Tube testing methods and equipment
By applying force on the annular sample of deep-water subsea pipeline and measuring positioning shift and stress, the accuracy and cost of the external pressure collapse test of pipeline in deep-water environment is solved, and an effective evaluation of pipeline performance is achieved.
Patent Information
- Application Number
- CN202110956704.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-06-20
- Filing Date
- 2018-06-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2038-06-19
AI Technical Summary
During the installation of deep-water subsea pipelines, external pressure leads to pipeline collapse. The existing testing methods are expensive and insufficient in accuracy, making it difficult to effectively evaluate the performance of pipelines in ultra-deep water environments.
An apparatus and method for testing an annular sample is designed, including two test chambers, sealing means, hydraulic cylinder, sensor and fluid inlet, and by applying force on the inner surface of the test ring and determining its displacement and stress, the Whether it is properly assembled and performed external pressure collapse test.
Improves the accuracy of external pressure collapse testing, reduces testing costs, and can effectively evaluate the performance of the pipeline in a smaller pressure chamber, ensuring the stability of the pipeline in deep water environments.
Smart Images

Figure CN113654904B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method and an apparatus for testing a pipe, for example for forming an underwater pipeline. Background Art
[0002] In the oil and gas industry, the manufacture of subsea pipelines suitable for installation and operation in ultra-deep water to access deepwater reservoirs of oil and / or natural gas has been steadily developing for nearly 20 years. Currently, small diameter pipes of about 16 inches (about 40.6 cm) in diameter are installed in water at a depth of 3,000 meters. Larger diameter pipes of up to 32 inches (81.1 cm) in diameter are installed in water at depths of up to 2,500 meters. Future projects may require the installation and operation of pipes in water as deep as 3,500 meters or even deeper.
[0003] The pipe is usually empty during installation, i.e. filled with air at ambient pressure, and is only filled with oil or gas under pressure once installation is complete. The main risk experienced when installing these deepwater pipelines is that the pressure exerted by the water causes the pipe to deform from an initial actual circular shape to an almost flat shape. This phenomenon is called external pressure collapse, which, if not controlled, will lead to the overall loss of the pipeline. Therefore, the size (i.e. diameter and wall thickness) of the extremely deepwater pipeline, and to a certain extent, the material properties of the extremely deepwater pipeline, are the main driving factors that determine the possibility of external pressure collapse. This is different from the design of traditional shallow water or onshore pipelines, where the wall thickness of shallow water or onshore pipelines is sized to resist the internal pressure from the fluid it carries, rather than the external pressure.
[0004] In order to design and manufacture thick-walled pipes, and thus manufacture pipelines for operation in ultra-deep water (i.e., depths greater than 2000 meters), design guidance is provided in DNV OS 101, in which the safety from pressure collapse during pipeline installation depends on the safety factor used. The safety factor is calibrated using the Load and Resistance Factor Design (LRFD) method and a comparison of the collapse pressure test results available when preparing the DNV guidance. Due to the huge financial issues involved in the loss of very long pipes during installation in ultra-deep water, in practice, the pipeline is further designed based on specific pipe joint collapse tests combined with DNV information. However, pressure testing of full-size pipe joints is an expensive process that requires appropriate pressure chambers. There are only a few chambers in the world that are capable of applying pressures corresponding to ultra-deep water, and it may be inconvenient and expensive to transport the pipe from the pipe mill to a suitable testing facility.
[0005] Alternative methods to assist in optimising pipe design, particularly pipe wall thickness, have been proposed to replace full-scale pipe testing. In WO2008 / 114049 a method and apparatus for testing pipes used in the manufacture of subsea pipelines is described which involves external pressure collapse testing of annular specimens cut and machined from manufactured pipe joints.
[0006] The present invention relates to a method and apparatus for improving the accuracy of an external pressure collapse test performed on annular specimens, such as the test described in WO 2008 / 114049. Summary of the invention
[0007] The present invention provides apparatus and methods for testing pipe used in the manufacture of pipelines for deepwater subsea environments.
[0008] Thus, one aspect of the invention comprises an apparatus for testing rings cut from a pipe used in the manufacture of a subsea pipeline, the apparatus comprising:
[0009] a first test chamber portion and a second test chamber portion that, when the first test chamber portion and the second test chamber portion are connected together, define a test chamber for receiving a test ring;
[0010] sealing means for forming a seal with the ring when the ring is installed in the chamber;
[0011] means for connecting the first and second parts together to form the chamber and for engaging the sealing means with the test ring to form a pressure-tight seal between an interior of the ring and an exterior of the ring when the test ring is installed in the chamber;
[0012] a fluid inlet in one of the chamber portions to allow pressurized fluid to enter the chamber outside the test ring;
[0013] a hydraulic cylinder for applying a force to an inner surface of the test ring when the test ring is installed in the chamber;
[0014] at least one sensor for measuring the force applied by the hydraulic cylinder to the test ring;
[0015] at least one sensor for measuring movement of the test ring; and
[0016] At least one sensor for determining stress and deformation of the test ring.
[0017] In use, a test ring is positioned between the first test chamber portion and the second test chamber portion and is engaged with a sealing arrangement such that an inner surface of the ring is isolated from an outer surface of the ring. The inner surface of the ring is exposed to atmospheric conditions. The outer surface of the ring may be exposed to a pressurized fluid in the chamber.
[0018] The apparatus may comprise means for pumping fluid to the hydraulic cylinder. Preferably, the means for pumping fluid to the hydraulic cylinder is a needle pump.
[0019] Preferably, the device comprises at least two sensors for determining the movement of the test ring. The sensors for determining the movement of the test ring are preferably displacement sensors. The sensors determine the movement of the test ring relative to the chamber part in which the test ring is mounted.
[0020] The sensor for determining the force applied by the hydraulic cylinder to the test ring is preferably a dynamometer.
[0021] The opposing surfaces of the test chamber parts are provided with at least one circumferential groove. A sealing device is located in each groove. Preferably, each test part has two circumferential grooves on its surface. The sealing device is preferably an elastic O-ring.
[0022] The apparatus may further comprise a spacer ring positioned between the first portion and the second portion. The spacer ring together with the first portion and the second portion may define the test chamber for accommodating the test ring.
[0023] Another aspect of the invention comprises a method of determining whether a test ring is correctly fitted in a test chamber for testing a pipe used in the manufacture of a subsea pipeline, wherein the test ring is cut from a pipe used in the manufacture of the pipeline and has substantially flat and parallel surfaces at the ends of the test ring; the method comprising:
[0024] i) installing the test ring into a pressure chamber so that an end of the test ring forms a seal with an opposing surface of the chamber to isolate the interior of the test ring from the exterior;
[0025] ii) providing means for determining the displacement of said test ring;
[0026] iii) providing means for determining the force applied to the inner surface of said test ring;
[0027] iv) applying a force to the inner surface of the test ring;
[0028] v) determining the displacement of the test ring and determining the force applied to the inner surface; and
[0029] vi) Using the displacement measurements and the force measurements to determine whether the test ring is correctly installed in the pressure chamber.
[0030] During the test, increasing forces are applied to the inner surface of the test ring at a predetermined time and rate. If the displacement measurements and force measurements indicate that the restraining force applied by the sealing device exceeds the permissible force range, subsequent pressure collapse tests on the test ring will not be continued. If the results indicate that the restraining force is within the permissible range, the pressure collapse test may continue.
[0031] The maximum acceptable force depends on the outer diameter of the test ring. For example, for a ring with an outer diameter of approximately 30 inches (76.2 cm), the maximum acceptable force applied by the hydraulic cylinder is preferably in the range of 0.1 kN to 6.5 kN. However, the range of acceptable forces will also depend on the pressure in the pressure chamber. If the pressure chamber is not pressurized, the maximum acceptable force for a ring with an outer diameter of approximately 30 inches (76.2 cm) is preferably in the range of 0.1 kN to 0.4 kN, preferably approximately 0.25 kN. If the pressure chamber is pressurized, for example at a pressure of 27 MPa, the maximum acceptable force will be in the range of 4.5 kN to 6.5 kN, preferably approximately 5.0 kN. Prior to testing, the maximum allowable force for diameters other than 30 inches (76.2 cm) can be determined.
[0032] When the force is applied to the inner surface of the test ring, the pressure in the pressure chamber may be about 0 MPa. Preferably, the test may be performed with a pressurized chamber so that the pressure is applied to the outer cylindrical surface of the test ring. In this case, a test is performed with a pressure in the pressure chamber above 0 MPa but below the expected collapse pressure of the pipe. The test may be performed with a pressure in the pressure test chamber in the range of 0 to 30 MPa or more, preferably in the range of 0 to 15 MPa or more. The pressure in the pressure chamber may be in the range of 0 to 0.7 times the expected collapse pressure of the pipe, preferably in the range of 0.5 to 0.7 times the expected collapse pressure.
[0033] The method may further comprise: once the test ring moves a predetermined distance, stopping the application of force to the inner surface of the test ring, i.e., stopping step iv) once the test ring moves a predetermined distance. Preferably, the predetermined distance is about 1 mm to 2 mm, preferably about 1 mm. Once the sensor detects that the test ring has moved a predetermined distance, pumping the fluid into the hydraulic cylinder is stopped, and the obtained measurement value can be used to determine whether the test ring has been correctly installed in the test chamber.
[0034] The steps of applying a force to the inner surface of the test ring and measuring the displacement of the test ring and the applied force may be repeated, when the force is applied to the inner surface of the test ring, the outer cylindrical surface of the test ring is subjected to a pressure different from the applied first pressure.
[0035] Before executing the above method, the same device may be used to perform a test to determine the range of permissible restraining forces. Therefore, in one embodiment of the present invention, the test may further include: determining the range of permissible restraining forces before executing steps i) to vi).
[0036] In this test, the force application and determination steps may be performed more than once, preferably each time for a new test ring. When the force application step is repeated, the method may include providing a second pressure to the pressure chamber, wherein the second pressure is above 0 MPa and below the expected collapse pressure when the force is applied to the inner surface of the test ring. With this method, the further repeating step may also include providing a third pressure to the pressure chamber, wherein the third pressure is above 0 MPa and below the expected collapse pressure, and the third pressure is different from the first pressure and the second pressure when the force is applied to the inner surface of the test ring.
[0037] The results of performing the test can be used to confirm whether an acceptable restraining force exists between the test device and the test ring. The restraining force depends on the geometry of the ring, i.e. the diameter and width of the ring, and on the pressure in the pressure chamber. However, in some embodiments, the acceptable restraining force is in the range of 0.1KN to 30kN. When the pressure in the annular pressure chamber is approximately 0MPa, preferably, the acceptable force is in the range of 0.1N to 0.4kN, preferably approximately 0.2kN. When the pressure in the chamber is approximately 27.6Mpa, the acceptable restraining force is in the range of 4.5kN to 6.5kN, preferably approximately 5.0kN.
[0038] The method further comprises the steps of holding the test ring in the pressure chamber and performing an external pressure collapse test on the test ring. The external pressure collapse test may comprise:
[0039] providing means for determining stress and deformation of said test ring;
[0040] increasing pressure outside the test ring and measuring stress and deformation on the test ring as the pressure increases; and
[0041] The external collapse pressure of the test ring is determined.
[0042] Determining the collapse pressure of the test ring includes determining a comparison between the pressure applied to the exterior of the ring and the measured maximum stress to detect the onset of an accelerated non-linear decrease in ring diameter with increasing pressure.
[0043] Prior to installing the ring in the chamber, the method may further comprise the steps of:
[0044] Cutting rings from tubes used to make pipes; and
[0045] Substantially flat and parallel surfaces are formed at the ends of the ring.
[0046] Yet another aspect of the invention includes a method for testing a pipe used in the manufacture of a subsea pipeline, comprising:
[0047] cutting rings from said tube used to make said pipe;
[0048] forming substantially flat and parallel surfaces at ends of the ring;
[0049] installing the ring into a pressure chamber so that ends of the ring form a seal with opposing walls of the chamber to isolate the interior of the test ring from the exterior;
[0050] providing means for determining the displacement of said test ring;
[0051] providing means for determining the force applied to the inner surface of the test ring;
[0052] applying a force to an inner surface of the test ring;
[0053] measuring a displacement of the test ring and measuring a force applied to the inner surface;
[0054] using the displacement measurements and the force measurements to determine whether the test ring is properly assembled in the pressure chamber;
[0055] providing means for determining stress and deformation of said ring;
[0056] increasing the pressure outside the ring and measuring the stress and deformation on the ring as the pressure increases; and
[0057] A comparison between the pressure applied to the exterior of the ring and the measured maximum stress is determined to detect the onset of an accelerated non-linear decrease in the diameter of the ring with increasing pressure.
[0058] The applying of the force to the inner surface of the test ring comprises: applying the force until the force applied to the test ring exceeds the lateral resistance between the sealing device and the test ring. A device for applying the force to the inner surface of the test ring is provided. Preferably, a hydraulic cylinder is provided to apply the force to the inner surface of the test ring. The hydraulic cylinder is connected to a pump for supplying fluid to the hydraulic cylinder. Preferably, the pump is a needle pump. Preferably, the opposing walls of the pressure chamber are each provided with a sealing device so that the ends of the ring engage with the opposing sealing devices to isolate the inner surface of the ring from the outer surface of the ring.
[0059] The fluid is supplied to the cylinder to increase the force applied to the inner surface of the test ring. During the test, the rate of force applied is about 0.002 kN / min to 0.04 k N / min. Preferably, the force is applied to the inner surface of the test ring for a period of 30 minutes to 4 hours, preferably 1 hour to 3 hours, more preferably 1 hour to 2 hours.
[0060] The means for applying a force to the inner surface of the test ring is removed from the test ring prior to performing the step of increasing the pressure on the exterior of the ring.
[0061] Preferably, the method is performed using the above-mentioned device.
[0062] Another aspect of the invention is a pipe testing device for performing the above-mentioned testing method. BRIEF DESCRIPTION OF THE DRAWINGS
[0063] Embodiments of the present invention will now be described, by way of example only, with reference to the accompanying drawings, in which:
[0064] Figure 1 The type of pipe used for testing according to the present invention is shown;
[0065] Figure 2 Shows from Figure 1 Cross-section of a test ring cut from a tube;
[0066] Figure 3 A schematic diagram of a test device according to the present invention is shown;
[0067] Figure 4 Shown along Figure 3 The section of the BB line where the test equipment is set up for the test phase;
[0068] Figure 5 shows a schematic diagram of a test apparatus having a test ring installed therein;
[0069] Figure 6 The edge set up for the preparation phase is shown Figure 3 The part intercepted by the BB line;
[0070] Figure 7 shows a top view of the test equipment and the test ring set up for the preparation phase;
[0071] Figure 8 A schematic diagram showing the test equipment and test loop set up for the preparation phase;
[0072] FIG9 shows the results of push-out tests performed at three different pressure levels (a) 0 MPa, (b) 13.8 MPa and (c) 27.6 MPa, the graphs showing the results of frictional resistance and displacement over time, where Lino 1 (48) and Lino 2 (50) refer to the linear displacement sensors at two separate positions of the movement of the measuring ring relative to the test device;
[0073] Figure 10 shows the results of push-out tests performed at three different pressures (a) 0 MPa, (b) 13.8 MPa and (c) 27.6 MPa, the graph showing the relationship between the friction resistance and the lateral displacement of the ring, where Lino 1 (48) and Lino 2 (50) refer to linear displacement sensors at two separate positions where the movement of the ring is measured. DETAILED DESCRIPTION
[0074] Tests on longer sections of various pipe joints have shown that the deformation leading to external collapse is almost uniform along the length of the pipe. This observation is supported by theoretical studies, practical tests and numerical simulations. This means that the external pressure collapse occurs in the same way for a ring cut from the pipe and for the pipe simply subjected to external pressure over the entire length of the joint. Therefore, as described in WO 2008 / 114049, a test method has been developed based on cutting shorter sections from the pipe and machining the rings to uniform length. However, before performing such a pressure collapse test, it is important to correctly set up the test ring in the test equipment.
[0075] By "pressure collapse test" or equivalent test, it is meant a test in which the pressure at which the test ring will collapse is determined by the pressure at which the test ring specimen is subjected to increasing pressures, such as the test described in WO2008 / 114049 or the test described by Selker et al. in "Proceedings of the Twentyfourth (2014) International Ocean and Polar Engineering Conference", volume 2, pages 88-95.
[0076] The purpose of the sealing ring located between the two cutting surfaces of the ring and the chamber portion (between which the ring is clamped) is to help establish a pressure test chamber on the outside of the test ring. The pressure chamber is defined by the outer surface of the test ring and the surface of the test equipment. In the second stage of the test, the pressure in the chamber causes the ring to deform due to the compressive stress around the circumference of the ring caused by the applied pressure. The increasing pressure in the chamber eventually causes the collapse of the ring. In order to establish a seal sufficient to prevent leakage of high-pressure hydraulic fluid, the sealing ring must be subjected to a suitable high pressure at the interface between the sealing ring and the surface of the test ring.
[0077] The interface pressure has the effect of creating a frictional restraining force between the ring and the test apparatus. The restraining force varies with changes in the pressure within the chamber. Applying a lubricant to the rubber-steel interface (i.e., between the surfaces of the sealing ring and the test ring) at the beginning of the test can reduce the restraining force. The initial setting of the interface pressure, and the resulting restraining force, can be determined by the ring test apparatus and the amount of interface pressure applied to the sealing ring. The manner in which the lubricant is applied and the position of the ring during setup of the apparatus will also affect the restraining force and the final collapse pressure.
[0078] During the initial setup of the test equipment, variations in restraint forces may cause inconsistent results from one pressure collapse test to another. In addition, restraint forces between the sealing ring and the surface of the test ring may increase the pressure level that collapses the sealing ring. Therefore, for each pressure collapse test, an initial test is performed to determine whether the test ring is properly assembled in the test equipment.
[0079] Therefore, according to the present invention, a test method for testing a pipe used in manufacturing a submarine pipeline comprises two test phases: a first test phase (S1) and a second test phase (S2). The first test phase is a setting test phase (S1) to determine whether the test ring is correctly set in the test device. The second test phase is a pressure collapse test phase (S2) to determine the collapse pressure of the pipe.
[0080] In the setup test phase, a force is applied to the inner surface of the test ring and the displacement of the test ring is measured to help determine whether the test ring is properly set in the equipment. In the second pressure collapse test phase (S2), increasing pressure is applied to the outer surface of the ring to determine the collapse pressure of the tube. The stress and deformation measurements obtained in this phase can be used to determine the appropriate wall thickness for the tube. The second test phase (S2) is performed only if the results of the first test phase indicate that the test ring is properly set in the test equipment.
[0081] Figure 1A pipe 10 for use in a submarine pipeline is shown. A typical example of a pipe is approximately 12.2 meters long and has an outer diameter of 508 mm and a wall thickness of 35 mm. A test ring 12 (also shown in FIG. Figure 2 The test ring 12 is cut from one end of the pipe (as shown in FIG. 1 ), and has a typical length of 50 mm, i.e., the length is greater than the wall thickness. Even if a ring of this length is cut, the pipe can still be used to build a pipeline. The end surfaces of the ring are machined to be substantially parallel and flat, i.e., as smooth as a practical surface. Substantially flat and parallel means that there is a tolerance of ±0.01 mm over the entire length of the ring. Preferably, the roughness factor should not exceed ISO N6 grade.
[0082] A test ring cut from a tube and having a machined end surface of the ring is mounted in a rigid frame consisting of at least two parts and sealing means, thereby forming a pressure chamber. The sealing means allow the machined surface of the test ring to be sealed to the device so that when the chamber is pressurized, pressure is applied only to the outer cylindrical surface of the ring. The inner cylindrical surface of the ring remains at atmospheric pressure.
[0083] The seals on the two machined flat surfaces of the ring are seals such that deformation of the annular surface of the ring is hindered during the second phase (S2). The seals on the flat surfaces of the ring are seals such that during the test the pressure is limited only to the outer annular surface of the ring and to a small area of the flat machined surface. The seals are seals such that the ring is subjected to relatively small forces parallel to the machined flat surfaces, resulting in that radial deformation of the ring is hindered during the test phase (S2).
[0084] The first stage of the testing process (S1) may include the following steps:
[0085] i) installing a test ring, which has been cut from the tube and whose ends are machined flat and parallel within specified tolerances, into the test fixture and fitting the seal in place so that a chamber is defined by the outer surface of the test ring and the test fixture;
[0086] ii) attaching means for determining the displacement of said test ring;
[0087] iii) attaching means for applying a force to the inner surface of said test ring;
[0088] iv) applying a force to the inner surface of the ring and recording the force applied to the test ring and the displacement of the test ring relative to the apparatus;
[0089] Between steps iii) and iv) there may also be performed the step of applying pressure to the outer cylindrical surface of the ring and ensuring that the seal is available and effective.
[0090] A hydraulic cylinder is added to the test apparatus so that the hydraulic cylinder contacts one side of the inner surface of the test ring to apply a force to the inner surface of the ring. A dynamometer is arranged between the end of the cylinder and the inner surface of the test ring. A displacement sensor is attached to the test ring to measure any movement of the test ring relative to the test apparatus.
[0091] The hydraulic cylinder is connected to a needle pump, which injects hydraulic fluid or other suitable fluid (such as water) into the cylinder under a certain pressure. The cylinder extends as the pressure increases and comes into contact with the inner surface of the test ring, thereby applying a force to this surface. The pressure in the cylinder increases at a very slow rate through the continuous pumping of the needle pump. As the pressure increases, the force applied by the cylinder to the ring, measured by the pressure gauge, also increases. This force eventually exceeds the (until now) unknown restraining force, and the ring moves laterally. The movement of the test ring is measured by a displacement sensor. The movement of the test ring is preferably limited to 1 mm (millimeter). Once it is determined that the test ring has moved by approximately 1 mm, the pumping of fluid into the cylinder will be stopped.
[0092] The needle pump adds small amounts of fluid to the cylinder chamber at regular time intervals, thereby increasing the force applied to the test ring at a very slow rate. Preferably, the displacement rate caused by the incremental force applied by the hydraulic cylinder is in the range of 0.01 mm / min (millimeter / minute) to 0.05 mm / min, and more preferably, the displacement rate is in the range of about 0.01 mm / min to 0.03 mm / min.
[0093] Preferably, the time period for performing the first stage (S1) of the test is substantially the same as the time period for performing the second stage (S2) of the test. The pressure on the cylinder, and the force applied to the inner surface of the ring, may be increased over a time period of about 30 minutes to about 4 hours, preferably, over a time period of about 1 hour to about 2 hours. The rate at which the force is applied by the hydraulic cylinder to the inner surface of the test ring is in the range of about 0.002 kN / min (kilonewtons per minute) to about 0.04 kN / min.
[0094] As force is applied to the inner surface of the ring, pressure is maintained in the pressure chamber at a predetermined pressure. The first stage can be performed in the chamber at a pressure of 0 MPa (megapascals). Alternatively, the test can be performed in a pressurized chamber. The chamber can be pressurized to below the expected collapse pressure. The test can be performed with the pressure in the pressure chamber being above 0 to 30 MPa, preferably above about 0 to 15 MPa, and more preferably above about 0 to 6 MPa. Preferably, the maximum pressure in the chamber that can be used in the test is 0.5 to 0.7 times the expected collapse pressure test.
[0095] Before performing setup tests to determine if the test ring is properly installed in the test equipment to subsequently perform pressure collapse tests, initial tests are performed to determine the restraining force effects for the particular setup used. These initial commissioning tests are performed for the S1 test. In the initial commissioning tests, the measured forces applied by the cylinders are used in numerical modeling to determine if these forces will result in excessive collapse pressures. For example, the process of performing initial commissioning tests may include:
[0096] i) installing a test ring, which has been cut from the tube and whose ends are machined flat and parallel within specified tolerances, into the test fixture and fitting the seal in place so that a chamber is defined by the outer surface of the test ring and the test fixture;
[0097] ii) attaching means for determining the displacement of said test ring;
[0098] iii) attaching means for applying a force to the inner surface of said test ring;
[0099] iiia) applying a first pressure to the outer cylindrical surface of the test ring;
[0100] iv) applying a force to the inner surface of the test ring and recording the force applied to the test ring and the displacement of the test ring relative to the device.
[0101] Once the results of the first test are obtained, steps i) to iv) are repeated with a second pressure applied in step iiia). The test is repeated with a third pressure applied in step iiia). The first pressure, the second pressure and the third pressure are different from each other. The results of these tests can be used to determine the range of permissible restraining forces.
[0102] Through initial commissioning testing and numerical modeling, a range of allowable restraining forces was created for use in setup test S1 to determine if the test ring fits acceptably in the test apparatus so that collapse testing of the ring can proceed.
[0103] If the setup test S1 shows that the restraining force applied by the sealing ring exceeds the permissible force range, the test is not continued. The equipment should be dismantled and the ring inspected. The test ring can then be reassembled with the test equipment to repeat the initial setup test.
[0104] Once it is determined that the test ring is properly positioned in the test apparatus, the hydraulic cylinder and displacement sensor can be removed from the test apparatus without disturbing the position of the test ring in the test apparatus, and the second phase of the testing process, the pressure collapse test, can be initiated.
[0105] The testing phase (S2), i.e. the collapse pressure test, may be performed as described in WO2008 / 114049 to determine the collapse pressure of the test ring and may comprise the following steps:
[0106] attaching an accessory for determining stress and deformation of the ring to the ring, the ring being positioned within the frame and the seal being in place;
[0107] increasing the pressure applied to the exterior of the ring and recording stress measurements and deformation measurements; and
[0108] The pressure is continued to increase until a maximum value is reached, i.e. until external pressure collapse occurs.
[0109] It is also possible to plot applied pressure versus measured maximum stress to detect the onset of an accelerated non-linear decrease in ring diameter with increasing pressure, independent of any leakage of hydraulic fluid past the seal.
[0110] For the first stage of the test method, the device for applying force to the outer annular surface of the ring and measuring the displacement of the ring is attached to the outer surface. In the second stage, the device for applying force to the inner cylindrical surface and measuring the displacement is removed, and the device for measuring the stress and deformation caused by the pressure of the outer cylindrical surface of the ring is attached to the inner surface of the ring.
[0111] Two pumps are used in the test method. One pump supplies fluid to a hydraulic cylinder so that the cylinder applies force to the inner surface of the test ring. Another pump, such as another hydraulic pump, provides pressurized fluid to a pressure chamber, such as the space around the outer surface of the ring.
[0112] Pressure is applied from an external pump so that the pressure is increased or decreased by adding or subtracting a specified volume of fluid to or from the space surrounding the outer annular surface of the ring. This arrangement allows the radial deformation of the ring caused by the pressure on the outer cylindrical surface to be increased or decreased in a controlled manner. As the pressure is increased, stress measurements and deformation measurements are recorded until the maximum pressure is reached.
[0113] like Figure 3 As shown, a test device 14 according to the present invention that can be used to perform the test method includes a first cylindrical portion 16, a second cylindrical portion 18, and a spacer ring portion 20 located between the first cylindrical portion 16 and the second cylindrical portion 18, which define the device in which the test ring 12 can be installed. The first portion and the second portion can form the top portion and the bottom portion of the device, respectively. The outer diameter of the first portion substantially corresponds to the outer diameter of the second portion.
[0114] The first part may be in the form of a ring having a central hole 42. The central hole of the first part provides access to the center of the test device and the inner surface of the test ring for the attachment of sensors and hydraulic cylinders. The second part may also be in the form of a ring having a central hole. The diameter of the hole of the second part substantially corresponds to the diameter of the hole of the first part. Alternatively, the second part may be in the form of a cylindrical part having a bottom part in the form of a solid plate and a top part in the form of a ring, so that the second part has a central void. The central void substantially corresponds to the central hole of the first cylindrical part. The diameter of the void of the second part substantially corresponds to the diameter of the hole of the first part.
[0115] The opposing surfaces of the first and second portions, i.e. the bottom surface of the first portion and the top surface of the second portion, are stepped to form a shoulder 44 which extends circumferentially around the bottom and top edges of the first and second portions 16, 18, respectively. This provides a protruding annular stepped portion 46 between the shoulder and the aperture of each portion. The shoulder 44 of each portion provides a support surface to locate the spacer ring 20 between the support surfaces. The annular stepped portion 46 of each of the first and second portions provides a support surface to mount the test ring 12 on the support surface. The outer diameter of the annular stepped portion substantially corresponds to the inner diameter of the spacer ring 20.
[0116] The spacer ring 20 is located between the outer edges of the two parts 16, 18. The edge of the spacer ring abuts against the shoulder 44 of each part, and the inner circumferential surface of the spacer ring 20 will abut against the side surface of the annular stepped portion 46. The spacer ring 20 helps to adjust the distance between the two surfaces of the first part and the second part. The spacer ring and the first and second parts, when combined together, form a frame for holding the test ring 12 to be tested. The inner diameter of the spacer ring 20 is smaller than the outer diameter of the first part 16 and the second part 18, and is larger than the diameter of the various holes and gaps therein. The outer diameter of the spacer ring 20 is larger than the outer diameter of the first part 16 and the first part 18.
[0117] refer to Figures 4 to 8 When the test ring is positioned in the device, a test pressure chamber 26 is defined between the top surface of the bottom portion and the bottom surface of the top portion, and between the inside surface of the spacer ring and the outer cylindrical surface 40 of the test ring. The device is provided with an inlet 38 to provide pressurized fluid to the pressure chamber 26.
[0118] Each of the first and second parts has at least one circumferential groove 22 for retaining a sealing device 24 in the facing faces of the first and second parts. Figure 4 and Figure 6As shown, each part has two concentric grooves for retaining sealing rings disposed in the opposing faces of the annular stepped portion 46 of the first part 16 and the first part 18. The test ring engages with the sealing device 24 located in the groove 22. Preferably, the test ring engages with the sealing device 24 but does not contact the opposing faces of the first and second parts. An additional sealing device 28 is disposed between the spacer ring 20 and the side surfaces of the annular stepped portion 46 of the first and second parts 16, 18. In some embodiments, a shim (not shown) is used between the upper surface of the spacer ring 20 and the lower surface of the first part 16 and between the lower surface of the spacer ring 20 and the upper surface of the second part 18 to align the various components. The shim can be a metal shim, such as a brass shim. The shim can help ensure that the ring does not contact the first and second parts during testing to help ensure that the pressure between the sealing ring and the test ring is sufficient to prevent leakage during testing and is as low as possible to avoid excessive frictional restraint on the test ring.
[0119] Figure 4 and Figure 5 An embodiment of an apparatus 14 according to the invention is shown, the apparatus being provided with a test ring 12 for performing a collapse pressure test (S2). Figures 6 to 8 An embodiment of an apparatus 14 according to the invention is shown, which is provided with a test ring 12 for performing an initial setup test (S1). The test ring 12 is mounted between a top part 16 and a lower part 18, wherein a spacer ring 20 defines a test chamber 26. Sealing means 24 (in the form of rubber O-rings) are provided in circumferential grooves in the surfaces of the top part and the bottom part. A first of the two sealing means 24 is provided between the top part and the test ring, and a second of the two sealing means 24 is provided between the bottom part and the test ring.
[0120] In use, an O-ring or pressurized pressure member containing a seal disposed on the bottom surface of the top portion and the top surface of the bottom portion engages with the test ring to form an annular gap defined by the inner cylindrical side of the opposing spacer ring and the outer cylindrical side of the test ring and by the top surface of the bottom portion and the bottom surface of the top portion. The defined annular gap provides a pressure chamber into which a pressurized hydraulic fluid can be introduced. The central void of the device is open to atmospheric pressure so that the outer surface of the ring is exposed to atmospheric pressure during testing.
[0121] The top and bottom sections are secured together by mechanical sealing means, such as screws (not shown). Around the outer edges of the apparatus, screws extend through holes 30 in the top section 16 and spacer ring 20 to engage holes 30 in the bottom section 18. Near the center of the apparatus, additional fixtures may extend through holes 30 in annular stepped portion 46 of the top section and engage holes in annular stepped portion 46 of the bottom section 18. Any number of fixtures may be used to ensure that the sections are properly clamped together. Other suitable fixtures, such as hydraulic piston devices, may also be used to clamp the sections of the test apparatus together.
[0122] The force holding the top section, bottom section and spacer ring together is sufficient to make the annular gap pressure tight to the pressure contained in the seal both inside and outside. The tolerances to which the ring is cut from the tube are such that leakage from the annular gap (pressure chamber) into the gap does not occur, while avoiding undue restraining friction forces to prevent radial movement inward from the outer diameter of the ring under hydraulic load. Perform a setup test (S1) to determine if the restraining forces are within the permissible limits when the test equipment is set up.
[0123] refer to Figure 6 9 , during a first setup test phase (S1), the test apparatus includes a hydraulic cylinder 34 in contact with the test ring. Two sensors in the form of displacement sensors 36 are positioned to measure the movement of the test ring during the test. Although two displacement sensors are shown, any suitable number of sensors may be used, for example, one, two, three, four or more displacement sensors may be used. The displacement sensor may be a linear voltage displacement transducer (LVDT). A dynamometer (not shown) is positioned to measure the force applied by the plunger 34 to the inner cylindrical surface of the test ring 12. A needle pump (P) supplies fluid to the hydraulic cylinder. The needle pump supplies fluid at a predetermined rate to increase the force applied by the cylinder to the test ring.
[0124] refer to Figure 4 In the second collapse pressure test phase (S2), the hydraulic cylinder and associated sensors are removed from the apparatus 34. Sensors (not shown) for determining stress and deformation of the ring are attached and the second phase of testing can be performed.
[0125] The method and apparatus according to the invention allow a representative sample of test rings taken from all the pipe joints required for a long deepwater pipeline to be tested to give direct physical quantitative evidence of the ability of these specimens to resist collapse by external hydrostatic pressure.
[0126] By performing an initial test prior to the ring collapse pressure test, the accuracy of the collapse test is improved by ensuring that the test ring is properly assembled in the test equipment. The performance of the initial test helps each ring collapse pressure test to be consistent with each other and helps prevent unacceptable results caused by incorrect application of the ring collapse pressure test.
[0127] Example
[0128] Tests were performed on steel test rings (D / t=20.5) using three exemplary pressures in the pressure chamber (0 MPa, 13.8 MPa, and 27.6 MPa). The test rings were cut from a tube with an outer diameter of 32 inches (812.8 mm) and a wall thickness of 39 mm. The length of the test ring was 50 mm.
[0129] The test ring is mounted in the test rig in a manner that replicates the conditions used for the collapse pressure test. A hydraulic cylinder is positioned and attached to the test ring.
[0130] Pressure was first applied to the chamber at one of the exemplary pressures (0 MPa, 13.8 MPa and 27.6 MPa). The pressure in the cylinder was then increased at a slow rate. The force applied by the cylinder was measured, and the lateral body movement of the ring was measured by two displacement sensors. A different steel ring and a new rubber sealing ring were used for each test. The time and load on the cylinder measured were recorded, and each test lasted about 120 minutes. During the test, the rate of force was measured to increase from about 0.002 kN / min to about 0.04 kN / min.
[0131] The results are shown in Figures 9 and 10. The results show that after a very small movement of the steel ring relative to the sealing ring (about 0.1 mm), the lateral restraining force (i.e., the cylinder force (52)) is substantially constant (Figure 9). The results also show that, without applying pressure to the test device, the cylinder force is quite small. This confirms that the rubber sealing ring will hardly deform at the beginning of any pressure collapse test that the device will be used for. The resistance exerted by the sealing ring increases with the pressure applied to the test ring.
[0132] It will be understood by those skilled in the art that the presently disclosed method and apparatus are taught by way of example and not by way of limitation. Therefore, the aspects contained in the above description or shown in the accompanying drawings should be interpreted as illustrative rather than restrictive. The appended claims are intended to cover all generic and specific features described herein, and all statements regarding the scope of the present method and apparatus as a verbal rhetoric may be considered to fall within the appended claims.
Claims
1. A method of determining whether a test ring is correctly fitted in a test chamber for testing a pipe used in the manufacture of a subsea pipeline, in, The test ring is cut from a tube used to make the pipe and has substantially flat and parallel surfaces at the ends of the test ring; the method comprising: i) installing the test ring into a pressure chamber so that an end of the test ring forms a seal with an opposing surface of the chamber to isolate the interior of the test ring from the exterior; ii) providing means for determining the displacement of said test ring; iii) providing means for determining the force applied to the inner surface of said test ring; iv) applying a force to the inner surface of the test ring; v) determining the displacement of the test ring and determining the force applied to the inner surface; and vi) Using the displacement measurements and the force measurements to determine whether the test ring is correctly installed in the pressure chamber.
2. The method according to claim 1, It is characterized in that include: Once the test ring has moved a predetermined distance, application of force to the inner surface of the test ring is stopped.
3. The method according to claim 2, It is characterized in that The predetermined distance is 1 mm.
4. The method according to claim 1, It is characterized in that include: When a force is applied to the inner surface of the test ring, a pressure higher than 0 MPa and lower than an expected collapse pressure is provided to the pressure chamber.
5. The method according to claim 1, It is characterized in that The method further comprises: before executing steps i) to v), determining a range of allowable restraining force.
6. The method according to claim 1, It is characterized in that The method also includes retaining the test ring in the pressure chamber and performing an external pressure collapse test on the test ring.
7. The method according to claim 6, It is characterized in that The external pressure collapse test includes: providing means for determining stress and deformation of said test ring; increasing pressure outside the test ring and measuring stress and deformation on the test ring as the pressure increases; and The external collapse pressure of the test ring is determined.
8. The method according to claim 7, It is characterized in that Determining the exterior collapse pressure of the test ring includes determining a comparison between the pressure applied to the exterior of the test ring and a measured maximum stress to detect the onset of an accelerated non-linear decrease in ring diameter with increasing pressure.
9. A method for testing a pipe used in the manufacture of a subsea pipeline, the method include: cutting rings from said tube used to make said pipe; forming substantially flat and parallel surfaces at ends of the test ring to provide a test ring; installing the test ring into a pressure chamber so that ends of the test ring form a seal with opposing walls of the chamber to isolate the interior of the test ring from the exterior; providing means for determining the displacement of the test ring, and providing means for determining the force applied to the inner surface of the test ring; applying a force to an inner surface of the test ring; measuring a displacement of the test ring and measuring a force applied to the inner surface, and using the displacement and force measurements to determine whether the test ring is properly assembled in the pressure chamber; providing means for determining stress and deformation of said test ring; increasing pressure outside the test ring and measuring stress and deformation on the test ring as the pressure increases; as well as A comparison between the pressure applied to the exterior of the test ring and the measured maximum stress is determined to detect the onset of an accelerated non-linear decrease in ring diameter with increasing pressure.
10. The method according to any one of claims 1 to 9, It is characterized in that Applying the force to the inner surface of the test ring includes applying the force until the force applied to the test ring exceeds a lateral resistance.
11. The method according to any one of claims 1 to 9, It is characterized in that Applying a force to an inner surface of the test ring includes providing means for applying a force to the inner surface of the test ring.
12. The method according to claim 11, It is characterized in that Providing means for applying a force to the inner surface of the test ring comprises providing a hydraulic cylinder, wherein the hydraulic cylinder is connected to a pump for supplying fluid to the hydraulic cylinder.
13. The method according to any one of claims 1 to 9, It is characterized in that Applying the force to the inner surface of the test ring includes applying the force at a force rate of 0.002 kN / min to 0.04 kN / min.
14. The method according to claim 7, 8 or 9, It is characterized in that Prior to performing the step of increasing the pressure on the exterior of the test ring, the means for applying a force to the interior surface of the test ring is removed from the test ring.
15. A pipe testing apparatus for performing the method according to any one of claims 1 to 14.