semi-solid cathode and / or semi-solid anode materials are mixed until the electrode material has at least about 10 -3 S / cm or at least about 10 -2S / cm, including all ranges therebetween. In some embodiments, the electrode materials are mixed until the electrode materials have an apparent viscosity (at about 5 s -1 In such an embodiment, the semi-solid cathode 140 may comprise about 35-75% by volume of active material and about 0.5-8% by volume of conductive material, and the semi-solid anode may comprise about 35-75% by volume of active material and about 0-10% by volume of conductive material. In addition, the electrochemical cell including the semi-solid cathode 140 and / or the semi-solid anode may have a capacity of at least about 7 mAh / cm 2 , for example at least about 8 mAh / cm 2 , at least about 9 mAh / cm 2 Or at least about 10mAh / cm 2 In some embodiments, the active material contained in the semi-solid cathode can be LFP. In such embodiments, the electrochemical cell can have at least about 7 mAh / cm at a C-rate of C / 4. 2 In some embodiments, the active material contained in the semi-solid cathode can be NCM. In such embodiments, the electrochemical cell can have at least about 7 mAh / cm at a C-rate of C / 4. 2 Area specific capacity.
[0108] In some embodiments, the mixing of electrode materials (e.g., semi-solid cathode or semi-solid anode) can be carried out using any one of, for example, a high shear mixer, a planetary mixer, a centrifugal planetary mixer, a zigzag mixer, a CAM mixer, and / or a roller mixer. In some embodiments, the mixing of electrode materials can provide a specific mixing energy of at least about 90 J / g, at least about 100 J / g, about 90 J / g to about 150 J / g, or about 100 J / g to about 120 J / g, including all ranges therebetween.
[0109] In some embodiments, the composition of the electrode materials and the mixing method can be selected to uniformly disperse the components of the slurry, achieve a permeating conductive network throughout the slurry and a sufficiently high bulk conductivity, which is related to the desired electrochemical properties further described in detail herein, to obtain a rheological state that is conducive to processing, which may include transferring, conveying (e.g., extrusion), dispensing, segmenting or cutting, and post-dispensing forming (e.g., press forming, rolling, calendaring, etc.) or any combination thereof.
[0110] In some embodiments, the slurry or "particle suspension" is initially stabilized by repulsive inter-particle steric forces generated by surfactant molecules. After loading the particle suspension into the positive and / or negative electroactive regions, chemical or thermal treatments can cause these surface molecules to collapse or evaporate and promote densification. In some embodiments, the steric forces of the suspension are intermittently altered during loading.
[0111] For example, the particle suspension can be initially stabilized by repulsive interparticle electrostatic double layer forces to reduce viscosity. The repulsive forces reduce the attraction between particles and reduce agglomeration. After the particle suspension is loaded into the positive and / or negative electroactive regions, the surface of the particles can be further modified to reduce the repulsive forces between particles and thereby promote particle attraction and filling. For example, ionic solutions such as salt solutions can be added to the suspension to reduce repulsive forces and promote aggregation and densification to produce an increased solid ratio loading after filling the electroactive regions. In some embodiments, salts are intermittently added during suspension loading to increase the density in incremental layers.
[0112] In some embodiments, the positive and / or negative electroactive regions are loaded with a particle suspension that is stabilized by repulsive forces between particles induced by an electrostatic double layer or by short-range spatial forces caused by an added surfactant or dispersant. After loading, the particle suspension is aggregated and densified by increasing the salt concentration of the suspension. In some embodiments, the added salt is a salt of a working ion for a battery (e.g., a lithium salt for a lithium ion battery), and when added, the liquid phase is changed to an ion-conducting electrolyte (e.g., for a rechargeable lithium battery, it may be one or more alkyl carbonates or one or more ionic liquids). When the salt concentration is increased, the electric double layer that causes the particles to repel each other "collapses", and attractive interactions cause the particles to flocculate, aggregate, consolidate or otherwise densify. This allows the battery's electrodes to be formed by the suspension when it has a low viscosity, such as by pouring, injecting or pumping to the positive and / or negative electroactive regions that can form a mesh electrode, and then allows the particles in the suspension to be consolidated for improved conductivity, higher packing density and longer shelf life.
[0113] In some embodiments, the cathode and / or anode semi-solid suspension may be initially flowable and may become non-flowable by "fixing". In some embodiments, fixation may be performed by the action of an electrochemical cycling battery. In some embodiments, the electrochemical cycling is performed within the current, voltage, or temperature range that the battery is subsequently used. In some embodiments, fixation is performed by electrochemical cycling of the battery to achieve a higher or lower current, higher or lower voltage, or higher or lower temperature than the range that the battery is subsequently used. In some embodiments, fixation may be performed by the action of photopolymerization. In some embodiments, fixation is performed by the action of electromagnetic radiation having a wavelength transmitted by the unfilled positive and / or negative electroactive regions of the electrochemical cell formed by the semi-solid cathode and / or semi-solid anode. In some embodiments, one or more additives are added to the semi-solid suspension to promote fixation.
[0114] In some embodiments, the injectable and flowable cathode and / or anode semisolids become less flowable or more flowable by "plasticization". In some embodiments, the rheological properties of the injectable and flowable semisolid suspensions can be changed by adding diluents, thickeners and / or plasticizers. In some embodiments, these reagents promote processability and help to maintain the uniformity of the composition of the semisolid under flow conditions and positive and negative electroactive zone filling operations. In some embodiments, one or more additives can be added to the flowable semisolid suspension to adjust its flow properties to adapt to processing requirements.
[0115] Figure 1B 1 is a flow chart illustrating a process 100B for repairing / regenerating electrode materials according to one embodiment. According to process 100B, one or more depleted electrode materials are first obtained at 110, optionally by separating (at 120) the one or more depleted electrode materials from an electrochemical cell that has reached its "end of service" or has at least partially degraded so that its active materials are no longer stoichiometric (i.e., there has been a change in the relative amounts of its components). Separation 120 may involve disassembling the electrochemical cell (the structure of which is discussed in detail above).
[0116] The separation of depleted electrode material (e.g., anode or cathode material) from an electrochemical cell may include mechanical removal, such as by scraping, brushing, wrinkling of a current collector, such that the depleted electrode material peels off, etc. In some embodiments, the separation of depleted electrode material from an electrochemical cell does not involve the use of chemicals (i.e., only mechanical). In some embodiments, the separation of depleted electrode material from an electrochemical cell includes "clean" removal of electrode material from its corresponding current collector (i.e., such that there is little or no damage to the current collector, and / or substantially no current collector material is present in the separated electrode material). Mechanical separation of depleted semi-solid electrode material (i.e., separation from a current collector) may particularly require only low applied force for removal.
[0117] The depleted electrode material is loaded into a processing vessel at 140. The processing vessel is selected based on the separation technique that will be subsequently used at 150. For example, the processing vessel may include, for example, a centrifuge vial / tube, a separation chamber of an air classification machine, a beaker, a tank, or any other suitable container. The depleted electrode material is then at least partially separated into component parts at 150 by using one or more separation techniques, such as centrifugation, air classification, or any other suitable separation / classification technique (e.g., filtration, sieving, sedimentation, field flow classification, electrophoresis, and / or the like). In certain embodiments of the method, the component materials may be separated based on other physical properties (e.g., magnetic properties), provided that there are significant differences in the relevant physical properties between the various components.
[0118] At least one component of the depleted electrode material is then optionally cleaned or washed at 130 to remove one or more residues, such as electrolyte salts. The cleaning medium can be any polar organic solvent such as dimethyl carbonate ("DMC") or any solvent that is miscible with the electrolyte and in which the electrolyte salt is soluble. The cleaning can be performed, for example, by immersing the depleted electrode material in a cleaning medium / solvent (e.g., in a jar, beaker, or other suitable container) with or without stirring. In some embodiments, the cleaning medium can be recycled or reused during or after process 100B. In the case of an electrode material having a surface reaction product such as an SEI, the cleaning or washing procedure can also remove such a reaction product. As a non-limiting example, a carbonaceous anode compound for a lithium ion battery may have a surface SEI composed at least in part of lithium carbonate. The anode can be cleaned in an acidic aqueous medium to remove the SEI. As a further non-limiting example, there may be surface reaction products formed by the decomposition of an electrolyte or other battery components that accumulate on the surface of the cathode active material. These surface layers can be removed by treatment with a cleaning solvent that preferentially dissolves these surface layers, or by a thermal treatment step, or both.
[0119] Optionally, process 100B forms a loop at 155B (i.e., steps 140, 150, and 130 may be repeated in a loop) such that one or more cleaned components (e.g., active materials) resulting from cleaning 130 are again loaded into a processing vessel at 140 for a second separation step 150 (which may involve the same separation technology used during the first pass, or alternatively, a different technology (e.g., centrifugation or air classification)). One or more "separation and cleaning" loops 155B may be performed as part of process 100B.
[0120] At 160B, at least one component (e.g., active cathode material, active anode material, or conductive carbon material) is recovered from the cleaning medium for reuse. A post-treatment step may be applied to the recovered component material at 170, for example, to correct its composition, or to repair or reconstruct it in other ways. For example, post-treatment may include adding one or more "missing" components by mixing (e.g., in the case where the original depleted electrode material is a cathode material, a lithium source such as lithium carbonate, lithium hydroxide, lithium nitrate, lithium sulfate, or any lithium salt may be added). In some embodiments, the at least one component, optionally in combination with any additive or material described herein, is formed into or incorporated into a fresh, recycled electrode. The repair atmosphere may be similar to the atmosphere used when the electrode material was originally produced (i.e., before depletion or at its original manufacture). For example, the repair of metal oxide cathodes such as LCO, NCM, NCA, LMO, LCP, and LNP can be carried out in an oxidizing or inert atmosphere, while the repair of metal oxide phosphates such as LFP, LMP, and LMFP can be carried out in an inert or reducing environment. Oxide anodes such as LTO can be repaired by firing in an oxidizing environment, while easily oxidized anodes such as carbon, metal alloys or silicon can be repaired by heat treatment in an inert or reducing environment. The regenerated electrode material and / or the recycled electrode can be subjected to one or more heat treatment steps, for example, to restore the crystal order and / or densify the regenerated material. In at least some embodiments, less heat energy input is used than in the original material synthesis, for example, by heat treatment at a lower temperature and / or time than the original synthesis conditions.
[0121] Figure 2 2 is a flow chart showing the evolution of the composition of an electrode material according to one embodiment. As shown, the use and recycling cycle 200 begins at 201 with a substantially stoichiometric (Li 1.17 Ni 0.37 Co 0.38 Mn 0.38 O2) NCM 111 cathode (e.g., as part of an electrochemical cell). Over time and / or use, the cathode material becomes depleted, resulting (at 221) in a non-stoichiometric NCM composition (e.g., shown as Li0.84 Ni 0.63 Co 0.25 Mn 0.38 O2). Then, on the non-stoichiometric / depleted NCM cathode material, for example, Figure 1A and 1B The described regeneration process resulted in 261 refurbished NCM 111 (Li 1.17 Ni 0.37 Co 0.38 Mn 0.38 O2) cathode. In some embodiments, the refurbished NCM cathode is substantially stoichiometric. In some embodiments, the refurbished NCM cathode is substoichiometric, but to a lesser extent than before regeneration. Many other electrode compositions (e.g., Li 1+x (Ni 0.5 Co 0.2 Mn 0.3 ) 1-y O2 ("NCM523"), Li 1+x (Ni 0.4 Co 0.2 Mn 0.4 ) 1-y O2 ("NCM424") and any other electrode described herein) may also exhibit compositional changes through use, and stoichiometric repair may be achieved through the regeneration methods presented herein.
[0122] Figure 3 is a photographic view of a sealed / packaged electrochemical cell prior to disassembly according to one embodiment.
[0123] Figure 4A is a schematic diagram of a detachable electrochemical cell according to one embodiment. A cathode (e.g., a semi-solid cathode) is arranged on a first surface of the positive current collector 400a near the separator 400b. The second surface of the positive current collector 400a far from the separator 400b is not coated. Similarly, an anode (e.g., a semi-solid anode) is arranged on a first surface of the negative current collector 400c near the separator 400b. The second surface of the negative current collector 400c far from the separator 400b is not coated. In other words, the cathode and the anode are arranged / coated only on one side of the positive current collector 400a and the negative current collector 400c, respectively. Although the electrode coating in this embodiment is only on one side of the corresponding current collector, the method is not limited in any way (e.g., double-sided electrodes can also be repaired according to the embodiments described herein). The cathode and the anode may include any components described herein with respect to the electrochemical cell structure (e.g., active materials and / or conductive materials, electrolytes, additives, gel polymers, etc.). Figure 4B is an illustration of a mechanical electrode material removal process according to one embodiment. Figure 4BAs shown, the cathode material disposed on the positive electrode collector 400a is scraped off the positive electrode collector 400a using a blade to obtain a separated depleted electrode material (cathode material in this case) 400d. Figure 5A and 5B Photographic partial views of positive (cathode) and negative (anode) current collectors, respectively, from which their respective electrode materials have been physically / mechanically removed, according to one embodiment.
[0124] Figure 6 is a photographic partial view of a centrifuge tube / vial containing cathode material that has been recovered (e.g., by mechanical separation from the current collector) but not yet centrifuged, according to one embodiment. Figure 6 As shown, about 15mL (height indicated by 620) of the recovered depleted cathode material has been loosely broken up and transferred to centrifuge vial "C". After this stage, a solvent such as DMC is added to the centrifuge vial, filling it to a total volume of about 50mL. As described herein, the solvent can be a freshly supplied solvent, or it can be a solvent previously used to clean / wash the depleted cathode material (and therefore can contain one or more dissolved salts and / or other residues). The vial is mechanically agitated (shaken) to disperse the solid material into the thin slurry, and then centrifuged. Figure 7 yes Figure 6 A photographic partial view of a centrifuge tube / vial showing the separated / stratified layers of depleted cathode material after centrifugation according to one embodiment. Figure 7 , the layers include supernatant 730a (solvent with dissolved electrolyte salts and / or other residues), conductive carbon 730b, and active material 730c. In some embodiments, supernatant 730a is then decanted and mixed with a non-polar solvent such as hexane to precipitate the salts for subsequent purification and / or use. In some embodiments, the conductive carbon and / or active material are removed and either immediately reused / reused or undergo additional washing and / or separation steps, as described herein, for example with reference to Figure 1A and 1B described.
[0125] In another embodiment, a similar method is used to repair an anode active material such as graphite from a negative electrode of an electrochemical cell, such as one disposed in Figure 4A The anode (eg, a semi-solid anode) shown on the negative electrode current collector 400c in FIG. Figure 5BAs shown, the anode material disposed on the negative current collector has been scraped off the negative current collector 514, resulting in the recovery of "waste" electrode material (in this case, anode material) 515. This recovered material is then further processed to recover and repair the active graphite material. In one embodiment, this recovered material containing residual electrolyte salts, SEI products, graphite active materials and conductive carbon is transferred to a centrifuge tube. A cleaning solution such as DMC is added, and the mixture is mechanically stirred to dissolve the residual electrolyte salt. This slurry is then centrifuged to separate the solid from the supernatant. The supernatant is separated (poured out) and added to a non-polar liquid such as hexane to precipitate a solid electrolyte salt that can be optionally purified. This washing process can be repeated until all the electrolyte salts are removed. The remaining solids, which now contain only SEI products, graphite active materials and conductive carbon, are now treated with an acid aqueous solution such as 1M hydrochloric acid to dissolve the SEI products. Again, a washing and centrifugation process is used to separate the graphite active material and the conductive carbon, using water as a cleaning solution. The material is washed with water and centrifuged repeatedly until the supernatant is essentially neutral (neither acidic nor basic). The recovered solid is now a mixture of graphite active material and carbon black. This solid mixture is ground to produce a free-flowing powder and separated using an air classifier, which separates the conductive carbon from the graphite active material.
[0126] The methods described herein can also be applied to any electrode material (i.e., non-depleted, stoichiometric, or substantially stoichiometric), such as waste electrode material from an electrode manufacturing process. Such waste material may not be "depleted," but may be subjected to one or more of the following: cleaning, separation, reconstitution / repair, thermal treatment (e.g., for re-densification), etc., so that it can be incorporated into a fresh electrochemical cell.
[0127] Although various embodiments of systems, methods and devices have been described above, it should be understood that they are provided as examples rather than limitations. Where the above methods and steps indicate that certain events occur in a certain order, those skilled in the art who benefit from the present disclosure will recognize that the ordering of certain steps can be changed, and such changes are in accordance with variations of the present invention. In addition, certain steps can be performed simultaneously in a parallel process if possible, and in the order as described above. In addition, one or more steps can be repeated in a given process. Embodiments have been specifically shown and described, but it will be understood that various changes in form and detail can be performed.
[0128] The present invention also relates to the following items:
[0129] Item 1: A method for repairing an electrode, the method comprising:
[0130] obtaining electrode materials;
[0131] cleaning at least a portion of the electrode material to remove residue; and
[0132] Separate electrode materials into their components for reuse.
[0133] Item 2. A method according to Item 1, wherein the electrode material is a depleted electrode material.
[0134] Item 3. A method according to Item 1, wherein the electrode material is a semi-solid electrode material.
[0135] Item 4. A method according to Item 1, wherein the electrode material is substantially free of a binder.
[0136] Item 5. A method according to Item 1, wherein separating the electrode material comprises at least one of centrifugation and air classification.
[0137] Item 6. A method according to Item 1, wherein obtaining the electrode material comprises disassembling an electrochemical cell containing the electrode material.
[0138] Item 7. A method according to Item 6, wherein obtaining the electrode material further comprises physically removing the electrode material from a portion of the disassembled electrochemical cell.
[0139] Item 8. The method according to Item 1, further comprising:
[0140] combining an additive with at least one of the separated components of the electrode material to alter its stoichiometry and / or crystallinity; and
[0141] The combined additive and at least one of the separated components of the electrode material are heat treated to form a repaired electrode material.
[0142] Item 9. The method according to Item 8 further comprises:
[0143] The repaired electrode material is incorporated into an electrochemical cell.
[0144] Item 10. A method according to Item 8, wherein the electrode material is a cathode material and the additive is a lithium-containing additive.
[0145] Item 11. A method according to Item 8, wherein the electrode material is a cathode material and the heat treatment is carried out in an oxidizing or inert atmosphere.
[0146] Item 12. The method according to Item 11, wherein the electrode material comprises LiCoO2 ("LCO"), Li(Ni,Mn,Co)O2 ("NMC"), LiNi 0.8 Co0.15 Al 0.05 At least one of O2 ("NCA"), LiMn2O4 ("LMO"), LiCoPO4 ("LCP"), and LiNiPO4 ("LNP").
[0147] Item 13. The method according to Item 11, wherein the electrode material comprises LiFePO4 ("LFP"), LiMnPO4 ("LMP"), LiMn 1-x Fe x PO4 ("LMFP") and Li4Ti5O 12 (“LTO”).
[0148] Item 14. A method according to Item 8, wherein the electrode material is an anode material, and the heat treatment is carried out in a reducing or inert atmosphere.
[0149] Item 15. A method according to Item 1, wherein separating the electrode material includes using centrifugation and causing the components to settle into layers.
[0150] Item 16. A method according to Item 1, wherein separating the electrode materials includes using air classification and causing the components to settle into layers.
[0151] Item 17. The method according to Item 1, further comprising:
[0152] The electrode material is loaded into a process vessel.
[0153] Item 18. A method according to Item 1, wherein cleaning comprises immersing at least a portion of the electrode material in an organic solvent.
[0154] Item 19. A method according to Item 1, wherein at least a portion of the electrode material is washed before separating the electrode material into multiple components.
[0155] Item 20. A method according to Item 1, wherein the electrode material is separated before cleaning.
[0156] Item 21. A method according to Item 1, wherein the cleaning is a first cleaning and the separation is a first separation, and the method further comprises a second cleaning and a second separation.
[0157] Item 22. A method for recycling electrode materials, the method comprising:
[0158] separating the binder-free electrode material from the current collector;
[0159] washing the binder-free electrode material to remove residue; and
[0160] The binder-free electrode material is separated into components for reuse.
[0161] Item 23. The method according to Item 22 further comprises:
[0162] An additive is combined with at least one of the isolated components to alter its stoichiometry and / or crystallinity.
[0163] Item 24. A method according to Item 23, wherein the binderless electrode material is a cathode material and the additive is a lithium-containing additive.
[0164] Item 25. The method according to Item 23 further comprises:
[0165] At least one of the additive and the separated components is heated to produce a repaired electrode material.
[0166] Item 26. A method according to Item 22, wherein separating the binder-free electrode material from the current collector includes using at least one of centrifugation, air classification, filtration, screening, sedimentation, field flow classification and electrophoresis.
[0167] Item 27. A method according to Item 22, wherein cleaning the binder-free electrode material comprises immersing at least a portion of the binder-free electrode material in an organic solvent.
[0168] Item 28. The method of item 22, wherein the residue comprises an electrolyte salt, an electrolyte solvent, and at least a portion of a reaction product, the reaction product comprising a solid electrolyte interphase material.
[0169] Item 29. A method for recycling electrode materials, the method comprising:
[0170] obtaining electrode materials;
[0171] washing the electrode material to remove at least a portion of the electrolyte salt, electrolyte solvent, and reaction products; and
[0172] The electrode material is separated into a first portion and a second portion, the first portion comprising an active electrode material and the second portion comprising a conductive carbon material.
[0173] Item 30. A method according to Item 29, wherein the electrode material is substantially free of a binder.
[0174] Item 31. The method according to Item 29, further comprising:
[0175] The electrode material is separated into a third portion, the third portion comprising a metal.
[0176] Item 31. A method according to Item 29, wherein the reaction product is a solid electrolyte interphase material.
[0177] Item 32. A method according to Item 29, wherein separating the electrode material into a first part and a second part comprises using at least one of centrifugation, air classification, filtration, screening, sedimentation, field flow classification and electrophoresis.
Claims
1. A method for repairing an electrode, the method comprising: obtaining a semisolid electrode material by mechanically separating the semisolid electrode material from a current collector, the semisolid electrode material comprising an active material, a conductive additive, an electrolyte salt, and an electrolyte solvent, and being substantially free of a binder and a current collector material after separation; washing the semisolid electrode material with an organic solvent to remove the electrolyte salt and the electrolyte solvent from the active material and the conductive additive; separating the semisolid electrode material into a first portion and a second portion using at least one of air classification, field flow fractionation, and electrophoresis, the first portion comprising the active material and the second portion comprising the conductive additive; wherein the semi-solid electrode material is a depleted semi-solid electrode material; and wherein the semi-solid electrode material is separated mechanically in the absence of chemicals.
2. The method according to claim 1, further comprising: combining an additive with at least one of the separated components of the semisolid electrode material to alter its stoichiometry and / or crystallinity; and The combined additive and at least one of the separated components of the semi-solid electrode material are heat treated to form a repaired semi-solid electrode material.
3. The method according to claim 2, further comprising: The repaired semisolid electrode material is incorporated into an electrochemical cell.
4. The method of claim 2, wherein the semi-solid electrode material is a cathode material and the heat treatment is performed in an oxidizing or inert atmosphere.
5. The method of claim 4, wherein the semi-solid electrode material comprises LiCoO2 ("LCO"), Li(Ni,Mn,Co)O2 ("NMC"), LiNi 0.8 Co 0.15 Al 0.05 At least one of O2 ("NCA"), LiMn2O4 ("LMO"), LiCoPO4 ("LCP"), and LiNiPO4 ("LNP").
6. The method of claim 4, wherein the semi-solid electrode material comprises LiFePO4 ("LFP"), LiMnPO4 ("LMP"), LiMn 1-x Fe x PO4("LMFP") and Li4Ti5O 12 ("LTO").
7. The method according to claim 1, wherein the organic solvent comprises at least one of ethyl methyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, dibutyl carbonate, butyl methyl carbonate, butyl ethyl carbonate, butyl propyl carbonate, γ-butyrolactone, dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 4-methyl-1,3-dioxolane, diethyl ether, cyclopentane, methyl cyclopentane, acetonitrile, propionitrile, ethyl acetate, methyl propionate, ethyl propionate, tetraethylene glycol dimethyl ether and 1,3-dioxolane.
8. The method according to claim 1, further comprising: The semi-solid electrode material is loaded into a processing vessel.
9. The method of claim 1, wherein the cleaning is a first cleaning and the separating is a first separating, the method further comprising a second cleaning and a second separating.
10. An electrode repair method, comprising: mechanically separating a binder-free semisolid electrode material from a current collector, the electrode material comprising an active material, a conductive additive, an electrolyte salt, and an electrolyte solvent and being substantially free of a binder and a current collector material after the separation; separating the binder-free electrode material into a first portion and a second portion using at least one of air classification, field flow fractionation, and electrophoresis, the first portion comprising the active material and the second portion comprising the conductive additive; wherein the semi-solid electrode material is a depleted semi-solid electrode material; and wherein the semi-solid electrode material is separated mechanically in the absence of chemicals.
11. The method according to claim 10, further comprising: An additive is combined with at least one of the isolated components to alter its stoichiometry and / or crystallinity.
12. The method of claim 11, wherein the binderless electrode material is a cathode material and the additive is a lithium-containing additive.
13. The method according to claim 11, further comprising: At least one of the additive and the separated components is heated to produce a repaired binder-free electrode material.
14. The method of claim 10, wherein separating the binder-free electrode material from the current collector further comprises using at least one of centrifugation, filtration, screening, and sedimentation.
15. The method of claim 10, wherein the binderless semi-solid electrode material is mechanically separated from the current collector in the absence of chemicals, wherein substantially no current collector material is present in the binderless electrode material after separation.
16. The method of claim 10, wherein the binder-free semi-solid electrode material is mechanically separated from the electrode material and washed with an organic solvent to remove residues.
17. The method of claim 16, wherein washing the binderless semi-solid electrode material comprises immersing at least a portion of the binderless electrode material in the organic solvent.
18. The method of claim 16, wherein the residue comprises an electrolyte salt, an electrolyte solvent, and at least a portion of a reaction product, the reaction product comprising a solid electrolyte interphase material.
19. A method for recycling a semi-solid electrode material, the method comprising: obtaining an electrode material by mechanically separating a semi-solid electrode material from at least one of a current collector and a separator in the absence of heat and chemicals, the semi-solid electrode material being substantially free of a binder and a current collector material after separation; washing the electrode material with an organic solvent to remove at least a portion of the electrolyte salt, the electrolyte solvent, and the reaction product; separating the electrode material into a first portion and a second portion using at least one of air classification, field flow fractionation, and electrophoresis, the first portion comprising an active electrode material and the second portion comprising a conductive carbon material; and The semi-solid electrode material is a depleted semi-solid electrode material.
20. The method of claim 19, wherein the organic solvent comprises at least one of ethyl methyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, dibutyl carbonate, butyl methyl carbonate, butyl ethyl carbonate, butyl propyl carbonate, γ-butyrolactone, dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 4-methyl-1,3-dioxolane, diethyl ether, cyclopentane, methyl cyclopentane, acetonitrile, propionitrile, ethyl acetate, methyl propionate, ethyl propionate, tetraethylene glycol dimethyl ether and 1,3-dioxolane.
21. The method of claim 19, further comprising: The electrode material is separated into a third portion, the third portion comprising a metal.
22. The method of claim 19, wherein the reaction product is a solid electrolyte interphase material.
Citation Information
Patent Citations
Conductive lithium storage electrode
US7338734B2
Stationary, fluid redox electrode
WO2012024499A1
Semi-solid electrodes having high rate capability
WO2014093876A1
Reintroduction of lithium into recycled battery materials
CN102017277A
Method for recovering oxide-containing battery material from waste battery material
CN102077409A